Metal AM copper alloy powder and manufacturing method for additive manufacturing products

A copper alloy powder with a Si-enriched surface layer addresses the instability in metal AM, enhancing the reproducibility and quality of additively manufactured products by improving laser absorption and reducing voids.

JP7586376B2Active Publication Date: 2024-11-19MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024513174
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-24
Filing Date
2023-10-24
Publication Date
2024-11-19
Estimated Expiration
2043-10-24

AI Technical Summary

Technical Problem

Metal structures produced by metal AM using copper alloys suffer from non-uniform microstructures, voids, and thermomechanical and electrical reliability issues due to unstable melting behavior and gas entrapment, leading to poor productivity and quality.

Method used

A copper alloy powder with a Si-enriched layer on its surface is developed, which enhances laser absorption and reduces impurities, ensuring uniform microstructure and fewer voids, thereby improving the reproducibility and quality of additively manufactured products.

Benefits of technology

The copper alloy powder with a Si-enriched layer stabilizes the microstructure and reduces voids, enabling high-quality, high-productivity metal AM products with improved thermal, electrical, and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586376000006
    Figure 0007586376000006
  • Figure 0007586376000007
    Figure 0007586376000007
  • Figure 0007586376000008
    Figure 0007586376000008
Patent Text Reader

Abstract

This metal AM copper alloy powder for use in metal additive manufacturing (AM) comprises a copper alloy containing Si. An Si-enriched layer is continuously formed on the surface of copper alloy particles of which the powder is composed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to copper alloy powder for metal additive manufacturing (metal AM), which is optimal for metal AM technology, and a manufacturing method for additively manufactured objects. This application claims priority based on Japanese Patent Application No. 2022-169921, filed on October 24, 2022, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, metal AM technology, which mainly uses powder as the raw material to create products using a metal 3D printer, has been put to practical use as a method for manufacturing metal parts with various three-dimensional shapes. The main metal AM technologies that use metal powder include powder bed fusion (PBF) using electron beams or laser light, and the binder jet method. Copper alloys have many basic properties suitable for industrial applications, such as electrical conductivity, thermal conductivity, mechanical properties, wear resistance, and heat resistance, and are used as materials for various components. In recent years, attempts have been made to form components of various shapes by metal AM using copper alloy powder in various fields such as space and electrical component applications, and there is a growing need for copper and copper alloy parts manufactured by metal AM.

[0003] For example, Patent Document 1 proposes a technique for producing an additive manufacturing object by metal AM using a copper alloy powder containing either Cr or Si. Moreover, Patent Document 2 proposes a technique for producing an additive manufacturing object by metal AM using a copper alloy powder containing Cr and Zr. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-211062 A [Patent Document 2] JP 2019-070169 A [Non-patent literature]

[0005] [Non-Patent Document 1] YM Arisoy et. al., "Influence of scan strategy and process parameters on microstructure and its optimization in additively manufactured nickel alloy 625 via laser powder bed fusion", The International Journal of Advanced Manufacturing Technology, Volume 90, pp 1393-1417 (2017). Summary of the Invention [Problem to be solved by the invention]

[0006] Metal structures created by metal AM are used as structural components for a variety of applications, so if voids are present in the additively manufactured body or if the microstructure of the metal material is uneven, this can cause problems in terms of thermomechanical and electrical reliability. Currently, the most commonly used building method for metal AM is laser PBF, and attempts have also been made to use laser PBF for copper and copper alloys. Incidentally, when performing additive manufacturing using a method of irradiating a laser beam or an electron beam, a thin layer of powder is first formed (powder bed), and then this powder bed is locally irradiated with a laser or an electron beam to melt and solidify the material. However, in the case of copper and copper alloys, compared to other metal materials such as iron, titanium, and nickel, copper itself has a high reflectance in the visible and infrared ranges, which causes the melting behavior of the copper alloy powder to become unstable during the laser PBF process, and voids are likely to occur inside the additively manufactured object, resulting in a number of issues such as unstable quality of the object manufactured by laser PBF and poor productivity, and there is a demand for improvements in the productivity and quality of copper and copper alloys manufactured by laser PBF.

[0007] Currently, the most widely used form of raw material for metal AM is powder. For example, in metal AM using laser PBF, the electromagnetic wave absorption characteristics of the particles due to the coupling and interaction between the surface layer of each particle constituting the raw material powder and the electromagnetic wave affect the melting behavior of the raw material powder, and greatly affect the productivity of the part and the quality including the defect density of the part. For example, in a metal AM process using a powder bed, the thickness of the powder bed formed in one lamination process is, for example, about several tens of μm (Non-Patent Document 1), and the raw material powder is melted by irradiating such a relatively thin powder bed with converged electromagnetic waves, and the desired molded structure is realized by repeating numerous laminations and melting and solidification. The electromagnetic wave absorption characteristics of solids have a significant effect on the elementary process of such additive manufacturing using a powder bed. For example, since the electromagnetic wave absorption characteristics of solids are affected by the material composition, it is extremely important to increase the uniformity of the material composition and microstructure of the powder in order to achieve stable quality and high productivity in the entire additive manufacturing product.

[0008] Here, the electromagnetic wave absorption characteristics of copper and copper alloys can be improved, for example, by simply adding a substance with a high absorption rate of the target laser wavelength as a component other than copper. However, as many past metallurgical studies have shown, when copper and copper alloys are used for a certain application, the properties required for that application can only be realized by appropriately selecting the type and amount of elements added to copper. Therefore, in order to improve the productivity and quality of metal AM objects made of copper or copper alloys, in other words, to improve the laser absorption of raw powders of copper or copper alloys, a simple approach such as adding various foreign elements with high laser absorption rates to copper or copper alloys of optimized composition or increasing the amount of such elements may deteriorate the performance of copper alloys required for various applications. Therefore, it has been required to realize copper alloy powders for metal AM with improved laser absorption characteristics while maintaining a material composition that can fully ensure the performance of copper alloys required for various applications.

[0009] One important approach to improve the laser absorption properties of powders is to improve the laser absorption ability of each particle by surface modification of the particle surface that constitutes the powder. For this surface modification, it is possible to apply a coating of a substance that has a high absorption rate at the laser wavelength used in metal AM to the surface of each particle of the powder having the desired copper alloy composition. As an approach to coating the particle surface, a desired coating material can be formed on the particle surface using a wet or gas phase process. However, such a coating process is accompanied by problems such as the control of the thickness of the coating layer on each particle, as well as the reproducibility of the coating thickness and the homogeneity of the coating material throughout the powder, resulting in a number of issues in the productivity and quality of the molded object.

[0010] In addition, as a result of various past research and development efforts, copper alloy materials that achieve high mechanical strength while maintaining high electrical conductivity, as well as materials with excellent heat resistance, have already been developed, and in metal AM, there is a societal demand to use such existing high-performance copper alloy materials to create metal AM parts with desired shapes. However, controlling the amount of specific components formed by the coating while also controlling the material composition of the copper alloy in the final product not only places a significant burden on the manufacturing process, but there were concerns that it could result in a number of major problems, such as deterioration of the performance of the molded parts due to variations in composition and microstructure, deterioration of mass producibility of parts, and issues with maintaining the quality of the parts.

[0011] Furthermore, one of the factors that can cause structural defects in metal AM objects is the generation of voids due to the entrapment of gas, etc. When conventional copper alloy powder is used for additive manufacturing by the PBF method, gas is generated due to impurities contained in the copper alloy powder when the powder is melted, and the molten copper alloy or solidified copper alloy traps the gas components, which can cause voids to form inside the additive manufactured object, making it difficult to stably produce high-quality additive manufactured objects.

[0012] Furthermore, when additive manufacturing is performed by irradiating a powder bed of the raw material with laser light or an electron beam, if there is a lack of reproducibility of the microstructure of the raw material powder, including the reproducibility of the composition of the powder particles at each location irradiated with the laser light, the melting behavior of the powder will be non-uniform, which could result in the occurrence of structural defects such as voids inside the molded object or a deterioration of the mechanical properties due to non-uniformity in the metal composition of the molded object.

[0013] In addition, the reproducibility of the microstructure of the raw material powder, including the reproducibility of the powder's material composition, is a similar problem to other metal AM methods such as the binder jet method. In metal AM of copper alloys, improving productivity has been a major challenge due to the issues with the various raw materials.

[0014] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a copper alloy powder for metal AM that can stably produce high-quality additively molded objects with high reproducibility of the microstructure of objects created by metal AM and few structural defects such as voids, and a method for manufacturing additively molded objects. [Means for solving the problem]

[0015] To solve this problem, we conducted research and development to produce copper alloy powder that has the copper alloy composition required for practical applications and can be used to produce high-performance, high-quality copper alloy parts with high productivity using a metal AM process. As a result, when a high-purity copper alloy is used as a raw material and a powdering process is performed, it was found that while the copper alloy powder as a whole has few impurities and maintains a uniform composition, when focusing on the surfaces of individual particles in the copper alloy powder, a thin layer is formed on the surface of the copper alloy particles that will be irradiated with a laser. Furthermore, it was found that in the thin layer formed on the surface of the copper alloy particles, a characteristic structure in which powder constituent elements that show higher laser absorption than copper are frequently present compared to the interior of the bulk copper alloy particles, is spontaneously formed in the direct powdering process from the copper alloy raw material without going through an individual coating process on the powder or an additional process.

[0016] In addition to these structural features of the copper alloy particle surface, the copper alloy powder is derived from high-purity copper alloy raw materials, which means that it contains fewer impurities that lead to gas components, thereby suppressing gas generation during melting.This makes it possible to realize dense copper alloy bodies that have high thermal, electrical, and mechanical properties, and it has been discovered that it is possible to manufacture copper alloy powder for metal AM that can achieve high productivity and high quality of copper alloy bodies that exhibit such high performance.

[0017] In copper alloy powder produced by atomizing copper alloys containing added Si, which are derived from copper raw materials with few impurities, we have succeeded in self-forming and continuous formation of a Si-enriched layer on the particle surface of the copper alloy powder due to the rapid micronization and microstructural changes induced by temperature changes during the atomization process in which molten copper alloy is sprayed. It was discovered that when additive manufacturing of copper alloys is performed using copper alloy powder for metal AM consisting of particles with such a characteristic surface structure, it is possible to significantly reduce the occurrence of voids in the additively manufactured object, and it is possible to produce dense additively manufactured copper alloy objects. It is believed that such copper alloy powders with excellent formability will achieve higher productivity than conventional copper alloy powders.

[0018] The present invention has been made based on the above-mentioned findings, and a copper alloy powder for metal AM according to a first aspect of the present invention is a copper alloy powder for metal AM used in metal AM, The copper alloy contains Cr, Si, and Ni as alloying elements, and has a composition in which the Cr content is within a range of 0.1% by mass to 0.8% by mass, the Si content is within a range of 0.4% by mass to 0.8% by mass, the Ni content is within a range of 1.8% by mass to 3.0% by mass, and the remainder is copper and impurities. The powder is characterized by the continuous formation of a Si-enriched layer on the surface of the copper alloy particles that make up the powder. As additive elements and impurity elements other than the alloy elements, at least one element selected from the group consisting of Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W and Mo may be included in a total amount of 0.07 mass% or less.

[0019] The copper alloy powder for metal AM of embodiment 1 of the present invention is made of a copper alloy containing Si, and a Si-enriched layer is continuously formed on the surface of the copper alloy particles that make up the powder. This makes it possible to consistently produce high-quality additive manufacturing objects with high reproducibility of the microstructure of objects produced by metal AM and with few structural defects such as voids.

[0020] In a second aspect of the present invention, in the copper alloy powder for metal AM of the first aspect, the copper alloy preferably contains Cr. The copper alloy powder for metal AM of aspect 2 of the present invention is made of a copper alloy containing Cr and Si, and a Si-enriched layer is continuously formed on the surface of the copper alloy particles, which enables the stable production of high-quality additive manufacturing objects with high reproducibility of the microstructure of objects produced by metal AM and few structural defects such as voids.

[0021] In a third aspect of the present invention, in the copper alloy powder for metal AM of the first or second aspect, the Si-enriched layer preferably contains oxygen. According to the copper alloy powder for metal AM of aspect 3 of the present invention, the Si-enriched layer formed on the surface of the copper alloy particles contains oxygen, thereby suppressing deterioration of the copper alloy powder for metal AM, and enabling the more stable production of high-quality additive manufacturing objects with high reproducibility of the microstructure of objects produced by metal AM and fewer structural defects such as voids.

[0023] The present invention Aspect 4 teeth, Any one of aspects 1 to 3In the copper alloy powder for metal AM, it is preferable that the 50% cumulative particle diameter D50 on a volume basis measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less. The present invention Aspect 4 According to this copper alloy powder for metal AM, the 50% cumulative particle diameter D50 on a volume basis measured by a laser diffraction / scattering method is within the range of 5 μm or more and 120 μm or less, so that it has a particle size distribution suitable for metal AM and enables the stable production of additive manufacturing objects.

[0024] The present invention Aspect 5 teeth, Any one of aspects 1 to 3 In the copper alloy powder for metal AM, it is preferable that the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is in the range of 1 μm or more and 80 μm or less. The present invention Aspect 5 According to this copper alloy powder for metal AM, the volume-based 10% cumulative particle diameter D10 measured by laser diffraction / scattering is within the range of 1 μm or more and 80 μm or less, so that it has a particle size distribution suitable for metal AM and enables the stable production of additive manufacturing objects.

[0025] The present invention Aspect 6 teeth, Any one of aspects 1 to 3 In the copper alloy powder for metal AM, it is preferable that the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is in the range of 10 μm or more and 150 μm or less. The present invention Aspect 8 According to this copper alloy powder for metal AM, the volume-based 90% cumulative particle diameter D90 measured by laser diffraction / scattering is within the range of 10 μm or more and 150 μm or less, so that it has a particle size distribution suitable for metal AM and enables the stable production of additive manufacturing objects.

[0026] The present invention Aspect 7 The method for manufacturing a layered object is as follows: Any one of aspects 1 to 6It is preferable that the method further comprises a preparation step of preparing the copper alloy powder for metal AM, a first step of forming a powder bed containing the copper alloy powder for metal AM, and a second step of solidifying the copper alloy powder for metal AM at a predetermined position in the powder bed to form a modeling bed, thereby producing an additive manufacturing process by sequentially repeating these steps.

[0027] The present invention Aspect 7 According to the method for producing a layered object, Any one of aspects 1 to 6 Because this technology uses copper alloy powder for metal AM, the microstructure of the object produced by additive manufacturing is highly reproducible, making it possible to consistently produce high-quality additive manufactured objects with few structural defects such as voids.

[0028] The present invention Aspect 8 The method for manufacturing a layered object is as follows: Aspect 7 In the method for manufacturing a layered object, it is preferable to further include a heat treatment step of performing a heat treatment at a temperature range of 300° C. or higher and lower than the melting point of pure copper after the molding step. By subjecting the fabricated additive manufacturing object to an appropriate heat treatment depending on the application, it is possible to control the microstructure of the fabricated copper alloy, and it is possible to realize the desired mechanical properties and electrical conductivity properties. Aspect 8 By carrying out heat treatment within the temperature range of the manufacturing method, a copper alloy shaped body with an appropriately controlled microstructure can be realized.

[0029] The present invention Aspect 9 The method for manufacturing a layered object is as follows: Aspect 7 In the method for manufacturing an additive manufacturing object, it is preferable to include a first heat treatment process in which heat treatment is performed in a temperature range of 800°C or higher and lower than the melting point of pure copper after the molding process, and a second heat treatment process in which heat treatment is performed in a temperature range of 300°C or higher and lower than 800°C after the first heat treatment. By carrying out a two-step heat treatment under such temperature conditions, it is possible to realize a copper alloy having a desired microstructure. Effect of the Invention

[0030] According to the present invention, it is possible to provide a copper alloy powder for metal AM that can stably produce high-quality additively molded objects with high reproducibility of the microstructure of objects produced by metal AM and few structural defects such as voids, and a method for manufacturing additively molded objects. [Brief description of the drawings]

[0031] [Figure 1] FIG. 1 is a schematic explanatory diagram of a copper alloy particle constituting a copper alloy powder for metal AM according to an embodiment. [Diagram 2] FIG. 1 is a flow diagram of a method for producing a copper alloy powder for metal AM according to the present embodiment. [Diagram 3] FIG. 1 is a schematic explanatory diagram of a continuous casting device used when producing the copper alloy powder for metal AM according to the present embodiment. [Figure 4] FIG. 2 is a flow diagram of a method for manufacturing a layered object according to the present embodiment. [Diagram 5] FIG. 2 is a schematic explanatory diagram of another continuous casting device used when producing the copper alloy powder for metal AM according to the present embodiment. [Figure 6A] FIG. 2 is a diagram showing the results of Auger electron spectroscopy analysis of the outermost surface of a particle constituting the copper alloy powder for metal AM of this embodiment, and is a secondary electron image of the particle surface. [Figure 6B] FIG. 2 is a diagram showing the results of Auger electron spectroscopy analysis of the outermost surface of a particle constituting the copper alloy powder for metal AM of this embodiment, and is an elemental mapping image of the particle surface. [Figure 7A] 1 is an example of a graph showing the results of Auger electron spectroscopy analysis of the outermost surface of a particle constituting the copper alloy powder for metal AM of this embodiment, and shows an O intensity depth profile. [Figure 7B] This is an example of a graph showing the results of Auger electron spectroscopy analysis of the outermost surface of a particle constituting the copper alloy powder for metal AM of this embodiment, and shows the intensity depth profile of Si. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] Hereinafter, a copper alloy powder for metal AM and a method for manufacturing an additive manufacturing object according to one embodiment of the present invention will be described with reference to the attached drawings. The copper alloy powder for metal AM of this embodiment is a copper alloy powder used for metal AM. Note that the copper alloy powder for metal AM of this embodiment is particularly suitable for the laser PBF method.

[0033] The copper alloy powder for metal AM of this embodiment is an aggregate of particles made of a copper alloy containing Si, and a Si-enriched layer is continuously formed on the surface of the copper alloy particles constituting the copper alloy powder for metal AM. That is, as shown in FIG. 1, a copper alloy particle 50 of the copper alloy powder for metal AM of this embodiment has a particle body (copper alloy particle) 51 made of a copper alloy containing Si, and a Si-enriched layer 52 formed on the surface (or surface layer) of the particle body 51. In this embodiment, the surface (particle surface) (or surface layer) of the copper alloy particle of the copper alloy powder for metal AM is a region from the outermost surface of the particle to a depth of 100 nm.

[0034] The Si-enriched layer 52 is a layer in which a portion having a Si intensity amplification factor (defined below) of 2 or more is analyzed from the results of Auger electron spectroscopy analysis of the surface of the particle body 51. This analysis method will be described below. Using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc., the signal intensity (I AES (t)) is measured.

[0035] The Si-enriched layer 52 is identified by Auger electron spectroscopy as follows. The signal intensity (I AES (t)) is measured. And, I AES Identify six or more areas where (t) is roughly constant, and compare these I AESIn the region where (t) is constant, I AES Calculate the average of (t). This average is taken as the average background intensity (I AES , BG AVE ) is defined as I AES (t) to I AES , BG AVE Divide this number by I AES, NORM (t) is defined as I AES, NORM (t) is expressed by the following equation (1). I AES, NORM (t) = I AES (t) / I AES , BG AVE Formula (1)

[0036] t-I AES,NORM In the Si-enriched layer 52, the I AES,NORM (t) increases continuously. AES,NORM The start time of the region where a continuous increase in (t) is observed is the time t s0 It is defined as: For example, in the Examples (see Table 5 below), t s0 is approximately 2 minutes. In addition, I calculated by formula (1) AES, NORM (t) is called the Si intensity amplification factor. According to Table 5, in the example in which the Si-enriched layer 52 is present, a Si intensity amplification factor exceeding 2 is clearly observed, and a situation in which the Si signal intensity is clearly stronger than the background intensity is confirmed.

[0037] Therefore, in this embodiment, when multiple areas where a Si intensity magnification factor is 2 or more, preferably more than 2, are observed on the surface of the particle body 51, it is defined that a Si-enriched layer 52 is present on the surface of the particle body 51. In the Si-enriched layer 52, since a gradient of the Si concentration is observed as shown in FIG. 7B, a portion of the Si-enriched layer 52 may have a Si intensity magnification factor of less than 2 to 1.7 or the like.

[0038] In this embodiment, it is preferable that the Si-enriched layer 52 formed on the surface of the particle body 51 of the copper alloy particle 50 of the copper alloy powder for metal AM contains oxygen (O). Moreover, the thickness of the Si-enriched layer 52 formed on the surface of the particle body 51 is preferably 1 nm or more and 100 nm or less. The thickness of the Si-enriched layer 52 is preferably 1 nm or more, and may be 5 nm or more, 10 nm or more, 20 nm or more, 30 nm or more, or 50 nm or more. The thickness of the Cr compound layer 52 is preferably 100 nm or less, and may be 95 nm or less, 90 nm or less, 80 nm or less, or 70 nm or less.

[0039] The thickness of the Si-enriched layer 52 can be calculated from the time until the particle surface made of SiO2 is no longer reduced or becomes equal to or less than a predetermined value by etching the surface of the copper alloy particle 50 of the copper alloy powder for metal AM under the standard etching conditions, and analyzing the surface of the copper alloy particle 50 of the copper alloy powder for metal AM by Auger electron spectroscopy using a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc. to obtain a Si mapping image showing Si compounds, and obtaining a silicon (Si) intensity depth profile (graph showing the relationship between intensity and etching time shown in FIG. 7B). That is, it can be calculated as follows: time (min) until the strength (cps) of silicon (Si) becomes equal to or lower than a predetermined value × etching rate under standard conditions 1.08 nm / min = thickness of the Cr compound layer 52.

[0040] The copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM according to this embodiment preferably contains Cr as an alloying element. This is because the addition of Cr to the copper alloy generates compounds of Cr and Si in the copper alloy, and in particular, the compounds of Cr and Si present on the surfaces of the copper alloy particles contribute to improving the laser absorptivity.

[0041] The copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM according to the present embodiment preferably contains Ni as an alloying element. This is because the addition of Ni to the copper alloy causes Ni to dissolve in the Cu crystal grains, which contributes to improving the laser absorptivity of the Cu crystal grains in the copper alloy particles. Here, the content of Ni contained as an alloying element is preferably 3.0 mass% or less. In addition, the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment preferably contains, as alloy elements, Cr in the range of 0.1 mass% to 0.8 mass%, Si in the range of 0.4 mass% to 0.8 mass%, Ni in the range of 1.8 mass% to 3.0 mass%, and the rest is copper and impurities. That is, the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment preferably has a composition equivalent to C18000.

[0042] In this embodiment, the alloy elements refer to Cr, Si, and Ni. The impurities referred to here are components including impurity elements described below as well as O, H, S, and N. In the composition of the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM, the numerical accuracy error is ±10% (excluding O, H, S, and N).

[0043] The lower limit of the Cr content is more preferably 0.2 mass% or more, and even more preferably 0.3 mass% or more.The upper limit of the Cr content is more preferably 0.8 mass% or less, and even more preferably 0.7 mass% or less. The lower limit of the Si content is more preferably 0.45 mass% or more, and even more preferably 0.5 mass% or more.The upper limit of the Si content is more preferably 0.7 mass% or less, and even more preferably 0.6 mass% or less. The lower limit of the Ni content is more preferably 1.9 mass% or more, and even more preferably 2.0 mass% or more.The upper limit of the Ni content is more preferably 2.9 mass% or less, and even more preferably 2.8 mass% or less.

[0044] Furthermore, the copper alloy constituting the copper alloy particles 50 of the copper alloy powder for metal AM may contain additive elements and impurity elements (excluding O, H, S, and N) other than the alloy elements. In this embodiment, the additive elements are elements that are intentionally added to the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment. On the other hand, the impurity elements (excluding O, H, S, and N) are elements that are unintentionally mixed into the copper alloy particles 50 of the copper alloy powder for metal AM of this embodiment, and originate from contamination during the manufacturing process or impurities contained in trace amounts in the raw materials. The impurity elements may be unavoidable impurities.

[0045] Examples of additive elements and impurity elements (excluding O, H, S, and N) other than the alloying elements constituting the copper alloy particles 50 of the copper alloy powder for metal AM include Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W, and Mo. The additive elements and impurity elements (excluding O, H, S, and N) other than the alloying elements may include at least one element selected from the group consisting of Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, and Ag, Ta, W, and Mo. Here, the total amount of additive elements and impurity elements (excluding O, H, S, and N) other than the alloy elements constituting the copper alloy particles 50 of the copper alloy powder for metal AM may be 0.07 mass% or less, 0.06 mass% or less, or 0.05 mass% or less, preferably 0.04 mass% or less, more preferably 0.03 mass% or less, even more preferably 0.02 mass% or less, and even more preferably 0.01 mass% or less. In addition, the upper limit of the content of each of the additive elements and impurity elements (excluding O, H, S, and N) other than the alloy elements constituting the copper alloy particles 50 of the copper alloy powder for metal AM is preferably 30 massppm or less, more preferably 20 massppm or less, and even more preferably 15 massppm or less.

[0046] In the copper alloy powder for metal AM of this embodiment, it is preferable that the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less, the 10% cumulative particle diameter D10 is in the range of 1 μm or more and 80 μm or less, and the 90% cumulative particle diameter D90 is in the range of 10 μm or more and 150 μm or less.

[0047] The lower limit of the 50% cumulative particle size D50 is more preferably 10 μm or more, and even more preferably 15 μm or more.The upper limit of the 50% cumulative particle size D50 is more preferably 100 μm or less, and even more preferably 90 μm or less. The lower limit of the 10% cumulative particle size D10 is more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the 10% cumulative particle size D10 is more preferably 70 μm or less, and even more preferably 60 μm or less. Furthermore, the lower limit of the 90% cumulative particle size D90 is more preferably 20 μm or more, and even more preferably 30 μm or more.The upper limit of the 90% cumulative particle size D90 is more preferably 140 μm or less, and even more preferably 120 μm or less.

[0048] An example of a method for producing copper alloy powder for metal AM according to the present embodiment will be described with reference to the flow diagram in Fig. 2. Note that, in this embodiment, copper alloy powder suitable for the laser PBF method is produced. The manufacturing method of copper alloy powder for metal AM according to this embodiment includes a melting and casting step S01 for obtaining a copper alloy ingot, a copper alloy raw material preparation step S02 for processing the obtained copper alloy ingot into a wire rod to obtain a copper alloy raw material, and a powder processing step S03 for processing the copper alloy raw material into powder.

[0049] (Melting and casting process S01) First, a copper alloy ingot having a predetermined composition is produced. The melting and casting process S01 includes a melting step, an alloy element adding step, and a continuous casting step. In this embodiment, a copper alloy ingot 1 is produced using a continuous casting apparatus 10 shown in FIG. This continuous casting apparatus 10 includes a melting furnace 11, a tundish 12 arranged downstream of the melting furnace 11, a connecting trough 13 connecting the melting furnace 11 and the tundish 12, an addition section 14 for adding alloy elements in the tundish 12, a continuous casting mold 15 arranged downstream of the tundish 12, and a pouring nozzle 16 for pouring molten copper alloy from the tundish 12 into the continuous casting mold 15.

[0050] In the melting furnace 11, the copper raw material is melted in a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere) to obtain molten copper 3 (melting step). Here, the copper raw material melted in the melting furnace 11 is high-purity copper with a purity of 99.99 mass% or more (e.g., high-purity electrolytic copper or oxygen-free copper). The copper raw material to be melted is high-purity copper of 4N grade (99.99 mass%) or more, more preferably high-purity copper of 5N grade (99.999 mass%) or more, and even more preferably high-purity copper of 6N (99.9999 mass%) or more. The obtained molten copper 3 is preferably oxygen-free molten copper.

[0051] In the connecting trough 13, the obtained molten copper 3 is supplied to the tundish 12 while maintaining a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere). The connecting trough 13 is disposed between the melting furnace 11 and the tundish 12, and the molten copper 3 passes through the inside of the connecting trough 13 in a non-oxidizing atmosphere. In addition, in the tundish 12, the molten copper 3 is held in a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere). In addition, since the melting furnace 11, the connecting trough 13, and the tundish 12 are in a non-oxidizing atmosphere (an inert gas atmosphere or a reducing atmosphere), the gas components (O, H) in the molten copper 3 are reduced.

[0052] In the tundish 12, alloy elements (Cr, Si, Ni, etc.) are appropriately added to the molten copper 3 using the adding section 14 (alloy element adding step). Also, additive elements may be appropriately added here. By adding alloying elements to the molten copper 3 in which the gas components (O, H) have been sufficiently reduced, the yield of the alloying elements added is good, so that the amount of the alloying elements used can be reduced, and the manufacturing cost of the copper alloy can be reduced. Furthermore, by adding alloying elements to the molten copper 3 flowing inside the tundish 12, the alloying elements can be uniformly dissolved, and a molten copper alloy having stable component values ​​can be continuously produced.

[0053] The obtained molten copper alloy is poured into a continuous casting mold 15 through a pouring nozzle 16 to continuously produce a copper alloy ingot 1 (continuous casting process). In this embodiment, a copper alloy ingot having a circular cross section is produced.

[0054] In this embodiment, the obtained copper alloy ingot 1 has an O concentration of 10 massppm or less and an H concentration of 5 massppm or less. In the obtained copper alloy ingot 1, the S concentration is preferably 15 massppm or less. Furthermore, in the obtained copper alloy ingot 1, the total content of impurity elements other than Cu and alloying elements is preferably 0.04 mass% or less. In the obtained copper alloy ingot 1, the total concentration of O, H and S is preferably 20 massppm or less.

[0055] (Copper alloy raw material preparation process S02) Next, the copper alloy ingot obtained in the melting and casting step S01 is processed into a wire rod to produce a copper alloy raw material. The copper alloy raw material preparation step S02 includes an extrusion step, a drawing step, and a cutting step. In this copper alloy raw material preparation step S02, first, a copper alloy ingot having a circular cross section is heated and processed by hot extrusion into a rod having a predetermined diameter (extrusion step). In this embodiment, the heating temperature during the hot extrusion process is preferably set within a range of 700°C or more and 1000°C or less.

[0056] Next, the obtained rod is drawn to produce a wire having a predetermined diameter (drawing step). The temperature for the drawing is not particularly limited, but is preferably within the range of -200°C to 200°C, which corresponds to cold or warm rolling, and particularly preferably at room temperature.

[0057] The obtained wire is then cut to a predetermined length to provide a copper alloy raw material (cutting step). Here, it is preferable that the O concentration in the obtained copper alloy raw material is 10 massppm or less, and the H concentration is 5 massppm or less. In addition, it is preferable that the S concentration in the obtained copper alloy raw material is 15 massppm or less. Furthermore, the total content of impurity elements (excluding O, H, and S) other than Cu and alloying elements in the obtained copper alloy raw material is preferably 0.04 mass% or less.

[0058] (Powder processing process S03) Next, the copper alloy raw material obtained in the copper alloy raw material preparation step S02 is subjected to an atomization process to produce copper alloy powder for metal AM. This powder processing step S03 includes a melting step, an atomizing step, and a classification step. In the melting step, the copper alloy raw material is heated and melted to obtain a molten alloy. In this embodiment, the melting atmosphere is preferably a non-oxidizing atmosphere. In the atomization process, powder is obtained by, for example, gas atomization. That is, the molten alloy obtained in the melting process is sprayed with high-pressure gas to rapidly cool the droplets of the molten alloy, thereby producing powder having a spherical or similar shape. Inert gases such as argon and nitrogen can be used as the gas used in the gas atomization process. In the classification step, the obtained powder is classified to obtain a copper alloy powder having a predetermined particle size distribution. The melting temperature of the copper alloy raw material in the gas atomization process (melting temperature during the gas atomization process) is preferably not lower than the melting point of copper and not higher than 1500°C. The melting temperature during the gas atomization process may be not lower than 1085°C and not higher than 1500°C.

[0059] The copper alloy powder for metal AM according to the present embodiment is produced by the above-mentioned steps. In the copper alloy powder for metal AM according to the present embodiment, the O concentration is preferably 1000 massppm or less, the H concentration is preferably 5 massppm or less, and the S concentration is preferably 10 massppm or less. Specifically, the O concentration may be about 2700 massppm or less, preferably 1000 massppm or less, and more preferably 900 massppm or less. The lower limit of the O concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0). If the O concentration is high, foreign matter such as oxygen or oxides may remain in the molded product, which may deteriorate various properties of the molded product. The H concentration may be 90 massppm or less, may be 60 massppm or less, and is preferably 5 massppm or less. The lower limit of the H concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0). The S concentration may be 90 massppm or less, may be 60 massppm or less, and is preferably 30 massppm or less. Furthermore, the S concentration in the copper alloy powder for metal AM is more preferably 10 massppm or less. In addition, the lower limit of the S concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0). In addition, in a process carried out under a finite pressure, such as an atomization process, atmospheric components contained in the atmosphere or during the process may cause atmospheric components to be contained in the powder. For example, nitrogen derived from atmospheric components may be contained in the powder. In the copper alloy powder for metal AM of this embodiment, the nitrogen concentration (N concentration) is preferably 30 massppm, more preferably 20 massppm, and even more preferably 10 massppm or less. In the copper alloy powder for metal AM of this embodiment, the nitrogen concentration (N concentration) is more preferably 5 massppm or less. In addition, the lower limit of the N concentration is not particularly limited, but may be a value that does not include 0 (or a value that exceeds 0).

[0060] In addition, copper alloy powder for metal AM may contain additive elements and impurity elements other than alloy elements as long as they do not affect the characteristics. Here, the total amount of additive elements other than alloy elements and impurity elements (excluding O, H, S, and N) may be 0.07 mass% or less, may be 0.06 mass% or less, may be 0.05 mass% or less, is preferably 0.04 mass% or less, is more preferably 0.03 mass% or less, is even more preferably 0.02 mass% or less, and is further preferably 0.01 mass% or less. In addition, the upper limit of the content of each of additive elements other than alloy elements and impurity elements (excluding O, H, S, and N) is preferably 30 massppm or less, more preferably 20 massppm or less, and even more preferably 15 massppm or less.

[0061] Next, the method for producing a layered object according to the present embodiment will be described with reference to the flow chart of FIG. The manufacturing method of an additive manufacturing object in this embodiment includes a preparation process S101 for preparing the above-mentioned copper alloy powder for metal AM, a first process S121 for forming a powder layer containing the copper alloy powder for metal AM, and a second process S122 for solidifying the copper alloy powder for metal AM at a predetermined position in the powder layer to form a modeling layer, and a modeling process S102 for producing an additive manufacturing object by sequentially repeating these steps. Through these steps, an additive manufacturing process is performed to produce an additive manufacturing product having a predetermined shape. Since the additive manufacturing product uses the copper alloy powder for metal AM according to the present embodiment, the additive manufacturing product has few structural defects such as voids and has excellent mechanical properties.

[0062] The copper alloy powder for metal AM of this embodiment, configured as described above, is composed of copper alloy particles 50 containing Si, and Si is segregated on the surface of the copper alloy particles 50 that constitute the copper alloy powder for metal AM, and a Si-enriched layer 52 is formed on the outer surface of the particle body 51.Therefore, the microstructure of the object produced by additive manufacturing is highly reproducible, and it is possible to consistently produce high-quality additive manufactured objects with few structural defects such as voids.

[0063] Here, in the copper alloy powder for metal AM of this embodiment, when the Si-enriched layer 52 formed on the surface of the particle body 51 is an oxide layer containing Si and O, deterioration of the copper alloy powder for metal AM can be suppressed, and it becomes possible to more stably produce higher quality additively manufactured objects with high reproducibility of the microstructure of the object produced by additive manufacturing and fewer structural defects such as voids.

[0064] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the copper alloy constituting the copper alloy particles 50 contains Cr in the range of 0.1 mass% or more and 0.8 mass% or less, Si in the range of 0.4 mass% or more and 0.8 mass% or less, Ni in the range of 1.8 mass% or more and 3.0 mass% or less, and the remainder is composed of copper and impurities, by subjecting an appropriate heat treatment to an additive manufacturing object produced using this copper alloy powder for metal AM, compounds can be precipitated, and it is possible to produce an additive manufacturing object with excellent electrical conductivity, thermal conductivity, and strength.

[0065] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is within the range of 5 μm or more and 120 μm or less, it has a particle size distribution suitable for metal AM, and it becomes possible to stably manufacture additive manufacturing objects.

[0066] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is within the range of 1 μm or more and 80 μm or less, it has a particle size distribution suitable for metal AM, and it becomes possible to stably manufacture additive manufacturing objects.

[0067] Furthermore, in the copper alloy powder for metal AM of this embodiment, when the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is within the range of 10 μm or more and 150 μm or less, it has a particle size distribution suitable for metal AM, and it becomes possible to stably manufacture additive manufacturing objects.

[0068] In the manufacturing method of the additive manufacturing object of this embodiment, the copper alloy powder for metal AM of this embodiment is used, so that the microstructure of the object produced by additive manufacturing is highly reproducible, and it is possible to consistently produce high-quality additive manufacturing objects with few structural defects such as voids.

[0069] The copper alloy powder for metal AM and the method for manufacturing an additive manufacturing object according to the embodiment of the present invention have been described above. However, the present invention is not limited thereto and can be modified as appropriate without departing from the technical concept of the invention. For example, in the above-described embodiment, the copper alloy powder for metal AM is produced by gas atomization, but this is not limited to this, and the copper alloy powder for metal AM may be produced by water atomization, centrifugal atomization, plasma atomization, or the like.

[0070] In addition, the copper alloy powder for metal AM obtained as described above may be appropriately heat-treated in a controlled atmosphere to stabilize the structure. Furthermore, in this embodiment, the copper alloy powder for metal AM suitable for the laser PBF method has been described as being produced, but this is not limited to this, and the copper alloy powder for metal AM applicable to other additive manufacturing methods may also be used.

[0071] Furthermore, after the shaping step S102, a heat treatment step may be performed in which heat treatment is performed at a temperature of 300° C. or more and the melting point of pure copper or less. Also, after the shaping step S102, a first heat treatment step may be performed in which heat treatment is performed at a temperature range of 800° C. or more and the melting point of pure copper or less, and after this first heat treatment step, a second heat treatment step may be performed in which heat treatment is performed at a temperature range of 300° C. or more and 800° C. or less. In addition, in the present embodiment, the copper alloy ingot is produced using the continuous casting apparatus shown in FIG. 3, but the present invention is not limited to this, and other casting apparatuses may be used.

[0072] For example, a continuous casting apparatus 101 shown in Fig. 5 may be used. This continuous casting apparatus 101 includes an oxygen-free copper supply means (molten copper supply section) 102 arranged at the most upstream portion, a heating furnace 103 arranged downstream thereof, a tundish 104 arranged downstream of the heating furnace 103 and supplied with molten copper, molten metal supply passages 105a, 105b, and 105c connecting the oxygen-free supply means 102 to the heating furnace 103, a trough 106 connecting the heating furnace 103 and the tundish 104, addition means (addition sections) 107 and 108 for adding alloy elements in a non-oxidizing atmosphere, and a continuous casting mold 142. The oxygen-free copper supply means 102, the heating furnace 103, the tundish 104, the molten metal supply passages 105a, 105b, and 105c, and the trough 106 each have a non-oxidizing atmosphere inside.

[0073] The oxygen-free copper supply means 102 is composed of a melting furnace 121 for melting the copper raw material, a holding furnace 122 for temporarily holding the molten copper obtained by melting in the melting furnace 121, a degassing treatment device 124 for removing oxygen and hydrogen from the molten copper, and molten metal supply paths 105a, 105b, and 105c connecting these.

[0074] The degassing treatment device 124 has a gas bubbling device as stirring means for stirring the molten copper therein, and removes oxygen and hydrogen from the molten copper by bubbling with an inert gas, for example. The molten metal supply passages 105a, 105b, and 105c have a non-oxidizing atmosphere therein to prevent the molten copper and the oxygen-free copper molten metal from being oxidized. The non-oxidizing atmosphere is formed by blowing an inert gas such as a mixture of nitrogen and carbon monoxide or argon into the molten metal supply passages.

[0075] As adding means for adding alloy elements, a first adding means 107 disposed in the heating furnace 103 and a second adding means 108 disposed in the tundish 104 are provided. When alloying elements are continuously or intermittently charged from first adding means 107 provided in heating furnace 103, the alloying elements are added to the oxygen-free copper molten metal stored in heating furnace 103. Here, the oxygen-free copper molten metal stored in the storage section is heated by a high-frequency induction coil, which promotes the melting of the added alloying elements. Furthermore, when alloying elements are continuously or intermittently charged from the second adding means 108 provided in the tundish 104, the alloying elements are added to the molten oxygen-free copper flowing in the tundish 104. Here, the molten oxygen-free copper flowing in the tundish 104 is heated in the heating furnace 103 and has a high temperature, and also flows within the tundish 104, which promotes the dissolution of the added alloying elements. EXAMPLES

[0076] The results of experiments carried out to confirm the effects of the present invention will be described below.

[0077] (Example of the present invention) First, by the manufacturing method described in the embodiment, a copper raw material made of high purity copper of 4N grade was used to produce an ingot of C18000 having the composition shown in Table 1. Next, using the produced C18000 ingot as the raw material, copper alloy powder for metal AM with the composition shown in Table 2 was produced by gas atomization using argon gas, and the powder was classified to a particle size suitable for the powder bed of metal AM. The melting temperature during gas atomization was 1400°C. The copper alloy powder for metal AM of the present invention was subjected to particle size distribution measurement using a Microtrac MT3300EXII, and the particle size distribution was as follows: 10% cumulative particle size by volume was 15 μm, 50% cumulative particle size was 24 μm, and 90% cumulative particle size was 38 μm. As described later, a Si-enriched layer was observed on the surface of the copper alloy particles in the copper alloy powder for metal AM of the present invention. Then, using the C18000 powder for metal AM of the present invention, a commercially available laser PBF device was used to set the energy density to 13 J / mm 2 A small piece of the additive manufacturing object was produced under the above conditions.

[0078] (Comparative Example) As a comparative example, a copper alloy powder for metal AM having a C18000 composition in which no Si-enriched layer was formed on the particle surface, unlike the examples of the present invention, was prepared. For the copper alloy powder for metal AM in the comparative example, particle size distribution measurement was performed using a Microtrac MT3300EXII. The particle size distribution was as follows: 10% cumulative particle size by volume was 16 μm, 50% cumulative particle size was 28 μm, and 90% cumulative particle size was 45 μm. Then, using a copper alloy powder for metal AM having the composition of C18000 of the comparative example and a commercially available laser PBF device, a small piece of an additively molded object was produced under the same molding conditions as the example of the present invention, including the layer thickness.

[0079] (Surface structure of copper alloy powder for metal AM) The particle microstructures of the copper alloy powders for metal AM of the present invention and comparative examples were evaluated using Auger electron spectroscopy. The results are shown in Figures 6A and 6B, and Figures 7A and 7B. In Figures 7A and 7B, the solid lines show the analysis results of the copper alloy powders for metal AM of the present invention, and the dotted lines show the analysis results of the copper alloy powders for metal AM of the comparative examples.

[0080] (Presence or absence of Si-enriched layer) For the copper alloy powders for metal AM of the present invention and comparative examples, a scanning Auger electron spectrometer PHI700xi manufactured by ULVAC-PHI, Inc. was used to measure the signal intensity (I AES (t)) was measured. And this I AES (t) for the Si element AES Identify six or more areas where (t) is roughly constant, and compare these I AES In the region where (t) is constant, I AES The average value of (t) was calculated. This average value was used as the average background intensity (I AES , BG AVE ) was defined. Next, I AES (t) to I AES , BG AVE The value was divided by I AES, NORM (t) is defined as I AES, NORM (t) is expressed by the following formula (1). I AES, NORM (t) = I AES (t) / I AES , BG AVE Formula (1)

[0081] t-I AES,NORM In the Si-enriched layer, the I AES,NORM (t) was increasing continuously. AES,NORM The start time of the region where a continuous increase in (t) is observed is the time t s0 It was defined as follows. In the present invention, t s0 The time was about 2 minutes. AES, NORM (t) is the Si intensity amplification factor. The measurement time (t) and signal intensity of the Si element (I AES (t)), Si intensity multiplier factor I AES, NORM(t) is shown in Table 5. In the present invention, the average background intensity (I AES , BG AVE ) was 2847.57. In Table 5, in the present invention examples in which a Si-enriched layer exists, a Si intensity magnification factor exceeding 2 was clearly observed, and it was confirmed that the Si signal intensity was clearly stronger than the background intensity. Therefore, it was confirmed that a Si-enriched layer exists in the particle body of the copper alloy powder for metal AM of the present invention example. On the other hand, in the comparative examples, no Si intensity magnification factor exceeding 2 was observed, and it was considered that no Si-enriched layer was present in the particle body of the copper alloy powder for metal AM.

[0082] (Composition of copper alloy powder for ingot and metal AM) The O concentration in the ingots shown in Table 1, the copper alloy powders for metal AM of the examples of the present invention, and the copper alloy powders for metal AM of the comparative examples was determined by inert gas fusion-infrared absorption method, the H concentration by inert gas fusion-thermal conductivity method, and the S concentration by combustion-infrared absorption method. In addition, the concentrations of components other than these substances, excluding copper, were determined by a combination of X-ray fluorescence analysis, glow discharge mass spectrometry, and inductively coupled plasma mass spectrometry. The evaluation results are shown in Tables 1 and 2.

[0083] (model density) The density of the layered object was evaluated from the cross section of the layered object and the area occupied by voids observed in the cross section of the layered object. In this specification, this density is defined as the density of the object. The density of the molded object was evaluated by first defining the cross-sectional area of ​​the object to be measured (this is called the evaluation cross-sectional area, 3.4 mm square), then checking for voids within this measurement cross-sectional area, and calculating the area occupied by voids in the evaluation cross-sectional area. The density of the molded object was then defined as (evaluation cross-sectional area - void occupied area) / evaluation cross-sectional area. The evaluation results of the density of the molded object are shown in Table 3.

[0084] (Evaluation of mechanical properties and electrical conductivity of the object) As a mechanical property of the fabricated additive manufacturing object, the Vickers hardness (HV unit) was measured at room temperature in accordance with JIS Z 2244: 2009. The Vickers hardness measurement load was 10 kgf. In addition, the electrical conductivity (%IACS unit) of the fabricated additive manufacturing object was measured at room temperature using an eddy current electrical conductivity meter. The evaluation results are shown in Table 4.

[0085] [Table 1] (The impurities shown in Table 1 exclude O, H, and S.)

[0086] [Table 2] (The impurities shown in Table 2 exclude O, H, S, and N.)

[0087] [Table 3]

[0088] [Table 4]

[0089] [Table 5]

[0090] Figures 6A and 6B show the results of Auger electron spectroscopy of the particle surface of the copper alloy powder for metal AM of the present invention. As shown in Figures 6A and 6B, it was confirmed that a Si-enriched layer exists on the surface (or surface layer) of the copper alloy particles of the copper alloy powder for metal AM of the present invention, and that the particle surface is entirely covered with the Si-enriched layer.

[0091] 7A and 7B show intensity depth profiles of Si and O obtained by Auger electron spectroscopy of the particle surface of the copper alloy powder for metal AM of the present invention. The etching rate of each element and the compound produced by each element on the particle surface of the copper alloy powder of the present invention example in the experimental system of this Auger electron spectroscopy is not clear, but since the etching rate of SiO2 in the experimental system of this Auger electron spectroscopy is 1.08 nm / min, it is considered that the structure after ion etching for 7 minutes is approximately 10 nm thick.

[0092] As shown in Fig. 7B, in the copper alloy powder for metal AM of the present invention, the Si concentration was high on the surface side of the powder, and it was confirmed that a Si-enriched layer was formed on the surface of the powder. From this result, it is considered that the thickness of the Si-enriched layer is generally in the range of about 1 nm to 100 nm. On the other hand, as shown in Fig. 7B, in the copper alloy powder for metal AM of the comparative example, Si was not segregated on the surface of the powder, and it was recognized that a Si-enriched layer was not formed on the surface of the powder.

[0093] Moreover, as shown in Figure 7A, in the copper alloy powder for metal AM of the present invention, the O concentration was high on the surface side of the powder, and it was confirmed that the Si-enriched layer formed on the surface of the powder contained oxygen (O). That is, it is considered that the Si-enriched layer in the copper alloy powder for metal AM of the present invention is composed of a layer containing Si and O. Thus, in the copper alloy powder for metal AM of the present invention, oxygen was also detected at the same time in the Si-enriched layer, and it is considered that surface deterioration of the copper alloy powder can be relatively suppressed. Essentially, the copper alloy powder for metal AM of the present invention contains oxygen as a copper alloy, so a certain amount of oxygen is present in the particle body, which is thought to constitute the background concentration of oxygen in the particle body. On the other hand, it is thought that a gradient of oxygen concentration on the order of the thickness of the above-mentioned Si-enriched layer can be generated on the particle surface, mainly due to the powdering process.

[0094] As shown in Table 3, when a mold was made using the copper alloy powder for metal AM of the present invention in which a Si-enriched layer was formed on the particle surface, the molded object density was 99.6%. On the other hand, when molding was performed using copper alloy powder for metal AM in which no Si-enriched layer was formed, the packing density was 99%, as shown in the comparative example. These results confirmed that the copper alloy powder for metal AM having a Si-enriched layer of the present invention can produce high-quality additive manufacturing objects in which the occurrence of voids, which is important for practical use, is significantly suppressed. Furthermore, as shown in Table 4, it was confirmed that by subjecting the layered object of the present invention to a heat treatment under the conditions shown in Table 4, a copper alloy shaped body having highly practical properties can be provided. [Explanation of symbols]

[0095] 50 Copper alloy particles constituting copper alloy powder for metal AM 51 Particle body 52 Si enriched layer

Claims

1. A copper alloy powder for metal AM used in metal AM, The copper alloy contains Cr, Si, and Ni as alloying elements, and has a composition in which the Cr content is within a range of 0.1 mass% or more and 0.8 mass% or less, the Si content is within a range of 0.4 mass% or more and 0.8 mass% or less, the Ni content is within a range of 1.8 mass% or more and 3.0 mass% or less, and the remainder is copper and impurities, A copper alloy powder for metal AM, characterized in that a Si-enriched layer is continuously formed on the surface of the copper alloy particles constituting the powder.

2. A copper alloy powder for metal AM as described in claim 1, characterized in that it contains at least one element selected from the group consisting of Zr, Mg, Ti, Al, Zn, Ca, Sn, Pb, Fe, Mn, Te, Nb, P, Co, Sb, Bi, Ag, Ta, W and Mo as additive elements and impurity elements other than the alloy elements in a total amount of 0.07 mass% or less.

3. 2. The copper alloy powder for metal AM according to claim 1, wherein the Si-enriched layer contains oxygen.

4. 2. The copper alloy powder for metal AM according to claim 1, characterized in that the volume-based 50% cumulative particle diameter D50 measured by a laser diffraction / scattering method is in the range of 5 μm or more and 120 μm or less.

5. 2. The copper alloy powder for metal AM according to claim 1, characterized in that the volume-based 10% cumulative particle diameter D10 measured by a laser diffraction / scattering method is in the range of 1 μm or more and 80 μm or less.

6. The copper alloy powder for metal AM according to claim 1, characterized in that the volume-based 90% cumulative particle diameter D90 measured by a laser diffraction / scattering method is in the range of 10 μm or more and 150 μm or less.

7. A preparation step of preparing a copper alloy powder for metal AM according to any one of claims 1 to 6; a molding process for producing an additive object by sequentially repeating a first process for forming a powder bed containing the copper alloy powder for metal AM and a second process for solidifying the copper alloy powder for metal AM at a predetermined position in the powder bed to form a molding bed; A method for manufacturing a layered object, comprising:

8. The method for manufacturing a layered object according to claim 7, further comprising a heat treatment step of performing a heat treatment at a temperature range of 300° C. or higher and lower than the melting point of pure copper after the shaping step.

9. The method for manufacturing an additively molded object according to claim 7, characterized in that it comprises a first heat treatment process in which heat treatment is performed in a temperature range of 800°C or higher and lower than the melting point of pure copper after the molding process, and a second heat treatment process in which heat treatment is performed in a temperature range of 300°C or higher and lower than 800°C after the first heat treatment.

Citation Information

Patent Citations

  • Manufacturing method of alloy structure

    JP2016023366A

  • Copper alloy powder, manufacturing method of laminate molded article and laminate molded article

    JP2016211062A

  • Copper alloy powder, heat treatment method for multilayer shaped structure, method for producing copper alloy shaped structure, and copper alloy shaped structure

    JP2019070169A

  • Copper powder having excellent laser light absorbency

    JP2020186429A

  • Cu-ni-si-based alloy for electronic material

    WO2008123433A1