Filament manufacturing method

By cooling filaments in a water tank with decreasing temperature, the method effectively reduces bubble formation and maintains roundness, improving the quality of 3D printed objects.

JP7587128B2Active Publication Date: 2024-11-20KYORAKU CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020215793
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-11-20
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Air and moisture trapped in resin materials used for manufacturing filaments lead to air bubbles in the filament, which degrade the quality of 3D printed objects.

Method used

A method involving an extrusion step followed by a cooling and winding process, where the filament is cooled in a water tank with decreasing water temperature from the inlet to the outlet, ensuring the filament is slowly solidified to minimize bubble formation and maintain roundness.

Benefits of technology

The method produces filaments with high roundness and reduced bubble formation, enhancing the quality of 3D printed objects by minimizing air bubbles during extrusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587128000002
    Figure 0007587128000002
  • Figure 0007587128000003
    Figure 0007587128000003
  • Figure 0007587128000004
    Figure 0007587128000004
Patent Text Reader

Abstract

To provide filaments with high roundness and few bubbles.SOLUTION: The invention provides a method for manufacturing filaments, comprising an extrusion process and a cooling and winding process. In the extrusion process, a melt-mixed raw material resin composition is continuously extruded from an extruder through a mouthpiece to form filaments, and in the cooling and winding process, the filaments are passed through water in a water tank to be cooled and solidified and then wound up. The water temperature in the water tank decreases with distance from the entrance of the water tank.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for manufacturing a filament that can be used in a fused deposition model 3D printer. [Background technology]

[0002] Patent Document 1 discloses a fused deposition model 3D printer in which a filament is extruded from a head and layered and deposited.

[0003] It is important that the filament used in this type of 3D printer has a constant wire diameter and is nearly a perfect circle. In Patent Document 2, a filament is produced by continuously extruding a molten and kneaded resin material from an extruder through a die, and then cooling and solidifying the extruded filament and winding it up. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2009-500194 [Patent Document 2] Japanese Patent Application Laid-Open No. 2016-193601 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the resin material used to manufacture the filament usually contains residual air and moisture, which can cause bubbles to form in the filament. If the filament contains bubbles, the linear molten resin extruded from the 3D printer head will also contain bubbles, leading to a decrease in the quality of the object obtained by 3D printing.

[0006] The present invention has been made in view of the above circumstances, and aims to provide a filament with high circularity and few bubbles. [Means for solving the problem]

[0007] According to the present invention, there is provided a method for producing a filament, comprising an extrusion step and a cooling and winding step, in which a melt-kneaded raw material resin composition is continuously extruded from an extruder through a die to form a filament, and in the cooling and winding step, the filament is cooled and solidified by passing it through water in a water tank, and then wound up, the temperature of the water in the water tank decreasing with increasing distance from the inlet of the water tank.

[0008] The inventor discovered that by setting the temperature of the water in the tank so that the temperature of the water in the tank decreases with increasing distance from the inlet of the tank, filaments with high circularity and few bubbles can be obtained, and thus completed the present invention.

[0009] Preferably, in the method described above, when the length that the filament passes through the water in the water tank is L and the difference in temperature between the water that the filament first comes into contact with in the water tank and the water that the filament comes into contact with just before leaving the water tank is ΔT, ΔT / L is 3°C / m or more. Preferably, in the method described above, the water tank has first to fourth zones in this order from the inlet side of the water tank, the filament passes through the first to fourth zones in this order, and when the temperatures of the water in the first to fourth zones are T1 to T4, respectively, T1≧T2≧T3≧T4. [Brief explanation of the drawings]

[0010] [Figure 1] 1 shows the configuration of a production line 30 for a filament 10 according to one embodiment of the present invention. [Figure 2] FIG. 2 is an exploded perspective view of the sizing device 33. [Figure 3] 2 is a cross-sectional view of the water tank 37 and its surrounding structure in FIG. 1, taken along a horizontal plane passing through the center of the filament 10. FIG. DETAILED DESCRIPTION OF THE INVENTION

[0011] The following describes embodiments of the present invention. The various features shown in the following embodiments can be combined with each other. Furthermore, each feature can be an independent invention.

[0012] 1. Filament 10 production line 30 First, a manufacturing line 30 for the filament 10 that can be used to implement the manufacturing method for the filament 10 according to one embodiment of the present invention will be described with reference to FIG.

[0013] As shown in FIG. 1, the production line 30 for the filament 10 includes an extruder 31, a die 32, a sizing device 33, a water tank 37, a fixed roller 41, an outer diameter measuring device 42, and a winding device 43.

[0014] The extruder 31 melts and kneads the raw material resin composition and continuously supplies it to the die 32, and is configured, for example, with a cylinder containing a screw, a hopper 31a for inputting the raw material, an injection nozzle, etc. The screw of the extruder 31 is not particularly limited, but is preferably a single-axis screw. The extruder 31 melts and kneads the raw material resin composition by rotating the screw in the cylinder, and extrudes it from the injection nozzle into the die 32. The raw material can be input in the form of pellets.

[0015] The die 32 extrudes the molten resin from the extruder 31 in the horizontal direction, and the molten resin extruded from here is cooled to become the filament 10.

[0016] The water tank 37 is formed in a box shape that is long along the conveyance direction of the filament 10. The filament 10 is introduced into the water tank 37 from the wall at one end of the water tank 37 and is discharged from the wall at the other end of the water tank 37. The water tank 37 stores water 37a in which the filament 10 is immersed and which cools the filament 10.

[0017] The sizing device 33 is disposed inside the wall at one end of the water tank 37. The sizing device 33 has the function of increasing the roundness of the filament 10 and uniformizing the outer diameter of the filament 10 to a predetermined dimension.

[0018] The sizing device 33 shapes the filament 10 by vacuum suction, thereby improving the roundness. The sizing device 33 can be omitted if not required.

[0019] As shown in FIG. 2, the sizing device 33 includes a pair of upper and lower members, a lower member 33D and an upper member 33U. The mating surfaces of the lower member 33D and the lower member 33U are provided with a semi-cylindrical first groove 33a formed along the conveying direction of the continuous filament 10, through which the filament 10 passes, and a plurality of second grooves 33b for vacuum suction (seven grooves arranged parallel to each other in this example) that intersect perpendicularly with the first groove 33a. The number of second grooves 33b for vacuum suction is optional and may be set appropriately so as to ensure sufficient shaping accuracy of the filament 10 after passing through the sizing device 33. The second grooves 33b for vacuum suction may be arranged in any direction, such as a horizontal direction, a vertical direction, or an oblique direction, and may be set appropriately so as to ensure sufficient shaping accuracy.

[0020] In the sizing device 33, vacuum suction is performed, and a vacuum suction force acts on the filament 10. As a result, the outer peripheral surface of the filament 10 is attracted to the wall surfaces facing the circular cross-sectional space of the groove 33a provided in the lower member 33D and the upper member 33U, and is shaped to the shape and diameter of the space formed by the groove 33a. As a result, the filament 10 that has passed through the sizing device 33 has a cross section that is approximately circular, and its diameter becomes constant and approximately coincides with the set value (diameter of the space).

[0021] The fixed roller 41 stabilizes the posture of the filament 10 in the water tank 37 after passing through the sizing device 33, and transports the filament 10 toward the winding device 43 side.

[0022] As shown in FIG. 3, the water tank 37 is divided into a plurality of zones Z1 to Z4 by partition plates 37b. The zones Z1 to Z4 are arranged in this order from the inlet 37c side of the water tank 37. The filament 10 passes through the zones Z1 to Z4 in this order and is cooled and solidified as it passes through. Each of the zones Z1 to Z4 is provided with a heater and a temperature sensor (not shown), allowing the water temperature to be independently controlled. The partition plates 37b are configured to allow the filament 10 to pass through and to suppress the movement of water between the zones. The number of zones is two or more, for example, 2 to 10, specifically, for example, 2, 3, 4, 5, 6, 7, 8, 9, or 10, and may be within a range between any two of the numerical values ​​exemplified here or any number greater than or equal to any one of the values ​​exemplified here.

[0023] The outer diameter measuring device 42 measures the outer diameter of the filament 10 cooled in the water tank 37. The winding device 43 includes a pair of upper and lower winding rollers 43a that sandwich the filament 10 that has passed through the outer diameter measuring device 42 and transport it downstream, and a bobbin winding machine 43b that is disposed downstream of the winding rollers 43a and has a winding shaft 43c that winds the filament 10.

[0024] 2. Filament manufacturing method Next, a method for manufacturing the filament 10 according to one embodiment of the present invention will be described. The following description will be given with reference to the manufacturing line 30, but the method according to this embodiment may be carried out using an apparatus other than the manufacturing line 30.

[0025] The method of this embodiment includes an extrusion step, a sizing step, a cooling step, and a winding step, each of which will be described in detail below.

[0026] (1) Extrusion process In the extrusion step, the melt-kneaded raw resin composition is continuously extruded from an extruder 31 through a die 32 to form the filament 10 .

[0027] The raw resin composition contains a thermoplastic resin and may contain additives. Examples of the thermoplastic resin include amorphous resins such as ABS resin, polystyrene, polyvinyl chloride, polymethyl methacrylate, polycarbonate, and modified polyphenylene ether, polyolefin resins such as polyethylene and polypropylene, crystalline resins such as polyester, polyamide, and polyvinyl alcohol, olefin-based, styrene-based, polyester-based, and urethane-based thermoplastic elastomers, and mixtures thereof.

[0028] Examples of additives include inorganic additives such as carbon black, carbon fiber, glass fiber, talc, mica, nanoclay, and magnesium, antioxidants, lubricants, and colorants.

[0029] The filament 10 may have a single layer structure or a multilayer structure. In the case of a multilayer structure, for example, the filament 10 includes a core and a covering layer covering the core. The core and the covering layer can each be formed using the raw resin composition described above. The multilayer filament 10 can be formed by co-extruding the raw resin compositions melt-kneaded and extruded in a plurality of extruders, which are then joined together in a die 32.

[0030] If the diameter of the filament 10 extruded from the nozzle 32 is D1, then D1 is, for example, 1.5 to 4 mm, and more specifically, for example, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, or 4.0 mm, and may be within a range between any two of the numerical values ​​exemplified here.

[0031] (2) Sizing process In the sizing process, the filament 10 extruded from the spinneret 32 ​​is passed through a sizing device 33 while being vacuum-suctioned. This improves the roundness of the filament 10 and uniforms the outer diameter of the filament 10 to a predetermined size. The sizing process can be omitted if it is not necessary.

[0032] If the diameter of the filament 10 immediately after passing through the sizing device 33 is D2, the value of (D1-D2) is, for example, 0 to 1 mm, preferably 0.1 to 1 mm, specifically, for example, 0, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 mm, and may be within a range between any two of the values ​​exemplified here.

[0033] (3) Cooling and winding process In the cooling and winding step, the filament 10 is passed through water in a water tank 37 to be cooled and solidified, and then wound around a winding shaft 43c.

[0034] The diameter of the filament 10 is reduced by cooling in the water bath 37. If the diameter of the filament 10 immediately after cooling in the water bath 37 is D3, the value of (D3 - D1) is, for example, 0.01 to 0.5 mm, specifically, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, specifically, for example, 0.1, 0.2, 0.2, 0.3, 0.3, 0.4, 0.4, 0.5, 0.5 mm, and may be within a range between any two of the numerical values ​​exemplified here.

[0035] D3 is, for example, 1.3 to 3.8 mm, preferably 2.0 to 3.8 mm, and specifically, for example, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8 mm, and may be within a range between any two of the numerical values ​​exemplified here.

[0036] When D3 is less than 2.0 mm, air bubbles are relatively unlikely to occur in the filament 10, and even if they do occur, they are unlikely to be expelled from the head during 3D printing. On the other hand, when D3 is 2.0 mm or more, air bubbles are likely to occur in the filament 10, and the air bubbles that do occur are likely to be expelled from the head during 3D printing. Therefore, when D3 is 2.0 mm or more, the technical significance of suppressing the occurrence of air bubbles using the present invention is significant.

[0037] In this embodiment, the temperature of the water in the water tank 37 is set to decrease with increasing distance from the inlet 37c of the water tank 37. Setting the water temperature in this manner suppresses the generation of bubbles in the filament 10 and also suppresses a decrease in the roundness of the filament 10. Bubbles in the filament 10 are generated when the interior of the filament 10 contracts and becomes decompressed after the surface of the filament 10 is rapidly cooled and solidified. When the temperature of the water in the water tank 37 is set as described above, the timing at which the surface of the filament 10 solidifies is delayed, making it difficult for the interior of the filament 10 to become decompressed, and suppressing the generation of bubbles.

[0038] If the length of the filament 10 passing through the water in the water bath 37 is L, and the difference between the temperature of the water that the filament 10 first comes into contact with in the water bath 37 (T1, in this embodiment, the temperature of the water in the first zone Z1) and the temperature of the water that the filament 10 comes into contact with just before leaving the water bath 37 (T4, in this embodiment, the temperature of the water in the fourth zone Z4) is ΔT (=T1-T4), ΔT / L is preferably 3°C / m or more. If this value is too small, the roundness of the filament 10 is likely to decrease or air bubbles are likely to occur in the filament 10. ΔT / L is, for example, 3 to 15°C / m, and specifically, for example, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15°C / m, and may be within a range between any two of the values ​​exemplified here or equal to or greater than any of them. ΔT is, for example, 10 to 50° C., specifically, for example, 10, 15, 20, 25, 30, 35, 40, 45, or 50° C., and may be within a range between any two of the values ​​exemplified here. L is, for example, 1 to 10 m, specifically, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 m, and may be within a range between any two of the values ​​exemplified here.

[0039] The speed at which the filament 10 passes through the water in the water tank 37 is, for example, 5 to 15 m / min. Specifically, this speed may be, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 m / min, or may be within a range between any two of the values ​​exemplified here.

[0040] The temperature of the water that the filament 10 first comes into contact with in the water tank 37 is, for example, 50 to 80°C. If this temperature is too low, bubbles are likely to form in the filament 10, and if this temperature is too high, the roundness of the filament 10 is likely to decrease. Specific examples of this temperature include 50, 55, 60, 65, 70, 75, and 80°C, and may be within a range between any two of the values ​​exemplified here. The temperature of the water that the filament 10 comes into contact with just before leaving the water tank 37 is, for example, 15 to 45°C. If this temperature is too low, bubbles are likely to form in the filament 10, and if this temperature is too high, the roundness of the filament 10 is likely to decrease. Specific examples of this temperature include 15, 20, 25, 30, 35, 40, and 45°C, and may be within a range between any two of the values ​​exemplified here.

[0041] If the temperatures of the water in the first to fourth zones Z1 to Z4 are T1 to T4, respectively, it is preferable that T1 ≥ T2 ≥ T3 ≥ T4, where "≥" means "=" or ">".

[0042] The filament 10 cooled in the water bath 37 may be wound onto the winding shaft 43c as is, or may be wound onto the winding shaft 43c after its outer diameter is measured by the outer diameter measuring device 42. In the latter case, if the obtained outer diameter is outside the standard width range, the manufacturing conditions can be revised so that the outer diameter falls within the standard width range. Once a predetermined length of the filament 10 has been wound onto the winding shaft 43c, a new filament 10 is wound onto the winding shaft 43c.

[0043] Through the above steps, the filament 10 wound around the winding shaft 43c can be manufactured.

[0044] The filament 10 preferably has an air bubble generation rate of 0 to 5%. The air bubble generation rate can be reduced by slowly cooling the filament 10 as in this embodiment. Specific examples of the air bubble generation rate are 0.0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, and 5.0%, and may be within a range between any two of the numerical values ​​exemplified here.

[0045] The bubble generation rate was calculated by cutting the filament 10 into 1 cm wide pieces to create more than 100 samples, visually inspecting the cut surfaces of the samples, and counting the number of samples in which bubbles with a diameter of 0.3 mm or more were found, based on the following formula. Bubble occurrence rate (%) = 100 x (number of samples in which bubbles were found) / (number of samples observed)

[0046] The filament 10 preferably has a circularity of 1.00 to 1.07. The circularity of a perfect circle is 1, and the closer the cross section of the filament 10 is to a perfect circle, the closer the circularity of the filament 10 is to 1 (a circularity closer to 1 is expressed as "high circularity"). By slowly cooling the filament 10 as in this embodiment, the circularity can be made closer to 1. Specifically, the circularity of the filament 10 is, for example, 1.00, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, or 1.07, and may be within a range between any two of the numerical values ​​exemplified here.

[0047] The circularity of the filament 10 can be measured by the following method. First, the maximum and minimum lengths passing through the center of the filament 10 are measured at each cross section of the filament 10 at three or more measurement points (the distance between adjacent measurement points is 10 cm), and the circularity (= maximum length / minimum length) at each measurement point is calculated. The filament 10 is approximately elliptical, and the maximum and minimum lengths correspond to the major and minor axis lengths of the ellipse. The average value of the circularity at all measurement points is taken as the circularity of the filament 10. [Example]

[0048] A filament 10 made of ABS resin was produced using a production line 30. The spinneret 32 ​​and sizing device were set so that D1 to D3 were 3.00 mm, 2.90 mm, and 2.85 mm, respectively. The lengths of zones Z1 to Z4 were each 0.75 m. The water temperatures in zones Z1 to Z4 were set as shown in Table 1. The passing speed of the filament 10 through the water tank 37 was 7.2 m / min. The bubble generation rate and circularity of the filament 10 obtained in each example and comparative example were measured. The results are shown in Table 1.

[0049] [Table 1]

[0050] As shown in Table 1, the filaments 10 of all Examples had high circularity and low bubble generation rates. On the other hand, the filaments 10 of all Comparative Examples had high bubble generation rates or low circularity. This result indicates that by setting the temperature of the water in the water tank 37 so that the temperature of the water in the water tank 37 decreases with increasing distance from the inlet 37c of the water tank 37, a filament 10 with high circularity and few bubbles can be obtained. [Explanation of symbols]

[0051] 10: Filament 30: Production line 31: Extruder 31a: Hopper 32: Cap 33: Sizing device 33D: Lower member 33U: Upper member 33a: First groove 33b: Second groove 37: Aquarium 37a: water 37b: Partition board 37c: Entrance 41: Fixed roller 42: Outer diameter measuring device 43: Winding device 43a: Winding roller 43b: Bobbin winding machine 43c: Winding shaft Z1: Zone 1 Z2: Second Zone Z3: Zone 3 Z4: Zone 4

Claims

1. A method for producing a filament, comprising the steps of: The method includes an extrusion process, and a cooling and winding process. In the extrusion step, the melt-kneaded raw resin composition is continuously extruded from an extruder through a die to form filaments; In the cooling and winding step, the filament is cooled and solidified by passing it through water in a water tank, and then wound up. the temperature of the water in the tank decreases with increasing distance from the inlet of the tank; Let L be the length that the filament passes through the water in the water tank, and ΔT be the difference in temperature between the water that the filament first comes into contact with in the water tank and the water that the filament comes into contact with just before it leaves the water tank. The method, wherein ΔT / L is 3° C. / m or more and 10° C. / m or less.

2. 2. The method of claim 1 , The water tank includes first to fourth zones in this order from an inlet side of the water tank, The filament passes through the first to fourth zones in this order; If the temperatures of the water in the first to fourth zones are T1 to T4, respectively, The method, wherein T1≧T2≧T3≧T4.

3. A method according to claim 1 or claim 2, comprising: The temperature of the water with which the filament comes into contact immediately before leaving the water tank is 35° C. or more and 45° C. or less; The temperature of the water that the filament first comes into contact with in the water tank is 50° C. or higher and 80° C. or lower; The water tank is divided into a plurality of zones by partitions, the partition plate is configured to allow the filaments to pass through and to inhibit the movement of the water between the zones; The water tank includes first to fourth zones in this order from an inlet side of the water tank, The filament passes through the first to fourth zones in this order; If the temperatures of the water in the first to fourth zones are T1 to T4, respectively, T1 ≧ T2 ≧ T3 ≧ T4, The method, wherein the speed at which the filaments pass through the water in the water tank is 5 m / min or more and 15 m / min or less.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing thermoplastic resin molded product

    JP1995001556A

  • Synthetic resin wire and manufacture thereof

    JP1997066550A

  • Rapid prototyping system with controlled raw materials

    JP2009500194A

  • Resin composition for molding and filament for molding

    JP2016037571A

  • Polylactic acid strand

    JP2016060048A