Porous membrane and method for producing the same
The porous membrane with a denser surface layer and nano-network structure addresses the issue of coarse and fine component clogging, achieving efficient filtration and stain resistance.
Patent Information
- Application Number
- JP2022576815
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-28
- Filing Date
- 2022-09-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-09-26
AI Technical Summary
Existing porous membranes face issues with stain resistance due to coarse components invading the membrane and fine particles being trapped, leading to clogging, especially when filtering solutions with high fouling substances.
A porous membrane design with a denser surface layer and controlled pore structure, including specific pore densities, diameters, and curvature ratios, along with a nano-network structure, to prevent coarse components from entering and efficiently allow fine components to pass through.
The membrane effectively filters solutions with high fouling substances while maintaining filtration efficiency and preventing clogging, ensuring high stain resistance and long-term performance.
Smart Images

Figure 0007586198000006 
Figure 0007586198000007 
Figure 0007586198000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous membrane and a method for producing the same. [Background technology]
[0002] In recent years, porous membranes such as microfiltration membranes and ultrafiltration membranes have been used in various fields, including water treatment fields such as water purification or wastewater treatment, medical fields such as blood purification, and food industry. Recently, there has been a demand for porous membranes with high fouling resistance that can efficiently filter "filtrate stock solutions that are easily fouled" that have been considered difficult to filter. Filtration stock solutions that are easily fouled by porous membranes are characterized by the fact that they contain more fouling substances than conventional stock solutions. The fouling substances often contain coarse components to be removed (Stokes diameter: 13 nm or more) and fine components (molecular weight: 10,000 Da or less) that are not to be removed but are useful substances and are preferably passed through.
[0003] The fouling resistance of a porous membrane means that when performing high-precision removal, problems such as clogging of the pores of the porous membrane are reduced for both coarse and fine components that are fouling substances or the objects to be removed, and the removal efficiency and water permeability of the objects to be removed can be maintained stably for a long period of time.
[0004] As an example of a porous membrane that exhibits stain resistance, Patent Document 1 discloses a porous membrane that has a three-dimensional mesh structure with large pores, thereby providing both a high removal rate of the target substance and a high water permeability coefficient.
[0005] Patent Document 2 discloses a technique for improving the removal rate of targets such as viruses by miniaturizing the pore size of a three-dimensional mesh structure. The three-dimensional mesh structure disclosed in Patent Document 2 has an average diameter of 0.01 μm or more and 1 μm or less, and does not substantially have macrovoids of 5 μm or more. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2006-82006 [Patent Document 2] Japanese Patent Publication No. 2010-94670 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the three-dimensional mesh structure having huge pores as described in Patent Document 1, the average pore size is large and the three-dimensional structure is spider web-like, so that coarse components penetrate the porous membrane and foul the porous membrane. In addition, since fine particles are captured in the gaps of the entangled fine filament structure, the porous membrane is easily clogged and has insufficient dirt resistance. The porous membrane described in Patent Document 2 is intended to remove relatively large components such as viruses, and only improves the removal ability, and the mesh structure has a relatively large pore size and a small number of pores. Therefore, dirt substances are easily accumulated in the porous membrane, and dirt resistance is sacrificed for the easily dirty filtrate raw liquid.
[0008] On the other hand, since the porous membrane is significantly fouled when the raw solution is easily soiled as described above, filtration is difficult. A porous membrane having high fouling resistance that enables filtration even when the raw solution is easily soiled is required.
[0009] Therefore, the present invention aims to provide a porous membrane having excellent stain resistance by removing coarse components at the outer surface of the porous membrane and allowing fine components to efficiently permeate the porous membrane. The outer surface is the surface portion of the porous membrane, in other words, the outer surface of the surface layer opposite to the inside. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention provides a porous membrane having the following configuration. 1. On at least one surface, a surface portion from the surface to a thickness of 10 μm is denser than the interior, the removal rate of dextran having a weight-average molecular weight of 40,000 Da: T is 60% to 95%, and the number of pores observed on the surface of the surface portion (hereinafter referred to as surface pores) per unit area is 200 pores / μm 2 ~2000 pieces / μm 2 It is a porous membrane. 2. The porous film according to 1, wherein the average surface pore diameter [nm] of the surface portion is 5.0 nm to 12 nm. 3. The number of surface pores per unit area [pieces / μm 2 ] as mentioned above Surface Divided by the average surface pore diameter [nm]: X is 30 to 100 pores / μm 2 3. The porous membrane according to claim 1 or 2, wherein the pore size is 1 / nm. 4. The porous membrane according to any one of 1 to 3, wherein the tortuosity R of the surface portion as represented by formula (1) is 1.0 to 8.0. R = (ε / 2k) 1 / 2 ·V / S ······································Formula (1) ε: Porosity k: Permeability coefficient [m 2 ] V: Pore specific volume [m 3 / g] S: Specific surface area [m 2 / g] where k is the permeability coefficient at 25°C and A is the membrane area at P [Pa]. 2 ] Pure water permeability: Q [cm 3 / sec] using formula (2) to calculate the coefficient k=8.76×Q / A / P×10 -15 ...Equation (2) 5. In the outermost surface portion from the surface of the surface portion to a thickness of 2 μm, the number of pores observed in a cross section of the outermost surface portion (hereinafter referred to as cross-sectional pores) per unit area is 100 pores / μm 2 ~1000 pieces / μm 2 and having a nanomesh structure in which the average cross-sectional pore diameter [nm] is 1 nm to 99 nm. 6. The number of holes per unit area [per μm 2 ] by the average cross-sectional pore diameter [nm]: Y is 3 to 10 pores / μm2 5. The porous membrane according to claim 5, wherein the pore size is 1 / nm. 7. The porous film according to 5 or 6, wherein the standard deviation of the cross-sectional pore diameter [nm] of the outermost surface portion is 1.0 nm to 50 nm. 8. The porous membrane according to any one of 2 to 7, wherein the standard deviation of the surface pore diameter [nm] of the surface portion is 0.5 nm to 5.0 nm. 9. The permeability coefficient k [m 2 ] is 0.5 × 10 -17 m 2 ~5.0×10 -17 m 2 9. The porous membrane according to any one of 4 to 8, wherein
[0011] 10. A method for producing a porous membrane, comprising: step (A): dissolving a polymer in a solvent to obtain a polymer solution; and then step (B): solidifying the polymer solution in a non-solvent to form a porous membrane, the step (A) comprising: The solvent contains a hydrogen bond solvent having a molecular weight of 500 Da or less and having hydrogen bond donor and hydrogen bond acceptor properties, and the polymer to be dissolved contains a polymer having hydrogen bond donor and / or hydrogen bond acceptor properties, The self-diffusion coefficient [m 2 / sec] is 0.8 × 10 -11 m 2 / sec~1.6×10 -11 m 2 / sec, and in step (B), the non-solvent contains 90 to 100% by weight of water and the temperature of the non-solvent is 6°C to 45°C. 11 The value obtained by dividing the number of moles of the hydrogen bond acceptor functional group contained in the hydrogen bond solvent in the step (A) by the number of moles of the hydrogen bond donor functional group contained in the polymer having hydrogen bond donor property and / or hydrogen bond acceptor property is 1.0 to 12. 10 2. A method for producing the porous membrane according to claim 1 . 12 The value obtained by dividing the number of moles of the hydrogen bond donor functional group contained in the hydrogen bond solvent in the step (A) by the number of moles of the hydrogen bond acceptor functional group contained in the polymer having hydrogen bond donor property and / or hydrogen bond acceptor property is 0.5 to 5.0. 10or 11 2. A method for producing the porous membrane according to claim 1 . 13 A method for filtering a liquid using a porous membrane described in any one of .1 to 9. Effect of the Invention
[0012] According to the present invention, it is possible to provide a porous membrane having excellent fouling resistance by removing coarse components on the outer surface of the porous membrane and allowing fine components to efficiently permeate the porous membrane. This makes it possible to filter the easily fouled filtrate with high accuracy, suppress clogging due to fouling, and maintain the filtration flux even during long-term use. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram showing the state of filtration using a porous membrane of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing the filtration state using a conventional porous membrane. [Diagram 3] FIG. 3 is a schematic diagram showing the filtration state using a conventional porous membrane. [Figure 4] FIG. 4 is a schematic diagram of the process for forming the porous membrane of the present invention. [Diagram 5] FIG. 5 is an electron microscope photograph showing a cross section (part) of a porous membrane according to one embodiment of the present invention. [Figure 6] FIG. 6 is an electron microscope photograph showing a cross section (part) of a porous membrane of the prior art. [Figure 7] FIG. 7 is a characteristic diagram showing the relationship between the number of surface pores and the dextran removal rate. [Figure 8] FIG. 8 is a characteristic diagram showing the relationship between the number of surface pores and the average surface pore diameter. [Figure 9] FIG. 9 is a characteristic diagram showing the relationship between the initial ratio of filtration flux and surface characteristics. [Figure 10] FIG. 10 is a characteristic diagram showing the relationship between the initial ratio of filtration flux and the self-diffusion coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings, but the present invention is not limited thereto. In this specification, "mass" and "weight" are synonymous. Furthermore, "filtrate stock" refers to the liquid to be filtered before permeating the porous membrane, and "permeate" refers to the liquid after permeating the porous membrane. Furthermore, the filtrate stock that is difficult to filter refers to a liquid that contains a large amount of contaminants that can clog the porous membrane. Contaminants are turbid matter, fungi, viruses, polysaccharides, proteins, organic compounds, and complexes thereof. The contaminants often contain coarse components (Stokes diameter: 13 nm or more) to be removed, and fine components (molecular weight: 10,000 Da or less) that are preferably permeated as useful materials, etc. Although the fine components should permeate the porous membrane, because they are fine, they are easily captured by the porous membrane and cause clogging. The porous membrane of the present invention exhibits high resistance to contamination even with a filtrate stock that contains a large amount of both coarse and fine components.
[0015] Concerning fouling resistance, fouling refers to the clogging of the porous membrane with coarse components (Stokes diameter: 13 nm or more) and fine components (molecular weight: 10,000 Da or less) contained in the raw filtrate during the filtration process. As the clogging of the porous membrane with coarse and fine components progresses, the filtration resistance increases and the amount of liquid that can pass through the porous membrane decreases.
[0016] In general, in order to remove the coarse components of the turbidity accumulated in the porous membrane from the pores, a fluid such as the permeate or compressed air is passed from the direction of the permeate to the direction of the raw filtrate, that is, back pressure washing is performed in the opposite direction to filtration to remove the coarse components captured in the porous membrane. In back pressure washing, it is easy to remove the coarse components that tend to accumulate outside the porous membrane, but it is difficult to remove the fine components that tend to accumulate inside the porous membrane. The improvement of the "fouling resistance" of the present invention makes the pores of the porous membrane less likely to be blocked, even if the raw filtrate contains coarse components and fine components, regardless of which component is used. The porous membrane with improved fouling resistance of the present invention will be described below.
[0017] <About porous membranes> The porous membrane according to the embodiment of the present invention has a surface portion having a thickness of 10 μm from the surface, which is denser than the inside, a dextran removal rate (T) of 60 to 95% having a weight-average molecular weight of 40,000 Da, and a surface pore number of 200 / μm. 2 ~2000 pieces / μm 2 The surface pores are pores observed on the surface of the surface portion.
[0018] FIG. 1 is a schematic diagram showing the filtration of a filtrate stock solution that is difficult to filter using the porous membrane of the present invention. FIG. 1 is a conceptual schematic diagram showing a part of a cross section of a porous membrane. A porous membrane 101 includes a surface portion 102 and an interior portion 103. The surface portion 102 has a denser structure than the interior portion 103. In FIG. 1, a solid line drawn on the surface portion 102 shows a schematic mesh structure. The filtration direction FL is the direction from the surface portion 102 to the interior portion 103. The filtration target of the filtrate stock solution contains coarse dirt components 201 and fine dirt components 202. The coarse dirt components 201 cannot penetrate into the porous membrane because the fine pores of the surface portion 102 are dense, and the surface portion 102 of the porous membrane is not blocked, making the porous membrane less susceptible to dirt. On the other hand, since a large number of pores are formed in the surface portion 102, minute dirt components 202 are dispersed and penetrate from the surface portion 102 of the porous membrane into the interior 103 in the filtration direction, making the porous membrane less susceptible to dirt.
[0019] That is, the surface portion from the surface to a thickness of 10 μm is denser than the inside, which prevents coarse dirt substances and objects to be removed in the filtrate from penetrating into the porous membrane, and shows high dirt resistance. The fact that the surface portion is denser than the inside can be confirmed by observing the cross section of the porous membrane at 10 μm thick areas with a scanning electron microscope (hereinafter referred to as "SEM") and finding that the porosity of the surface portion from the surface to a thickness of 10 μm is lower than the porosity of the inside portion 10 μm or more thick from the surface. To calculate the porosity, the image obtained by observing the cross section of the porous membrane with an SEM is binarized using the free software "ImageJ". When binarizing, create background as 1 pixel in Subtract Background, and then select the condition: Persentile in Threshold (binarization threshold). In the obtained binarized image, select Area in Analyze Particles to find the area of the pores, and divide it by the area of the observed porous membrane to calculate the porosity. The porosity of the surface portion should be smaller than that of the interior, and is preferably 55 to 90%, and more preferably 63 to 80%.
[0020] The surface portion being denser than the inside is preferable because it allows the coarse dirt components and objects to be removed held on the outside of the surface portion to be efficiently discharged from the porous membrane, particularly when a back pressure washing step in which filtration is performed in the reverse direction is performed during filtration. It is also preferable because it allows the coarse dirt components and objects to be removed held on the surface portion to be efficiently discharged from the porous membrane, particularly when a cross flow filtration step in which liquid is made to flow perpendicular to the filtration direction or a flushing step is performed during filtration.
[0021] The inventors discovered that in order to make it difficult for coarse components to be removed (Stokes diameter: 13 nm or more) to penetrate into the porous membrane, and to efficiently remove small amounts of coarse components that have penetrated the porous membrane from the porous membrane by back pressure washing, etc., it is necessary for the removal rate: T of dextran with a weight average molecular weight of 40,000 Da to be 60% or more. By specifying the removal rate of dextran with a specific molecular weight, it is possible to obtain a porous membrane with excellent fouling resistance, in which fouling substances are difficult to penetrate into the surface and fouling substances can be efficiently removed from the porous membrane by back pressure washing, etc.
[0022] The dextran removal rate: T is preferably 68% or more, and more preferably 70% or more. It has been found that when the dextran removal rate: T is 95% or less, fine components (molecular weight: 10,000 Da or less) that are not the target of removal but are preferably permeated are not captured in the porous membrane, and the fine components are sufficiently permeated, thereby exhibiting high anti-fouling properties. When the dextran removal rate: T is 95% or less, the permeation resistance of the porous membrane is easily reduced, and a high filtrate volume is exhibited. The dextran removal rate: T is more preferably 90% or less, and particularly preferably 85% or less. When the dextran removal rate: T for a weight-average molecular weight of 40,000 Da is 60 to 95%, coarse contaminants and objects to be removed in the filtrate stock solution are sufficiently prevented from penetrating into the membrane, and excellent anti-fouling properties are exhibited. The dextran removal rate: T is preferably 68 to 90%, more preferably 70 to 90%, and most preferably 70 to 85%.
[0023] The dextran removal rate (T) can be calculated by the following formula (3) using an aqueous dextran solution prepared at 25°C and containing 1,000 ppm of commercially available dextran with a weight-average molecular weight of 40,000 Da, and filtered through a porous membrane at a cross-flow linear velocity of 1.0 m / sec and a transmembrane pressure difference of 10 kPa. T = {(Refractive index of the original solution) - (Refractive index of the transmitted solution)} / (Refractive index of the original solution) × 100 Equation (3) Here, the cross-flow linear velocity is the flow rate of the raw liquid permeated in a direction perpendicular to the filtration direction divided by the cross-sectional area of the flow path, and the transmembrane pressure is the difference in pressure between the raw liquid permeated and the permeated liquid permeated across the porous membrane.
[0024] The number of surface pores observed on the surface of the porous membrane is 200 / μm 2 ~2000 pieces / μm 2 By having a surface pore size of 200 / μm, the contaminants in the raw solution can be dispersed within the porous membrane, and the membrane exhibits excellent fouling resistance. Furthermore, even if the contaminants in the raw solution block some of the surface pores as the filtration progresses, the large number of surface pores ensures a sufficient number of flow paths through which the raw solution can pass through the porous membrane, making it easy to exhibit excellent fouling resistance. 2 If the number of pores is more than 290, the flow path can be sufficiently secured before cleaning such as back pressure washing is performed, even if the filtrate is easily soiled. In addition, the filtrate reaches the pores on the surface of the porous membrane frequently, and tends to flow straight through the porous membrane. The number of pores on the surface of the porous membrane is 290 / μm. 2 ~1500 pieces / μm 2 More preferably, the number of particles is 350 / μm 2 ~1000 pieces / μm 2 It is particularly preferred that:
[0025] The number of surface pores in a porous membrane is the number of pores present within the plane when the surface of the porous membrane is observed. To find the number of surface pores in a porous membrane, the image obtained by observing the surface of the porous membrane with an SEM is binarized using the free software "ImageJ". When binarizing, create a background with 1 pixel in Subtract Background, then select the condition: Renyi Entropy in Threshold (binarization threshold). In the obtained binarized image, find the number of pores in the range observed with Analyze Particles. Number of surface pores per unit area [number / μm 2 To determine the area permeability, observe at least one thousand pores and divide the number of pores by the total area of the region observed.
[0026] Fig. 7 is a characteristic diagram showing the relationship between the number of surface pores and the dextran removal rate. The porous membrane of the prior art is shown in Fig. 7 as a comparative example (△ mark), and there is a trade-off between the number of surface pores, which tends to be high, the dextran removal rate, and conversely, the number of surface pores, which tends to be low, and high dextran removal rate, respectively. The porous membrane of the present invention is shown in Fig. 7 as an example (◯ mark), and there is a trade-off between the number of surface pores, which tends to be low, the dextran removal rate, and high dextran removal rate, and low dextran removal rate. 2 As described above, it is clear that the dextran removal rate is set to 60% or more. The porous membrane of the present invention overcomes the trade-off of the conventional technology, and achieves both a large number of surface pores and a high dextran removal rate, thereby exhibiting excellent stain resistance.
[0027] When the average value of the surface pore diameter [nm] of the surface part of the porous membrane is 5.0 nm to 12.0 nm, coarse dirt components and fine objects to be removed in the filtration stock solution are prevented from penetrating into the porous membrane, and high fouling resistance is easily exhibited, which is preferable. When the average value of the surface pore diameter [nm] is 12.0 nm or less, coarse components to be removed in the filtration stock solution (Stokes diameter: 13 nm or more) are prevented from penetrating into the porous membrane, and high fouling resistance is easily exhibited, which is preferable. When the average value of the surface pore diameter [nm] is 5.0 nm or more, fine components (molecular weight: 10,000 Da or less) that are not to be removed and are preferably allowed to permeate are not captured in the porous membrane, and high fouling resistance is easily exhibited, which is preferable. The average value of the surface pore diameter [nm] of the surface part is more preferably 5.0 to 9.0 nm, and particularly preferably 5.0 to 8.0 nm.
[0028] The surface pore size is the diameter of the pores present in the plane when the surface of the porous membrane is observed. To find the surface pore size of a porous membrane, the image obtained by observing the surface of the porous membrane with an SEM is binarized using the free software "ImageJ". When binarizing, create a background with 1 pixel in Subtract Background, and then select the condition: Renyi Entropy in Threshold (binarization threshold). In the obtained binarized image, select Area in Analyze Particles to find the area of each pore, and the diameter calculated assuming each pore is a circle is used as the surface pore size. The average surface pore size is found by averaging the pore sizes of more than 1,000 pores.
[0029] The number of surface pores on the surface of the porous membrane (sometimes abbreviated as the number of surface pores) divided by the average surface pore size: X is 30 to 100 pores / μm 2 / nm, it is preferable because it is possible to prevent coarse dirt components and removal objects in the filtrate from penetrating into the porous membrane while ensuring a sufficient number of flow paths through which the filtrate passes through the porous membrane, and therefore it is easy to show excellent dirt resistance. A large X means that there are many small pores. Usually, when the pore size is small, the ratio of polymers constituting the porous membrane tends to be high so as to fill the pores of the porous membrane, and therefore the number of pores tends to be small. As a result, as shown in the comparative example: △ in Figure 8, as the surface pore size becomes smaller, the number of surface pores also decreases, and there is a trade-off between the surface pore size and the number of surface pores.
[0030] As a result of intensive research, the inventors have found that small pores prevent coarse dirt components and objects to be removed in the raw filtrate from penetrating into the porous membrane, while large pores ensure a sufficient number of flow paths through which the raw filtrate passes through the porous membrane, and dirt components can be dispersed, making it easy to exhibit excellent dirt resistance. In other words, it is preferable from the viewpoint of dirt resistance to have both a good (small) surface pore size and a good (large) number of surface pores. Since the number of surface pores and the surface pore size both satisfy a positive correlation that makes them good, and both contribute to dirt resistance, it is preferable to use the X value that takes both into consideration as an index of dirt resistance. In addition, since the number of surface pores is negatively correlated with the surface pore size, it is preferable to use the X value divided by the surface pore size as an index rather than using only the number of surface pores as an index.
[0031] A porous membrane having such a large number of surface pores and a small surface pore diameter has not been obtained by conventional techniques. Fig. 9 shows the value X obtained by dividing the number of surface pores by the average surface pore diameter, and the initial ratio of filtration flux. The closer the initial ratio of filtration flux: F2 / F1 is to 1, the better the filtration for a long time. However, as shown in the examples and comparative examples, the porous membrane of the present invention has a value of X=30 to 100 pores / μm. 2 It has been shown that when the above F2 / F1 ratio is satisfied, good filtration with an F2 / F1 ratio of 0.50 or more can be maintained for a long period of time.
[0032] As described later, in the porous membrane of the present invention, the self-diffusion coefficient of the polymer is made relatively small in the process of forming the porous membrane, that is, the polymer is made less mobile, thereby suppressing the progress of excessive phase separation and coarsening, and the porous membrane is solidified in a state in which a large number of fine pores are present, making it easy to overcome the trade-off between pore size and number of pores. 2 / nm is preferable because it shows excellent stain resistance, and 32 to 80 particles / μm 2 / nm, and more preferably 50 to 70 / μm 2 It is particularly preferred that the thickness is 1 / nm.
[0033] The tortuosity ratio: R of 1.0 to 8.0 allows fine dirt components in the raw filtrate to pass through the porous membrane without clogging, and the porous membrane is likely to exhibit excellent dirt resistance, which is preferable. The tortuosity ratio is also called the bending degree, and means the degree to which the flow path through which the raw filtrate passes is bent. In other words, the lower the tortuosity ratio, the closer the flow path is to a straight line, and the dirt components pass through a short flow path, so that clogging is less likely to occur in the porous membrane. On the other hand, as shown in FIG. 3, the higher the tortuosity ratio, the more the flow path is bent, and the dirt components pass through a long flow path, so that clogging is more likely to occur in the porous membrane. Note that FIG. 3 is a schematic diagram showing the filtration state by a porous membrane of the prior art.
[0034] The tortuosity ratio: R is generally calculated based on the Kozeny-Carman formula, and is described, for example, in Journal of the Japanese Association for Petroleum Technology (Vol. 75, No. 2 (March, 2010) pp. 164-176). The tortuosity ratio: R is preferably 1.0 to 6.0, and more preferably 1.0 to 5.5. Here, when the tortuosity ratio: R is 1.0, it means that the pores are cylindrical and lie on a straight line.
[0035] In the present invention, the curvature ratio: R is calculated using the following formula (1). R = (ε / 2k) 1 / 2 ·V / S ······································Formula (1) ε: Porosity k: Permeability coefficient [m 2 ] V: Pore specific volume [m 3 / g] S: Specific surface area [m 2 / g] where k is the permeability coefficient at 25°C and A is the membrane area at P [Pa]. 2 ] Pure water permeability: Q [cm 3 / sec] using formula (2).
[0036] k=8.76×Q / A / P×10 -15 ...Equation (2) As mentioned above, the porosity: ε can be obtained by observing the cross section of the porous membrane from the surface to a depth of 10 μm using an SEM and analyzing the binarized image. The specific surface area: S and the specific pore volume: V can generally be measured by the BET method using a commercially available nitrogen adsorption measurement device. In addition, the permeability coefficient: k[m 2 ] is 0.5 × 10 -17 m 2 ~5.0×10 -17 m 2 From the viewpoint of stably obtaining good properties of the porous film, it is preferable that the above-mentioned range is satisfied.
[0037] The porous membrane sample to be used for the nitrogen adsorption measurement is prepared by collecting the surface of the porous membrane using a commercially available freezing microtome. After moving the porous membrane a certain distance in the microtome, the blade can be brought into contact with the porous membrane to cut it. The blade is set in a direction parallel to the surface of the porous membrane. First, the porous membrane is cut once by approaching the blade at intervals of 0.5 μm. After that, the moving distance is set to 10 μm and another cut is made, allowing the surface portion to be collected with a thickness of 10 to 10.5 μm from the surface.
[0038] The permeability coefficient k is calculated based on the formula (2) by filtering the entire amount of pure water through a porous membrane. The permeability coefficient k is 0.5×10 -17 ~5.0×10 -17 It is preferable that the ratio is 1.2×10 -17 ~5.0×10 -17 More preferably, it is 1.5×10 -17 ~5.0×10 -17 It is most preferable that the above formula (2) is used. Here, the membrane area A is the surface area of the porous membrane that is in contact with the raw filtrate. The pressure P is the above-mentioned transmembrane pressure difference. As described above, the surface portion of the porous membrane that is 10 μm thick from the surface is the densest, so the formula (2) is calculated assuming a surface thickness of 10 μm.
[0039] The surface of the porous membrane is such that the average cross-sectional pore diameter [nm] of the cross section of the most surface part from the surface to a thickness of 2 μm is 1 nm to 99 nm, and the number of cross-sectional pores is 100 / μm.2 ~1000 pieces / μm 2 Since the porous membrane has a nanomesh structure, it is preferable that the porous membrane exhibits excellent stain resistance. The cross-sectional pores refer to pores observed in the cross section of the outermost surface. Since the average cross-sectional pore diameter [nm] in the cross section of the outermost surface is as fine as 1 nm to 99 nm, it is easy to capture coarse stain components and objects to be removed in the filtrate at the outermost surface of the porous membrane and prevent them from penetrating into the porous membrane. Furthermore, when the number of cross-sectional pores is 100 / μm 2 ~1000 pieces / μm 2 Since the number of holes is large, the holes are formed vertically, horizontally, and in all directions, and the flow paths are easily connected in a straight line, that is, the tortuosity is low, and the porous membrane is less likely to become clogged when fine dirt components permeate it. In addition, even if some of the holes are clogged, the flow path for the filtrate to permeate the porous membrane can be secured, so the porous membrane is preferred because it tends to exhibit excellent resistance to dirt.
[0040] That is, referring again to FIG. 1, the surface portion 102 of the porous membrane has a dense structure, and has many pores, and the pores that extend three-dimensionally are connected vertically and horizontally. The pore diameter is smaller than 0.1 μm, and the number of pores is an ultra-high density nano-mesh structure. The fine dirt components 202 pass through any of the multiple connected pores without being captured by the resin part of the mesh structure. When passing fine components, the size of the pores of the porous membrane is adjusted according to the size of the fine components, but by forming many pores densely, the fine dirt components 202 are less likely to be captured by the mesh, so the more pores there are, the better, and it is preferable from the viewpoint of improving the dirt resistance and good permeability. Furthermore, since the porous membrane has many pores, that is, densely present, the lower the tortuosity, the shorter the shortest distance formed by several pores, and even if some of the pores are blocked, a flow path can be secured by another pore nearby, so that it is easier to maintain permeability from the viewpoint of small change in the tortuosity corresponding to the shortest distance.
[0041] The nanomesh structure of the present invention is characterized by a finer pore size and a larger number of pores than a general mesh structure. A general mesh structure has a coarse pore size and a smaller number of pores. For example, the mesh structure shown in the figure of Patent Document 1 has a pore size of 1 to 2 μm and a pore number of 0.1 / μm. 2 The pore size of the mesh structure in the example of Patent Document 2 is as small as 300 nm, and the number of pores is several tens per μm. 2 In contrast, in the nanomesh structure, the polymer resin portion forms a mesh, and as described above, each pore in the mesh is very small, and there are many dense pores.
[0042] In this way, the general mesh structure known so far has a large pore size, so that the large dirt components 201 penetrate into the inside of the porous membrane and easily cause clogging, and the small number of pores makes it difficult for the flow paths to be connected linearly, resulting in a high tortuosity and a long flow path through which the fine dirt components 202 pass, which makes them more likely to be captured in the porous membrane and cause clogging. A schematic diagram of the filtration of a filtrate that is difficult to filter using such a porous membrane is shown in Figure 2.
[0043] In FIG. 2, coarse dirt components 201 are not easily blocked by the surface layer 102, and tend to penetrate and remain in the porous membrane, causing clogging. Also, fine dirt components 202 tend to get caught in the mesh structure with a large pore size and high tortuosity, making it difficult for them to pass through the porous membrane and resulting in their retention in the porous membrane. Compared to FIG. 1, the coarse dirt components 201 and the fine dirt components 202 foul the porous membrane, making it difficult to maintain the filtration capacity for a long period of time.
[0044] The average cross-sectional pore size is more preferably 1.0 nm to 38 nm, and particularly preferably 1.0 to 36 nm. The number of cross-sectional pores is 120 to 800 / μm. 2 More preferably, the number of particles is 140 to 600 particles / μm 2 It is particularly preferred that:
[0045] The cross-sectional pore size of the porous membrane is obtained as follows. The cross-sectional sample for observation is obtained by embedding the porous membrane using a commercially available embedding agent for preparing frozen tissue sections, cutting the porous membrane at a thickness of 100 nm at low temperature using a freezing microtome, and vacuum drying at room temperature for 12 hours. The cross-section of the outermost surface of the porous membrane is observed with a transmission electron microscope (hereinafter, "TEM") to obtain an image, which is then binarized using the free software "ImageJ". When binarizing, select the condition: Minimum in Threshold (binarization threshold). In the obtained binarized image, select Area in Analyze Particles to obtain the area of each hole, and the diameter calculated assuming each hole to be a circle is used as the cross-sectional pore size. The average cross-sectional pore size is calculated by averaging the pore sizes of more than 1,000 pores. In addition, the number of cross-sectional pores is divided by the total area of the analyzed image to obtain the number of pores per unit area. As with the pore size, it is calculated by analyzing an image containing more than 1,000 pores.
[0046] The value obtained by dividing the number of cross-sectional pores on the outermost surface of the porous membrane by the average cross-sectional pore diameter: Y is 3 to 10 pores / μm 2 / nm, it is preferable that the number of flow paths through which the raw filtrate permeates the porous membrane is sufficiently secured while preventing coarse dirt components and removal objects in the raw filtrate from penetrating into the porous membrane. A large Y means that there are many small pores. As described above regarding the surface pores, when the cross-sectional pore size is small, the number of cross-sectional pores is likely to be small, and there is a trade-off between the pore size and the number of pores. As a result of intensive research, the inventors have found that even in the cross section of the outermost surface, the cross-sectional pores are small, preventing coarse dirt components and removal objects in the raw filtrate from penetrating into the porous membrane, and the cross-sectional pores are large, ensuring a sufficient number of flow paths through which the raw filtrate permeates the porous membrane, and dispersing the dirt components, so that the Y value is likely to show excellent dirt resistance. The number of cross-sectional pores and the cross-sectional pore size are correlated, and both contribute to dirt resistance, so it is preferable to use the Y value taking both into consideration as an index of dirt resistance. In addition, since the number of cross-sectional pores is negatively correlated with the cross-sectional pore diameter, it is preferable to use the Y value divided by the cross-sectional pore diameter as an index rather than using only the number of cross-sectional pores as an index. The porous membrane of the present invention has a Y value of 3 to 10 pores / μm, which is higher than the usual trade-off relationship.2 / nm is preferable because it shows excellent stain resistance, and 4 to 10 particles / μm 2 / nm, and more preferably 5 to 10 / μm 2 It is particularly preferred that the thickness is 1 / nm.
[0047] At the outermost surface of the porous membrane, the standard deviation of the cross-sectional pore size [nm] is 1.0 nm to 50 nm, which can make the load of fouling substances on the porous membrane uniform and is easy to show excellent fouling resistance, and is preferable. The standard deviation of the cross-sectional pore size is more preferably 1.0 nm to 35 nm. The standard deviation of the cross-sectional pore size can be calculated by binarizing and analyzing the TEM image of the cross-section of the porous membrane as described above to obtain data on each cross-sectional pore size.
[0048] The standard deviation of the surface pore size [nm] of the surface part of the porous membrane is preferably 0.5 to 5.0 nm, since the load of the fouling substance on the porous membrane can be uniform, and the membrane is more likely to exhibit excellent fouling resistance. The smaller the standard deviation of the surface pore size, the smaller the variation in the pore size, but it is more preferably 0.5 to 4.0 nm, and even more preferably 0.5 to 3.0 nm. The standard deviation of the surface pore size can be calculated by binarizing and analyzing the SEM image of the surface of the porous membrane as described above to obtain data on each surface pore size.
[0049] <About the manufacturing method of the porous membrane> The porous membrane of the present invention comprises a step (A): a step of dissolving a polymer in a solvent to obtain a polymer solution, and then a step (B): a porous membrane formation step of solidifying the polymer solution in a non-solvent to form a porous membrane, and in the polymer solution obtained in the step (A), the self-diffusion coefficient [m 2 / sec] is 0.8 × 10 -11 m 2 / sec~1.6×10 -11 m 2 / sec, the non-solvent used in step (B) contains 90 to 100% by weight of water, and the temperature of the non-solvent is 6°C to 45°C.
[0050] The type of polymer used in step (A) is not particularly limited, and specific examples include polysulfone resins, polyethersulfone resins, polyvinylidene fluoride resins, nylon, cellulose esters such as cellulose acetate and cellulose acetate propionate, fatty acid vinyl esters, polyvinyl alcohol, polyvinyl acetate, polyvinylpyrrolidone, acrylic acid esters or methacrylic acid esters such as ethylene oxide, propylene oxide or polymethyl methacrylate, or copolymers thereof.
[0051] In particular, in order to use the porous membrane for long-term filtration, it is preferable to periodically clean accumulated dirt components with chemicals, and it is particularly preferable to include a polyvinylidene fluoride resin with excellent chemical resistance. The polyvinylidene fluoride resin refers to a homopolymer of vinylidene fluoride or a copolymer of vinylidene fluoride. Here, the copolymer of vinylidene fluoride refers to a polymer having a vinylidene fluoride residue structure. The polymer having a vinylidene fluoride residue structure is typically a copolymer of a vinylidene fluoride monomer and other fluorine-based monomers. Examples of such fluorine-based monomers include vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, and trifluorochloroethylene. In the copolymer of vinylidene fluoride, ethylene other than the fluorine-based monomers may be copolymerized to an extent that does not impair the effects of the present invention.
[0052] The polyvinylidene fluoride resin is more preferably contained in an amount of 50% by weight or more, and particularly preferably contained in an amount of 60% by weight or more, when the weight of the porous membrane is taken as 100%. The weight-average molecular weight of the polymer is preferably 50 to 1,000,000 Da, which makes it easier to control the self-diffusion coefficient described below to a relatively slow range within an appropriate range. A mixture of multiple polymers may be used. The solvent preferably contains a good solvent. Here, the term "good solvent" refers to a solvent that can dissolve 5% by weight or more of the polymer even in a low temperature range of 60°C or less. Examples of good solvents include N-methyl-2-pyrrolidone (hereinafter, "NMP"), 2-pyrrolidone (hereinafter, "2P"), ε-caprolactam (hereinafter, "ε-CL"), dimethylacetamide, dimethylformamide, methyl ethyl ketone, acetone, tetrahydrofuran, tetramethylurea, trimethyl phosphate, or a mixture thereof. The good solvent is more preferably contained in an amount of 40% by weight or more, and particularly preferably contained in an amount of 60% by weight or more, of the solvent. By containing a large amount of good solvent, the polymer chains spread in the polymer solution, and the self-diffusion coefficient described later is relatively slow, and it is easy to control it to an appropriate range, so it is preferable. Here, the "non-solvent" in step (B) refers to a solvent that does not dissolve or swell the polymer even when the non-solvent is heated to a high temperature up to the boiling point. Examples of the non-solvent include water, hexane, pentane, benzene, toluene, methanol, ethanol, carbon tetrachloride, o-dichlorobenzene, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, and low molecular weight polyethylene glycol, and other aliphatic hydrocarbons, aromatic hydrocarbons, aliphatic polyhydric alcohols, aromatic polyhydric alcohols, chlorinated hydrocarbons, other chlorinated organic liquids, and mixtures thereof.
[0053] The polymer concentration (wt%) in the polymer solution is preferably equal to or higher than the entanglement concentration in order to control the self-diffusion coefficient within an appropriate range, and more specifically, 10 to 40 wt% is preferred, 12 to 30 wt% is even more preferred, and 15 to 25 wt% is particularly preferred. It has been found that a polymer concentration of 10 wt% or more can relatively slow down the self-diffusion coefficient, and can coagulate in a state in which the pores in the porous membrane are fine and present in large quantities. The polymer concentration is more preferably 12 wt% or more, and particularly preferably 15 wt% or more. In addition, by setting the polymer concentration to 40 wt% or less, the proportion of the polymer in the porous membrane can be reduced, and the number of pores can be sufficiently secured. The polymer concentration is more preferably 30 wt% or less, and particularly preferably 25 wt% or less.
[0054] The porous membrane formation process in step (B), in which the polymer solution is solidified in a non-solvent to form a porous membrane, is a process for forming a porous membrane by so-called non-solvent-induced phase separation. When the polymer solution comes into contact with the non-solvent, the polymer cannot be completely dissolved in the solvent, and the phase separates into a phase containing a large amount of polymer and a phase containing a large amount of solvent, and each phase coarsens while merging with the same phase around it.
[0055] Figure 4 is a schematic diagram showing the porous membrane formation process in step (B). Phase separation progresses in the polymer solution in the order of Figure 4(a) to (f), and the areas with high polymer concentration (phase 301 containing a large amount of polymer) become coarse. In this phase separation and / or coarse-graining process, the exchange of the solvent and non-solvent progresses, and when the concentration of the non-solvent becomes higher than a certain level, the polymer solidifies and the structure of the porous membrane is fixed. At this time, the phase 302 containing a large amount of solvent becomes the pores of the porous membrane.
[0056] As a result of intensive research, the inventors have found that in the production of the porous membrane of the present invention, the self-diffusion coefficient of the polymer is set to a relatively low range of 0.8 × 10 -11 m 2 / sec~1.6×10 -11 m 2 / sec, it was found that excessive phase separation and coarsening could be suppressed, and the polymer-rich phase 301 and the solvent-rich phase 302 could be solidified in a state in which they exist in fine and large quantities. -11 m 2 / sec or more, the polymer and the solvent have a sufficient diffusion coefficient for phase separation, and pores are easily formed. If the diffusion of the polymer is so slow that phase separation is difficult, pores are difficult to form. -11 m 2 / sec or less, excessive phase separation and coarsening are suppressed, and the coalescence of pores is suppressed, making it easier to form many micropores. In other words, by appropriately controlling the self-diffusion coefficient of the polymer within a relatively low range, it is possible to form a porous film with many micropores. The self-diffusion coefficient is 0.8×10 -11 m 2 / sec~1.4×10 -11 m 2 / sec is more preferably 0.8×10 -11 m 2 / sec~1.1×10 -11 m 2 It is even more preferable that the .mu.m / sec.
[0057] The self-diffusion coefficient can be determined by all-atom molecular dynamics calculations. All-atom molecular dynamics calculations are a method for determining the trajectory of each atom by solving the equation of motion of a molecular group system for all of the constituent atoms one by one. First, a polymer solution system is created to have the polymer concentration (weight %) that will actually be used. At this time, a single model polymer chain is modeled so that its molecular weight is 800 to 6000 and 1 / 200 to 1 / 5 of the weight average molecular weight of the polymer that will actually be used. Potential parameters used in molecular dynamics calculations can be well-known parameters such as those from DREIDING [SL Mayo, BD Olafson, WA Goddard III, J. Phys. Chem. 94, 8897 (1990)], GAFF [J. Wang, RM Wolf, JW Caldwell, PA Kollman, DACase, J. Comput. Chem. 25, 1157 (2004)], OPLS-AA [WL Jorgensen, DS Maxwell, Julian Tirado-Rives, J. Am. Chem. Soc. 118, 11225 (1996)], and CHARMM [BR Brooks, RE Bruccoleri, BD Olafson, DJ States, S. Swaminathan, M. Karplus, J. Comput. Chem. 4, 187 (1983)], but parameters that reproduce density and cohesive energy, which are physical quantities that represent the aggregation state of a solution system, are preferred.
[0058] As a result of the inventors' investigation into the reproducibility of the aggregated state, it was found that it is particularly preferable to use GAFF or OPLS-AA. In addition, a constant pressure-temperature ensemble is constructed by controlling the temperature to 25°C using the Nose-Hoover method [Hoover, WG Phys. Rev. A, 31, 1695 (1985)] and the pressure to 1 bar using the Andersen method [HC Andersen, J. Chem. Phys. 72, 2384 (1980)]. At this time, the short-range Lennard-Johns interaction is handled by applying a switch function from 1.0 nm and cutting off at 1.2 nm, and the long-range electrostatic interaction is calculated using the Particle Mesh Ewald method. After performing molecular dynamics calculations in the constant pressure-temperature ensemble until the density becomes constant, the unit cell length is adjusted to obtain the average density, and an additional calculation of 11 ns is performed in the constant temperature ensemble. Using a 10 ns trajectory, the mean square displacement (MSD) of each atom of the polymer is obtained, and the self-diffusion coefficient of the polymer is calculated from the following formula (4). At this time, it is confirmed that the range of MSD and t used to calculate D is within the range of 0.9 to 1.1, where log(MSD) divided by log(t). When multiple types of polymers are mixed to make a polymer solution, the self-diffusion coefficient of the polymer in the polymer solution is determined by taking the weighted average of the self-diffusion coefficients of each polymer, based on the weight percentage of the polymer. D = MSD / 6t (4) D: self-diffusion coefficient t: time.
[0059] In the production of the porous membrane of the present invention, when the non-solvent used for coagulation contains 90 to 100% by weight of water, coagulation is rapid and the self-diffusion coefficient in the polymer solution is likely to affect the speed of phase separation and coarsening. In other words, the effect of controlling the self-diffusion coefficient in the polymer solution to a relatively low range is easily obtained. Furthermore, when the temperature of the non-solvent is 6°C to 45°C, coagulation is rapid and the self-diffusion coefficient in the polymer solution is likely to affect the speed of phase separation and coarsening. The temperature of the non-solvent is more preferably 10°C to 35°C, and even more preferably 15°C to 30°C.
[0060] In the above-mentioned step (A) of the production of the porous membrane of the present invention, the solvent contains a hydrogen bond solvent having a molecular weight of 500 Da or less and hydrogen bond donor and hydrogen bond acceptor properties, which is preferable because it is easy to control the self-diffusion coefficient of the polymer to an appropriate range. Having hydrogen bond donor properties means having positively polarized hydrogen atoms, specifically, having a hydroxyl group (OH group), a carboxyl group (COOH group), an amino group (NH group), etc. Having hydrogen bond acceptor properties means having a lone electron pair, specifically, having a carbonyl group, an alkoxy group, a cyano group, etc. When the solvent has hydrogen bond donor properties and hydrogen bond acceptor properties, the interaction due to hydrogen bonds between the solvents is strong, which suppresses the movement of the solvated polymer, and it is easy to control the self-diffusion coefficient of the polymer to a relatively slow, appropriate range. The hydrogen bond donor and hydrogen bond acceptor solvents are not particularly limited, but specific examples include 2P, ε-CL, 1,3-dimethylurea, N-methylacetamide, hydantoin, 2-imidazolidinone, DL-pyroglutamic acid, and the like.
[0061] In the above-mentioned step (A), the polymer to be dissolved preferably contains a polymer having hydrogen bond donor properties and / or hydrogen bond acceptor properties, which makes it easier to control the self-diffusion coefficient of the polymer within an appropriate range. When the polymer has hydrogen bond donor properties and / or hydrogen bond acceptor properties, it interacts with the solvent having hydrogen bond donor properties and hydrogen bond acceptor properties through hydrogen bonds, making it easier to control the self-diffusion coefficient of the polymer to a relatively slow, appropriate range. It is more preferable that the polymer having hydrogen bond donor properties and / or hydrogen bond acceptor properties is contained in an amount of 10% by weight to 50% by weight of the porous membrane, from the viewpoint of controlling the self-diffusion coefficient of the polymer within an appropriate range.
[0062] Furthermore, when the value obtained by dividing the number of moles of the hydrogen bond acceptor functional group contained in the solvent in the above-mentioned step (A) by the number of moles of the hydrogen bond donor functional group contained in the polymer having hydrogen bond donor property and / or hydrogen bond acceptor property is 1.0 to 12, the hydrogen bond between the polymer and the solvent is in an appropriate range, and the self-diffusion coefficient of the polymer is relatively slow and easy to control in an appropriate range. The value is more preferably 2.0 to 9.0, and particularly preferably 5.4 to 8.0.
[0063] When the value obtained by dividing the number of moles of the hydrogen bond donor functional group contained in the solvent in the above-mentioned step (A) by the number of moles of the hydrogen bond acceptor functional group contained in the polymer having hydrogen bond donor property and / or hydrogen bond acceptor property is 0.5 to 5.0, the hydrogen bond between the polymer and the solvent is in an appropriate range, and the self-diffusion coefficient of the polymer is relatively slow and easy to control in an appropriate range. The value is more preferably 1.5 to 2.3, and particularly preferably 1.8 to 2.3.
[0064] The porous membrane of the present invention may further comprise other layers. In that case, it is preferable that the porous membrane of the present invention is disposed on the surface portion. By disposing the porous membrane of the present invention on the surface portion, the components contained in the filtrate are less likely to penetrate into the inside of the porous membrane, and high permeability can be maintained for a long period of time. The other layer is not particularly limited as long as it is a component that can be overlapped with the porous membrane to form a layered structure, but it is preferable that the other layer is a support. Here, the "support" refers to a structure that has a higher breaking strength than the porous membrane for physically reinforcing the porous membrane. In order to increase the breaking strength of the support, the breaking strength (breaking strength per unit area) of the support is preferably 3 MPa or more, more preferably 10 MPa or more. In addition, when the composite membrane in which the other layer and the porous membrane of the present invention are arranged in layers is in the form of a hollow fiber, the breaking strength of the support is preferably 300 gf or more, more preferably 800 gf or more. EXAMPLES
[0065] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. First, measurement methods and evaluation methods are described below.
[0066] (i) Measurement of porosity The surface of the porous membrane was sampled using a commercially available freezing microtome and used for observation. In the microtome, the porous membrane can be cut by moving it a certain distance and then contacting the blade with the porous membrane. The porous membrane immersed in distilled water was frozen at -20°C using a freezing microtome (Leica; Jung CM3000), and the blade was placed perpendicular to the surface of the porous membrane. First, the porous membrane was cut once by moving the blade close to it at 30 μm intervals to obtain a section. The section was vacuum dried at 25°C for 12 hours. The cross section of the porous membrane was observed continuously in 10 μm areas in the thickness direction of the porous membrane using a SEM (HITACHI; SU-1510), and the porosity of each area was calculated. To calculate the porosity, the image obtained by SEM observation of the cross section of the porous membrane was binarized using the free software "ImageJ". When binarizing, we created a background with 1 pixel in Subtract Background, then selected Persentile as the Threshold (binarization threshold). In the obtained binarized image, we selected Area in Analyze Particles to obtain the area of the pores, and divided it by the total area of the observation region of the porous membrane to calculate the porosity as a percentage.
[0067] (ii) Permeability coefficient The entire amount of pure water at 25°C is filtered through the porous membrane, and the permeability coefficient: k [m 2 ] was calculated. Here, the membrane area: A [m 2 ] is the surface area of the porous membrane in contact with the raw filtrate. The pressure: P [Pa] is the transmembrane pressure difference mentioned above. Here, the permeability coefficient is calculated for a thickness of 10 μm, taking into account the thickness [m] of the densest surface part of the porous membrane. k=8.76×Q / A / P×10 -15 ...Equation (2).
[0068] (iii) Measurement of specific pore volume and specific surface area The surface of the porous membrane was sampled using a commercially available freezing microtome (Jung CM3000, manufactured by Leica). The porous membrane was immersed in distilled water and frozen at -20°C using a freezing microtome (Jung CM3000, manufactured by Leica), and the blade was placed parallel to the surface of the porous membrane. First, the porous membrane was cut once by moving the blade close to it at intervals of 0.5 μm. Then, the moving distance was set to 10 μm and cutting was performed once more to sample a surface portion 10 to 10.5 μm thick from the surface. The slices of the obtained surface portion were measured for the specific pore volume: V [m by the BET method using a commercially available nitrogen adsorption measuring device (BELSORP-miniII, manufactured by Microtrack Bell). 3 / g] and specific surface area S [m 2 / g] was measured.
[0069] (iv) Curvature ratio The porosity calculated in (i) was used for a region 10 μm thick from the surface of the porous membrane, and the tortuosity ratio: R was calculated by substituting the permeability coefficient, specific pore volume, and specific surface area calculated in (ii) and (iii) into equation (1). R = (ε / 2k) 1 / 2 ·V / S ···································Formula (1).
[0070] (v) Method for evaluating the removal rate of dextran with a weight-average molecular weight of 40,000 Da Dextran (manufactured by Aldrich; weight-average molecular weight 40,000 Da) was mixed with 1000 ppm distilled water to prepare an aqueous dextran solution. The prepared aqueous dextran solution was supplied to a porous membrane at 25°C so that the transmembrane pressure difference was 10 kPa, and cross-flow filtration was performed at a cross-flow linear velocity of 1.0 m / sec, and the permeate was sampled. At the same time that the permeate was sampled, the aqueous dextran solution (stock solution) supplied to the porous membrane was sampled. The refractive indexes of the permeate and stock solution were measured, and the removal rate: T (%) was calculated based on formula (3). T = {(Refractive index of original solution) – (Refractive index of transmitted solution)} / (Refractive index of original solution) × 100 Equation (3).
[0071] (vi) Surface structure of the surface area (pore size, number, standard deviation) After vacuum drying the porous membrane for 12 hours at 25°C, it was observed at a magnification of 30,000 to 100,000 times using a SEM (Hitachi High-Technologies Corporation; S-5500). The image obtained by observing the surface of the porous membrane with the SEM was binarized using the free software "ImageJ". When binarizing, after creating a background with 1 pixel in Subtract Background, the condition: Renyi Entropy was selected in Threshold (binarization threshold). In the obtained binarized image, the area of each surface pore was obtained by selecting Area in Analyze Particles, and the diameter calculated assuming each surface pore to be a circle was used as the surface pore size. When calculating the average surface pore size, the surface pore sizes of more than 1,000 pores were averaged. Similarly, the standard deviation was calculated from the data of each surface pore size. The number of surface pores was divided by the total area of the observed region to obtain the number of surface pores per unit area.
[0072] (vii) Cross-sectional structure of the outermost surface (presence or absence of nanomesh structure, pore size, number, standard deviation) The porous membrane was embedded in a commercially available embedding medium for frozen tissue sectioning (OCT compound, Tissue-Tec), and a 100-nm-thick section was taken perpendicular to the surface of the porous membrane at -40°C using a cryo-ultramicrotome (FC7, Leica). The section was then vacuum-dried at room temperature for 12 hours. The cross section of the outermost surface of the porous membrane was observed with a TEM (JEM-1400Plus, JEOL Ltd.), and images were obtained and binarized using the free software "ImageJ." When binarizing, the condition: Minimum was selected for Threshold (binarization threshold). In the obtained binarized image, the area of each cross-sectional hole was calculated by selecting Area in Analyze Particles, and the diameter calculated assuming each cross-sectional hole to be a circle was used as the cross-sectional hole diameter.
[0073] When calculating the average cross-sectional pore size, the cross-sectional pore sizes of 1,000 or more cross-sectional pores are averaged. The number of cross-sectional pores per unit area is calculated by dividing the number of cross-sectional pores by the total area of the analyzed region. In this case, as with the surface pore size, the calculation is performed by analyzing an image containing 1,000 or more pores. Similarly, the standard deviation was calculated from the data of each cross-sectional pore size. Within the surface portion of the porous membrane, the outermost surface portion from the surface to a thickness of 2 μm has an average cross-sectional pore size [nm] of 1 nm to 99 nm in the cross section of the outermost surface portion, and the number of cross-sectional pores is 100 / μm. 2 ~1000 pieces / μm 2 When the mesh structure was larger than 100 nm, it was judged to have a nano-mesh structure.
[0074] (viii) Self-diffusion coefficient of polymer The self-diffusion coefficient was determined by all-atom molecular dynamics calculations. A polymer solution system was prepared to have the polymer concentration (wt%) actually used. At this time, one model polymer chain was modeled to have a molecular weight of 800 to 6000 and 1 / 200 to 1 / 5 of the weight-average molecular weight of the polymer actually used. GAFF2 was used as the potential parameter for the molecular dynamics calculation. A constant pressure-temperature ensemble was constructed by controlling the temperature to 25°C and the pressure to 1 bar. At this time, the short-range Lennard-Johns interaction was handled by applying a switch function from 1.0 nm and cutting off at 1.2 nm, and the long-range electrostatic interaction was calculated using the Particle Mesh Ewald method. After performing molecular dynamics calculations in the constant pressure-temperature ensemble until the density became constant, the unit cell length was adjusted to obtain the average density, and an additional calculation of 11 ns was performed in the constant temperature ensemble. The mean square displacement (MSD) of each atom of the polymer was obtained using the 10 ns trajectory, and the self-diffusion coefficient was calculated from the following equation (4). In this case, it was confirmed that the range of MSD and t used in calculating D was 0.9 to 1.1, where log(MSD) divided by log(t). When multiple types of polymers were mixed to prepare a polymer solution, the self-diffusion coefficient of each polymer was weighted-averaged based on the weight percentage of the polymer, and this was regarded as the self-diffusion coefficient of the polymer in the polymer solution.
[0075] D = MSD / 6t (4) D: self-diffusion coefficient t: time.
[0076] (ix) Filtration evaluation method for gelatin aqueous solution Gelatin (Gelatin Silver, manufactured by Nitta Gelatin Co., Ltd.) was mixed with 1000 ppm distilled water to prepare an aqueous gelatin solution. The prepared aqueous gelatin solution was supplied to a porous membrane at 60°C so that the transmembrane pressure difference was 120 kPa, and cross-flow filtration was performed at a cross-flow linear velocity of 1.0 m / sec, and the permeate was sampled. At the same time that the permeate was sampled, the aqueous gelatin solution (stock solution) supplied to the porous membrane was sampled. The refractive indexes of the permeate and stock solution were measured, and the removal rate (%) was calculated based on formula (5): T ゼラチン The amount of permeated liquid was 20 L / m 2 Filtration flux (L / m 2 / h) was calculated. T ゼラチン = {(Absorbance at 292 nm of original solution) - (Absorbance at 292 nm of permeated solution)} / (Absorbance at 292 nm of original solution) × 100 Equation (5).
[0077] (x) Apple juice filtration evaluation method Apple juice (manufactured by Ichiryu Co., Ltd.; fully ripe apple juice) was supplied to the porous membrane at 25°C so that the transmembrane pressure difference was 100 kPa, and the entire amount was filtered, and the permeated liquid was sampled. At the same time that the permeated liquid was sampled, the apple juice (undiluted liquid) supplied to the porous membrane was also sampled. The turbidity of the permeated liquid and the undiluted liquid was measured, and the removal rate (%) was calculated based on the formula (6): T りんご The amount of permeated liquid was 6 L / m 2 The filtration flux at this time was calculated. T りんご = {(Turbidity of original solution) - (Turbidity of permeated solution)} / (Turbidity of original solution) × 100 Equation (6).
[0078] (xi) Filtration evaluation method for industrial wastewater Wastewater from a chemical plant (TOC: 30 mg / L, turbidity: 11 NTU) was fed to the porous membrane at 25°C so that the transmembrane pressure difference was 100 kPa, and the entire amount was filtered, and the permeated liquid volume was measured.2 When this occurs, the reverse filtration permeation rate is 3 L / m so that the transmembrane pressure difference is 150 kPa. 2 Filtration and backfiltration were repeated until the filtration flux (F1) immediately after the start of filtration and the amount of permeated liquid per unit area reached 400 L / m 2 The ratio of the filtration flux (F2) to the filtration flux immediately after the start of filtration after reaching the above value (F1 / F2) was calculated and used as the initial ratio of the filtration flux. The closer the initial ratio of the filtration flux is to 1, the more the initial characteristics are maintained, and the porous membrane is less likely to clog even after long-term use. A guideline for maintaining good filtration is 0.50 or more.
[0079] Example 1 The porous membrane used was a hollow fiber porous membrane containing a support obtained by the following manufacturing method. 38% by mass of PVDF (Kureha Corporation; KF1300, weight average molecular weight 350,000 Da) and 62% by mass of γ-butyrolactone were mixed and dissolved at 160°C to prepare a support membrane stock solution. This support membrane stock solution was discharged from a double-tube nozzle while accompanying an 85% by mass γ-butyrolactone aqueous solution as a hollow part forming liquid. The discharged support membrane stock solution was solidified in a cooling bath containing an 85% by mass γ-butyrolactone aqueous solution at a temperature of 20°C installed 30 mm below the nozzle, to prepare a hollow fiber support having a spherical structure.
[0080] A polymer solution having the composition shown in Table 1 was prepared by mixing 12% by mass of PVDF1 (Arkema Corporation; "Kynar" (registered trademark) 710, weight average molecular weight 180,000 Da), 4.8% by mass of cellulose diacetate (Eastman Corporation; CA-398-3), 2.4% by mass of cellulose triacetate (Eastman Corporation; CA-436-80S), 68.8% by mass of NMP, and 12% by mass of 2P and stirring at 120°C for 4 hours.
[0081] Next, the polymer solution was uniformly applied to the outer surface of the hollow fiber support at 10 m / min (thickness 50 μm). The support to which the polymer solution was applied was taken up at 10 m / min, and 1 second after application, it was passed through a coagulation bath of distilled water at 25° C. for 10 seconds to be immersed, and coagulated to form a porous membrane having a three-dimensional mesh structure. The evaluation results of the obtained porous membrane are shown in Table 1. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. An image of the cross section of the outermost surface portion of the porous membrane observed by TEM is shown in FIG. 5. It was determined to have a nanomesh structure from the cross-sectional pore diameter and the number of cross-sectional pores. The tortuosity: R of the obtained porous membrane was 4.9, the dextran removal rate: T was 72%, and the number of surface pores: 444 / μm 2 The number of surface pores divided by the average surface pore diameter: X is 62 / μm 2 / nm, which was good. Furthermore, (xi) the long-term stability was evaluated using the industrial wastewater filtration evaluation method, and the permeate volume was 400 L / m 2 The initial ratio (F2 / F1) of the filtration flux after (F2) and immediately after the start of filtration (F1) was 0.63. The filtration flux was maintained even after long-term use. The evaluation results are shown in Table 1.
[0082] Example 2 A porous membrane was obtained by the same membrane production as in Example 1, except that 2P in the polymer solution was changed to ε-CL. The evaluation results of the porous membrane are shown in Table 1. The surface portion of the porous membrane up to a thickness of 10 μm from the surface was denser than the inside. The tortuosity of the obtained porous membrane: R was 4.1, the dextran removal rate: T was 65%, and the number of surface pores: 291 / μm. 2 The number of surface pores divided by the average surface pore diameter: X is 33 / μm 2 (xi) In the evaluation method for filtration of industrial wastewater, the filtration flux ratio (F2 / F1) was 0.58, and the filtration flux was maintained even after long-term use.
[0083] Example 3 A porous membrane was obtained in the same manner as in Example 1, except that the composition ratio in the polymer solution was changed as shown in Table 1. The evaluation results of the porous membrane are shown in Table 1. The surface portion of the porous membrane up to a thickness of 10 μm from the surface was denser than the inside. The tortuosity of the obtained porous membrane: R was 5.9, the dextran removal rate: T was 72%, and the number of surface pores: 329 / μm 2 The number of surface pores divided by the average surface pore diameter: X is 46 / μm 2 (xi) In the evaluation method for filtration of industrial wastewater, the filtration flux ratio (F2 / F1) was 0.55, and the filtration flux was maintained even after long-term use.
[0084] Example 4 A porous membrane was obtained by the same membrane production as in Example 1, except that the composition ratio in the polymer solution was changed as shown in Table 1. The porous membrane had a nanomesh structure. The evaluation results of the porous membrane are shown in Table 1. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. The tortuosity of the obtained porous membrane: R was 4.9, the dextran removal rate: T was 69%, and the number of surface pores: 420 / μm. 2 The number of surface pores divided by the average surface pore diameter: X is 58 / μm 2 (xi) In the evaluation method for industrial wastewater filtration, the filtration flux ratio (F2 / F1) was 0.62, and the filtration flux was maintained even after long-term use.
[0085] Example 5 (ix) The filtration performance of the porous membrane was evaluated using the gelatin aqueous solution filtration evaluation method. The porous membrane of Example 1 was used as a representative. When the gelatin aqueous solution was filtered, the gelatin removal rate: T ゼラチン is 65%, and the filtration flux is 70 L / m 2 The results of the evaluation of the filtration of the gelatin solution are shown in Table 3. The tortuosity of the porous membrane used in the evaluation was 4.9, the dextran removal rate was 72%, and the number of surface pores was 444 / μm. 2 The number of surface pores divided by the average surface pore diameter: X is 62 / μm 2 / nm.
[0086] Example 6 (x) The filtering property of the porous membrane was evaluated using the apple juice filtering evaluation method. The porous membrane of Example 1 was used as a representative. When the apple juice was filtered, the removal rate of the apple juice: T りんご is 99.9%, and the filtration flux is 37 L / m 2 The filtration rate of apple juice was good, at 1.2 / h. The results of the evaluation are shown in Table 4. The tortuosity of the porous membrane used in the evaluation was 4.9, the dextran removal rate was 72%, and the number of surface pores was 444 / μm. 2 The number of surface pores divided by the average surface pore diameter: X is 62 / μm 2 / nm.
[0087] Comparative Example 1 A porous membrane was obtained by the same membrane production as in Example 1, except that all the solvents in the polymer solution were changed to NMP and the composition ratio was changed. The evaluation results of the porous membrane are shown in Table 2. The porous membrane did not have a nanomesh structure. The surface part of the porous membrane from the surface to a thickness of 10 μm was denser than the inside, but the number of surface pores and the dextran removal rate: T did not satisfy the conditions. (xi) In the method for evaluating the filtration of industrial wastewater, the initial filtration flux ratio (F2 / F1) was 0.45, and after long-term use, the filtration flux decreased to less than half.
[0088] Comparative Example 2 A porous membrane was obtained by the same membrane production as in Comparative Example 1, except that the PVDF1 in the polymer solution was replaced with PVDF2 (Arkema: HSV900, melt viscosity 4700 Pa s) and the composition ratio was changed. The evaluation results of the porous membrane are shown in Table 2. The surface part of the porous membrane from the surface to a thickness of 10 μm was denser than the inside, but the number of surface pores and the dextran removal rate: T did not satisfy the conditions. (xi) In the method for evaluating the filtration of industrial wastewater, the initial filtration flux ratio (F2 / F1) was 0.40, and the filtration flux significantly decreased after long-term use.
[0089] Comparative Example 3 A porous membrane was obtained by the same membrane production as in Comparative Example 1, except that PVDF1 in the polymer solution was changed to PVDF3 (Solef9009 manufactured by Solvay). The evaluation results of the porous membrane are shown in Table 2. The porous membrane did not have a nanomesh structure. The surface part of the porous membrane from the surface to a thickness of 10 μm was denser than the inside, but the number of surface pores, the tortuosity: R, and the dextran removal rate: T did not satisfy the conditions. (xi) In the method for evaluating the filtration of industrial wastewater, the initial filtration flux ratio (F2 / F1) was 0.40, and the filtration flux significantly decreased after long-term use.
[0090] Comparative Example 4 The porous membrane in Comparative Example 4 was an ST membrane manufactured by Synder. Figure 6 shows an image of the cross section of the outermost surface of the porous membrane observed by TEM. The evaluation results are shown in Table 2. The porous membrane did not have a nanomesh structure. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside, but the number of surface pores, the tortuosity: R, and the dextran removal rate: T did not satisfy the conditions. (xi) In the industrial wastewater filtration evaluation method, the amount of permeated liquid was extremely small, making it difficult to measure the filtration flux, which was below the lower limit of measurement. It is believed that the filtration flux was extremely low because the number of surface pores was small and the dextran removal rate: T was excessively large.
[0091] Comparative Example 5 A porous membrane was obtained in the same manner as in Comparative Example 3, except that the composition ratio in the polymer solution was changed. The composition ratio of 2P was 30 mass%. The evaluation results of the porous membrane are shown in Table 2. The surface part of the porous membrane from the surface to a thickness of 10 μm was denser than the inside, but the number of surface pores, the tortuosity: R, and the dextran removal rate: T did not satisfy the conditions. (xi) In the method for evaluating the filtration of industrial wastewater, the initial filtration flux ratio (F2 / F1) was 0.45, and the filtration flux significantly decreased after long-term use.
[0092] Comparative Example 6 A porous membrane was obtained by the same membrane production as in Example 1, except that 2P in the polymer solution was changed to γ-butyrolactone. The evaluation results of the porous membrane are shown in Table 2. The surface part of the porous membrane from the surface to a thickness of 10 μm was denser than the inside, but the average surface pore size, tortuosity: R, and dextran removal rate: T did not satisfy the conditions. (xi) In the method for evaluating the filtration of industrial wastewater, the initial filtration flux ratio (F2 / F1) was 0.40, and the filtration flux significantly decreased after long-term use.
[0093] (Comparative Example 7) (ix) The filtration performance of the porous membrane was evaluated using the gelatin aqueous solution filtration evaluation method. The porous membrane used was the one used in Comparative Example 1. When the gelatin aqueous solution was filtered, the gelatin removal rate: T ゼラチン is 63%, and the filtration flux is 58 L / m 2 The number of surface pores on the porous membrane used in the evaluation was 196 / μm 2 The tortuosity ratio: R was 6.4, and the dextran removal rate: T was 55%.
[0094] Comparative Example 8 (x) The filtering property of the porous membrane was evaluated using the apple juice filtering evaluation method. The porous membrane used was that of Comparative Example 4. When the apple juice was filtered, the removal rate of the apple juice: T りんご is 99.9%, and the filtration flux is 4L / m 2 / h, the filtration flux was low and poor. The number of surface pores of the porous membrane used in the evaluation was below the lower limit of observation, the tortuosity ratio: R was 66.9, and the dextran removal rate: T was 99.9%. It is believed that the extremely low filtration flux was due to the small number of surface pores and the excessively large dextran removal rate: T.
[0095] Comparative Example 9 A polymer solution was prepared by mixing 12% by mass of PVDF3 (Solef9009 manufactured by Solvay), 7% by mass of cellulose triacetate: CTA (LT-35 manufactured by Daicel Corporation), and 81% by mass of NMP and stirring at 120° C. for 4 hours.
[0096] Next, the polymer solution was uniformly applied (thickness 50 μm) to the outer surface of the hollow fiber support at 10 m / min. The support coated with the polymer solution was taken up at 10 m / min, and 1 second after application, it was passed through a coagulation bath of distilled water at 15°C for 10 seconds to coagulate, forming a porous membrane having a three-dimensional mesh structure. The evaluation results of the obtained porous membrane are shown in Table 5. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. The tortuosity of the obtained porous membrane: R was 6.0, the dextran removal rate: T was 71%, and the number of surface pores: 49 / μm 2 The number of surface pores divided by the average surface pore size: X is 6 pores / μm 2 / nm, and it was determined that it did not have a nanomesh structure based on the cross-sectional pore size and the number of cross-sectional pores. (xi) In the method for evaluating the filtration of industrial wastewater, the initial filtration flux ratio (F2 / F1) was 0.42, and the filtration flux significantly decreased after long-term use.
[0097] Comparative Example 10 A porous membrane was obtained in the same manner as in Comparative Example 1, except that the coagulation bath temperature was changed to 6°C. The evaluation results of the porous membrane are shown in Table 5. The surface portion of the porous membrane up to a thickness of 10 μm from the surface was denser than the inside. The tortuosity of the obtained porous membrane: R was 13.2, the dextran removal rate: T was 70%, and the number of surface pores: 78 / μm. 2 The number of surface pores divided by the average surface pore size: X is 10 pores / μm 2 / nm, and (xi) in the evaluation method for industrial wastewater filtration, the initial filtration flux ratio (F2 / F1) was 0.37, and the filtration flux significantly decreased after long-term use.
[0098] Comparative Example 11 A polymer solution was prepared by mixing 20% by mass of polyethersulfone: PES (Sumika Excel Co., Ltd.: 5900P), 4.1% by mass of polyvinylpyrrolidone: PVP (Nippon Shokubai Co., Ltd.: K-30), 4.1% by mass of polyethylene glycol: PEG (Wako Pure Chemical Industries, Ltd.: PEG300), 35.9% by mass of 2P, and 35.9% by mass of NMP at 120°C for 4 hours.
[0099] Next, the polymer solution was uniformly applied (thickness 50 μm) to the outer surface of the hollow fiber support at 10 m / min. The support to which the polymer solution was applied was taken up at 10 m / min, and 1 second after application, it was passed through a coagulation bath of distilled water at 25° C. for 30 seconds to be immersed therein for coagulation, forming a porous membrane having a three-dimensional mesh structure. The evaluation results of the obtained porous membrane are shown in Table 5. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. The dextran removal rate of the obtained porous membrane: T was 24%, and the number of surface pores: 2 / μm 2 The number of surface pores divided by the average surface pore diameter: X is 0.01 pores / μm 2 / nm, and (xi) in the industrial wastewater filtration evaluation method, the amount of permeated liquid was extremely small, making it difficult to measure the filtration flux, which was below the lower limit of measurement. It is considered that the filtration flux was extremely low because the number of surface pores was small and the dextran removal rate: T was low.
[0100] Comparative Example 12 A polymer solution was prepared by mixing 10% by mass of cellulose diacetate: CDA (Daicel: L-70), 4.1% by mass of polyvinylpyrrolidone: PVP (Nippon Shokubai: K-30), 4.1% by mass of polyethylene glycol: PEG (Wako Pure Chemical Industries: PEG300), 40.9% by mass of 2P, and 40.9% by mass of NMP at 120°C for 4 hours.
[0101] Next, the polymer solution was uniformly applied (thickness 50 μm) to the outer surface of the hollow fiber support at 10 m / min. The support coated with the polymer solution was taken up at 10 m / min, and 1 second after application, it was passed through a coagulation bath of distilled water at 25°C for 30 seconds to coagulate, forming a porous membrane having a three-dimensional mesh structure. The evaluation results of the obtained porous membrane are shown in Table 5. The surface portion of the porous membrane from the surface to a thickness of 10 μm was denser than the inside. The dextran removal rate of the obtained porous membrane: T was 43%, and the number of surface pores: 9 / μm 2 The number of surface pores divided by the average surface pore diameter: X is 0.4 / μm 2 / nm, and (xi) in the evaluation method for industrial wastewater filtration, the initial filtration flux ratio (F2 / F1) was 0.47, and the filtration flux significantly decreased after long-term use.
[0102] FIG. 10 shows the relationship between the self-diffusion coefficient and the initial ratio (F2 / F1) of the filtration flux for the example and the comparative example. -11 m 2 / sec~1.6×10 -11 m 2 / sec range, the initial ratio of filtration flux was 0.50 or more, and good filtration performance was maintained even after long-term operation.
[0103] [Table 1]
[0104] [Table 2]
[0105] [Table 3]
[0106] [Table 4]
[0107] [Table 5] [Explanation of symbols]
[0108] 101 Porous membrane 102 Surface part 103 Internal 201 Coarse dirt components 202 Fine dirt components 300 Polymer Solution 301 Polymer-rich phase 302 Solvent-rich phase FL Filtration direction
Claims
1. In at least one of the surfaces, a surface portion from the surface to a thickness of 10 μm is denser than the inside, the removal rate of dextran having a weight-average molecular weight of 40,000 Da: T is 60% to 95%, and the number of pores observed on the surface of the surface portion (hereinafter referred to as surface pores) per unit area is 200 pores / μm 2 ~2000 pieces / μm 2 The average surface pore diameter [nm] of the surface portion is 5.0 nm to 12 nm, and the tortuosity R of the surface portion represented by formula (1) is 1.0 to 8.
0. R=(ε / 2k) 1 / 2 ・V / S ...Formula (1) ε: Porosity k: Permeability coefficient [m 2 ] V: specific pore volume [m 3 / g] S: specific surface area [m 2 / g] Here, k: permeability coefficient is a coefficient calculated from the pure water permeability: Q [cm 3 / sec] of the membrane area: A [m 2 ] at the pressure: P [Pa] at 25° C. using the formula (2). k=8.76×Q / A / P×10-15...Formula (2)
2. The number of surface pores per unit area [pieces / μm 2 ] by the average surface pore diameter [nm] of the surface portion: X is 30 to 100 pores / μm 2 The porous membrane according to claim 1, wherein the molecular weight is 1 / nm.
3. The number of holes observed in a cross section of the outermost surface portion from the surface to a thickness of 2 μm is 100 / μm 2 ~1000 pieces / μm 2 The porous membrane according to claim 1 or 2, which has a nanomesh structure having an average cross-sectional pore diameter [nm] of 1 nm to 99 nm.
4. The number of the cross-sectional holes per unit area [pieces / μm 2 ] by the average cross-sectional pore diameter [nm]: Y is 3 to 10 pores / μm 2 The porous membrane according to claim 3, wherein the molecular weight is 1 / nm.
5. The porous membrane according to claim 3, wherein the standard deviation of the cross-sectional pore diameter [nm] of the outermost surface portion is 1.0 nm to 50 nm.
6. The porous membrane according to claim 1 or 2, wherein the standard deviation of the surface pore diameter [nm] of the surface portion is 0.5 nm to 5.0 nm.
7. The permeability coefficient k [m 2 ] is 0.5 × 10 -17 m 2 ~5.0 x 10 -17 m 2 The porous membrane according to claim 1,
8. A method for producing a porous membrane, comprising: step (A): dissolving a polymer in a solvent to obtain a polymer solution; and then step (B): solidifying the polymer solution in a non-solvent to form a porous membrane, In the step (A), the solvent contains a hydrogen bond solvent having a molecular weight of 500 Da or less and having hydrogen bond donor and hydrogen bond acceptor properties, the polymer to be dissolved contains a polymer having hydrogen bond donor and / or hydrogen bond acceptor properties, and the self-diffusion coefficient [m 2 / sec] is 0.8 × 10 -11 m 2 / sec ~ 1.6 x 10 -11 m 2 / sec, The method for producing a porous membrane, wherein step (B) is characterized in that the non-solvent contains 90 to 100% by weight of water and the temperature of the non-solvent is 6°C to 45°C.
9. The method for producing a porous membrane according to claim 8, wherein the value obtained by dividing the number of moles of the hydrogen bond acceptor functional group contained in the hydrogen bond solvent in the step (A) by the number of moles of the hydrogen bond donor functional group contained in the polymer having hydrogen bond donor property and / or hydrogen bond acceptor property is 1.0 to 12.
10. The method for producing a porous membrane according to claim 8 or 9, wherein the value obtained by dividing the number of moles of the hydrogen bond donor functional group contained in the hydrogen bond solvent in the step (A) by the number of moles of the hydrogen bond acceptor functional group contained in the polymer having hydrogen bond donor property and / or hydrogen bond acceptor property is 0.5 to 5.
0.
11. A method for filtering a liquid using the porous membrane according to claim 1 or 2.
Citation Information
Patent Citations
Production of hollow yarn membrane made of polysulfone
JP1989176407A
Filter material and manufacturing method therefor
JP2006082006A
Polyvinylidene fluoride-based multiple membrane and method for producing the same
JP2010094670A
Polyamide ultrafilter membrane having organic solvent resistance, and method for manufacturing the same
JP2014036946A
Porous membrane
WO2016031834A1