Material for 3D modeling, 3D model, and method for manufacturing 3D model

A 3D printing material with thermoplastic resin, elastomer, and filler addresses warping issues by controlling thermal expansion and layer adhesion, enhancing the accuracy and integrity of printed structures.

JP7586828B2Active Publication Date: 2024-11-19MITSUI CHEMICALS INC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021548932
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-13
Filing Date
2020-09-23
Publication Date
2024-11-19
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

Conventional material extrusion methods for 3D printing using thermoplastic resin result in deformation, particularly warping, of three-dimensional objects due to heat shrinkage, leading to inaccurate models.

Method used

A three-dimensional modeling material comprising thermoplastic resin, thermoplastic elastomer, and filler, such as talc, with specific mass content ratios, is used to suppress deformation by controlling thermal expansion and adhesion between layers.

Benefits of technology

The proposed material effectively reduces warpage and maintains structural integrity of 3D printed objects, ensuring higher accuracy and fidelity to the original design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586828000007
    Figure 0007586828000007
  • Figure 0007586828000008
    Figure 0007586828000008
  • Figure 0007586828000001
    Figure 0007586828000001
Patent Text Reader

Abstract

A three-dimensional modeling material that includes a thermoplastic resin, a thermoplastic elastomer, and a filler. The filler includes talc. The filler is 5–70 mass% of the total mass of the three-dimensional modeling material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a material for three-dimensional modeling, a three-dimensional model, and a method for manufacturing a three-dimensional model. [Background technology]

[0002] In recent years, a method of forming a three-dimensional object using a manufacturing device for three-dimensional modeling has been attracting attention as one of the efficient modeling techniques. To form a three-dimensional object, three-dimensional coordinate data of the three-dimensional object (hereinafter referred to as "3D data") is required. Slicer software slices the 3D data into slices to generate multiple pieces of two-dimensional data. The manufacturing device for three-dimensional modeling sequentially stacks two-dimensional layers based on the multiple pieces of two-dimensional data. In this way, a three-dimensional object is formed (see, for example, Patent Document 1).

[0003] Methods for forming 3D objects include the material extrusion (MEX) method, photolithography, inkjet method, powder adhesion modeling method, powder sintering modeling method, etc. Among these methods, the material extrusion method is attracting particular attention because it allows for a wide range of material selection.

[0004] The material extrusion method is a method for forming a three-dimensional object by extruding a thermoplastic resin melted by heat from a nozzle and laminating the resin. Patent Document 2 discloses a method for forming a three-dimensional object by the material extrusion method.

[0005] Patent Document 1: JP 2017-189885 A Patent Document 2: International Publication No. 2015 / 129733 Summary of the Invention [Problem to be solved by the invention]

[0006] However, conventional methods for forming 3D objects using the material extrusion method use thermoplastic resin alone as the forming material. Therefore, when the molten thermoplastic resin extruded from the nozzle solidifies into a 3D object, there is a risk that the 3D object may be deformed due to effects such as thermal contraction. Deformation of the 3D object includes warping of the 3D object. As a result, it was sometimes difficult to obtain a 3D object with high accuracy.

[0007] The present disclosure has been made in consideration of the above circumstances. An object of the present disclosure is to provide a material for three-dimensional printing that suppresses deformation (particularly warpage) of a three-dimensional object. A problem to be solved by another embodiment of the present disclosure is to provide a three-dimensional object in which deformation (particularly warpage) is suppressed, and a manufacturing method thereof. [Means for solving the problem]

[0008] Specific means for solving the problems include the following aspects.

[0009] <1> The composite material includes a thermoplastic resin, a thermoplastic elastomer, and a filler, The filler comprises talc; A material for three-dimensional printing, wherein the content of the filler is 5% by mass or more and 70% by mass or less, based on the total mass of the material for three-dimensional printing. <2> The content of the thermoplastic resin is 0.1% by mass or more and less than 100% by mass with respect to the total mass of the material for three-dimensional modeling. <1> The three-dimensional modeling material according to claim 1. <3> The content of the thermoplastic elastomer is 10% by mass or more and less than 100% by mass with respect to the total mass of the material for three-dimensional modeling. <1> or <2> The three-dimensional modeling material according to claim 1. <4> The thermoplastic resin includes a propylene-based polymer. <1> ~ <3> 3. The three-dimensional modeling material according to claim 1 . <5> When molded into a hot-pressed product for measurement, the hot-pressed product for measurement has a tensile modulus X (MPa) according to JIS K7161-2:2014 that satisfies the following formula (I): The average warpage Y (mm) of the honeycomb structure for measurement when laminated to the honeycomb structure for measurement satisfies the following formula (IIa), The hot-pressed product for measurement is a 1BA type test piece defined in JIS K7161-2:2014 obtained by hot-press molding the material for three-dimensional modeling, The honeycomb object for measurement is A rectangular parallelepiped frame part measuring 250 mm x 100 mm x 15 mm in height obtained by layering the three-dimensional modeling material by a material extrusion method so that a filling rate, which indicates the ratio of the volume of the three-dimensional modeling material to a unit space volume, is 100%; and and a honeycomb structure portion obtained by layer-forming the three-dimensional modeling material by the material extrusion method in the rectangular parallelepiped frame portion so that the filling rate is 30%, The average warpage amount Y indicates an arithmetic average value of the amount of lift of the four corners of the rectangular parallelepiped frame part from a surface plate when the honeycomb structure for measurement is placed on the surface plate. <1> ~ <4> 3. The three-dimensional modeling material according to claim 1 . Formula (I) 50≦X≦4000 Formula (IIa) 0≦Y≦6.0 <6> The content of the thermoplastic elastomer is 10% by mass or more and less than 70% by mass with respect to the total mass of the material for three-dimensional modeling, The content of the filler is 10% by mass or more and less than 50% by mass with respect to the total mass of the material for three-dimensional modeling, The total content of the thermoplastic elastomer and the filler is 20% by mass or more and less than 90% by mass with respect to the total mass of the material for three-dimensional modeling. <1> ~ <5> 3. The material for three-dimensional modeling according to any one of claims 1 to 2. <7> The breaking stress α [MPa] of the measurement object in a tensile test in accordance with JIS K7161-2:2014 when additively manufactured into the measurement object satisfies the following formula (III), The average warpage Y [mm] of the honeycomb structure for measurement when laminated to the honeycomb structure for measurement satisfies the following formula (IIb), The measurement object is a 1BA type test piece defined in JIS K7161-2:2014, which is obtained by additively manufacturing the material for three-dimensional printing by a material extrusion method and machining it so that the filling rate, which indicates the ratio of the volume of the material for three-dimensional printing to the unit space volume, is 100% and the stacking direction of the material for three-dimensional printing is parallel to the tensile direction of the measurement object in the tensile test, The honeycomb object for measurement is A rectangular parallelepiped frame part of 250 mm x 100 mm x 15 mm height obtained by layering the three-dimensional modeling material by the material extrusion method so that the filling rate was 100%. and a honeycomb structure portion obtained by layer-forming the three-dimensional modeling material by the material extrusion method in the rectangular parallelepiped frame portion so that the filling rate is 30%, The average warpage amount Y indicates an arithmetic average value of the amount of lift of the four corners of the rectangular parallelepiped frame part from a surface plate when the honeycomb structure for measurement is placed on the surface plate. <1> ~ <6> 3. The three-dimensional modeling material according to claim 1 . Formula (III) 6.5 ≦ α < 200 Formula (IIb) 0≦ Y ≦ 4.0 <8> <1> ~ <7> A melting step of melting the material for three-dimensional modeling according to any one of the above items; a modeling step of extruding the molten material for three-dimensional modeling from a nozzle of a three-dimensional object manufacturing device to form a three-dimensional object; A method for manufacturing a three-dimensional object having the above structure. <9> <1> ~ <7> 2. A three-dimensional object made from the material for three-dimensional modeling according to claim 1 . Effect of the Invention

[0010] According to one embodiment of the present disclosure, there is provided a material for three-dimensional printing that suppresses deformation (particularly warpage) of a three-dimensional object. According to another embodiment of the present disclosure, there is provided a three-dimensional object in which deformation (particularly warpage) is suppressed, and a method for manufacturing the same. [Brief description of the drawings]

[0011] [Figure 1] 1 is a perspective photograph showing a honeycomb object for measurement. [Diagram 2] FIG. 13 is a side view of a measurement honeycomb shaped object for explaining an average amount of warpage Y. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0013] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0014] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.

[0015] ≪3D modeling materials≫ The material for three-dimensional modeling of the present disclosure is a feedstock supplied to the modeling process of a three-dimensional object. The three-dimensional modeling material of the present disclosure includes a thermoplastic resin, a thermoplastic elastomer, and a filler. The filler includes talc. The content of the filler is 5% by mass or more and 70% by mass or less with respect to the total mass of the three-dimensional modeling material. Therefore, deformation such as warping of a three-dimensional object obtained by modeling using the three-dimensional modeling material of the present disclosure is suppressed.

[0016] (filling material) The three-dimensional modeling material of the present disclosure includes a filler.

[0017] 〔talc〕 The filler includes talc. Talc does not change in volume at the modeling temperature, and the thermal expansion coefficient of talc is lower than the thermal expansion coefficients of thermoplastic resin and thermoplastic elastomer, so deformation (particularly warping) of the three-dimensional object is suppressed. When the three-dimensional object is modeled by a material extrusion method, the modeling temperature refers to the nozzle temperature of the three-dimensional object manufacturing device. The fact that talc does not change in volume at the modeling temperature means that the talc does not melt, does not dissolve, and does not undergo phase transition at the modeling temperature.

[0018] Talc is also known as talc. Talc is hydrated magnesium silicate. Hydrated magnesium silicate is a type of layered clay mineral, and is composed of magnesium (Mg) and silicon (Si) combined with oxygen and hydroxyl groups. The chemical structure of talc is generally: [Mg3Si4O 10 (OH)2] or [3MgO 4SiO2 H2O].

[0019] The shape of the talc is not particularly limited, and is preferably, for example, scaly, elliptical, or the like.

[0020] The upper limit of the volume average particle diameter of the talc is preferably 30 μm or less, more preferably 10 μm or less.The lower limit of the volume average particle diameter of the talc is preferably 1 μm or more, more preferably 5 μm or more.

[0021] The volume average particle size of talc is defined as the particle size value at which the cumulative volume of each particle, measured while talc is dispersed in water using a particle size distribution measuring device such as a laser diffraction / scattering type particle size distribution measuring device, is 50% of the total volume when the volume of each particle is cumulatively calculated from the smallest particle size side based on the particle size of each particle.

[0022] The content of talc is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on 100% by mass of the total amount of the filler.

[0023] In addition to talc, the filler may include inorganic fillers, organic fillers, glittering powders, pigment powders, composite fillers thereof, etc. The fillers may be used alone or in combination of two or more kinds.

[0024] The filler may include an inorganic filler. For example, examples of inorganic fillers include inorganic powders other than talc (hereinafter simply referred to as "inorganic powders"), glittering inorganic powders, composite inorganic powders, and inorganic fibers. Examples of inorganic powders include titanium oxide, black titanium oxide, konjou, ultramarine, red iron oxide, yellow iron oxide, black iron oxide, zinc oxide, aluminum oxide, silica, magnesium oxide, zirconium oxide, magnesium carbonate, calcium carbonate, chromium oxide, chromium hydroxide, carbon black, aluminum silicate, magnesium silicate, aluminum magnesium silicate, mica, synthetic mica iron, sericite, moss-hige (magnesium sulfate whiskers), kaolin, silicon carbide, barium sulfate, bentonite, smectite, and boron nitride. Examples of the shiny inorganic powder include bismuth oxychloride, titanium oxide-coated mica, iron oxide-coated mica, iron oxide-coated mica titanium, iron oxide-titanium oxide sintered body, and aluminum powder. Examples of the composite inorganic powder include fine particle titanium oxide-coated mica titanium, fine particle zinc oxide-coated mica titanium, barium sulfate-coated mica titanium, titanium oxide-containing silica, and zinc oxide-containing silica. The inorganic fibers include glass fibers. Among the above, the inorganic filler preferably contains at least one of inorganic powder and inorganic fiber, from the viewpoint of further suppressing deformation (particularly warpage) of the three-dimensionally shaped object.

[0025] The inorganic filler may contain both talc and glass fiber from the viewpoint of increasing the tensile modulus of elasticity of the three-dimensional object and smoothing the appearance of the three-dimensional object. In this case, the content ratio (Talc:Fiber) of the talc (Talc) and the glass fiber (Fiber) is preferably 90:10 to 40:60, more preferably 85:15 to 45:55, by mass. In particular, when the content ratio (Talc:Fiber) is 85:15 or more, fluffing of the surface of the three-dimensional object tends to be further suppressed. The occurrence of fluffing of the surface of the three-dimensional object is a problem specific to three-dimensional printing materials including not only glass fiber but also fibrous materials such as carbon fiber.

[0026] The filler may include an organic filler. For example, the organic filler may be resin particles, pulp, or the like. Examples of the resin particles include carbon fiber, polyethylene, polypropylene, polystyrene, tetrafluoroethylene, silicone powder, and polyphenylene ether. Examples of pulp include cellulose and cellulose derivatives.

[0027] The shape of the filler may be any of spherical, plate-like, and needle-like. The filler may be porous or non-porous.

[0028] In order to further suppress deformation (particularly warping) of the three-dimensional object, the content of the filler is from 5% by mass to 70% by mass or less, preferably from more than 5% by mass to 55% by mass or less, and more preferably from more than 5% by mass to 45% by mass or less, relative to the total mass of the material for three-dimensional modeling. If the content of the filler is 5% by mass or more and 70% by mass or less, deformation (particularly warping) of the three-dimensional object is suppressed.

[0029] (thermoplastic resin) The three-dimensional modeling material of the present disclosure includes a thermoplastic resin. In this disclosure, the tensile modulus of a thermoplastic resin at 25° C. is 6.0×108 Pa or more. The thermoplastic resin is not particularly limited, and any known thermoplastic resin can be used. The thermoplastic resin may be used alone or in combination of two or more kinds. For example, thermoplastic resins include general-purpose plastics, engineering plastics, and super engineering plastics. Examples of general-purpose plastics include high-density polyethylene (HDPE), low-density polyethylene (LDPE), propylene-based polymers (propylene homopolymer (PP)), polyvinyl chloride (PVC), polyvinylidene chloride, polystyrene (PS), polyvinyl acetate (PVAc), polytetrafluoroethylene (PTFE), acrylonitrile butadiene styrene resin (ABS resin), styrene-acrylonitrile copolymer (AS resin), and acrylic resin (PMMA, etc.). Engineering plastics include polyamide (PA), polyacetal (POM), polycarbonate (PC), modified polyphenylene ether (m-PPE, modified PPE, PPO), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), syndiotactic polystyrene (SPS), and cyclic polyolefin (COP). Examples of super engineering plastics include polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), polyetheretherketone (PEEK), thermoplastic polyimide (PI), and polyamideimide (PAI). Among them, the thermoplastic resin preferably contains one or more selected from the group consisting of high density polyethylene (HDPE), propylene-based polymer, polyamide (PA), polybutylene terephthalate (PBT), syndiotactic polystyrene (SPS), polyphenylene sulfide (PPS) and polyacetal (POM), and more preferably contains a propylene-based polymer.

[0030] The thermoplastic resin may be a crystalline thermoplastic resin or an amorphous thermoplastic resin. For example, from the viewpoint of affinity with the thermoplastic elastomer and the viewpoint of suitably dispersing the filler in the thermoplastic resin, the thermoplastic resin preferably contains a crystalline thermoplastic resin, more preferably contains at least one selected from the group consisting of high density polyethylene (HDPE), propylene-based polymer, polyamide (PA), polybutylene terephthalate (PBT), syndiotactic polystyrene (SPS), polyphenylene sulfide (PPS) and polyacetal (POM), and further preferably contains a crystalline propylene-based polymer. The "crystalline" of a thermoplastic resin refers to having an endothermic peak in differential scanning calorimetry. On the other hand, the "amorphous" of a thermoplastic resin refers to no clear endothermic peak being observed in differential scanning calorimetry.

[0031] The propylene polymer is a polymer having at least propylene as a constituent unit. The propylene-based polymer may be a homopolymer of propylene or a copolymer of propylene and another monomer. When the propylene-based polymer is a copolymer, for example, a copolymer of propylene and an α-olefin having 2 to 20 carbon atoms (excluding propylene) can be mentioned. For example, the copolymer of propylene and an α-olefin having 2 to 20 carbon atoms can be propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-ethylene-1-butene copolymer, propylene-4-methyl-1-pentene copolymer, mixtures thereof, etc.

[0032] When the propylene-based polymer is a copolymer, the propylene-based polymer may be any one of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer.

[0033] When the propylene-based polymer is a copolymer, the ratio of the structural units derived from propylene in the propylene-based polymer may be appropriately designed according to the desired properties of the three-dimensional object. For example, the ratio of the structural units derived from propylene in the propylene-based polymer is preferably 50 mol% or more, more preferably 70 mol% to 99.5 mol%, and even more preferably 80 mol% to 98 mol%, relative to 100 mol% of all structural units in the propylene-based polymer.

[0034] The stereoregularity of the propylene polymer may be any of isotactic, syndiotactic and a mixture thereof.

[0035] The content of the propylene-based polymer is preferably 95.0% by mass or more, more preferably 98.0% by mass or more, and even more preferably 99.9% by mass or more, based on 100% by mass of the total amount of the thermoplastic resin.

[0036] The crystallization temperature (Tc) of the thermoplastic resin is preferably from 90°C to 140°C, and more preferably from 110°C to 130°C. The crystallization temperature of a thermoplastic resin is measured by a differential scanning calorimeter (DSC) at a temperature drop rate of 10° C. / min.

[0037] The crystallinity of the thermoplastic resin is preferably from 2% to 80%, and more preferably from 5% to 75%. The degree of crystallinity of a thermoplastic resin is calculated from the heat of fusion resulting from the melting of the main component in the heat flow curve obtained using a differential scanning calorimeter (DSC). The heat flow curve is obtained by holding the thermoplastic resin at -40°C for 5 minutes under a nitrogen atmosphere, and then raising the temperature at 10°C / min. Specifically, a differential scanning calorimeter (Perkin-Elmer, DSC-7) is used to obtain a heat flow curve by holding 5 mg of a sample at -40°C for 5 minutes under a nitrogen atmosphere, and then raising the temperature at 10°C / min. The heat of fusion is calculated from the heat of fusion resulting from the melting of the main component in the obtained heat flow curve using the following formula. Crystallinity = (ΔH / ΔH0)×100(%) In the formula, ΔH is the heat of fusion (J / g) calculated from the heat of fusion curve derived from the melting of the main component of the thermoplastic resin, and ΔH0 is the heat of fusion (J / g) of perfect crystallization of the main component. For example, when the main component is ethylene, ΔH0 is 293 J / g, and when the main component is propylene, ΔH0 is 210 J / g.

[0038] The melting point of the thermoplastic resin is preferably 90°C or higher, more preferably 110°C or higher and 200°C or lower, and even more preferably 110°C or higher and 180°C or lower.

[0039] The melting point can be measured in the same manner as in the measurement of the melting point of a thermoplastic elastomer described below.

[0040] From the viewpoint of further suppressing deformation (particularly warping) of the three-dimensional object, the content of the thermoplastic resin can be in the range of 0.1 mass % or more and less than 100 mass % relative to the total mass of the material for three-dimensional printing, more preferably in the range of 10 mass % to 70 mass %, and even more preferably in the range of 20 mass % to 60 mass %.

[0041] (Thermoplastic elastomer) The three-dimensional modeling material of the present disclosure includes a thermoplastic elastomer. When the three-dimensional modeling material contains a thermoplastic elastomer, deformation of the three-dimensional model is effectively suppressed.

[0042] Thermoplastic elastomers have rubber-like elasticity. Rubber-like elasticity refers to the property that when a load is applied to a resin, the shape of the resin changes, and when the load is removed, the shape of the resin returns to its original shape. Specifically, a thermoplastic elastomer has a tensile modulus of elasticity of 6.0×10 at 25°C. 8 It refers to a thermoplastic resin having a modulus of elasticity of less than Pa. In this respect, a thermoplastic elastomer is distinguished from a thermoplastic resin.

[0043] The thermoplastic elastomer is preferably a copolymer containing structural units derived from an α-olefin and structural units derived from an olefin different from the α-olefin.

[0044] The α-olefin may generally contain one kind of α-olefin having 2 to 20 carbon atoms alone or two or more kinds of α-olefins in combination. Among them, the α-olefin is preferably an α-olefin having 3 or more carbon atoms, and more preferably an α-olefin having 3 to 8 carbon atoms.

[0045] Examples of the α-olefin include 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 4-methyl-1-pentene, 1-octene, etc. One or more of the α-olefins are used. Among these, from the viewpoint of availability, 1-butene, 1-pentene, 1-hexene, and 4-methyl-1-pentene are preferred as the α-olefin.

[0046] The olefin other than the α-olefin is preferably an olefin having 2 to 4 carbon atoms, and examples of the olefin include ethylene, propylene, butene, etc. Among them, the olefin other than the α-olefin is more preferably an olefin having 2 to 3 carbon atoms.

[0047] Examples of copolymers that are thermoplastic elastomers include ethylene-α-olefin copolymers, propylene-α-olefin copolymers, and butene-α-olefin copolymers.

[0048] Examples of thermoplastic elastomers include ethylene-propylene copolymers (EPR), ethylene-1-butene copolymers (EBR), ethylene-1-pentene copolymers, ethylene-1-octene copolymers (EOR), propylene-1-butene copolymers (PBR), propylene-1-pentene copolymers, and propylene-1-octene copolymers (POR).

[0049] Among these, the thermoplastic elastomer is preferably a copolymer containing a structural unit derived from an α-olefin having 2 to 8 carbon atoms and a structural unit derived from an olefin having 2 to 3 carbon atoms. Propylene-based elastomers are preferred because they have excellent compatibility with thermoplastic resins (particularly propylene-based polymers) and further suppress deformation of three-dimensionally shaped objects.

[0050] Furthermore, the α-olefins may form random copolymers or block copolymers.

[0051] The melting point of the thermoplastic elastomer is preferably from 30°C to 120°C. When the melting point is between 30°C and 120°C, the thermoplastic elastomer acts as an adhesive between the modeling layers of a three-dimensional object modeled by the material extrusion method. This improves the adhesive strength between the modeling layers of a three-dimensional object modeled by the material extrusion method. In the material extrusion method, the modeling layers are made of the three-dimensional modeling material extruded from the nozzle.

[0052] The melting point is a value determined as the temperature Tm at the melting peak position appearing on an endothermic curve by differential scanning calorimetry (DSC). The melting point is determined from the endothermic curve obtained by placing a sample in an aluminum pan, heating it to 230°C at 100°C / min, holding it at 230°C for 5 minutes, lowering it to -70°C at -10°C / min, and then heating it again at 10°C / min.

[0053] The lower limit of the melt flow rate (MFR; 230° C., 2.16 kg load) of the thermoplastic elastomer is preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, further preferably 2 g / 10 min or more, and particularly preferably 5 g / 10 min. The upper limit of the melt flow rate (MFR; 230° C., 2.16 kg load) of the thermoplastic elastomer is preferably 70 g / 10 min or less, more preferably 35 g / 10 min or less, and further preferably 30 g / 10 min or less. When the upper and lower limits of the MFR of the thermoplastic elastomer are within the above ranges, deformation of the three-dimensional object can be more effectively suppressed.

[0054] The melt flow rate (MFR) is a value measured in accordance with ASTM D1238-65T under conditions of 230° C. and a load of 2.16 kg.

[0055] The thermoplastic elastomer is preferably a thermoplastic elastomer having a Shore A hardness of 50-99, or a thermoplastic elastomer having a Shore D hardness of 30-60. When the hardness of the thermoplastic elastomer is 50 or more in Shore A hardness or 30 or more in Shore D hardness, the thermoplastic elastomer is less likely to deform. In other words, the shape of the thermoplastic elastomer is more likely to be maintained. Therefore, when a three-dimensional object is formed using a three-dimensional object manufacturing device described later, the thermoplastic elastomer is more likely to enter the screw of the cylinder. As a result, the discharge efficiency of the molten three-dimensional object material is improved. This makes it easier to obtain a three-dimensional object with a smooth surface and excellent appearance. For the same reasons as above, the lower limit of the hardness is preferably a Shore A hardness of 55 or more or a Shore D hardness of 40 or more, and more preferably a Shore A hardness of 60 or more or a Shore D hardness of 50 or more. There is no particular restriction on the upper limit of the hardness, and it is preferably a Shore A hardness of 96 or less or a Shore D hardness of 60 or less. Among the above, for the same reasons as above, the lower limit of the hardness is more preferably a Shore D hardness of 40 or more, and even more preferably a Shore D hardness of 50 or more.

[0056] The Shore A hardness and Shore D hardness are values ​​measured in accordance with the method described in ASTM D2240.

[0057] Specific examples of thermoplastic elastomers include the TAFMER (registered trademark) series manufactured by Mitsui Chemicals, Inc. (e.g., TAFMER DF605, TAFMER DF610, TAFMER DF640, TAFMER DF710, TAFMER DF740, TAFMER DF7350, TAFMER DF810, TAFMER DF840, TAFMER DF8200, TAFMER DF940, TAFMER DF9200, TAFMER DF110, TAFMER H-0530S ... Examples of such polyimide resins include TAFMER H-1030S, TAFMER H-5030S, TAFMER XM-7070, TAFMER XM-7080, TAFMER XM-7090, TAFMER BL2491M, TAFMER BL2481M, TAFMER BL3110M, TAFMER BL3450M, TAFMER MA8510, TAFMER MH7010, TAFMER MH7020, TAFMER MH5020, TAFMER PN-2070, and TAFMER PN-3560. Among the above, the Toughmer XM series, which is a propylene-based elastomer, is preferred because it has excellent compatibility with thermoplastic resins (particularly propylene-based polymers) and further suppresses deformation of three-dimensional objects. The Toughmer XM series has excellent compatibility with thermoplastic resins (especially propylene-based polymers) and can maintain the breaking stress α required for 3D objects. This improves the adhesive strength between the layers of 3D objects created by the material extrusion method.

[0058] The thermoplastic elastomer is preferably a propylene-based elastomer. The propylene-based elastomer is a thermoplastic elastomer having at least propylene as a constituent unit. The thermoplastic elastomer is preferably a propylene-based elastomer having a melting point of 80° C. to 120° C., a Shore D hardness of 40 to 60, and an MFR of 2 g / 10 min to 20 g / 10 min, so that the three-dimensional object has smaller stress distortion and is less prone to warping. An example of a propylene-based elastomer having a melting point of 80° C. to 120° C., a Shore D hardness of 40 to 60, and an MFR of 2 g / 10 min to 20 g / 10 min is Toughmer XM-7090.

[0059] The content of the thermoplastic elastomer is preferably in the range of more than 0.1% by mass and less than 100% by mass, more preferably in the range of 10% by mass or more and less than 100% by mass, even more preferably in the range of 10% by mass to 70% by mass, and particularly preferably in the range of 20% by mass to 50% by mass, relative to the total mass of the material for 3D modeling.

[0060] It is preferable that the three-dimensional modeling material satisfies the following (a1), (b1), and (c1). (a1) The content of thermoplastic elastomer is 10% by mass or more and less than 70% by mass of the total mass of the material for 3D modeling. (b1) The content of the filler is 10% by mass or more and less than 50% by mass of the total mass of the material for 3D modeling. (c1) The total content of the thermoplastic elastomer and the filler is 20% by mass or more and less than 90% by mass of the total mass of the material for 3D modeling.

[0061] It is more preferable that the three-dimensional modeling material satisfies any one of the following (a2), (b2), and (c2). A three-dimensional object formed using a material for three-dimensional printing that satisfies any one of the following (a2), (b2), and (c2) has smaller stress distortion, is less likely to break, and is less likely to warp. (a2) The content of thermoplastic elastomer is 15% by mass or more and 25% by mass or less, and the content of filler is 35% by mass or more and 45% by mass or less, based on the total mass of the material for three-dimensional modeling. (b2) The content of thermoplastic elastomer is 25% by mass or more and 35% by mass or less, and the content of filler is 15% by mass or more and 45% by mass or less, based on the total mass of the material for 3D modeling. (c2) The content of thermoplastic elastomer is 35% by mass or more and 45% by mass or less, and the content of filler is 15% by mass or more and 35% by mass or less, based on the total mass of the material for 3D modeling.

[0062] Of the above (a2), (b2), and (c2), the three-dimensional modeling material more preferably satisfies any one of the following (a3) ​​and (b3). A three-dimensional object made using a material for three-dimensional printing that satisfies either one of the following (a3) ​​and (b3) has even smaller stress distortion and can more faithfully materialize 3D data. (a3) The content of thermoplastic elastomer is 25% by mass or more and 35% by mass or less, and the content of filler is 25% by mass or more and 35% by mass or less, based on the total mass of the material for three-dimensional modeling. (b3) The content of thermoplastic elastomer is 35% by mass or more and 45% by mass or less, and the content of filler is 15% by mass or more and 35% by mass or less, based on the total mass of the material for 3D modeling.

[0063] (Properties of materials for 3D modeling) From the viewpoint of further suppressing deformation (particularly warping) of the three-dimensional object, the melting point of the material for three-dimensional modeling is preferably 90°C or higher, more preferably 110°C or higher and 200°C or lower, and even more preferably 110°C or higher and 180°C or lower.

[0064] There are no particular limitations on the method for setting the melting point of the three-dimensional modeling material within the above range. For example, the method may involve setting the type of filler, thermoplastic resin, or thermoplastic elastomer to the types described below.

[0065] The three-dimensional modeling material of the present disclosure, for example, has a tensile modulus X (MPa) that satisfies the following formula (I), and when formed into a three-dimensional rectangular parallelepiped object with dimensions of 250 mm × 100 mm × height 15 mm and a full honeycomb filling rate of 30%, it is preferable that the average warpage Y (mm) satisfies formula (IIa), and it is more preferable that the material satisfies the following formula (I) and the average warpage Y (mm) satisfies formula (IIb). Formula (I) 50≦X≦4000 Formula (IIa) 0≦Y≦6.0 Formula (IIb) 0≦Y≦4.0

[0066] In formula (I), X is preferably 300≦X≦4000. In an embodiment according to the present disclosure, X can be 1000≦X≦2500.

[0067] [Tensile modulus of elasticity X of hot-pressed product for measurement] The lower limit of the tensile modulus X of the hot-pressed product for measurement when the material for three-dimensional modeling is molded into the hot-pressed product for measurement (hereinafter simply referred to as the "tensile modulus X of the hot-pressed product for measurement") is preferably 50 MPa or more, more preferably 300 MPa or more, and even more preferably 1000 MPa or more. The upper limit of the tensile modulus X of the hot-pressed product for measurement is preferably 4000 MPa or less, and more preferably 2500 MPa or less.

[0068] In the present disclosure, the tensile modulus X of the hot-pressed product for measurement is measured in accordance with JIS K7161-2: 2014. The test speed is 0.5 mm / min.

[0069] The hot-pressed specimen for measurement is a 1BA type test piece as specified in JIS K7161-2:2014, obtained by hot-pressing a material for 3D modeling. The total length of the hot-pressed specimen for measurement is 75 mm. The thickness of the hot-pressed specimen for measurement is 2 mm. The heating temperature of the hot press molding is 200° C. The pressing pressure of the hot press molding is 50 MPa. The pressing time of the hot press molding is 3 minutes. The hot-pressed product for measurement may be a machined product obtained by hot-press molding a material for three-dimensional modeling and then machining the hot-press molded product.

[0070] [Thermal expansion coefficient of the hot-pressed product for measurement] The thermal expansion coefficient of the hot-pressed product for measurement (hereinafter simply referred to as the "thermal expansion coefficient of the hot-pressed product for measurement") when the three-dimensional modeling material is molded into the hot-pressed product for measurement is set to 1×10 -6 ( / ℃)~1×10 -3 ( / ℃), and preferably 1×10 -6 ( / ℃)~5×10 -4 ( / °C) is more preferred.

[0071] The thermal expansion coefficient of the hot-pressed product for measurement is measured in accordance with JIS K7197:2012.

[0072] [Crystallization temperature of hot-pressed product for measurement] The crystallization temperature (Tc) of the hot-pressed product for measurement when the material for three-dimensional modeling is molded into the hot-pressed product for measurement (hereinafter simply referred to as the "crystallization temperature (Tc) of the hot-pressed product for measurement") is preferably 80°C to 140°C, and more preferably 100°C to 130°C.

[0073] The method for measuring the crystallization temperature (Tc) of the hot-pressed product for measurement is the same as the method for measuring the crystallization temperature of a thermoplastic resin.

[0074] [Melting point of hot-pressed product for measurement] The melting point of the hot-pressed product for measurement (hereinafter referred to as the "melting point of the hot-pressed product for measurement") when the three-dimensional modeling material is molded into the hot-pressed product for measurement is preferably 90°C or higher, more preferably 110°C or higher and 200°C or lower, and even more preferably 110°C or higher and 180°C or lower, from the viewpoint of further suppressing deformation (particularly warping) when made into a three-dimensional object.

[0075] The method for measuring the melting point of the hot-pressed product for measurement is the same as the method for measuring the melting point of the thermoplastic elastomer.

[0076] [Average warpage Y of honeycomb objects for measurement] The average warpage Y of the measurement honeycomb object 10 when the 3D modeling material is layer-by-layer manufactured into the measurement honeycomb object 10 (hereinafter simply referred to as the "average warpage Y of the measurement honeycomb object 10") is preferably 6.0 mm or less, more preferably 4.0 mm or less, the lower the better, and particularly preferably 0 mm.

[0077] The above statement that "when a three-dimensional rectangular prism-shaped object is formed with dimensions of 250 mm x 100 mm x 15 mm height and a full honeycomb filling rate of 30%, the average warpage Y (mm) satisfies formula (IIa)" indicates that the average warpage Y (mm) of the honeycomb object 10 used for measurement satisfies formula (IIa).

[0078] Next, the honeycomb object 10 for measurement will be described with reference to Fig. 1. Fig. 1 is a perspective photograph of the honeycomb object 10 for measurement. As shown in Fig. 1, the honeycomb object 10 for measurement is composed of a honeycomb structure portion 11 and a rectangular parallelepiped frame portion 12. The honeycomb structure portion 11 is located within the rectangular parallelepiped frame portion 12. The honeycomb structure portion 11 and the rectangular parallelepiped frame portion 12 are integrated together. The honeycomb object 10 for measurement is an approximately rectangular parallelepiped object. The rectangular parallelepiped frame portion 12 surrounds the peripheral edge of the honeycomb structure portion 11 in a direction perpendicular to the up-down direction (see FIG. 1). The rectangular parallelepiped frame portion 12 is obtained by layered molding of a material for 3D modeling using a material extrusion method so that the filling rate is 100%. The rectangular parallelepiped frame portion 12 is 250 mm x 100 mm x 15 mm high. More specifically, in FIG. 1, the length of the rectangular parallelepiped frame portion 12 in the front-rear direction is 250 mm. The length of the rectangular parallelepiped frame portion 12 in the left-right direction is 100 mm. The length in the up-down direction is 15 mm. The rectangular parallelepiped frame portion 12 is composed of four plate portions. Each of the four plate portions has a thickness of 5 mm. The honeycomb structure portion 11 has a honeycomb structure. The honeycomb structure portion 11 is obtained by layer-by-layer molding of a three-dimensional molding material in a rectangular parallelepiped frame portion 12 by a material extrusion method so that the filling rate is 30%. The filling rate refers to the ratio of the volume of the material for three-dimensional modeling to the volume of a unit space.

[0079] Next, the average amount of warpage Y of the measurement honeycomb object 10 will be described with reference to Fig. 2. Fig. 2 is a side view of the measurement honeycomb object 10 for explaining the average amount of warpage Y. The average warpage amount Y of the honeycomb object 10 to be measured is the amount of lift Y of the four corners of the rectangular parallelepiped frame portion 12 from the surface plate 20 when the honeycomb object 10 to be measured is placed on the surface plate 20. A The arithmetic mean value of The amount of lift Y of the corner E12 of the rectangular frame portion 12 Ais measured as follows. As shown in Fig. 2, the honeycomb object 10 to be measured is placed on the surface of a surface plate 20 so that the first surface TS10 of the honeycomb object 10 to be measured faces upward. Next, the maximum height of the underside BS10 of the corner E12 of the honeycomb object 10 to be measured from the surface of the surface plate 20 is measured. A height gauge can be used to measure the maximum height. The measured value obtained is the amount of lift Y of the corner E12 of the rectangular parallelepiped frame portion 12. A Shows. The average warpage amount Y of the honeycomb structure 10 to be measured is calculated by subtracting the amount of lift Y of each of the four corners of the honeycomb structure 10 to be measured. A It is obtained by adding and dividing the resulting sum by 4.

[0080] When a three-dimensional object is formed by a material extrusion method, from the viewpoint of increasing the adhesive strength between the modeling layers of the three-dimensional object, it is preferable that a modeling layer (hereinafter referred to as the "first modeling layer") made of a molten three-dimensional modeling material extruded from a nozzle and a modeling layer (hereinafter referred to as the "second modeling layer") on which the first modeling layer is deposited are melt-bonded. Furthermore, it is preferable that the second modeling layer is melted by the heat of the first modeling layer, or that the crystallization of the second modeling layer does not progress until the first modeling layer is completely deposited on the second modeling layer. Therefore, the crystallization temperature (Tc) of the three-dimensional modeling material is preferably 80°C to 140°C, and more preferably 100°C to 130°C. The crystallization temperature of the material for three-dimensional modeling can be measured in the same manner as the measurement method for the thermoplastic resin described above.

[0081] [Breaking stress of measurement object] The lower limit of the breaking stress α of the measurement object when the material for 3D printing is layer-by-layer-printed into the measurement object (hereinafter simply referred to as the "breaking stress α of the measurement object") is preferably 4.0 MPa or more, more preferably 5 MPa or more, more preferably 6.5 MPa or more, and even more preferably 8.0 MPa or more. The upper limit of the breaking stress α of the measurement object is preferably 200.0 MPa.

[0082] The breaking stress α of a 3D object is measured in accordance with JIS K7161-2:2014 (test speed: 50 mm / min) by creating a rectangular prism object 2 mm thick, punching out a test piece (JIS K7161-2 1BA:2014) from its wall so that the tensile direction is the layering direction. This allows the breaking stress α of the 3D object in the layering direction to be confirmed. The breaking stress α of a 3D object in the layering direction of the 3D object is generally the smallest of all the breaking stresses of 3D objects. If the 3D object yields before it breaks, the smaller of the breaking stress and yield stress is used as the breaking stress α.

[0083] In other words, the breaking stress α of the measurement object is the measured value of a tensile test conforming to JIS K7161-2:2014.

[0084] The object for measurement is a 1BA type test piece defined in JIS K7161-2:2014, which is obtained by layering the material for 3D modeling using the material extrusion method and machining it. The total length of the object for measurement is 75 mm. The thickness of the object for measurement is 2 mm. The measurement object before machining (hereinafter referred to as the "measurement object before machining") is, for example, a rectangular prism-shaped object with a thickness of 2 mm. The measurement object before machining is obtained by layering the material for 3D printing using a material extrusion method so that the filling rate is 100% and the stacking direction of the material for 3D printing is parallel to the tensile direction of the measurement object in the tensile test.

[0085] [Tensile elastic modulus Z of the measurement object] The lower limit of the tensile modulus Z of the measurement object when the three-dimensional modeling material is layer-by-layer manufactured into the above-mentioned measurement object (hereinafter simply referred to as the "tensile modulus Z of the measurement object") is preferably 200 MPa or more, more preferably 800 MPa or more, and even more preferably 1000 MPa or more. The upper limit of the tensile elastic modulus X of the material for three-dimensional modeling is preferably 4000 MPa or less, more preferably 2500 MPa or less, and more preferably 2000 MPa or less.

[0086] In the present disclosure, the tensile modulus Z of the measurement object is measured in accordance with JIS K7161-2: 2014. The test speed is 0.5 mm / min. The stacking direction of the material for 3D printing of the measurement object is parallel to the tensile direction of the measurement object in the tensile test conforming to JIS K7161-2:2014.

[0087] In the three-dimensional modeling material, it is preferable that the breaking stress α (MPa) of the measurement object satisfies the following formula (III), and the average warpage Y (mm) of the measurement honeycomb object 10 satisfies the following formula (IIb). Formula (III) 6.5 ≦ α < 200 Formula (IIb) 0≦ Y ≦ 4.0

[0088] (Other ingredients) The three-dimensional modeling material in the present disclosure may contain other components in addition to the above-mentioned thermoplastic elastomer and thermoplastic resin.

[0089] Examples of other components include ultraviolet absorbing agents, stabilizers, antioxidants, plasticizers, colorants, tinting agents, flame retardants, antistatic agents, fluorescent brighteners, matting agents, and impact strength improvers.

[0090] (Form of material for 3D modeling) The material for three-dimensional modeling may be a molded article. The molding method for the molded product is not particularly limited, and the molded product may be molded by a known molding method such as extrusion molding. The molded article may be in the form of pellets or filaments. Pellets refer to small amounts of pre-shaped solid matter. A filament is a long, thin, string-like object with a uniform cross section. Filaments are generally used in the form wound around a reel.

[0091] The material for three-dimensional printing may be in the form of either pellets or filaments, or may be a mixture of materials in the form of both pellets and filaments. From the viewpoint of printing a three-dimensional object having a relatively large size, the material for three-dimensional printing is preferably in the form of pellets.

[0092] When the three-dimensional modeling material is molded into pellets, the molding method is not limited. For example, the three-dimensional modeling material is kneaded and extruded by a melt extruder (e.g., a twin-screw extruder) and the extruded rod-shaped strands are cut by a pelletizer. The three-dimensional modeling material to be fed into the melt extruder may be a dry blend. The dry blend is prepared by previously mixing a part or all of the three-dimensional modeling material with a Henschel mixer or the like.

[0093] <Manufacturing method for 3D objects> The manufacturing method of the three-dimensional object according to the present disclosure includes a melting step of melting the above-described three-dimensional object manufacturing material according to the present disclosure, and a modeling step of extruding the molten three-dimensional object manufacturing material from a nozzle of a three-dimensional object manufacturing apparatus to form a three-dimensional object. The melting step and the modeling step are performed in this order.

[0094] (Melting process) In the melting step in the present disclosure, the above-described three-dimensional modeling material of the present disclosure is melted. The heating means for melting the three-dimensional modeling material is not particularly limited, and any known heating means can be used.

[0095] In the melting step, it is preferable to use a three-dimensional object manufacturing device equipped with a heating means such as an electric heater.

[0096] The temperature at which the three-dimensional modeling material is melted is not particularly limited and may be set appropriately depending on the properties of the thermoplastic resin. The temperature at which the three-dimensional modeling material is melted may be, for example, a temperature of +10°C to +150°C based on the melting point or glass transition temperature (Tg) of the thermoplastic resin, whichever is higher.

[0097] In the melting step, for example, the material for three-dimensional printing may be melted and kneaded. In particular, when the material for three-dimensional printing contains glass fiber, it is preferable that the material for three-dimensional printing is melted and kneaded in the melting step. By melting and kneading the material for three-dimensional printing, the material for three-dimensional printing tends to be mixed more uniformly. Therefore, the occurrence of unevenness in the material of the obtained three-dimensional object is easily suppressed. As a result, the deformation of the three-dimensional object tends to be further suppressed.

[0098] (modeling process) In the modeling process according to the present disclosure, the three-dimensional modeling material melted in the melting process is extruded from a nozzle to form a three-dimensional object.

[0099] In the modeling process, for example, a molten 3D modeling material is extruded from the nozzle of a 3D model manufacturing device, and 2D layers are sequentially stacked on a substrate based on multiple 2D data, thereby forming a 3D object. The multiple 2D data are generated by slicing the 3D coordinate data of the 3D object to be formed into slices using slicer software.

[0100] The three-dimensional object manufacturing device may be a material extrusion type three-dimensional object manufacturing device. There are no particular limitations on the material extrusion type three-dimensional object manufacturing device, and any known device or known device configuration may be used.

[0101] The three-dimensional object manufacturing device may be, for example, a device including a cylinder, a nozzle, and a heating means. The three-dimensional modeling material is supplied to the cylinder. The nozzle is provided at a location on the downstream side of the cylinder in the discharge direction of the three-dimensional modeling material. The nozzle discharges the three-dimensional modeling material. The heating means is provided on the cylinder. The heating means heats and melts the three-dimensional modeling material. The 3D modeling device extrudes heated and melted 3D modeling material from a nozzle, and layer-by-layer models the 3D modeling material extruded from the nozzle, thereby creating a 3D model.

[0102] The cylinder may have a screw therein. The screw kneads the three-dimensional modeling material. The three-dimensional object manufacturing apparatus may further include a table device that is disposed opposite the nozzle. The molten three-dimensional object material extruded from the nozzle is stacked on the table device. The three-dimensional object manufacturing apparatus may further include a control means for controlling the spatial coordinates of the substrate and the nozzle, and the amount of the three-dimensional object material extruded from the nozzle. It is preferable that the control means controls the discharge of the molten three-dimensional object material extruded from the nozzle, and controls the movement of the nozzle and / or the table device in the X-axis, Y-axis, and Z-axis directions relative to a reference plane.

[0103] (Other processes) The method for manufacturing a three-dimensional object according to the present disclosure may further include, for example, a processing step in which the three-dimensional object manufactured in the modeling step is processed.

[0104] <3D object> The three-dimensional object of the present disclosure is an object made from the above-described three-dimensional object material of the present disclosure. The material for three-dimensional modeling of the present disclosure is used as a raw material for the three-dimensional modeling of the present disclosure, and therefore deformation of the three-dimensional model due to thermal shrinkage or the like is suppressed.

[0105] The three-dimensional object of the present disclosure is not particularly limited as long as it is an object made from the above-described three-dimensional modeling material of the present disclosure, and may be one that is modeled by any method. In particular, the three-dimensional object of the present disclosure is preferably one that is modeled by the above-described method for manufacturing a three-dimensional object of the present disclosure. EXAMPLES

[0106] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples as long as it does not exceed the gist of the disclosure. In addition, unless otherwise specified, "parts" are based on mass. The melting point, Shore hardness, MFR, crystallization temperature, crystallinity, tensile modulus X, thermal expansion coefficient, breaking stress, average warpage Y, and tensile modulus Y shown below were each measured by the above-mentioned method.

[0107] --Preparing materials-- Details of the materials used in this example (that is, the components contained in the material for three-dimensional modeling) are as follows. (Thermoplastic elastomer) DF8200: Toughmer (registered trademark; hereafter the same) DF8200 (Mitsui Chemicals, Inc.) XM7090: Toughmer XM-7090 (Mitsui Chemicals, Inc.) DF610: Toughmer DF610 (Mitsui Chemicals, Inc.) DF710: Toughmer DF710 (Mitsui Chemicals, Inc.) PN2070: Toughmer PN-2070 (Mitsui Chemicals, Inc.) PN3560: Toughmer PN-3560 (Mitsui Chemicals, Inc.) EP1001: Absomer EP1001 (Mitsui Chemicals, Inc.) ·TS6000N: Milastomer TS6000N (Mitsui Chemicals, Inc.) 6030NS: Milastomer 6030NS (Mitsui Chemicals, Inc.)

[0108] (thermoplastic resin) J966HP: Prime Polypro (registered trademark; hereafter the same) J-966HP (propylene-ethylene copolymer, Prime Polymer Co., Ltd.) J105G: Prime Polypro J-105G (propylene homopolymer, Prime Polymer Co., Ltd.) J108M: Prime Polypro J108M (propylene homopolymer, Prime Polymer Co., Ltd.) J721GR: Prime Polypro J721GR (propylene-ethylene copolymer, Prime Polymer Co., Ltd.) J229E: Prime Polypro J229E (propylene-ethylene copolymer, Prime Polymer Co., Ltd.) J707G: Prime Polypro J707G (propylene-ethylene copolymer, Prime Polymer Co., Ltd.) J705UG: Prime Polypro J705UG (propylene-ethylene copolymer, Prime Polymer Co., Ltd.) J708UG: Prime Polypro J708UG (propylene-ethylene copolymer, Prime Polymer Co., Ltd.)

[0109] (filling material) Talc: Volume average particle size 5μm~10μm Glass fiber (GF): Weight average fiber length 0.5~2mm

[0110] Tables 1 to 6 show the melting point, Shore hardness, and MFR of the thermoplastic elastomer, and the crystallization temperature and crystallinity of the thermoplastic resin, as listed in the manufacturer's catalog. In the table, "A" before the numerical value in the "Shore Hardness" column indicates Shore A hardness. In the table, "D" before the numerical value in the "Shore Hardness" column indicates Shore D hardness. For example, "A86" in Example 1 indicates that the Shore A hardness is 86. Similarly, "D58" in Example 9 indicates that the Shore D hardness is 58. In the table, the items "Melting point: Tm [℃]," "Shore hardness," and "MFR [g / min]" located immediately below the "(Thermoplastic elastomer)" heading indicate the catalog values ​​of the melting point, Shore hardness, and MFR of the thermoplastic elastomer. In the table, the items "Crystallization temperature: Tc [℃]" and "Crystallization degree [%]" located immediately below the "(Thermoplastic resin)" heading indicate the catalog values ​​of the crystallization temperature and crystallinity of the thermoplastic resin (propylene-based polymer), which is a component of the 3D modeling material.

[0111] [Examples 1 to 38 and Comparative Examples 1 to 19]

[0112] -Measurement of tensile modulus X of hot-pressed test piece- The material for 3D modeling was hot-press molded under conditions of a heating temperature of 200°C, a press pressure of 50 MPa, and a press time of 3 minutes to obtain the above-mentioned hot-pressed product for measurement. The obtained hot-pressed product for measurement was a 1BA type test piece as specified in JIS K7161-2:2014. The total length of the hot-pressed product for measurement was 75 mm. The thickness of the hot-pressed product for measurement was 2 mm. The tensile modulus X of the obtained hot-pressed product for measurement was measured. The measurement results are shown in Tables 1 to 6. In the table, the item "Tensile modulus X [MPa]" located immediately below the item "(Hot-pressed product)" indicates the measurement result of the tensile modulus X of the hot-pressed product for measurement.

[0113] In the table, the content (%) listed next to the thermoplastic resin means the mass content of the thermoplastic resin relative to the total mass of the material for 3D modeling. The content (%) listed next to the thermoplastic elastomer means the mass content of the thermoplastic elastomer relative to the total mass of the material for 3D modeling. The content (%) listed next to the filler means the mass content of the filler relative to the total mass of the material for 3D modeling.

[0114] -Melting point, crystallization temperature, and thermal expansion coefficient of the hot-pressed product for measurement- A hot-pressed product for measurement was obtained in the same manner as in "Measurement of tensile modulus X of hot-pressed product for measurement." The melting point, crystallization temperature, and thermal expansion coefficient of the hot-pressed product for measurement were each measured. The measurement results are shown in Tables 1 to 6. In the table, under the heading "(Heat-pressed product)", "Melting point: Tm [℃]", "Crystallization temperature: Tc [℃]", and "Thermal expansion coefficient [10 -5 / °C] indicates the measurement results of the melting point, crystallization temperature, and thermal expansion coefficient of the hot-pressed product used for measurement. In the tables, "-" in the "Components and Content" column indicates that the component is not contained, and "-" is also shown in the corresponding physical properties column. In the tables, "-" in the "Physical Properties and Evaluation" column indicates that the corresponding measurement or evaluation was not performed.

[0115] -Measurement of deformation (average warpage Y) of the honeycomb object 10 for measurement- The above-mentioned honeycomb object 10 for measurement was formed using a material extrusion type three-dimensional object manufacturing device ("DeltaWASP 3MT Industrial" manufactured by WASP Corporation, nozzle diameter: 3 mm) and application software ("Simplify3D" manufactured by Simplify3D Corporation). First, the 3D modeling materials shown in Tables 1 to 6 were put into a hopper, and the 3D modeling materials were supplied into the cylinder through the hopper. The components constituting the 3D modeling materials were the thermoplastic elastomers, thermoplastic resins, and fillers shown in each table. Next, the 3D modeling materials were heated to a temperature of 180°C to 240°C by a heater provided in the cylinder, and melted (melting process).

[0116] Next, the following 3D data was sliced ​​by application software to generate multiple pieces of 2D data. Based on the multiple pieces of 2D data, the application software's setting parameters were set as follows, and a honeycomb object 10 for measurement, as shown in Fig. 1, was modeled by material extrusion (MEX). Specifically, based on the three-dimensional coordinate data, molten three-dimensional modeling material was layered in sequence on a substrate to model a three-dimensional rectangular parallelepiped object with dimensions of 250 mm x 100 mm x height 15 mm and a full honeycomb filling rate of 30% (modeling process). <3D data> · 250mm x 100mm x 15mm height cuboid <Setting parameters of the honeycomb structure 11 of the honeycomb object 10 for measurement> - Build speed: 3000mm / min Nozzle temperature: 240℃ Layer pitch: 1.5mm ·Filling rate: 30% Filling pattern: Honeycomb <Setting parameters of the rectangular parallelepiped frame portion 12 of the honeycomb object 10 for measurement> - Build speed: 3000mm / min Nozzle temperature: 240℃ Layer pitch: 1.5mm ·Filling rate: 100% Fill Pattern: Solid

[0117] The average amount of warpage Y (mm) of the obtained honeycomb shaped article for measurement 10 was measured. The measurement results are shown in Tables 1 to 6. In this evaluation, examples marked with "-" in the table indicate that a honeycomb object 10 for measurement, which is necessary for measurement, could not be obtained due to deformation during shaping. In the table, the "average amount of warpage Y" located under the heading "(three-dimensional object)" indicates the average amount of warpage Y of the honeycomb objects 10 used for measurement.

[0118] -Evaluation of the appearance and surface of the honeycomb structure 10 for measurement- The appearance and surface condition of the measurement honeycomb object 10 were visually evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 1 to 6. In the table, "Evaluation of appearance and surface" located under the heading "(3D object)" indicates the evaluation results of the appearance and surface of the honeycomb object 10 for measurement.

[0119] <Evaluation criteria> G1: The surface of the honeycomb object 10 to be measured is smooth, the appearance is good, and the 3D data (three-dimensional coordinate data) can be reproduced more faithfully. G2: The surface of the honeycomb object 10 for measurement is smooth and the appearance is good. G3: The surface of the honeycomb object 10 for measurement has some irregularities, but the appearance is acceptable. G4: Unacceptable significant irregularities are observed on the surface of the honeycomb object 10 to be measured, or 3D data (three-dimensional coordinate data) cannot be reproduced.

[0120] -Measurement of breaking stress α and tensile modulus Z of the measurement object- To create the above-mentioned measurement object, a material extrusion type 3D object manufacturing device ("DeltaWASP 3MT Industrial" manufactured by WASP Corporation, nozzle diameter: 2 mm) and application software ("Simplify3D" manufactured by Simplify3D Corporation) were used. First, the 3D modeling materials shown in Tables 1 to 6 were put into a hopper, and the 3D modeling materials were supplied into the cylinder through the hopper. The components constituting the 3D modeling materials were the thermoplastic elastomers, thermoplastic resins, and fillers shown in each table. Next, the 3D modeling materials were heated to a temperature of 180°C to 240°C by a heater provided in the cylinder, and melted (melting process).

[0121] Next, the application software sliced ​​the 3D data below to generate multiple 2D data sets. Based on the multiple 2D data sets, the application software's parameters were set as shown below, and a measurement object before machining was created using the material extrusion method (MEX) (modeling process). <3D data> · 130mm x 130mm x 2mm thick rectangular prism <Setting parameters> - Build speed: 3000mm / min Nozzle temperature: 240℃ Layer pitch: 1.0mm ·Filling rate: 100% Fill Pattern: Solid

[0122] Next, the obtained unmachined measurement object was machined to obtain a measurement object. The measurement object obtained was a 1BA type test piece as specified in JIS K7161-2:2014. The total length of the measurement hot-pressed product was 75 mm. The thickness of the measurement object was 2 mm. The breaking stress α and tensile modulus Z of the measurement object were each measured. When measuring the breaking stress α and tensile modulus Z of the measurement object, the stacking direction of the material for 3D printing and the tensile direction of the measurement object in the tensile test were parallel. The measurement results are shown in Tables 1 to 6. In the table, "Breaking stress α [MPa]" and "Tensile modulus Z [MPa]" located under the heading "(3D object)" indicate the measurement results of the breaking stress and tensile modulus Z of the measurement object.

[0123] [Table 1]

[0124] [Table 2]

[0125] [Table 3]

[0126] [Table 4]

[0127] [Table 5]

[0128] [Table 6]

[0129] As shown in Tables 1 to 6, the 3D printing materials of Examples 1 to 38 contain a thermoplastic resin, a thermoplastic elastomer, and a filler. The filler contains talc. The content of the filler was 5 mass % or more and 70 mass % or less with respect to the total mass of the 3D printing material. Therefore, the average warpage Y of the honeycomb object 10 for measurement was 6.0 mm or less. In other words, it was found that deformation (especially warpage) of the 3D printed objects using the 3D printing materials of Examples 1 to 38 was suppressed.

[0130] Moreover, the 3D modeling materials of Examples 7 to 9 are fillers that combine talc and glass fiber. Therefore, it was found that the 3D models using the 3D modeling materials of Examples 7 to 9 had small stress distortion and a smooth appearance.

[0131] On the other hand, the 3D modeling materials of Comparative Examples 1 to 8 were made of a thermoplastic resin and did not contain a thermoplastic elastomer or a filler. The 3D modeling materials of Comparative Examples 9 to 19 were made of a thermoplastic resin and a thermoplastic elastomer and did not contain a filler. Therefore, the average warpage Y of the honeycomb objects 10 for measurement was more than 6.0 mm. In other words, it was found that the deformation (especially warpage) of the 3D models using the 3D modeling materials of Comparative Examples 1 to 19 was not suppressed.

[0132] The disclosures of Japanese Patent Application No. 2019-174751, filed on September 25, 2019, and Japanese Patent Application No. 2020-071719, filed on April 13, 2020, are incorporated herein by reference in their entireties. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.

Claims

1. The composite material is made of a thermoplastic resin, a thermoplastic elastomer, and a filler. the thermoplastic resin is a propylene-based polymer, The filler comprises talc; The content of the filler is 25% by mass or more and 50% by mass or less with respect to the total mass of the material for three-dimensional modeling, The content of the thermoplastic elastomer is 20% by mass or more based on the total mass of the material for three-dimensional modeling, The thermoplastic elastomer is a propylene-based elastomer having a melting point of 80°C to 120°C, a Shore D hardness of 40 to 60, and a melt flow rate of 2g / 10min to 20g / 10min, and is a material for three-dimensional modeling (excluding cases where an acid-modified polyolefin-based resin is included).

2. The material for three-dimensional printing according to claim 1 , wherein the content of the thermoplastic resin is 0.1% by mass or more and 50% by mass or less with respect to a total mass of the material for three-dimensional printing.

3. 3. The material for three-dimensional printing according to claim 1, wherein a content of the thermoplastic elastomer is 20% by mass or more and 40% by mass or less with respect to a total mass of the material for three-dimensional printing.

4. When molded into a hot-pressed product for measurement, the hot-pressed product for measurement has a tensile modulus X (MPa) according to JIS K7161-2:2014 that satisfies the following formula (I), The average warpage Y (mm) of the honeycomb structure to be measured when laminated to the honeycomb structure to be measured satisfies the following formula (IIa): The hot-pressed product for measurement is a 1BA type test piece defined in JIS K7161-2:2014 obtained by hot-press molding the material for three-dimensional modeling, The honeycomb object for measurement is a rectangular parallelepiped frame portion measuring 250 mm x 100 mm x 15 mm in height, obtained by layering the three-dimensional modeling material by a material extrusion method so that a filling rate, which indicates a ratio of the volume of the three-dimensional modeling material to a unit space volume, is 100%; and a honeycomb structure portion obtained by layer-forming the three-dimensional modeling material by the material extrusion method in the rectangular parallelepiped frame portion so that the filling rate is 30%, A three-dimensional modeling material according to any one of claims 1 to 3, wherein the average warpage amount Y indicates the arithmetic mean value of the amount of lift of the four corners of the rectangular frame portion from the base plate when the measurement honeycomb object is placed on the base plate. Formula (I) 50≦X≦4000 Formula (IIa) 0≦Y≦6.0

5. The content of the thermoplastic elastomer is 20% by mass or more and less than 70% by mass with respect to the total mass of the three-dimensional modeling material, The content of the filler is 25% by mass or more and less than 50% by mass with respect to the total mass of the material for three-dimensional printing, 5. The material for three-dimensional printing according to claim 1, wherein a total content of the thermoplastic elastomer and the filler is 45% by mass or more and less than 90% by mass with respect to a total mass of the material for three-dimensional printing.

6. The breaking stress α [MPa] of the measurement object, when additively manufactured, in a tensile test in accordance with JIS K7161-2:2014 satisfies the following formula (III), The average warpage Y [mm] of the honeycomb structure for measurement when laminated to the honeycomb structure for measurement satisfies the following formula (IIb), the measurement object is a 1BA-type test piece defined in JIS K7161-2:2014, which is obtained by layer-forming the material for three-dimensional printing by a material extrusion method and machining the material so that the filling rate, which indicates the ratio of the volume of the material for three-dimensional printing to a unit space volume, is 100% and the stacking direction of the material for three-dimensional printing is parallel to the tensile direction of the measurement object in the tensile test; The honeycomb object for measurement is A rectangular parallelepiped frame part of 250 mm x 100 mm x 15 mm height obtained by layering the three-dimensional modeling material by the material extrusion method so that the filling rate is 100%. and a honeycomb structure portion obtained by layer-forming the three-dimensional modeling material by the material extrusion method in the rectangular parallelepiped frame portion so that the filling rate is 30%, A three-dimensional modeling material according to any one of claims 1 to 5, wherein the average warpage amount Y indicates the arithmetic mean value of the amount of lift of the four corners of the rectangular frame portion from the base plate when the measurement honeycomb object is placed on the base plate. Formula (III) 6.5≦ α <200 Formula (IIb) 0≦Y≦4.0

7. A melting step of melting the material for three-dimensional modeling according to any one of claims 1 to 6; a modeling step of extruding the molten material for three-dimensional modeling from a nozzle of a three-dimensional object manufacturing apparatus to form a three-dimensional object; A method for manufacturing a three-dimensional object comprising the steps of:

8. A three-dimensional object produced by using the three-dimensional modeling material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Resin molding material for three-dimensional molding devices and filament for three-dimensional molding devices

    JP2018131497A

  • Molded resin strand

    WO2017057424A1

  • Resin composition for three-dimensional modeling, three-dimensional modeled article, and method for manufacturing three-dimensional modeled article

    WO2019146474A1