Conductive composition, conductive paste, electronic component, and multilayer ceramic capacitor

A conductive composition with a dual dispersant system addresses the dispersibility and density issues in thin electrode layers, achieving smooth and precise electrode patterns for advanced electronic components.

JP7586088B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021548467
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-26
Filing Date
2020-09-25
Publication Date
2024-11-19
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

The challenge of maintaining high dispersibility and density of conductive powder in thin internal electrode layers of multilayer ceramic capacitors, which is exacerbated by the use of smaller particle sizes leading to increased surface activity and agglomeration, affects the precision and smoothness of electrode patterns.

Method used

A conductive composition comprising a combination of a first and second acid-based dispersant with specific molecular weights and branched or linear structures, along with a conductive powder and binder resin, enhances dispersibility and achieves high dry film density and smoothness.

Benefits of technology

The solution results in improved dispersibility and high dry film density, ensuring uniform and precise electrode patterns with reduced surface roughness, suitable for smaller electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586088000002
    Figure 0007586088000002
  • Figure 0007586088000001
    Figure 0007586088000001
Patent Text Reader

Abstract

Provided, inter alia, is an electroconductive composition that exhibits an excellent dispersibility. The electroconductive composition contains electroconductive powder and a dispersant wherein the dispersant comprises a first acidic dispersant, which has an average molecular weight of greater than 500 and not greater than 2000 and has one or more hydrocarbon group-containing branch chains per main chain, and comprises a carboxyl group-bearing second acidic dispersant which is other than the first dispersant.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive composition, a conductive paste, an electronic component, and a multilayer ceramic capacitor. [Background technology]

[0002] As electronic devices such as mobile phones and digital devices become smaller and more powerful, there is a demand for smaller electronic components, including multilayer ceramic capacitors, with higher capacitance. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are alternately stacked, and by thinning these dielectric layers and internal electrode layers, it is possible to achieve smaller size and higher capacitance.

[0003] For example, a multilayer ceramic capacitor is manufactured as follows. First, a conductive paste for internal electrodes is printed (applied) in a predetermined electrode pattern on the surface of a dielectric green sheet containing a dielectric powder such as barium titanate (BaTiO3) and a binder resin, and then dried to form a dry film. Next, the dry film and the green sheet are alternately stacked to obtain a laminate. Next, this laminate is heated and pressed to be integrated to form a pressed body. This pressed body is cut, and an organic binder removal process is performed in an oxidizing atmosphere or an inert atmosphere, and then sintered to obtain a sintered chip. Next, a paste for external electrodes is applied to both ends of the sintered chip, and after sintering, nickel plating or the like is performed on the surface of the external electrodes to obtain a multilayer ceramic capacitor.

[0004] Generally, the conductive paste used to form the internal electrode layer contains a conductive powder, a ceramic powder, a binder resin, and an organic solvent. The conductive paste may also contain a dispersant to improve the dispersibility of the conductive powder and the like. In recent years, the thickness of the internal electrode layer has become thinner, and the conductive powder also tends to become smaller in particle size. When the particle size of the conductive powder is small, the specific surface area of ​​the particle surface becomes large, and the surface activity of the conductive powder (metal powder) becomes high, which may result in a decrease in dispersibility and a decrease in viscosity characteristics.

[0005] Therefore, attempts have been made to improve the viscosity characteristics of conductive pastes over time. For example, Patent Document 1 describes a conductive paste containing at least a metal component, an oxide, a dispersant, and a binder resin, in which the metal component is Ni powder having a specific surface composition, the dispersant has an acid site number of 500 to 2000 μmol / g, and the binder resin has an acid site number of 15 to 100 μmol / g. According to Patent Document 2, this conductive paste is said to have good dispersibility and viscosity stability.

[0006] Also, Patent Document 2 describes a conductive paste for internal electrodes that is made of conductive powder, resin, organic solvent, common material of ceramic powder mainly composed of BaTiO3, and coagulation inhibitor, the content of the coagulation inhibitor being 0.1% by weight or more and 5% by weight or less, and the coagulation inhibitor being a tertiary amine or secondary amine represented by a specific structural formula. According to Patent Document 2, this conductive paste for internal electrodes is said to suppress coagulation of the common material components, has excellent long-term storage properties, and enables the thinning of multilayer ceramic capacitors.

[0007] On the other hand, when the internal electrode layer is thinned, it is required that the density of the dry film obtained by printing the conductive paste for the internal electrode on the surface of the dielectric green sheet and drying it is high. For example, Patent Document 3 proposes a metal ultrafine powder slurry containing an organic solvent, a surfactant, and ultrafine metal particles, the surfactant being oleoyl sarcosine, the metal ultrafine powder slurry containing 70 mass% or more and 95 mass% or less of the metal ultrafine powder, and the surfactant containing more than 0.05 mass parts and less than 2.0 mass parts per 100 mass parts of the metal ultrafine powder. According to Patent Document 3, it is said that by preventing the aggregation of ultrafine particles, a metal ultrafine powder slurry without aggregated particles is obtained, which has excellent dispersibility and dry film density. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2015-216244 A [Patent Document 2] JP 2013-149457 A [Patent Document 3] JP 2006-063441 A Summary of the Invention [Problem to be solved by the invention]

[0009] In recent years, with the trend toward thinner electrode patterns and dielectric layers, there is a demand for internal electrode layers that have smoother electrode surfaces and denser electrode densities than ever before, without surface roughness caused by coarse particles formed by agglomeration of conductive powder, in order to maintain the clearance between each electrode pattern with precision.

[0010] In view of the above circumstances, an object of the present invention is to provide a conductive composition which has excellent dispersibility of conductive powder and high dry film density, which is the basis of electrode density. [Means for solving the problem]

[0011] In a first aspect of the present invention, there is provided a conductive composition containing a conductive powder and a dispersant, the dispersant including a first acid-based dispersant and a second acid-based dispersant, the first acid-based dispersant having an average molecular weight of more than 500 and not more than 2000 and having one or more branched chains consisting of hydrocarbon groups on a main chain, and the second acid-based dispersant being an acid-based dispersant other than the first dispersant and having a carboxyl group.

[0012] The second acid dispersant may be a straight-chain acid dispersant. The second acid dispersant may be a branched acid dispersant with a molecular weight of 250 to 1400. The first acid dispersant preferably has a carboxyl group. The first acid dispersant is preferably a hydrocarbon graft copolymer with a polycarboxylic acid as the main chain. The first acid dispersant is preferably contained in an amount of 0.2 to 2 parts by mass relative to 100 parts by mass of the conductive powder, and the second acid dispersant is preferably contained in an amount of 0.3 to 2 parts by mass relative to 100 parts by mass of the conductive powder. The conductive powder preferably contains at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. The conductive powder preferably has an average particle size of 0.05 μm to 1.0 μm.

[0013] In a second aspect of the present invention, there is provided a conductive paste containing the above-mentioned conductive composition, a binder resin, and an organic solvent.

[0014] The conductive paste preferably further contains a ceramic powder. The ceramic powder preferably contains a perovskite oxide. The ceramic powder preferably has an average particle size of 0.01 μm or more and 0.5 μm or less. The binder resin preferably contains at least one of a cellulose-based resin, an acrylic-based resin, and a butyral-based resin. The conductive paste is preferably for use in an internal electrode of a multilayer ceramic component.

[0015] In a third aspect of the present invention, there is provided an electronic component formed using the above-mentioned conductive paste.

[0016] In a fourth aspect of the present invention, there is provided a multilayer ceramic capacitor having at least a laminate in which dielectric layers and internal electrodes are laminated, the internal electrodes being formed using the above-mentioned conductive paste. Effect of the Invention

[0017] The conductive composition (conductive paste) of the present invention has high dry film density due to excellent dispersibility of the conductive powder. In addition, the electrode pattern of an electronic component such as a multilayer ceramic capacitor formed using the conductive paste of the present invention has excellent printability of the conductive paste even when forming a thin electrode, and can have a uniform width and thickness with high precision. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a perspective view and a cross-sectional view showing a multilayer ceramic capacitor according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] [Conductive composition and conductive paste] The conductive composition according to the present embodiment includes a conductive powder and a dispersant. The conductive paste according to the present embodiment includes the conductive powder and the dispersant, a binder resin, and an organic solvent. The conductive paste may further include a ceramic powder. Each component included in the conductive powder or the conductive paste will be described in detail below.

[0020] (conductive powder) The conductive powder is not particularly limited, and a metal powder can be used, for example, a powder of one or more selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. Among these, from the viewpoints of conductivity, corrosion resistance, and cost, a powder of Ni or its alloy (hereinafter, both may be collectively referred to as "Ni powder") is preferable. As the Ni alloy, for example, an alloy of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd can be used. The Ni content in the Ni alloy is, for example, 50 mass% or more, preferably 80 mass% or more. In addition, the Ni powder may contain about several hundred ppm of element S in order to suppress rapid gas generation due to partial thermal decomposition of the binder resin during the binder removal process.

[0021] The average particle size of the conductive powder is preferably 0.05 μm or more and 1.0 μm or less, more preferably 0.1 μm or more and 0.5 μm or less. When the average particle size of the conductive powder is within the above range, it can be suitably used as an internal electrode paste for a thin-film multilayer ceramic capacitor (multilayer ceramic component), and for example, the smoothness and density of the dry film are improved. The average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 10,000 times.

[0022] The content of the conductive powder is preferably 30% by mass or more and less than 70% by mass, more preferably 40% by mass or more and 60% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0023] (ceramic powder) The ceramic powder is not particularly limited, and for example, in the case of a paste for an internal electrode of a multilayer ceramic capacitor, a known ceramic powder is appropriately selected depending on the type of multilayer ceramic capacitor to be applied. Examples of the ceramic powder include perovskite oxides containing Ba and Ti, and preferably barium titanate (BaTiO3).

[0024] The ceramic powder may be a ceramic powder containing barium titanate as a main component and oxides as sub-components. Examples of oxides include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. The ceramic powder may be a perovskite-type oxide ferroelectric ceramic powder in which the Ba and Ti atoms of barium titanate (BaTiO3) are replaced with other atoms, such as Sn, Pb, and Zr.

[0025] When used as an internal electrode paste, the ceramic powder may be powder of the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor (electronic component). This suppresses the occurrence of cracks due to the mismatch of shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. In addition to the above, such ceramic powders include oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R (rare earth element)2O3, TiO2, and Nd2O3. Note that one type of ceramic powder may be used, or two or more types may be used.

[0026] The average particle size of the ceramic powder is, for example, 0.01 μm to 0.5 μm, preferably 0.01 μm to 0.3 μm. When the average particle size of the ceramic powder is in the above range, it is possible to form a sufficiently fine, thin, and uniform internal electrode when used as an internal electrode paste. The average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 50,000 times.

[0027] The content of the ceramic powder is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 3 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the conductive powder.

[0028] The content of the ceramic powder is preferably 1% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 20% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0029] (binder resin) The binder resin is not particularly limited, and known resins can be used. Examples of the binder resin include cellulose-based resins such as methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and nitrocellulose, acrylic resins, and butyral-based resins such as polyvinyl butyral. Among them, it is preferable to include ethyl cellulose from the viewpoint of solubility in a solvent and combustion decomposition. In addition, when used as an internal electrode paste, it may contain a butyral-based resin from the viewpoint of improving the adhesive strength with the green sheet, or a butyral-based resin may be used alone. One type of binder resin may be used, or two or more types may be used. In addition, it is preferable to use a mixture of a cellulose-based resin and a butyral-based resin as the binder resin from the viewpoint of improving various properties. In addition, the molecular weight of the binder resin is, for example, about 20,000 to 200,000.

[0030] The content of the binder resin is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the conductive powder.

[0031] The content of the binder resin is preferably 0.5% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 6% by mass or less, based on the total amount of the conductive paste. When the content of the binder resin is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0032] (Organic solvent) The organic solvent is not particularly limited, and any known organic solvent capable of dissolving the binder resin can be used. Examples of the organic solvent include acetate-based solvents such as dihydroterpineyl acetate, isobornyl acetate, isobornyl propionate, isobornyl butyrate and isobornyl isobutyrate, ethylene glycol monobutyl ether acetate, and dipropylene glycol methyl ether acetate, terpene-based solvents such as terpineol and dihydroterpineol, and hydrocarbon-based solvents such as tridecane, nonane, and cyclohexane. Among these, it is preferable to use a terpene-based solvent such as terpineol. The organic solvent may be used alone or in combination of two or more.

[0033] The content of the organic solvent is preferably 40 parts by mass or more and 100 parts by mass or less, more preferably 65 parts by mass or more and 95 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductive powder has excellent conductivity and dispersibility.

[0034] The content of the organic solvent is preferably 20% by mass or more and 60% by mass or less, and more preferably 35% by mass or more and 55% by mass or less, based on the total amount of the conductive paste. When the content of the organic solvent is within the above range, the conductive paste has excellent conductivity and dispersibility.

[0035] (Dispersant) The present inventors have investigated various dispersants for use in the conductive composition, and have found that the dispersibility of the conductive powder is particularly improved and the dry film density is improved by using a first dispersant containing an acid dispersant having one or more, preferably multiple, branched chains made of hydrocarbon groups and an average molecular weight of more than 500 and not more than 2000, and a second acid dispersant having a carboxyl group other than the first acid dispersant. The dispersant according to this embodiment will be described in more detail below.

[0036] (First acid-based dispersant) The first acid-based dispersant used in this embodiment is an acid-based dispersant having an average molecular weight of more than 500 and not more than 2000, and having one or more branched chains consisting of hydrocarbon groups on the main chain. By containing the first acid-based dispersant, the conductive composition according to this embodiment has a high dry film density and improved smoothness of the dry film surface, compared to conventional conductive compositions that do not contain the first acid-based dispersant.

[0037] Although the details of the reason for this are unclear, it is believed that the presence of one or more branched chains consisting of hydrocarbon groups in the main chain effectively forms steric hindrance, thereby suppressing the aggregation of the powder material. In addition, by setting the average molecular weight of the first dispersant within the above range, it is possible to maintain a suitable viscosity when made into a paste depending on the application of the conductive composition. Note that the present invention is not restricted by the above theory (reason).

[0038] The first acid dispersant preferably has a carboxyl group, and is more preferably a hydrocarbon graft copolymer having a polycarboxylic acid as the main chain. The polycarboxylic acid preferably has an ester structure.

[0039] In addition, the hydrocarbon group which is the branched chain of the first acid-based dispersant preferably has a chain structure. The hydrocarbon group may be an alkyl group. In addition, the alkyl group may be composed of only carbon and hydrogen, and a part of the hydrogen constituting the alkyl group may be substituted with a substituent. In addition, it is preferable that the main chain and the hydrocarbon group do not have a ring structure.

[0040] (Second acid-based dispersant) The second acid-based dispersant is an acid-based dispersant having a carboxyl group other than the first dispersant. By using the second acid-based dispersant together with the first acid-based dispersant, the conductive composition according to the present embodiment can further improve the dry film density.

[0041] The second acid dispersant may be a straight-chain acid dispersant. That is, the second acid dispersant has a straight-chain structure and may not have a branched chain consisting of a hydrocarbon group with respect to the main chain. In this case, the molecular weight of the second acid dispersant is preferably 5000 or less, and may be 250 to 1400. The second acid dispersant preferably contains an alkyl group having 10 to 20 carbon atoms or an alkenyl group having 10 to 20 carbon atoms. The second acid dispersant preferably has a smaller molecular weight than the first acid dispersant. By using the second acid dispersant as described above together with the first acid dispersant, the dry film density can be increased and the smoothness of the dry film surface can be further improved.

[0042] The second acid dispersant may be an acid dispersant having a branched chain. In this case, the second acid dispersant is preferably an acid dispersant having a molecular weight of 250 to 1400. The second acid dispersant may be a dicarboxylic acid. The second acid dispersant having a branched chain preferably contains an alkyl group having 15 to 100 carbon atoms or an alkenyl group having 15 to 100 carbon atoms, more preferably contains an alkyl group having 15 to 50 carbon atoms or an alkenyl group having 15 to 50 carbon atoms, and further preferably contains an alkyl group having 15 to 25 carbon atoms or an alkenyl group having 15 to 25 carbon atoms. The second acid dispersant preferably has a smaller molecular weight than the first acid dispersant. By using the second acid dispersant as described above together with the first acid dispersant, the dry film density can be increased and the smoothness of the dry film surface can be further improved.

[0043] Each acid-based dispersant may be selected from commercially available products that satisfy the above-mentioned characteristics. The acid-based dispersant may be produced by a conventionally known production method so as to satisfy the above-mentioned characteristics.

[0044] (Dispersant content) The first acid dispersant is contained in an amount of, for example, 0.2 parts by mass or more and 2 parts by mass or less per 100 parts by mass of the conductive powder, and the second acid dispersant is contained in an amount of, for example, 0.01 parts by mass or more and 2 parts by mass or less per 100 parts by mass of the conductive powder. When the content of the dispersant is within the above range, the dispersibility of the conductive powder is improved, the smoothness of the dried electrode surface after application is more excellent, the dry film density is also improved, and the viscosity of the conductive paste can be adjusted to an appropriate range, compared to when the same amount of the first acid dispersant is contained alone. In addition, sheet attack and peeling failure of the green sheet can be suppressed.

[0045] In addition, the content of the first acid dispersant may be 1 part by mass or less, or 0.5 parts by mass or less, within the above range. Even if the content of the first acid dispersant is small, high dispersibility can be obtained by using the second acid dispersant in combination. In addition, sheet attack and peeling failure of the green sheet caused by residual dispersant are further suppressed.

[0046] The lower limit of the content of the second acid-based dispersant is preferably 0.3 parts by mass or more, and may be 0.5 parts by mass or more, relative to 100 parts by mass of the conductive powder. When the lower limit of the content of the second dispersant is within the above range, the smoothness of the dry film surface can be further improved. The upper limit of the content of the second acid-based dispersant may be 1.5 parts by mass or less, or may be 1.2 parts by mass or less, from the viewpoint of having a higher dry film density and further suppressing sheet attack and peeling failure of the green sheet caused by residual dispersant. The content of the second dispersant may be greater than the content of the first dispersant, from the viewpoint of further improving the dry film density.

[0047] The total amount of the acid dispersant is preferably 3% by mass or less based on the total amount of the conductive paste. The upper limit of the dispersant content is preferably 2% by mass or less, more preferably 1% by mass or less. The lower limit of the dispersant content is not particularly limited, but is, for example, 0.01% by mass or more, preferably 0.05% by mass or more. When the dispersant content is within the above range, the viscosity of the conductive paste can be adjusted to an appropriate range, and sheet attack and peeling failure of the green sheet can be suppressed.

[0048] The conductive paste may contain a dispersant other than the above-mentioned acid-based dispersant within a range that does not impair the effects of the present invention. Examples of dispersants other than the above-mentioned may include acid-based dispersants containing higher fatty acids, polymeric surfactants, base-based dispersants, amphoteric surfactants, and polymeric dispersants, and it is more preferable to contain a base-based dispersant. These dispersants may be used alone or in combination of two or more.

[0049] When a dispersant other than an acid-based dispersant is contained, the content of the entire dispersant (total content), including the acid-based dispersant that is mainly added, is preferably 0.01 parts by mass or more and 3 parts by mass or less, and may be 2.5 parts by mass or less, 2.0 parts by mass or less, or 1.5 parts by mass or less, relative to 100 parts by mass of the conductive powder.

[0050] (Conductive paste) The conductive paste according to the present embodiment can be produced by mixing (stirring and kneading) the above-mentioned respective materials. Specifically, the conductive paste can be produced by preparing the above-mentioned respective components and stirring and kneading them with a mixer.

[0051] The above materials may be mixed at the same time, or, for example, a conductive powder, a dispersant, and an organic solvent may be mixed in advance to prepare a conductive powder slurry. This allows the dispersant to be applied in advance to the conductive powder surface. If the dispersant is applied in advance to the conductive powder surface, the conductive powder will remain in a sufficiently dispersed state without agglomeration even when mixed with other materials to produce a conductive paste, making it easier to obtain a uniform conductive paste.

[0052] The conductive powder slurry ( / application of a dispersant onto the surface of a conductive powder) is prepared ( / applied) by, for example, mixing ( / applying) 0.01 parts by mass or more and less than 5 parts by mass, preferably 0.1 parts by mass or more and 3 parts by mass or less, of a dispersant per 100 parts by mass of the conductive powder.

[0053] Also, for example, a ceramic powder, a dispersant, and an organic solvent may be mixed in advance to prepare a ceramic powder slurry. This allows the dispersant to be applied to the ceramic powder in advance. If the dispersant is applied in advance to the surface of the ceramic powder, the ceramic powder will maintain a sufficiently dispersed state without agglomeration even when mixed with other materials to produce a conductive paste, making it easier to obtain a uniform conductive paste.

[0054] The ceramic powder slurry ( / application of a dispersant to a ceramic powder) is prepared ( / applied) by mixing (for example) 0.01 parts by mass or more and 10 parts by mass or less, preferably 0.1 parts by mass or more and 5 parts by mass or less, of a dispersant with respect to 100 parts by mass of the conductive powder.

[0055] Alternatively, a binder resin may be dissolved in an organic solvent for a vehicle to prepare an organic vehicle, and then a conductive powder, a ceramic powder, an organic vehicle and a dispersant may be added to the organic solvent for a paste, followed by stirring and kneading with a mixer to prepare a conductive paste.

[0056] In addition, among the organic solvents, the organic solvent for the vehicle is preferably the same as the organic solvent for the paste that adjusts the viscosity of the conductive paste in order to improve the compatibility of the organic vehicle. The content of the organic solvent for the vehicle is, for example, 5 parts by mass or more and 80 parts by mass or less with respect to 100 parts by mass of the conductive powder. The content of the organic solvent for the vehicle is preferably 10% by mass or more and 40% by mass or less with respect to the total amount of the conductive paste.

[0057] The conductive paste preferably has a viscosity of 10 Pa s to 50 Pa s 24 hours after production. The viscosity of the conductive paste can be measured using a Brookfield Type B viscometer at 10 rpm (shear rate = 4 sec-1).

[0058] In addition, the dry film density (DFD) of the dried film obtained by screen printing the conductive paste and drying it is 5.0 g / cm 3 It is preferable that the density exceeds 5.5 g / cm 3 More preferably, it should exceed 5.6 g / cm 3 The upper limit of the dry film density is not particularly limited, and is, for example, 6.5 g / cm. 3 The upper limit of the dry film density is the true density of the conductive powder used (e.g., 9.8 g / cm in the case of metallic nickel). 3 ) shall not exceed.

[0059] Furthermore, when the conductive paste is screen-printed and dried in air at 120°C for 1 hour to produce a dried film having a size of 20 mm square and a thickness of 1 to 3 μm, the surface roughness Ra (arithmetic mean roughness) is preferably 0.045 μm or less, more preferably 0.04 μm or less. The lower limit of the surface roughness Ra (arithmetic mean roughness) is not particularly limited, and it is preferable that the surface is flat, but a value exceeding 0 and a smaller value are preferable.

[0060] The Rt (maximum cross-sectional height) of the above-mentioned dry film is preferably 0.4 μm or less. The lower limit of the surface roughness Ra (arithmetic mean roughness) is not particularly limited, and the surface is preferably flat, but a value exceeding 0 and a smaller value are preferable.

[0061] The conductive paste can be suitably used in electronic components such as multilayer ceramic capacitors. A multilayer ceramic capacitor has dielectric layers formed using dielectric green sheets and internal electrode layers formed using the conductive paste.

[0062] In a multilayer ceramic capacitor (electronic component), the dielectric ceramic powder contained in the dielectric green sheet and the ceramic powder contained in the conductive paste are preferably powders of the same composition. In a multilayer ceramic device manufactured using the conductive paste of this embodiment, sheet attack and peeling failure of the green sheet are suppressed even when the thickness of the dielectric green sheet is, for example, 3 μm or less.

[0063] [Electronic components] Hereinafter, embodiments of electronic components and the like of the present invention will be described with reference to the drawings. In the drawings, the components may be shown diagrammatically or at a different scale as appropriate. The positions and directions of components will be described with reference to an XYZ orthogonal coordinate system shown in FIG. 1 as appropriate. In this XYZ orthogonal coordinate system, the X and Y directions are horizontal directions, and the Z direction is vertical (up-down direction).

[0064] The electronic component of the present embodiment is formed using the conductive paste of the present embodiment described above. Figures 1A and 1B are diagrams showing a multilayer ceramic capacitor 1, which is an example of an electronic component according to an embodiment. The multilayer ceramic capacitor 1 includes a laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately laminated, and an external electrode 20. The multilayer ceramic capacitor 1 is formed using the conductive paste of the present embodiment described above.

[0065] A method for manufacturing a multilayer ceramic capacitor using the conductive paste will be described below. First, the conductive paste is printed on a dielectric layer made of a ceramic green sheet, and dried to form a dry film. A plurality of dielectric layers having this dry film on the upper surface are laminated by pressure bonding to obtain a laminate, and then the laminate is fired and integrated to produce a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately laminated. Then, a pair of external electrodes is formed on both ends of the ceramic laminate 10 to manufacture a multilayer ceramic capacitor 1. A more detailed description will be given below.

[0066] First, a ceramic green sheet, which is an unfired ceramic sheet, is prepared. For example, the ceramic green sheet is prepared by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a raw powder of a specific ceramic such as barium titanate, applying the dielectric layer paste to a support film such as a PET film in a sheet form, and drying to remove the solvent. The thickness of the dielectric layer made of the ceramic green sheet is not particularly limited, but is preferably 0.05 μm or more and 3 μm or less from the viewpoint of the demand for miniaturization of the multilayer ceramic capacitor.

[0067] Next, the above-mentioned conductive paste is printed (applied) on one side of the ceramic green sheet by a known method such as screen printing, and then dried to form a dry film, to prepare a plurality of sheets. Note that, from the viewpoint of the requirement for thinning of the internal electrode layer 11, it is preferable that the thickness of the printed conductive paste (dried film) is 1 μm or less after drying.

[0068] Next, the ceramic green sheet is peeled off from the support film, and the dielectric layer made of the ceramic green sheet and the dry film formed on one side thereof are alternately laminated, and then a laminate is obtained by a heat and pressure treatment. Note that a configuration in which protective ceramic green sheets not coated with the conductive paste are further arranged on both sides of the laminate may be adopted.

[0069] Next, the laminate is cut to a predetermined size to form green chips, and the green chips are subjected to a binder removal process and fired under a reducing atmosphere to manufacture the ceramic laminate 10. The binder removal process is preferably performed in air or N2 gas. The temperature during the binder removal process is, for example, 200°C or higher and 400°C or lower. The temperature is preferably held for 0.5 hours or higher and 24 hours or lower during the binder removal process. The firing is performed in a reducing atmosphere to suppress oxidation of the metal used in the internal electrode layers, and the temperature during firing of the laminate is, for example, 1000°C or higher and 1350°C or lower, and the temperature is held for, for example, 0.5 hours or higher and 8 hours or lower.

[0070] By firing the green chip, the organic binder in the green sheet is completely removed, and the ceramic raw material powder is fired to form the ceramic dielectric layer 12. The organic vehicle in the dry film is also removed, and the nickel powder or the alloy powder mainly composed of nickel is sintered or melted and integrated to form the internal electrodes, forming a multilayer ceramic sintered body in which a plurality of dielectric layers 12 and internal electrode layers 11 are alternately stacked. Note that, from the viewpoint of taking oxygen into the dielectric layers to increase reliability and suppressing reoxidation of the internal electrodes, the sintered multilayer ceramic sintered body may be subjected to an annealing treatment.

[0071] A pair of external electrodes 20 is then provided on the produced fired laminated ceramic body to manufacture the laminated ceramic capacitor 1. For example, the external electrode 20 includes an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. Note that, for example, copper, nickel, or an alloy thereof can be suitably used as the material for the external electrode 20. Note that the electronic component can also be an electronic component other than a laminated ceramic capacitor. EXAMPLES

[0072] The present invention will be described in detail below based on examples and reference examples, but the present invention is not limited to these examples.

[0073] [Evaluation method] (Dry film density) The conductive paste thus prepared was placed on a PET film and stretched to a length of approximately 100 mm using an applicator with a width of 50 mm and a gap of 125 μm. The resulting PET film was dried at 120°C for 40 minutes to form a dried body, which was then cut into four pieces measuring 2.54 cm (1 inch) square. After removing the PET film, the thickness and weight of each of the four dried films were measured to calculate the dry film density (average value).

[0074] (Surface roughness) The conductive paste was screen-printed onto a 2.54 cm (1 inch) square piece of heat-resistant tempered glass, and dried in air at 120°C for 1 hour to produce a 20 mm square dry film with a thickness of 1 to 3 μm. The surface roughness Ra (arithmetic mean roughness) and Rt (maximum cross-sectional height) of the dry film were measured according to the JIS B0601-2001 standard.

[0075] [Materials used] (conductive powder) As the conductive powder, Ni powder (SEM average particle size: 0.2 μm) was used.

[0076] (binder resin) The binder resins used were ethyl cellulose resin (EC resin) and polyvinyl butyral resin (PVB resin). When preparing the conductive slurry, an organic vehicle was prepared by dissolving 12 parts by mass of the binder resin (a 2:1 mixture of EC resin and PVB resin) in 88 parts by mass of terpineol.

[0077] (Dispersant) As the first acid-based dispersants, (i) acid-based dispersant A, which is a hydrocarbon-based graft copolymer with a polycarboxylic acid main chain and has an average molecular weight of 800, and (ii) acid-based dispersant B, which is a hydrocarbon-based graft copolymer with a polycarboxylic acid main chain and has an average molecular weight of 1,500, were used.

[0078] In addition, as the second acid-based dispersants, (i) acid-based dispersant C, which is a straight-chain dispersant having a carboxyl group and has an average molecular weight of 350, (ii) acid-based dispersant D, which is a straight-chain dispersant having a carboxyl group and has an average molecular weight of 290, and (iii) acid-based dispersant F, which has two carboxyl groups and a branched chain relative to the main chain and has an average molecular weight of 370, were used.

[0079] As the second acid-based dispersant, (iv) in Example 12, acid-based dispersant B (corresponding to the first dispersant) which is a hydrocarbon-based graft copolymer with a polycarboxylic acid main chain and has an average molecular weight of 1,500 was used, and (v) in Example 13, acid-based dispersant E which has two carboxyl groups, a branched chain on the main chain, and has an average molecular weight of 230 was used.

[0080] (Organic solvent) As the organic solvent, terpineol (a terpene-based solvent) was used.

[0081] Example 1 A conductive paste for evaluation was prepared by mixing 100 parts by mass of conductive powder (Ni powder) with 50 parts by mass of an organic vehicle containing a binder resin made of a 2:1 mixture of EC resin and PVB resin, 0.5 parts by mass of acid-based dispersant A as the first acid-based dispersant, and 1 part by mass of acid-based dispersant C as the second acid-based dispersant, and adding an organic solvent so that the mixed material was 85.5% by mass. The types of dispersants used in the conductive paste are shown in Table 1.

[0082] In addition, a dry film was prepared using the obtained conductive paste by the method described in the evaluation method above, and the dry film density and the surface roughness of the dry film were evaluated by the methods described above. The evaluation results are shown in Table 1.

[0083] (Examples 2 to 13) A conductive paste was prepared under the same conditions as in Example 1, except that the dispersant was used in the combination of type and content shown in Table 1. The dry film density and surface roughness of the dry film prepared using the conductive paste were evaluated by the above-mentioned method. The evaluation results are shown in Table 1 together with the type and content of the acid-based dispersant used.

[0084] (Reference examples 1~3) A conductive paste was prepared under the same conditions as in Example 1, except that the dispersants were used in the combinations of type and content shown in Table 1. The dry film density and surface roughness of the dry film prepared using the conductive paste were evaluated by the above-mentioned method. The evaluation results are shown in Table 1 together with the type and content of the acid-based dispersant used.

[0085] [Table 1]

[0086] (Evaluation Results) From the results in Table 1, it was confirmed that the conductive pastes containing the first acid-based dispersant and the second acid-based dispersant in Examples 1 and 4 to 13 had higher dry film density and smaller dry film surface roughness and were smoother than the conductive paste of Reference Example 1, which had the same content of the first acid-based dispersant but did not contain the second acid-based dispersant.

[0087] In addition, the conductive pastes of Examples 2 and 3, which were produced under the same conditions as Example 1 except that the content of the first acid-based dispersant was changed to 0.2 parts by mass or 2.0 parts by mass, also had high dry film density and small dry film surface roughness (Ra and Rt), similar to the other examples.

[0088] Furthermore, when comparing Examples 4 to 7 in which the content of the second acid-based dispersant was varied within the range of 0.01 to 2.0 parts by mass, it was confirmed that the surface roughness (Ra and Rt) of the dried film was further reduced and the film had high smoothness (i.e., Ra: 0.045 μm or less, and Rt: 0.4 μm or less) in the conductive pastes of Examples 6 and 7 in which the content of the second acid-based dispersant was 0.3 parts by mass or more.

[0089] On the other hand, in the conductive paste of Reference Example 2, in which the content of only the first acid-based dispersant was the same as the total amount of the dispersants in Examples 1 and 8 to 10 (1.5 parts by mass), the dry film density was improved, but was lower than those of these Examples, and the improvement in smoothness (particularly the reduction in Rt) was not sufficient.

[0090] In addition, in the conductive paste of Reference Example 3, in which the content of only the second acid-based dispersant was the same as the total dispersion amount in Examples 1 and 8 to 10 (1.5 parts by mass), the dry film density was improved as in Reference Example 2, but the dry film density was lower than those examples, and the improvement in smoothness (particularly the reduction in Rt) was not sufficient.

[0091] In addition, the conductive pastes of Examples 12 and 13, which used a dispersant having a branched chain and a molecular weight exceeding 1400 or less than 250 as the second dispersant, had improved dry film density compared to Comparative Example 2, but did not show sufficient reduction in dry film surface roughness (Ra and Rt) compared to other Examples. Therefore, from the viewpoint of further improving smoothness, it is preferable to use, as the second acid-based dispersant, an acid-based dispersant having a linear structure as in Example 1, or an acid-based dispersant having a molecular weight of 250 to 1400 and having a branched chain as in Examples 10 and 11.

[0092] The technical scope of the present invention is not limited to the aspects described in the above-mentioned embodiments. For example, the conductive paste for printing electrodes, wiring, etc. on electronic components can be the conductive paste prepared in the examples as it is, but ceramic powder may be further added to improve adhesion with the dielectric layer. It has been confirmed that the inclusion of ceramic powder does not inhibit the dispersibility of the conductive paste. Therefore, the conductive paste according to this embodiment can also be used as a conductive paste for electrodes such as internal electrodes of multilayer ceramic capacitors. [Industrial Applicability]

[0093] The conductive paste according to this embodiment has excellent dispersibility, and therefore has excellent dry film density and surface smoothness after application. In particular, it can be suitably used as a raw material for the internal electrodes of multilayer ceramic capacitors, which are chip components in electronic devices such as mobile phones and digital devices that are becoming increasingly miniaturized.

[0094] Note that one or more of the requirements described in the above embodiments may be omitted. The requirements described in the above embodiments may be combined as appropriate. In addition, to the extent permitted by law, the disclosures of all documents cited in the above embodiments are incorporated by reference into this text. In addition, to the extent permitted by law, the contents of Japanese Patent Application No. 2019-175455 are incorporated by reference into this text. [Explanation of symbols]

[0095] 1. Multilayer ceramic capacitors 10 Ceramic laminate 11 Internal electrode layer 12 Dielectric layer 20 External electrode 21 External electrode layer 22 Plating layer

Claims

1. A conductive composition comprising a conductive powder and a dispersant, The dispersant includes a first acid-based dispersant and a second acid-based dispersant, the first acid-based dispersant is a hydrocarbon-based graft copolymer having a polycarboxylic acid main chain and an average molecular weight of more than 500 and not more than 2000, and having one or more branched chains composed of hydrocarbon groups on the main chain; the second acid-based dispersant is an acid-based dispersant having a carboxyl group other than the first acid-based dispersant.

2. The conductive composition of claim 1 , wherein the second acid-based dispersant is a linear acid-based dispersant.

3. The conductive composition according to claim 1 , wherein the second acid-based dispersant has a branched chain and a molecular weight of 250 or more and 1,400 or less.

4. The conductive composition according to any one of claims 1 to 3, wherein the first acid-based dispersant has a carboxyl group.

5. The conductive composition according to any one of claims 1 to 4, wherein the first acid-based dispersant is contained in an amount of 0.2 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the conductive powder, and the second acid-based dispersant is contained in an amount of 0.3 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the conductive powder.

6. The conductive composition according to any one of claims 1 to 5, wherein the conductive powder contains at least one metal powder selected from the group consisting of Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof.

7. The conductive composition according to any one of claims 1 to 6, wherein the conductive powder has an average particle size of 0.05 µm or more and 1.0 µm or less.

8. A conductive paste comprising the conductive composition according to any one of claims 1 to 7, a binder resin and an organic solvent.

9. The conductive paste according to claim 8 , further comprising a ceramic powder.

10. The conductive paste according to claim 9 , wherein the ceramic powder contains a perovskite oxide.

11. 11. The conductive paste according to claim 9, wherein the ceramic powder has an average particle size of 0.01 μm or more and 0.5 μm or less.

12. The conductive paste according to any one of claims 8 to 11, wherein the binder resin contains at least one of a cellulose-based resin, an acrylic-based resin, and a butyral-based resin.

13. The conductive paste according to any one of claims 8 to 12, which is for use in an internal electrode of a multilayer ceramic part.

14. An electronic component formed by using the conductive paste according to any one of claims 8 to 12.

15. The laminate has at least a dielectric layer and an internal electrode laminated thereon, A multilayer ceramic capacitor, wherein the internal electrodes are formed using the conductive paste according to claim 13.

Citation Information

Patent Citations

  • Ultrafine metal powder slurry

    JP2006063441A

  • Conductive paste for internal electrode

    JP2013149457A

  • Method for producing conductive paste

    JP2014029845A

  • Conductive paste and ceramic electronic part

    JP2015216244A

  • Die attach paste for semiconductor and semiconductor device

    JP2016219600A