Multilayer ceramic capacitor and its manufacturing method
The multilayer ceramic capacitor design addresses reliability issues by minimizing pores and optimizing magnesium content in side margin regions, enhancing moisture resistance and capacitance in ultra-small capacitors.
Patent Information
- Application Number
- JP2020105838
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-01
- Filing Date
- 2020-06-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-06-19
AI Technical Summary
Existing methods for manufacturing small-sized and high-capacity multilayer ceramic capacitors result in reduced reliability due to the generation of pores at the interface between the ceramic body and the side margin, leading to decreased moisture resistance and sintered density.
The multilayer ceramic capacitor design includes a ceramic body with internal electrodes exposed on opposite surfaces, featuring first and second side margin parts with distinct regions that have adjusted pore density and dielectric grain sizes to minimize pores and enhance moisture resistance, along with specific magnesium content to improve reliability.
The design improves moisture resistance reliability and mechanical toughness by reducing pores per unit area and optimizing magnesium content, ensuring high capacitance and reliability in ultra-small capacitors.
Smart Images

Figure 0007586458000001 
Figure 0007586458000002 
Figure 0007586458000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic capacitor capable of improving reliability and a method for manufacturing the same. [Background technology]
[0002] Typically, electronic components using ceramic materials, such as capacitors, inductors, piezoelectric elements, varistors, or thermistors, comprise a ceramic body made of a ceramic material, an internal electrode formed inside the body, and an external electrode provided on the surface of the ceramic body so as to be connected to the internal electrode.
[0003] In recent years, as electronic products become smaller and more multifunctional, chip components also tend to become smaller and more functional. This has created a demand for multilayer ceramic capacitors that are small yet have a large capacitance.
[0004] In order to miniaturize and increase the capacitance of multilayer ceramic capacitors, it is necessary to maximize the effective electrode area (increase the effective volume fraction required to achieve capacitance).
[0005] In order to realize a small-sized, high-capacity multilayer ceramic capacitor as described above, when manufacturing a multilayer ceramic capacitor, a method is applied in which the internal electrodes are exposed in the width direction of the body, thereby maximizing the area of the internal electrodes in the width direction by a margin-free design, and after the chip is manufactured and before firing, a side margin portion is separately attached to the electrode exposed surface in the width direction of the chip to complete the chip.
[0006] However, in the above method, many pores are generated at the interface where the ceramic body and the side margin contact each other during the process of forming the side margin, which may reduce reliability.
[0007] Furthermore, the pores may cause a decrease in the sintered density of the outer side, resulting in a decrease in the reliability of moisture resistance.
[0008] Therefore, research is needed to prevent the deterioration of moisture resistance reliability in ultra-small and high-capacity products. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent Publication No. 2010-0136917 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a multilayer ceramic capacitor capable of improving reliability and a method for manufacturing the same. [Means for solving the problem]
[0011] An embodiment of the present invention includes a ceramic body including a dielectric layer, the ceramic body having a first surface and a second surface opposed to each other, a third surface and a fourth surface connecting the first surface and the second surface, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and opposed to each other, a plurality of internal electrodes disposed inside the ceramic body and exposed to the first surface and the second surface, and one end of the internal electrodes being exposed to the third surface or the fourth surface, and a first side margin portion and a second side margin portion disposed on ends of the internal electrodes exposed to the first surface and the second surface, The body includes a plurality of internal electrodes arranged to face each other with the dielectric layer therebetween, an active portion in which capacitance is formed, and cover portions formed on upper and lower portions of the active portion, the first and second side margin portions being divided into a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the internal electrodes exposed on the first and second surfaces, and the number of pores per unit area in the second region is smaller than the number of pores per unit area in the first region.
[0012] Another embodiment of the present invention includes the steps of: preparing a first ceramic green sheet on which a plurality of first internal electrode patterns are formed at predetermined intervals, and a second ceramic green sheet on which a plurality of second internal electrode patterns are formed at predetermined intervals; laminating the first ceramic green sheet and the second ceramic green sheet so that the first internal electrode pattern and the second internal electrode pattern cross each other to form a ceramic green sheet laminate body; cutting the ceramic green sheet laminate body so that ends of the first internal electrode pattern and the second internal electrode pattern have side surfaces exposed in a width direction; and forming a first sintered body on the side surfaces exposed at the ends of the first internal electrode pattern and the second internal electrode pattern. and forming a dome margin portion and a second side margin portion; and firing the cut laminated body to manufacture a ceramic body including a dielectric layer and first and second internal electrodes, wherein the ceramic body includes first and second internal electrodes arranged to face each other with the dielectric layer therebetween, an active portion in which capacitance is formed, and cover portions formed on upper and lower portions of the active portion, the first and second side margin portions being divided into a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the exposed internal electrodes, and the number of pores per unit area in the second region is smaller than the number of pores per unit area in the first region. Effect of the Invention
[0013] According to one embodiment of the present invention, the first and second side margin portions are divided into a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the internal electrodes exposed to the first and second surfaces of the ceramic body, and the number of pores per unit area in the second region is adjusted to be less than the number of pores per unit area in the first region, thereby improving moisture resistance reliability.
[0014] In addition, by adjusting the size of the dielectric grains contained in the first region to be smaller than the size of the dielectric grains contained in the second region, a gap sheet with high toughness can be formed, thereby improving mounting cracks.
[0015] Furthermore, the moisture resistance reliability can be improved by adjusting the magnesium (Mg) content in the side margin region adjacent to the width direction of the ceramic body.
[0016] Meanwhile, the cover part is divided into a first region adjacent to the outer surface of the ceramic body and a second region adjacent to the outermost internal electrode among the plurality of internal electrodes, and the number of pores and the magnesium (Mg) content contained in the first region and the second region can be adjusted to improve moisture resistance reliability. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a perspective view showing the appearance of the ceramic body of FIG. [Diagram 3] 3 is a perspective view showing the ceramic green sheet laminate body of FIG. 2 before firing. FIG. [Figure 4] FIG. 3 is a side view seen from the direction A in FIG. 2. [Diagram 5] FIG. 5 is an enlarged view of region B in FIG. [Figure 6] FIG. 3 is a side view of a ceramic body according to another embodiment of the present invention, taken from the direction A in FIG. 2. [Figure 7a] 5A to 5C are cross-sectional views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 7b] 5A to 5C are cross-sectional views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 7c] 5A to 5C are cross-sectional views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 7d] 10 is a perspective view illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 7e] 5A to 5C are cross-sectional views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 7f] 5A to 5C are cross-sectional views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 7g] 5A to 5C are cross-sectional views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 8] 1 is a graph comparing moisture resistance reliability test results according to an embodiment of the present invention and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for a clearer description.
[0019] FIG. 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment of the present invention.
[0020] FIG. 2 is a perspective view showing the appearance of the ceramic body of FIG.
[0021] FIG. 3 is a perspective view showing the ceramic green sheet laminate body of FIG. 2 before firing.
[0022] FIG. 4 is a side view seen from the direction A in FIG.
[0023] 1 to 4, the multilayer ceramic capacitor 100 according to the present embodiment includes a ceramic body 110, a plurality of internal electrodes 121, 122 formed inside the ceramic body 110, and external electrodes 131, 132 formed on the outer surface of the ceramic body 110.
[0024] The ceramic body 110 may have a first surface 1 and a second surface 2 facing each other, a third surface 3 and a fourth surface 4 connecting the first surface and the second surface, and a fifth surface 5 and a sixth surface 6 which are an upper surface and a lower surface.
[0025] The first surface 1 and the second surface 2 can be defined as surfaces facing each other in the width direction of the ceramic body 110, the third surface 3 and the fourth surface 4 can be defined as surfaces facing each other in the length direction, and the fifth surface 5 and the sixth surface 6 can be defined as surfaces facing each other in the thickness direction.
[0026] The shape of the ceramic body 110 is not particularly limited, but may be a rectangular parallelepiped as shown in the drawing.
[0027] A plurality of internal electrodes 121 and 122 formed inside the ceramic body 110 have one end exposed to the third surface 3 or the fourth surface 4 of the ceramic body.
[0028] The internal electrodes 121 and 122 may be a pair of a first internal electrode 121 and a second internal electrode 122 having different polarities.
[0029] One end of the first internal electrode 121 may be exposed to the third surface 3 , and one end of the second internal electrode 122 may be exposed to the fourth surface 4 .
[0030] The other ends of the first internal electrode 121 and the second internal electrode 122 are formed at a predetermined distance from the third surface 3 or the fourth surface 4.
[0031] A first external electrode 131 may be formed on a third surface 3 of the ceramic body and may be electrically connected to the first internal electrode 121. A second external electrode 132 may be formed on a fourth surface 4 of the ceramic body and may be electrically connected to the second internal electrode 122.
[0032] The multilayer ceramic capacitor 100 according to one embodiment of the present invention includes a plurality of internal electrodes 121, 122 disposed inside the ceramic body 110, exposed to the first and second surfaces 1, 2, and having one end exposed to the third or fourth surface 3 or 4, and a first side margin portion 112 and a second side margin portion 113 disposed on the ends of the internal electrodes 121, 122 exposed to the first and second surfaces 1 and 2.
[0033] A plurality of internal electrodes 121, 122 are formed inside the ceramic body 110, and each end of the plurality of internal electrodes 121, 122 is exposed to a first surface 1 and a second surface 2, which are the widthwise surfaces of the ceramic body 110, and a first side margin portion 112 and a second side margin portion 113 are respectively disposed on the exposed ends.
[0034] The first side margin portion 112 and the second side margin portion 113 may have an average thickness of not less than 2 μm and not more than 15 μm.
[0035] According to an embodiment of the present invention, the ceramic body 110 may be composed of a laminate in which a plurality of dielectric layers 111 are stacked, and a first side margin portion 112 and a second side margin portion 113 disposed on both sides of the laminate.
[0036] The plurality of dielectric layers 111 are in a sintered state, and the boundaries between adjacent dielectric layers may be integrated to the extent that they cannot be recognized.
[0037] The length of the ceramic body 110 corresponds to the distance from the third surface 3 to the fourth surface 4 of the ceramic body.
[0038] The length of said dielectric layer 111 defines the distance between the third face 3 and the fourth face 4 of the ceramic body.
[0039] Although not limited thereto, according to one embodiment of the present invention, the length of the ceramic body may be 400 to 1400 μm. More specifically, the length of the ceramic body may be 400 to 800 μm, or 600 to 1400 μm.
[0040] The internal electrodes 121 and 122 may be formed on the dielectric layer 111. The internal electrodes 121 and 122 may be formed inside the ceramic body 110 by sintering with one dielectric layer sandwiched therebetween.
[0041] 3, a first internal electrode 121 is formed on a dielectric layer 111. The first internal electrode 121 is not formed over the entire length of the dielectric layer. That is, one end of the first internal electrode 121 is formed at a predetermined distance from the fourth surface 4 of the ceramic body, and the other end of the first internal electrode 121 is formed up to the third surface 3 and exposed to the third surface 3.
[0042] The end of the first internal electrode exposed to the third surface 3 of the ceramic body is connected to the first external electrode 131 .
[0043] Unlike the first internal electrode, one end of the second internal electrode 122 is formed at a predetermined distance from the third surface 3, and the other end of the second internal electrode 122 is exposed to the fourth surface 4 and connected to the second external electrode 132.
[0044] In order to realize a multilayer ceramic capacitor with high capacitance, the internal electrodes may be laminated in 400 layers or more, but the number of layers is not necessarily limited thereto.
[0045] The dielectric layer 111 may have the same width as the first internal electrode 121. That is, the first internal electrode 121 may be formed over the entire dielectric layer 111 in the width direction.
[0046] Although not limited thereto, according to one embodiment of the present invention, the width of the dielectric layer and the width of the internal electrode may be 100 to 900 μm. More specifically, the width of the dielectric layer and the width of the internal electrode may be 100 to 500 μm, or 100 to 900 μm.
[0047] As the ceramic body becomes smaller, the thickness of the side margin may affect the electrical characteristics of the multilayer ceramic capacitor. According to an embodiment of the present invention, the thickness of the side margin is formed to be 15 μm or less, thereby improving the characteristics of the miniaturized multilayer ceramic capacitor.
[0048] That is, by forming the side margin portion to have a thickness of 15 μm or less, the overlapping area of the internal electrodes that form the capacitance is maximized, thereby realizing a multilayer ceramic capacitor that is high in capacitance and small in size.
[0049] The ceramic body 110 may be composed of an active portion that contributes to forming the capacitance of the capacitor, and upper and lower cover portions that are formed above and below the active portion as upper margin portions.
[0050] The active portion can be formed by repeatedly stacking a plurality of first and second internal electrodes 121 and 122 with a dielectric layer 111 sandwiched therebetween.
[0051] The upper and lower cover parts may have the same material and structure as the dielectric layer 111, except that they do not include internal electrodes.
[0052] That is, the upper and lower cover parts may include a ceramic material, for example, a barium titanate (BaTiO3) based ceramic material.
[0053] The upper and lower cover parts may each have a thickness of 20 μm or less, but are not necessarily limited thereto.
[0054] In an embodiment of the present invention, the internal electrodes and the dielectric layers are cut and formed at the same time, and the width of the internal electrodes and the width of the dielectric layers may be formed to be the same, which will be described in more detail below.
[0055] In the present embodiment, the width of the dielectric layer is formed to be the same as the width of the internal electrodes, so that ends of the internal electrodes 121 and 122 can be exposed to the first and second faces 1 and 2 in the width direction of the ceramic body 110.
[0056] A first side margin portion 112 and a second side margin portion 113 may be formed on both widthwise sides of the ceramic body 110 where the ends of the internal electrodes 121 and 122 are exposed.
[0057] The first side margin portion 112 and the second side margin portion 113 may have a thickness of 15 μm or less. As the thicknesses of the first side margin portion 112 and the second side margin portion 113 are smaller, an overlapping area of the internal electrodes formed in the ceramic body may become relatively larger.
[0058] The thickness of the first side margin portion 112 and the second side margin portion 113 is not particularly limited as long as it is a thickness that can prevent short-circuiting of the internal electrodes exposed on the side of the ceramic body 110, but for example, the thickness of the first side margin portion 112 and the second side margin portion 113 may be 2 μm or more.
[0059] If the thickness of the first and second side margin portions is less than 2 μm, there is a risk that the mechanical strength against external impact will decrease, and if the thickness of the first and second side margin portions is more than 15 μm, the overlapping area of the internal electrodes will be relatively reduced, which may make it difficult to ensure high capacitance of the multilayer ceramic capacitor.
[0060] In order to maximize the capacitance of a multilayer ceramic capacitor, methods such as thinning the dielectric layers, stacking the thinned dielectric layers at a high density, and improving the coverage of the internal electrodes have been considered.
[0061] Also, a method of increasing the overlapping area of the internal electrodes that form the capacitance has been considered.
[0062] In order to increase the overlapping area of the internal electrodes, it is necessary to minimize the marginal area where no internal electrodes are formed.
[0063] In particular, as multilayer ceramic capacitors become smaller, it is necessary to minimize the area of the marginal portion in order to increase the overlapping area of the internal electrodes.
[0064] According to this embodiment, the internal electrodes are formed over the entire width of the dielectric layer, and the thickness of the side margin portion is set to 15 μm or less, thereby providing a feature that the overlapping area of the internal electrodes is large.
[0065] Generally, the higher the number of dielectric layers, the thinner the dielectric layers and the internal electrodes become. Therefore, there is a risk of short circuits occurring frequently between the internal electrodes. In addition, if the internal electrodes are formed only on a part of the dielectric layers, a step is generated by the internal electrodes, which may reduce the accelerated life and reliability of the insulation resistance.
[0066] However, according to the present embodiment, even if thin internal electrodes and dielectric layers are formed, the internal electrodes are formed across the entire width of the dielectric layers, so that the overlapping area of the internal electrodes is increased, thereby enabling the capacitance of the multilayer ceramic capacitor to be increased.
[0067] In addition, by reducing the steps due to the internal electrodes, the accelerated life of the insulation resistance is improved, and a multilayer ceramic capacitor having excellent capacitance characteristics and reliability can be provided.
[0068] FIG. 5 is an enlarged view of region B in FIG.
[0069] Referring to FIG. 5, the first and second side margin portions 112, 113 are divided into first regions 112a, 113a adjacent to the outer surfaces of the side margin portions 112, 113 and second regions 112b, 113b adjacent to the internal electrodes 121, 122 exposed to the first surface 1 and the second surface 2 of the ceramic body 110, and the number of pores P per unit area in the second regions 112b, 113b is smaller than the number of pores P per unit area in the first regions 112a, 113a.
[0070] The first and second side margin portions 112, 113 arranged on the sides of the ceramic body 110 are divided into two regions having different sizes of dielectric grains, and in this case, the number of pores P per unit area in the second regions 112b, 113b is adjusted to be less than the number of pores P per unit area in the first regions 112a, 113a, thereby improving moisture resistance reliability.
[0071] Meanwhile, by adjusting the size d1 of the dielectric grains contained in the first regions 112a, 113a to be smaller than the size d2 of the dielectric grains contained in the second regions 112b, 113b, a highly tough gap sheet can be formed in the first regions 112a, 113a adjacent to the outer surfaces of the first and second side margin portions 112, 113, thereby improving mounting cracks.
[0072] Usually, during the process of forming the side margin, many pores are generated at the interface where the ceramic body and the side margin contact each other, which may reduce reliability.
[0073] In addition, pores formed at the interface between the ceramic body and the side margins may reduce the sintered density on the outside, thereby causing a decrease in moisture resistance reliability.
[0074] According to one embodiment of the present invention, the number of pores P per unit area in the second regions 112b, 113b of the side margin portion adjacent to the internal electrodes 121, 122 exposed to the first surface 1 and the second surface 2 of the ceramic body 110 is adjusted to be less than the number of pores P per unit area in the first regions 112a, 113a adjacent to the outer surfaces of the first and second side margin portions 112, 113, thereby improving moisture resistance reliability.
[0075] According to one embodiment of the present invention, the ratio of the number of pores P per unit area in the second regions 112b, 113b to the number of pores P per unit area in the first regions 112a, 113a may be 0.8 or less.
[0076] By adjusting the ratio of the number of pores P per unit area in the second regions 112b, 113b to the number of pores P per unit area in the first regions 112a, 113a to 0.8 or less, the moisture resistance reliability can be improved.
[0077] When the ratio of the number of pores P per unit area in the second regions 112b, 113b to the number of pores P per unit area in the first regions 112a, 113a exceeds 0.8, there is no difference between the number of pores P per unit area in the first regions 112a, 113a and the second regions 112b, 113b, so that the effect of improving the moisture resistance reliability is slight.
[0078] There is no particular limitation on the method for adjusting the number of pores P per unit area in the second regions 112b, 113b of the side margin portion adjacent to the internal electrodes 121, 122 exposed to the first surface 1 and the second surface 2 of the ceramic body 110 to be less than the number of pores P per unit area in the first regions 112a, 113a adjacent to the outer surfaces of the first and second side margin portions 112, 113. For example, this can be achieved by adjusting the size of the ceramic powder as a raw material input during the formation of the first regions 112a, 113a and the second regions 112b, 113b.
[0079] For example, this can be achieved by making the grain size of barium titanate (BaTiO3) powder, which is the raw material for forming the second regions 112b, 113b of the side margin portions adjacent to the internal electrodes 121, 122, larger than the grain size of barium titanate (BaTiO3) powder, which is the raw material for forming the first regions 112a, 113a adjacent to the outer surfaces of the first and second side margin portions 112, 113.
[0080] Although not particularly limited, for example, the particle size of barium titanate (BaTiO3) powder, which is the raw material for forming the second regions 112b, 113b of the side margin portions adjacent to the internal electrodes 121, 122, may be about 70 nm, and the particle size of barium titanate (BaTiO3) powder, which is the raw material for forming the first regions 112a, 113a adjacent to the outer surfaces of the first and second side margin portions 112, 113, may be about 40 nm.
[0081] According to one embodiment of the present invention, by adjusting the size of the ceramic powder as raw material input during the formation process of the first regions 112a, 113a and the second regions 112b, 113b as described above, after firing, the size d1 of the dielectric grains contained in the first regions 112a, 113a can be set to 90 nm or more and 410 nm or less, and the size d2 of the dielectric grains contained in the second regions 112b, 113b can be set to 170 nm or more and 700 nm or less.
[0082] The size of the dielectric grains contained in the first regions 112a, 113a and the second regions 112b, 113b can be obtained by measuring the lengths of the major and minor axes of the dielectric grains extracted from each corresponding region and calculating the average size.
[0083] The length of the major axis of the dielectric grain corresponds to the grain size of the dielectric grain at the longest measured point among a number of points measured as the grain size of the dielectric grain, assuming that the shape of the dielectric grain is elliptical, and the length of the minor axis of the dielectric grain corresponds to the grain size of the dielectric grain at the shortest measured point among a number of points measured as the grain size of the dielectric grain.
[0084] Meanwhile, according to one embodiment of the present invention, the first and second side margin portions 112, 113 arranged on the sides of the ceramic body 110 are divided into two regions having different compositions, and in this case, the magnesium (Mg) content contained in each region is made different, thereby improving the density of the first and second side margin portions 112, 113 and improving the moisture resistance characteristics.
[0085] Specifically, the magnesium (Mg) content in the second regions 112b, 113b of the first and second side margin portions 112, 113 is greater than the magnesium (Mg) content in the outer first regions 112a, 113a. By adjusting in this manner, the density of the second regions 112b, 113b of the side margin portions 112, 113 can be improved, thereby improving the moisture resistance characteristics.
[0086] In particular, by reducing the magnesium (Mg) content in the first regions 112a, 113a of the first and second side margin portions 112, 113 adjacent to the outer surfaces of the side margin portions 112, 113, mounting crack defects can be improved.
[0087] The magnesium (Mg) content in the second regions 112b, 113b can be adjusted to be greater than the magnesium (Mg) content in the first regions 112a, 113a by making the dielectric compositions for forming the first and second side margin portions different between the first and second regions during the manufacturing process of the multilayer ceramic capacitor.
[0088] That is, in the dielectric composition for forming the first and second side margin portions, by increasing the magnesium (Mg) content in the dielectric composition for forming the second region, the magnesium (Mg) content contained in the second regions 112b, 113b can be adjusted to be greater than the magnesium (Mg) content contained in the first regions 112a, 113a.
[0089] This can improve the density of the second regions 112b, 113b of the side margin portions 112, 113, and improve the moisture resistance. In addition, the electric field concentrated at the ends of the internal electrodes can be alleviated, which can prevent dielectric breakdown, one of the main defects in multilayer ceramic capacitors, and improve the reliability of the multilayer ceramic capacitor.
[0090] According to an embodiment of the present invention, the content of magnesium (Mg) in the second regions 112b and 113b may be 10 moles or more and 30 moles or less with respect to 100 moles of titanium (Ti) contained in the first and second side margin portions.
[0091] The magnesium (Mg) content of the second regions 112b and 113b is adjusted to be 10 moles or more and 30 moles or less with respect to 100 moles of titanium (Ti) contained in the first and second side margin portions, thereby increasing the breakdown voltage (BDV) and improving the moisture resistance reliability.
[0092] If the magnesium (Mg) content of the second regions 112b, 113b is less than 10 moles relative to 100 moles of titanium (Ti) contained in the first and second side margin portions, the formation of an oxide layer in the pores generated at the interface where the ceramic body and the side margin portions contact each other is insufficient, which may result in a low breakdown voltage (BDV) and an increase in short circuit defects.
[0093] On the other hand, if the magnesium (Mg) content of the second regions 112b, 113b exceeds 30 moles relative to 100 moles of titanium (Ti) contained in the first and second side margin portions, there is a possibility that a problem will occur in which reliability is reduced due to a decrease in sinterability.
[0094] According to an embodiment of the present invention, the dielectric layer 111 has a thickness of 0.4 μm or less, and the internal electrodes 121 and 122 have a thickness of 0.4 μm or less, thereby providing an ultra-small multilayer ceramic capacitor.
[0095] When thin dielectric layers and internal electrodes are applied, such as in one embodiment of the present invention, in which the thickness of the dielectric layer 111 is 0.4 μm or less and the thickness of the internal electrodes 121, 122 is 0.4 μm or less, the reliability problem caused by pores occurring at the boundary between the ceramic body and the side margin portion becomes a very important issue.
[0096] In other words, the conventional multilayer ceramic capacitor has no significant problem in terms of reliability even if the size of the dielectric grains in each region of the side margin portion included in the multilayer ceramic capacitor according to an embodiment of the present invention is not adjusted.
[0097] However, in products in which thin dielectric layers and internal electrodes are applied, such as in one embodiment of the present invention, the number of pores contained in each region of the side margin must be controlled to prevent a decrease in BDV and reliability due to pores generated at the interface where the ceramic body and the side margin contact each other.
[0098] That is, in one embodiment of the present invention, the number of pores P per unit area in the second regions 112b, 113b is adjusted to be less than the number of pores P per unit area in the first regions 112a, 113a, thereby improving moisture resistance reliability even when the dielectric layer 111 and the first and second internal electrodes 121, 122 are thin films having a thickness of 0.4 μm or less.
[0099] However, the above thin film does not mean that the thickness of the dielectric layer 111 and the first and second internal electrodes 121, 122 is 0.4 μm or less, but can be understood as a concept including a dielectric layer and internal electrodes that are thinner than those of conventional products.
[0100] Meanwhile, the thickness t1a of the first regions 112a and 113a may be 12 μm or less, and the thickness t1b of the second regions 112b and 113b may be 3 μm or less, but is not necessarily limited thereto.
[0101] Referring to FIG. 4, the ratio of the thickness t2 of the first or second side margin region contacting the end of the internal electrode located at the outermost position to the thickness t1 of the first or second side margin region contacting the end of the internal electrode located in the center among the multiple internal electrodes 121, 122 may be 1.0 or less.
[0102] The lower limit of the ratio of the thickness t2 of the first or second side margin region in contact with the end of the internal electrode located at the outermost position to the thickness t1 of the first or second side margin region in contact with the end of the internal electrode located in the central portion is not particularly limited, but is preferably 0.9 or more.
[0103] According to one embodiment of the present invention, unlike the conventional technology, the first or second side margin portion is formed by attaching a ceramic green sheet to a side of a ceramic body, so that the thickness of each position of the first or second side margin portion is uniform.
[0104] That is, conventionally, the side margins have been formed by coating or printing a ceramic slurry, and therefore the thickness of the side margins varies greatly from position to position.
[0105] Specifically, in the past, the thickness of the first or second side margin region that contacts the end of the internal electrode arranged in the center of the ceramic body was made thicker than the thickness of other regions.
[0106] For example, in the past, the ratio of the thickness of the first or second side margin region in contact with the end of the internal electrode located at the outermost position to the thickness of the first or second side margin region in contact with the end of the internal electrode located in the central portion was less than 0.9, showing a large variation.
[0107] In the conventional case where there was large variation in thickness from position to position in the side margin portion, the side margin portion occupied a large portion of a multilayer ceramic capacitor of the same size, making it impossible to ensure a large size for the capacitance forming portion, and therefore difficult to ensure high capacitance.
[0108] In contrast, in one embodiment of the present invention, the average thickness of the first and second side margin portions 112, 113 is 2 μm or more and 10 μm or less, and the ratio of the thickness t2 of the first or second side margin portion region contacting the end of the internal electrode located at the outermost position to the thickness t1 of the first or second side margin portion region contacting the end of the internal electrode located in the center of the multiple internal electrodes 121, 122 is 0.9 or more and 1.0 or less, so that the thickness of the side margin portion is thin, the thickness variation is small, and a large size of the capacitance forming portion can be ensured.
[0109] This makes it possible to realize a high-capacity multilayer ceramic capacitor.
[0110] Meanwhile, referring to FIG. 4, the ratio of the thickness t3 of the first or second side margin region contacting the corner of the ceramic body 110 to the thickness t1 of the first or second side margin region contacting the end of the internal electrode located in the center of the plurality of internal electrodes 121, 122 may be 1.0 or less.
[0111] It is preferable that the lower limit of the ratio of the thickness t3 of the first or second side margin region in contact with the corner of the ceramic body 110 to the thickness t1 of the first or second side margin region in contact with the end of the internal electrode arranged in the central portion is 0.9 or more.
[0112] Due to the above-mentioned features, the variation in thickness between the regions of the side margin portion is small, so that the size of the capacitance forming portion can be ensured to be large, thereby making it possible to realize a multilayer ceramic capacitor with high capacitance.
[0113] FIG. 6 is a side view showing a ceramic body according to another embodiment of the present invention, as viewed from the direction A in FIG.
[0114] Referring to FIG. 6, in a multilayer ceramic electronic component according to another embodiment of the present invention, the cover parts 114, 115 are divided into first regions 114a, 115a adjacent to the fifth surface 5 and the sixth surface 6 of the ceramic body 110 and second regions 114b, 115b adjacent to the internal electrodes 121, 122, and the number of pores per unit area in the second regions 114b, 115b may be less than the number of pores per unit area in the first regions 114a, 115a.
[0115] The cover parts 114 and 115 may be composed of an upper cover part 114 and a lower cover part 115 formed on the upper and lower parts of the active part.
[0116] The upper cover part 114 and the lower cover part 115 may be divided into first regions 114a and 115a adjacent to the fifth surface 5 and the sixth surface 6 of the ceramic body 110, and second regions 114b and 115b adjacent to the internal electrodes 121 and 122, respectively.
[0117] The upper cover part 114 and the lower cover part 115 are divided into two regions having different sizes of dielectric grains, and the number of pores in the second regions 114b and 115b is adjusted to be less than the number of pores in the first regions 114a and 115a, thereby improving moisture resistance reliability.
[0118] According to one embodiment of the present invention, in the cover portion, the ratio of the number of pores per unit area in the second regions 114b, 115b to the number of pores per unit area in the first regions 114a, 115a may be 0.8 or less.
[0119] By adjusting the ratio of the number of pores per unit area in the second regions 114b and 115b to the number of pores per unit area in the first regions 114a and 115a to 0.8 or less, the moisture resistance reliability can be improved.
[0120] When the ratio of the number of pores per unit area in the second regions 114b, 115b to the number of pores per unit area in the first regions 114a, 115a exceeds 0.8, there is no difference between the number of pores per unit area in the first regions 114a, 115a and the second regions 114b, 115b, and therefore the improvement in moisture resistance reliability is slight.
[0121] There is no particular limitation on the method for adjusting the number of pores per unit area in the second regions 114b, 115b adjacent to the internal electrodes 121, 122 to be less than the number of pores per unit area in the first regions 114a, 115a adjacent to the fifth surface 5 and sixth surface 6 of the ceramic body 110, but this can be achieved, for example, by adjusting the size of ceramic powder as raw material added during the formation of the first regions 114a, 115a and the second regions 114b, 115b.
[0122] For example, this can be achieved by making the grain size of barium titanate (BaTiO3) powder, which is the raw material for forming the second regions 114b, 115b of the cover portion adjacent to the internal electrodes 121, 122, larger than the grain size of barium titanate (BaTiO3) powder, which is the raw material for forming the first regions 114a, 115a adjacent to the fifth surface 5 and sixth surface 6 of the ceramic body 110.
[0123] Although not particularly limited, for example, the particle size of barium titanate (BaTiO3) powder, which is the raw material for forming the second regions 114b, 115b of the cover part adjacent to the internal electrodes 121, 122, may be about 70 nm, and the particle size of barium titanate (BaTiO3) powder, which is the raw material for forming the first regions 114a, 115a adjacent to the fifth surface 5 and sixth surface 6 of the ceramic body 110, may be about 40 nm.
[0124] According to one embodiment of the present invention, by adjusting the size of the ceramic powder as a raw material input during the formation process of the first regions 114a, 115a and the second regions 114b, 115b as described above, after firing, the size of the dielectric grains contained in the first regions 114a, 115a can be 90 nm or more and 410 nm or less, and the size of the dielectric grains contained in the second regions 114b, 115b can be 170 nm or more and 700 nm or less.
[0125] The method for measuring the size of the dielectric grains is the same as the method for measuring the size of the dielectric grains included in the side margin portion described above.
[0126] In the upper and lower cover parts 114 and 115, the second regions 114b and 115b contain more magnesium (Mg) than the first regions 114a and 115a.
[0127] The upper and lower cover parts 114, 115 of the ceramic body 110 are divided into two regions having different compositions, and in this case, the magnesium (Mg) content in each region is made different, thereby improving the density of the upper and lower cover parts 114, 115 and improving the moisture resistance.
[0128] By adjusting the magnesium (Mg) content in the second regions 114b, 115b of the upper and lower cover parts 114, 115 to be greater than the magnesium (Mg) content in the outer first regions 114a, 115a, the density of the second regions 114b, 115b of the upper and lower cover parts 114, 115 can be improved, thereby improving the moisture resistance.
[0129] In addition, the content of magnesium (Mg) in the second regions 114b and 115b of the upper and lower cover parts 114 and 115 may be 10 moles or more and 30 moles or less based on the titanium (Ti) contained in the upper and lower cover parts 114 and 115.
[0130] The magnesium (Mg) content of the second regions 114b, 115b of the upper and lower cover parts 114, 115 is adjusted to be 10 moles or more and 30 moles or less relative to the titanium (Ti) contained in the upper and lower cover parts 114, 115, thereby improving the moisture resistance reliability.
[0131] 7a to 7g are cross-sectional and perspective views illustrating a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention.
[0132] According to another embodiment of the present invention, a method for manufacturing a ceramic green sheet laminate includes the steps of: preparing a first ceramic green sheet on which a plurality of first internal electrode patterns are formed at predetermined intervals, and a second ceramic green sheet on which a plurality of second internal electrode patterns are formed at predetermined intervals; laminating the first ceramic green sheet and the second ceramic green sheet such that the first internal electrode pattern and the second internal electrode pattern cross each other to form a ceramic green sheet laminate body; cutting the ceramic green sheet laminate body so that ends of the first internal electrode pattern and the second internal electrode pattern have side surfaces exposed in a width direction; and forming a first sub-layer on the side surfaces exposed at the ends of the first internal electrode pattern and the second internal electrode pattern. forming an edge margin portion and a second side margin portion; and firing the cut laminated body to manufacture a ceramic body including a dielectric layer and first and second internal electrodes, wherein the ceramic body includes first and second internal electrodes arranged to face each other with the dielectric layer therebetween, an active portion in which capacitance is formed, and cover portions formed on upper and lower portions of the active portion, the first and second side margin portions being divided into a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the exposed internal electrodes, and the number of pores per unit area in the second region is smaller than the number of pores per unit area in the first region.
[0133] Hereinafter, a method for manufacturing a multilayer ceramic capacitor according to another embodiment of the present invention will be described.
[0134] 7a, a plurality of stripe-shaped first internal electrode patterns 221 are formed at predetermined intervals on a ceramic green sheet 211. The plurality of stripe-shaped first internal electrode patterns 221 may be formed parallel to each other.
[0135] The ceramic green sheet 211 may be formed of a ceramic paste containing ceramic powder, an organic solvent, and an organic binder.
[0136] The ceramic powder is a material having a high dielectric constant, and may be, but is not limited to, a barium titanate (BaTiO3)-based material, a lead complex perovskite-based material, or a strontium titanate (SrTiO3)-based material, and preferably, a barium titanate (BaTiO3) powder. When the ceramic green sheet 211 is fired, it becomes the dielectric layer 111 that constitutes the ceramic body 110.
[0137] The stripe-shaped first internal electrode pattern 221 may be formed of an internal electrode paste containing a conductive metal, which may be, but is not limited to, nickel (Ni), copper (Cu), palladium (Pd), or an alloy thereof.
[0138] The method for forming the stripe-shaped first internal electrode pattern 221 on the ceramic green sheet 211 is not particularly limited, and may be, for example, a printing method such as a screen printing method or a gravure printing method.
[0139] Although not shown, a plurality of stripe-shaped second internal electrode patterns 222 may be formed on another ceramic green sheet 211 at predetermined intervals.
[0140] Hereinafter, the ceramic green sheet on which the first internal electrode pattern 221 is formed will be referred to as a first ceramic green sheet, and the ceramic green sheet on which the second internal electrode pattern 222 is formed will be referred to as a second ceramic green sheet.
[0141] Next, as shown in FIG. 7b, the first and second ceramic green sheets may be alternately laminated so that the stripe-shaped first internal electrode pattern 221 and the stripe-shaped second internal electrode pattern 222 are laminated in an intersecting manner.
[0142] Thereafter, the stripe-shaped first internal electrode pattern 221 may become the first internal electrode 121 , and the stripe-shaped second internal electrode pattern 222 may become the second internal electrode 122 .
[0143] According to another embodiment of the present invention, the first and second ceramic green sheets have a thickness td of 0.6 μm or less, and the first and second internal electrode patterns have a thickness te of 0.5 μm or less.
[0144] The present invention is characterized in that the dielectric layer has a thickness of 0.4 μm or less, and the internal electrode has a thickness of 0.4 μm or less, and the first and second ceramic green sheets have a thickness td of 0.6 μm or less, and the first and second internal electrode patterns have a thickness te of 0.5 μm or less.
[0145] FIG. 7c is a cross-sectional view showing a ceramic green sheet laminated body 220 in which first and second ceramic green sheets are stacked according to one embodiment of the present invention, and FIG. 7d is a perspective view showing a ceramic green sheet laminated body 220 in which first and second ceramic green sheets are stacked.
[0146] Referring to Figures 7c and 7d, a first ceramic green sheet having a plurality of parallel stripe-shaped first internal electrode patterns 221 printed thereon and a second ceramic green sheet having a plurality of parallel stripe-shaped second internal electrode patterns 222 printed thereon are alternately stacked on each other.
[0147] More specifically, the first ceramic green sheet may be laminated such that the center of the stripe-shaped first internal electrode pattern 221 printed on the first ceramic green sheet overlaps with the space between the stripe-shaped second internal electrode patterns 222 printed on the second ceramic green sheet.
[0148] 7d, the ceramic green sheet laminated body 220 may be cut across the plurality of stripe-shaped first internal electrode patterns 221 and the plurality of stripe-shaped second internal electrode patterns 222. That is, the ceramic green sheet laminated body 220 may become a laminated body 210 cut along C1-C1 and C2-C2 cutting lines that are perpendicular to each other.
[0149] More specifically, the stripe-shaped first internal electrode pattern 221 and the stripe-shaped second internal electrode pattern 222 can be cut in the length direction to divide them into a plurality of internal electrodes having a certain width. At this time, the laminated ceramic green sheets are also cut together with the internal electrode patterns. As a result, the dielectric layer can be formed to have the same width as the width of the internal electrodes.
[0150] Also, cutting can be performed along the C2-C2 cutting line according to the size of each individual ceramic body. That is, before forming the first side margin portion and the second side margin portion, the rod-shaped laminate can be cut along the C2-C2 cutting line to the size of each individual ceramic body, thereby forming a plurality of laminate bodies 210.
[0151] That is, the bar-shaped laminate can be cut so that the center of the overlapping first internal electrodes and the predetermined gap formed between the overlapping second internal electrodes are cut along the same cutting line, whereby one end of the first internal electrodes and one end of the second internal electrodes can be alternately exposed on the cut surface.
[0152] Then, a first side margin portion and a second side margin portion may be formed on the first and second side surfaces of the laminated body 210 .
[0153] Next, as shown in FIG. 7e, a second region 212b of the first side margin portion may be formed on the first side surface of the laminated body 210. As shown in FIG.
[0154] Specifically, the second region 212b of the first side margin is formed by placing a ceramic green sheet for the side surface on top of a punched elastic material 300 made of rubber.
[0155] Next, the multilayer body 210 is rotated 90 degrees so that a first side surface of the multilayer body 210 faces the side surface ceramic green sheet, and then the multilayer body 210 is pressed and adhered to the side surface ceramic green sheet.
[0156] When the laminated body 210 is pressed against the ceramic green sheet for the side surface to transfer the ceramic green sheet for the side surface to the laminated body 210, the ceramic green sheet for the side surface can be formed up to the corners of the side surface of the laminated body 210 by the rubber punching elastic material 300, and the remaining portion can be cut off.
[0157] This makes it possible to form the second region 212b of the first side margin portion on the first side surface of the laminated body 210, as shown in FIG. 7f.
[0158] Thereafter, the laminated body 210 is rotated, whereby a second region of the second side margin portion can be formed on the second side surface of the laminated body 210.
[0159] Next, as shown in FIG. 7g, a first region 212a of a first side margin portion may be formed on a first side surface of the laminated body 210. As shown in FIG.
[0160] The method of forming the first region 212a of the first side margin portion on the first side surface of the laminated body 210 is similar to the method of forming the second region 212b of the first side margin portion on the first side surface of the laminated body 210 described above.
[0161] Next, the laminated body 210 having the first and second side margin portions formed on both sides thereof is calcined and fired to form a ceramic body including the dielectric layer and the first and second internal electrodes.
[0162] Then, external electrodes may be formed on a third side surface of the ceramic body where the first internal electrode is exposed and a fourth side surface of the ceramic body where the second internal electrode is exposed.
[0163] According to another embodiment of the present invention, the side ceramic green sheets are thin and have small variations in thickness, so that a large size of the capacitance forming portion can be ensured.
[0164] Specifically, the average thickness of the first and second side margin portions 112, 113 after firing is between 2 μm and 15 μm, and there is little variation in thickness from position to position, so that a large size of the capacitance forming portion can be ensured.
[0165] This makes it possible to realize a high-capacity multilayer ceramic capacitor.
[0166] In addition, descriptions of features that are the same as those in the embodiment of the present invention described above will be omitted here to avoid duplication.
[0167] The present invention will be described in more detail below by way of experimental examples. However, these are merely for the purpose of concretely understanding the invention, and the scope of the present invention is not limited to these experimental examples.
[0168] Experimental Example According to an embodiment of the present invention, a comparative example in which a conventional side margin portion is formed and an example in which a side margin portion including first and second regions having different sizes of dielectric grains is formed were prepared.
[0169] Then, a ceramic green sheet laminate body was formed so that the internal electrodes were exposed in the width direction and side ceramic green sheets could be attached to the electrode exposed portions of the green chips that had no margins, as in the above comparative example and example, to form side margin portions.
[0170] A multilayer ceramic capacitor green chip with 0603 size (width x length x height: 0.6mm x 0.3mm x 0.3mm) was produced by attaching ceramic green sheets for forming sides to both sides of the ceramic green sheet laminate body while applying a certain temperature and pressure under conditions that minimize deformation of the chip.
[0171] The multilayer ceramic capacitor test pieces thus manufactured were subjected to a calcination process in a nitrogen atmosphere at 400°C or less, and then sintered under the conditions of a sintering temperature of 1200°C or less and a hydrogen concentration of 0.5% H2 or less, and then electrical characteristics such as appearance defects, insulation resistance, and moisture resistance were comprehensively checked.
[0172] FIG. 8 is a graph comparing the results of a moisture resistance reliability test according to an embodiment of the present invention and a comparative example.
[0173] In Figure 8, Figure 8(a) is a comparative example, which has a conventional multilayer ceramic capacitor structure and has no difference in the number of pores contained in the side margin portions, and Figure 8(b) is an embodiment, which shows that in the first and second side margin portions 112, 113, the number of pores per unit area in the second regions 112b, 113b is smaller than the number of pores per unit area in the first regions 112a, 113a.
[0174] It is clear that the comparative example has a problem with moisture resistance reliability, whereas the embodiment example has excellent moisture resistance reliability.
[0175] The present invention is not limited by the above-described embodiments and the accompanying drawings, but is limited by the scope of the accompanying claims. Therefore, within the scope of the technical idea of the present invention described in the claims, various substitutions, modifications, and changes are possible by a person having ordinary skill in the art, and these also belong to the scope of the present invention. [Explanation of symbols]
[0176] 110 Ceramic body 111 Dielectric layer 112 First side margin 113 Second side margin 121 1st internal electrode 122 2nd internal electrode 131 1st external electrode 132 2nd external electrode
Claims
1. a ceramic body including a dielectric layer, the ceramic body having a first surface and a second surface facing each other, a third surface and a fourth surface connecting the first surface and the second surface, and a fifth surface and a sixth surface connecting the first surface to the fourth surface and facing each other; a plurality of internal electrodes disposed inside the ceramic body, exposed to the first surface and the second surface, and having one end exposed to the third surface or the fourth surface; a first side margin portion and a second side margin portion disposed on ends of the internal electrodes exposed on the first surface and the second surface, the ceramic body includes a plurality of internal electrodes arranged to face each other with the dielectric layer interposed therebetween, an active portion in which capacitance is formed, and cover portions formed on upper and lower portions of the active portion, a first region adjacent to an outer surface of the side margin portion and a second region adjacent to an internal electrode exposed to the first surface and the second surface, a number of pores per unit area in the second region being smaller than a number of pores per unit area in the first region, a size of dielectric grains included in the first region being smaller than a size of dielectric grains included in the second region, and a magnesium (Mg) content included in the second region being greater than a magnesium (Mg) content included in the first region.
2. 2. The multilayer ceramic capacitor according to claim 1, wherein a ratio of the number of pores per unit area in the second region to the number of pores per unit area in the first region is 0.8 or less.
3. 3. The multilayer ceramic capacitor according to claim 1, wherein the cover portion is divided into a first region adjacent to a fifth surface and a sixth surface of the ceramic body and a second region adjacent to the internal electrode, and the number of pores per unit area in the second region is smaller than the number of pores per unit area in the first region.
4. 4. The multilayer ceramic capacitor according to claim 3, wherein a ratio of the number of pores per unit area in the second region to the number of pores per unit area in the first region of the cover is 0.8 or less.
5. The multilayer ceramic capacitor of claim 3 , wherein a magnesium (Mg) content in the second region of the cover is greater than a magnesium (Mg) content in the first region of the cover.
6. 2. The multilayer ceramic capacitor according to claim 1, wherein the dielectric layer has a thickness of 0.4 μm or less.
7. 2. The multilayer ceramic capacitor according to claim 1, wherein the internal electrodes have a thickness of 0.4 [mu]m or less.
8. 2. The multilayer ceramic capacitor according to claim 1, wherein the dielectric layers have a thickness of 0.4 [mu]m or less, and the internal electrodes have a thickness of 0.4 [mu]m or less.
9. 2. The multilayer ceramic capacitor according to claim 1, wherein the first region has a thickness of 12 [mu]m or less, and the second region has a thickness of 3 [mu]m or less.
10. preparing a first ceramic green sheet having a plurality of first internal electrode patterns formed at predetermined intervals and a second ceramic green sheet having a plurality of second internal electrode patterns formed at predetermined intervals; forming a ceramic green sheet laminate body by stacking the first ceramic green sheet and the second ceramic green sheet such that the first internal electrode pattern and the second internal electrode pattern cross each other; cutting the ceramic green sheet laminate body so that ends of the first internal electrode pattern and the second internal electrode pattern have exposed sides in a width direction; forming a first side margin portion and a second side margin portion on sides where ends of the first internal electrode pattern and the second internal electrode pattern are exposed; and firing the cut laminated body to manufacture a ceramic body including the dielectric layers and the first and second internal electrodes. the ceramic body includes first and second internal electrodes disposed to face each other with the dielectric layer therebetween, an active portion in which capacitance is formed, and cover portions formed on upper and lower portions of the active portion, a first region adjacent to an outer surface of the side margin portion and a second region adjacent to the exposed internal electrode, a number of pores per unit area in the second region being smaller than a number of pores per unit area in the first region, a size of dielectric grains included in the first region being smaller than a size of dielectric grains included in the second region, and a magnesium (Mg) content included in the second region being greater than a magnesium (Mg) content included in the first region.
11. The method for producing a multilayer ceramic capacitor according to claim 10 , wherein a ratio of the number of pores per unit area in the second region to the number of pores per unit area in the first region is 0.8 or less.
12. 12. The method for manufacturing a multilayer ceramic capacitor according to claim 10, wherein the cover portion is divided into a first region adjacent to a fifth surface and a sixth surface of the ceramic body and a second region adjacent to the internal electrode, and the number of pores per unit area in the second region is smaller than the number of pores per unit area in the first region.
13. The method for manufacturing a multilayer ceramic capacitor according to claim 12 , wherein a ratio of the number of pores per unit area in the second region to the number of pores per unit area in the first region of the cover is 0.8 or less.
14. The method of claim 12, wherein a magnesium content in the second region of the cover is greater than a magnesium content in the first region of the cover.
15. The method for manufacturing a multilayer ceramic capacitor according to claim 10, wherein the first ceramic green sheet and the second ceramic green sheet have a thickness of 0.6 μm or less.
16. The method of claim 10, wherein the first internal electrode pattern and the second internal electrode pattern have a thickness of 0.5 μm or less.
17. The method of claim 10, wherein the dielectric layers have a thickness of 0.4 μm or less, and the first and second internal electrodes have a thickness of 0.4 μm or less.
18. The method for manufacturing a multilayer ceramic capacitor according to claim 10, wherein the first region has a thickness of 12 μm or less, and the second region has a thickness of 3 μm or less.
Citation Information
Patent Citations
Multilayer ceramic electronic component
JP2006278557A
Multilayer ceramic capacitor and manufacturing method for the same
JP2017147429A
Multilayer ceramic capacitor and method for manufacturing the same
JP2018107239A