EMM-58 zeolite compositions, synthesis and uses

The synthesis of EMM-58 aluminosilicate zeolite with tailored pore structures addresses the limitations of existing zeolites by enabling efficient adsorption and conversion of small molecules, improving catalytic performance in various chemical processes.

JP7587017B2Active Publication Date: 2024-11-19EXXONMOBIL TECHNOLOGY & ENGINEERING CO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023508108
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-07
Publication Date
2024-11-19
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Current zeolite frameworks do not effectively utilize smaller pore sizes for adsorption and conversion of small molecules, limiting their applicability in processes such as organic compound conversions and gas separations.

Method used

The development of an aluminosilicate zeolite (EMM-58) with unique 8-ring pores and specific unit cell dimensions, synthesized using silicon and aluminum sources with structural directing agents like N,N',2-trimethylbenzimidazolium, allowing for the production of zeolites with Si to Al ratios between 3 to 10, and optimized reaction conditions to achieve desired pore structures.

Benefits of technology

EMM-58 zeolite provides favorable sites for adsorption and conversion of small molecules, enhancing catalytic performance in processes like hydrocarbon conversions, selective catalytic reduction of NOx, CO2 and N2 adsorption, and production of amines, with improved selectivity and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587017000008
    Figure 0007587017000008
  • Figure 0007587017000009
    Figure 0007587017000009
  • Figure 0007587017000010
    Figure 0007587017000010
Patent Text Reader

Abstract

The aluminosilicate zeolite may have a molar ratio of Si to Al of about 3 to about 10, a monoclinic space group C2 / m with unit cell dimensions of a 13.6 Å + / - 5%, b 21.7 Å + / - 5%, c 6.7 Å + / - 5%, and β 93° + / - 3°, 12-ring pores with dimensions of 7 Å + / - 5% × 6 Å + / - 5% along the c-axis and 8-ring pores with dimensions of 3 Å + / - 5% × 3 Å + / - 5% along the a-axis. The aluminosilicate zeolite may be useful in hydrocarbon conversion processes, selective catalytic reduction of NOx, CO and / or N adsorption, carbonylation reactions, and mono- and di-alkylamine synthesis.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to aluminosilicate zeolite compositions, synthesis and uses. [Background technology]

[0002] Zeolites are a family of porous materials that have an ordered inorganic framework structure with multiple pores or channels of defined set sizes therein. The size of the pores or channels varies for different zeolites and determines the width of molecules that can enter the interior of a particular zeolite. Because of their microporosity of defined size and the molecular specificity that results therefrom, zeolites often find particular utility in adsorption, ion exchange, gas separation and catalytic applications. The various zeolite framework structures recognized by the Structure Commission of the International Zeolite Association are maintained in a structure database accessible at http: / / www.iza-structure.org / databases.

[0003] The idealized inorganic framework structure of zeolite is a framework silicate in which all tetrahedral atoms are connected by the four next nearest tetrahedral atoms and oxygen atoms. As used herein, the term "silicate" refers to a material that includes at least silicon and oxygen atoms that are alternately bonded to each other (i.e., -O-Si-O-Si-), and optionally includes other atoms in an inorganic framework structure, including atoms such as boron, aluminum, or other metals (e.g., transition metals such as titanium, vanadium, or zinc). Atoms other than silicon and oxygen in framework silicate occupy some of the lattice sites that would otherwise be occupied by silicon atoms in an "all-silica" framework silicate. Thus, as used herein, the term "framework silicate" refers to any atomic lattice, including silicate, borosilicate, gallosilicate, ferrisilicate, aluminosilicate, titanosilicate, zincosilicate, vanadosilicate, and the like.

[0004] The structure of the framework silicate within a given zeolite determines the size of the pores or channels present therein. The size of the pores or channels may determine the types of processes to which a given zeolite is applicable. Currently, over 200 unique zeolite framework silicate structures are known and recognized by the International Zeolite Association's Structure Committee, which defines a range of pore geometries and orientations.

[0005] Zeolite framework silicates are generally characterized in terms of their ring size, where ring size refers to the number of oxygen atoms and tetrahedrally coordinated silicon atoms (or other atoms such as those listed above) in the loops that define the pores or channels within the zeolite. For example, an "8-ring" zeolite refers to a zeolite that has pores or channels defined by eight alternating tetrahedral atoms and eight oxygen atoms in the loops. The pores or channels defined within a given zeolite can be symmetrical or asymmetrical, depending on the various structural constraints present within a particular framework silicate. Summary of the Invention [Means for solving the problem]

[0006] The present disclosure relates to aluminosilicate zeolite compositions, synthesis and uses.

[0007] The present disclosure relates to a crystal having (a) a monoclinic space group C2 / m with unit cell dimensions of a of 13.6 Å + / - 5%, b of 21.7 Å + / - 5%, c of 6.7 Å + / - 5% and β of 93° + / - 3°, (b) a 12-ring cavity with dimensions along the c-axis of 7 Å + / - 5% by 6 Å + / - 5%, and (c) an 8-ring cavity with dimensions along the a-axis of 3 Å + / - 5% by 3 Å + / - 5%. Si to Al ratio is about 3 to about 10 The composition includes an aluminosilicate zeolite having a molar ratio of:

[0008] The present disclosure includes aluminosilicate zeolites having a coordination series of T atoms of T1 4 10 19 32 48 69 98 126 154 192; T2 4 11 17 30 48 72 100 125 150 186; T3 4 10 20 32 47 69 96 126 159 191; and T4 4 10 19 31 48 71 97 125 156 189.

[0009] The present disclosure provides a process for producing a silicon atom-containing fluoride ... Si to Al ratio is about 3 to about 10 and (ii) providing an aluminosilicate zeolite having (a) a monoclinic space group C2 / m with unit cell dimensions of a 13.6 Å + / - 5%, b 21.7 Å + / - 5%, c 6.7 Å + / - 5% and β of 93° + / - 3°, (b) a 12-ring pore with dimensions along the c-axis of 7 Å + / - 5% by 6 Å + / - 5%, and (c) an 8-ring pore with dimensions along the a-axis of 3 Å + / - 5% by 3 Å + / - 5%.

[0010] The disclosure includes a method comprising maintaining an aqueous reaction mixture comprising a source of silicon atoms, a source of aluminum atoms, and a structure directing agent selected from the group consisting of N,N',2-trimethylbenzimidazolium, N,N',2-dimethylbenzimidazolium, and combinations thereof, at a temperature of about 135°C to about 180°C to provide an aluminosilicate zeolite having a coordination series of T atoms of T1 4 10 19 32 48 69 98 126 154 192; T2 4 11 17 30 48 72 100 125 150 186; T3 4 10 20 32 47 69 96 126 159 191; and T4 4 10 19 31 48 71 97 125 156 189.

[0011] The aluminosilicate zeolites and aluminosilicate zeolites produced by the methods described above may be applied to one or more of organic compound conversion processes (e.g., hydrocarbon conversion processes), selective catalytic reduction of NOx, CO2 and / or N2 adsorption, carbonylation reactions, and the production of mono- and di-alkylamines. For example, a method may include carrying out a hydrocarbon conversion process selected from the group consisting of cracking, hydrocracking, disproportionation, alkylation, and isomerization in the presence of the aluminosilicate zeolites.

[0012] The following figures are included to illustrate certain aspects of the present disclosure and should not be considered as exclusive configurations. The disclosed subject matter is capable of considerable modification, alteration, combinations and equivalents in form and function, as will occur to those skilled in the art and having the benefit of this disclosure. [Brief description of the drawings]

[0013] [Figure 1] 1 is a scanning electron microscope (SEM) image of sample 5. [Figure 2A-2B] 1 is an SEM image of sample 6. [Diagram 3] 1 is a plot including the XRD patterns of Sample 6 as-prepared (bottom) and after firing (top). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present disclosure relates to aluminosilicate zeolite compositions, synthesis and uses. The aluminosilicate zeolite, herein referred to as EMM-58 zeolite, has a unique structure similar to mordenite but with smaller 8-ring pores. Advantageously, the smaller 8-ring pores of EMM-58 zeolite may provide favorable sites for the adsorption and / or conversion of small molecules.

[0015] The EMM-58 zeolite described herein has a coordination series of T atoms of T1 4 10 19 32 48 69 98 126 154 192; T2 4 11 17 30 48 72 100 125 150 186; T3 4 10 20 32 47 69 96 126 159 191; and T4 4 10 19 31 48 71 97 125 156 189.

[0016] The EMM-58 zeolite of the present disclosure (as prepared, after treatment (e.g., with acid or acid and steam) and / or after calcination) has a structure with (a) a monoclinic space group C2 / m with unit cell dimensions of a of 13.6 Å + / - 5%, b of 21.7 Å + / - 5%, c of 6.7 Å + / - 5%, and β of 93° + / - 3°, (b) a 12-ring pore with dimensions along the c-axis of 7 Å + / - 5% by 6 Å + / - 5%, and (c) an 8-ring pore with dimensions along the a-axis of 3 Å + / - 5% by 3 Å + / - 5%.

[0017] The EMM-58 zeolite described herein contains N,N',2-trimethylbenzimidazolium (Compound 1, where X - The counter ion is OH - , F - , Cl - , Br - , I - N,N',2-dimethylbenzimidazolium (compound 2, where X - The counter ion is OH - , F - , Cl - , Br - , I - ) or prepared using a mixture of compounds 1 and 2. [ka]

[0018] The EMM-58 zeolite described herein can be prepared by heating an aqueous reaction mixture containing a silicon atom source, an aluminum atom source, and an SDA (e.g., N,N',2-trimethylbenzimidazolium, N,N',2-dimethylbenzimidazolium, or mixtures thereof) to a temperature of about 135°C to about 180°C (or 145°C to about 175°C, or about 150°C to about 170°C, or about 155°C to about 165°C); The ratio of Si to Al is about 3 to about 10 (or about 3 to about 7, or about 5 to about 10). The aluminosilicate zeolite is synthesized by obtaining an EMM-58 zeolite having the molar ratio described herein. The aqueous reaction mixture can be maintained at about 135°C to about 180°C (or 145°C to about 175°C, or about 150°C to about 170°C, or about 155°C to about 165°C) for about 20 days to about 36 days (or about 25 days to about 30 days).

[0019] Examples of silicon atom sources include, but are not limited to, colloidal suspensions of silica, precipitated silica alkali metal silicates, tetraalkyl orthosilicates, different Si-containing zeolites, and the like, and any combination thereof.

[0020] Examples of aluminum atom sources include, but are not limited to, aluminum nitrate, aluminum sulfate, sodium aluminate, aluminum oxide, alumina sol, alumina trihydrate, clays (e.g., kaolin and metakaolin), other Al-containing zeolites (e.g., FAU-type zeolites such as zeolite Y), and the like, and any combination thereof.

[0021] In the aqueous reaction mixture The molar ratio of Si to Al is about 2 to about 50 (or about 2 to about 25, or about 15 to about 40, or about 25 to about 50). It could be.

[0022] In the aqueous reaction mixture The molar ratio of Si to SDA (e.g., N,N',2-trimethylbenzimidazolium, N,N',2-dimethylbenzimidazolium, or a combination thereof) is about 0.1 to about 1 (or about 0.1 to about 0.5, or about 0.2 to about 0.7, or about 0.5 to about 1). It could be.

[0023] In the aqueous reaction mixture The molar ratio of water to Si is about 20 to about 100 (or about 20 to about 50, or about 40 to about 70, or about 50 to about 75, or about 70 to about 90, or about 80 to about 100). It could be.

[0024] OH -Acids and bases may be added to the aqueous reaction mixture to achieve the desired concentration of OH on alumina. - The higher the concentration, the more soluble the silica becomes, so the ratio of OH to Si becomes - It is believed that a high molar ratio of Si to Al reduces the molar ratio of Si to Al in the EMM-58 zeolite. OH vs. Si - The molar ratio is about 0.3 to about 1 (or about 0.3 to about 0.6, or about 0.5 to about 1). It could be.

[0025] Optionally, seeds can be included in the aqueous reaction mixture. The amount of seeds in the reaction mixture can be about 0.1% to about 10% by weight (or about 0.5% to about 7% by weight, or about 1% to about 5% by weight) based on the weight of the silicon atom source in the reaction mixture.

[0026] In some instances, at least a portion of the aluminum in EMM-58 zeolite can be released or removed from the structure to further increase the Si to Al ratio in EMM-58 zeolite. This can be accomplished by treating EMM-58 zeolite with acid or steam followed by acid. For example, EMM-58 zeolite can be exposed to acid at about 25° C. to about 80° C. (or 25° C. to about 50° C. or 45° C. to about 80° C.) for about 2 hours to about 36 hours (or about 2 hours to about 12 hours, or about 8 hours to about 24 hours, or about 12 hours to about 36 hours). In another example, EMM-58 zeolite can be exposed to water vapor and then exposed to acid at about 25° C. to about 80° C. (or 25° C. to about 50° C. or 45° C. to about 80° C.) for about 2 hours to about 36 hours (or about 2 hours to about 12 hours, or about 8 hours to about 24 hours, or about 12 hours to about 36 hours), and can be exposed to acid for about 2 hours to about 36 hours (or about 2 hours to about 12 hours, or about 8 hours to about 24 hours, or about 12 hours to about 36 hours). In these two examples, the resulting EMM-58 zeolite can be Si to Al ratio of about 3 to about 10 (or about 3 to about 8, or about 4 to about 6) The molar ratio may be:

[0027] Examples of acids suitable for treating EMM-58 zeolite include, but are not limited to, sulfuric acid, hydrochloric acid, acetic acid, nitric acid, and any combination thereof.

[0028] The EMM-58 zeolite of the present disclosure (as prepared or after treatment with acid or steam / acid) can be calcined (e.g., in air or another oxygen-containing gas) at a temperature of about 500° C. to about 900° C. (or 550° C. to about 850° C., or about 600° C. to about 800° C.). Calcination can be for about 10 minutes to about 8 hours (or about 30 minutes to about 5 hours, or about 1 hour to about 3 hours).

[0029] The EMM-58 zeolite of the present disclosure can have an average diameter of about 0.1 microns to about 25 microns (or about 1 micron to about 15 microns or about 3 microns to about 10 microns). The particle size can be determined by imaging the crystals with a scanning electron microscope and averaging the diameters of at least 100 crystals. The crystals have a faceted shape. Thus, the diameter is defined as the maximum distance from one side to the other side through the center of the crystal.

[0030] The EMM-58 zeolite of the present disclosure has a molecular weight of about 350 m 2 / g~about 700m 2 / g (or about 350m 2 / g~about 550m 2 / g or about 500m 2 / g~about 700m 2 / g. Surface area is determined using Brunauer, Emmett and Teller (BET) analysis by nitrogen adsorption (ASTM D4365-13).

[0031] The EMM-58 zeolite of the present disclosure has a thickness of about 0.15 cm 3 / g ~ approx. 0.30cm 3 / g(about 0.15cm 3 / g ~ approx. 0.25cm 3 / g or about 0.20 cm 3 / g ~ approx. 0.30cm 3 / g) Micropore volume as determined by nitrogen adsorption according to ASTM D4365-13.

[0032] The EMM-58 zeolite of the present disclosure can have a characteristic X-ray diffraction (XRD) pattern, the essential (most intense) reflections of which can be seen in Table 1 (synthetic form) and Table 2 (calcined form). In the tables, d is the range in which the peak intensities are specified. Once specified, the relative peak areas are measured and normalized with the maximum peak area being 100. That is, the ranges provided are not necessarily the ranges used to measure the relative percent areas.

[0033] [Table 1]

[0034] [Table 2]

[0035] application The EMM-58 zeolite of the present disclosure can be used as a catalyst to promote one or more organic compound conversion processes, including many of current commercial / industrial importance. Examples of organic compound conversion processes (e.g., hydrocarbon conversion processes) include, but are not limited to, cracking, hydrocracking, disproportionation, transalkylation, alkylation, and isomerization. Such catalysts can include (a) EMM-58 zeolite and (b) rare earth metals and / or metals from Groups 2 to 15 of the Periodic Table of the Elements. As used herein, the numbering of the Periodic Table Groups is as disclosed in Chemical and Engineering News, 63(5), 27 (1985).

[0036] The EMM-58 zeolite and metals may be formed into a catalyst by known methods, including, but not limited to, co-crystallization, exchange onto the EMM-58 zeolite structure, impregnation onto the EMM-58 zeolite structure, intimate physical incorporation, and the like, and any combination thereof.

[0037] As with many catalysts used in organic compound (hydrocarbon) conversion processes, it may be desirable to incorporate EMM-58 zeolite into another material that is resistant to the temperatures and other conditions utilized in the organic conversion process. Such materials may include active and inactive materials, as well as synthetic or naturally occurring zeolites, and inorganic materials such as clays, silica and / or metal oxides such as alumina. The latter may be naturally occurring or in the form of gelatinous precipitates or gels including mixtures of silica and metal oxides. The use of materials together with EMM-58 zeolite tends to alter the conversion and / or selectivity of the catalyst in a particular organic conversion process. Inactive materials can be advantageously used as diluents to control the amount of conversion in a given process so that products can be obtained in an economical and orderly manner without utilizing other (more expensive) means to control the reaction rate. These materials can be incorporated into naturally occurring clays (e.g., bentonite and kaolin) to improve the crush strength of the catalyst under commercial operating conditions. The materials (i.e., clays, oxides, etc.) can function as binders for the catalyst. In commercial use, it may be desirable to provide a catalyst with good crush strength, since it may be desirable to prevent the catalyst from breaking down into powder-like materials (attrition). These clay and / or oxide binders are usually utilized solely for the purpose of improving the crush strength of the catalyst.

[0038] Naturally occurring clays that can be composited with EMM-58 zeolite include, but are not limited to, the montmorillonite and kaolin families, including sub-bentonite and kaolin commonly known as Dixie, McNamee, Georgia, and Florida clays, or others whose major mineral component is halloysite, kaolinite, dickite, nacrite, or anauxite. Such clays can be used in their raw, as-mined state or after initial calcination, acid treatment, or chemical modification. Binders useful for composited with EMM-58 zeolite can additionally or alternatively include inorganic oxides such as silica, zirconia, titania, magnesia, beryllia, alumina, and mixtures thereof.

[0039] Alternatively or in addition to the aforementioned materials, the EMM-58 zeolite may be composited with a porous matrix material such as silica-alumina, silica-magnesia, silica-zirconia, silica-thoria, silica-beryllia, silica-titania, and / or one or more ternary compositions such as silica-aluminum-thoria, silica-alumina-zirconia, silica-magnesia-zirconia.

[0040] The relative proportions of EMM-58 zeolite and inorganic oxide matrix can vary widely, with the EMM-58 zeolite content ranging from about 1% to about 90% by weight, more usually from about 2% to about 80% by weight of the composite, especially when the composite is prepared in the form of beads. Exemplary matrix content ranges can include from about 10% to about 50% by weight.

[0041] In another example, a catalyst comprising (a) EMM-58 zeolite and (b) rare earth metals and / or metals from Groups 2-15 of the Periodic Table of Elements (preferably cobalt, tungsten, vanadium or combinations thereof) may be useful for selective catalytic reduction. Nitrogen oxides (NOx) are produced, for example, by the reaction of nitrogen with oxygen in a combustion chamber under high temperature and pressure conditions. NOx can also be produced, for example, in fluid catalytic converters (FCC) and furnaces by the combustion of nitrogen from FCC feed, heating oil and / or fuel oil. Such nitrogen oxides can include any one or combination of nitric oxide and nitrogen dioxide. Various selective catalytic reduction methods have been developed to reduce NOx emissions. In general, selective catalytic reduction is a process that can reduce NOx to diatomic nitrogen and water. As a non-limiting example, ammonia (NH3) can be mixed into the exhaust stream in a catalytic reactor to act as a reducing agent (also commonly known as a "reductant"). NOx can react with ammonia in the presence of a catalyst to produce diatomic nitrogen and water. The efficiency of NOx reduction can vary with various parameters, such as temperature, exhaust flow rate, ratio of reductant to NOx, and the presence of other chemicals in the exhaust stream. One of the factors that influences the reduction efficiency is the catalyst selected.

[0042] Thus, the disclosed method for selective catalytic reduction of NOx includes providing an exhaust stream comprising an amount of NOx from a combustion operation. At least a portion of the exhaust stream and a reductant stream comprising ammonia are introduced into a catalytic reactor comprising at least one zeolite catalyst ((a) EMM-58 zeolite, and (b) a rare earth metal and / or a metal of Groups 2-15 of the Periodic Table of the Elements, preferably cobalt, tungsten, vanadium, or combinations thereof) to reduce the amount of NOx in the exhaust stream. And, the NOx-reduced exhaust stream is discharged from the catalytic reactor. Further, the system for selective catalytic reduction of NOx includes a conduit in fluid communication with a source of the exhaust stream comprising NOx from the combustion operation and a source of a reductant stream comprising ammonia. The system includes a catalytic reactor in fluid communication with the conduit and the source of the reductant stream. The catalytic reactor includes at least one zeolite catalyst including (a) EMM-58 zeolite and (b) a rare earth metal and / or a metal from Groups 2-15 of the Periodic Table of the Elements, preferably cobalt, tungsten, vanadium, or a combination thereof. The catalytic reactor is configured to receive at least a portion of the exhaust stream and the reductant stream at suitable operating conditions and reduce the amount of NOx in the streams. The system also includes an outlet in fluid communication with the catalytic reactor for directing the NOx-reduced exhaust stream from the catalytic reactor.

[0043] CO2 and / or N2 adsorption is another application of the EMM-58 zeolite described herein. The pores of the EMM-58 zeolite may be of a suitable size for the adsorption of CO2 and / or N2.

[0044] The EMM-58 zeolite described herein may also be useful in carbonylation reactions, which generally refer to reactions in which CO is incorporated into a substrate. Here, the EMM-58 zeolite may be used in acid form, ion-exchanged form, or in combination with transition metals (e.g., copper, silver, gold, nickel iridium, rhodium, platinum, palladium, cobalt, or combinations thereof). For example, dimethyl ether, dimethyl carbonate, or methanol reacted with carbon monoxide in the presence of EMM-58 zeolite may be useful in the production of at least one of ethanol, acetic acid, and methyl acetate.

[0045] The EMM-58 zeolite described herein is also useful in the reaction of organic oxygenates with ammonia to produce mono- and dialkylamines, particularly methylamine and dimethylamine. Examples of organic oxygenate compounds suitable for use in this reaction include alcohols having 1 to 3 carbon atoms, specifically methanol, ethanol, n-propanol and isopropanol, and their ether counterparts, including methyl ethyl ether, dimethyl ether, diethyl ether and diisopropyl ether. The reaction is preferably, but not exclusively, carried out in a gaseous fixed bed or fluidized bed flow system, and the molar ratio of ammonia to oxygenate is generally from about 0.5 to about 20, for example from about 1 to about 5. Reaction conditions typically include a temperature of about 200° C. to about 400° C. (or about 250° C. to about 360° C.), a pressure of about 0.1 MPa to about 10 MPa (or about 0.5 MPa to about 2 MPa), and a reaction time of about 100 hours. -1 ~Approx. 10,000 hours -1 Includes Gas Hourly Space Velocity (GHSV).

[0046] Exemplary embodiments A first non-limiting exemplary embodiment of the present disclosure has (a) a monoclinic space group C2 / m with unit cell dimensions of 13.6 Å + / - 5%, b 21.7 Å + / - 5%, c 6.7 Å + / - 5%, and β of 93° + / - 3°, (b) a 12-ring cavity with dimensions along the c-axis of 7 Å + / - 5% by 6 Å + / - 5%, and (c) an 8-ring cavity with dimensions along the a-axis of 3 Å + / - 5% by 3 Å + / - 5%. Si to Al ratio of about 3 to about 10 A first non-limiting exemplary embodiment may include one or more of the following: Element 1: a composition having, in as-synthesized form, an X-ray diffraction pattern including d-spacings (d(Å)) and peak relative percentage areas according to Table 1; Element 2: a composition having, in calcined form, an X-ray diffraction pattern including d-spacings (d(Å)) and peak relative percentage areas according to Table 2; Element 3. a composition further including one or more selected from the group consisting of mordenite, DON-type zeolite, analcime, quartz, and cristobalite; Element 4: a composition in which the aluminosilicate zeolite is a hydrogenating metal. Examples of combinations include, but are not limited to, a combination of Element 1 with Element 3, Element 4, or Element 3 and 4; a combination of Element 2 with Element 3, Element 4, or Element 3 and 4; and a combination of Element 3 and 4.

[0047] The composition of the first non-limiting exemplary embodiment in combination with element 4 (and optionally one or more of elements 1-3) may be useful in a process comprising carrying out in the presence of said composition a hydrocarbon conversion process selected from the group consisting of cracking, hydrocracking, disproportionation, alkylation and isomerization.

[0048] A second non-limiting exemplary embodiment of the present disclosure is an aluminosilicate zeolite having a coordination series of T atoms of T1 4 10 19 32 48 69 98 126 154 192; T2 4 11 17 30 48 72 100 125 150 186; T3 4 10 20 32 47 69 96 126 159 191; and T4 4 10 19 31 48 71 97 125 156 189. The second non-limiting exemplary embodiment is an aluminosilicate zeolite having a coordination series of T atoms of T1 4 10 19 32 48 69 98 126 154 192; T2 4 11 17 30 48 72 100 125 150 186; T3 4 10 20 32 47 69 96 126 159 191; and T4 4 10 19 31 48 71 97 125 156 189. Si to Al ratio of about 3 to about 10 and element 6: the aluminosilicate zeolite may include one or more of: (a) a monoclinic space group C2 / m with unit cell dimensions of 13.6 Å+ / -5% a, 21.7 Å+ / -5% b, 6.7 Å+ / -5% c and β of 93°+ / -3°, (b) a 12-ring pore with dimensions of 7 Å+ / -5%×6 Å+ / -5% along the c-axis, and (c) an 8-ring pore with dimensions of 3 Å+ / -5%×3 Å+ / -5% along the a-axis. Examples of combinations include, but are not limited to, combinations of element 1 with one or more of elements 3-6; combinations of element 2 with one or more of elements 3-6; and combinations of two or more of elements 3-6.

[0049] The composition of the second non-limiting exemplary embodiment in combination with element 4 (and optionally one or more of elements 1-3 and 5-6) may be useful in a process comprising carrying out in the presence of said composition a hydrocarbon conversion process selected from the group consisting of cracking, hydrocracking, disproportionation, alkylation and isomerization.

[0050] A third non-limiting exemplary embodiment of the present disclosure provides a method for producing a silicon-based cation exchange polymer comprising: (i) maintaining an aqueous reaction mixture comprising a silicon atom source, an aluminum atom source, and a structure directing agent selected from the group consisting of N,N',2-trimethylbenzimidazolium, N,N',2-dimethylbenzimidazolium, and combinations thereof, at a temperature of about 135°C to about 180°C; Si to Al ratio of about 3 to about 10and (ii) providing an aluminosilicate zeolite having (a) a monoclinic space group C2 / m with unit cell dimensions of a 13.6 Å + / - 5%, b 21.7 Å + / - 5%, c 6.7 Å + / - 5% and β of 93° + / - 3°, (b) a 12-ring pore with dimensions along the c-axis of 7 Å + / - 5% by 6 Å + / - 5%, and (c) an 8-ring pore with dimensions along the a-axis of 3 Å + / - 5% by 3 Å + / - 5%.

[0051] A fourth non-limiting exemplary embodiment of the present disclosure provides a method for producing a fluorinated ... providing an aluminosilicate zeolite having a coordination series of 189 T atoms.

[0052] A third or fourth non-limiting exemplary embodiment is Element 7: The aqueous reaction mixture Si to Al ratio is about 2 to about 50 Element 8: the aqueous reaction mixture has a molar ratio of Si to structure directing agent of about 0.1 to about 1 Element 9: the aqueous reaction mixture has a molar ratio of Molar ratio of water to silicon between about 20 and about 100Element 10: wherein the silicon atom source is selected from the group consisting of a colloidal suspension of silica, precipitated silica alkali metal silicates, tetraalkyl orthosilicates, different Si-containing zeolites, and any combination thereof; Element 11: wherein the aluminum atom source is selected from the group consisting of aluminum nitrate, aluminum sulfate, sodium aluminate, aluminum oxide, alumina sol, alumina trihydrate, clay, another Al-containing zeolite, and any combination thereof; Element 12: wherein the temperature is from about 150°C to about 170°C; Element 13: wherein the method further comprises maintaining the aqueous reaction mixture at from about 135°C to about 180°C for from about 20 days to about 36 days; Element 14: wherein the aqueous reaction mixture further comprises seeds having the structure of an aluminosilicate zeolite. Element 15: maintaining the aqueous mixture further provides one or more selected from the group consisting of mordenite, DON type zeolite, analcime, quartz, and cristobalite; Element 16: in the as-synthesized form, the X-ray diffraction pattern of the aluminosilicate zeolite has d-space and peak relative percentage areas according to Table 1; Element 17: the method further comprises treating the aluminosilicate zeolite with acid or steam followed by acid; Element 18: the method comprises calcining the aluminosilicate zeolite at 500°C to 900°C to produce a calcined aluminosilicate zeolite; Element 19: may further comprise one or more of Element 18 and the calcined aluminosilicate zeolite has an X-ray diffraction pattern having d-space and peak relative percentage areas according to Table 2. Examples of combinations include, but are not limited to, combinations of two or more of elements 7-9; combinations of one or more of elements 7-9 with one or more of elements 10-13; combinations of element 14 with one or more of elements 7-13; combinations of element 15 with one or more of elements 7-14; combinations of element 16 with one or more of elements 7-15; combinations of element 17 with one or more of elements 7-16; and combinations of element 18 (and optionally element 19) with one or more of elements 7-17.

[0053] Numerical ranges used herein are inclusive of the numbers recited in the range, for example, the numerical range "1% to 10% by weight" includes the 1% and 10% by weight numbers within the stated range.

[0054] Unless otherwise indicated, all numerical values ​​expressing quantities of ingredients, properties such as molecular weight, reaction conditions, and the like used in the specification and related claims are understood to be modified in all instances by the term "about." Accordingly, unless indicated to the contrary, the numerical parameters set forth in the following specification and appended claims are approximations that may vary depending upon the desired properties sought to be obtained by embodiments of the present invention. At the very least, no attempt is made to limit the application of the doctrine of equivalents to the scope of the claims, and each numerical parameter should, at the very least, be construed in light of the number of reported significant digits and by applying ordinary rounding techniques.

[0055] One or more exemplary embodiments incorporating embodiments of the invention disclosed herein are presented. For clarity, not all features of a physical implementation are described or shown in this application. It is understood that in developing a physical embodiment incorporating an embodiment of the invention, numerous implementation-specific decisions must be made to achieve the developer's goals, such as complying with system-related, business-related, government-related and other constraints, which vary from implementation to implementation and from time to time. Although the developer's efforts may be time-consuming, such efforts would nevertheless be routine for one of ordinary skill in the art and having the benefit of this disclosure.

[0056] Although compositions and methods are described herein in terms of "comprising" various components or steps, the compositions and methods can also "consist essentially of" or "consist of" the various components and steps.

[0057] To facilitate a better understanding of the embodiments of the present invention, the following examples of preferred or representative embodiments are given. The following examples should not be read to limit or define the scope of the invention. EXAMPLES

[0058] Example 1. A silica atom source, an aluminum atom source, sodium hydroxide, N,N',2-trimethylbenzimidazolium (SDA) and optionally EMM-58 zeolite seeds were combined according to Table 3. For samples 2 and 5, HCl was added at a molar ratio of 0.25 HCl:Si to produce a net OH. - The OH:Si molar ratio was decreased. - The :Si molar ratio was 0.31.

[0059] [Table 3]

[0060] Sample 1 yielded primarily the EMM-58 zeolite of the present disclosure with minor mordenite contamination. Sample 2 yielded primarily the EMM-58 zeolite of the present disclosure with minor quartz contamination. Sample 3 yielded a mixture of mordenite and quartz. Sample 4 yielded an anathyme zeolite. Sample 5 yielded nearly pure EMM-58 zeolite of the present disclosure. Sample 6 yielded nearly pure EMM-58 zeolite of the present disclosure. Sample 7 yielded an EMM-58 zeolite with a Si to Al molar ratio of 4.

[0061] Figure 1 is an SEM image of Sample 5 showing EMM-58 zeolite and minor layered phase impurities. Figures 2A and 2B are SEM images of Sample 6 showing essentially pure EMM-58 zeolite. Figure 3 is a plot containing the XRD patterns of Sample 6 as prepared (bottom) and after calcination at 540°C in air for 1 hour (top).

[0062] Three additional samples were prepared according to Table 4.

[0063] [Table 4]

[0064] Thus, the present invention is well adapted to attain the objects and advantages mentioned, as well as those inherent therein. The particular embodiments disclosed above are illustrative only, as the invention may be modified and practiced in different but equivalent manners apparent to those skilled in the art having the benefit of the teachings herein. Moreover, no limitations are intended to the details of construction or design shown herein, other than as set forth in the following claims. It is therefore apparent that the particular exemplary embodiments disclosed above may be altered, combined or modified, and all such variations are considered to be within the scope and spirit of the invention. The invention illustratively disclosed herein may suitably be practiced in the absence of any element not specifically disclosed herein and / or any optional element disclosed herein. Although the compositions and methods are described in terms "comprising," "containing," or "comprising" various components or steps, the compositions and methods may also "consist essentially of" or "consist of" the various components and steps. All of the numerical values ​​and ranges disclosed above may vary by some amount. Whenever a numerical range with a lower and upper limit is disclosed, any numerical value falling within that range and any included range is specifically disclosed. In particular, any numerical range disclosed herein (in the form of "about a to about b," or equivalently, "about a to b," or equivalently, "about a to b") is understood to define any numerical value and range encompassed within the broader numerical range. Additionally, the terms set forth in the claims have their plain and ordinary meaning unless expressly and specifically defined by the patentee. Additionally, the indefinite article "a" or "an" used in the claims is defined herein to mean one or more of the element it introduces.

[0065] All priority documents are hereby incorporated by reference in their entirety for all jurisdictions in which such incorporation is permitted. Additionally, all documents cited herein, including testing procedures, are hereby incorporated by reference in their entirety for all jurisdictions in which such incorporation is permitted.

Claims

1. 1. A composition comprising: an aluminosilicate zeolite having a molar ratio of Si to Al that is between 3 and 10, having (a) a monoclinic space group C2 / m with unit cell dimensions of a 13.6 Å + / - 5%, b 21.7 Å + / - 5%, c 6.7 Å + / - 5% and β of 93° + / - 3°, (b) a 12-ring pore with dimensions along the c-axis of 7 Å + / - 5% by 6 Å + / - 5%, and (c) an 8-ring pore with dimensions along the a-axis of 3 Å + / - 5% by 3 Å + / - 5%.

2. 10. The composition of claim 1, in its as-synthesized form, having an X-ray diffraction pattern with the following d-spacings (d(Å)) and relative percent areas of peaks: 【Table 1】

3. 2. The composition of claim 1, in the calcined form, having an X-ray diffraction pattern comprising the following d-spacings (d(Å)) and relative percent areas of peaks: 【Table 2】

4. 2. The composition of claim 1, further comprising one or more selected from the group consisting of mordenite, DON-type zeolite, analcime, quartz, and cristobalite.

5. 10. The composition of claim 1, wherein the aluminosilicate zeolite further comprises a hydrogenation metal.

6. A process comprising carrying out a hydrocarbon conversion process in the presence of the composition according to any one of claims 1 to 5, said hydrocarbon conversion process being selected from the group consisting of cracking, hydrocracking, disproportionation, alkylation and isomerization.

7. Aluminosilicate zeolites having a coordination series of T atoms of: T1 4 10 19 32 48 69 98 126 154 192; T2 4 11 17 30 48 72 100 125 150 186; T3 4 10 20 32 47 69 96 126 159 191; and T4 4 10 19 31 48 71 97 125 156 189.

8. 5. A method for preparing the composition of any one of claims 1 to 4, comprising maintaining an aqueous reaction mixture comprising a source of silicon atoms, a source of aluminum atoms, and a structure directing agent selected from the group consisting of N,N',2-trimethylbenzimidazolium, N,N',2-dimethylbenzimidazolium, and combinations thereof, and having a molar ratio of water to Si of 70 to 100, at a temperature of 135°C to 180°C.

9. The aqueous reaction mixture comprises Si to Al, which is 2 to 50; A structure directing agent for Si, which is 0.1 to 1; Water for Si of 80-100 9. The method of claim 8, wherein the molar ratio of

10. 9. The method of claim 8, wherein the silicon atom source is selected from the group consisting of colloidal suspensions of silica, precipitated silica alkali metal silicates, tetraalkyl orthosilicates, different Si-containing zeolites, and any combination thereof.

11. 9. The method of claim 8, wherein the aluminum atom source is selected from the group consisting of aluminum nitrate, aluminum sulfate, sodium aluminate, aluminum oxide, alumina sol, alumina trihydrate, clay, another Al-containing zeolite, and any combination thereof.

12. The method of claim 8, wherein the temperature is between 150°C and 170°C.

13. 9. The method of claim 8, further comprising maintaining the aqueous reaction mixture at 135° C. to 180° C. for 20 to 36 days.

14. 9. The method of claim 8 further comprising treating the aluminosilicate zeolite with acid or steam followed by acid.

15. 9. The method of claim 8, further comprising calcining the aluminosilicate zeolite at 500° C. to 900° C. to produce a calcined aluminosilicate zeolite.

Citation Information

Patent Citations

  • A method for preparing ultraporous silicate molecular sieves

    CN107892309B

  • Super-macroporous silicate molecular sieve NUD-6 and preparation method thereof

    CN111348662A

  • Zeolite synthesis and directing agents

    JP2022504239A

  • Highly siliceous forms of zeolite RHO

    JP2022511672A

  • Zeolite syntheses and directing agents

    US20200109058A1