Plastic containers

A plastic container with a polyolefin and pulverized woody biomass composite layer adjacent to a gas barrier layer addresses the adhesive strength issue, simplifying manufacturing and reducing costs by eliminating the need for an adhesive layer.

JP7587129B2Active Publication Date: 2024-11-20KYORAKU CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020218989
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-11-20
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Existing plastic containers with biomass content require a gas barrier layer and an adhesive layer due to the low adhesive strength of materials like ethylene-vinyl alcohol copolymers with polyolefin layers, increasing manufacturing complexity and costs.

Method used

A plastic container design with a composite layer of polyolefin and pulverized woody biomass adjacent to a gas barrier layer, eliminating the need for an additional adhesive layer by leveraging the high adhesiveness between these layers.

Benefits of technology

Ensures sufficient adhesive strength between the composite and gas barrier layers without additional adhesive layers, simplifying the manufacturing process and reducing costs while maintaining environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587129000002
    Figure 0007587129000002
  • Figure 0007587129000003
    Figure 0007587129000003
  • Figure 0007587129000001
    Figure 0007587129000001
Patent Text Reader

Abstract

To provide a plastic container having a composite layer containing polyolefin and woody biomass pulverized material and a gas barrier layer, which secures sufficient adhesive strength while suppressing complication of a layer structure.SOLUTION: A plastic container 1 contains: a composite layer 4 containing a polyolefin and a woody biomass pulverized material and arranged outside a gas barrier layer 3; a polyolefin layer arranged further outside the composite layer; and a gas barrier layer containing an ethylene-vinyl alcohol copolymer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plastic container for containing ground wood biomass. [Background technology]

[0002] In recent years, also in the field of synthetic resin molded products, composite materials containing biomass materials (paper powder, wood powder, bamboo powder, etc.) and synthetic resins have been used as an environmentally friendly measure.

[0003] Patent Document 1 discloses a plastic container in which cellulose contained in the biomass material is mixed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-234443 A Summary of the Invention [Problem to be solved by the invention]

[0005] The plastic container described in Patent Document 1 has a three-layer structure of a polyolefin layer / a cellulose-containing polyolefin layer / a polyolefin layer.

[0006] On the other hand, many plastic containers available on the market have a gas barrier resin such as an ethylene-vinyl alcohol copolymer as an intermediate layer to prevent deterioration of the contents due to oxygen in the air. Therefore, it is desirable to provide a gas barrier layer in the same manner for biomass-containing plastic containers such as those described in Patent Document 1.

[0007] However, many gas barrier resins, such as ethylene-vinyl alcohol copolymers and polyamides, do not have sufficient adhesive strength when adjacent to a polyolefin layer, making it necessary to provide an adhesive layer between the two, such as an acid-modified polyolefin, which leads to more complex molding machines and increased manufacturing costs.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to introduce a gas barrier layer into a wood-based biomass-containing plastic container while preventing the layer structure from becoming too complicated. [Means for solving the problem]

[0009] According to the present invention, there is provided a plastic container comprising a composite layer containing polyolefin and ground wood biomass, and a gas barrier layer, characterized in that the composite layer and the gas barrier layer are adjacent to each other.

[0010] As a result of intensive research, the present inventors have discovered that a composite layer containing a polyolefin and ground wood biomass has high adhesion to a gas barrier layer. They have also discovered that in a plastic container having a gas barrier layer, sufficient adhesive strength can be ensured without providing an adhesive layer by arranging the composite layer and the gas barrier layer adjacent to each other, and have completed the present invention.

[0011] Preferably, the composite layer is disposed on the outer side of the gas barrier layer. Preferably, a polyolefin layer is disposed on the outer side of the composite layer. Preferably, the gas barrier layer comprises an ethylene-vinyl alcohol copolymer. Effect of the Invention

[0012] According to the present invention, in a plastic container having a composite layer containing polyolefin and pulverized wood biomass, and a gas barrier layer, the composite layer and the gas barrier layer are adjacent to each other, thereby making it possible to ensure sufficient adhesive strength without providing an adhesive layer between them. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram of a plastic container shown as an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the layer structure of a plastic container shown as an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, embodiments of the present invention will be described. Note that the embodiments described below are intended to provide a better understanding of the gist of the invention, and do not limit the present invention unless otherwise specified.

[0015] 1 is a schematic diagram of a plastic container according to an embodiment of the present invention. The plastic container 1 according to this embodiment is used by being filled with, for example, food products such as beverages and seasonings, or pharmaceutical products such as detergents and medicines.

[0016] The plastic container 1 can be formed by blow molding a parison having a multi-layer structure, which will be described later. The blow molding may be direct blow molding or injection blow molding. In direct blow molding, a container is manufactured by sandwiching a molten parison extruded from an extruder between a pair of split dies and blowing air into the parison. In injection blow molding, a test tube-shaped parison with a bottom, called a preform, is formed by injection molding, and the parison is used to manufacture a container by blow molding. The molding temperature when molding the plastic container 1 is preferably 200° C. or lower, and more preferably 180° C. or lower, in order to prevent discoloration of the ground wood biomass contained in the composite layer described below.

[0017] The plastic container 1 has a multi-layer structure. Fig. 2 shows a typical example of the layer structure of the plastic container 1, which includes, from the inside surface side of the plastic container 1, an inner layer 2, a gas barrier layer 3, a composite layer 4, and an outer layer 5.

[0018] <Inner layer 2> The inner layer 2 may have a single layer structure or a multi-layer structure. In this embodiment, the inner layer 2 includes, in order from the inner surface side of the plastic container 1, an innermost layer 2a and an adhesive layer 2b. The inner layer 2 may include layers other than those shown here, or may not include some of the layers shown here. For example, when the adhesion between the innermost layer 2a and the gas barrier layer 3 is high, the adhesive layer 2b can be omitted.

[0019] Examples of materials constituting the innermost layer 2a include polyolefins (e.g., polyethylene and polypropylene), polyesters (e.g., PET), ethylene-vinyl alcohol copolymers, and nylon. The innermost layer 2a may contain additives in addition to the materials listed here. Examples of additives include lubricants and fillers.

[0020] The adhesive layer 2b is composed of an adhesive resin. Examples of the adhesive resin include acid-modified polyolefin resins (e.g., maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene). By providing the adhesive layer 2b, the adhesion between the layers adjacent to the adhesive layer 2b is improved.

[0021] <Gas barrier layer 3> The gas barrier layer 3 is composed of a resin composition containing a gas barrier resin. Examples of the gas barrier resin include ethylene-vinyl alcohol copolymer, polyamide resin, and polyester resin. Among these, it is preferable to use an ethylene-vinyl alcohol copolymer as a resin that has particularly excellent barrier properties against oxygen and aroma components. The resin composition constituting the gas barrier layer 3 may contain only the gas barrier resin, or may contain polyolefin and the like as a resin component in addition to the gas barrier resin.

[0022] The ethylene-vinyl alcohol copolymer may be any known ethylene-vinyl alcohol copolymer. For example, a saponified copolymer obtained by saponifying an ethylene-vinyl acetate copolymer having an ethylene content of 20 to 60 mol%, particularly 25 to 50 mol%, to a degree of saponification of 96 mol% or more, particularly 99 mol% or more may be used.

[0023] <Composite layer 4> The composite layer 4 is made of a resin composition in which pulverized wood biomass is blended with polyolefin.

[0024] Examples of the polyolefin constituting the composite layer 4 include polyethylenes such as low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), polypropylene, ethylene-propylene copolymers, polybutene-1, ethylene-butene-1 copolymers, propylene-butene-1 copolymers, etc. These may be used alone or in the form of a blend of two or more kinds.

[0025] The woody biomass pulverized material to be blended in the composite layer 4 may be a cellulose-based powder made by pulverizing at least one of hardwood pulp and softwood pulp into a powder using a pulverizer; a powder made by pulverizing broken or damaged paper generated during paper manufacturing into a powder using a pulverizer; a powder made by pulverizing waste paper into a powder using a pulverizer; or a powder made by mixing these materials in a predetermined ratio. The size of the woody biomass pulverized material is not particularly limited, but for example, a powder of 30 μm or less is used. The pulp may be any of mechanical pulp, chemical mechanical pulp, semi-chemical pulp, and chemical pulp. The waste paper may be newspaper waste, magazine waste, printing waste, packaging waste, cardboard waste, or office waste.

[0026] The content of the pulverized wood biomass in the composite layer 4 is preferably 30% by mass or more, and more preferably 40% by mass or more. If the content is less than 30% by mass, not only will the gas barrier layer 3 and the composite layer 4 not exhibit sufficient adhesive strength, but the effect of reducing the environmental load by blending the pulverized wood biomass will decrease. If the content of the pulverized wood biomass exceeds 70% by mass, holes or tears may occur in the parison when the plastic container 1 is blow molded, which is not preferable. Therefore, the content of the pulverized wood biomass is preferably 70% by mass or less. For the above reasons, the content of the pulverized wood biomass is preferably 30 to 70% by mass, and more preferably 40 to 60% by mass.

[0027] The gas barrier layer 3 and the composite layer 4 are adjacent to each other without an adhesive layer etc. The adhesive strength between the gas barrier layer 3 and the composite layer 4 varies depending on the usage environment and application of the plastic container 1, but is preferably, for example, 150 gf / 15 mm or more, and more preferably 200 gf / 15 mm or more.

[0028] <Outer layer 5> The outer layer 5 is composed of a resin composition containing a polyolefin. Examples of the polyolefin constituting the outer layer 5 include polyethylene, polypropylene, and an ethylene-propylene copolymer. In particular, from the viewpoint of the adhesive strength between the composite layer 4 and the outer layer 5, it is preferable to use the same polyolefin as that constituting the composite layer 4 as the polyolefin constituting the outer layer 5.

[0029] In the various layer configurations described above, the thickness of each layer may be set appropriately depending on the application of the plastic container 1 so that the characteristics of each layer are fully exhibited.

[0030] In the present invention, the fact that the composite layer and the gas barrier layer have high adhesion as described above is a phenomenon that was discovered as a result of many experiments, and is unpredictable from Patent Document 1 and other known techniques. Although the exact reason has not been clarified, the present inventors presume that it is due to the following reasons.

[0031] In general, the adhesive strength between a gas barrier layer in a multilayer plastic container and a resin layer adjacent to the gas barrier layer is strengthened by chemical interaction between the two. In particular, when the resin layer adjacent to the gas barrier layer has a polar group such as an OH group, hydrogen bonds are formed between the polar group and the polar group contained in the gas barrier layer, and the adhesive strength is greatly improved.

[0032] In other words, in the present invention, since the cellulose, hemicellulose, and lignin, which are components of the pulverized wood-based biomass material contained in the composite layer 4, have a large number of OH groups, it is presumed that hydrogen bonds are formed between these OH groups and the polar groups contained in the gas barrier layer 3, making it possible to obtain high adhesion.

[0033] In the plastic container of the present invention, the components in the above embodiment may be replaced with any components as long as the composite layer containing polyolefin and ground woody biomass and the gas barrier layer are adjacent to each other. For example, in the above embodiment, the composite layer 4 is disposed on the outside of the gas barrier layer 3, which has the effect of preventing the odor derived from the woody biomass constituting the composite layer 4 from transferring to the contents filled in the plastic container 1. However, the composite layer 4 may be disposed on the inside of the gas barrier layer 3. EXAMPLES

[0034] The present invention will now be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to these examples.

[0035] (1) Preparation of plastic container 1 <Example 1> A plastic container 1 having the layer structure shown in FIG. 2 was produced by direct blow molding at a molding temperature of 190°C.

[0036] The layers of the plastic container 1 were made from the following materials. Innermost layer 2a / Outer layer 5: Polypropylene 1 (Sumitomo Chemical Co., Ltd. Noble FSX16E9) Adhesive layer 2b: Acid-modified polypropylene (Mitsubishi Chemical Corporation, Modic P674V) Gas barrier layer 3: Ethylene-vinyl alcohol copolymer (Mitsubishi Chemical Corporation, Soarnol D2908) Composite layer 4: Paper powder-containing polypropylene (MAPKA KM-MB51-WP, manufactured by the Environmental Management Research Institute, paper powder content (weight ratio): 51%)

[0037] <Example 2> A plastic container 1 was produced in the same manner as in Example 1, except that a mixed resin of 59 mass% paper powder-containing polypropylene and 41 mass% polypropylene 2 (Noblen FH3315 manufactured by Sumitomo Chemical Co., Ltd.) was used as the composite layer 4 (the paper powder content (weight ratio) was 30%).

[0038] <Comparative Example 1> A plastic container 1 was produced in the same manner as in Example 2, except that the compounding ratio of the composite layer 4 was 39 mass % of paper powder-containing polypropylene and 61 mass % of polypropylene 2 (paper powder content (weight ratio) was 20%).

[0039] <Comparative Example 2> A plastic container 1 was produced in the same manner as in Example 1, except that polypropylene 2 was used as the composite layer 4 .

[0040] (2) Evaluation The following evaluations were carried out for the above Examples and Comparative Examples. The results are shown in Table 1. From these results, it can be seen that by using paper powder-containing polypropylene for the composite layer 4, the adhesive strength with the gas barrier layer 3 is improved, and it is preferable that the paper powder content is 30 mass % or more.

[0041] [Table 1]

[0042] <Adhesive strength> A measurement sample was cut from the body of the produced plastic container 1, and a Tensilon universal material testing machine (manufactured by A&D Corporation) was used to measure the test force when peeling the gas barrier layer 3 and composite layer 4. The adhesive strength indicates the test force in a T-shaped peel when the edge of the sample was peeled off, the two sides of the peeled surface were clamped with a chuck, and the sample was peeled off for 40 mm at a speed of 300 mm / min. ○:150gf / 15mm or more ×: Less than 150gf / 15mm [Explanation of symbols]

[0043] 1: Plastic container 2: Inner layer 2a: Innermost layer 2b: Adhesive layer 3: Gas barrier layer 4: Composite layer 5: Outer layer

Claims

1. A composite layer comprising polyolefin and ground wood biomass; A gas barrier layer; A plastic container comprising: The composite layer and the gas barrier layer are adjacent to each other, A plastic container, wherein the content of the pulverized wood biomass material in the composite layer is 30% by mass or more and 51% by mass or less.

2. The composite layer is disposed on the outer side of the gas barrier layer. The plastic container of claim 1.

3. A polyolefin layer is disposed on the outer side of the composite layer. The plastic container according to claim 2.

4. The gas barrier layer contains an ethylene-vinyl alcohol copolymer. The plastic container according to any one of claims 1 to 3.

5. The size of the woody biomass pulverized material is 30 μm or less. The plastic container according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Pollution-free heat insulation container

    JP1999348958A

  • Pouch

    JP2002052668A

  • Container made of composite material

    JP2002293317A

  • Cellulose-containing container

    JP2014234443A

  • Adhesive resin composition and laminate

    JP2017082033A