Refrigerant Transport Hose
The refrigerant transport hose addresses weight and permeability issues by using a thermoplastic resin composition with a sea-island structure, ensuring low gas permeability and durability for automotive air conditioners.
Patent Information
- Application Number
- JP2023538392
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-01
- Filing Date
- 2022-07-08
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2042-07-08
AI Technical Summary
Existing refrigerant transport hoses in automobile air conditioners face challenges in reducing weight while maintaining low permeability to gases such as refrigerant and water vapor, and are not durable enough for long-term use in hot and humid environments.
A refrigerant transport hose composed of an outer layer made of thermoplastic resin composition A with a sea-island structure containing polyolefin resin and butyl elastomer, and an inner layer made of thermoplastic resin composition B with a sea-island structure containing polyamide resin and butyl elastomer, which reduces permeability and enhances flexibility and durability.
The hose achieves low water vapor and refrigerant permeability, is lightweight, and maintains flexibility and durability, with improved processability and reduced moisture absorption, thereby enhancing its performance in automotive applications.
Smart Images

Figure 0007587192000005 
Figure 0007587192000006 
Figure 0007587192000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hose for transporting refrigerant used in an air conditioner of an automobile. [Background technology]
[0002] In order to comply with carbon dioxide emission regulations, weight reduction of automobiles has become an important issue. For this reason, weight reduction is also required for refrigerant transport hoses used in air conditioners mounted on automobiles. If the inner and outer layers constituting the hose are made thinner to reduce weight, there is a risk that the permeability of the transported refrigerant and gases such as oxygen and water vapor may decrease. For this reason, it has been proposed to replace the constituent material of the inner layer from rubber to a polyamide-based resin composition with excellent gas permeability (see, for example, Patent Documents 1 and 2).
[0003] Since air conditioners and the like are installed in a limited narrow space in an automobile, refrigerant transport hoses are required to be highly flexible and easy to install in a narrow space. Furthermore, they are required to be durable enough to withstand long-term use in a high-temperature, high-humidity environment in an engine room. However, the resin hose described in Patent Document 1 and the refrigerant transport piping described in Patent Document 2 are made of a polyamide-based resin composition, so there is a concern about the water vapor permeability to moisture outside the hose, and there is a risk of gas permeability decreasing due to moisture absorption of the polyamide-based resin composition. Therefore, there is room for improvement in obtaining a refrigerant transport hose that is lightweight and highly flexible while reducing the permeability of the refrigerant being transported and the water vapor permeability of moisture outside the hose. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 2013-155793 [Patent Document 2] Japanese Patent Application Publication No. 2021-46490 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a hose for transporting a refrigerant which has low permeability to gases such as refrigerants and water vapor, and which is flexible and lightweight. [Means for solving the problem]
[0006] The hose for transporting a refrigerant of the present invention which achieves the above-mentioned object comprises at least an outer layer, a reinforcing layer and an inner layer, the outer layer having at least a layer made of thermoplastic resin composition A, and the inner layer having at least a layer made of thermoplastic resin composition B, the thermoplastic resin composition A has a sea-island structure with thermoplastic resin a as a matrix and elastomer a as domains, the thermoplastic resin a containing at least a polyolefin-based resin, the elastomer a containing at least a butyl-based elastomer, the elastomer a containing 51 to 85 mass% of elastomer a in 100 mass% of thermoplastic resin composition A, the thermoplastic resin composition B having a sea-island structure with thermoplastic resin b as a matrix and elastomer b as domains, the thermoplastic resin b containing at least a polyamide-based resin, and the elastomer b containing at least a butyl-based elastomer. Effect of the Invention
[0007] The refrigerant transport hose of the present invention has an outer layer made of a thermoplastic resin composition A containing a polyolefin resin, which reduces the water vapor permeability of moisture outside the hose, and an inner layer made of a thermoplastic resin composition B containing a polyamide resin, which reduces the permeability of the transported refrigerant. Furthermore, the outer layer, which has excellent low water vapor permeability, can be made thin, and the inner layer, which has excellent low refrigerant permeability, can be made thin, which allows the hose to be made lighter. Moreover, the thermoplastic resin composition A and the thermoplastic resin composition B have a sea-island structure with a butyl-based elastomer as a domain, which allows the hose to have excellent flexibility.
[0008] The refrigerant transport hose preferably contains 51 to 85 mass % of elastomer b in 100 mass % of the thermoplastic resin composition B, making the hose more flexible.The refrigerant transport hose preferably does not have a layer made of vulcanized rubber, making it possible to improve the productivity of the refrigerant transport hose.
[0009] The fluorocarbon permeability coefficient of the thermoplastic resin composition B is preferably smaller than that of the thermoplastic resin composition A, which can efficiently reduce the permeability of the fluorocarbons transported by the hose and suppress the occurrence of blisters. On the other hand, the water vapor permeability coefficient of the thermoplastic resin composition A is preferably smaller than that of the thermoplastic resin composition B, which can suppress the permeation and diffusion of moisture from the outside of the hose, prevent the inner layer containing a polyamide resin from absorbing moisture, and maintain low permeability of fluorocarbons.
[0010] In the thermoplastic resin composition A, the thermoplastic resin a preferably contains at least a polypropylene resin, and the elastomer a preferably contains at least a halogenated butyl rubber, so that the hose can have excellent flexibility while being less permeable to moisture from the outside. In the thermoplastic resin composition B, the thermoplastic resin b preferably contains at least a polyamide 6 resin, and the elastomer b preferably contains at least a halogenated isobutylene-paramethylstyrene copolymer rubber, so that the hose can have excellent flexibility while being less permeable to the refrigerant being transported. Furthermore, it is preferable that a part of the domain of the thermoplastic resin composition A and / or a part of the domain of the thermoplastic resin composition B are crosslinked, so that the durability of the outer layer and / or the inner layer can be increased.
[0011] The hose for transporting refrigerant may have a water-based adhesive, a solvent-based adhesive, a chemical reaction adhesive, or a hot melt adhesive interposed between the outer layer and the reinforcing layer and / or between the inner layer and the reinforcing layer, thereby making it possible to further increase the durability of the hose.
[0012] The thermoplastic resin composition A was subjected to a shear rate of 243.2 s- at 250°C. 1It is preferable that the melt viscosity at 200°C or less is 1000 Pa s, which can improve the extrusion processability when molding the outer layer. It is preferable that the thermoplastic resin a contains one or more thermoplastic resins having a melting point of 150°C or more, and the thermoplastic resin b contains one or more thermoplastic resins having a melting point of 200°C or more, which can improve the processability when extruding the outer layer around the outer periphery of the extruded inner layer.
[0013] The thermoplastic resin composition A has a tensile stress at 10% deformation of 10 MPa or less and a water vapor permeability coefficient of 3.0 g mm / (m 2 The thermoplastic resin composition B has a tensile stress of 10 MPa or less at 10% deformation and an oxygen permeability coefficient of 0.05 cm or less. 3 mm / (m 2 Therefore, it is possible to provide the inner layer with a high level of both low permeability to the refrigerant and flexibility.
[0014] The thermoplastic resin composition A may have a tensile breaking strength of 3 MPa or more and a tensile breaking elongation of 200% or more at 23°C, so that the durability of the outer layer at room temperature or normal temperature can be ensured. The thermoplastic resin composition A may have a tensile breaking strength of 0.4 MPa or more and a tensile breaking elongation of 50% or more at 150°C, so that the durability of the outer layer at high temperatures can be ensured. Furthermore, the thermoplastic resin composition A and the thermoplastic resin composition B may have an Izod impact strength of -40°C that is non-destructive, so that the durability of the outer layer and the inner layer at low temperatures can be ensured. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is an explanatory view illustrating a cross section of a hose for transporting a refrigerant according to the present invention. [Diagram 2] FIG. 2 is an explanatory diagram illustrating a method for measuring the flexibility of a hose. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The refrigerant transport hose of the present invention refers to a hose for transporting refrigerants, used in automobile air conditioners, etc. Examples of refrigerants include hydrofluorocarbons (HFCs), hydrofluoroolefins (HFOs), hydrocarbon compounds, carbon dioxide, ammonia, water, etc. Examples of HFCs include R410A, R32, R404A, R407C, R507A, and R134a. Examples of HFOs include R1234yf, R1234ze, R1233zd, R1123, R1224yd, and R1336mzz. Examples of hydrocarbon compounds include methane, ethane, propane, propylene, butane, isobutane, pentane, heptafluoropropane, and hexafluoropropane.
[0017] FIG. 1 is an explanatory diagram illustrating a cross section of a hose for transporting a refrigerant. The hose for transporting a refrigerant 1 is composed of at least an outer layer 3, a reinforcing layer 4, and an inner layer 2, with the outer layer 3 being disposed on the outer periphery of the reinforcing layer 4, and the inner layer 2 being disposed on the inner periphery of the reinforcing layer 4. The outer layer 3 and the inner layer 2 are each configured in a cylindrical shape. A plurality of reinforcing layers 4 may be provided, in which case the inner layer 2 is disposed on the inner periphery of the innermost reinforcing layer 4, and the outer layer 3 is disposed on the outer periphery of the outermost reinforcing layer 4. In addition, layers other than the outer layer 3, the reinforcing layer 4, and the inner layer 2 include an adhesive layer, a barrier layer, a rubber layer, and the like. The adhesive layer may be interposed between the outer layer 3 and the reinforcing layer 4 and / or between the inner layer 2 and the reinforcing layer 4.
[0018] The outer layer 3 of the refrigerant transport hose has at least a layer made of thermoplastic resin composition A, and may have, on the inner peripheral side and / or the outer peripheral side thereof, a layer other than the layer made of thermoplastic resin composition A. The properties of the layer other than the layer made of thermoplastic resin composition A are not particularly limited as long as they do not impede the object of the present invention.
[0019] The inner layer 2 of the refrigerant transport hose has at least a layer made of thermoplastic resin composition B, and may have, on the inner peripheral side and / or the outer peripheral side thereof, a layer other than the layer made of thermoplastic resin composition B. The properties of the layer other than the layer made of thermoplastic resin composition B are not particularly limited as long as they do not impede the object of the present invention.
[0020] The thermoplastic resin composition A constituting the outer layer has a sea-island structure with the thermoplastic resin a as the matrix and the elastomer a as the domain. The sea-island structure refers to a dispersion form in which the matrix is a sea phase (continuous phase) and the domain is an island phase (discontinuous phase, dispersed phase). The shape of the domain is not particularly limited and may be any of a sphere, an ellipsoid, a cylinder, a needle, and an indefinite shape. The dispersion form of the thermoplastic resin composition A can be observed by a scanning probe microscope (SPM) or the like on a cross section perpendicular to the extrusion grain direction. The observation magnification can be appropriately determined according to the size of the domain.
[0021] The thermoplastic resin a includes at least a polyolefin resin. The thermoplastic resin a may be only a polyolefin resin or may be a blend with other thermoplastic resins. By including a polyolefin resin, the water vapor permeability can be reduced and improved. Examples of the polyolefin resin include polyethylene resin, polypropylene resin, polybutene resin, etc. Among them, polypropylene resin is preferable. By including a polypropylene resin in the thermoplastic resin a, it is possible to provide both low water vapor permeability and heat resistance. Examples of the polypropylene resin include propylene homopolymer, propylene-ethylene block copolymer, propylene-ethylene-1-butene block copolymer, propylene-ethylene random copolymer, propylene-1-butene random copolymer, propylene-ethylene-1-butene random copolymer, propylene-ethylene random block copolymer, and propylene-ethylene-1-butene random block copolymer. Among them, propylene homopolymer, propylene-ethylene block copolymer, and propylene-ethylene random copolymer are preferable. The polyolefin resin may at least partially contain a modified polyolefin resin having a functional group such as maleic anhydride. The polyolefin resin may be used alone or in combination.
[0022] Examples of thermoplastic resins other than polyolefin resins that can be contained in the thermoplastic resin a include polyamide resins, polyester resins, polyvinyl alcohol resins, polyketone resins, etc. These may be blended alone or in combination with the polyolefin resin. When blending other thermoplastic resins, the polyolefin resin should be 51% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more, based on 100% by mass of the thermoplastic resin a.
[0023] The thermoplastic resin a preferably contains one or more thermoplastic resins having a melting point of 150°C or higher. By containing a thermoplastic resin having a melting point of 150°C or higher, the heat resistance required for the hose is improved. The melting point of the polyolefin resin and / or other thermoplastic resin is preferably 150°C or higher, more preferably 155 to 170°C, and more preferably 162 to 170°C. In this specification, the melting point of the thermoplastic resin is measured using a DSC method, and is the temperature of the endothermic peak accompanying melting during the temperature rise process.
[0024] The thermoplastic resin a is preferably 15 to 49 mass%, more preferably 15 to 40 mass%, and even more preferably 15 to 31 mass% in 100 mass% of the thermoplastic resin composition A. When the thermoplastic resin a is 15 mass% or more, a dispersed form of a sea-island structure in which the thermoplastic resin a serves as a matrix can be secured, and water vapor permeability can be reduced. Also, when the content is 49 mass% or less, flexibility can be secured.
[0025] The elastomer a includes at least a butyl-based elastomer. The elastomer a may be only a butyl-based elastomer, or may be a blend with other elastomers. By including a butyl-based elastomer, it is possible to provide both low water vapor permeability and flexibility. The butyl-based elastomer included in the elastomer a may be the same as or different from the butyl-based elastomer included in the elastomer b. Examples of the butyl-based elastomer include butyl rubber, halogenated butyl rubber, isobutylene-paramethylstyrene copolymer rubber, halogenated isobutylene-paramethylstyrene copolymer rubber, and styrene-isobutylene-styrene block copolymer rubber. Among them, the halogenated butyl rubber is preferable as the elastomer a. Examples of the halogenated butyl rubber include brominated butyl rubber and chlorinated butyl rubber. By including the halogenated butyl rubber in the elastomer a, the flexibility and water vapor permeability resistance of the hose are improved, and the durability is improved by dynamically crosslinking the elastomer during kneading of the thermoplastic resin composition A. The butyl-based elastomer may be used alone or in combination.
[0026] Examples of elastomers other than butyl-based elastomers that can be contained in elastomer a include olefin-based elastomers, styrene-based elastomers, urethane-based elastomers, ester-based elastomers, amide-based elastomers, and acrylic-based elastomers. These may be blended alone or in combination with the butyl-based elastomer. When blending other elastomers, the butyl-based elastomer should account for 51% by mass or more, preferably 75% by mass or more, and more preferably 95% by mass or more of the 100% by mass of elastomer a.
[0027] The elastomer a is 51 to 85 mass%, preferably 60 to 85 mass%, and more preferably 69 to 85 mass%, of 100 mass% of the thermoplastic resin composition A. When the elastomer a is 51 mass% or more, flexibility can be ensured. Also, when it is 85 mass% or less, a dispersed form of a sea-island structure in which the elastomer a becomes a domain can be ensured, and water vapor permeability can be reduced and excellent.
[0028] It is preferable that a part of the domain of the thermoplastic resin composition A is crosslinked. By crosslinking a part of the domain, the strength of the thermoplastic resin composition A can be increased, and the durability of the outer layer can be further increased. The method for crosslinking a part of the domain is not particularly limited, and examples thereof include dynamic crosslinking by adding a crosslinking agent and melt-kneading.
[0029] The thermoplastic resin composition A forming the outer layer was heated at 250°C and a shear rate of 243.2 s- 1 The melt viscosity at 200° C. is preferably 1000 Pa s or less. By setting the melt viscosity at 1000 Pa s or less, the processability during hose extrusion is improved. In this specification, the melt viscosity can be measured under specified conditions using a capillary rheometer.
[0030] The thermoplastic resin composition A preferably has a tensile stress at 10% deformation of 10 MPa or less, more preferably 1 to 9 MPa, and even more preferably 1 to 5 MPa. By having a tensile stress at 10% deformation of 10 MPa or less, the flexibility of the outer layer can be excellent.
[0031] The thermoplastic resin composition A has a tensile strength at break of preferably 3 MPa or more and a tensile elongation at break of preferably 200% or more at room temperature (23°C). By making the tensile strength at break 3 MPa or more and the tensile elongation at break 200% or more, the durability of the outer layer at room temperature (23°C) to normal temperature (20°C ± 15°C) can be ensured. The tensile strength at break is more preferably 3.5 MPa or more, and even more preferably 4 MPa or more. The tensile elongation at break is more preferably 250% or more, and even more preferably 300% or more.
[0032] The thermoplastic resin composition A has a tensile strength at break of preferably 0.4 MPa or more at 150°C and a tensile elongation at break of preferably 50% or more at 150°C. By making the tensile strength at break at 150°C 0.4 MPa or more and the tensile elongation at break at 150°C 50% or more, the durability of the outer layer at high temperatures can be ensured. The tensile strength at break at 150°C is more preferably 0.5 MPa or more. The tensile elongation at break at 150°C is more preferably 100% or more, and even more preferably 200% or more.
[0033] In this specification, the tensile stress at 10% deformation, the tensile strength at break at 23°C and 150°C, and the tensile elongation at break at 23°C and 150°C can be determined in accordance with the measurement method specified in JIS K6251 "Vulcanized rubber and thermoplastic rubber - Determination of tensile properties."
[0034] The thermoplastic resin composition A preferably has a non-destructive Izod impact strength at -40°C, and can ensure the durability of the outer layer at low temperatures. In this specification, the Izod impact strength at -40°C can be measured using a notched test piece in accordance with the measurement method specified in JIS K7110.
[0035] The thermoplastic resin composition A preferably has a water vapor permeability coefficient of 3.0 g mm / (m 2 ·24h) or less, preferably 1.0 to 3.0g·mm / (m 2 ·24h), and more preferably 1.0 to 2.0 g·mm / (m 2 The water vapor permeability coefficient of thermoplastic resin composition A is 3.0 g mm / (m 2 By setting the drying time to 24 h or less, the low water vapor permeability of the outer layer can be improved. In this specification, the water vapor permeability coefficient can be determined at a temperature of 60° C. and a relative humidity of 95% using a 0.2 mm thick sheet of the thermoplastic resin composition as a sample, as described in the Examples below.
[0036] The thermoplastic resin composition B constituting the inner layer has a sea-island structure with the thermoplastic resin b as the matrix and the elastomer b as the domain. The sea-island structure refers to a dispersion form in which the matrix is a sea phase (continuous phase) and the domain is an island phase (discontinuous phase, dispersed phase). The shape of the domain is not particularly limited and may be any of a sphere, an ellipsoid, a cylinder, a needle, and an indefinite shape. The dispersion form of the thermoplastic resin composition B can be observed with a scanning probe microscope (SPM) or the like on a cross section perpendicular to the extrusion grain direction. The observation magnification can be appropriately determined according to the size of the domain.
[0037] The thermoplastic resin b includes at least a polyamide resin. The thermoplastic resin b may be only a polyamide resin or may be a blend with other thermoplastic resins. By including a polyamide resin, oxygen permeability and refrigerant permeability can be reduced and improved. Examples of polyamide resins include polyamide 6 resin, polyamide 66 resin, polyamide 11 resin, polyamide 12 resin, polyamide 610 resin, polyamide 6 / 66 copolymer, polyamide 6 / 12 copolymer, polyamide 46 resin, polyamide 6T resin, polyamide 9T resin, polyamide MXD6 resin, etc. Among them, polyamide 6 resin is preferable. By including a polyamide 6 resin in the thermoplastic resin a, it is possible to provide low refrigerant permeability, low oxygen permeability, and heat resistance. The polyamide resin may be used alone or in combination.
[0038] Examples of thermoplastic resins other than polyamide-based resins that can be contained in thermoplastic resin b include polyolefin resins, polyester resins, polyvinyl alcohol resins, polyketone resins, etc. These may be blended alone or in combination with the polyamide-based resin. When blending other thermoplastic resins, the polyamide-based resin may account for 51% by mass or more, preferably 75% by mass or more, and more preferably 95% by mass or more of 100% by mass of thermoplastic resin b.
[0039] The thermoplastic resin b preferably contains one or more thermoplastic resins having a melting point of 200° C. or higher. By containing a thermoplastic resin having a melting point of 200° C. or higher, it is possible to provide heat resistance. The melting point of the polyamide resin and / or other thermoplastic resin is preferably 200° C. or higher, more preferably 200 to 280° C., and more preferably 210 to 280° C.
[0040] The thermoplastic resin b is preferably 15 to 49 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 39 mass% in 100 mass% of the thermoplastic resin composition B. When the thermoplastic resin b is 15 mass% or more, it is easy to ensure a dispersion form of a sea-island structure in which the thermoplastic resin b serves as a matrix, and it is possible to reduce the refrigerant permeability and oxygen permeability. Furthermore, when it is 49 mass% or less, flexibility can be ensured.
[0041] The elastomer b includes at least a butyl-based elastomer. The elastomer b may be only a butyl-based elastomer, or may be a blend with other elastomers. By including a butyl-based elastomer, it is possible to provide low oxygen permeability, low refrigerant permeability, and flexibility. The butyl-based elastomer contained in the elastomer b may be the same as or different from the butyl-based elastomer contained in the above-mentioned elastomer a. Examples of the butyl-based elastomer include butyl rubber, halogenated butyl rubber, isobutylene-paramethylstyrene copolymer rubber, halogenated isobutylene-paramethylstyrene copolymer rubber, and styrene-isobutylene-styrene block copolymer rubber. Among them, the halogenated isobutylene-paramethylstyrene copolymer rubber is preferable as the elastomer b. Examples of the halogenated isobutylene-paramethylstyrene copolymer rubber include brominated isobutylene-paramethylstyrene copolymer rubber and chlorinated isobutylene-paramethylstyrene copolymer rubber. By including the halogenated isobutylene-paramethylstyrene copolymer rubber in the elastomer b, the flexibility, oxygen permeation resistance, and refrigerant permeation resistance of the hose are improved, and the durability is improved by dynamically crosslinking the elastomer during kneading with the thermoplastic resin composition B. The butyl-based elastomer may be used alone or in combination.
[0042] Examples of elastomers other than butyl-based elastomers that can be contained in elastomer b include olefin-based elastomers, styrene-based elastomers, urethane-based elastomers, ester-based elastomers, amide-based elastomers, and acrylic-based elastomers. These may be blended alone or in combination with the butyl-based elastomer. When blending other elastomers, the butyl-based elastomer should account for 51% by mass or more, preferably 75% by mass or more, and more preferably 95% by mass or more of 100% by mass of elastomer b.
[0043] The elastomer b is preferably 51 to 85 mass%, more preferably 60 to 85 mass%, of 100 mass% of the thermoplastic resin composition B. When the elastomer b is 51 mass% or more, flexibility can be ensured. When the elastomer b is 85 mass% or less, a dispersed form of a sea-island structure in which the elastomer b becomes a domain can be ensured, and the refrigerant permeability and oxygen permeability can be reduced and improved.
[0044] It is preferable that a part of the domain of the thermoplastic resin composition B is crosslinked. By crosslinking a part of the domain, the strength of the thermoplastic resin composition B can be increased, and the durability of the inner layer can be further increased. The method for crosslinking a part of the domain is not particularly limited, and examples thereof include dynamic crosslinking by adding a crosslinking agent and melt-kneading.
[0045] The thermoplastic resin composition B has a tensile stress at 10% deformation of preferably 10 MPa or less, more preferably 1 to 9 MPa, and even more preferably 1 to 7 MPa. By having a tensile stress at 10% deformation of 10 MPa or less, the flexibility of the inner layer can be excellent. In addition, the thermoplastic resin composition B preferably has an Izod impact strength at -40°C that is non-destructive, and the durability of the inner layer at low temperatures can be ensured.
[0046] The thermoplastic resin composition B preferably has an oxygen permeability coefficient of 0.05 cm 3 mm / (m 2·day·mmHg) or less, more preferably 0.0001 to 0.02 cm 3 mm / (m 2 ·day·mmHg), more preferably 0.0001 to 0.01 cm 3 mm / (m 2 The oxygen permeability of thermoplastic resin composition B is 0.05 cm 3 mm / (m 2 By making the oxygen permeability coefficient (Hg) equal to or less than 1 / 2 day / mmHg, the oxygen permeability of the inner layer can be improved and at the same time the permeability of the refrigerant can be reduced. In this specification, the oxygen permeability coefficient can be determined under conditions of 21°C and 50 RH% using a 0.2 mm thick sheet of the thermoplastic resin composition as a sample, as described in the Examples below.
[0047] The fluorocarbon permeability coefficient of the thermoplastic resin composition B is preferably smaller than that of the thermoplastic resin composition A. This can efficiently reduce the permeability of the fluorocarbons transported by the hose, and suppress the occurrence of blisters. Therefore, the fluorocarbon permeability coefficient of the thermoplastic resin composition for the outer layer is preferably larger than that of the thermoplastic resin composition for the inner layer, and the ratio of the fluorocarbon permeability coefficient of the thermoplastic resin composition for the outer layer to that of the thermoplastic resin composition for the inner layer [outer layer / inner layer] is preferably 1.0 or more, more preferably 10 or more. In this specification, the fluorocarbon permeability coefficient can be determined from the amount of permeation at 80°C for 72 hours using a fluorocarbon HFO-1234yf, using a sheet of the thermoplastic resin composition with a thickness of 0.2 mm as a sample, as described in the examples described later.
[0048] On the other hand, the water vapor permeability coefficient of the thermoplastic resin composition A is preferably smaller than that of the thermoplastic resin composition B. This suppresses the permeation and diffusion of moisture from the outside of the hose, prevents the inner layer containing the polyamide resin from absorbing moisture, and maintains low permeability of fluorocarbons. Therefore, the water vapor permeability coefficient of the thermoplastic resin composition for the outer layer is preferably smaller than that of the thermoplastic resin composition for the inner layer, and the ratio of the water vapor permeability coefficient of the thermoplastic resin composition for the outer layer to that of the thermoplastic resin composition for the inner layer [outer layer / inner layer] is preferably less than 1.0, more preferably 0.4 or less.
[0049] The refrigerant transport hose comprises an outer layer having at least a layer made of thermoplastic resin composition A, a reinforcing layer, and an inner layer having a layer made of thermoplastic resin composition B. The outer diameter of the refrigerant transport hose is not particularly limited, but may be, for example, 4 to 30 mm, and the inner diameter is not particularly limited, but may be, for example, 3 to 25 mm.
[0050] The outer layer may be composed only of a layer made of the thermoplastic resin composition A, or may be laminated with other layers. The thickness of the outer layer is not particularly limited, but may be, for example, 0.5 to 4 mm.
[0051] The inner layer may be composed only of a layer made of the thermoplastic resin composition B, or may be laminated with other layers. The thickness of the inner layer is not particularly limited, but may be, for example, 0.2 to 3 mm.
[0052] The refrigerant transport hose has a reinforcing layer between the outer layer and the inner layer. By having the reinforcing layer, the strength of the hose can be ensured and the pressure resistance can be excellent. The thickness of the reinforcing layer is not particularly limited, but may be, for example, 0.3 to 3 mm.
[0053] The reinforcing material that can form the reinforcing layer is not particularly limited, and may be either an organic material or an inorganic material. For example, the organic material may be a polymer (fiber material), such as polyester, polyamide, aramid, vinylon, rayon, PBO (polyparaphenylene benzobisoxazole), polyketone, polyarylate, polyketone, etc. As the inorganic material, a metal may be used, such as a brass-plated wire or a zinc-plated wire. The reinforcing material may be surface-treated. The reinforcing layer is preferably made of polyester-based fiber, from the viewpoint of excellent fatigue resistance and cost performance.
[0054] The reinforcing layer (reinforcing material) may preferably be braided into a spiral structure and / or a braid structure, and may be either a single reinforcing layer or multiple reinforcing layers.
[0055] The hose for transporting refrigerant may have an adhesive layer between the outer layer and the reinforcing layer and / or between the inner layer and the reinforcing layer. The adhesive layer can increase the durability of the hose. The adhesive layer may be made of, for example, a water-based adhesive, a solvent-based adhesive, a chemical reaction adhesive, or a hot melt adhesive.
[0056] The refrigerant transport hose may have layers other than the outer layer, reinforcing layer, and inner layer, such as an adhesive layer, a barrier layer, and a rubber layer, but preferably does not have a layer made of vulcanized rubber. By not having a layer made of vulcanized rubber, the vulcanization step can be omitted, and the number of steps required to manufacture the refrigerant transport hose can be reduced, thereby improving productivity.
[0057] The refrigerant transport hose preferably has a moisture permeability of 1.5 mg / (cm 2 ·240h) or less, preferably 1.3mg / (cm 2 The moisture permeability of the refrigerant transport hose is 1.5mg / (cm 2When the moisture permeability is less than 1 / 240 h, the moisture and / or water vapor in the air is inhibited from penetrating and diffusing into the inside of the hose, the inner layer containing the polyamide resin is prevented from absorbing moisture, and low permeability of fluorocarbons can be maintained. In this specification, the moisture permeability of a hose for transporting refrigerants is measured at a temperature of 50°C and a relative humidity of 95% for 1 cm of the inner surface area of the hose. 2 The moisture permeability of a refrigerant transport hose is calculated by filling the hose with a weighed amount of desiccant and sealing the opening, leaving it in an atmosphere of 50°C and 95% relative humidity, measuring the increase in the mass of the desiccant after 120 hours and 360 hours, and dividing the increase in mass over 240 hours by the internal surface area of the test sample to obtain the moisture permeability [mg / (240h cm 2 )] was calculated.
[0058] The refrigerant transport hose preferably has a fluorocarbon HFO-1234yf permeation rate (hereinafter sometimes referred to as the "refrigerant permeation rate") of 10 kg / (m 2 ·year) or less, more preferably 3.0kg / (m 2 ·year) or less. The refrigerant permeability of the hose for transporting refrigerant is 3.0kg / (m 2 ·year), the refrigerant permeation rate of a hose for transporting refrigerant is suppressed when the refrigerant permeation rate is 1 m2 of the surface area of the inner periphery of the hose at 80°C. 2 This refers to the mass (kg) of refrigerant that permeates from the inner surface to the outer surface per year (8760 hours). The refrigerant permeation rate of refrigerant transport hoses was measured in accordance with SAE J2064 AUG2015. Each test sample was 1.07 m long and contained 1 cm of internal volume of the test sample. 3 The test sample was left in an atmosphere of 80°C for 25 days, and the mass loss (amount of refrigerant permeated) was measured during the last specified period (5 to 7 days) of the 25-day period. The mass loss was divided by the internal surface area of the test sample to obtain the refrigerant permeation amount [kg / (m 2 ·year) was calculated.
[0059] The method for producing the refrigerant transport hose is not particularly limited, and examples include a production method in which a prepared thermoplastic resin composition A is extruded into a cylindrical shape by extrusion molding to form an inner layer, a reinforcing layer and, optionally, an adhesive layer are formed on the outer peripheral surface of the inner layer, and then a prepared thermoplastic resin composition B is extruded into a cylindrical shape by extrusion molding on the outer peripheral surface of the reinforcing layer and, optionally, an adhesive layer are formed, to form an outer layer.
[0060] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES
[0061] Thermoplastic resin composition A and thermoplastic resin composition B shown in Tables 1-2 were prepared by the following method. First, butyl-based rubber was processed into pellets using a rubber pelletizer (manufactured by Moriyama Seisakusho Co., Ltd.). In preparing the thermoplastic resin compositions (A-1 to A-5, A'-6 to A'-8, B-1, B'-2 to B'3) having the blends shown in Tables 1-2, the materials were fed into a twin-screw kneading extruder (manufactured by The Japan Steel Works, Ltd.) in the blending ratios shown in Tables 1-2, and kneaded at 235°C for 3 minutes. The kneaded material was continuously extruded from the extruder in the form of a strand, cooled with water, and cut with a cutter to obtain pellet-shaped thermoplastic resin composition A and thermoplastic resin composition B. Dynamic crosslinking proceeds in the twin-screw kneading extruder.
[0062] The obtained pellets of the thermoplastic resin composition for the inner and outer layers were molded into sheets with an average thickness of 0.2 mm and 2 mm using a 40 mmφ single screw extruder with a 200 mm wide T-shaped die (manufactured by Plagiken Co., Ltd.) under conditions of a cylinder temperature and die temperature set to 10°C higher than the melting point of the component with the highest melting point in the thermoplastic resin composition, a cooling roll temperature of 50°C, and a take-up speed of 3 m / min. The 0.2 mm thick sheets were cut out and used to measure the water vapor permeability coefficient, oxygen permeability coefficient, and fluorocarbon permeability coefficient, tensile stress, tensile breaking strength at 23°C and 150°C, and tensile breaking elongation at 23°C and 150°C. The 2 mm thick sheets were also used to measure the Izod impact strength at -40°C.
[0063] The pellets of the thermoplastic resin composition B for the inner layer described above were extruded onto a mandrel previously coated with a release agent, with the cylinder temperature and die temperature set to 10°C higher than the melting point of the component with the highest melting point in the thermoplastic resin composition B, using a 40mmφ single-screw extruder with a die having an annular slit (manufactured by Plagiken Co., Ltd.), and a cylindrical inner layer was extruded to a thickness of 0.8 mm. An adhesive was applied to the outer periphery of the obtained inner layer, and polyester fibers were braided using a braiding machine to form a reinforcing layer, which was then further coated with an adhesive. Furthermore, the pellets of the thermoplastic resin composition A for the outer layer described above were extruded onto the outer periphery of the reinforcing layer, using a 40mmφ single-screw extruder with a die having an annular slit (manufactured by Plagiken Co., Ltd.), with the cylinder temperature and die temperature set to 10°C higher than the melting point of the component with the highest melting point in the thermoplastic resin composition A, and a cylindrical outer layer was extruded to a thickness of 0.4 mm. The mandrel was removed to produce a refrigerant transport hose (Examples 1 to 7, Comparative Examples 1 to 3) consisting of an inner layer, a reinforcing layer, and an outer layer. Note that none of the refrigerant transport hoses had a layer made of vulcanized rubber.
[0064] The obtained hose for transporting refrigerant was used to measure the presence or absence of blisters, and the amount of refrigerant permeated and the amount of water permeated through the hose for transporting refrigerant. The properties of the thermoplastic resin compositions for the inner and outer layers and the hose for transporting a refrigerant were measured by the following methods.
[0065] (1) Melt Viscosity of Thermoplastic Resin Composition for Outer Layer The thermoplastic resin composition was pre-dried at 100°C for 4 hours, and then measured at a temperature of 250°C and a shear rate of 243.2 s-1 using a capillary rheometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.) with a capillary of 10 mm in length and 1 mm in inner diameter. 1 The melt viscosity (Pa·S) was measured by detecting the load under the above conditions. The results are shown in Table 1.
[0066] (2) Water vapor permeability coefficient of the thermoplastic resin composition for the inner layer and the outer layer The thermoplastic resin composition obtained above was used as a sheet having a thickness of 0.2 mm, and the water vapor permeability coefficient (unit: g mm / (m)) was measured at a temperature of 60°C and a relative humidity of 95% using a water vapor permeability tester manufactured by GTR Tech Co., Ltd. 2 The water vapor permeability coefficient of the thermoplastic resin composition for the outer layer is shown in Table 1. The water vapor permeability coefficient of the thermoplastic resin composition for the inner layer was calculated by calculating the ratio [outer layer / inner layer] to the water vapor permeability coefficient of the thermoplastic resin composition for the outer layer. The ratios [outer layer / inner layer] of 0.4 or less were rated as "excellent," those between 0.4 and 1.0 were rated as "good," and those of 1.0 or more were rated as "poor." These are shown in Tables 3 and 4.
[0067] (3) Oxygen permeability coefficient of thermoplastic resin composition for inner layer and outer layer The thermoplastic resin composition obtained above was used as a sheet having a thickness of 0.2 mm, and the oxygen permeability coefficient (unit: cm) was measured at a temperature of 21°C and a relative humidity of 50% using OXTRAN 1 / 50 manufactured by MOCON. 3 mm / (m 2 The oxygen permeability coefficients of the thermoplastic resin compositions for the outer layer and the inner layer are shown in Table 1 and Table 2, respectively.
[0068] (4) Fluorocarbon permeability coefficient of thermoplastic resin composition for inner layer and outer layer The fluorocarbon permeability coefficient was measured using a 0.2 mm thick sheet of the thermoplastic resin composition obtained above (hereinafter referred to as the "sample sheet") and fluorocarbon HFO-1234yf. Fluorocarbon HFO-1234yf was placed in a stainless steel cup until half of the cup's capacity was reached, and the opening of the cup was sealed with the sample sheet using a specified tool so as to cover it. In this state, a static test was carried out at a temperature of 80°C for 72 hours. Before and after the static test, the mass of the cup containing fluorocarbon sealed with the sample sheet was measured to determine the mass of fluorocarbon lost, and the fluorocarbon permeability coefficient (unit: g mm / (72h cm) 2The results were calculated by calculating the ratio [outer layer / inner layer] of the fluorocarbon permeability coefficient of the thermoplastic resin composition for the outer layer to the fluorocarbon permeability coefficient of the thermoplastic resin composition for the inner layer, and the ratio [outer layer / inner layer] exceeding 10 was rated as "excellent," that exceeding 1.0 and not more than 10 was rated as "good," and that not more than 1.0 was rated as "poor." These results are shown in Tables 3 and 4.
[0069] (5) Tensile test properties of thermoplastic resin compositions for inner and outer layers A 0.2 mm thick sheet of the thermoplastic resin composition obtained above was punched out into a JIS No. 3 dumbbell shape, and a tensile test was performed at 23°C and 150°C at a tensile speed of 500 mm / min in accordance with the measurement method specified in JIS K6251 "Vulcanized rubber and thermoplastic rubber - Determination of tensile properties". From the obtained stress-strain curve, the tensile stress, tensile breaking strength, and tensile breaking elongation at 10% deformation at 23°C, and the tensile breaking strength and tensile breaking elongation at 150°C were measured. The obtained results are shown in Tables 1 and 2.
[0070] (6) Izod test properties of thermoplastic resin compositions for inner and outer layers The 2 mm thick sheet of the thermoplastic resin composition obtained above was processed into a notched test piece having a length of 63.5 mm, a width of 10 mm and a thickness of 2 mm in accordance with JIS K7110, and an Izod impact test was performed at -40°C. The results are shown in Tables 1 and 2. In addition, when the notched test piece did not break even after the Izod impact test, it is shown as "NB" in the table.
[0071] (7) Blisters in hoses for transporting refrigerants The refrigerant transport hose obtained above was observed to evaluate the presence or absence of blisters. The results are shown in Tables 3 and 4.
[0072] (8) Flexibility of refrigerant transport hoses As shown in Fig. 2, one end of the refrigerant transport hose in the longitudinal direction is fixed by a fixture such as a clamp, and a spring balance is attached at a position separated by a predetermined length L (120 + hose outer diameter / 2) × π [mm]) from the fixed position, and the refrigerant transport hose is bent in a semicircular arc from the state shown by the dashed line to the state shown by the solid line. Then, in the bent state where the hose inner radius R is 120 mm, the tensile force F (unit: N) measured by the spring balance pulling in the horizontal direction was obtained. The obtained results are shown in Tables 3 and 4 as an index with the value of Comparative Example 1 being 100. Note that the hose of Comparative Example 3 was not evaluated because the thickness of the inner layer and the outer layer was different from the other hoses.
[0073] (9) Refrigerant permeation rate through hoses used for transporting refrigerants The refrigerant permeation rate of the refrigerant transport hose was measured in accordance with SAE J2064 AUG2015. The refrigerant transport hose was cut to a length of 1.07 m to prepare a test sample, and the internal volume was 1 cm 3 The test sample was left to stand in an atmosphere at 80°C for 25 days, and the mass loss (refrigerant permeation amount) per day (24 hours) was measured during the last specified period (5 to 7 days) of the 25-day period. This loss was divided by the internal surface area of the test sample to obtain the refrigerant permeation amount (unit: kg / (m2)) of the refrigerant transport hose per year (8760 hours). 2 The smaller the refrigerant permeation rate, the better the refrigerant permeation resistance. 2 ·year), it can be evaluated that the material has sufficient resistance to refrigerant permeation for practical use. 2 ·year) or less is "Excellent", 3.0kg / (m 2 ·year) exceeds 10kg / (m 2 ·year) or less is "good", and 10kg / (m 2 Those exceeding this limit are categorized as "poor" and are listed in Tables 3 and 4.
[0074] (10) Moisture permeability of refrigerant transport hoses The refrigerant transport hose was left in an oven at 50°C for 5 hours, and then the test sample was filled with a desiccant in a volume equivalent to 80% of the internal volume and sealed. The test sample was left in an atmosphere at 50°C and 95% RH, and the increase in the mass of the desiccant was measured after 120 hours and 360 hours. The increase in mass (unit: mg) over the 240 hours was multiplied by the internal surface area (unit: cm) of the test sample. 2 ) to obtain the moisture permeability (unit: mg / (cm 2 The moisture permeability was calculated as 1.3 mg / (cm 2 240h) or less is "Excellent", and the moisture permeability is 1.3mg / (cm 2 240h) exceeds 1.5mg / (cm 2 240h) or less is considered "good" and 1.5mg / (cm 2 Those exceeding 240h are categorized as "poor" and are listed in Tables 3 and 4.
[0075] [Table 1]
[0076] [Table 2]
[0077] The types of raw materials used in Tables 1 and 2 are shown below. Resin a-1: Propylene homopolymer, Prime Polypro J108M manufactured by Prime Polymer, melting point 165℃ Resin a-2: Propylene-ethylene random copolymer, Novatec MG05ES manufactured by Japan Polypropylene Corporation, melting point 147°C Resin a-3: Propylene-ethylene block copolymer, Novatec BC06C manufactured by Japan Polypropylene Corporation, melting point 165°C Resin b-1: Polyamide 6, Ube Industries nylon 6 "UBE nylon" 1011FB, melting point 225℃ Resin b-2: Polyamide 12, Ube Industries nylon 12 "UBESTA" (registered trademark) 3012U, melting point 176°C Resin b-3: Polyamide 612, Nylon 6 / 12 copolymer "UBE Nylon" 7024B manufactured by Ube Industries, melting point 201℃ Elastomer A: Brominated butyl rubber, Exxon Mobil Chemical "Exxon Bromobutyl 2255" Elastomer B: Brominated isobutylene-paramethylstyrene copolymer rubber, ExxonMobil Chemical Company "EXXPRO" (registered trademark) 3745 Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. Crosslinking agent: Solutia's N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine "SANTOFLEX" (registered trademark) 6PPD Viscosity stabilizer: Calcium stearate, Sakai Chemical Industry Co., Ltd. calcium stearate SC-PG
[0078] [Table 3]
[0079] [Table 4]
[0080] The types of raw materials used in Tables 3 and 4 are shown below. Thermoplastic resin compositions A-1 to A-5, A'-6 to A'-8 constituting the outer layer: see Table 1 ·PET fiber: Polyethylene terephthalate fiber Adhesive-1: Acid-modified polyolefin adhesive Adhesive-2: Moisture-curing urethane adhesive Thermoplastic resin compositions B-1, B'-2, and B'-3 constituting the inner layer: see Table 2
[0081] As is clear from Table 3, the refrigerant transport hoses of Examples 1 to 7 were confirmed to have low water vapor permeability and fluorocarbon permeability, and to be flexible and lightweight. In the refrigerant transport hose of Example 7, the resin composition (B'-2) constituting the inner layer contained less than 51 mass % of elastomer b, so the effect of improving the flexibility of the hose tends to be somewhat small. As is clear from Table 4, the refrigerant transport hose of Comparative Example 1 has less than 51 mass % of elastomer a in the resin composition (A'-6) constituting the outer layer, so the flexibility of the hose is inferior to that of Examples 1-7. The refrigerant transport hose of Comparative Example 2 has poor water vapor permeability because, in the resin composition (A'-7) constituting the outer layer, the thermoplastic resin a contains a polyamide resin instead of a polyolefin resin. The refrigerant transport hose of Comparative Example 3 has a poor refrigerant permeation rate because, in the resin composition (A'-8) constituting the outer layer, the thermoplastic resin a contains a polyamide-based resin instead of a polyolefin-based resin, and, in the resin composition (B'-3) constituting the inner layer, the thermoplastic resin b contains a polyolefin-based resin instead of a polyamide-based resin. [Explanation of symbols]
[0082] 1 Refrigerant transport hose 2. Inner layer 3 Reinforcement layer 4 Outer layer
Claims
1. A hose for transporting a refrigerant, comprising at least an outer layer, a reinforcing layer, and an inner layer, and not including a layer made of vulcanized rubber, the outer layer has at least a layer made of a thermoplastic resin composition A, and the inner layer has at least a layer made of a thermoplastic resin composition B, The thermoplastic resin composition A has a sea-island structure with a thermoplastic resin a as a matrix and an elastomer a as a domain, the thermoplastic resin a contains at least a polyolefin-based resin, the elastomer a contains at least a butyl-based elastomer, and the elastomer a accounts for 51 to 81 mass% of 100 mass% of the thermoplastic resin composition A, A hose for transporting a refrigerant, wherein a thermoplastic resin composition B has an island-sea structure with a thermoplastic resin b as a matrix and an elastomer b as a domain, the thermoplastic resin b contains at least a polyamide-based resin, the elastomer b contains at least a butyl-based elastomer, and the elastomer b accounts for 45 to 60 mass% of 100 mass% of the thermoplastic resin composition B.
2. 2. The hose for transporting a refrigerant according to claim 1, wherein the thermoplastic resin composition B has a lower fluorocarbon permeability coefficient than the thermoplastic resin composition A.
3. 3. The hose for transporting a refrigerant according to claim 1, wherein the thermoplastic resin composition A has a water vapor permeability coefficient smaller than the water vapor permeability coefficient of the thermoplastic resin composition B.
4. 4. The hose for transporting a refrigerant according to claim 1, wherein the thermoplastic resin a comprises at least a polypropylene resin, and the elastomer a comprises at least a halogenated butyl rubber.
5. 5. The hose for transporting a refrigerant according to claim 1, wherein the thermoplastic resin b contains at least a polyamide 6 resin, and the elastomer b contains at least a halogenated isobutylene-paramethylstyrene copolymer rubber.
6. The hose for transporting a refrigerant according to any one of claims 1 to 5, wherein a part of the domain of the thermoplastic resin composition A and / or a part of the domain of the thermoplastic resin composition B is crosslinked.
7. The hose for transporting a refrigerant according to any one of claims 1 to 6, wherein a water-based adhesive, a solvent-based adhesive, a chemical reaction-based adhesive, or a hot melt-based adhesive is interposed between the outer layer and the reinforcing layer and / or between the inner layer and the reinforcing layer.
8. The thermoplastic resin composition A was subjected to a shear rate of 243.2 s at 250°C. 1 The hose for transporting a refrigerant according to any one of claims 1 to 7, wherein the melt viscosity at 0.5°C is 1000 Pa·s or less.
9. 9. The refrigerant transport hose according to any one of claims 1 to 8, wherein the thermoplastic resin a comprises one or more thermoplastic resins having a melting point of 150°C or higher, and the thermoplastic resin b comprises one or more thermoplastic resins having a melting point of 200°C or higher.
10. The thermoplastic resin composition A has a tensile stress of 1 MPa or more and 10 MPa or less at 10% deformation, and a water vapor permeability coefficient of 1.0 to 3.0 g mm / (m 2 The hose for transporting a refrigerant according to any one of claims 1 to 9, wherein the refrigerant transport temperature is 24 h.
11. The thermoplastic resin composition B has a tensile stress of 1 MPa or more and 10 MPa or less at 10% deformation, and an oxygen permeability coefficient of 0.0001 to 0.02 cm 3 mm / (m 2 The hose for transporting a refrigerant according to any one of claims 1 to 10, wherein the refrigerant flow rate is 100%. .day.mmHg.
12. The hose for transporting a refrigerant according to any one of claims 1 to 11, wherein the thermoplastic resin composition A has a tensile break strength at 23 ° C. of 3 MPa or more and 10 MPa or less and a tensile break elongation at 23 ° C. of 200% or more and 605% or less.
13. The hose for transporting a refrigerant according to any one of claims 1 to 12, wherein the thermoplastic resin composition A has a tensile break strength of 0.4 MPa or more and 0.5 MPa or less at 150°C and a tensile break elongation of 50% or more and 821% or less at 150°C.
14. The hose for transporting a refrigerant according to any one of claims 1 to 13, wherein the thermoplastic resin composition A and the thermoplastic resin composition B have an Izod impact strength at -40°C that is non-destructive.
Citation Information
Patent Citations
Polyamide resin composition and method for producing the same and hose for transporting coolant
JP2010275361A
Resin hose, and method of producing the same
JP2013155793A
Thermoplastic resin composition for refrigerant transportation piping and refrigerant transportation piping
JP2021046490A
Hose for transferring refrigerant
WO2011018904A1
Thermoplastic resin composition for cooling medium transportation pipes, and cooling medium transportation pipe
WO2021054058A1