Steel plate for hot pressing, hot pressing member, and method for manufacturing hot pressing member
A Ni or Ni-based alloy coating on hot press steel plates addresses adhesion and cracking issues, ensuring effective scale prevention and enhanced corrosion resistance.
Patent Information
- Application Number
- JP2023520275
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-08
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-23
AI Technical Summary
Conventional hot press steel plates with surface plating layers face issues such as adhesion to heating equipment, liquid metal embrittlement cracking, and reduced corrosion resistance after painting due to oxidation and scale formation during hot pressing.
A steel plate with a 7 to 20 μm thick coating layer made of Ni or Ni-based alloy, containing 0 to 10% Zn and optionally Ti, V, Cr, Mn, Fe, Co, or Mo, which suppresses oxidation and prevents adhesion to heating equipment while enhancing corrosion resistance.
The solution effectively prevents scale formation, reduces adhesion to heating equipment, prevents liquid metal embrittlement cracking, and ensures excellent corrosion resistance after painting.
Smart Images

Figure 0007586303000001 
Figure 0007586303000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel plate for hot pressing, a hot pressed member, and a method for manufacturing a hot pressed member. [Background technology]
[0002] In recent years, in the field of automobiles, high-strength steel sheets have been used as materials for automobile parts in order to satisfy the conflicting demands of improving the strength of automobile bodies while reducing their weight, and the strength required for such high-strength steel sheets has tended to increase year by year.
[0003] However, generally speaking, increasing the strength of steel sheets reduces press formability, making it difficult to obtain complex part shapes. Examples of parts with complex shapes for automotive applications include chassis and other undercarriage components and frame structural components such as B-pillars.
[0004] In light of this, the use of hot pressing technology, which forms steel sheets hot rather than cold, is becoming more common. Hot pressing is a forming method in which steel sheets are heated to the austenite temperature range, then press-formed while still at a high temperature, and then quenched by contact with a die. In hot pressing, press forming is performed when the material steel sheet has a relatively low strength, and the strength is then increased by quenching, making it possible to achieve both high strength and press formability.
[0005] However, in the hot pressing, as described above, the steel sheet is heated to a high temperature, and therefore there is a problem that the surface of the steel sheet is oxidized and scale is generated. If scale is present on the surface of the steel sheet, oxides derived from the scale adhere to the heating equipment. The heating is typically performed in a heating furnace, and in this case, oxides adhere to the inner wall of the heating furnace and the conveying rollers installed in the furnace. This requires maintenance of the heating equipment, which reduces productivity. In addition, if scale is present on the surface of the steel sheet, sufficient paint film adhesion cannot be obtained in the subsequent painting process. Therefore, it has been necessary to remove the scale by shot blasting or the like after hot pressing.
[0006] Therefore, steel sheets having a coating such as an Al-based plating layer, a Zn-based plating layer, and an Al-Zn-based plating layer on the surface thereof are widely used as steel sheets for hot pressing (Patent Documents 1 and 2). The presence of the plating layer suppresses oxidation of the surface of the base steel sheet during hot pressing, and prevents the generation of scale. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2000-038640 A [Patent Document 2] JP 2003-073774 A Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, by using a steel sheet for hot pressing having a plating layer on the surface, oxidation of the surface of the base steel sheet during hot pressing can be suppressed, and the generation of scale can be prevented.
[0009] However, the above-mentioned conventional steel sheets for hot press work have the following problems.
[0010] One problem is the adhesion of the plating metal to the heating equipment. That is, in hot pressing, the steel sheet is heated to the austenite temperature range. This heating causes the metal contained in the plating layer to melt or evaporate, and adhere to the heating equipment, for example, the inner wall of the heating furnace or the rollers installed in the furnace. As in the case of the scale described above, when the plating metal adheres to the heating equipment, maintenance is required and productivity decreases. In addition, when the metal adheres to the roller, the adhered metal reacts with the material of the roller, causing embrittlement, which may lead to serious accidents such as damage to the roller.
[0011] Another problem is liquid metal embrittlement cracking. When tensile stress is applied to a solid metal while it is in contact with the surface of the solid metal, the solid metal becomes embrittled. This phenomenon is called liquid metal embrittlement (LME). In hot pressing, too, when the metal contained in the plating layer melts due to heating and press forming is performed in that state, liquid metal embrittlement cracking occurs in the bent parts that are subjected to tensile stress.
[0012] As described above, conventional hot press steel sheets having a plating layer have had problems of metal adhesion to heating equipment and liquid metal embrittlement cracking.
[0013] Furthermore, since the steel sheet for hot press use is generally used in a painted state after hot pressing, the hot press member finally obtained from the steel sheet for hot press use is also required to have excellent corrosion resistance after painting.
[0014] The present invention has been made in view of the above circumstances, and has an object to provide a steel sheet for hot press-forming and a hot press member that can satisfy the following requirements (1) to (3). (1) The adhesion of oxides and metals to heating equipment is reduced. (2) No liquid metal embrittlement cracking occurs during hot press forming. (3) Excellent corrosion resistance after painting. [Means for solving the problem]
[0015] The present invention has been completed based on the aim of solving the above problems, and the gist of the present invention is as follows.
[0016] 1. A base steel plate; A steel sheet for hot press comprising a coating layer having a thickness of 7 to 20 μm provided on both sides of the base steel sheet, The steel sheet for hot press use, wherein the coating layer is made of Ni or a Ni-based alloy, and the Zn content in the coating layer is 0 to 10 mass %.
[0017] 2. The steel sheet for hot press use according to 1 above, wherein the coating layer contains at least one selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Mo, and W in a total amount of 50 mass% or less.
[0018] 3. A base steel plate; A hot press member having a coating layer having a thickness of 7 to 20 μm provided on both sides of the base steel plate, The coating layer is made of Ni or a Ni-based alloy, and the Zn content in the coating layer is 0 to 10 mass %.
[0019] 4. The hot-pressed member according to claim 3, further comprising an oxide layer having a thickness of 10 μm or less on the coating layer.
[0020] 5. The hot-pressed member according to 4 above, wherein the proportion of Ni in the metal elements in the oxide layer is 50 atomic % or more.
[0021] 6. A method for producing a hot-pressed member, comprising hot-pressing the steel plate for hot-pressing according to 1 or 2 above to obtain a hot-pressed member. Effect of the Invention
[0022] According to the present invention, the above problems can be solved. That is, since the steel plate for hot pressing of the present invention has a coating layer on the surface, it is possible to prevent the generation of scale during hot pressing and reduce the adhesion of oxides to the heating equipment. In addition, by using a coating layer made of Ni or a Ni-based alloy and having a Zn concentration of 10% or less as the coating layer, it is possible to reduce the adhesion of molten metal to the heating equipment and prevent liquid metal embrittlement cracking during hot press forming. Furthermore, the hot press member obtained by hot pressing the steel plate for hot pressing of the present invention has excellent corrosion resistance after painting. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment for carrying out the present invention will be specifically described. Note that the present invention is not limited to this embodiment. In addition, the unit of content "%" in the composition of the coating layer and the steel sheet represents "mass %" unless otherwise specified.
[0024] [Steel sheets for hot pressing] The steel sheet for hot press use in one embodiment of the present invention includes a base steel sheet and coating layers having a thickness of 7 to 20 μm provided on both sides of the base steel sheet. The coating layers are made of Ni or a Ni-based alloy, and have a Zn concentration of 0 to 10%.
[0025] [[Coating layer]] The coating layer may be a coating layer made of Ni (Ni coating layer), or a coating layer made of a Ni-based alloy (Ni-based alloy coating layer). Here, the "Ni-based alloy" refers to an alloy with a Ni content of 50% or more. In other words, the coating layer of the present invention is a coating layer with a Ni content of 50% or more.
[0026] As mentioned above, in the heating process prior to hot pressing, the surface layer of the steel sheet is oxidized by oxygen and water vapor in the atmosphere. However, since the steel sheet for hot pressing of the present invention has a Ni-based coating layer on the surface, which has a high melting point and oxidation resistance, it is possible to suppress the oxidation of the base steel sheet and prevent the generation of scale.
[0027] From the viewpoint of enhancing the above-mentioned effects, the Ni content in the coating layer is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. On the other hand, the upper limit of the Ni content in the coating layer is not particularly limited and may be 100%.
[0028] Zn: 0-10% If the coating layer contains a large amount of Zn, the oxidation resistance decreases. In addition, Zn melts when heated, and liquid metal embrittlement cracking occurs during hot forming. Therefore, the Zn content in the coating layer is set to 10% or less. From the viewpoint of preventing liquid metal embrittlement cracking, the Zn content is preferably 5% or less, and more preferably 1% or less. On the other hand, the lower the Zn content, the better, so the lower limit of the Zn content is set to 0%.
[0029] The coating layer may optionally contain at least one selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Mo, and W in a total amount of 50% or less. By adding at least one of Ti, V, Cr, Mn, Co, Mo, and W, even better oxidation resistance can be obtained. In addition, when the coating layer is formed by electroplating, Fe dissolved from the base steel sheet into the plating bath may be incorporated into the coating layer. If the content of these elements is excessive, the Ni content in the coating layer is relatively reduced, and the function of the coating layer is impaired. Therefore, the total content of the elements is 50% or less, preferably 40% or less, and more preferably 35% or less. The lower limit of the total content is not particularly limited and may be 0%.
[0030] The Fe content in the coating layer is preferably 20% or less, more preferably 5% or less, and even more preferably 1% or less. The lower limit of the Fe content may be 0%.
[0031] The coating layer in one embodiment of the present invention comprises, in mass %, Zn: 0-10%, At least one selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Mo, and W: 0 to 50% in total; The balance is Ni and unavoidable impurities.
[0032] Thickness: 7~20μm When the hot press steel plate is heated, Ni in the coating layer and Fe in the base steel plate are mutually diffused, and a Ni-based alloy layer with an increased Fe concentration is formed on the surface of the hot press member. If the thickness of the coating layer of the hot press steel plate is less than 7 μm, the Fe that has diffused and reached the surface layer is oxidized, particularly when heated at high temperature for a long time, and a thick and brittle Fe-containing oxide layer is formed. If a thick and brittle Fe-containing oxide is present, the oxide adheres to and accumulates on the conveying roller and press mold during the hot press process. This requires maintenance of the equipment, and the productivity decreases. In addition, the oxide accumulated on the conveying roller and press mold adheres to the surface of the hot press member, which impairs the surface quality of the hot press member. Therefore, from the viewpoint of suppressing the growth of Fe oxide, i.e., the scale guard function, the thickness of the coating layer is set to 7 μm or more. In addition, the thicker the coating layer remains after heating, the better the corrosion resistance can be obtained, so the thickness of the coating layer is preferably 8 μm or more, and more preferably 9 μm or more. On the other hand, if the thickness of the coating layer exceeds 20 μm, the oxidation resistance and corrosion resistance improving effects are saturated, and the manufacturing cost increases. Therefore, the thickness of the coating layer is set to 20 μm or less, preferably 16 μm or less, and more preferably 12 μm or less.
[0033] Here, the thickness of the coating layer is defined as the thickness per one side of the steel sheet. The steel sheet for hot press use of the present invention has coating layers on both sides, and the thickness of the coating layer on one side may be the same as or different from the thickness of the coating layer on the other side.
[0034] [[Base material steel plate]] The base steel sheet is not particularly limited and any steel sheet can be used. The base steel sheet may be either a hot-rolled steel sheet or a cold-rolled steel sheet.
[0035] From the viewpoint of obtaining a hot-pressed member having a tensile strength exceeding 980 MPa class after hot pressing, the base steel sheet contains, in mass %, C: 0.05 to 0.50%, Si: 0.1 to 0.5%, Mn: 0.5-3.0%, P: 0.1% or less, S: 0.01% or less, Al: 0.10% or less, and N: Contains 0.01% or less, It is preferable to use a steel sheet having a composition with the balance being Fe and unavoidable impurities. The reason why the above composition is preferable will be explained below.
[0036] C: 0.05 to 0.50% C improves strength by forming martensite or the like as a steel structure. In order to obtain a strength exceeding 980 MPa, the C content must be 0.05% or more. Therefore, the C content is preferably 0.05% or more, and more preferably 0.10% or more. On the other hand, if the C content exceeds 0.50%, the toughness of the spot weld decreases. Therefore, the C content is preferably 0.50% or less. The C content is more preferably 0.45% or less, even more preferably 0.43% or less, and most preferably 0.40% or less.
[0037] Silicon: 0.1 to 0.5% Silicon is an effective element for strengthening steel to obtain good material properties. In order to obtain the above effect, the amount of silicon must be 0.1% or more. Therefore, the amount of silicon is preferably 0.1% or more, and more preferably 0.2% or more. On the other hand, if the amount of silicon exceeds 0.5%, ferrite is stabilized, and hardenability decreases. Therefore, the amount of silicon is preferably 0.5% or less. The amount of silicon is more preferably 0.4% or less, and even more preferably 0.3% or less.
[0038] Mn: 0.5-3.0% Mn is an element effective for ensuring strength after cooling over a wide range of cooling rates. In order to ensure excellent mechanical properties, particularly strength, it is desirable to set the Mn content to 0.5% or more. Therefore, the Mn content is preferably 0.5% or more, more preferably 0.7% or more, and even more preferably 1.0% or more. On the other hand, if the Mn content exceeds 3.0%, not only will the cost increase but the effect will saturate. Therefore, the Mn content is preferably 3.0% or less. The Mn content is more preferably 2.5% or less, even more preferably 2.0% or less, and most preferably 1.5% or less.
[0039] P: 0.1% or less If the P content exceeds 0.1%, the balance between strength and ductility is reduced through deterioration of local ductility due to grain boundary embrittlement caused by P segregation to the austenite grain boundaries during casting. Therefore, the P content is preferably 0.1% or less. On the other hand, there is no particular lower limit for the P content, and it may be 0%, but from the viewpoint of refining costs, the P content is preferably 0.002% or more.
[0040] S: 0.01% or less S becomes inclusions such as MnS, which deteriorates impact resistance and causes cracks along the metal flow of the weld. Therefore, it is desirable to reduce the S content as much as possible, and it is preferable to set the S content to 0.01% or less. From the viewpoint of ensuring good stretch flangeability, it is more preferable to set the S content to 0.005% or less, and even more preferable to set it to 0.001% or less. On the other hand, the lower limit of the S content is not particularly limited and may be 0%, but it is preferable to set it to 0.0002% or more from the viewpoint of refining costs.
[0041] Al: 0.10% or less If the Al content exceeds 0.1%, the blanking workability and hardenability of the steel sheet material are deteriorated. Therefore, the Al content is preferably 0.10% or less. The Al content is more preferably 0.07% or less, and further preferably 0.04% or less. On the other hand, the lower limit of the Al content is not particularly limited and may be 0%, but from the viewpoint of ensuring the effect as a deoxidizing agent, it is preferably 0.01% or more.
[0042] N: 0.01% or less If the N content exceeds 0.01%, nitrides of AlN are formed during hot rolling or heating before hot pressing, which reduces the blanking workability and hardenability of the steel sheet material. Therefore, the N content is preferably 0.01% or less. On the other hand, the lower limit of the N content is not particularly limited and may be 0%, but from the viewpoint of refining costs, the N content is preferably 0.001% or more.
[0043] In addition, in order to further improve the properties, the composition of the base steel sheet may optionally further contain at least one selected from the group consisting of Nb: 0.10% or less, Ti: 0.05% or less, B: 0.0002 to 0.005%, Cr: 0.1 to 1.0%, and Sb: 0.003 to 0.03%.
[0044] Nb: 0.10% or less Nb is an effective component for strengthening steel, but if it is contained in excess, the rolling load increases. Therefore, when Nb is contained, the Nb content is set to 0.10% or less, preferably 0.06% or less, and more preferably 0.03% or less. On the other hand, the lower limit of the Nb content is not particularly limited and may be 0%, but from the viewpoint of refining costs, it is preferable to set it to 0.005% or more.
[0045] Ti: 0.05% or less Ti is also effective in strengthening steel like Nb, but if it is contained in excess, shape fixability decreases. Therefore, when Ti is contained, the Ti content is set to 0.05% or less, preferably 0.03% or less. On the other hand, the lower limit of the Ti content is not particularly limited and may be 0%, but from the viewpoint of refining costs, it is preferable to set it to 0.003% or more.
[0046] B: 0.0002~0.005% B is an element that has the effect of suppressing the formation and growth of ferrite from the austenite grain boundaries. When B is contained, in order to obtain the above effect, the B content is preferably 0.0002% or more, and more preferably 0.0010% or more. On the other hand, excessive B content significantly impairs formability. Therefore, when B is contained, the B content is 0.005% or less, preferably 0.003% or less.
[0047] Cr: 0.1-1.0% Cr is an element that improves the strengthening and hardenability of steel, similar to Mn. When Cr is added, the Cr content is set to 0.1% or more, preferably 0.2% or more, in order to obtain the above-mentioned effect. On the other hand, since Cr is expensive, adding more than 1.0% will lead to a significant increase in costs. Therefore, when Cr is contained, the C content is set to 1.0% or less, preferably 0.5% or less, and more preferably 0.2% or less.
[0048] Sb: 0.003 to 0.03% Sb is an element that has the effect of suppressing decarburization of the surface layer of a steel sheet during the annealing process when manufacturing a base steel sheet. When Sb is contained, the Sb content is set to 0.003% or more, preferably 0.005% or more, in order to obtain the above effect. On the other hand, if the Sb content exceeds 0.03%, the rolling load increases, resulting in a decrease in productivity. Therefore, when Sb is contained, the Sb content is set to 0.03% or less, preferably 0.02% or less, more preferably 0.01% or less.
[0049] [Manufacturing method of hot-press steel sheets] The steel sheet for hot press-forming according to the present invention can be produced by any method without particular limitation, but preferred production conditions will be described below.
[0050] First, a base steel sheet is produced. The base steel sheet can be produced by rolling a steel slab typically obtained by casting. As the steel slab, it is preferable to use a steel slab having the above-mentioned component composition.
[0051] In the rolling, the hot slab obtained by casting may be directly subjected to hot rolling (without reheating), or the cold slab whose temperature has been reduced after casting may be reheated and then subjected to hot rolling. There is almost no difference in the properties of the steel sheet obtained when the hot slab is directly rolled and when the cold slab is reheated and then rolled. When the cold slab is reheated before hot rolling, the reheating temperature is not particularly limited, but is preferably in the range of 1000°C to 1300°C in consideration of productivity.
[0052] The hot rolling can be either a normal hot rolling process or a continuous hot rolling process in which slabs are joined and rolled in finish rolling. The rolling end temperature in the hot rolling is not particularly limited, but it is preferably set to the Ar3 transformation point or higher from the viewpoints of productivity and plate thickness accuracy.
[0053] The hot-rolled steel sheet obtained by the hot rolling is then cooled according to a conventional method. The coiling temperature at this time is preferably 550°C or higher from the viewpoint of productivity. If the coiling temperature is too high, pickling properties deteriorate, so the coiling temperature is preferably 750°C or lower. After the cooling, pickling is preferably performed according to a conventional method.
[0054] When a cold-rolled steel sheet is used as the base steel sheet, after the above pickling, cold rolling may be further carried out in a conventional manner.
[0055] Next, a coating layer is formed on the surface of the obtained steel sheet. The method for forming the coating layer is not particularly limited, and it can be formed by any method such as plating, PVD (physical vapor deposition), clad rolling, etc. Examples of the plating include electroplating. Examples of the PVD include vacuum deposition, sputtering, ion plating, etc. When clad rolling is used, layers having a desired composition are laminated on both sides of the base steel sheet, and then rolled.
[0056] The method for forming the coating layer is preferably selected according to the composition of the coating layer to be formed. For example, when the coating layer is a Ni layer, a Ni-Cr alloy layer, or a Ni-Zn alloy layer, it is preferable to form the layer by electroplating, but other methods can also be used without problems. When the coating layer has a composition that is difficult to electrolytically deposit from an aqueous solution, such as a Ni-Ti alloy, it is preferable to form the layer by PVD.
[0057] Regardless of the method used to form the coating layer, the conditions may be adjusted so that the coating layer on one side (front side) of the steel sheet and the other side (back side) of the steel sheet have the desired thickness. For example, in the case of electroplating, the thickness of the coating layer on each side can be adjusted by changing either or both of the current density and the current application time on each side.
[0058] [Hot-pressed parts] The hot-pressed member in one embodiment of the present invention is a hot-pressed member having a base steel plate and a coating layer having a thickness of 7 to 20 μm provided on both sides of the base steel plate, wherein the coating layer is made of Ni or a Ni-based alloy and has a Zn content of 0 to 10%.
[0059] In another embodiment of the present invention, the hot-pressed member further has an oxide layer having a thickness of 10 μm or less on the coating layer. That is, the hot-pressed member of this embodiment has a base steel sheet, coating layers having a thickness of 7 to 20 μm provided on both sides of the base steel sheet, and an oxide layer having a thickness of 10 μm or less provided on the coating layers, the coating layers being made of Ni or a Ni-based alloy, and the Zn content in the coating layers being 0 to 10%.
[0060] The above-mentioned explanations of the base steel sheet and the coating layer in the steel sheet for hot press use are applied to the base steel sheet and the coating layer.
[0061] [Oxide layer] The oxide layer is formed by the reaction of the components contained in the coating layer or the base steel sheet with oxygen or water vapor in the atmosphere during the hot pressing process. The composition and thickness of the oxide layer vary depending on the heating conditions, such as the heating temperature, heating time, and atmosphere. If the thickness of the oxide layer exceeds 10 μm, the coating adhesion decreases, and as a result, sufficient corrosion resistance after painting cannot be obtained. Therefore, if an oxide layer exists, the thickness of the oxide layer is set to 10 μm or less, preferably 7 μm or less, and more preferably 5 μm or less.
[0062] On the other hand, since the oxide layer is not necessarily required, the lower limit of the thickness may be 0 μm. However, by providing a thin oxide layer on the coating layer, the coating adhesion can be improved and the corrosion resistance after painting can be further improved. Therefore, from the viewpoint of further improving the corrosion resistance after painting, the thickness of the oxide layer is preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more.
[0063] The oxide layer formed may be removed by shot blasting after hot pressing, but removing the oxide layer increases the manufacturing cost, so removing the oxide layer is not essential.
[0064] The thickness of the oxide layer can be measured by observing the cross section of the hot-pressed part with a scanning electron microscope (SEM). More specifically, it can be measured by the method described in the examples.
[0065] The composition of the oxide layer is not particularly limited. However, the present inventors have found that when the fraction of Ni in the metal elements in the oxide layer is 50 atomic % or more, even better corrosion resistance can be obtained. The reason for this is considered as follows. That is, as described above, the oxide layer is formed by oxidizing the components contained in the coating layer or the base steel sheet in the hot pressing process. For example, when the oxide layer is mainly composed of oxides of Fe contained in the base steel sheet, the electrical resistance of the oxide layer is relatively low. In contrast, since the oxide of Ni has a higher electrical resistance than other oxides such as oxides of Fe, electrochemical corrosion can be suppressed by increasing the proportion of Ni oxide contained in the oxide layer. Therefore, from the viewpoint of suppressing electrochemical corrosion and further increasing corrosion resistance, it is preferable that the fraction of Ni in the metal elements in the oxide layer is 50 atomic % or more. On the other hand, the upper limit of the fraction of Ni is not particularly limited and may be 100%, but from the viewpoint of ease of manufacture, it is preferable to set it to 98% or less.
[0066] The Ni fraction in the metal elements in the oxide layer can be measured by quantitatively analyzing the cross section of the hot-pressed member with an EPMA (electron probe microanalyzer). More specifically, it can be measured by the method described in the examples.
[0067] [Manufacturing method of hot-pressed parts] In one embodiment of the present invention, a hot-pressed member is manufactured by hot-pressing a plated steel sheet for hot press. The method of hot pressing is not particularly limited, and can be performed according to a conventional method. Typically, the steel sheet for hot press is heated to a predetermined heating temperature (heating step), and then the steel sheet for hot press heated in the heating step is hot-pressed (hot pressing step). Preferred hot pressing conditions are described below.
[0068] If the heating temperature in the heating step is lower than the Ac3 transformation point of the base steel plate, the strength of the final hot press member will be low. Therefore, the heating temperature is preferably equal to or higher than the Ac3 transformation point of the base steel plate. The heating temperature is preferably equal to or higher than 860°C. On the other hand, if the heating temperature exceeds 1000°C, the oxide layer formed by oxidation of the base material or the coating layer becomes excessively thick, which may deteriorate the paint adhesion of the obtained hot press member. Therefore, the heating temperature is preferably equal to or lower than 1000°C, more preferably equal to or lower than 960°C, and even more preferably equal to or lower than 920°C. The Ac3 transformation point of the base steel plate varies depending on the steel composition, but is determined by a Formaster test.
[0069] The temperature at which the heating is started is not particularly limited, but is generally room temperature.
[0070] The time required for the temperature to rise from the start of heating to the heating temperature (temperature rise time) is not particularly limited and can be any time. However, if the temperature rise time exceeds 300 seconds, the time of exposure to high temperatures will be long, and the oxide layer generated by oxidation of the base material and plating layer will become excessively thick. Therefore, from the viewpoint of suppressing the decrease in paint adhesion due to oxides, the temperature rise time is preferably 300 seconds or less, more preferably 270 seconds or less, and even more preferably 240 seconds or less. On the other hand, if the temperature rise time is less than 150 seconds, the coating layer may melt excessively during heating, causing the heating device and the mold to be soiled. Therefore, from the viewpoint of further enhancing the effect of preventing the heating device and the mold from being soiled, the temperature rise time is preferably 150 seconds or more, more preferably 180 seconds or more, and even more preferably 210 seconds or more.
[0071] After reaching the heating temperature, the temperature may be held at the heating temperature. When the holding is performed, the holding time is not particularly limited, and the holding may be performed for any length of time. However, if the holding time exceeds 300 seconds, the oxide layer formed by oxidation of the base material or the coating layer becomes excessively thick, and the paint adhesion of the obtained hot press member may deteriorate. Therefore, the holding time is preferably 300 seconds or less, more preferably 210 seconds or less, and even more preferably 120 seconds or less. On the other hand, since the holding is an optional process, the holding time may be 0 seconds. However, from the viewpoint of homogeneously austenitizing the base steel sheet, the holding time is preferably 10 seconds or more.
[0072] The atmosphere in the heating step is not particularly limited, and heating can be performed in any atmosphere. The heating may be performed, for example, in an air atmosphere, or in an atmosphere into which air flows in. From the viewpoint of reducing the amount of diffusible hydrogen remaining in the member after hot pressing, it is preferable that the dew point of the atmosphere is 10°C or less. The lower limit of the dew point is not particularly limited, but in order to make the dew point less than -80°C, special equipment is required to prevent the inflow of air from the outside and maintain the low dew point, which increases costs. Therefore, from the viewpoint of cost, it is preferable to make the dew point -80°C or more, and more preferably -40°C or more.
[0073] The method for heating the steel sheet for hot pressing is not particularly limited, and it can be heated by any method. The heating can be performed, for example, by furnace heating, electric heating, induction heating, high frequency heating, flame heating, etc. As the heating furnace, any heating furnace such as an electric furnace or a gas furnace can be used.
[0074] Following the heating, hot press processing is performed, and simultaneously with or immediately after processing, cooling is performed using a mold or a coolant such as water to produce a hot press member. In the present invention, the hot press conditions are not particularly limited. For example, pressing can be started at a general hot press temperature range of 600 to 800°C. In addition, since the steel sheet for hot press of the present invention does not have the risk of liquid metal embrittlement, it is also possible to perform forming at a higher temperature than general hot press. Therefore, the hot press start temperature is preferably 600 to 1000°C. EXAMPLES
[0075] The present invention will now be described in detail with reference to examples.
[0076] The base steel sheet used was a cold-rolled steel sheet with a thickness of 1.4 mm, containing, by mass%, C: 0.34%, Si: 0.25%, Mn: 1.20%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Ti: 0.02%, B: 0.002%, Cr: 0.18%, Sb: 0.008%, with the balance being Fe and unavoidable impurities. The Ac3 transformation point of the base steel sheet was 783°C, and the Ar3 transformation point was 706°C.
[0077] Coating layers were formed on both sides of the base steel sheet by the methods shown in Table 1. Each of the methods used is explained below. For comparison, in Comparative Example No. 1, no coating layer was formed.
[0078] (Electroplating) The formation of the coating layer by electroplating was carried out under the following conditions: In each case, electrolysis was carried out using the base steel sheet as the cathode and the iridium oxide-coated titanium sheet as the anode, and the thickness of the coating layer was adjusted by changing the current application time.
[0079] (1) Nickel plating Plating solution composition: Nickel sulfate hexahydrate 240g / L Boric acid 30g / L pH: 3.0 ·Temperature: 50℃ ·Current density: 40A / dm 2
[0080] (2) Ni-Fe alloy plating Plating solution composition: Nickel sulfate hexahydrate 192g / L Iron sulfate heptahydrate 48g / L, Boric acid 30g / L pH: 3.0 ·Temperature: 50℃ ·Current density: 40A / dm 2
[0081] (3) Ni-Co alloy plating Plating solution composition: Nickel sulfate hexahydrate 180g / L Cobalt sulfate heptahydrate 60g / L Boric acid 30g / L pH 3.0, ·Temperature: 50℃ ·Current density: 40A / dm 2
[0082] (4) Ni-Mo alloy plating Plating solution composition: Nickel sulfate hexahydrate 13g / L Sodium molybdate dihydrate 19g / L Citric acid 88g / L pH: 3.5 ·Temperature: 25℃ ·Current density: 10A / dm 2
[0083] (5) Ni-W alloy plating Plating solution composition: Nickel sulfate hexahydrate 13g / L Sodium tungstate dihydrate 30g / L Citric acid 88g / L pH: 3.5 ·Temperature: 25℃ ·Current density: 10A / dm 2 in
[0084] (6) Ni-Zn alloy plating Plating solution composition: Nickel sulfate hexahydrate 240g / L Zinc sulfate heptahydrate 20g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2
[0085] (7) Ni-Zn alloy plating Plating solution composition: Nickel sulfate hexahydrate 240g / L Zinc sulfate heptahydrate 30g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2
[0086] (8) Zn plating Plating solution composition: Zinc sulfate heptahydrate 240g / L pH: 2.0 ·Temperature: 50℃ ·Current density: 40A / dm 2
[0087] (PVD) The formation of the coating layer by PVD was carried out by ion plating using a batch-type radio frequency (RF) excited ion plating device manufactured by Showa Vacuum Co., Ltd. The temperature of the base steel plate was 400°C, the pressure was 3 Pa, and the bias voltage was -20 V. The composition of the coating layer was controlled by adjusting the composition of the metal used as the deposition source. The thickness of the coating layer was also controlled by adjusting the deposition time.
[0088] (Clad rolling) A 300 μm thick Ni-15.5% Cr-8% Fe alloy (Alloy 600) was laminated on both sides of a 30 mm thick steel slab having the same composition as the above-mentioned base steel plate, and the resulting laminate was rolled to produce a steel plate for hot pressing.
[0089] (Hot-dip plating) The coating layer was formed by hot-dipping the base steel sheet in a hot-dip galvanizing bath for 1 second, followed by N2 gas wiping. The composition of the coating layer was controlled by adjusting the composition of the hot-dip galvanizing bath used.
[0090] The component composition and thickness of the coating layer of the obtained steel sheet for hot press use were measured by the following methods. The measurement results are shown in Table 1.
[0091] (Component composition of coating layer) The hot press steel plate to be evaluated was sheared to obtain a 10 mm x 15 mm sample. The sample was embedded in conductive resin to prepare a cross-sectional sample of the hot press steel plate. Next, the average composition in the range from the outermost layer of the coating layer to the interface between the coating layer and the base steel plate was measured using an EPMA (electron probe microanalyzer). Similar measurements were performed on three samples, and the measured values were averaged to obtain the component composition of the coating layer.
[0092] (Coating layer thickness) The thickness of the coating layer of the hot press steel sheet was measured by observing the cross-sectional sample with a SEM (scanning electron microscope). Specifically, the thickness of the coating layer was measured at 10 arbitrary points within a field of view with a width of 100 μm or more. The same measurement was performed on three samples, and the average of all the measured values was determined as the thickness of the coating layer.
[0093] Next, the steel plate for hot pressing was subjected to hot pressing. Specifically, a test piece of 100 mm x 200 mm was taken from the steel plate for hot pressing, and the test piece was heated in a roll conveying type far-infrared heating furnace. The heating was performed under the following conditions: heating temperature: 900°C, heating time: 180 seconds, and holding time: 10 seconds.
[0094] Next, a hat-shaped hot press was performed at 2 spm (Strokes Per Minute) using a press device installed adjacent to the heating furnace. The forming start temperature was 750°C. The shape of the obtained hot-pressed part was 100 mm long on the top flat part, 50 mm long on the side flat part, and 50 mm long on the bottom flat part. The bending radius of the mold was 7R on both shoulders of the top and bottom.
[0095] Furthermore, the hot-pressed member of Example No. 8 was subjected to air pressure shot blasting to remove the oxide layer. In the shot blasting, the air pressure was set to 2 kgf / cm. 2 The distance between the nozzle and the hot-pressed part was set to 20 mm, and steel balls with an average particle size of 0.3 mm were used as shot bullets.
[0096] (Component composition and thickness of coating layer) The component composition and thickness of the coating layer of the obtained hot press member were measured. First, the flat part of the top of the hot press member pressed into the hat shape was cut out and further sheared to obtain a sample of 10 mm x 15 mm. Next, the sample was embedded in a conductive resin to prepare a cross-sectional sample of the flat part of the hot press member. Using the cross-sectional sample, the component composition and thickness of the coating layer were measured in the same manner as in the measurement of the coating layer in the hot press steel plate described above. The measurement results are shown in Table 2.
[0097] The composition and thickness of the oxide layer in the hot-pressed member were measured by the following methods. The measurement results are shown in Table 2.
[0098] (Oxide layer composition) The composition of the oxide layer in the hot-pressed member was measured by EPMA using the cross-sectional sample. Point analysis was performed at 10 arbitrary points within a field of view of 100 μm or more in width. The Ni fraction in the oxide layer was calculated by dividing the Ni atomic concentration in the measured value by the sum of the atomic concentrations of all metal elements.
[0099] (Oxide layer thickness) The thickness of the oxide layer in the hot-pressed member was measured by observing the cross-sectional sample with a scanning electron microscope (SEM). Specifically, the thickness of the coating layer was measured at 10 arbitrary points within a field of view of 100 μm or more, and the average of all the measured values was determined as the thickness of the oxide layer.
[0100] <Adhesion to transport rollers> In order to evaluate the adhesion of metals and oxides to the heating equipment, 60 shots of hot pressing were performed on each hot pressing steel plate. After that, the conveying rollers of the heating furnace used in the hot pressing were cooled to room temperature, and the presence or absence of adhesion on the surface of the conveying rollers was visually confirmed. 2 Based on the percentage of rollers on which adhesions of this size or larger were found (adhesion roller rate), the adhesion to the transport rollers was evaluated into the following four levels. Evaluation results of 1 to 3 were deemed to be acceptable. The evaluation results are shown in Table 2. 1: Adhesion roller rate = 0% 2: 0%<Adhesive roller rate≦5% 3: 5%< adhesion roller rate ≦ 10% 4: Adhesion roller rate > 10%
[0101] <LME cracking during molding> In order to evaluate liquid metal embrittlement cracking during hot press forming, cracks in the obtained hot press members were measured. Specifically, first, the shoulder of the upper surface of the hat-shaped hot press member was cut out, embedded in resin, and then etched with 3% nital. Next, the cross section was observed, and the depth of the cracks that had progressed from the surface of the shoulder to the inside of the plate thickness was measured. For each example, observation was performed on three samples, and LME cracking during forming was evaluated into the following four levels based on the length of the longest crack. Evaluation results of 1 to 3 were deemed to be acceptable. The evaluation results are shown in Table 2. 1: Maximum crack length = 0 mm 2: 0mm<max crack length≦0.01mm 3: 0.01mm<max crack length≦0.1mm 4: Maximum crack length >0.1mm
[0102] <Corrosion resistance after painting> The post-painting corrosion resistance of the obtained hot-pressed member was evaluated by the following procedure. First, a test piece cut from the flat part of the upper surface of the hot-pressed member was subjected to a zinc phosphate-based conversion treatment and electrodeposition coating to prepare a sample. The zinc phosphate-based conversion treatment was performed under standard conditions using PB-SX35 manufactured by Nihon Parkerizing Co., Ltd., and the electrodeposition coating was performed using Electron GT100 cationic electrodeposition paint manufactured by Kansai Paint Co., Ltd. so that the coating thickness was 15 μm. The baking conditions were 170° C. and 20 minutes.
[0103] The obtained samples were subjected to a corrosion test (SAE-J2334) and the corrosion state after 60 cycles was evaluated. The maximum blister width on one side from the cross cut was measured, and the corrosion resistance after painting was evaluated on the basis of the maximum blister width on one side according to the following four levels. The evaluation results of 1 to 3 were deemed to be acceptable. The evaluation results are shown in Table 2. 1: Maximum bulge width on one side <1.5mm 2: 1.5mm≦Maximum bulge width on one side<2.0mm 3: 2.0mm≦Maximum bulge width on one side<3.0mm 4: Maximum bulge width on one side 3.0mm or less
[0104] As can be seen from the results of Tables 1 and 2, the steel plate for hot press use of the present invention reduced adhesion of metals and oxides to heating equipment and prevented liquid metal embrittlement cracking during hot press forming. Furthermore, the hot press member obtained by hot pressing the steel plate for hot press use of the present invention also had excellent corrosion resistance after painting.
[0105] [Table 1]
[0106] [Table 2]
Claims
1. A base steel plate; A steel plate for hot press comprising a coating layer having a thickness of 7 to 20 μm provided on both sides of the base steel plate, The coating layer is made of a Ni-based alloy containing at least one selected from the group consisting of Ti, V, and Fe in a total amount of 50 mass% or less, and the Zn content in the coating layer is 0 to 5 mass%.
2. A base steel plate; A coating layer having a thickness of 7 to 20 μm provided on both sides of the base steel sheet; A hot-pressed member having an oxide layer having a thickness of 10 μm or less provided on the coating layer, The coating layer is made of a Ni-based alloy containing at least one selected from the group consisting of Ti, V, and Fe in a total amount of 50 mass% or less, and the Zn content in the coating layer is 0 to 10 mass%.
3. The hot-pressed member according to claim 2 , wherein a proportion of Ni in the metal elements in the oxide layer is 50 atomic % or more.
4. A method for producing a hot-pressed member, comprising hot-pressing the steel sheet for hot press according to claim 1 to obtain a hot-pressed member.
Citation Information
Patent Citations
Hot rolled and cold rolled coated steel sheet excellent in durability after heat treatment
JP2000038640A
Plated steel sheet for hot press
JP2003073774A
Hot press member and method for producing the same
JP2011122207A
Coated heat-treated steel product, and method for manufacturing the same
JP2012062500A
Steel sheet for hot pressing, and method of producing hot-pressed member utilizing the same