Polystyrene resin foam sheet and polystyrene resin foam container

A heat-resistant polystyrene resin foam sheet with controlled bubble diameters and reduced foaming agent content addresses surface blistering and tertiary foaming issues in microwave containers, enhancing safety and performance.

JP7586750B2Active Publication Date: 2024-11-19SEKISUI PLASTICS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021054749
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-11-19
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Polystyrene resin foam containers used for microwave heating often experience surface blistering and tertiary foaming due to local heating, which is a problem exacerbated by the use of flammable and hazardous dimethyl ether as a blowing agent in existing manufacturing methods.

Method used

A polystyrene resin foam sheet is developed with a heat-resistant layer that includes specific bubble diameter ratios and a controlled foaming agent content, eliminating the need for dimethyl ether, thereby reducing the likelihood of surface blistering and tertiary foaming during heating.

Benefits of technology

The solution effectively prevents surface blistering and tertiary foaming in polystyrene resin foam containers when heated, ensuring safety and reliability without using hazardous chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586750000002
    Figure 0007586750000002
  • Figure 0007586750000003
    Figure 0007586750000003
  • Figure 0007586750000001
    Figure 0007586750000001
Patent Text Reader

Abstract

To provide a polystyrene-based resin foam sheet which enables thermoforming of a resin foam container that is difficult to generate a blister and tertiary foaming thereon with minimizing dimethylether.SOLUTION: A polystyrene-based resin foam sheet contains a heat-resistant polystyrene-based resin foam layer obtained by extrusion-foaming a resin composition containing a polystyrene-based resin and a foaming agent, wherein a content of the foaming agent with respect to 100 pts.mass of the polystyrene-based resin is 0.5-3.5 pts.mass, and when an average bubble diameter in an MD direction of air bubbles that the foam layer has is represented by dM (mm), an average bubble diameter in a TD direction is represented by dT (mm) and an average bubble diameter in a VD direction is represented by dV (mm), the average bubble diameters satisfy Expression (1) and Expression (2), and satisfy Expression (3) or Expression (4). Expression (1): 0≤(dM-dV) / dM<0.6, Expression (2): 0≤(dT-dV) / dT<0.6, Expression (3): 0≤(dM-dT) / dM<0.2, wherein dM≥dT, and Expression (4): 0<(dT-dM) / dT<0.2, wherein dT>dM.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polystyrene-based resin foamed sheet and a polystyrene-based resin foamed container. [Background technology]

[0002] Containers obtained by thermoforming polystyrene-based resin foam sheets are widely used in convenience stores and the like as various containers such as trays, lunch boxes, rice bowls, and cups. Among them, in recent years, there has been an increasing demand for so-called microwave-ready containers, which are intended for heating cooked foods in a packaged state in a microwave oven. As such microwave-ready containers, those thermoformed from heat-resistant polystyrene-based resin foam sheets are widely used. Such polystyrene-based resin foam sheets are usually produced by laminating other functional films, as necessary, on a foam sheet obtained by extruding and foaming a resin composition containing a polystyrene-based resin and a foaming agent.

[0003] From the viewpoints of light weight and cost reduction, it is preferable that the polystyrene-based resin foam sheet used for forming a microwaveable container has a low apparent density. However, when a container obtained by thermoforming a polystyrene-based resin foam sheet having a low apparent density is heated in a microwave oven while food such as pasta is packed in the container, there is a problem that partial swelling (blisters) or worm-like bubbles (tertiary foaming) occur on the surface of the container. This is presumably caused by localized heating of the surface of the container due to heat transfer from the food.

[0004] In order to solve the above problems, a method for producing a polystyrene-based resin foamed sheet using a foaming agent containing butane and dimethyl ether has been reported (Patent Document 1).

[0005] However, the manufacturing method described in Patent Document 1 uses dimethyl ether, a highly flammable, explosive, and harmful combustible high-pressure gas, and therefore mass-producing polystyrene-based resin foam sheets using this manufacturing method is extremely dangerous. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-210312 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made to solve the above-mentioned problems in the conventional art, and its main object is to provide a polystyrene-based resin foam sheet capable of thermoforming a polystyrene-based resin foam container which is less likely to develop blisters or tertiary expansion on its surface when heated, with minimal use of dimethyl ether, and to provide a polystyrene-based resin foam container which is less likely to develop blisters or tertiary expansion on its surface when heated. [Means for solving the problem]

[0008] The polystyrene-based resin foam sheet according to the embodiment of the present invention is A polystyrene-based resin foam sheet comprising a heat-resistant polystyrene-based resin foam layer (A), The heat-resistant polystyrene-based resin foam layer (A) is obtained by extrusion foaming a resin composition containing a polystyrene-based resin (I) and a foaming agent, The content of the foaming agent relative to 100 parts by mass of the polystyrene-based resin (I) is 0.5 parts by mass to 3.5 parts by mass, The extrusion flow direction of the polystyrene-based resin foamed sheet is defined as the MD direction, the width direction perpendicular to the MD direction on the surface of the polystyrene-based resin foamed sheet is defined as the TD direction, and the thickness direction perpendicular to both the MD direction and the TD direction is defined as the VD direction, When the average cell diameter in the MD direction of the bubbles in the heat-resistant polystyrene-based resin foam layer (A) is dM (mm), the average cell diameter in the TD direction is dT (mm), and the average cell diameter in the VD direction is dV (mm), the heat-resistant polystyrene-based resin foam layer (A) satisfies formulas (1) and (2) and also satisfies formula (3) or formula (4). 0≦(dM-dV) / dM<0.6 (1) 0≦(dT-dV) / dT<0.6 (2) 0≦(dM-dT) / dM<0.2 (where dM≧dT) (3) 0<(dT-dM) / dT<0.2 (where dT>dM) (4)

[0009] In one embodiment, the polystyrene resin (I) includes a heat-resistant polystyrene resin (i) having a Vicat softening temperature of 110° C. or higher.

[0010] In one embodiment, the polystyrene-based resin foam sheet according to the embodiment of the present invention has a thickness of 0.5 mm to 4.0 mm.

[0011] In one embodiment, the polystyrene-based resin foam sheet according to the embodiment of the present invention has a basis weight of 80 g / m 2 ~400g / m 2 It is.

[0012] In one embodiment, the heat-resistant polystyrene-based resin foam layer (A) has an expansion ratio of 13 times or less.

[0013] In one embodiment, the apparent density of the heat-resistant polystyrene-based resin foam layer (A) is 0.05 g / cm 3 ~0.30g / cm 3 It is.

[0014] In one embodiment, the heat-resistant polystyrene resin foam layer (A) has an average cell diameter of 0.05 mm to 0.50 mm.

[0015] The laminated polystyrene resin foam sheet according to the embodiment of the present invention is obtained by laminating a non-foamed resin film on the polystyrene resin foam sheet according to the embodiment of the present invention.

[0016] The polystyrene-based resin foam container according to the embodiment of the present invention is obtained by thermoforming the polystyrene-based resin foam sheet according to the embodiment of the present invention or the laminated polystyrene-based resin foam sheet according to the embodiment of the present invention.

[0017] In one embodiment, the polystyrene-based resin foam container according to the embodiment of the present invention has a foaming agent content of 3.1% by mass or less. Effect of the Invention

[0018] According to the present invention, it is possible to provide a polystyrene-based resin foam sheet capable of thermoforming a polystyrene-based resin foam container which is resistant to the formation of blisters or tertiary expansion on its surface when heated, while using dimethyl ether as little as possible, and a polystyrene-based resin foam container which is resistant to the formation of blisters or tertiary expansion on its surface when heated. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a schematic explanatory view showing one embodiment of a method for producing a heat-resistant polystyrene-based resin foam layer (A). [Diagram 2] 1 is a schematic perspective view showing one embodiment of a polystyrene-based resin foam container of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0021] In this specification, "(meth)acrylic" means acrylic and / or methacrylic, and "(meth)acrylate" means acrylate and / or methacrylate.

[0022] <<Polystyrene resin foam sheet>> The polystyrene-based resin foam sheet according to the embodiment of the present invention is a polystyrene-based resin foam sheet including a heat-resistant polystyrene-based resin foam layer (A). The heat-resistant polystyrene-based resin foam layer (A) may be a single layer or two or more layers.

[0023] The polystyrene-based resin foam sheet according to the embodiment of the present invention may be composed of, for example, only the heat-resistant polystyrene-based resin foam layer (A).

[0024] The polystyrene-based resin foam sheet according to the embodiment of the present invention may include any other appropriate layer as long as it includes the heat-resistant polystyrene-based resin foam layer (A) and does not impair the effects of the present invention. Examples of such other layers include other polystyrene-based resin foam layers. The other polystyrene-based resin foam layer may be only one layer or two or more layers.

[0025] The thickness of the polystyrene-based resin foamed sheet according to the embodiment of the present invention may be any appropriate thickness within a range that does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, the thickness of the polystyrene-based resin foamed sheet according to the embodiment of the present invention is preferably 0.5 mm to 4.0 mm, more preferably 0.8 mm to 3.5 mm, even more preferably 1.0 mm to 3.0 mm, and particularly preferably 1.1 mm to 2.5 mm.

[0026] The basis weight of the polystyrene-based resin foamed sheet according to the embodiment of the present invention may be any appropriate thickness within a range that does not impair the effects of the present invention. In order to more effectively exhibit the effects of the present invention, the basis weight of the polystyrene-based resin foamed sheet according to the embodiment of the present invention is preferably 80 g / m 2 ~400g / m 2 and more preferably 90 g / m 2 ~350g / m 2 and more preferably 100 g / m 2 ~300g / m 2 and particularly preferably 110 g / m 2 ~250g / m 2 It is.

[0027] <Heat-resistant polystyrene resin foam layer (A)> The heat-resistant polystyrene-based resin foam layer (A) is typically formed by foaming a polystyrene-based resin (I). The heat-resistant polystyrene-based resin foam layer (A) is typically obtained by extruding and foaming a resin composition containing a polystyrene-based resin (I) and a foaming agent. More specifically, the heat-resistant polystyrene-based resin foam layer (A) is typically formed by heating and melting and kneading the polystyrene-based resin (I), the foaming agent, and various additives such as a cell regulator added as necessary together in an extruder, cooling to a predetermined temperature, extruding from a die into a sheet shape and foaming, and immediately cooling.

[0028] The thickness of the heat-resistant polystyrene-based resin foam layer (A) may be any appropriate thickness within the range that does not impair the effects of the present invention. The thickness of the heat-resistant polystyrene-based resin foam layer (A) is preferably 0.5 mm to 4.0 mm, more preferably 0.8 mm to 3.5 mm, further preferably 1.0 mm to 3.0 mm, and particularly preferably 1.1 mm to 2.5 mm, in order to further exhibit the effects of the present invention.

[0029] The basis weight of the heat-resistant polystyrene-based resin foam layer (A) may be any appropriate basis weight within a range that does not impair the effects of the present invention. The basis weight of the heat-resistant polystyrene-based resin foam layer (A) is preferably 80 g / m2 in order to further exhibit the effects of the present invention. 2 ~400g / m 2 and more preferably 90 g / m 2 ~350g / m 2 and more preferably 100 g / m 2 ~300g / m 2 and particularly preferably 110 g / m 2 ~250g / m 2 It is.

[0030] The expansion ratio of the heat-resistant polystyrene-based resin foam layer (A) may be any appropriate expansion ratio within a range that does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, the expansion ratio of the heat-resistant polystyrene-based resin foam layer (A) is preferably 13 times or less, more preferably 2 to 13 times, even more preferably 3 to 12 times, and particularly preferably 4 to 11 times.

[0031] The apparent density of the heat-resistant polystyrene-based resin foam layer (A) may be any appropriate apparent density within a range that does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, the apparent density of the heat-resistant polystyrene-based resin foam layer (A) is preferably 0.05 g / cm 3 ~0.30g / cm 3 and more preferably 0.08 g / cm 3 ~0.25g / cm 3 and more preferably 0.08 g / cm 3 ~0.20g / cm 3 and particularly preferably 0.08 g / cm 3 ~0.18g / cm 3 The apparent density of the heat-resistant polystyrene-based resin foam layer (A) is measured, for example, by the method described in JIS K7222:1999 "Foamed plastics and rubber - Measurement of apparent density".

[0032] The density of the surface layer (200 μm thick part from the surface) of the heat-resistant polystyrene-based resin foam layer (A) (hereinafter, sometimes referred to as the surface layer density) is preferably higher than the overall apparent density. When the surface layer density is higher than the overall apparent density, the impact resistance of the heat-resistant polystyrene-based resin foam layer (A) is enhanced. The surface layer having a density higher than the overall apparent density may be formed on one side of the heat-resistant polystyrene-based resin foam layer (A) or on both sides. The surface layer density can be adjusted to an arbitrary range by adjusting the temperature and air volume of the cooling air, the temperature of the circular die, the cooling temperature at the mandrel, etc., when producing the heat-resistant polystyrene-based resin foam layer (A). The ratio represented by (surface layer density / overall apparent density) (hereinafter, sometimes referred to as the surface layer density ratio) is preferably 1.5 to 2.5, more preferably 1.8 to 2.2. If the surface layer density ratio is within the above range, the impact resistance of the heat-resistant polystyrene-based resin foam layer (A) can be increased and foaming properties suitable for molding can be exhibited.

[0033] The midpoint glass transition temperature (Tmg) of the heat-resistant polystyrene resin foam layer (A) is preferably 100°C or higher, more preferably 105°C or higher, even more preferably 110°C or higher, and particularly preferably 115°C or higher, in order to further exert the effects of the present invention.

[0034] The heat-resistant polystyrene resin foam layer (A) has a volume (V 2 ) and the apparent volume of the foam layer (V 1 ) based on the following formula, is preferably 20% or less, more preferably 15% or less, further preferably 12% or less, and particularly preferably 10% or less. Open cell ratio (%) = 100 × [(V 1 -V 2 ) / V 1 ]

[0035] The polystyrene resin (I) may be one type of polystyrene resin or a mixture of two or more types of polystyrene resins.

[0036] In the polystyrene-based resin foam sheet according to the embodiment of the present invention, the content of the foaming agent relative to 100 parts by mass of the polystyrene-based resin (I) is preferably 0.5 parts by mass to 3.5 parts by mass, more preferably 1.0 parts by mass to 3.4 parts by mass, even more preferably 1.5 parts by mass to 3.4 parts by mass, and particularly preferably 2.0 parts by mass to 3.4 parts by mass, in order to more effectively exhibit the effects of the present invention. If the content of the foaming agent relative to 100 parts by mass of the polystyrene-based resin (I) is too high outside the above range, when the polystyrene-based resin foam container obtained by thermoforming the polystyrene-based resin foam sheet is heated, blisters or tertiary foaming may occur on the container surface. If the content of the foaming agent relative to 100 parts by mass of the polystyrene-based resin (I) is too low outside the above range, the foaming state of the polystyrene-based resin foam container obtained by thermoforming the polystyrene-based resin foam sheet may be poor, and there may be a risk of a decrease in toughness or the occurrence of cracks.

[0037] Examples of the polystyrene resin (I) include homopolymers of styrene monomers such as styrene, α-methylstyrene, vinyltoluene, ethylstyrene, i-propylstyrene, t-butylstyrene, dimethylstyrene, bromostyrene, and chlorostyrene; copolymers of the above styrene monomers; copolymers of the above styrene monomers and carboxylic acid esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cetyl (meth)acrylate, (meth)acrylonitrile, dimethyl maleate, dimethyl fumarate, diethyl fumarate, and ethyl fumarate); copolymers of the above styrene monomers and bifunctional monomers (e.g., divinylbenzene, alkylene glycol dimethacrylate, and the like); block copolymers having a rubber component block such as butadiene or isoprene and a styrene block, and high impact polystyrenes (high impact polystyrene, HIPS) such as graft copolymers in which the rubber component block is grafted to a molecular chain made of styrene; and the like. The polystyrene resin (I) may be a polystyrene resin made from recycled raw materials. The styrene monomer preferably contains at least styrene. The content of styrene in the total amount of the styrene monomer is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0038] As the polystyrene resin (I), a commercially available product mixed with other resins may be used. The other resins may be one type only or two or more types.

[0039] The polystyrene resin (I) may be used in combination with other resins to form a resin composition containing the polystyrene resin (I) and a foaming agent. The other resins may be one type or two or more types.

[0040] In order to further exert the effects of the present invention, the content of the polystyrene-based resin (I) in the resin composition containing the polystyrene-based resin (I) and a foaming agent is preferably 30% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, even more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass.

[0041] Examples of such other resins include polyolefin resins, (meth)acrylic resins, polyphenylene ether resins such as poly(2,6-dimethylphenylene-1,4-ether), poly(2,6-diethylphenylene-1,4-ether), and poly(2,6-dichlorophenylene-1,4-ether), styrene-butadiene-styrene copolymer rubber (SBS), styrene-isoprene-styrene block copolymer rubber (SIPS), styrene-butadiene-butylene-styrene copolymer rubber (SBBS), styrene-ethylene-butylene-styrene block copolymer rubber (SEBS), styrene-ethylene-propylene-styrene block copolymer rubber (SEPS), and acrylonitrile-butadiene-styrene copolymer.

[0042] Specific examples of polyolefin resins include polyethylene resins such as branched low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, and crosslinked products of these polymers; polypropylene resins such as propylene homopolymer, propylene-vinyl acetate copolymer, ethylene-propylene random copolymer, propylene-1-butene copolymer, and ethylene-propylene-butene random copolymer; and the like. Among these polyolefin resins, preferred are ethylene-vinyl acetate copolymer, high-density polyethylene, linear low-density polyethylene, and mixtures thereof. The low density is preferably 0.91 g / cm. 3 ~0.94g / cm 3 and more preferably 0.91 g / cm 3 ~0.93g / cm 3The high density is preferably 0.95 g / cm 3 ~0.97g / cm 3 and more preferably 0.95 g / cm 3 ~0.96g / cm 3 Medium density is a density between low and high density.

[0043] The polystyrene resin (I) preferably contains a heat-resistant polystyrene resin (i) having a Vicat softening temperature of 110° C. or more, in terms of being able to more effectively exhibit the effects of the present invention. The Vicat softening temperature is typically specified in JIS K7206. The heat-resistant polystyrene resin (i) may be of only one type, or of two or more types. Examples of the heat-resistant polystyrene resin (i) include a mixed resin of a polystyrene resin and polyphenylene ether (e.g., trade name "Noryl EFN4230" manufactured by Sabic Corporation), a styrene-methacrylic acid copolymer, a styrene-maleic anhydride copolymer, a styrene-maleimide copolymer, and a polyparamethylstyrene resin.

[0044] The content of the heat-resistant polystyrene resin (i) in the polystyrene resin (I) may be any appropriate content ratio within the range that does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, the content of the heat-resistant polystyrene resin (i) in the polystyrene resin (I) is preferably 10% by mass to 50% by mass, more preferably 10% by mass to 45% by mass, even more preferably 10% by mass to 40% by mass, and particularly preferably 10% by mass to 30% by mass.

[0045] The heat-resistant polystyrene foam layer (A) preferably satisfies formulas (1) and (2) and also formula (3) or (4) in that the effects of the present invention can be more effectively exhibited when the average cell diameter in the MD direction of the heat-resistant polystyrene foam layer (A) is dM (mm), the average cell diameter in the TD direction is dT (mm), and the average cell diameter in the VD direction is dV (mm). 0≦(dM-dV) / dM<0.6 (where dM≧dV) (1) 0≦(dT-dV) / dT<0.6, where dT≧dV) (2) 0≦(dM-dT) / dM<0.2 (where dM≧dT) (3) 0<(dT-dM) / dT<0.2 (where dT>dM) (4)

[0046] Here, the MD direction is the extrusion flow direction of the polystyrene-based resin foam sheet, the TD direction is the width direction perpendicular to the MD direction on the surface of the polystyrene-based resin foam sheet, and the VD direction is the thickness direction perpendicular to both the MD and TD directions.

[0047] Formula (1) is the flattening ratio when the bubble diameter dM in the MD direction and the bubble diameter dV in the VD direction of the bubbles in the heat-resistant polystyrene-based resin foam layer (A) are viewed in a plane, and formula (2) is the flattening ratio reflecting the distortion of the flattening ratio when the bubble diameter dT in the TD direction and the bubble diameter dV in the VD direction of the bubbles in the heat-resistant polystyrene-based resin foam layer (A) are viewed in a plane. By satisfying formulas (1) and (2), the bubbles in the heat-resistant polystyrene-based resin foam layer (A) become nearly spherical, and therefore, even if the amount of foaming agent is reduced, when a polystyrene-based resin foam container obtained by thermoforming a polystyrene-based resin foam sheet is heated, blisters and tertiary foaming may be unlikely to occur on the container surface.

[0048] Formula (3) represents the circularity in the plane formed by the MD and TD directions when dM≧dT, and formula (4) represents the circularity in the plane formed by the MD and TD directions when dT>dM. By satisfying formula (3) or (4), the circularity in the plane formed by the MD and TD directions of the bubbles in the heat-resistant polystyrene-based resin foam layer (A) becomes close to a perfect circle. As a result, even if the amount of foaming agent is reduced, when a polystyrene-based resin foam container obtained by thermoforming a polystyrene-based resin foam sheet is heated, blisters and tertiary foaming are unlikely to occur on the container surface.

[0049] The average cell diameter of the bubbles in the heat-resistant polystyrene foam layer (A) may be any appropriate average cell diameter within the range not impairing the effects of the present invention. In order to more effectively exhibit the effects of the present invention, the average cell diameter of the bubbles in the heat-resistant polystyrene foam layer (A) is preferably 0.05 mm to 0.50 mm, more preferably 0.08 mm to 0.45 mm, even more preferably 0.10 mm to 0.40 mm, and particularly preferably 0.15 mm to 0.36 mm.

[0050] The average cell diameter of the entire cells in the heat-resistant polystyrene resin foam layer (A) is calculated by the cube root of (dM x dT x dV) using the average cell diameter in the MD direction dM (mm), the average cell diameter in the TD direction dT (mm), and the average cell diameter in the VD direction dV (mm). Average bubble diameter d(mm)=(dM(mm)×dT(mm)×dV(mm)) (1 / 3)

[0051] The heat-resistant polystyrene-based resin foam layer (A) is typically obtained by extrusion foaming a resin composition containing a polystyrene-based resin (I) and a foaming agent.

[0052] As the blowing agent, any appropriate blowing agent can be used as long as it does not impair the effects of the invention. Examples of such blowing agents include propane, i-butane, n-butane, i-pentane, n-pentane, N 2 , CO 2 , N 2 / CO 2 , water, water and -OH, -COOH, -CN, -NH 3 , -OSO 3 H, -NH, CO, NH 2 , -CONH 2 , -COOR, -CHSO 3 H, -SO 3 H, -COONH 4 In terms of being able to more effectively exhibit the effects of the present invention, the blowing agent is preferably at least one selected from i-butane and n-butane.

[0053] In the present invention, it is preferable that the foaming agent contains as little dimethyl ether as possible. By containing as little diethyl ether as possible, it is possible to safely mass-produce polystyrene resin foamed sheets without using dimethyl ether, which is a highly flammable, explosive, and harmful combustible high-pressure gas. The content of dimethyl ether in the foaming agent is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 10% by mass or less, particularly preferably 5% by mass or less, and most preferably substantially 0% by mass.

[0054] The resin composition containing the polystyrene resin (I) and the foaming agent may contain additives such as a cell regulator, a stabilizer, an ultraviolet absorber, an antioxidant, a colorant (including a pigment), a deodorant, a foam nucleating agent, a nucleating agent, a lubricant, a flame retardant, an antistatic agent, etc. The additives may be of only one kind or of two or more kinds.

[0055] Examples of the foam regulator include inorganic powders such as talc and silica; acid salts of polycarboxylic acids; and reaction mixtures of polycarboxylic acids with sodium carbonate or sodium bicarbonate.

[0056] Examples of the stabilizer include calcium zinc-based heat stabilizers, tin-based heat stabilizers, and lead-based heat stabilizers.

[0057] Examples of the ultraviolet ray absorbent include cesium oxide-based ultraviolet ray absorbents and titanium oxide-based ultraviolet ray absorbents.

[0058] Examples of the antioxidant include cerium oxide, cerium oxide / zirconia solid solution, cerium hydroxide, carbon, carbon nanotubes, titanium oxide, and fullerene.

[0059] Examples of colorants include titanium oxide, carbon black, titanium yellow, iron oxide, ultramarine blue, cobalt blue, calcined pigments, metallic pigments, mica, pearl pigments, zinc oxide, precipitated silica, and cadmium red.

[0060] Examples of deodorants include silica, zeolite, zirconium phosphate, and calcined hydrotalcite.

[0061] <Production of heat-resistant polystyrene resin foam layer (A)> The heat-resistant polystyrene-based resin foam layer (A) can be produced by any appropriate method as long as the effects of the present invention are not impaired.

[0062] One embodiment of the method for producing a heat-resistant polystyrene-based resin foam layer (A) will be described with reference to Fig. 1. The production apparatus 1 in Fig. 1 is an apparatus for obtaining a heat-resistant polystyrene-based resin foam layer (A) by extrusion molding, and includes an extruder 10, a foaming agent supply source 18, a circular die 20, a mandrel 30, and two winders 40.

[0063] The extruder 10 is a so-called tandem type extruder, and is configured such that a first extrusion section 11 and a second extrusion section 12 are connected by a pipe 16. The first extrusion section 11 is equipped with a hopper 14, and a foaming agent supply source 18 is connected to the first extrusion section 11. A circular die 20 is connected to the second extrusion section 12, and a mandrel 30 equipped with a cutter 32 is provided downstream of the circular die 20. A cooling blower (not shown) is provided between the circular die 20 and the mandrel 30.

[0064] First, the raw material constituting the heat-resistant polystyrene-based resin foam layer (A) is charged from the hopper 14 into the first extrusion section 11. The raw material charged from the hopper 14 is the resin constituting the heat-resistant polystyrene-based resin foam layer (A) and additives that are mixed as necessary.

[0065] In the first extrusion section 11, the raw materials are mixed while being heated to a given temperature to form a resin melt, and a foaming agent is supplied from a foaming agent supply source 18 to the first extrusion section 11, and the foaming agent is mixed with the resin melt to form a mixture. The heating temperature is appropriately determined taking into consideration the type of resin, etc.

[0066] The mixture is supplied from the first extrusion section 11 through the pipe 16 to the second extrusion section 12, where it is further mixed and cooled to a desired temperature, and then guided to a resin flow path in the circular die 20. The mixture guided to the resin flow path is extruded from the circular die 20, and the foaming agent foams to form a cylindrical foamed sheet 2a.

[0067] The cylindrical foamed sheet 2a is guided to the mandrel 30 while being blown with cooling air sent from a cooling blower. The cylindrical foamed sheet 2a passes over the outer surface of the mandrel 30, is cooled to a desired temperature, and is cut into two pieces by a cutter 32 to form a sheet-like heat-resistant polystyrene-based resin foamed layer (A) 2. The heat-resistant polystyrene-based resin foamed layer (A) 2 is wound around a guide roll 42 and a guide roll 44, respectively, and taken up by a winder 40 to form a roll-like heat-resistant polystyrene-based resin foamed layer (A) 4.

[0068] From the viewpoint of further exerting the effects of the present invention, it is preferable to produce the heat-resistant polystyrene-based resin foam layer (A) under the following conditions. By producing the heat-resistant polystyrene-based resin foam layer (A) under the following conditions, when the average cell diameter in the MD direction of the cells of the heat-resistant polystyrene-based resin foam layer (A) is dM (mm), the average cell diameter in the TD direction is dT (mm), and the average cell diameter in the VD direction is dV (mm), the formulas (1) and (2) can be satisfied, and also the formula (3) or (4) can be satisfied. 0≦(dM-dV) / dM<0.6 (1) 0≦(dT-dV) / dT<0.6 (2) 0≦(dM-dT) / dM<0.2 (where dM≧dT) (3) 0<(dT-dM) / dT<0.2 (where dT>dM) (4)

[0069] (Blow-up ratio) The ratio of the mandrel aperture to the die lip aperture of the circular die (blow-up ratio) is preferably 3.0 to 4.5, and more preferably 3.5 to 4.5.

[0070] (Die lip clearance) The die lip clearance is preferably 0.20 mm to 1.0 mm, and more preferably 0.25 mm to 1.0 mm.

[0071] (Extruder temperature) The extruder temperature is preferably set to 90°C to 310°C.

[0072] (shear rate) The shear rate is preferably 1000 sec -1 ~8000sec -1 More preferably, 1500 sec -1 ~8000sec -1 Let us assume that.

[0073] (Temperature of molten resin near the mold exit) The temperature of the molten resin near the die outlet is preferably 145°C to 200°C.

[0074] (Extrusion amount) The extrusion rate is preferably 75 kg / h to 800 kg / h.

[0075] (Air temperature) The temperature of the air used after extrusion through a circular die and foam molding into a cylindrical shape is preferably 10°C to 80°C.

[0076] (Air volume) The amount of air used after extruding from the circular die and foaming into a cylindrical shape is preferably 0.1 m 3 / m 2 ~5.0m 3 / m 2 Let us assume that.

[0077] (Air timing) The treatment is preferably carried out within 5 seconds immediately after the material is extruded from the circular die and foam-molded into a cylindrical shape.

[0078] <Other polystyrene resin foam layers> The polystyrene resin foam sheet of the present invention may contain other polystyrene resin foam layers in addition to the heat-resistant polystyrene resin foam layer (A).

[0079] As the other polystyrene-based resin foam layer, any appropriate polystyrene-based resin foam layer can be used as long as it is a foam layer different from the heat-resistant polystyrene-based resin foam layer (A) and does not impair the effects of the present invention.

[0080] The other polystyrene-based resin foam layer is a polystyrene-based resin foam layer having lower heat resistance than the heat-resistant polystyrene-based resin foam layer (A), and typically is a polystyrene-based resin foam layer similar to the heat-resistant polystyrene-based resin foam layer (A) except that it is formed by foaming a polystyrene-based resin (II) different from the polystyrene-based resin (I).

[0081] When the polystyrene-based resin foam sheet of the present invention is a laminate of a heat-resistant polystyrene-based resin foam layer (A) and another polystyrene-based resin foam layer, the production method thereof is typically as follows: the raw material constituting the heat-resistant polystyrene-based resin foam layer (A) is heated and melted in a first extruder together with various additives such as a foaming agent and a bubble regulator added as necessary, and the raw material constituting the other polystyrene-based resin foam layer is heated and melted in a second extruder together with various additives such as a foaming agent and a bubble regulator added as necessary, and laminated and foamed by supplying to a joining die, and then cooling to a predetermined temperature as necessary, and then co-extruded from a die and immediately cooled to produce the polystyrene-based resin foam sheet of the present invention, which is a laminate of the heat-resistant polystyrene-based resin foam layer (A) and another polystyrene-based resin foam layer. The polystyrene-based resin foam sheet after production is preferably left for a while, and the remaining foaming gas is replaced with air.

[0082] In the case where the polystyrene-based resin foam sheet of the present invention is a laminate of a heat-resistant polystyrene-based resin foam layer (A) and another polystyrene-based resin foam layer, a more specific preferred embodiment of the production method thereof is as follows: a raw material constituting the heat-resistant polystyrene-based resin foam layer (A) is supplied to a first extruder together with a foaming agent and various additives such as a cell regulator added as required, a raw material constituting the other polystyrene-based resin foam layer is supplied to a second extruder together with a foaming agent and various additives such as a cell regulator added as required, the molten resin extruded from the first extruder and the molten resin extruded from the second extruder are joined at a joining die, the molten resin joined at the joining die is separated into an outer peripheral side and an inner peripheral side, and extruded and foamed into a cylindrical shape, and a slit is formed. A cylindrical foam having a two-layer structure is formed using a circular die or the like, and the cylindrical foam extruded and foamed from the annular outlet of the circular die is fed to a cooling mandrel arranged downstream (forward in the extrusion direction) of the circular die, the diameter of which is larger than the outlet, and the foam is drawn while the inner surface of the foam is brought into sliding contact with the outer circumferential surface of the cooling mandrel, the foam is expanded in diameter by the cooling mandrel and cooled from the inside, and the foam is continuously cut in the extrusion direction by a cutter provided downstream of the cooling mandrel and developed into a flat sheet into a long strip, thereby producing the polystyrene foam sheet of the present invention, which is a laminate of a heat-resistant polystyrene foam layer (A) and another polystyrene foam layer. The polystyrene foam sheet after production is preferably left to stand for a while to replace the remaining foaming gas with air.

[0083] <<Polystyrene resin laminated foam sheet>> The laminated polystyrene resin foam sheet according to the embodiment of the present invention is obtained by laminating a non-foamed resin film on the polystyrene resin foam sheet according to the embodiment of the present invention.

[0084] Examples of non-foamed resin films include non-foamed impact-resistant polystyrene-based resin films and non-foamed films containing thermoplastic resins.

[0085] The polystyrene-based resin laminated foam sheet according to the embodiment of the present invention can be produced by any appropriate method within the scope of not impairing the effects of the present invention. As a representative example of such a production method, the polystyrene-based resin laminated foam sheet according to the embodiment of the present invention can be produced by laminating a non-foamed resin film on the polystyrene-based resin foam sheet according to the embodiment of the present invention. Specifically, for example, the raw material constituting the non-foamed resin film is supplied to an extruder together with various additives added as necessary, heated and melted, kneaded, cooled to a predetermined temperature, extruded from a die into a film, and laminated on the surface of the polystyrene-based resin foam sheet according to the embodiment of the present invention before it is completely cooled, and heat treatment is performed during the lamination. As a result, the non-foamed resin film is laminated on the polystyrene-based resin foam sheet according to the embodiment of the present invention.

[0086] Examples of various additives that may be added to the raw materials constituting the non-foamed resin film as necessary include stabilizers, ultraviolet absorbers, antioxidants, colorants (including pigments), deodorants, lubricants, flame retardants, and antistatic agents. The additives may be one type or two or more types. The explanation of these additives may be cited from the explanation of the additives that may be added in the production of the heat-resistant polystyrene-based resin foam layer (A).

[0087] <Non-foamed impact-resistant polystyrene resin film> The thickness of the non-foamed impact-resistant polystyrene resin film may be any appropriate thickness depending on the purpose, as long as the effects of the present invention are not impaired. In consideration of various purposes, the thickness of the impact-resistant polystyrene resin film is preferably 80 μm to 180 μm, more preferably 80 μm to 170 μm, even more preferably 80 μm to 150 μm, and particularly preferably 100 μm to 145 μm. The thickness of the non-foamed impact-resistant polystyrene resin film is preferably smaller than the thickness of the heat-resistant polystyrene resin foam layer (A).

[0088] The non-foamed impact-resistant polystyrene-based resin film is typically formed from a resin composition containing a polystyrene-based resin (III) and a rubber-modified polystyrene-based resin.

[0089] As for the polystyrene resin (III), the same polystyrene resin as the polystyrene resin (I) forming the heat-resistant polystyrene resin foam layer (A) or the polystyrene resin (II) forming other polystyrene resin foam layers can be used within the scope of not impairing the effects of the present invention. The polystyrene resin (III) may be the same as or different from the polystyrene resin (I) or the polystyrene resin (II).

[0090] The polystyrene resin (III) may be of one type only, or of two or more types.

[0091] The rubber-modified polystyrene resin may be one in which the molecule itself is modified, or one in which the resin is modified in a bulk state. Examples of such rubber-modified polystyrene resins include copolymers of one or more styrene monomers and one or more rubber component monomers, and blends of one or more polystyrene resins and one or more rubbers.

[0092] Specific examples of rubber-modified polystyrene resins include so-called high impact polystyrene resin (HIPS) and mixed resins of high impact polystyrene resin (HIPS: high impact polystyrene) and styrene homopolymers such as general purpose polystyrene resin (GPPS).

[0093] When a mixed resin of high impact polystyrene resin (HIPS) and general purpose polystyrene resin (GPPS) is used as the rubber-modified polystyrene resin, it is preferable for the mixed resin to contain 40 mass% or more of high impact polystyrene resin (HIPS) from the viewpoint of imparting impact resistance, etc.

[0094] Any suitable high impact polystyrene resin (HIPS) may be used as the high impact polystyrene resin (HIPS) as long as the effects of the present invention are not impaired. Examples of such high impact polystyrene resin (HIPS) include those in which a styrene-butadiene copolymer is dispersed in a salami structure and the particle size is 0.3 μm to 10 μm. Further, examples of the polystyrene resin (II) forming the polystyrene resin layer include linear low-density polyethylene, high-density polyethylene, low-density polyethylene, propylene homopolymer, ethylene-propylene random polymer, ethylene-propylene block polymer, ethylene-propylene-butene-terpolymer, ethylene-vinyl acetate copolymer, ethylene-unsaturated carboxylic acid ester copolymer (e.g., ethylene-methyl methacrylate copolymer), ethylene-unsaturated carboxylic acid metal salt copolymer (e.g., ethylene-magnesium (or zinc) acrylate copolymer), propylene-vinyl chloride copolymer, propylene-butene copolymer, propylene-maleic anhydride copolymer, propylene-olefin copolymer (propylene-ethylene copolymer, propylene-butene-1 copolymer), unsaturated carboxylic acid (e.g., maleic anhydride) modified polyethylene or polypropylene, ethylene-propylene rubber, atactic polypropylene, polyethylene terephthalate, polybutylene terephthalate, and mixtures thereof.

[0095] <Non-foamed film containing thermoplastic resin> The polystyrene-based resin laminate foam sheet according to the embodiment of the present invention may include a non-foamed film containing a thermoplastic resin on the side opposite to the non-foamed impact-resistant polystyrene-based resin film as viewed from the heat-resistant polystyrene-based resin foam layer (A). Also, the polystyrene-based resin laminate foam sheet according to the embodiment of the present invention may include a non-foamed film containing a thermoplastic resin on the side opposite to the heat-resistant polystyrene-based resin foam layer (A) as viewed from the non-foamed impact-resistant polystyrene-based resin film.

[0096] By laminating a non-foamed film containing a thermoplastic resin, the surface of the polystyrene-based resin laminated foamed sheet according to the embodiment of the present invention becomes more beautiful, the rigidity becomes higher, and the heat resistance and oil resistance are further improved.

[0097] Examples of thermoplastic resins that form the non-foamed film containing a thermoplastic resin include polystyrene resins, impact-resistant polystyrene resins, polyethylene resins, polypropylene resins, polyethylene terephthalate resins, polyphenylene ether resins, polyvinylidene chloride resins, ethylene-vinyl alcohol copolymer resins, etc. These may be used alone or in combination of two or more kinds.

[0098] The non-foamed film containing a thermoplastic resin may be one layer or two or more layers. When it is two or more layers, the layers may be laminated by, for example, dry lamination.

[0099] A coloring agent (pigment, dye, etc.) may be added to the non-foamed film containing a thermoplastic resin. By adding a coloring agent (pigment, dye, etc.), it can be colored in various colors, and various patterns and designs can be displayed by printing on the surface.

[0100] The thickness of the non-foamed film containing a thermoplastic resin may be any appropriate thickness within a range that does not impair the effects of the present invention. Such a thickness is preferably 10 μm to 150 μm, more preferably 10 μm to 100 μm, in terms of being able to more effectively exhibit the effects of the present invention. If the thickness of the non-foamed film containing a thermoplastic resin is too thin outside the above range, the film may be difficult to stretch during thermoforming, and may be prone to defects. If the thickness of the non-foamed film containing a thermoplastic resin is too thick outside the above range, the cost may increase, and the film may not be laminated at a low temperature during lamination, resulting in a loss of gloss.

[0101] <<Polystyrene resin foam container>> The polystyrene-based resin foam container according to the embodiment of the present invention is obtained by thermoforming the polystyrene-based resin foam sheet according to the embodiment of the present invention or the laminated polystyrene-based resin foam sheet according to the embodiment of the present invention.

[0102] In order to manufacture the polystyrene-based resin foam container according to the embodiment of the present invention, the polystyrene-based resin foam sheet according to the embodiment of the present invention or the polystyrene-based resin laminated foam sheet according to the embodiment of the present invention wound into a roll is heated to a constant temperature in the heating zone of a molding machine, and then molded into a desired container shape in the molding zone. The container shape can be various shapes such as a bowl shape, a cup shape, a box shape, a tray shape, etc.

[0103] The polystyrene-based resin foam container according to the embodiment of the present invention is typically formed into a container shape such that the polystyrene-based resin laminated foam sheet according to the embodiment of the present invention is on the inside and the non-foamed polystyrene-based resin film is on the inside, as shown in Fig. 2. In Fig. 2, the container inside of the polystyrene-based resin foam container 1000 is 200 and the container outside is 300.

[0104] The polystyrene-based resin foam container according to the embodiment of the present invention has a foaming agent content of preferably 3.1 mass% or less, more preferably 2.8 mass% or less, even more preferably 2.6 mass% or less, particularly preferably 2.4 mass% or less, and most preferably 2.2 mass% or less. If the foaming agent content in the polystyrene-based resin foam container according to the embodiment of the present invention is within the above range, a polystyrene-based resin foam container is provided that is less likely to develop blisters or tertiary foaming on the surface due to heat. EXAMPLES

[0105] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows.

[0106] <Thickness> Twenty-one arbitrary positions in the width direction (direction perpendicular to the extrusion flow direction) were used as measurement points. These measurement points were measured with a thickness measuring device (manufactured by Techlock Corporation, model: SM-125) to the nearest 0.01 mm. The arithmetic mean of these measurements was used as the thickness.

[0107] <Basic weight> Excluding 20 mm from both ends in the width direction (direction perpendicular to the extrusion flow direction), ten pieces of 10 cm x 10 cm were cut out at equal intervals in the width direction, and the mass (g) of each piece was measured to the nearest 0.001 g. The average mass (g) of each piece was calculated using the formula: 2 The converted value is expressed as the mass per unit weight (g / m 2 ) was decided.

[0108] <Apparent density> 50cm to avoid changing the bubble structure. 3 The sheet was cut out to prepare a test piece, the mass and volume of the test piece were measured, and the overall apparent density was calculated using the following formula: The test piece was cut out from a sheet that was 72 hours or more old (maximum 90 days) after production, and left for 24 hours in an atmospheric condition of 23°C±2°C and 50RH%±5RH%. Apparent density (g / cm 3 ) = mass of test piece (g) ÷ volume of test piece (cm 3 )

[0109] <Surface density> Using a slicer (splitting machine manufactured by Fortuna (Germany), model AB-320-D), the sheet was sliced ​​from the surface to a thickness of 200 μm, and then cut into pieces of 25 mm width and 150 mm length to obtain a surface layer. The mass and volume of the obtained surface layer were measured, and the surface layer density was calculated using the following formula. Note that the surface layer was cut out from a foamed sheet that had been produced for 72 hours or more (maximum 90 days), and left for 24 hours under atmospheric conditions of 23°C ± 2°C and 50 RH% ± 5 RH%. Surface layer density (g / cm 3 ) = mass of surface layer (g) ÷ volume of surface layer (cm 3 )

[0110] <Open cell ratio> The open cell ratio of the foamed layer was measured by the method described in JIS K7138:2006 "Rigid foamed plastics - Determination of open cell ratio and closed cell ratio."

[0111] <Glass transition temperature (Tg)> (Pretreatment) Prior to the measurement of the glass transition temperature, 5 to 6 g of the foamed layer was weighed out on a balance, sandwiched between two polytetrafluoroethylene sheets, and pressed in the following manner to perform a pretreatment for defoaming. Press equipment: Toyo Seiki Co., Ltd., small press equipment "Lab Press 10T" Upper heater temperature: 180℃ Lower heater temperature: 180℃ Pressing process: pressing at 0.54 MPa for 3 minutes, performing 5 cycles of pressing, with one cycle consisting of "pressing at 0.54 MPa for 2 seconds" and "pressure release for 2 seconds", and then pressing at 15.5 MPa for 2 minutes. (Glass transition temperature: Tg) The glass transition temperature (midpoint glass transition temperature) (Tg) of the sample degassed as described above was measured by the method described in JIS K7121:1987 "Method of measuring glass transition temperature of plastics." However, the sampling method and temperature conditions were as follows. A DSC6220 type (manufactured by SII Nano Technology Co., Ltd.) was used as a differential scanning calorimeter, and about 6 mg of sample was filled into the bottom of an aluminum measurement container so that there were no gaps, and the sample was heated from 30°C to 220°C at a heating rate of 20°C / min under a nitrogen gas flow rate of 20 mL / min, held for 10 minutes, quickly removed, and allowed to cool in an environment of 25±10°C. The midpoint glass transition temperature was calculated from the DSC curve obtained when the sample was heated from 30°C to 220°C at a heating rate of 20°C / min (9.3 "How to determine the glass transition temperature"). Alumina was used as the reference material.

[0112] <Average bubble diameter d, average bubble diameter in MD direction dM, average bubble diameter in TD direction dT (mm), average bubble diameter in VD direction dV> A piece was cut from the widthwise center of the original sheet perpendicular to the surface of the original sheet along the MD direction (extrusion flow direction) and TD direction (width direction perpendicular to the MD direction on the surface of the sheet). The cross section was photographed at a magnification of 50x using a scanning electron microscope (SU1510, Hitachi High-Technologies Corporation). The microscopic images were photographed so that the specified magnification would be achieved when two images (four images in total) were printed side by side on a single sheet of A4 paper in landscape orientation. Specifically, 60mm arbitrary straight lines parallel to each of the MD and TD directions and 60mm arbitrary straight lines perpendicular to each direction (VD direction) were drawn on the image, and two microscope images of a total of four fields of view were taken for each of the cross sections cut along the MD direction (MD cross section) and the cross section cut along the TD direction (TD cross section) and printed on A4 paper. Three arbitrary straight lines (60mm long) parallel to the MD direction were drawn on each of the two images of the MD cross section, and three arbitrary straight lines (60mm long) parallel to the TD direction were drawn on each of the two images of the TD cross section. In addition, three straight lines (60mm long) parallel to the VD direction were drawn on one image of the MD cross section and one image of the TD cross section, and six arbitrary straight lines of 60mm long parallel to the MD, TD, and VD directions were drawn in each direction. Note that the arbitrary straight lines were made as far as possible so that bubbles would not come into contact only at the contact points, and if there was contact, the bubbles were also counted. The number of bubbles D counted for six arbitrary straight lines in each of the MD, TD, and VD directions was calculated as the arithmetic mean, which was used as the number of bubbles in each direction. The average chord length t of the bubbles in each direction was calculated from the image magnification at which the number of bubbles was counted and the number of bubbles using the following formula. Average chord length t (mm) = 60 / (number of bubbles x image magnification) (Average chord length in MD direction tM (mm) = 60 / (number of bubbles in MD direction × image magnification)) (Average chord length in TD direction tT (mm) = 60 / (number of bubbles in TD direction × image magnification)) (Average chord length in the VD direction tV (mm) = 60 / (number of bubbles in the VD direction × image magnification)) The image magnification was calculated by measuring the scale bar on the image to the nearest 1 / 100 mm using a Digimatic Caliper (manufactured by Mitutoyo Corporation) and using the following formula: Image magnification = Scale bar actual value (mm) / Scale bar display value (mm) The bubble diameter in each direction was calculated using the following formula. Average bubble diameter in MD direction dM(mm)=tM(mm) / 0.616 Average bubble diameter in TD direction dT(mm)=tT(mm) / 0.616 Average bubble diameter in VD direction dV(mm)=tV(mm) / 0.616 Furthermore, the cube root of the product was determined as the average bubble diameter. Average bubble diameter d(mm)=(dM(mm)×dT(mm)×dV(mm)) (1 / 3)

[0113] <Forming pasta containers> A standard pasta container mold was used, which had 4 pieces in the width direction and 5 pieces in the flow direction, and was shaped to fit an internal fitting lid with a diameter of φ200 and a height of 45 mm. The pasta containers were molded under the conditions of 2 zone heating and 4.5 seconds / shot (total heating time 9 seconds). The heaters on both the top and bottom were set to 280°C.

[0114] <Blister evaluation, tertiary foaming evaluation> Spaghetti Napolitan (contents: approx. 400g) was placed in a pasta container, the container was covered with a special lid, and heated in a microwave oven at 1600W for 91 seconds. After heating, the bottom of the container was evaluated according to the following criteria. (Blister rating) ◎: No blisters were generated ◯: There is almost no blistering and the appearance is within the acceptable range. ×: Blisters were observed and the appearance was poor. (Tertiary foaming evaluation) ⊚: No tertiary foaming occurs. ○: Tertiary foaming is almost nonexistent, and the appearance is within the acceptable range. ×: Tertiary foaming occurred and the appearance was poor.

[0115] <Blowing agent content in container> A test piece of 10-20 mg cut from the bottom of the container was precisely weighed and sealed in a 20 ml dedicated glass vial, set in a Perkins-Elmer headspace sampler "TurboMatrix HS40", heated at 160°C for 20 minutes, and then quantified by the MHE method using a Perkins-Elmer gas chromatograph "Clarus500GC" (detector: FID). When a non-foamed film was included, the concentration was converted to the concentration relative to the foamed sheet to avoid the influence of the mass of the non-foamed film. The measurement conditions for the headspace sampler were a needle temperature of 160° C., a sample introduction time of 0.8 minutes, and a transfer line temperature of 180° C. The measurement conditions for the gas chromatograph were a DB-1 column manufactured by J&W (0.25 mmφ×60 m, film thickness of 1 μm, column temperature: 50° C. for 6 minutes, heated to 270° C. at 40° C. / min, and heated to 270° C. for 1 minute at 270° C.), a carrier gas of helium (introduction conditions: 18 psi for 10 minutes, increased to 24 psi at 0.5 psi / min), an inlet temperature of 200° C., a detector temperature of 250° C., range=20, and Att=1.

[0116] [Examples 1 to 3, Comparative Examples 1 to 5] Using the manufacturing apparatus of FIG. 1, a mixture of polystyrene resin (PS) (product name: XC-515, rubber content: 0 mass%, manufactured by DIC Corporation), a mixture of polyphenylene ether resin (PPE) and PS (product name: Noril EFN4230, PPE / PS=70 / 30 (mass ratio), rubber content: 0 mass%, manufactured by Sabic Corporation) and a foam nucleating agent (product name: DSM1401A, manufactured by Toyo Styrene Co., Ltd.) were mixed according to the composition of Table 1 to obtain a mixture. The above mixture was fed from a hopper to a first extrusion section (screw diameter: 115 mm), heated to a maximum temperature of 315° C., and melt-kneaded to form a molten resin. A foaming agent (a mixture of isobutane:normal butane = 70:30 (mass ratio)) was supplied to the first extrusion section, and the resin melt and the foaming agent were mixed to form a mixture. The amount of the foaming agent was the parts by mass shown in Table 1 relative to 100 parts by mass of the resin. The mixture was fed from the first mixing section to the second mixing section (screw diameter: 180 mm), cooled to 180°C, and extruded through a circular die (diameter: 160 mm) and foamed to obtain a cylindrical foamed sheet. Immediately after being extruded from the circular die, cooling air (30°C) was blown onto the inner and outer surfaces of the cylindrical foamed sheet to cool it. The cooled cylindrical foamed sheet was cut along the extrusion direction to obtain raw sheets of heat-resistant polystyrene-based resin foamed sheets (1) to (3) and (C1) to (C5) shown in Table 1, each having a width of 1,050 mm. For the purpose of replacing the foaming gas, the original rolls of the heat-resistant polystyrene resin foam sheets (1) to (3) and (C1) to (C5) were stored for 14 days after production. A dry laminate film (polystyrene resin film layer / polypropylene resin film layer=30 μm / 40 μm, total: 70 μm) (CPPS) consisting of a polystyrene resin film and a non-oriented polypropylene resin film laminated together was dry laminated on one side of this foam sheet (the surface that will become the inside of the container to be produced), and a PS film (CPS film, thickness 35 μm) was heat laminated on the other side (the surface that will become the outside of the container to be produced) to produce polystyrene-based resin laminated foam sheets (1) to (3), (C1) to (C5). These polystyrene-based resin laminated foam sheets (1) to (3), (C1) to (C5) were used to mold pasta containers, thereby obtaining polystyrene-based resin foam containers (1) to (3), (C1) to (C5). The results are shown in Table 1.

[0117] [Example 4, Comparative Example 6] In Example 4 and Comparative Example 6, the foam layer is made up of two layers, that is, a first foam layer and a second foam layer. As the base polymer for the first foam layer, a mixed resin was prepared by mixing styrene-methacrylic acid copolymer resin (styrene monomer content = 92 mass%, methacrylic acid monomer content = 8 mass%) (product name "T080", manufactured by Toyo Styrene Co., Ltd.) and styrene-butadiene block copolymer resin (SBS: styrene block copolymer) (product name "Tufprene 125", manufactured by Asahi Kasei Chemicals Corporation) in a mass ratio of 92:8 (T080:Tufprene 125). In addition to the base polymer, a master batch (product name "DSM1401M") incorporating talc (air bubble regulator) was also prepared. The amount of the masterbatch was set so as to obtain the average bubble diameter shown in Table 1, and the mixture was blended and charged into a batch-type continuous mixer. After thorough mixing, the mixture was fed into the hopper of the upstream extruder (screw diameter 90 mm) of a tandem extruder having a screw diameter of 90 mm and a screw diameter of 115 mm. In the upstream extruder, the maximum cylinder temperature was set to 280°C, and approximately 2.3 parts by mass of mixed butane (relative to 100 parts by mass of mixed resin) was added as a foaming agent midway, and the mixture was melt-kneaded together with the mixed resin and other ingredients before being supplied to the downstream extruder. The downstream extruder was adapted to supply the molten mixture supplied from the upstream extruder to a joining die at a rate of 120 kg / h. Meanwhile, in another tandem extruder having a screw diameter of 90 mm and a screw diameter of 115 mm, the material for forming the second foam layer was melt-kneaded and supplied to the above-mentioned joining die. As a material for forming the second foam layer, GPPS (product name "HRM12", manufactured by Toyo Styrene Co., Ltd.) was prepared as a base polymer, and a master batch (product name "DSM1401M") containing talc (a bubble regulator) was prepared separately from the base polymer. The amount of the masterbatch was set so as to obtain the average bubble diameter shown in Table 1, and the mixture was blended and charged into a batch-type continuous mixer. After thorough mixing, the mixture was fed into the hopper of the upstream extruder (screw diameter 90 mm) of a tandem extruder having a screw diameter of 90 mm and a screw diameter of 115 mm. In the upstream extruder, the maximum cylinder temperature was set to 260°C, and approximately 2.1 parts by mass of mixed butane (relative to 100 parts by mass of GPPS) was added as a foaming agent midway, melt-kneaded with the above-mentioned GPPS, and supplied to the downstream extruder. The downstream extruder was adapted to supply the molten mixture supplied from the upstream extruder to a joining die at a rate of 120 kg / h. The two kinds of melt kneaded materials fed to the joining die were joined and laminated in the joining die, and the foamed mixture was fed to an annular die with a diameter of 175 mm and a slit clearance of 0.5 mm, and passed through the slit of the die to form a cylindrical foam. Immediately after that, the cylindrical foam was cooled by blowing air (30°C) and was taken along the outer surface of a cooling device (mandrel) with a diameter of 675 mm, and was further cut into two pieces along the extrusion direction to obtain raw sheets of heat-resistant polystyrene resin foam sheets (4) and (C6) with a width of 1050 mm as shown in Table 1. For the purpose of replacing the foaming gas, the original rolls of the heat-resistant polystyrene resin foam sheets (4) and (C6) were stored for 14 days after production. A CPS film (thickness 20 μm) was laminated on the second foam layer of the original roll of the heat-resistant polystyrene resin foam sheet (4), (C6). Then, 100 parts by mass of high impact polystyrene resin (product name "E-641", manufactured by Toyo Styrene Co., Ltd.) was melted in a 120 mm diameter extruder set at a maximum temperature of 240°C as the impact-resistant polystyrene resin film to be laminated, extruded into a film form from a T-die, and laminated to a thickness of 100 μm on the first foam layer side of the original roll of the heat-resistant polystyrene resin foam sheet (4), (C6) before it was completely cooled. Immediately after that, a film "CPP / PS 45 μm plain" in which a CPP film (thickness 25 μm) and a CPS film (thickness 20 μm) were laminated by dry lamination was laminated to produce a polystyrene resin laminated foam sheet (4), (C6). The polystyrene-based resin laminated foam sheets (4) and (C6) were used to mold pasta containers, to obtain polystyrene-based resin foam containers (4) and (C6). The results are shown in Table 1.

[0118] [Table 1] [Industrial Applicability]

[0119] The polystyrene-based resin foamed sheet according to the embodiment of the present invention or a container obtained by thermoforming the laminated polystyrene-based resin foamed sheet according to the embodiment of the present invention can be widely used as various containers such as trays, lunch boxes, rice bowls, cups, etc. in convenience stores and the like, and can be suitably used, for example, as microwaveable containers. [Explanation of symbols]

[0120] 1 Manufacturing equipment 2. Heat-resistant polystyrene resin foam layer (A) 2a Foam sheet 4. Roll-shaped heat-resistant polystyrene resin foam layer (A) 10 Extruder 11 First extrusion section 12 Second extrusion section 14 Hopper 16 Piping 18 Blowing Agent Source 20 Circular Die 30 Mandrel 32 Cutter 40 Winder 42 Guide Roll 44 Guide Roll 1000 Foam Containers 200 Inside the container 300 Outside the container

Claims

1. A polystyrene-based resin foam sheet comprising a heat-resistant polystyrene-based resin foam layer (A), The heat-resistant polystyrene-based resin foam layer (A) is obtained by extrusion foaming a resin composition containing a polystyrene-based resin (I) and a foaming agent, the content of the foaming agent is 0.5 parts by mass to 3.5 parts by mass based on 100 parts by mass of the polystyrene-based resin (I); The polystyrene resin (I) contains a heat-resistant polystyrene resin (i) having a Vicat softening temperature of 110° C. or higher, The expansion ratio of the heat-resistant polystyrene-based resin foam layer (A) is 13 times or less, The extrusion flow direction of the polystyrene-based resin foamed sheet is defined as the MD direction, the width direction perpendicular to the MD direction on the surface of the polystyrene-based resin foamed sheet is defined as the TD direction, and the thickness direction perpendicular to both the MD direction and the TD direction is defined as the VD direction, When the average cell diameter in the MD direction of the bubbles in the heat-resistant polystyrene-based resin foam layer (A) is dM (mm), the average cell diameter in the TD direction is dT (mm), and the average cell diameter in the VD direction is dV (mm), the heat-resistant polystyrene-based resin foam layer (A) satisfies formulas (1) and (2) and also satisfies formula (3) or formula (4). Polystyrene resin foam sheet. 0≦(dM-dV) / dM<0.6...(1) 0≦(dT-dV) / dT<0.6...(2) 0≦(dM−dT) / dM<0.2 (where dM≧dT) ... (3) 0<(dT-dM) / dT<0.2 (where dT>dM) ... (4)

2. The polystyrene resin foam sheet according to claim 1, having a thickness of 0.5 mm to 4.0 mm.

3. Basis weight 80g / m 2 Up to 400 g / m 2 The polystyrene-based resin foam sheet according to claim 1 or 2,

4. The apparent density of the heat-resistant polystyrene-based resin foam layer (A) is 0.05 g / cm 3 ~0.30g / cm 3 The polystyrene resin foamed sheet according to any one of claims 1 to 3,

5. The polystyrene-based resin foam sheet according to any one of claims 1 to 4, wherein the heat-resistant polystyrene-based resin foam layer (A) has an average cell diameter of 0.05 mm to 0.50 mm.

6. A laminated polystyrene resin foam sheet, comprising the polystyrene resin foam sheet according to any one of claims 1 to 5 and a non-foamed resin film laminated thereon.

7. A polystyrene-based resin foam container, which is thermoformed from the polystyrene-based resin foam sheet according to any one of claims 1 to 5 or the laminated polystyrene-based resin foam sheet according to claim 6.

8. The polystyrene-based resin foam container according to claim 7, wherein the foaming agent content is 3.1% by mass or less.

Citation Information

Patent Citations

  • Heat resistant resin foam sheet and container

    JP2014205761A

  • Styrenic resin composition for foaming, styrenic resin foam sheet, method for manufacturing the same, and food packaging container

    JP2014227459A

  • Styrene resin composition for foaming, styrene resin foam sheet, method for manufacturing the same, and food packaging container

    JP2016113580A

  • Method for producing polystyrene-based resin foam sheet, polystyrene-based resin foam sheet, polystyrene-based resin foam sheet roll material, and container for microwave heating

    JP2019210312A

  • Styrenic resin composition for extrusion foaming, foam sheet, container, and tabular foam

    JP2019210439A