Tube member having locally excellent foldability and manufacturing method thereof
A tube member with regions of different alloy structures and controlled phase transitions addresses the issue of arbitrary bending in stainless steel instruments, enabling precise alignment and reducing distortion for improved surgical instruments.
Patent Information
- Application Number
- JP2022576435
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-04
- Filing Date
- 2021-06-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-06-04
AI Technical Summary
Conventional stainless steel tube members used in sinus surgery instruments lack the ability to adjust bending angles arbitrarily, leading to inaccurate positioning and irreversible distortion due to slip dislocation, which compromises the circular shape of the tube member at the bending point.
A tube member with regions of different alloy structures, including a first region in a cold-worked or austenitic phase and a second region in a martensitic phase, allowing for locally excellent bendability by controlling phase transitions through heat treatment to achieve specific bending angles.
The tube member can be freely bent to various angles, ensuring accurate alignment with the patient's sinus anatomy, reducing distortion, and maintaining a circular cross-section, thereby enhancing surgical efficiency.
Smart Images

Figure 0007586520000001 
Figure 0007586520000002 
Figure 0007586520000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a tube member having locally excellent bendability and a manufacturing method thereof, and more particularly to a tube member having locally excellent bendability in which bending is freely performed only in a specific region of the tube member at working temperature, allowing a user to variably adjust the bending angle of the tube member, and a manufacturing method thereof. [Background technology]
[0002] The nasal cavity of the human body is the open space in the nose in the middle of the face, the front of which communicates with the outside world through the external nostrils, and the back of which communicates with the pharynx through the posterior nostrils. The paranasal sinuses are the empty spaces filled with air in the facial bones that communicate with the nasal cavity, and serve to protect the brain inside the skull from external shocks. There are various types of paranasal sinuses, including the maxillary sinus, frontal sinus, ethmoid sinus, and sphenoid sinus.
[0003] Since the location of each type of paranasal sinus varies, when inserting a surgical instrument made of a tube member through a nostril, the approach angle may vary depending on the type of paranasal sinus and the patient's body shape. For example, the angle of approach for the sphenoid sinus is about 0° to 30°, the angle of approach for the frontal sinus is about 70° to 90°, and the angle of approach for the maxillary sinus is about 110° to 120°. Therefore, in order to accommodate various approach angles according to the type of paranasal sinus, surgical instruments for the paranasal sinus are provided with stainless steel tube members bent at several approach angles (e.g., bending angles of 0°, 12°, 40°, 60°, 90°, and 120°). Summary of the Invention [Problem to be solved by the invention]
[0004] However, such a conventional stainless steel tube member used as a sinus surgery instrument cannot adequately accommodate situations where various approach angles are required depending on the patient's body shape and the type of sinus, resulting in the inconvenience that the position of the tube member does not accurately match the target. In addition, when the conventional tube member is made of stainless steel and the tube is bent arbitrarily to adjust the approach angle, the strain is generated by slip dislocation due to the characteristics of stainless steel, and the strain is likely to concentrate locally and occurs irreversibly, so that the cross section of the tube member is difficult to maintain a circular shape, and the tube member is blocked at the bent point, resulting in the inconvenience that it is essentially impossible to arbitrarily adjust the bending angle of the stainless steel tube member.
[0005] The present invention is intended to solve the above-mentioned problems and other problems, and aims to provide a tube member having excellent local bendability, which allows the user to freely bend only a specific area of the tube member when performing work, and to adjust the bending angle of the tube member in various ways depending on the work environment, and a method for manufacturing the same. However, these problems are merely exemplary and do not limit the scope of the present invention. It should be noted that the present invention can be used as the sinus surgery instrument described above, but this is merely exemplary and the present invention can be applied to any application in which the operator can freely bend the tube member depending on the purpose of the work. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided an alloy tube member including a first region and a second region having different alloy structures, the tube member having locally excellent bendability.
[0007] According to one embodiment of the present invention, the first region may be in a cold worked state or have an austenite phase at a predetermined operating temperature, and the second region may have a martensite phase at the operating temperature, and the yield stress of the second region may be lower than the yield stress of the first region.
[0008] According to one embodiment of the present invention, when the first region has an austenite phase, the first region has a first phase transition temperature, and the second region has a second phase transition temperature higher than the first phase transition temperature, where the first and second phase transition temperatures refer to temperatures at which a phase transition occurs from a martensite phase on a low temperature side to an austenite phase on a high temperature side.
[0009] According to one embodiment of the present invention, the first phase transition temperature may be a temperature lower than the working temperature, and the second phase transition temperature may be a temperature higher than the working temperature.
[0010] According to one embodiment of the present invention, the first region may comprise one end of the tube member, and the second region may be formed to connect to the first region and comprise the other end of the tube member.
[0011] According to one embodiment of the present invention, the tube member may further include a third region that is in a cold worked state or has an austenite phase at a predetermined working temperature, wherein the first region comprises one end of the tube member, the third region comprises the other end of the tube member, and the second region is formed such that one end is connected to the first region and the other end is connected to the third region, forming an intermediate portion of the tube member.
[0012] According to one embodiment of the present invention, the third region may have a third phase transition temperature, which may be lower than the working temperature.
[0013] According to an embodiment of the present invention, the third phase transition temperature may be equal to the first phase transition temperature.
[0014] According to one embodiment of the present invention, the third region may have a cutting member coupled to one end forming the other end of the tube member.
[0015] According to one embodiment of the present invention, the working temperature may be in the range of 10°C to 50°C.
[0016] According to one embodiment of the present invention, the tubular member may be a member constituting a sinus surgery instrument.
[0017] According to one embodiment of the present invention, the tube member may comprise a guide tube member for inserting an electric wire.
[0018] According to one embodiment of the present invention, the second region may have a shape bent at a predetermined bending angle.
[0019] According to an embodiment of the present invention, the alloy tube member is preferably made of an alloy including any one of a nickel-titanium (Ni-Ti) alloy, a copper-zinc (Cu-Zn) alloy, a gold-cadmium (Au-Cd) alloy, and an indium-thallium (In-Ti) alloy.
[0020] In accordance with another aspect of the present invention, a sinus surgery instrument is provided having an alloy tubular member.
[0021] According to one embodiment of the present invention, the alloy tube member includes a first region and a third region having an austenite phase at a working temperature where a surgery is performed, and a second region having a martensite phase at the working temperature, a cutting member is attached to one end of the third region, and the first region to the third region have a phase transition temperature at which a phase transition from the martensite phase on the low temperature side to the austenite phase on the high temperature side occurs. In this case, the phase transition temperature of the second region may be higher than the phase transition temperatures of the first region and the third region.
[0022] According to yet another aspect of the present invention, there is provided a method for producing a tube member having locally excellent foldability.
[0023] According to one embodiment of the invention, the method may include providing a cold worked alloy tube member defined in a first region and a second region; bending at least a portion of the second region of the tube member to a predetermined bend angle; and locally heat treating only the second region of the tube member such that the second region has a martensitic phase.
[0024] According to one embodiment of the present invention, the step of performing the heat treatment is performed so that a phase transition occurs in the second region from a martensite phase on the lower side to an austenite phase on the higher side, and the temperature at which the phase transition occurs may be even higher than the working temperature at which the bending operation of the second region is performed.
[0025] According to one embodiment of the present invention, a method may include providing a cold worked alloy tube member defined in a first region, a second region and a third region; bending at least a portion of the second region of the tube member to a predetermined bend angle; subjecting the entire region of the tube member to a first heat treatment at a first temperature such that the tube member has an austenitic phase; and subjecting only the second region of the tube member to a second heat treatment such that the second region has a martensite phase.
[0026] According to one embodiment of the present invention, the steps of applying the first and second heat treatments are performed such that the heat treated regions undergo a phase transition from a martensite phase on the lower side to an austenite phase on the higher side, and the phase transition temperature of the second region may be even higher than the phase transition temperature of the first region or the third region.
[0027] According to one embodiment of the present invention, a method may include cold working an alloy into a tubular shape to provide a straight tube member defined in a first region, a second region, and a third region; bending at least a portion of the second region of the tube member to a predetermined bend angle; performing a first heat treatment locally on only the second region of the tube member such that the third region has an austenitic phase; and performing a second heat treatment locally on only the second region of the tube member such that the second region has a martensite phase.
[0028] According to one embodiment of the present invention, the steps of applying the first and second heat treatments are performed so that the heat treated region undergoes a phase transition from a martensite phase on the lower side to an austenite phase on the higher side, and the temperature at which the phase transition of the second region occurs may be even higher than the working temperature at which the bending operation of the second region is performed.
[0029] According to one embodiment of the present invention, the method may further include the steps of locally cooling only the third region of the tube member to a temperature lower than the first phase transition temperature, expanding one end of the cooled third region to connect a cut member, and heating the third region to a temperature higher than the first phase transition temperature.
[0030] According to one embodiment of the present invention, the alloy tube member is preferably made of a shape memory alloy including any one of a nickel-titanium (Ni-Ti) alloy, a copper-zinc (Cu-Zn) alloy, a gold-cadmium (Au-Cd) alloy, and an indium-thallium (In-Ti) alloy. Effect of the Invention
[0031] According to an embodiment of the present invention having the above-mentioned configuration, the tube member can be freely bent only in a specific region, and the operator can adjust the bending angle of the tube member in various ways depending on the working environment. Therefore, the present invention is applicable to all applications where the operator can freely bend the tube member when such bending is required. For example, when the tube member is used as a sinus surgery instrument, the bending angle can be easily adjusted to various approach angles depending on the patient's body shape and the type of sinus with one tube member, so that the position of the tube member inserted into the sinus can be perfectly matched with the target, making it easier to treat the patient.
[0032] As another example, in addition to medical surgical instruments, it is possible to provide a tube member with excellent localized bendability that can be used in a variety of work sites, such as a guide member for inserting electric wires or various other components into places that are difficult for workers to reach.
[0033] Needless to say, such effects are not intended to limit the scope of the present invention. [Brief description of the drawings]
[0034] [Figure 1] 1 is a cross-sectional view illustrating a tube member having locally excellent foldability according to one embodiment of the present invention. [Diagram 2] 10 is a cross-sectional view that shows a schematic view of a tube member having locally excellent foldability according to another embodiment of the present invention. FIG. [Diagram 3] 3 is a graph showing the phase transition temperature for each region of the tube member having locally excellent foldability of FIGS. 1 and 2. [Figure 4] 1A to 1C are cross-sectional views showing steps in a process for manufacturing a tube member having locally excellent foldability. [Diagram 5] 1A to 1C are cross-sectional views showing steps in a process for manufacturing a tube member having locally excellent foldability. [Figure 6] 1A to 1C are cross-sectional views showing steps in a process for manufacturing a tube member having locally excellent foldability. [Figure 7] The results show an example of the production of a tube member having locally excellent foldability. [Figure 8] The results show an example of the production of a tube member having locally excellent foldability. [Figure 9] The results show an example of the production of a tube member having locally excellent foldability. [Figure 10] The results show an example of the production of a tube member having locally excellent foldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] The present invention relates to an alloy tube member including a first region and a second region having different alloy structures, the first region is in a cold worked condition or has an austenitic phase at a predetermined operating temperature; the second region has a martensite phase at the operating temperature; The yield stress of the second region is lower than the yield stress of the first region, resulting in a tube member with locally excellent foldability.
[0036] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0037] The embodiments of the present invention are provided to more completely explain the present invention to those having ordinary skill in the art, and the following embodiments can be modified into various other forms, and the scope of the present invention is not limited to the following embodiments. Rather, these embodiments are provided to make this disclosure more thorough and more complete, and to fully convey the idea of the present invention to those skilled in the art. In the drawings, the thickness and size of each layer are exaggerated for ease of explanation and clarity.
[0038] Hereinafter, the embodiments of the present invention will be described based on the drawings that show an ideal embodiment of the present invention. In the drawings, for example, depending on manufacturing techniques and / or tolerances, distortion of the illustrated shapes can be expected. Therefore, the embodiments of the concept of the present invention should not be interpreted as being limited to the specific shapes of the regions disclosed in this specification, and should include, for example, changes in shapes that are caused by manufacturing convenience.
[0039] FIG. 1 is a perspective view showing a tube member 100 according to an embodiment of the present invention, FIG. 2 is a cross-sectional view showing a tube member 200 according to another embodiment of the present invention, and FIG. 3(a) and (b) are graphs showing the phase transformation temperatures of the regions 110, 120, and 130 of the tube members 100 and 200 shown in FIG. 1 and FIG. 2. Here, the regions in the tube members 100 and 200 may refer to regions that have different phases and form a boundary within the same tube. The phase transformation temperature refers to the temperature at which the martensite phase on the low temperature side is transformed to the austenite phase on the high temperature side as the temperature increases.
[0040] First, as shown in Fig. 1, a tube member 100 according to an embodiment of the present invention is tubular and made of an alloy, and may include a first region 110 and a second region 120. In this case, the first region 110 and the second region 120 may include regions having different phase transition temperatures Af from the martensite phase (M phase) to the austenite phase (A phase), as shown in Fig. 3(a).
[0041] Specifically, the tube member 100 may be a nickel-titanium (Ni-Ti) alloy, which is a shape memory alloy containing 45 at% to 55 at% nickel (Ni), 48 at% to 55 at% nickel, 45 at% to 52 at% nickel, or 50 at% to 51 at% nickel, with the remainder being titanium (Ti). However, the alloy constituting the tube member 100 is not necessarily limited to the nickel-titanium (Ni-Ti) alloy, and is preferably made of a wide variety of alloys that can have the properties of a shape memory alloy, such as a copper-zinc (Cu-Zn) alloy, a gold-cadmium (Au-Cd) alloy, and an indium-thallium (In-Ti) alloy.
[0042] In such shape memory alloys, the crystal arrangement is significantly different between the parent phase, which has an austenite phase on the high temperature side, and the martensite phase on the low temperature side. Therefore, even if the shape is deformed on the low temperature side, the alloy can exhibit a shape memory effect in which it returns to its original shape (parent phase) if heated to a temperature higher than a certain temperature.
[0043] This shape memory effect is only achieved when the material is cold worked into a tubular shape and then heat treated at a given temperature range; a tube that is simply cold worked will exhibit the same stress-strain effect as a normal alloy material.
[0044] The tube member 100 may be formed in a straight shape so that an operator can easily bend it for use, and may be composed of a first region 110 having sufficient rigidity to act as a support, and a second region 120 that is freely bendable at working temperature. In this case, the first region 110 may comprise one end of the tube member 100, and the second region 120 may be formed to be connected to the first region 110 and comprise the other bent end of the tube member 100.
[0045] Here, the working temperature may be the temperature of the environment in which the second region 120 is bent by a worker or in which the worker works on the bent tube member 200 .
[0046] Fig. 3(a) conceptually shows the phases and phase transition temperatures for each region of the tube member 100 shown in Fig. 1. Referring to Fig. 3(a), the phase transition temperature Af1 of the first region 110 is lower than the working temperature T, and therefore the first region 110 has an austenite phase (A phase) at the working temperature T. In contrast, the phase transition temperature Af2 of the second region 120 is higher than the working temperature T, and therefore the second region 120 has a martensite phase (M phase) at the working temperature T.
[0047] In a variant, the second region 120 of the tube member 100 may have a martensite phase, and the first region 110 may have a state in which it has only been cold worked and does not have phase transition characteristics with changes in temperature.
[0048] At the working temperature T, the first region 110 having the austenite phase or a normal cold-worked state is rigid enough to be held by an operator for working or to be used in combination with a separate gripping part, whereas the second region 120 having the martensite phase is flexible enough to be easily distorted by a small force, as will be described in more detail in another embodiment below.
[0049] In another embodiment of the present invention, when the tube member 200 is used as a medical tube member such as a sinus surgery instrument, it may be necessary to attach a cutting member S to the tube member 200 so that the tube member 200 can enter the human body and remove a surgical site such as inflammation. In this case, as shown in Fig. 2, the tube member 200 may include a first region 110 that can function as a support, a second region 120 that can be bent freely, and a third region 130 into which the cutting member S can be inserted and attached. In this case, the cutting member S may be separately manufactured and connected to one end of the third region 130, or may be integrally formed by forming a sawtooth shape at one end of the third region 130.
[0050] For example, the first region 110 may comprise one end of the tube member 200, the third region 130 may comprise the other end of the tube member 200, and the second region 120 may be formed such that one end is connected to the first region 110 and the other end is connected to the third region 130, forming a middle portion of the tube member 200. In this case, the second region 120 has a shape bent at a predetermined bending angle at a predetermined working temperature T, so that the tube member 200 can be formed into a generally bent tube shape.
[0051] Such a tube member 200 may be formed to include regions having different phase transition temperatures so that bending can be easily performed only in specific regions at a predetermined working temperature T.
[0052] 3(b), the first region 110 may have an austenite phase (A phase) and a first phase transition temperature Af1 at a predetermined operating temperature T, and the third region 130 may have an austenite phase (A phase) and a third phase transition temperature Af3. The first phase transition temperature Af1 of the first region 110 and the third phase transition temperature Af3 of the third region 130 may be formed to be the same as or different from each other within a range lower than the operating temperature T.
[0053] The second region 120, which is easily bent to a predetermined bending angle at the working temperature T, may have a martensite phase (M phase) at the working temperature T and a second phase transition temperature Af2 higher than the first phase transition temperature Af1 and the third phase transition temperature Af3. The yield stress (or the yield point) of the second region 120 may have a value lower than the yield stresses of the first region 110 and the third region 130. This allows the second region 120 to be formed as a section in which sintering distortion is even more likely to occur than the first region 110 and the third region 130.
[0054] For example, if the alloy forming the tube member 200 is a nickel-titanium alloy known as Nitinol, when it is cold forged, rolled, extruded, drawn, or drawn into a tube, it can be hardened to have high strength and high elasticity without being easily distorted by external forces. A cold-worked tube will have crystal grains stretched in a specific direction or exhibit microstructural characteristics such as microstructure refinement depending on the processing method. When such a cold-worked alloy is subsequently heat-treated, the microstructural changes and alloy properties will occur.
[0055] For example, when the alloy is subjected to heat treatment at a certain temperature after cold working, the alloy exhibits the property of undergoing a phase transition as it is heated or cooled. That is, the alloy exhibits a phase transition property in which the alloy has an austenite phase at temperatures higher than the phase transition temperature and a martensite phase at temperatures lower than the phase transition temperature. The temperature at which the phase transition occurs can vary within a range of -100°C to +100°C depending on the nickel-titanium alloy components and the heat treatment method. Such heat treatment can memorize the shape of the tube member and change the microstructure to impart superelasticity or shape memory effect properties.
[0056] At a temperature lower than the second phase transition temperature Af2, the second region 120 having the martensite phase may be distorted due to the reversible movement of the twin boundary of the martensite phase. Therefore, the force required for the distortion of the second region 120 is very small, so it feels as if it is soft and distorted, and when the stress is removed, it remains in a distorted state like a normal metal, so it is easy to make it into a desired shape. At this time, the distortion rate caused by the movement of the twin boundary can reach about 7 to 8% based on tensile strain, and when the second region 120 is heated to a temperature higher than the second phase transition temperature Af2 after distortion, a shape memory effect can be achieved in which the shape before distortion is restored while a phase transition to the austenite phase occurs.
[0057] In such alloys that exhibit the shape memory effect, the austenite phase has superelastic properties and is quite stiff, whereas the martensite phase has mechanical properties that allow it to be easily distorted by low stresses.
[0058] As a result, as shown in FIG. 3, by adjusting the heat treatment conditions, etc. to set the second phase transition temperature Af2 of the second region 120 of the tube member 200 higher than the working temperature T, the second region 120 can have a martensite phase at the working temperature T.
[0059] When the tube member is applied to a sinus surgery instrument, the working temperature T may be room temperature, at which a doctor locally bends the tube member to perform surgery, or a temperature including the body temperature of a human body that the tube member directly touches, and may have a range of 10°C to 50°C, preferably 20°C to 40°C.
[0060] Therefore, when applied to a sinus surgery instrument, the tube member 200 allows the second region 120 to be bent freely into a desired bent shape according to the angle of the patient's sinus by making the second region 120 have the martensite phase above the working temperature T. That is, since the working temperature T, which is the patient's body temperature, is lower than the second phase transition temperature Af2 of the second region 120, the second region 120 having the martensite phase can be bent freely.
[0061] As another example, when used in various work sites as a guide member for inserting electric wires or various components into places that are difficult for workers to reach, the temperature may be set within a range that is approximately the same as the room temperature of the worker's working environment.
[0062] At this time, even if all the regions 110, 120, 130 of the tube member 200 are made of martensite phase at the working temperature T, it is possible to perform a minimum desired bending operation. However, if distortion occurs freely in all the regions 110, 120, 130 of the tube member 200, distortion also occurs in the first region 110 or the third region 130, making it difficult to distort the second region 120 to a desired angle, and since unnecessary distortion is likely to occur in the first region 110 or the third region 130 when the tube member 200 is inserted into the human body, there is a risk that the efficiency of work such as treating a patient will decrease.
[0063] Therefore, as shown in FIG. 3, the first phase transition temperature Af1 and the third phase transition temperature Af3 of the first region 110 and the third region 120, excluding the second region 120 where free bending is required, can be set lower than the working temperature T, so that the first region 110 and the third region 130 have an austenite phase that is not easily distorted above the working temperature T.
[0064] This allows each region 110, 120, 130 of the tube member 200 to be given different properties according to its role, so that the first region 110 having an austenite phase at the working temperature T can be used as a portion connecting to a handle or handpiece, the second region 120 having a martensite phase can be easily distorted and used as a portion for adjusting the bending angle, and the third region 130 having an austenite phase can be used as a portion for connecting or joining a cutting member S having saw teeth.
[0065] Alternatively, the second region 120 of the tube member 200 may have a martensite phase and one or more of the first region 110 and the third region 130 may have a cold worked state at the operating temperature, again with the cold worked region having minimal stiffness due to work hardening.
[0066] A method for manufacturing the tube member 200 having locally excellent foldability described above will be described in detail below.
[0067] Figures 4 to 6 are cross-sectional views showing the steps of the process for manufacturing a tube member 200 having locally excellent foldability, and Figure 7 is an image showing an actual product of a tube member having locally excellent foldability.
[0068] First, as shown in Fig. 4, an alloy having a shape memory effect such as nickel-titanium (Ni-Ti) can be cold worked into a tube shape to prepare a straight tube member 200 defined into a first region 110, a second region 120, and a third region 130. Such a tube member 200 may be cold worked during forging, rolling, extrusion, drawing, wire drawing, or the like, and may be formed into an overall straight tube shape. At this time, since the tube member 200 has only been cold worked, it may have considerable rigidity like a normal alloy.
[0069] Next, as shown in FIG. 5, at least a part of the second region 120 of the tube member 200 can be bent to a predetermined bending angle before the heat treatment of the tube member 200. At this time, the bending angle of the second region 120 can be set in consideration of the range of bending angles required by the user. For example, when a straight tube member 200 is bent, it can be bent within a range of about 100° without damaging the cross-sectional area of the tube member 200. That is, when the desired bending angle range of the tube member 200 is 0° to 120°, the second region 120 can be bent to a bending angle of about 40° before the heat treatment of the tube member 200 to accommodate any range of required bending angles.
[0070] In addition to the second region 120 of the tube member 200 which needs to be freely bent, the first region 110 and the third region 130 which are bonded to the supporting material and the cutting member S and need to be strong enough not to be easily distorted may be maintained in a cold-worked state without being subjected to heat treatment, or may be heat-treated to set the phase transition temperature lower than the working temperature T, thereby maintaining the superelastic state above the working temperature T.
[0071] For example, a predetermined heat treatment may be locally applied to only the second region 120 of the tube member 200 so that the first region 110 and the third region 130 maintain the cold-worked state and the second region 120 has a second phase transition temperature Af2 higher than the working temperature T. For example, in the case of a nickel-titanium alloy, the heat treatment temperature may be in the range of 400 to 450°C. The heat treatment of the second region 120 may be performed by locally heating the region using a laser, or by placing only the second region 120 in a heat treatment chamber and locally heating the region. However, the heat treatment method is not limited thereto, and various heat treatment methods are applicable as long as the heat treatment can be performed by locally heating only the second region 120.
[0072] As a result, the second region 120 of the tube member 200 has a second phase transition temperature Af2 higher than the working temperature T, and can have a martensite phase above the working temperature T. At this time, the first region 110 and the third region 130 have only been subjected to cold working, and therefore may have considerable rigidity like a normal alloy.
[0073] Therefore, the second region 120 of the tube member 200 is easily distorted even when a small amount of force is applied, and the distortion is maintained even when the force is removed, whereas the first region 110 and the third region 130 are not easily distorted even when a force is applied, and exhibit stiff behavior in which they quickly return to their original state when the force is removed. This allows an operator to freely bend the second region 120, which has a martensite phase and is easily distorted, while holding the first region 110 or the third region 130, which has considerable rigidity, or while it is joined to another holding body. This manufacturing method can be used when manufacturing the cut member S by processing the third region 103 by oneself, without inserting the cut member S into the third region 130.
[0074] When the cutting member S is inserted into the third region 130 for coupling, in order to make it easier to insert the cutting member S, it may be necessary to heat treat the third region 130.
[0075] For example, after cold working, the entire regions 110, 120, 130 of the tube member 200 may be subjected to a first heat treatment at a first temperature so that the entire tube member 200 in which the second region 120 is bent at a predetermined bending angle has a first phase transition temperature Af1 lower than the working temperature T. Then, the phase transition temperature of the second region 120 may be reset by locally performing a second heat treatment at a second temperature only on the second region 120 of the tube member 200 so that the second region 120 has a second phase transition temperature Af2 higher than the working temperature T. In this case, when the tube member 200 is a nickel-titanium alloy, the temperature of the first heat treatment may be in the range of 500 to 550°C and the temperature of the second heat treatment may be in the range of 350 to 450°C depending on the composition.
[0076] 6, only the third region 130 of the tube member 200 is locally cooled to a temperature lower than the first phase transition temperature Af1, so that the third region 130 has a martensite phase. Then, one end of the third region 130, which is cooled to have a martensite phase and can be easily distorted, can be expanded to connect the cutting member S. At this time, the insertion portion of the cutting member S to be inserted into the third region 130 may be formed to have an outer diameter slightly larger than the inner diameter of the third region 130 before expansion.
[0077] Next, when the third region 130 is heated to a temperature higher than the first phase transition temperature Af1, one end of the expanded third region 130 shrinks again, and the cut member S can be firmly fixed in the form of an interference fit. At this time, the temperature of the cooled third region 130 may be raised by separate heating, but if the phase transition temperature is set lower than room temperature, it may be sufficient to simply leave it at room temperature.
[0078] As an example of a modified example, even when manufacturing a tube member 100 including a first region 110 and a second region 120, the manufacturing process can be carried out in substantially the same manner, except for the operations performed in the third region 130 described above, and a detailed description of the manufacturing method will be omitted.
[0079] The following describes examples of the present invention to aid in the understanding of the present invention. The following examples are disclosed as examples to aid in the understanding of the present invention, and it is needless to say that the present invention is not limited to the following examples.
[0080] [Production Example 1] A straight tube member made of a cold-worked 50.2 at% Ni-Ti alloy is prepared. A portion of the tube member is bent by about 30 degrees to distort it, and only the bent portion (second region) is heat-treated at 350°C or higher. After the heat treatment, the bent portion is in a distorted state and has a phase transition temperature of about 45°C, so that it is configured in a martensite state above the working temperature (room temperature or body temperature).
[0081] FIG. 7 shows a tube member manufactured by Manufacturing Example 1. When the bent portion is distorted, it shows a soft distortion behavior, while the remaining portion that has not been heat treated remains cold worked and shows a very strong behavior. In FIG. 7, the portions corresponding to the first and third regions are shown with a graph of stress-strain rate showing elasticity as a mechanical property of the cold worked alloy. In addition, the portion corresponding to the second region is shown with a graph of stress-strain rate showing that sintering distortion occurs even at low stress.
[0082] [Production Example 2] A straight tube of cold-worked 50.6 at% Ni-Ti alloy is prepared. A portion of the tube is bent by about 40 degrees to distort it, and then the entire tube is heat-treated at 500°C for 5 minutes or more. After the heat treatment, the phase transition temperature is about 15°C, which is lower than the working temperature, which is in the range of room temperature and body temperature, so that the entire tube exhibits superelastic behavior when distorted.
[0083] In this case, if only the bent portion is subjected to heat treatment at about 450°C, the phase transition temperature rises and the bent portion, which is the portion that has been further heat treated, exhibits soft distortion behavior, while the remaining portion exhibits superelastic behavior. This is because, when heated to a temperature of 450°C, Ni 4 Ti 3 This is because the precipitates of Ni occur, which reduces the concentration of Ni, which is known, and raises the phase transition temperature. As a result, the tube member exhibits the characteristics shown in FIG. 8. In the parts corresponding to the first and third regions of FIG. 8, a graph of the stress-strain ratio showing the superelastic characteristics is also shown. When such a tube member is distorted, it can be seen that the bent part can be easily adjusted to various angles, as shown in FIG. 9.
[0084] Next, a step of inserting a cutting member into the portion corresponding to the third region was performed. Since the inner diameter of the tube member was 3.6 mm, a stainless steel saw blade with a diameter of 3.7 mm, which is slightly larger than the inner diameter, was prepared. Only the portion corresponding to the third region was locally cooled to lower the temperature below room temperature, and then the entrance at the end of the tube was expanded. Next, the prepared cutting member was inserted, and the temperature was raised again to room temperature. While the inner diameter of the tube was shrinking at room temperature, it was joined with a very strong bonding force as the cutting member was tightened. Figure 10 shows the result after the cutting member was joined.
[0085] Although the present invention has been described with reference to the illustrated embodiment, this is merely illustrative, and a person skilled in the art should understand that various modifications and equivalent embodiments can be adopted. Therefore, the true technical scope of protection of the present invention should be determined by the technical ideas of the claims. [Industrial Applicability]
[0086] The tube member of the present invention can be freely bent by a worker when required and can be applied to any application for which it can be used, and therefore can be used in a variety of ways in various work sites. [Explanation of symbols]
[0087] 110 First Area 120 Second Area 130 The Third Region 100, 200 Tube material S-cut material T Working temperature Af1 First phase transition temperature Af2 Second phase transition temperature Af3 Third phase transition temperature
Claims
1. A nickel-titanium (Ni-Ti) shape memory alloy tube member including a first region and a second region having different alloy structures, the first region is in a cold worked condition or has an austenite phase at a predetermined operating temperature, the second region has a martensite phase at the operating temperature, and the yield stress of the second region is lower than the yield stress of the first region; The predetermined working temperature is the temperature of the environment at which a worker bends the second region or works on the bent tube member. A tube member having locally excellent bendability.
2. the first region has an austenite phase; 2. The tube member having locally excellent bendability according to claim 1, wherein the first region has a first phase transition temperature, the second region has a second phase transition temperature higher than the first phase transition temperature, and the first and second phase transition temperatures are temperatures at which a phase transition occurs from a martensite phase on a low temperature side to an austenite phase on a high temperature side.
3. 3. The tube member having locally excellent foldability according to claim 2, wherein the first phase transition temperature is a temperature lower than the working temperature, and the second phase transition temperature is a temperature higher than the working temperature.
4. 2. A tube member having locally excellent bendability as described in claim 1, wherein the first region comprises one end of the tube member, and the second region is formed to be connected to the first region and comprises the other end of the tube member.
5. 2. The tube member having locally excellent bendability according to claim 1, further comprising a third region that is in a cold worked state or has an austenite phase at a predetermined working temperature, the first region comprising one end of the tube member, the third region comprising the other end of the tube member, and the second region being formed so that one end is connected to the first region and the other end is connected to the third region, forming an intermediate portion of the tube member.
6. 6. The tube member having locally excellent foldability according to claim 5, wherein the third region has a third phase transition temperature, the third phase transition temperature being lower than the working temperature.
7. 7. The tube member having locally excellent foldability according to claim 6, wherein the third phase transition temperature is equal to the first phase transition temperature.
8. 6. The tube member having locally excellent foldability according to claim 5, wherein the third region has one end which forms the other end of the tube member and to which a cut member is joined.
9. 9. The tube member having locally excellent foldability according to claim 1, wherein the working temperature is in the range of 10°C to 50°C.
10. 10. The tubular member having locally excellent foldability according to claim 9, wherein the tubular member is a member constituting a paranasal sinus surgery instrument.
11. The tube member is a guide tube portion for inserting an electric wire. The tube member having locally excellent foldability according to claim 1 , comprising a material.
12. 11. The tube member having locally excellent foldability according to claim 1, wherein the second region has a shape bent at a predetermined bending angle.
13. A sinus surgery instrument having a nickel-titanium (Ni-Ti) shape memory alloy tube member, The tube member is a first region and a third region having an austenitic phase at a working temperature at which the operation is to be performed; a second region having a martensite phase at the operating temperature; a cutting member is bonded to one end of the third region, and the first region to the third region have a phase transition temperature at which a phase transition occurs from a martensite phase on the low temperature side to an austenite phase on the high temperature side; A sinus surgery instrument, wherein the second region has a phase transition temperature greater than the phase transition temperatures of the first region and the third region.
14. A method for manufacturing a tube member having locally excellent bendability, comprising the steps of: preparing a cold worked nickel-titanium (Ni-Ti) shape memory alloy tube member defined into a first region and a second region; bending at least a portion of the second region of the tube member to a predetermined bending angle; and locally heat treating only the second region of the tube member so that the second region has a martensite phase, wherein the heat treating step is performed so that the second region undergoes a phase transition from a martensite phase on a lower side to an austenite phase on a higher side, the phase transition occurring at a temperature that is higher than a working temperature at which the bending operation of the second region is performed.
15. 2. A method for manufacturing a tube member having locally excellent bendability, comprising the steps of: preparing a cold worked nickel-titanium (Ni-Ti) shape memory alloy tube member defined into a first region, a second region, and a third region; bending at least a portion of the second region of the tube member to a predetermined bend angle; subjecting the entire region of the tube member to a first heat treatment at a first temperature such that the tube member has an austenite phase; and subjecting only the second region of the tube member to a second heat treatment such that the second region has a martensite phase, wherein the first and second heat treatments are performed such that the heat treated region undergoes a phase transition from a low temperature martensite phase to a high temperature austenite phase, the phase transition temperature of the second region being higher than the phase transition temperature of the first region or the third region.
16. A method for producing a straight tube member by cold working a nickel-titanium (Ni-Ti) shape memory alloy into a tubular shape, the straight tube member being defined into a first region, a second region, and a third region; and bending at least a portion of the second region of the tube member to a predetermined bending angle.
1. A method for manufacturing a tube member having locally excellent bendability, comprising the steps of: locally applying a first heat treatment to only the second region of the tube member such that the third region has an austenite phase; and locally applying a second heat treatment to only the second region of the tube member such that the second region has a martensite phase, wherein the steps of applying the first and second heat treatments are performed such that the heat-treated region undergoes a phase transition from a martensite phase on a lower temperature side to an austenite phase on a higher temperature side, and the temperature at which the phase transition of the second region occurs is even higher than a working temperature at which a bending operation of the second region is performed.
17. 17. The method for manufacturing a tube member having locally excellent foldability according to claim 16, further comprising the steps of: locally cooling only the third region of the tube member to a low temperature lower than a first phase transition temperature; expanding one end of the cooled third region to join a cut member; and heating the third region to a temperature higher than the first phase transition temperature.
Citation Information
Patent Citations
Parts partially having superelasticity, and its manufacturing method
JP2003247053A
Apparatus, system, and method for delivering hardening material into bone
JP2010517683A
Device for guiding a medical needle
US20140257203A1
Flexible Member for Angled System