Hardened polymer compound and resin composition containing the compound
A resin composition with a specific polymer compound structure addresses the limitations of existing adhesives by providing low dielectric properties and strong adhesion, suitable for high-frequency circuit applications.
Patent Information
- Application Number
- JP2021006235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-19
AI Technical Summary
Existing polymer compounds used in film adhesives for electronic devices have low heat resistance, high dielectric constant, and dielectric loss tangent, making them unsuitable for high-frequency circuit applications, and compatibility and adhesion issues with low-roughness copper foils are significant.
A resin composition containing a polymer compound with a specific structure, comprising a copolymer of N-hydroxyphenyl (meth)acrylamide and styrene, reacted with (meth)acrylic acid chloride, and combined with a radical initiator, to form a film with excellent dielectric and adhesive properties.
The cured product exhibits low dielectric constant and loss tangent, high adhesion to low-roughness copper foils, and improved heat resistance, suitable for high-frequency circuit applications.
Smart Images

Figure 0007586717000001 
Figure 0007586717000002 
Figure 0007586717000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer compound which can be easily formed into a film by casting a solution onto a substrate, which can undergo a thermal or photocuring reaction when used in combination with a radical initiator, and which produces a cured product with excellent dielectric properties and adhesiveness. [Background technology]
[0002] Phenoxy resin is a polymeric compound with a very large molecular weight obtained by polymerizing a bifunctional epoxy resin and a bifunctional phenolic compound. By adding this phenoxy resin, general epoxy resin compositions and radically polymerizable compositions can be made into a film shape, so it is used in a wide range of fields as an important component of film-type adhesives, and is particularly used in the electrical and electronic fields for interlayer insulation layers of printed wiring boards and resin-coated copper foils. Although the cured product of the resin composition containing the phenoxy resin has excellent adhesiveness and film-forming ability, it has low heat resistance and high dielectric constant and dielectric dissipation factor (dielectric constant is about 3.5 and dielectric dissipation factor is about 0.03 at a frequency of 1 GHz), and therefore cannot be used in electronic devices, which have recently become faster in signal response speed. Polymeric fluorine compounds such as polytetrafluoroethane (PTFE) (Patent Document 1) and liquid crystal polymers (Patent Document 2) are generally known as resins with excellent dielectric properties, but these resins have extremely low compatibility with other resins and insufficient adhesiveness. Patent Document 3 describes a curable polymer compound obtained by esterifying a monomer having one or more ethylenically unsaturated groups and one carboxy group with an aliphatic hydroxyl group in a random copolymer of a monomer having one ethylenically unsaturated group of 70% or less by weight and a (meth)acrylate having one or more aliphatic hydroxyl groups of 30% or more by weight. However, when the present inventors conducted further tests, the cured product of the curable polymer compound obtained by the structural formula in the document had a dielectric loss tangent of about 0.005 at 10 GHz, which does not fully satisfy the low dielectric properties required for current high-frequency circuit board applications. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-001274 A [Patent Document 2] JP 2014-060449 A [Patent Document 3] Japanese Patent Application Publication No. 10-017812 Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made in consideration of the above points, and has an object to provide a curable polymer compound that has sufficient flexibility to be formed into a film, has high adhesion to low-roughness copper foil, and has a low dielectric constant and dielectric tangent. [Means for solving the problem]
[0005] As a result of extensive investigations, the present inventors have found that the above problems can be solved by using a resin composition containing a polymer compound having a specific structure, and have thus completed the present invention. That is, the present invention is (1)The following formula (1)
[0006] [ka]
[0007] (wherein R1 and R2 each independently represent a hydrogen atom or a methyl group; m and n each independently represent an average number of repeating units and each independently represent a real number in the range of 1 to 2,000), (2) A resin composition comprising the polymer compound according to the above item (1) and a radical initiator. (3) The resin composition according to the above item (2), further comprising a radical reactive monomer having two or more functional groups in one molecule. (4) The resin composition according to the above item (3), wherein the radical reactive monomer is a maleimide compound. (5) A film-like adhesive comprising the resin composition according to any one of (2) to (4) above, and (6) A cured product of the resin composition according to any one of the preceding items (2) to (4) or the film-like adhesive according to the preceding item (5). Regarding. Effect of the Invention
[0008] The polymer compound according to the present invention and a resin composition containing the same can be cured by using a radical initiator in combination with heat or light energy, and the cured product of the resin composition can provide a polymer compound having excellent dielectric properties, adhesion, heat resistance and water resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described. The polymer compound of the present invention represented by the above formula (1) is a dehydrochlorination condensation product of a hydroxyl group of a random copolymer of N-hydroxyphenyl(meth)acrylamide and styrene and a (meth)acrylic acid chloride group, or a dehydration condensation product of a hydroxyl group of the copolymer and (meth)acrylic acid. In addition, in formula (1), the structure of the polymer compound is represented by the average number of repeating units of the units derived from styrene and the units derived from N-hydroxyphenyl(meth)acrylamide and (meth)acrylic acid chloride groups, but the polymer compound of the present invention is formed by randomly bonding m units derived from styrene and n units derived from N-hydroxyphenyl(meth)acrylamide and (meth)acrylic acid chloride groups (both m and n are average values), and the following formula (2) in this specification is also represented with the same intention.
[0010] First, the copolymer which is the intermediate raw material of the polymer compound of the present invention will be described. Specific examples of N-hydroxyphenyl(meth)acrylamide, which is a raw material for the copolymer, include N-(4-hydroxyphenyl)methacrylamide, N-(4-hydroxyphenyl)acrylamide, N-(3-hydroxyphenyl)methacrylamide, N-(3-hydroxyphenyl)acrylamide, N-(2-hydroxyphenyl)methacrylamide, and N-(2-hydroxyphenyl)acrylamide, with N-(4-hydroxyphenyl)methacrylamide being preferred. In this specification, the term "(meth)acrylamide" means both "acrylamide and methacrylamide".
[0011] The following formula (2) is a structural formula of a random copolymer of N-hydroxyphenyl(meth)acrylamide and styrene, and R1, m, and n in formula (2) have the same meanings as R1, m, and n in formula (1). That is, the polymer compound represented by formula (1) of the present invention (polymer compound having a structure represented by formula (1)) is a polymer compound obtained by using the copolymer represented by formula (2) as an intermediate raw material.
[0012] [ka]
[0013] The method for copolymerizing N-hydroxyphenyl(meth)acrylamide with styrene is not particularly limited as long as it is a known method, and examples thereof include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization. Solvents that can be used in solution polymerization include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, propylene glycol monomethyl ether acetate, N-methylpyrrolidone, N,N-dimethylformamide, and γ-butyrolactone. Emulsion polymerization and suspension polymerization usually use water and a surfactant, and the copolymerization reaction is carried out in a state where the raw material components are emulsified or suspended in water.
[0014] The copolymerization reaction may be any of radical polymerization, cationic polymerization, and anionic polymerization. In the case of radical polymerization, it is preferable to use a radical polymerization initiator. Specific examples of the radical polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, hydrogen peroxide, di-t-butyl peroxide, dicumyl peroxide, and benzoyl peroxide. The amount of the radical polymerization initiator is usually 0.001 to 5 parts by mass per 100 parts by mass of the raw material components of the copolymer. The polymerization temperature is usually 50 to 250° C., preferably 60 to 200° C., and the polymerization time is usually 0.5 to 30 hours, preferably 1 to 20 hours. The radical polymerization reaction is preferably carried out under a nitrogen gas atmosphere to prevent polymerization inhibition by oxygen in the air.
[0015] Specific examples of cationic polymerization initiators include inorganic acids such as sulfuric acid and hydrochloric acid, organic acids such as CF3COOH and CCl3COOH, and super strong acids such as CF3SO3H and HClO4. Specific examples of anionic polymerization initiators include butyl lithium, Na-naphthalene complexes, alkali metals, alkyl lithium compounds, sodium amides, Grignard reagents, and lithium alkoxides. However, since there is a concern that the ionic initiators used in cationic polymerization and anionic polymerization remain in the copolymer even after the polymerization reaction and adversely affect the dielectric properties and insulating properties, it is preferable to synthesize the copolymer that is the intermediate raw material of the polymer compound of the present invention by radical polymerization. The amount of the cationic polymerization initiator or anionic polymerization initiator is usually 0.01 to 5 parts by mass per 100 parts by mass of the raw materials for the copolymer. The polymerization temperature is usually 40 to 150° C., preferably 50 to 120° C., and the polymerization time is usually 0.5 to 20 hours, preferably 1 to 15 hours.
[0016] The number average molecular weight of the copolymer serving as the intermediate raw material for the polymer compound of the present invention is usually 3,000 to 300,000, and preferably 5,000 to 200,000. In order to obtain a copolymer having a number average molecular weight within the above range, it is preferable to adjust the amount of initiator used when synthesizing the copolymer to an appropriate amount.The amount of initiator required to obtain a copolymer having a number average molecular weight within the above range depends on the type of N-hydroxyphenyl(meth)acrylamide and the amount of N-hydroxyphenyl(meth)acrylamide and styrene used in the copolymerization reaction, so it cannot be generally stated, but it is generally known that a copolymer having a large molecular weight can be obtained by reducing the amount of initiator, and it is sufficient to select the amount of initiator that can obtain a copolymer having a desired molecular weight within the above range.
[0017] The ratio of N-hydroxyphenyl(meth)acrylamide and styrene used in synthesizing the copolymer that is the intermediate raw material of the polymer compound of the present invention is not particularly limited, but the amount (mass) of styrene used is usually 4 to 99.5 times, preferably 4.5 to 99.7 times, the mass of N-hydroxyphenyl(meth)acrylamide. By setting the ratio of the raw materials of the copolymer used in the above range, the polymer compound of the present invention can be obtained whose cured product exhibits excellent dielectric properties (low dielectric constant and low dielectric loss tangent).
[0018] The polymer compound of the present invention can be obtained by a dehydrochlorination reaction between the phenolic hydroxyl group of the copolymer (this hydroxyl group is the hydroxyl group originally possessed by the raw material N-hydroxyphenyl(meth)acrylamide) and the chloride group of (meth)acrylic acid chloride, or by a dehydration condensation reaction between the phenolic hydroxyl group of the copolymer and (meth)acrylic acid.
[0019] The ratio of the copolymer and (meth)acrylic acid chloride or (meth)acrylic acid used when synthesizing the polymer compound of the present invention is not particularly limited, but if there is an excess or insufficient amount of (meth)acrylic acid chloride or (meth)acrylic acid relative to the hydroxyl groups of the copolymer, the (meth)acrylic acid chloride or (meth)acrylic acid remaining unreacted in the polymer compound and the hydroxyl groups remaining unreacted with (meth)acrylic acid chloride or methacrylic acid may adversely affect the properties of the cured product, so it is preferable to use an equivalent amount of (meth)acrylic acid chloride or (meth)acrylic acid to the hydroxyl groups of the copolymer.
[0020] The reaction between the copolymer and (meth)acrylic acid chloride may be carried out by adding (meth)acrylic acid chloride to an organic solvent solution of the copolymer under stirring. The organic solvent that can be used here is not particularly limited as long as it can dissolve the copolymer and (meth)acrylic acid chloride, and when the copolymer as an intermediate raw material is synthesized in a solvent, the copolymer solution after the polymerization reaction may be used as it is. The concentration of the copolymer solution to be reacted with (meth)acrylic acid chloride is usually 10 to 90% by mass, preferably 20 to 80% by mass. The reaction temperature is usually 30 to 120°C, preferably 40 to 110°C, and the reaction time is usually 0.5 to 4 hours, preferably 1 to 3 hours.
[0021] Since the reaction between the copolymer and (meth)acrylic acid chloride is a dehydrochlorination reaction, it is preferable to add a tertiary amine such as triethylamine or pyridine to the reaction solution in advance in order to trap the generated hydrochloric acid and further promote the reaction. The amount of the tertiary amine used is preferably equimolar to 4 times the amount of (meth)acrylic acid chloride, more preferably equimolar to 3 times the amount of (meth)acrylic acid chloride. The hydrochloric acid generated during the reaction precipitates as the hydrochloride salt of the amine, and can be removed by filtration after the reaction. In addition, the excess tertiary amine can be distilled out of the system after filtration under heating and reduced pressure.
[0022] The reaction of the copolymer with (meth)acrylic acid may be a conventionally known esterification reaction, for example, a method in which the copolymer and (meth)acrylic acid are heated and stirred in the presence of a catalyst. Since the reaction of the copolymer with (meth)acrylic acid is a dehydration reaction, it is preferable to carry out the reaction while distilling off water from the reaction system by azeotropy, and therefore it is preferable to carry out the reaction using a solvent that is not completely miscible with water, such as toluene, xylene, ethyl acetate, butyl acetate, and methyl isobutyl ketone. The amount of the solvent used is preferably an amount that makes the concentration of the raw material components of the polymer compound 20 to 80% by mass. Examples of the catalyst used in the esterification reaction include acid catalysts such as sulfuric acid, methanesulfonic acid, and p-toluenesulfonic acid, and the amount used is preferably 0.1 to 5% by mass based on the total mass of the raw materials of the polymer compound used in the reaction, the solvent, etc. The reaction temperature is usually 50 to 150° C., preferably 60 to 140° C., and the reaction time is usually 0.5 to 4 hours, preferably 1 to 3 hours.
[0023] In addition, in order to prevent the polymerization reaction between (meth)acryloyl groups in the polymer compound of the present invention during storage, it is preferable to add a small amount of polymerization inhibitor to the polymer compound solution after the completion of the synthesis reaction.Specific examples of polymerization inhibitors include hydroquinone, paramethoxyphenol, methylhydroquinone, di-t-butylhydroxytoluene, t-butylhydroquinone, 2-t-butyl-1,4-benzoquinone, 1,4-benzoquinone, 1,1-diphenyl-2-picrylhydrazyl free radical, 6-t-butyl-2,4-xylenol, 4-t-butylpyrocatechol, 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, and phenothiazine.
[0024] The number average molecular weight of the polymer compound of the present invention thus obtained is preferably in the range of 11,000 to 300,000, more preferably 15,000 to 200,000. If the molecular weight is smaller than the above range, the adhesion to low-roughness copper foil will be low, and if it is larger, the viscosity will be high, which may make coating, etc. difficult. In this specification, the molecular weight refers to a value calculated in terms of polystyrene based on the results of GPC measurement.
[0025] The resin composition of the present invention contains the polymer compound of the present invention and a radical initiator. Preferred thermal radical initiators include peroxides such as benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, α,α-bis(t-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilylperoxide.
[0026] Examples of preferred photoradical initiators include benzoin and its alkyl ethers such as benzoin, benzoin methyl ether, and benzoin ethyl ether; acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone; anthraquinones such as 2-methylanthraquinone, 2-amyl anthraquinone, 2-t-butyl anthraquinone, and 1-chloro anthraquinone; thioxanthones such as 2,4-dimethylthioxanthone, 2,4-diisopropylthioxanthone, and 2-chlorothioxanthone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzophenones such as benzophenone; 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1; acylphosphine oxides, and xanthones.
[0027] The content of the radical initiator in the resin composition of the present invention is usually 0.1 to 10 parts by mass, preferably 0.1 to 8 parts by mass, per 100 parts by mass of the polymer compound and the resin components such as the optional radical reactive monomer described below.
[0028] The resin composition of the present invention may be used in combination with a radical reactive monomer. By using a radical reactive monomer in combination, the reactivity of the resin composition of the present invention and the heat resistance of the cured product can be improved. The radical reactive monomer is preferably one having two or more functional groups, and specific examples thereof include ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, neopentyl glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-Nonanediol dimethacrylate, glycerin dimethacrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, ethylene oxide adduct methacrylate of bisphenol A, trimethylolpropane trimethacrylate, tricyclodecane dimethanol dimethacrylate, glycerin dimethacrylate, trimethylolpropane trimethacrylate, ethoxylated isocyanuric acid triacrylate, ε-caprolactone modified tris-(2-acryloxyethyl) isocyanurate, penta Erythritol triacrylate, ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, pentaerythritol tetraacrylate, dipentaerythritol polyacrylate, dipentaerythritol hexaacrylate, triallyl isocyanurate, triallyl cyanurate, divinylbenzene, divinyl isophthalate, N-phenyl-maleimide, N-phenyl-methylmaleimide, N-phenyl-chloromaleimide, Np-chlorophenyl-maleimide , Np-methoxyphenyl-maleimide, Np-methylphenyl-maleimide, Np-nitrophenyl-maleimide, Np-phenoxyphenyl-maleimide, Np-phenylaminophenyl-maleimide, Np-phenoxycarbonylphenyl-maleimide, 1-maleimido-4-acetoxysuccinimide-benzene, 4-maleimido-4'-acetoxysuccinimide-diphenylmethane, 4-maleimido-4'-acetoxysuccinimide-diphenylether, 4-maleimido-4'-acetamide -diphenyl ether, 2-maleimide-6-acetamido-pyridine, 4-maleimide-4'-acetamido-diphenylmethane, and Np-phenylcarbonylphenyl-maleimide N-ethylmaleimide, N-2,6-xylylmaleimide, N-cyclohexylmaleimide, N-2,3-xylylmaleimide, xylylmaleimide, 2,6-xylenemaleimide, and 4,4'-bismaleimidediphenylmethane are examples of the maleimide compounds, and those having a maleimide group as a functional group (maleimide compounds) are preferred. These radical reactive monomers may be used alone or in combination of two or more.
[0029] The resin composition of the present invention may be used in combination with an organic solvent. Specific examples of the organic solvent include aromatic solvents such as toluene and xylene, ether solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether monoacetate, and propylene glycol monobutyl ether, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone, lactones such as γ-butyrolactone and γ-valerolactone, amide solvents such as N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide, and N,N-dimethylimidazolidinone, and sulfones such as tetramethylene sulfone. The content of the organic solvent in the resin composition of the present invention is usually 90% by mass or less, preferably 30 to 80% by mass in the resin composition.
[0030] The resin composition of the present invention may be used in combination with a polymerization inhibitor to improve storage stability. The polymerization inhibitor that can be used in combination is not particularly limited as long as it is a generally known one, and examples thereof include quinones such as hydroquinone, methylhydroquinone, p-benzoquinone, chloranil, and trimethylquinone, aromatic diols, and di-t-butylhydroxytoluene.
[0031] The resin composition of the present invention can be used by blending fillers and additives in amounts that do not impair the inherent performance, for the purpose of imparting desired performance depending on the application. The fillers may be in the form of fibers or powders, and examples of such fillers include silica, carbon black, alumina, talc, mica, glass beads, and glass hollow spheres.
[0032] The resin composition of the present invention can also be used in combination with a flame-retardant compound, an additive, and the like. These are not particularly limited as long as they are commonly used. For example, flame-retardant compounds include bromine compounds such as 4,4-dibromobiphenyl, phosphate esters, melamine phosphate, phosphorus-containing epoxy resins, nitrogen compounds such as melamine and benzoguanamine, oxazine ring-containing compounds, silicon-based compounds, and the like. Additives include ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent brighteners, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, dispersants, leveling agents, gloss agents, and the like, and can be used in appropriate combination as desired.
[0033] The resin composition of the present invention can be used by coating or impregnating it onto various substrates. For example, when a thermal radical initiator is used, it can be used as an interlayer insulating layer of a multilayer printed circuit board by coating it onto a PET film, as a coverlay by coating it onto a polyimide film, or as a resin-coated copper foil by coating it onto copper foil and drying it. It can also be used as a printed wiring board or a prepreg for CFRP by impregnating it into glass cloth, glass paper, carbon fiber, various nonwoven fabrics, etc. Furthermore, it can also be used as various resists by using a photoradical initiator.
[0034] The interlayer insulating layer, coverlay, resin-coated copper foil, prepreg, and the like of the present invention can be heated and pressurized in a hot press or the like to form a cured product. EXAMPLES
[0035] The present invention will be described in more detail below with reference to examples and comparative examples, although the present invention is not limited to these examples.
[0036] Example 1 (Synthesis of the polymer compound of the present invention) (Step 1) Synthesis of a copolymer (copolymer 1) represented by the following formula (3) A flask equipped with a thermometer, a cooling tube, a nitrogen gas inlet tube, and a stirrer was charged with 38.5 parts of styrene, 1.5 parts of N-(4-hydroxyphenyl) methacrylamide, 0.05 parts of azobisisobutyronitrile, and 10 parts of propylene glycol monomethyl ether acetate (PGMEA), and reacted for 5 hours at 120 to 130°C under a nitrogen atmosphere to obtain a PGMEA solution of copolymer 1 represented by the following formula (3). A part of the PEGMEA solution was heated under reduced pressure to remove the solvent and unreacted styrene, and the dry mass was calculated as the solid content to obtain copolymer 1, which was 34.8 parts. Considering that the amount of unreacted styrene was 5.2 parts, the obtained copolymer was a copolymer of 33.3 parts of styrene and 1.5 parts of N-(4-hydroxyphenyl) methacrylamide. The number average molecular weight of the sample used for the measurement of the dry mass was 42,000, and the weight average molecular weight was 175,000. From the copolymerization ratio of styrene and N-(4-hydroxyphenyl)methacrylamide and the number average molecular weight, the value of n in formula (3) is calculated to be 386 and the value of m is calculated to be 10.
[0037] [ka]
[0038] (Step 2) Synthesis of the polymer compound of the present invention (polymer compound 1) represented by the following formula (4): From the PGMEA solution of copolymer 1 obtained in step 1, unreacted styrene was distilled off together with PGMEA under heating and reduced pressure, and then PGMEA was added to obtain 138 parts of a 25% by mass solution of copolymer 1. 5 parts of triethylamine were added to this solution, and 0.88 parts of methacrylic acid chloride were added at 60°C under stirring and reacted for 1 hour. The reaction solution was pressure-filtered with a filter paper having a capture particle size of 1 micron to remove triethylamine hydrochloride, and excess triethylamine and PGMEA were distilled off from the filtrate using a rotary evaporator, and the amount of PGMEA was adjusted to obtain 142 parts of a solution containing 25% by mass of the polymer compound of the present invention (polymer compound 1) represented by the following formula (4). The number average molecular weight of the obtained polymer compound 1 was 43,000, and the weight average molecular weight was 181,000.
[0039] [ka]
[0040] Comparative Example 1 (Synthesis of a comparative polymer compound represented by the following formula (6)) (Step 3) Synthesis of Comparative Copolymer (Copolymer 2) A PGMEA solution of copolymer 2 represented by the following formula (5) was obtained in accordance with step 1, except that 1.5 parts of N-(4-hydroxyphenyl) methacrylamide was replaced with 1.5 parts of 2-hydroxyethyl methacrylate. A part of the PEGMEA solution was heated under reduced pressure to remove the solvent and unreacted styrene, and the dry mass of the copolymer 2 was calculated as the solid content, giving a total mass of 35.0 parts. Considering that the amount of unreacted styrene was 5.0 parts, the obtained copolymer was a copolymer of 33.5 parts of styrene and 1.5 parts of 2-hydroxyethyl methacrylate. The number average molecular weight of the sample used for the measurement of the dry mass was 41,000, and the weight average molecular weight was 172,000. From the copolymerization ratio and number average molecular weight of styrene and hydroquinone monomethacrylate, the value of n in formula (3) was calculated to be 377, and the value of m was calculated to be 13.
[0041] [ka]
[0042] (Step 4) Synthesis of the polymer compound of the present invention (polymer compound 2) represented by the following formula (6): Except for changing Copolymer 1 to Copolymer 2 obtained in step 3 and changing the amount of methacrylic acid chloride used from 0.88 parts to 1.21 parts, 143 parts of a solution containing 25 mass% of a comparative polymer compound (polymer compound 2) represented by the following formula (6) was obtained in accordance with step 2. The number average molecular weight of the obtained polymer compound 2 was 47,000 and the weight average molecular weight was 185,000.
[0043] [ka]
[0044] Example 2 (Preparation of Resin Composition of the Present Invention) To 10 parts of the PGMEA solution of the polymer compound 1 of the present invention obtained in Example 1, 0.05 parts of dicumyl peroxide as a radical initiator was added and mixed uniformly to obtain a resin composition 1 of the present invention.
[0045] Comparative Example 2 (Preparation of Comparative Resin Composition) Comparative resin composition 1 was obtained in the same manner as in Example 2, except that the PGMEA solution of polymer compound 1 of the present invention was changed to the PGMEA solution of comparative polymer compound 1 obtained in Comparative Example 1.
[0046] (Evaluation of dielectric properties of cured resin composition) Using an applicator, the resin composition 1 of the present invention and the comparative resin composition 1 obtained in Example 2 and Comparative Example 2 were applied to a mirror surface of a copper foil having a thickness of 18 μm to a thickness of 280 μm, and the solvent was dried by heating at 90 ° C for 10 minutes to obtain a copper foil having a film-like adhesive made of a resin composition. The film-like adhesive on the copper foil obtained above was heated and cured at 180 ° C for 1 hour using a vacuum oven, and then immersed in an etching solution to remove the copper foil, thereby obtaining a cured film-like adhesive having a thickness of 70 μm that can be handled as a film. The dielectric constant and dielectric loss tangent at 10 GHz of the cured product obtained above were measured by a cavity resonance method using a network analyzer 8719ET (manufactured by Agilent Technologies). The results are shown in Table 1.
[0047] (Evaluation of Adhesive Strength of Cured Resin Composition) Using an applicator, the resin composition 1 of the present invention and the comparative resin composition 1 obtained in Example 2 and Comparative Example 2 were applied to a matte surface of a 12 μm thick high-frequency low-roughness copper foil (CF-T4X-SV: manufactured by Fukuda Metal Foil Powder Co., Ltd.) to a thickness of 50 μm, and the solvent was dried by heating at 90° C. for 10 minutes to obtain a copper foil having a film-like adhesive made of the resin composition. The matte surface of the same copper foil as above was placed on the adhesive surface of the resin-coated copper foil obtained above, and the copper foil was heated and cured for 1 hour at a pressure of 3 MPa in a vacuum press, and the 90° peel strength (adhesive strength) between the copper foils was measured using an autograph AGX-50 (manufactured by Shimadzu Corporation). The results are shown in Table 1.
[0048] [Table 1]
[0049] As described above, the polymer compound of the present invention, when cured using a radical initiator, formed a flexible film and further exhibited excellent dielectric properties and adhesive properties.
Claims
1. A film-like adhesive comprising a polymer compound obtained by reacting a copolymer represented by the following formula (2) having a number average molecular weight of 3,000 to 300,000 with (meth)acrylic acid chloride or (meth)acrylic acid, and a radical initiator. [Formula 1] (In formula (2), R1 represents a hydrogen atom or a methyl group. m and n represent the average number of repeating units and each independently represents a real number in the range of 1 to 2,000.)
2. The film-like adhesive according to claim 1 , further comprising a radical-reactive monomer having two or more functional groups in one molecule.
3. 3. The film-like adhesive according to claim 2, wherein the radical reactive monomer is a maleimide compound.
4. A cured product of the film-like adhesive according to any one of claims 1 to 3.
Citation Information
Patent Citations
Kankoseisoseibutsu
JP1976046204A
Photopolymerizable composition
JP1991075750A
Ultraviolet-curable ink composition
JP1998017812A
Image recording material
JP2004045625A
Fluoroplastic copper-clad laminate and manufacturing method thereof
JP2005001274A