Fibers, fiber manufacturing methods
A fiber manufacturing method using IGCC waste as a raw material addresses the inefficiency in waste utilization by producing high-strength fibers suitable for diverse applications, enhancing waste management and reducing material costs.
Patent Information
- Application Number
- JP2022510035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-24
- Filing Date
- 2021-03-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-18
AI Technical Summary
There is a lack of effective methods to utilize waste generated from integrated coal gasification combined cycle (IGCC) power generation, limiting the efficient use of this waste material.
The development of a fiber manufacturing method that utilizes IGCC waste, such as slag and coal ash, as a raw material, specifically controlling the composition of SiO2, Al2O3, and CaO to achieve high melt spinnability and amorphousness, resulting in high-strength fibers.
This method enables the effective utilization of IGCC waste by producing high-strength fibers that can be processed into various materials, such as rovings, chopped strands, and woven fabrics, thereby reducing waste and lowering material costs.
Smart Images

Figure 0007586515000001 
Figure 0007586515000002 
Figure 0007586515000003
Abstract
Description
[Technical field]
[0001] The present invention relates to fibers and methods for producing fibers. [Background technology]
[0002] Integrated coal gasification combined cycle (IGCC) is known as one type of thermal power generation that uses coal as fuel. In IGCC, coal gasification gas is used as fuel to drive a gas turbine to generate electricity, and exhaust heat from the gas turbine is recovered to generate steam, which is then used to drive a steam turbine to generate electricity.
[0003] By using IGCC, it is possible to generate electricity with higher thermal efficiency than conventional coal-fired power plants. Specifically, in the case of a commercial IGCC at 1400-1500 degrees, a thermal efficiency of about 48-50% based on the lower heating value can be achieved at the transmission end. This is higher than the thermal efficiency of about 40% for conventional supercritical coal-fired power plants (SC) and ultra-supercritical coal-fired power plants (USC), and is equivalent to the thermal efficiency of advanced ultra-supercritical coal-fired power plants (A-USC) currently under development. In addition, IGCC can use low-grade coal that could not be used in conventional coal-fired power plants, so it is expected to reduce fuel costs and diversify fuel procurement sources.
[0004] As described above, IGCC is expected to be a highly efficient next-generation power generation method. However, the only established method for utilizing the waste generated during the operation of IGCC is to crush and process it as aggregate for cement (see Patent Document 1), and there is room for further improvement. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-014052 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a fiber and a fiber manufacturing method that can more effectively utilize waste discharged from integrated coal gasification combined cycle power generation. [Means for solving the problem]
[0007] In order to solve the above problems, the fiber according to the present invention is characterized in that it contains waste discharged from an integrated coal gasification combined cycle (IGCC) as a raw material. Effect of the Invention
[0008] According to the present invention, it is possible to provide a fiber and a fiber manufacturing method that can more effectively utilize waste discharged from an integrated coal gasification combined cycle power generation. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a diagram showing the component composition of the raw material (IGCC waste) in Example 1. [Diagram 2] FIG. 1 is a diagram showing an outline of an electric furnace used in Example 1. [Diagram 3] 1 is a table showing the results of melt spinnability in Example 1. [Figure 4] 1 is a table showing temperature conditions in Example 1. [Diagram 5] 2 is a graph showing temperature conditions in Example 1. [Figure 6] 1 is an XRD spectrum of a fiber formed from raw material S1. [Figure 7] FIG. 2 is a magnified view (micrograph) of a fiber formed from feedstock S1. [Figure 8] FIG. 11 is a diagram showing the mixing ratio (%) of raw materials according to Example 2. [Figure 9] FIG. 10 is a diagram showing the component composition of waste materials etc. according to Example 2. [Figure 10]FIG. 4 is a diagram showing the component composition of raw materials according to Example 2. [Figure 11] 1 is a table showing the results of melt spinnability and the like of the raw material according to Example 2. [Figure 12] 1 is a table showing temperature conditions in Example 2. [Figure 13] 1 is a graph showing temperature conditions in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. SiO 2 is called the S component, and SiO 2 The content of may be indicated as [S]. Al 2 O 3 is called the A component, and Al 2 O 3 The content of may be expressed as [A]. CaO is sometimes referred to as the C component, and the CaO content is sometimes expressed as [C].
[0011] [Embodiment 1] The fiber according to the first embodiment is made from waste discharged from an integrated coal gasification combined cycle (IGCC) (hereinafter, also referred to as IGCC waste. IGCC waste includes slag, coal ash, etc. discharged from IGCC). The IGCC waste, which is the raw material, is a material containing SiO 2 and Al 2 O 3 The main component is SiO in the fiber. 2 and Al 2 O 3 Al in the total 2 O 3 The ratio of is within a specific range, and further contains a specific amount of CaO.
[0012] The raw material of the fiber according to the first embodiment is IGCC waste, and the SiO 2 and Al 2 O 3The total content of [S] and [A] is preferably 40% by mass or more and 70% by mass or less. When the total of [S] and [A] is less than 40% by mass or more than 70% by mass, the melting temperature of the raw material becomes high or the viscosity of the melt becomes high, resulting in poor melt spinnability. Melt spinning refers to a technique in which the raw material is melted by heat, the molten material is discharged from a hole (through hole) formed in a spinneret, and then cooled and solidified. Melt spinnability refers to the ease of producing fibers by melt spinning.
[0013] The raw material of the fiber according to the first embodiment is SiO 2 and Al 2 O 3 Al in the total 2 O 3 The ratio ([A] / ([A]+[S])) (mass ratio) is preferably within the range of 0.15 to 0.40. When the ratio (mass ratio) [A] / ([A]+[S]) is either less than 0.15 or more than 0.40, the fiber has a high melting temperature or a high viscosity of the molten material, resulting in poor melt spinnability.
[0014] The raw material of the fiber according to the first embodiment preferably contains CaO in an amount of 5% by mass or more and 30% by mass or less. If the CaO content is less than 5% by mass, the melting temperature of the fiber becomes high, which is undesirable from the viewpoint of energy saving. In addition, the CaO content is more preferably 30% by mass or less.
[0015] The raw material of the fiber according to the first embodiment is SiO 2 , Al 2 O 3 As long as the above-mentioned compositional conditions are satisfied, the fiber according to the first embodiment can be obtained without any restriction on the raw materials. As the raw material for the fiber according to the first embodiment, it is preferable to use waste materials discharged by integrated coal gasification combined cycle (IGCC) (IGCC waste materials) and the like. The IGCC waste materials contain SiO, SiO2, SiO3, SiO4, SiO5, SiO6, SiO7, SiO8, SiO9, SiO2, SiO2, SiO2, SiO3, SiO4, SiO5, SiO6, SiO2, SiO2, SiO2, SiO2, SiO2, SiO2, SiO3, SiO4, SiO5, SiO2 ... 2 , Al 2 O 3This is because it is suitable for obtaining the fiber according to the first embodiment and the raw material cost can be reduced.
[0016] The fiber according to the first embodiment does not exclude the inclusion of unavoidable impurities. The main unavoidable impurities are MgO, Na 2 OK 2 O, TiO 2 , CrO 2 etc.
[0017] In the present embodiment 1, there is no substantial difference between the component ratio (mass ratio) of the raw material and the component ratio (mass ratio) of the fiber produced by melting the raw material, and therefore the component ratio of the raw material can be regarded as the component ratio of the fiber produced by melting the raw material.
[0018] The fiber according to the first embodiment is highly amorphous. Therefore, the fiber hardly experiences a decrease in strength due to separation between the crystalline phase and the amorphous phase, and a high-strength fiber can be obtained. Here, the degree of amorphousness, which is a measure of amorphousness, is calculated from an X-ray diffraction (XRD) spectrum by the following formula (1). Amorphousity (%)=[la / (la+lc)]×100...(1) In the above formula (1), la and lc are as follows, respectively. la: the integral of the scattering intensity of the amorphous halo. lc: the integral value of the scattering intensity of the crystalline peak when the fiber is subjected to X-ray diffraction analysis. The degree of amorphization of the fiber according to the first embodiment usually exhibits a value of 90% or more, depending on the composition. The degree of amorphization of the fiber can reach 95% or more in high cases, and in the highest case, the fiber is substantially composed of only an amorphous phase. Here, "substantially composed of only an amorphous phase" means that only an amorphous halo is observed in the X-ray diffraction spectrum, and no crystalline peaks are observed. EXAMPLES
[0019] The first embodiment will be described below. In the following test examples, IGCC waste discharged from an integrated coal gasification combined cycle (IGCC) was prepared as the raw material for the fiber (raw material S1). The IGCC waste used was discharged from a domestic integrated coal gasification combined cycle. Raw material S1 was 100% IGCC waste.
[0020] In this Example 1, the components of the raw material S1 (IGCC waste) were analyzed by fluorescent X-ray analysis. Figure 1 shows the component composition of the raw material S1 (IGCC waste).
[0021] An electric furnace was used to manufacture the raw material S1 into a fiber. The outline of the electric furnace is shown in FIG. 2. The electric furnace 1 is a cylinder having a height H of 60 cm and an outer diameter D of 50 cm, with a through hole 4 having an inner diameter d of 10 cm formed in the center. A Tammann tube 2 having an inner diameter of 2.1 cm and a length of 10 cm is suspended in the through hole 4 by a hanging rod 3. 30 g of raw material (raw material S1) is charged in the Tammann tube 2. A hole having a diameter of 2 mm is provided in the center of the bottom of the Tammann tube 2, and when the compound is melted by heating, it flows out from the hole provided in the bottom of the Tammann tube by gravity. The melt that flows out comes into contact with the outside air, cools, and solidifies to become a fiber. Here, the melt that flows out is rapidly cooled, so that the fiber is substantially composed of only amorphous matter.
[0022] The electric furnace is heated according to a predetermined heating program, and it has been confirmed in advance that the temperature of the molten material in the Tammann tube 2 follows a temperature approximately 50° C. lower than the temperature inside the furnace.
[0023] The melt spinning conditions and the results of melt spinning of the raw material S1 in Example 1 are shown in FIG. In this Example 1, the melt spinnability was evaluated as follows. 〇: It becomes a long continuous thread. △: The molten and softened raw material comes out from the hole at the bottom of the Tammann tube, and although very short fibers are generated, they do not form a continuous long thread. ×: Nothing comes out of the hole provided at the bottom of the Tammann tube, and no thread is formed.
[0024] Fig. 3 is a table showing the results of the temperature maintenance (annealing), the temperature change, and the melt spinnability of the raw material S1 used in Examples A1 and A2 and Comparative Examples E1 to E3. Fig. 4 is a table showing the change in the furnace temperature over time in Examples A1 and A2 and Comparative Examples E1 to E3. FIG. 4(a) is a table showing the change in furnace temperature over time in Example A1. FIG. 4(b) is a table showing the change in furnace temperature over time in Example A2. FIG. 4(c) is a table showing the change in furnace temperature over time in Comparative Example E1. FIG. 4(d) is a table showing the change in furnace temperature over time in Comparative Example E2. FIG. 4(e) is a table showing the change in furnace temperature over time in Comparative Example E3. FIG. 5 is a graph showing the change over time in the temperature inside the furnace for Examples A1 and A2 and Comparative Examples E1 to E3 shown in FIG.
[0025] (Example A1) Raw material S1 was placed in a Tamman tube. Next, the temperature inside the furnace was raised to 1350°C (the temperature of raw material S1 was 1300°C), and then it was held at approximately 1350°C for a specified time (55 minutes) (temperature holding: "Good"). After that, the temperature inside the furnace was changed (temperature change: "Good") and the spinnability was checked, and raw material S1 became a fiber (melt spinnability: "Good").
[0026] (Example A2) Raw material S1 was placed in a Tamman tube. Next, the temperature inside the furnace was raised to 1375°C (the temperature of raw material S1 was 1325°C), and then it was maintained at approximately 1375°C for a specified time (120 minutes) (temperature maintenance: "Good"). After that, the spinnability was checked while changing the temperature inside the furnace (temperature change: "Good"). Raw material S1 became a fiber (melt spinnability: "Good").
[0027] (Comparative Example E1) After the raw material S1 was placed in the Tamman tube, the temperature inside the furnace was raised to 1350°C (the temperature of the raw material S1 was 1300°C), and then it was maintained at approximately 1350°C for a specified time (94 minutes) (temperature maintenance: "Good"). After that, the spinnability was checked without changing the temperature inside the furnace (temperature change: "Poor"). However, the raw material S1 did not become a fiber (melt spinnability: "Poor").
[0028] (Comparative example E2) After setting raw material S1 in the Tammann tube, the temperature inside the furnace was raised to 1400°C (the temperature of raw material S1 was 1350°C), and then the spinnability was checked while changing the temperature inside the furnace (temperature change "◯"), but although the molten and softened raw material came out from the hole at the bottom of the Tammann tube and very short fibers were generated, raw material S1 did not become fiber (melt spinnability "△"). In addition, after raising the temperature to 1400°C, the temperature was not maintained for a specified period of time (temperature maintenance "X").
[0029] (Comparative example E3) After placing raw material S1 in the Tamman tube, the temperature inside the furnace was raised to 1320°C (the temperature of raw material S1 was 1270°C), and then it was maintained at approximately 1320°C for a specified time (20 minutes) (temperature maintenance: "Good"). Thereafter, it was confirmed whether raw material S1 could be spun without changing the temperature inside the furnace (temperature change: "Poor"). However, raw material S1 did not become fiber (melt spinnability: "Poor").
[0030] (Consideration) Examples A1 and A2 and Comparative Examples E1 to E3 demonstrated that fibers can be produced using IGCC waste discharged from an integrated coal gasification combined cycle (IGCC) plant as a raw material. It was confirmed that the following conditions are preferable for producing fiber using IGCC waste as a raw material. (1) Heat to over 1,300 degrees. (2) Before being molded into fiber, the material is kept at a temperature of 1,300° C. or higher for a predetermined period of time (preferably 50 minutes or more, and more preferably 55 minutes or more). (3) The IGCC waste is allowed to flow out of the formation hole while changing its temperature (in this embodiment, the temperature is increased).
[0031] Figure 6 shows the XRD spectrum of the fiber formed from the raw material S1. As shown in Figure 6, the XRD spectrum of the fiber obtained in Example A1 shows only an amorphous halo and no crystalline peak. This indicates that the fiber produced from the IGCC waste is substantially composed of only amorphous matter.
[0032] FIG. 7 is an enlarged view (microscope photograph) of a fiber formed from the raw material S1 shown in FIG. 6. As shown in FIG. 7, a fiber having an outer diameter exceeding 500 μm was obtained. This fiber is substantially made of only amorphous material, as described with reference to FIG. 6. This is believed to be because the IGCC waste in a molten state flows out of the hole provided in the center of the bottom of the Tammann tube 2, and then is rapidly cooled, resulting in a loss of regular atomic arrangement and becoming amorphous. In this Example 1, it was found that the fiber having an outer diameter exceeding 500 μm was substantially made of only amorphous material. Here, it is generally believed that the smaller the outer diameter of a fiber, the faster the cooling rate. Therefore, if the outer diameter is smaller than the outer diameter (505.97 μm) of the fiber shown in FIG. 7, it can be estimated that the fiber is substantially made of only amorphous material. More specifically, if the outer diameter is 500 μm or less, it can be estimated that the fiber is substantially made of only amorphous material.
[0033] [Embodiment 2] The fiber according to the second embodiment contains waste discharged from an integrated coal gasification combined cycle (IGCC) as a raw material. Specifically, the fiber according to the second embodiment contains at least one of waste discharged from a thermal power plant that is not an IGCC and uses coal as fuel, in addition to the waste discharged from an integrated coal gasification combined cycle (IGCC), as a raw material. As in the first embodiment, the SiO in the raw material of the fiber according to the second embodiment 2 and Al 2 O 3 The total content of is preferably 40% by mass or more and 70% by mass or less. 2 and Al2 O 3 Al in the total 2 O 3 The ratio ([A] / ([A]+[S])) (mass ratio) is preferably within a range of 0.15 to 0.40. The raw material for the fiber according to the second embodiment preferably has a CaO content of 5 mass % or more and 30 mass % or less. Similarly to the fiber according to the first embodiment, the fiber according to the second embodiment preferably consists essentially of an amorphous phase. EXAMPLES
[0034] The second embodiment will now be described. In this Example 2, IGCC waste, waste discharged from a thermal power plant that is not an IGCC using coal as fuel, and basalt were mixed at a predetermined mixing ratio (mass%) as the raw material for the fiber. The mixing ratio of each raw material S2 to S11 will be described below with reference to FIG. 8 (the total does not necessarily equal 100% because the decimal points are rounded off). In FIG. 8, IGCC slag indicates IGCC waste, and FA1 to FA8 indicate waste from a coal-fired power plant that is not an IGCC (FA1 to FA8 are different power plants). Also, BA1 indicates basalt. In this Example 2, the components of the raw materials S2 to S11 were analyzed by fluorescent X-ray analysis. Also, the electric furnace described with reference to FIG. 2 was used to manufacture the fiber from the raw materials S2 to S11.
[0035] The raw material S2 is a mixture of 50% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC) and 50% by mass of waste discharged from a coal-fired power plant FA2.
[0036] The raw material S3 is a mixture of 75 mass % waste discharged from an integrated coal gasification combined cycle (IGCC) and 25 mass % waste discharged from a coal-fired power plant FA2.
[0037] The raw material S4 is a mixture of 90 mass % of waste discharged from an integrated coal gasification combined cycle (IGCC) and 10 mass % of waste discharged from a coal-fired power plant FA2.
[0038] Raw material S5 is a mixture of 30% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC), 5% by mass of basalt, 15% by mass of waste discharged from a coal-fired power plant FA2, and 50% by mass of waste discharged from a coal-fired power plant FA7.
[0039] The raw material S6 is a mixture of 50% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC) and 50% by mass of waste discharged from a coal-fired power plant FA3.
[0040] Raw material S7 is a mixture of 20% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC), 10% by mass of waste discharged from a coal-fired power plant FA2, 30% by mass of waste discharged from a coal-fired power plant FA3, and 40% by mass of waste discharged from a coal-fired power plant FA4.
[0041] Raw material S8 is a mixture of 25% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC), 10% by mass of waste discharged from a coal-fired power plant FA4, and 65% by mass of waste discharged from a coal-fired power plant FA6.
[0042] Raw material S9 is a mixture of 10% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC), 16% by mass of waste discharged from a coal-fired power plant FA2, 36% by mass of waste discharged from a coal-fired power plant FA3, and 37% by mass of waste discharged from a coal-fired power plant FA6.
[0043] Raw material S10 is a mixture of 25% by mass of waste discharged from an integrated coal gasification combined cycle (IGCC), 10% by mass of waste discharged from a coal-fired power plant FA4, and 65% by mass of waste discharged from a coal-fired power plant FA6.
[0044] The raw material S11 is a mixture of 60 mass % waste discharged from an integrated coal gasification combined cycle (IGCC) and 40 mass % waste discharged from a coal-fired power plant FA2.
[0045] In this Example 2, the components of the waste and basalt (waste, etc.) that are to be the raw materials S2 to S11 were analyzed by X-ray fluorescence analysis. For the analysis, an X-ray fluorescence analyzer (Philips PW2404) made by Philips Japan Ltd. was used, and the sample chamber of the X-ray fluorescence analyzer was placed in a vacuum state to analyze the components of the waste, etc. FIG. 9 shows the component composition of the waste, etc. according to Example 2. Note that in the following, 0 mass % means a trace amount that cannot be measured, and does not mean strictly "0".
[0046] Waste discharged from a domestic integrated coal gasification combined cycle (IGCC) plant contains 9% by mass [F], 54% by mass [S], 11% by mass [A], 17% by mass [C], and other contents of 9% by mass.
[0047] Basalt (Basalt BA1) contains 19 mass% [F], 46 mass% [S], 11 mass% [A], 17 mass% [C], and other contents of 6 mass%.
[0048] The waste discharged from domestic coal-fired power plant FA1 contains 13% by mass [F], 57% by mass [S], 17% by mass [A], 6% by mass [C], and other contents of 7% by mass.
[0049] The waste discharged from the domestic coal-fired power plant FA2 contains 55% by mass [F], 35% by mass [S], 5% by mass [A], 2% by mass [C], and other contents of 3% by mass.
[0050] The waste discharged from the domestic coal-fired power plant FA3 contains 2% by mass of [F], 62% by mass of [S], 27% by mass of [A], 3% by mass of [C], and other contents of 5% by mass.
[0051] The waste discharged from the domestic coal-fired power plant FA4 contains 97% by mass of [F], 0% by mass of [S], 0% by mass of [A], 0% by mass of [C], and other contents of 3% by mass.
[0052] The waste discharged from the domestic coal-fired power plant FA5 contains 21% by mass [F], 35% by mass [S], 12% by mass [A], 22% by mass [C], and other contents of 10% by mass.
[0053] The waste discharged from domestic coal-fired power plant FA6 contains 1% by mass [F], 73% by mass [S], 22% by mass [A], 0% by mass [C], and other contents of 4% by mass.
[0054] The waste discharged from the domestic coal-fired power plant FA7 contains 1% by mass [F], 19% by mass [S], 17% by mass [A], 55% by mass [C], and other contents of 8% by mass.
[0055] The waste discharged from the domestic coal-fired power plant FA8 contains 0 mass% [F], 34 mass% [S], 13 mass% [A], 42 mass% [C], and other contents of 11 mass%.
[0056] Fig. 10 is a diagram showing the composition of raw materials S2 to S11 according to Example 2. The composition shown in Fig. 10 was calculated from the mixing ratio of each of raw materials S2 to S11 in Fig. 8 and the composition of waste materials, etc. in Fig. 9. Note that the total does not necessarily add up to 100% because the figures are rounded off to the nearest whole number.
[0057] Raw material S2 contains 32% by mass of [F], 45% by mass of [S], 8% by mass of [A], 10% by mass of [C], and other contents of 6% by mass. In addition, [S] + [A] is 53% by mass, and [A] / ([S] + [A]) is 0.15.
[0058] Raw material S3 contains 21% by mass of [F], 49% by mass of [S], 10% by mass of [A], 13% by mass of [C], and other contents of 8% by mass. In addition, [S] + [A] is 59% by mass, and [A] / ([S] + [A]) is 0.16.
[0059] Raw material S4 contains 14% by mass of [F], 52% by mass of [S], 10% by mass of [A], 16% by mass of [C], and other contents of 8% by mass. In addition, [S] + [A] is 63% by mass, and [A] / ([S] + [A]) is 0.17.
[0060] Raw material S5 contains 12% by mass of [F], 33% by mass of [S], 13% by mass of [A], 34% by mass of [C], and other contents of 8% by mass. In addition, [S] + [A] is 46% by mass, and [A] / ([S] + [A]) is 0.28.
[0061] Raw material S6 contains 6% by mass of [F], 58% by mass of [S], 19% by mass of [A], 10% by mass of [C], and 7% by mass of other ingredients. In addition, [S] + [A] is 77% by mass, and [A] / ([S] + [A]) is 0.25.
[0062] Raw material S7 contains 47% by mass of [F], 33% by mass of [S], 11% by mass of [A], 5% by mass of [C], and 4% by mass of other ingredients. In addition, [S] + [A] is 44% by mass, and [A] / ([S] + [A]) is 0.25.
[0063] Raw material S8 contains 13% by mass of [F], 61% by mass of [S], 17% by mass of [A], 5% by mass of [C], and 4% by mass of other substances. In addition, [S] + [A] is 78% by mass, and [A] / ([S] + [A]) is 0.22.
[0064] Raw material S9 contains 11% by mass of [F], 60% by mass of [S], 20% by mass of [A], 3% by mass of [C], and other contents of 6% by mass. In addition, [S] + [A] is 80% by mass, and [A] / ([S] + [A]) is 0.25.
[0065] Raw material S10 contains 13% by mass of [F], 61% by mass of [S], 17% by mass of [A], 5% by mass of [C], and other contents of 4% by mass. In addition, [S] + [A] is 78% by mass, and [A] / ([S] + [A]) is 0.22.
[0066] Raw material S11 contains 27% by mass of [F], 46% by mass of [S], 9% by mass of [A], 11% by mass of [C], and 7% by mass of other substances. In addition, [S] + [A] is 55% by mass, and [A] / ([S] + [A]) is 0.16.
[0067] Fig. 11 is a table summarizing the results of the temperature maintenance (annealing) and temperature change of raw materials S2 to S11, and the melt spinnability. Fig. 12 is a table showing the temperature conditions (time change of temperature inside the furnace) of raw materials S2 to S11 in Example 2. Here, FIG. 12(a) is a table showing the change in furnace temperature over time in Examples A3 and A4. FIG. 12(b) is a table showing the change in furnace temperature over time in Comparative Example A5. FIG. 12(c) is a table showing the change in furnace temperature over time in Comparative Example E4-9. FIG. 12(d) is a table showing the change in furnace temperature over time in Comparative Example E10. FIG. 13 is a graph showing the temperature conditions (time-dependent changes in the temperature inside the furnace) of the raw materials S2 to S11 in Example 2.
[0068] (Example A3) Raw material S2 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature holding "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1450°C (raw material temperature 1400°C) over 15 hours (temperature change "Good"), while the melt was allowed to flow out of the hole at the bottom of the Tammann tube by gravity. From the hole at the center of the bottom of the Tammann tube, the melt solidified into a sphere and fell, and the melt then fell in the form of a fiber, generating a fiber (melt spinnability "Good"). In addition, when the XRD spectrum of the fiber obtained from raw material S2 was examined, a crystalline peak was observed (amorphousness "No").
[0069] (Example A4) Raw material S3 was placed in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature holding "good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1450°C (raw material temperature 1400°C) over 15 hours (temperature change "good"), while the melt was allowed to flow out of the hole at the bottom of the Tammann tube by gravity. The melt solidified into a sphere and fell from the hole at the center of the bottom of the Tammann tube, and the melt then fell in the form of fiber, generating a fiber (melt spinnability "good"). In addition, when the XRD spectrum of the fiber obtained from raw material S3 was examined, only an amorphous halo was observed in the X-ray diffraction (XRD) spectrum of the fiber, and no crystalline peaks were observed (amorphousness "good").
[0070] (Example A5) Raw material S4 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature holding "good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 8 hours (temperature change "good"), while the melt was allowed to flow out of the hole at the bottom of the Tammann tube by gravity. The melt solidified into a sphere and fell from the hole at the center of the bottom of the Tammann tube, and the melt then fell in the form of fiber, generating a fiber (melt spinnability "good"). In addition, when the XRD spectrum of the fiber obtained from raw material S4 was examined, only an amorphous halo was observed in the X-ray diffraction (XRD) spectrum of the fiber, and no crystalline peaks were observed (amorphousness "good").
[0071] (Comparative Example E4) Raw material S5 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature hold "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 5 hours (temperature change "Good"), while the melt was allowed to flow out of the hole at the bottom of the Tammann tube by gravity. The melt solidified into a sphere and fell from the hole at the center of the bottom of the Tammann tube, but the melt did not fall in the form of fibers, and no fibers were produced (melt spinnability "X"). In addition, since no fibers were obtained, the XRD spectrum was not confirmed (amorphousness "-").
[0072] (Comparative Example E5) Raw material S6 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature hold "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 5 hours (temperature change "Good"), while the melt was allowed to flow out from the hole at the bottom of the Tammann tube by gravity. The melt did not fall in the form of fibers from the hole at the center of the bottom of the Tammann tube (melt spinnability "Poor"). In addition, since no fibers were obtained, the XRD spectrum was not confirmed (amorphous property "-").
[0073] (Comparative example E6) Raw material S7 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature hold "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 5 hours (temperature change "Good"), while the melt was allowed to flow out from the hole at the bottom of the Tammann tube by gravity. The melt did not fall in the form of fibers from the hole at the center of the bottom of the Tammann tube (melt spinnability "Poor"). Since no fibers were obtained, the XRD spectrum was not confirmed (amorphous property "-").
[0074] (Comparative example E7) Raw material S8 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature hold "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 5 hours (temperature change "Good"), while the melt was allowed to flow out from the hole at the bottom of the Tammann tube by gravity. The melt did not fall in the form of fibers from the hole at the center of the bottom of the Tammann tube (melt spinnability "Poor"). In addition, since no fibers were obtained, the XRD spectrum was not confirmed (amorphous property "-").
[0075] (Comparative Example E8) Raw material S9 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature hold "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 5 hours (temperature change "Good"), while the melt was allowed to flow out from the hole at the bottom of the Tammann tube by gravity. The melt did not fall in the form of fibers from the hole at the center of the bottom of the Tammann tube (melt spinnability "Poor"). Since no fibers were obtained, the XRD spectrum was not confirmed (amorphous property "-").
[0076] (Comparative Example E9) Raw material S10 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 1375°C (raw material temperature 1325°C), and then held at about 1375°C for 1 hour (temperature hold "Good"). After that, the temperature inside the furnace was raised from about 1375°C (raw material temperature 1325°C) to about 1400°C (raw material temperature 1350°C) over 5 hours (temperature change "Good"), while the melt was allowed to flow out from the hole at the bottom of the Tammann tube by gravity. The melt did not fall in the form of fibers from the hole at the center of the bottom of the Tammann tube (melt spinnability "X"). In addition, since no fibers were obtained, the XRD spectrum was not confirmed (amorphous property "-").
[0077] (Comparative Example E10) Raw material S11 was set in the Tammann tube. Next, the temperature inside the furnace was raised from room temperature (25°C) to about 800°C (raw material temperature 750°C) over about 20 minutes, and then the temperature inside the furnace was raised from about 800°C (raw material temperature 750°C) to about 1350°C (raw material temperature 1300°C) over about 60 minutes by changing the heating rate. Thereafter, the temperature inside the furnace was raised from about 1350°C (raw material temperature 1300°C) to about 1375°C (raw material temperature 1325°C) over about 340 minutes by changing the heating rate (temperature change "O"), while the melt was allowed to flow out from the hole at the bottom of the Tammann tube by gravity (melt spinnability "O", temperature retention "X"). In addition, when the XRD spectrum of the fiber obtained from raw material S11 was examined, a crystalline peak was observed (amorphousness "X").
[0078] (Consideration) The results of Example 2 above show that fiber can be produced from a raw material containing IGCC waste discharged from an integrated coal gasification combined cycle (IGCC). More specifically, it shows that fiber can be produced from a raw material containing at least one of waste discharged from a non-IGCC thermal power plant that uses coal as fuel and basalt, in addition to IGCC waste.
[0079] In addition, from the results of Example 2, the SiO 2 and Al2 O 3 It was found that the total content of is preferably 40% by mass or more and 70% by mass or less. 2 and Al 2 O 3 Al in the total 2 O 3 It was found that the ratio ([A] / ([A]+[S])) (mass ratio) is preferably within a range of 0.15 to 0.40. It was also found that the CaO content of the fiber raw material is preferably 5 mass % or more and 30 mass % or less. In addition, although not essential to the present invention, it is preferable that the fiber be composed essentially of an amorphous phase in order to obtain a high-strength fiber with almost no loss in strength due to peeling between the crystalline phase and the amorphous phase. [Industrial Applicability]
[0080] Fibers obtained from raw materials including IGCC waste can be processed into rovings, chopped strands, woven fabrics, nonwoven fabrics, etc., and can be used as coating materials or reinforcing materials. [Explanation of symbols]
[0081] 1 Electric furnace 2. Tamman tube 3 Hanging rod 4 Openings 5. Fiber D Electric furnace outer diameter H Electric furnace height d Electric furnace opening inner diameter
Claims
[Claim 1] A method for producing a fiber using 50 to 100 parts by mass of waste discharged from an integrated coal gasification combined cycle (IGCC) plant and 0 to 50 parts by mass of waste from a coal-fired power plant other than an integrated coal gasification combined cycle (IGCC) plant as raw materials, comprising: In the raw material, i) SiO 2 and Al 2 O 3 The total content of is 40% by mass or more and 70% by mass or less, ii) Al 2 O 3 / (SiO 2 +Al 2 O 3 ) (mass ratio) is in the range of 0.15 to 0.40, iii) The CaO content is 10% by mass or more and 30% by mass or less, and A step (I) of heating the raw material to a temperature of 1300° C. or more and 1325° C. or less; A step (II) of maintaining the temperature of the raw material reached in the step (I) for a period of 50 minutes or more and 120 minutes or less; The method for producing a fiber includes a step (III) of forming the raw material into a fiber shape by letting it flow out of a forming hole while increasing the temperature of the raw material that has been subjected to the step (II) to a maximum of 1400°C.
Citation Information
Patent Citations
Apparatus for fiberizing and pulverizing high viscosity slag
JP2006124253A
Method of manufacturing coal gasification slag having controlled composition
JP2008266038A
Concrete, concrete structure and manufacturing method of concrete