Multi-layer resin molded body and its manufacturing method
The multilayer resin molded body with a specific layer structure addresses the issue of insufficient protrusion formation by using a base material and ethylene-vinyl alcohol copolymer resin layer with a modified polyolefin resin layer to create stable, height-appropriate protrusions for marking.
Patent Information
- Application Number
- JP2021034995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-05
AI Technical Summary
Conventional methods for forming protrusions in resin molded articles using laser irradiation often result in insufficient foaming, preventing effective marking.
A multilayer resin molded body structure is employed, comprising a base material, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer, where the latter is interposed between the base material and the ethylene-vinyl alcohol copolymer resin layer, allowing for sufficient foaming and protrusion formation by vaporizing volatile components within the modified polyolefin layer while the ethylene-vinyl alcohol copolymer layer acts as a gas barrier to retain the foamed bulge.
The multilayer structure enables the formation of protrusions with heights ranging from 0.3 to 1.5 mm, suitable for markings, without significant surface roughness or loss of volatile components, thereby enhancing marking quality and consistency.
Smart Images

Figure 0007586736000002 
Figure 0007586736000003 
Figure 0007586736000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-layer resin molded article and a method for producing the same. [Background technology]
[0002] Conventionally, a resin molding made of a thermoplastic resin such as an acrylic resin is irradiated with laser light to foam the resin at the portion irradiated with the laser light, thereby forming a protrusion, thereby providing a resin molding with markings such as letters and figures (see, for example, Patent Document 1).
[0003] The resin molding described in Patent Document 1 is said to be capable of forming a protrusion for marking by irradiating a resin molding made of a thermoplastic resin with laser light to soften and melt the thermoplastic resin, and then vaporizing the volatile components contained in the molten resin, utilizing the phenomenon in which the vaporized components cause the molten resin to foam and rise. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 13287 / 1987 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the resin molding described in Patent Document 1 has the disadvantage that when the molten resin that is softened and melted by the irradiation of the laser light foams, it may not be possible to form a protrusion sufficient for marking.
[0006] An object of the present invention is to provide a multilayer resin molding which overcomes the above-mentioned disadvantages and is capable of forming a protrusion sufficient for marking by foaming a thermoplastic resin, and a method for producing the same. [Means for solving the problem]
[0007] The present inventors have thoroughly investigated the reason why, when laser light is irradiated onto a resin molded product made of a thermoplastic resin and the resin in the area irradiated with the laser light foams, it may not be possible to form a protrusion sufficient for marking.
[0008] As a result, the present inventors discovered that when a resin molded product made of the thermoplastic resin is irradiated with a laser beam to soften and melt the thermoplastic resin, and then volatile components contained in the molten resin are vaporized, the vaporized components are released to the outside of the resin molded product, resulting in insufficient foaming of the molten resin. Based on the above findings, the present inventors conducted further studies and discovered that when a multilayer resin molded product having a specific layer structure is irradiated with a laser beam, the resin melted by the laser beam is sufficiently foamed without the vaporized components being released to the outside of the multilayer resin molded product, and a protrusion sufficient for marking can be formed, thereby arriving at the present invention.
[0009] Therefore, the multilayer resin molding of the present invention is a multilayer resin molding comprising a substrate made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer interposed between the substrate and the ethylene-vinyl alcohol copolymer resin layer, and is characterized in having a foamed, bulging portion formed by the modified polyolefin resin layer, and a protrusion comprising the ethylene-vinyl alcohol copolymer resin layer covering the foamed, bulging portion.
[0010] The multilayer resin molding of the present invention can be produced by a method for producing a multilayer resin molding, comprising: irradiating a multilayer resin molding comprising a substrate made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer interposed between the substrate and the ethylene-vinyl alcohol copolymer resin layer with laser light to heat and soften the ethylene-vinyl alcohol copolymer resin layer, and to heat and foam the modified polyolefin resin layer, and to form protruding portions in which foamed bulges protruding from the surface of the multilayer resin molding due to the foaming are covered with the ethylene-vinyl alcohol copolymer resin layer.
[0011] In the method for producing a multilayer resin molded product of the present invention, a multilayer resin molded product including a substrate made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer interposed between the substrate and the ethylene-vinyl alcohol copolymer resin layer is irradiated with laser light. In this manner, the ethylene-vinyl alcohol copolymer resin layer and the modified polyolefin resin layer are heated, and the ethylene-vinyl alcohol copolymer resin layer is softened, while low molecular weight components and volatile components contained in the modified polyolefin resin layer, and trace amounts of gas components such as air that are inevitably mixed in during the molding process for forming the multilayer resin molded product are vaporized.
[0012] At this time, since the ethylene-vinyl alcohol copolymer resin layer has excellent gas barrier properties, the vaporized components are not released to the outside of the multilayer resin molding, and the modified polyolefin resin layer can be sufficiently foamed to form the foamed bulge. Also, since the ethylene-vinyl alcohol copolymer resin layer is softened by heating, it bulges out following the foamed bulge while maintaining a state of covering the foamed bulge, forming a protrusion in which the foamed bulge is covered by the ethylene-vinyl alcohol copolymer resin layer, thereby obtaining the multilayer resin molding of the present invention.
[0013] In the multilayer resin molding of the present invention, the protrusion preferably has a marking shape such as a letter, a symbol, or a graphic.
[0014] In the multilayer resin molding of the present invention, the protrusion preferably protrudes from the surface of the multilayer resin molding by a height in the range of 0.3 to 1.5 mm. The multilayer resin molding of the present invention is suitable for having the shape of the marking when the protrusion protrudes from the surface of the multilayer resin molding by a height in the range. If the height of the protrusion is less than 0.3 mm, the shape of the marking may be insufficient, and it is technically difficult to make it more than 1.5 mm.
[0015] In the multilayer resin molded product of the present invention, the modified polyolefin resin layer may serve as, for example, an adhesive layer that bonds the substrate and the ethylene-vinyl alcohol copolymer resin layer.
[0016] In the multilayer resin molded product of the present invention, the modified polyolefin resin layer is preferably made of a resin containing an acid-modified polyethylene resin or an acid-modified polypropylene resin modified by copolymerization or graft polymerization of an unsaturated carboxylic acid. The modified polyolefin resin layer is made of the resin, and has a lower melting point than an ethylene-vinyl alcohol copolymer resin, so that the foamed bulge can be easily formed, and the modified polyolefin resin layer can be suitably used as an adhesive layer for bonding the substrate and the ethylene-vinyl alcohol copolymer resin layer.
[0017] The multilayer resin molded article of the present invention can also be made into a synthetic resin container.
[0018] In the method for producing a multilayer resin molded product of the present invention, the laser light is preferably, for example, a UV laser.
[0019] In the method for producing a multilayer resin molded product of the present invention, the ethylene-vinyl alcohol copolymer resin layer preferably has a thickness in the range of 30 to 120 μm. If the ethylene-vinyl alcohol copolymer resin layer has a thickness of less than 30 μm, the vaporized components may be released to the outside of the multilayer resin molded product, resulting in insufficient formation of the foamed bulging portions, whereas if the thickness exceeds 120 μm, the ethylene-vinyl alcohol copolymer resin layer may inhibit the formation of the foamed bulging portions.
[0020] In the method for producing a multilayer resin molding of the present invention, the modified polyolefin resin layer preferably has a thickness in the range of 20 to 90 μm. When the modified polyolefin resin layer has a thickness of less than 20 μm, the formation of the foamed bulging portion may be insufficient, and when the thickness exceeds 90 μm, the foaming may be excessive. [Brief description of the drawings]
[0021] [Figure 1] 1 is a front view showing one embodiment of a synthetic resin container made of a multilayer resin molded product of the present invention. [Diagram 2] FIG. 1 is an explanatory cross-sectional view showing a configuration of a multilayer resin molded body of the present invention. [Diagram 3] FIG. 3 is an explanatory cross-sectional view showing a configuration of a protrusion in the multilayer resin molding of the present invention. [Figure 4] 3 is a photograph showing one embodiment of a protrusion in a multilayer resin molding of the present invention. [Diagram 5] 6 is a photograph showing another embodiment of a protrusion in a multilayer resin molding of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Next, embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0023] As shown in FIG. 1, a synthetic resin container 1 made of the multilayer resin molding of this embodiment is, for example, a multilayer synthetic resin container for toiletries such as cosmetics, and is provided with markings made of protrusions 3a, 3b on the surface of the multilayer resin molding, for example, on the flat body portions 2a, 2b as display areas.
[0024] In the synthetic resin container 1, the protruding portion 3a is hemispherical, and the protruding portion 3b is a truncated pyramid shape that is rectangular in plan view. In the synthetic resin container 1, the protruding portions 3a and 3b protrude from the surfaces of the body flat portions 2a and 2b to a height of 0.3 to 1.5 mm, and can have any marking shape such as letters, symbols, or figures. As a result, the synthetic resin container 1 can be displayed as required by the markings made of the protruding portions 3a and 3b.
[0025] As shown in FIG. 2, the multilayer resin molding 4 forming the synthetic resin container 1 includes a base material 5 made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer 6, and a modified polyolefin resin layer 7 interposed between the base material 5 and the ethylene-vinyl alcohol copolymer resin layer 6.
[0026] Examples of the synthetic resin constituting the base material 5 include polyolefin resins such as polyethylene and polypropylene, and polyester resins such as polyethylene terephthalate.
[0027] The ethylene-vinyl alcohol copolymer resin constituting the ethylene-vinyl alcohol copolymer resin layer 6 has an oxygen permeability of, for example, 3.5 cm 3 20μm / m 2 24hrs atm or less range, preferably 2.5cm 3 20μm / m 2 It has a gas barrier property in the range of 24 hrs·atm or less, and a melting point in the range of 150 to 200° C., preferably 160 to 200° C. The ethylene-vinyl alcohol copolymer resin layer 6 preferably has a thickness in the range of 30 to 120 μm.
[0028] The modified polyolefin resin layer 7 also functions as an adhesive layer that bonds the substrate 5 and the ethylene-vinyl alcohol copolymer resin layer 6, and is preferably made of a resin containing, for example, an acid-modified polyethylene resin or an acid-modified polypropylene resin modified by copolymerization or graft polymerization of an unsaturated carboxylic acid, and is preferably made of a resin having a melting point or softening point lower than that of the ethylene-vinyl alcohol copolymer resin constituting the ethylene-vinyl alcohol copolymer resin layer 6. The modified polyolefin resin layer 7 preferably has a thickness in the range of 20 to 90 μm.
[0029] 3, the protrusions 3a and 3b can be formed by irradiating the multilayer resin molding 4 with laser light to heat and soften the ethylene-vinyl alcohol copolymer resin layer 6, while heating and softening the modified polyolefin resin layer 7 to foam, and covering the foamed bulging portion 8 that has bulged out from the surface of the multilayer resin molding 4 due to the foaming with the ethylene-vinyl alcohol copolymer resin layer 6. As the laser light, a UV laser having a wavelength of 10 to 400 nm in the ultraviolet region, such as a YVO4 laser, can be used.
[0030] Next, an embodiment of the present invention will be described. EXAMPLES
[0031] Example 1 In this embodiment, the substrate 5 is made of black polyethylene containing a black pigment, and the gas barrier property as oxygen permeability is 1.9 cm 3 20μm / m 2 The synthetic resin container 1 was formed as a multilayer resin molded body 4 by co-extrusion molding, with an ethylene-vinyl alcohol copolymer resin (manufactured by Kuraray Co., Ltd., product name: EVAL) having a melting point of 165°C (softening point of 152°C) and a viscosity of 1.0 s·24 hrs·atm used as the ethylene-vinyl alcohol copolymer resin layer 6, and an acid-modified polyethylene (manufactured by Mitsui Chemicals, Inc., product name: Admer NB550) having an acid value of 3.0 to 10 mg / g and a softening point of 126°C, which was obtained by graft-polymerizing an unsaturated carboxylic acid onto polyethylene, being disposed between the substrate 5 and the ethylene-vinyl alcohol copolymer resin layer 6 as the modified polyolefin resin layer 7.
[0032] The synthetic resin container 1 obtained in this example had a substrate 5 having a thickness of 1.0 mm, an ethylene-vinyl alcohol copolymer resin layer 6 having a thickness of 80 μm, and a modified polyolefin resin layer 7 having a thickness of 60 μm.
[0033] Next, a circular area of 1.4 mm in diameter on the body flat portion 2a of the synthetic resin container 1 obtained in this embodiment was irradiated with a YVO4 laser having a wavelength of 355 nm and an output of 2.5 W using a laser irradiation device (manufactured by Keyence Corporation, product name: MD-U1000C) under the conditions of laser power 80%, moving speed 1000 mm / sec, distance between forward and backward paths 50 μm, and irradiation time 0.1 sec to form a protruding portion 3a protruding in a hemispherical shape with a height of about 0.5 mm from the surface of the body flat portion 2a. The obtained protruding portion 3a is shown in FIG. 4.
[0034] The surface of the obtained protrusion 3a was smooth, just like the surface of the ethylene-vinyl alcohol copolymer resin layer 6 before irradiation with the laser beam, and when the protrusion 3a was magnified 30 times to observe the unevenness of the surface, no significant unevenness was observed.
[0035] Example 2 In this example, a rectangular region 2.0 mm wide and 4.5 mm long on the flat body portion 2b of the same synthetic resin container 1 as in Example 1 was irradiated with laser light while moving it in the vertical (length) and horizontal (width) directions, forming a protrusion 3b protruding in the shape of a truncated pyramid having a rectangular shape in plan view at a height of about 0.7 mm from the surface of the flat body portion 2b under exactly the same conditions as in Example 1. The resulting protrusion 3b is shown in FIG.
[0036] The surface of the obtained protrusion 3b was observed in exactly the same manner as in Example 1, and was found to be smooth, similar to the surface of the protrusion 3a in Example 1, with no significant irregularities being observed. Next, five measurement points a to e were selected from within a range of 2.4 mm in the longitudinal direction of the surface of the protrusion 3b, and the surface roughness was measured using a surface roughness measuring device (manufactured by Tokyo Seimitsu Co., Ltd.). The results are shown in Table 1.
[0037] Separately, five measurement points a to e were selected from a range of 2.4 mm in length from the portion of the surface of the ethylene-vinyl alcohol copolymer resin layer 6 that was not irradiated with the laser beam, and the surface roughness was measured in the same manner as the surface of the protrusion 3b. The results are shown in Table 1.
[0038] [Table 1]
[0039] From Table 1, the average value of the surface roughness Ra of the non-irradiated portion of the surface of the ethylene-vinyl alcohol copolymer resin layer 6 is 0.168 μm, whereas the average value of the surface roughness Ra of the surface of the protrusion 3b is 0.201 μm, which is only an increase of 19.6%. Therefore, there is no significant change in the surface roughness Ra of the surface of the ethylene-vinyl alcohol copolymer resin layer 6 before and after the laser beam irradiation, and it is clear that the surface of the protrusion 3b obtained by the laser beam irradiation in this embodiment maintains the same smoothness as the surface of the ethylene-vinyl alcohol copolymer resin layer 6 before the laser beam irradiation, even though it is formed through a process in which the surface of the ethylene-vinyl alcohol copolymer resin layer 6 is heated and softened by the laser beam irradiation, bulges and protrudes, and then cooled and solidified.
[0040] Comparative Example 1 In this comparative example, a laser beam was irradiated to the surface of a resin molding consisting of only a base material 5 made of black polyethylene containing the same black pigment as used in Example 2 in exactly the same manner as in Example 2. As a result, no protrusions were formed on the surface of the resin molding as in Example 2. Even when the laser beam irradiation time was extended, the surface was merely roughened and no protrusions were formed. [Explanation of symbols]
[0041] 1...synthetic resin container; 2a, 2b...flat body portion; 3a, 3b...protruding portion; 4...multilayer resin molded body; 5...substrate; 6...ethylene-vinyl alcohol copolymer resin layer; 7...modified polyolefin resin layer; 8...foamed bulge portion.
Claims
1. A multilayer resin molded article comprising a substrate made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer interposed between the substrate and the ethylene-vinyl alcohol copolymer resin layer, The multi-layer resin molded article is characterized by comprising a protruding portion formed by foaming the modified polyolefin resin layer and an ethylene-vinyl alcohol copolymer resin layer covering the foamed bulge.
2. 2. The multi-layer resin molding according to claim 1, wherein said protrusion has a marking shape selected from the group consisting of letters, symbols, and figures.
3. 3. The multilayer resin molding according to claim 1, wherein the protrusion protrudes from the surface of the multilayer resin molding to a height in the range of 0.3 to 1.5 mm.
4. The multilayer resin molding according to any one of claims 1 to 3, wherein the modified polyolefin resin layer is an adhesive layer that bonds the substrate and an ethylene-vinyl alcohol copolymer resin layer.
5. The multilayer resin molding according to any one of claims 1 to 4, wherein the modified polyolefin resin layer is made of a resin containing an acid-modified polyethylene resin or an acid-modified polypropylene resin modified by copolymerization or graft polymerization of an unsaturated carboxylic acid.
6. The present invention comprises a multilayer resin molded product including a substrate made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer interposed between the substrate and the ethylene-vinyl alcohol copolymer resin layer, The synthetic resin container is characterized by comprising a protruding portion formed by foaming the modified polyolefin resin layer and an ethylene-vinyl alcohol copolymer resin layer covering the foamed bulging portion.
7. A multilayer resin molded product including a substrate made of a synthetic resin, an ethylene-vinyl alcohol copolymer resin layer, and a modified polyolefin resin layer interposed between the substrate and the ethylene-vinyl alcohol copolymer resin layer is irradiated with laser light; the ethylene-vinyl alcohol copolymer resin layer is heated to soften it, while the modified polyolefin resin layer is heated to foam it, The method for producing a multi-layer resin molded article comprises forming a protrusion by covering a foamed bulge portion bulging out from the surface of the multi-layer resin molded article by the foaming with the ethylene-vinyl alcohol copolymer resin layer.
8. 8. The method for producing a multi-layer resin molded article according to claim 7, wherein the laser light is a UV laser.
9. 9. The method for producing a multi-layer resin molded article according to claim 7, wherein the ethylene-vinyl alcohol copolymer resin layer has a thickness in the range of 30 to 120 μm.
10. The method for producing a multilayer resin molded article according to any one of claims 7 to 9, wherein the modified polyolefin resin layer has a thickness in the range of 20 to 90 µm.
Citation Information
Patent Citations
Polyolefin composition and multilayer laminate
JP1981072033A
Marking method for resin
JP1987013287A
Method for cutting coating of laminate
JP1990284779A
Multilayered structure obtained by co-extrusion coating and production thereof
JP2000177067A
Thermoplastic resin composition for white color marking use
JP2006335849A