Electronic devices including one or more monolayer amorphous films and methods for forming same - Patents.com

Monolayer amorphous films, particularly monoatomic layer amorphous carbon, address the challenges of moisture and interdiffusion in flexible electronic devices by providing effective, transparent, and durable barriers, enabling improved device scalability and performance.

JP7587210B2Active Publication Date: 2024-11-20NATIONAL UNIVERSITY OF SINGAPORE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022514514
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-20
Filing Date
2020-09-18
Publication Date
2024-11-20
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

Existing flexible electronic devices, such as OLED displays and perovskite solar cells, face degradation due to moisture and oxygen penetration, while conventional barrier layers compromise flexibility and transparency, and interconnects in silicon-based circuits suffer from interdiffusion issues with copper and cobalt, limiting device scalability and performance.

Method used

The use of monolayer amorphous films, such as monoatomic layer amorphous carbon (MAC), as barrier layers that inhibit moisture and gas penetration and suppress interdiffusion, formed through low-temperature laser chemical vapor deposition, providing flexibility, transparency, and effective protection.

Benefits of technology

The monolayer amorphous films offer superior barrier properties with high transparency, thermal stability, and mechanical durability, enhancing the lifespan and performance of flexible devices and preventing interconnect corrosion, while being compatible with existing semiconductor processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587210000004
    Figure 0007587210000004
  • Figure 0007587210000005
    Figure 0007587210000005
  • Figure 0007587210000006
    Figure 0007587210000006
Patent Text Reader

Abstract

Various embodiments may relate to an electronic device comprising a substrate comprising a suitable semiconductor material or a suitable polymer material and a barrier comprising one or more atomically amorphous film layers overlying the substrate. The barrier may be configured to inhibit or reduce permeation of moisture or gas from the environment into the substrate. Various embodiments may relate to an electronic device comprising a first device structure comprising a conductive material, a second device structure comprising a further conductive or semiconductor material, and a barrier comprising one or more atomically amorphous film layers between the first and second device structures. The barrier may be configured to inhibit or reduce interdiffusion between the first and second device structures.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority to Singapore Patent No. 10201908768S, filed on September 20, 2019, the contents of which are incorporated herein by reference in their entirety and for all purposes.

[0002] Various aspects of the present disclosure relate to electronic devices that include one or more layers of atomically amorphous films (MAFs).Various aspects of the present disclosure relate to methods of forming electronic devices that include one or more layers of atomically amorphous films (MAFs). [Background technology]

[0003] Flexible electronic devices, such as organic light-emitting diode (OLED) displays, thin film transistors (TFTs), and perovskite organic solar cells, have polymer substrates so that the devices are transparent, flexible, and low power consumption. However, the organic materials utilized as the self-emitting components of, for example, OLED displays, are highly sensitive to moisture and atmospheric oxygen, especially in high humidity conditions. Moisture gradually degrades the functionality of the devices. Therefore, protective barrier layers or films are required to protect OLED displays, or other organic or perovskite solar cell devices, from oxygen and moisture penetration. This can extend the life of such devices. The quality of the barrier layer film is evaluated by the water vapor transmission rate (WVTR) in addition to the oxygen penetration.

[0004] Polymer coatings such as Parylene C, polyethylene terephthalate (PET), and metallized polyethylene terephthalate / polyethylene (PET / PE) have been used as barrier layers in the past because they can maintain the flexibility and transparency of OLED displays. However, these polymer coatings are sensitive to moisture and oxygen, and are mechanically weak under stress, limiting the protection they can provide. Alternatively, inorganic materials such as glass, silicon dioxide (SiO2), silicon nitride (SiN), and aluminum oxide (Al2O3) are mechanically strong and provide sufficient protection against moisture at reasonable thicknesses. However, barriers or films containing these inorganic materials are rigid, compromising the flexibility and transparency of the device. Furthermore, atomic layer deposition (ALD) is typically used to fabricate these inorganic barriers or films. ALD introduces undesirable pinhole defects in the barrier or film and requires very long processing times, making such encapsulation techniques inefficient.

[0005] On a different note, copper (Cu) and cobalt (Co) interconnects are commonly used in silicon (Si)-based integrated circuits due to their high electrical conductivity and low line resistance, enabling the miniaturization of microelectronic devices. However, Cu and Co face the problem of interdiffusion with the underlying silicon (Si) chip or dielectric chip, which results in compromising the operability of the device. Therefore, a connecting diffusion barrier layer on the interconnect is required to prevent the migration of Cu or Co. However, an ideal diffusion barrier should have properties such as strong adhesion to Cu or Co, ultrathinness, and thermal stability.

[0006] According to the International Roadmap for Devices and Systems (IRDS) 2017, one of the main challenges for miniaturization and ultra-large scale integration (ULSI) is the further scaling of interconnects. The scaling of interconnects is currently limited by the required minimum thickness of diffusion barrier materials. Figure 1 shows the International Technology Roadmap for Semiconductors. Conventional diffusion barriers are typically 10 nm titanium nitride (TiN) or tantalum nitride (TaN) grown by ALD. This thickness is required to prevent Cu and Co ions from diffusing into the semiconductor layers. However, such thickness is too thick to achieve future device scaling as shown in Figure 1. Furthermore, thicker layers of highly resistive barrier materials significantly increase the resistivity of Cu interconnects, thus adversely affecting device performance. Therefore, the International Roadmap for Semiconductors (http: / / www.itrs2.net / ) foresees atomically thin diffusion barrier materials with thicknesses of less than 2 nm to realize future devices with significant scaling. Furthermore, the candidate diffusion barriers need to be inert to both interfaces and have strong adhesion. The challenges currently facing the industry relate to reducing the barrier thickness and reducing the process temperature for fabricating the diffusion barrier to temperatures below 400° C. to prevent dopant diffusion. Summary of the Invention

[0007] Various embodiments may relate to an electronic device. The electronic device may include a substrate including a suitable semiconductor material or a suitable polymer material. The electronic device may also include a barrier on the substrate including one or more monolayer amorphous films. The barrier may be configured to inhibit or reduce the penetration of moisture or gas from the environment into the substrate.

[0008] Various embodiments may relate to a method of forming an electronic device. The method may include forming a barrier on a substrate, the barrier comprising one or more monoatomic amorphous films. The substrate may comprise a suitable semiconductor material or a suitable polymeric material. The barrier may be configured to inhibit or reduce the permeation of moisture or gas from the environment into the substrate.

[0009] Various embodiments may relate to an electronic device. The electronic device may include a first device structure including a conductive material. The electronic device may also include a second device structure including a further conductive or semiconducting material. The electronic device may further include a barrier between the first device structure and the second device structure, the barrier including one or more monolayer amorphous films. The barrier may be configured to inhibit or reduce interdiffusion between the first device structure and the second device structure.

[0010] Various embodiments may relate to a method of forming an electronic device. The method may include forming a first device structure including a conductive material. The method may also include forming a second device structure including an additional conductive or semiconducting material. The method may further include forming a barrier between the first device structure and the second device structure, the barrier comprising one or more monolayer amorphous films. The barrier may be configured to inhibit or reduce interdiffusion between the first device structure and the second device structure. [Brief description of the drawings]

[0011] The present invention will be more fully understood with reference to the detailed description and when considered in conjunction with the non-limiting examples and the accompanying drawings, in which: [Figure 1] It shows the international semiconductor technology roadmap. [Diagram 2] 1 is a schematic diagram illustrating an electronic device according to various embodiments. [Diagram 3] 1A-1D are schematic diagrams illustrating methods of forming electronic devices according to various embodiments. [Figure 4] 1 is a schematic diagram illustrating an electronic device according to various embodiments. [Diagram 5] 1 is a schematic diagram illustrating a method of forming an electronic device according to various embodiments. [Figure 6] 1 shows a schematic diagram of a device overlying a substrate with a monolayer amorphous carbon (MAC) film, according to various embodiments. [Figure 7] FIG. 1 is a schematic diagram illustrating a device comprising a substrate and a monolayer amorphous carbon (MAC) film overlying the substrate, with an inset showing the amorphous-like atomic arrangement, according to various embodiments. [Figure 8] 1 shows optical images of graphene encapsulated copper after 4 months of aging in ambient atmosphere (left) and copper encapsulated with monolayer amorphous carbon (MAC) according to various embodiments after 4 months of aging in ambient atmosphere (right). [Figure 9] 1 shows an optical image (left) showing crack propagation along grain boundaries in graphene after indentation, and an optical image (right) of an atomically-layer amorphous carbon (MAC) film according to various embodiments showing no crack propagation after indentation. [Figure 10A] 1 shows an atomic force microscopy (AFM) image (top) of a crosslinked monolayer amorphous carbon (MAC) film according to various embodiments after an indentation has been made in the film, and a graph (bottom) of height (in nanometers (i.e., nm)) as a function of distance (in nanometers (i.e., nm)) showing a corresponding height profile illustrating the indentation peak after the AFM has left the monolayer amorphous carbon (MAC) film. [Figure 10B]1 shows another atomic force microscopy (AFM) image (top) of a crosslinked monolayer amorphous carbon (MAC) film according to various embodiments after a second indentation has been made in the film (to the right of the first indentation) and a graph (bottom) of height (in nanometers (i.e., nm)) as a function of distance (in nanometers (i.e., nm)) showing a corresponding height profile indicating the second indentation peak after the AFM has moved away from the monolayer amorphous carbon (MAC) film. [Figure 10C] 1 shows a three-dimensional atomic force microscopy (AFM) image of a cross-linked monolayer amorphous carbon (MAC) film according to various embodiments with two indentations. [Figure 11] 1 shows an optical image (left) of a bubble test in which some holes are covered by an atomically-layered amorphous carbon (MAC) film according to various embodiments and gas is injected to cause the MAC film to form respective ridges, and an atomic force microscopy (AFM) image (right) showing the ridges of the monolayer film after removal from the high pressure gas chamber. [Figure 12] FIG. 1 shows a plot of transmittance (in percent (i.e., %)) as a function of wavelength (in nanometers (i.e., nm)) illustrating the transmittance spectrum of atomically layer amorphous carbon (MAC) in accordance with various embodiments. [Figure 13A] 1 shows a scanning electron microscope image of a copper (Cu) interconnect after a monolayer amorphous carbon (MAC) film is grown on the copper interconnect using laser chemical vapor deposition according to various embodiments. [Figure 13B] 1 shows an atomic force microscopy (AFM) image of a copper (Cu) interconnect after a monolayer amorphous carbon (MAC) film is grown on the copper interconnect using laser chemical vapor deposition, according to various embodiments. [Figure 13C]FIG. 1 is a plot of Raman intensity (arbitrary units (i.e., au)) as a function of wavenumber (in 1 / cm units of per centimeter) showing a Raman spectrum with D and G bands for a monolayer amorphous carbon (MAC) / copper (Cu) interconnect, according to various embodiments. [Figure 14A] FIG. 1 shows atomic force microscopy (AFM) images of bare copper (Cu) interconnects before (left) and after (center and right) exposure to ammonium persulfate (APS). [Figure 14B] 1 shows atomic force microscopy (AFM) images of a copper (Cu) interconnect coated with amorphous carbon (MAC) according to various embodiments before exposure to ammonium persulfate (APS) (left) and after exposure to ammonium persulfate (APS) (center and right). [Figure 15] 1 shows scanning electron microscope (SEM) images of copper (Cu) foil coated with atomically layered amorphous carbon (MAC) according to various embodiments after exposure to acid (left) and graphene coated copper (Cu) foil after exposure to acid (center), as well as a plot (right) comparing copper (Cu) ion loss (in parts per million (i.e., ppm)) for a standard copper (Cu) electrode, a graphene coated (Cu) electrode, and a copper (Cu) electrode coated with atomically layered amorphous carbon (MAC) according to various embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the following detailed description, reference is made to the accompanying drawings which illustrate specific details and embodiments in which the invention may be practiced. These embodiments are described in sufficient detail to enable those skilled in the art to practice the invention. Other embodiments may be utilized, and structural and logical changes may be made without departing from the scope of the present invention. The various embodiments are not necessarily mutually exclusive, and some embodiments may be combined with one or more other embodiments to form new embodiments.

[0013] An embodiment described in the context of either a method or a device is equally valid for the other method or device, and similarly, an embodiment described in the context of a method is equally valid for the device and vice versa.

[0014] Features described in the context of one embodiment may be applicable to the same or similar features of other embodiments as well. Features described in the context of one embodiment may be applicable to other embodiments as well, even if they are not explicitly described in such other embodiments. Furthermore, additions and / or combinations and / or alternatives described for a feature in the context of one embodiment may be applicable to the same or similar features of other embodiments as well.

[0015] It will be understood that the devices described herein may be operable in a variety of orientations, and therefore terms such as "upper", "lower", and the like, when used in the following description, are used for convenience to aid in understanding relative positions or orientations, and are not intended to limit the orientation of the devices.

[0016] In the context of various embodiments, the articles "a," "an," and "the" used in reference to a feature or element include a reference to one or more of those features or elements.

[0017] In the context of various embodiments, the term "about" or "approximately" applied to a numerical value encompasses the true value and reasonable variation.

[0018] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0019] Various embodiments may relate to electronic devices that include one or more atomically-layered amorphous films (MAFs), which may alternatively be referred to as two-dimensional (2D) amorphous films.

[0020] 2 is a schematic diagram illustrating an electronic device according to various embodiments. The electronic device may include a substrate 202 including a suitable semiconductor material or a suitable polymeric material. The electronic device may also include a barrier 204 including one or more layers of a monolayer amorphous film (MAF) on the substrate 202. The barrier 204 may be configured to inhibit or reduce the permeation of moisture or gases (e.g., oxygen) from the environment to the substrate.

[0021] For the avoidance of doubt, Figure 2 is not intended to limit the shape, size, orientation, etc. of the device or its various components. For example, while Figure 2 illustrates a substrate 202 having a rectangular cross-section, various embodiments may include a substrate of any suitable shape. Additionally, while Figure 2 illustrates a barrier 204 having one layer of an atomically amorphous film, various embodiments may include a barrier 204 having multiple layers of atomically amorphous films.

[0022] In the present context, an "amorphous solid" may refer to a solid that lacks the long-range order that is characteristic of a crystal.

[0023] In the present context, the term "monolayer" may refer to a layer that is one atom thick.

[0024] The one or more monolayer amorphous films may include, but are not limited to, monolayer amorphous carbon (MAC) films, amorphous boron nitride (a-BN) films, monolayer amorphous molybdenum disulfide films, monolayer amorphous tungsten disulfide films, monolayer amorphous borophene (a-BP) films, other monolayer amorphous transition metal dichalcogenide (a-TMD) films, monolayer amorphous boron nitride carbon films, or heteroatom doped films and alloys.

[0025] In the present context, the term "amorphous carbon" may refer to a carbon structure that lacks long-range order and crystalline structure. Monolayer amorphous carbon (MAC) films can alternatively be referred to as sp 2 It is sometimes called an atomic layer of bonded carbon. In this context, monolayer amorphous carbon (MAC) films can have structures and properties that differ from bulk amorphous carbon (i.e., diamond-like carbon, glassy carbon, soot, etc.). For example, bulk amorphous carbon may not be suitable as an interdiffusion barrier, since it can transmit moisture and gases (such as oxygen). Graphene, on the other hand, is a sp 2 It is an atomic layer of bonded carbon lattice that forms a crystalline material (single or polycrystalline). Graphene requires high temperatures to synthesize, and its growth is mostly limited to transition metal substrates (Cu, Ni, Co, etc.). MACs, in contrast, can be formed on any substrate at much lower temperatures. Similarly, other monolayer amorphous films (MAFs) may have different structures and properties than their bulk and 2D crystalline equivalents.

[0026] In various embodiments, each of the one or more monoatomic amorphous films may have a thickness selected from the range of 0.4 nm to 1 nm.

[0027] In various embodiments, one or more monolayer amorphous films may form a stack.

[0028] In various embodiments, the electronic device may further include a protective layer on the substrate 202. The protective layer may include an oxide or a polymer. The oxide may be aluminum oxide (Al2O3) or hafnium oxide (HfO2). The polymer may be parylene C. An atomic layer deposition (ALD) process may be used to form or deposit the protective layer. The protective layer may be included as part of the barrier 204.

[0029] In various embodiments, one or more monolayer amorphous films may be between the protective layer and the substrate 202. In various other embodiments, a protective layer may be between one or more amorphous films and the substrate 202.

[0030] In various embodiments, the electronic device may be, but is not limited to, an organic light-emitting diode (OLED) or a thin film transistor (TFT). For example, an OLED may include a first electrode, a second electrode, and an organic light-emitting layer between the first and second electrodes. The light-emitting layer may be on the first electrode, and the second electrode may be on the light-emitting layer. The second electrode may include, for example, a conductive material (e.g., a semiconductor such as indium tin oxide). The light-emitting layer may include a polymer configured to emit light upon application of a potential difference across the light-emitting layer. A barrier 204 including one or more layers of amorphous film may be provided on the second electrode and / or on the organic light-emitting layer. Meanwhile, a top-gate TFT may include a layer of semiconductor material (e.g., amorphous silicon), a dielectric layer on the layer of semiconductor material, a gate electrode on the dielectric layer, and drain and source electrodes at least partially embedded in the layer of semiconductor layer. The drain and source electrodes may be on a first surface of the dielectric layer, and the gate electrode may be on a second surface opposite the first surface of the dielectric layer. The gate electrode may include a semiconductor such as ITO. A barrier 204 including one or more layers of amorphous film may be provided on the gate electrode. A bottom-gate TFT may include a gate electrode, a dielectric layer on the gate electrode, and drain and source electrodes on or above the dielectric layer. A bottom-gate TFT may include a layer of semiconductor material (e.g., silicon) on the source and drain electrodes. A barrier 204 including one or more layers of amorphous film may be provided on the layer of semiconductor material.

[0031] In various embodiments, the one or more monolayer amorphous films are primarily sp 2 In various embodiments, the sp 2 bond present in the one or more monolayer amorphous films may be present. 3 / sp 2 may have a bond ratio of 0.1 or less.

[0032] In various embodiments, the oxygen permeation rate of one or more monoatomic amorphous films is 10 -4 cc·m-2 ·day -1 ~10 -2 cc·m -2 ·day -1 Even if the amount selected is within the range of 10 -4 cc·m -2 ·day -1 In various embodiments, the water vapor transmission rate (WVTR) of the one or more monoatomic amorphous films may be less than 10 -5 g m -2 ·day -1 ~10 -6 g m -2 ·day -1 Even if the value is selected from the range of 10 -5 g m -2 ·day -1 A value less than this may be used.

[0033] In various embodiments, the transparency (measured at 550 nm) of one or more monolayer amorphous films may be greater than 95%, such as greater than 98%, such as 98.1%. In various embodiments, the sheet resistance of one or more monolayer amorphous films may be 100 GΩ / □ or greater. The monolayer amorphous film may have a mixture of hexagonal and non-hexagonal rings. The non-hexagonal rings may be in the form of four-, five-, seven-, eight-, nine-membered rings. The rings may be fully connected to each other to form a polygonal network in large area films that are at least on the scale of microns. Crystallinity may refer to the degree of structural order in a solid and may be measured based on the ratio of hexagonal to non-hexagonal rings. In the present context, a monolayer amorphous film may be a film with a crystallinity (C) equal to or less than 80% (C≦80%). In various embodiments, such as for amorphous MAC films, the crystallinity may be equal to or greater than 60% (C≧60%). The crystallinity of one or more monolayer amorphous films may be adjusted to any suitable value between 60% and 80% inclusive, which may alter the barrier properties as well.

[0034] In various embodiments, suitable semiconductors may be, for example, silicon, germanium, gallium arsenide (GaAs), indium gallium zinc oxide (IGZO), zinc oxide (ZnO), etc. In various embodiments, suitable polymeric materials may be, for example, silicon oxide (SiO2), polyethylene terephthalate (PET), polyphenylene vinylene (PPV), polyfluorene (PF), polyparaphenylene (PPP), etc.

[0035] 3 is a schematic diagram illustrating a method of forming an electronic device according to various embodiments. The method may include, at 302, forming a barrier comprising one or more monoatomic amorphous films on a substrate. The substrate may include a suitable semiconductor material or a suitable polymeric material. The barrier may be configured to inhibit or reduce the permeation of moisture or gases (e.g., oxygen) from the environment into the substrate.

[0036] In various embodiments, one or more monolayer amorphous films may be formed on a substrate by a chemical vapor deposition (CVD) process. In various embodiments, the chemical vapor deposition process is a laser chemical vapor deposition (LCVD) process. The temperature at which the chemical vapor deposition process is performed may be any suitable temperature below 300° C.

[0037] In various embodiments, one or more monolayer amorphous films or barriers may be formed as free-standing films prior to being transferred onto a substrate, i.e., one or more monolayer amorphous films or barriers may be formed and subsequently transferred onto a polymeric or semiconductor substrate without the use of a polymethylmethacrylate (PMMA) support.

[0038] 4 is a schematic diagram illustrating an electronic device according to various embodiments. The electronic device may include a first device structure 402 including a conductive material. The electronic device may also include a second device structure 404 including an additional conductive or semiconducting material. The electronic device may further include a barrier 406 including one or more monolayer amorphous films between the first device structure 402 and the second device structure 404. The barrier 406 may be configured to inhibit or reduce interdiffusion between the first device structure and the second device structure.

[0039] For the avoidance of doubt, Figure 4 is not intended to limit the shape, size, orientation, etc. of the device or its various components. For example, while Figure 4 illustrates structures 402, 404 having identical rectangular cross-sections, various embodiments may include structures of any suitable shape. In various embodiments, the shape of structure 402 may differ from the shape of structure 404. Additionally, while Figure 4 illustrates barrier 406 having one layer of monolayer amorphous film, various embodiments may include barrier 406 having multiple layers of monolayer amorphous film.

[0040] In various embodiments, the conductive material may be a metal, a metal alloy, a doped metal oxide, or conductive carbon. In various embodiments, the conductive material or metal may be copper (Cu) or cobalt (Co).

[0041] In various embodiments, the additional conductive material may be a metal, a metal alloy, a doped metal oxide, or conductive carbon.

[0042] In various embodiments, the semiconductor material may be, for example, silicon, germanium, gallium arsenide (GaAs), indium gallium zinc oxide (IGZO), zinc oxide (ZnO), or any other suitable semiconductor material.

[0043] In one example, one or more monoatomic amorphous films may be between two interconnects, i.e., the first device structure 402 may be a first interconnect and the second device structure 404 may be a second interconnect.

[0044] In another example, the one or more monolayer amorphous films may be between an interconnect and a substrate. In other words, the first device structure 402 may be an interconnect and the second device structure may be a substrate, for example, a semiconductor substrate such as a silicon substrate, a germanium substrate, a gallium arsenide (GaAs) substrate, an indium gallium zinc oxide (IGZO) substrate, a zinc oxide (ZnO) substrate, etc. In yet another example, the one or more amorphous films may be between two metal contacts, such as a gate metal stack.

[0045] In various embodiments, the sp 2 atoms present in one or more monolayer amorphous films 3 / sp 2 may have a bond ratio of 0.1 or less.

[0046] In various embodiments, the electronic device may be, but is not limited to, a transistor, a diode, a memory device, or an electromechanical device, an integrated circuit chip, a microprocessor, or an electronic sensing device.

[0047] Various embodiments may relate to circuit arrangements that include electronic devices as described herein.

[0048] 5 is a schematic diagram illustrating a method of forming an electronic device according to various embodiments. The method may include forming or providing a first device structure, at 502, comprising a conductive material. The method may also include forming or providing a second device structure, at 504, comprising an additional conductive or semiconducting material. The method may further include forming a barrier, at 506, between the first device structure and the second device structure, comprising one or more monolayer amorphous films. The barrier may be configured to inhibit or reduce interdiffusion between the first device structure and the second device structure.

[0049] To avoid any misunderstanding, no order of the various steps is shown or limited in Figure 5. In various embodiments, step 506 may be performed before step 504, and step 502 may be performed after step 504.

[0050] In various embodiments, the one or more monolayer amorphous films may be formed on the second device structure and then the first device structure may be formed on the one or more monolayer amorphous films, such that the one or more monolayer amorphous films are between the first device structure and the second device structure.

[0051] In various embodiments, the monolayer amorphous film or films may be formed by a chemical vapor deposition process (CVD), which may be a laser chemical vapor deposition process (LCVD).

[0052] In various embodiments, the temperature at which the chemical vapor deposition process is carried out may be any suitable temperature below 300°C.

[0053] In various embodiments, one or more monoatomic amorphous films may be formed as free-standing films prior to being transferred onto the second device structure.

[0054] Monolayer amorphous films (MAFs), such as monolayer amorphous carbon (MAC) films, may potentially be grown directly on polymer or semiconductor substrates using processes such as laser-assisted low-temperature and ultrafast CVD (Chemical Vapor Deposition), making this an industrially viable sealing method. MACs, from single to multilayer, have been shown to block atoms larger than a proton with a homogeneous atomic structure. Thus, MAC films can be used to block atoms larger than a proton with a 10 -5 g m -2 ·day -1 It is expected that the water vapor transmission rate (WVTR) will remain below that of graphene (10 -3 ~10 -1 g m -2 ·day -1 ) is at least two orders of magnitude better.

[0055] 6 shows a schematic diagram of a device according to various embodiments, including a monolayer amorphous carbon (MAC) film on a substrate. The transparency of MAC is over 98.1%, which can be higher than any other conventional ultrathin barrier film. Therefore, MAC may be ideal for transparent OLEDs.

[0056] One cause of defects in existing flexible devices is due to mechanical failure of inorganic barrier films due to crack propagation without plastic deformation when bent, which can lead to a short service life. However, MAC films have high fracture toughness, which provides high plasticity and reduces or minimizes crack propagation in the barrier film, thus enhancing the durability of the MAC barrier layer and the flexibility of the device.

[0057] Furthermore, MAF may be used for diffusion barriers due to its excellent properties such as thermal stability, chemical inertness, and atomic thinness. A monolayer amorphous film (MAF) such as MAC may be formed between a semiconductor substrate and an interconnect. MAC may be grown directly on a silicon (Si) or germanium (Ge) semiconductor layer prior to forming a copper (Cu) interconnect. Corrosion tests show that MAC can reduce copper (Cu) oxidation and copper corrosion rates by more than 7 times compared to graphene-coated copper (Cu) and bare copper (Cu). MAF may be used for diffusion barriers (e.g., in both the back-end (BEOL) and the front-end (FEOL)) since it has been demonstrated to reduce or block the diffusion of both copper (Cu) and cobalt (Co) (Co is intended to replace copper (Cu)).

[0058] The chemical inertness of MAC can be advantageous when compared to other applied metal diffusion barrier layers such as titanium (Ti), palladium (Pd), etc., which react with copper (Cu) at higher temperatures. Because MAC has insulating properties, MAC can prevent possible shorting of (Cu) interconnects. At the same time, the high thermal conductivity of MAC may result in fast heat diffusion, which leads to efficient thermal management of high power density devices.

[0059] Although the experimental data provided herein is primarily for monolayer amorphous carbon (MAC) films, other monolayer amorphous films (MAFs) may be expected to have similar properties and may be used in similar applications. Such other MAFs may include, for example, amorphous boron nitride films, monolayer amorphous molybdenum disulfide films, monolayer amorphous tungsten disulfide films, monolayer amorphous borophene films, monolayer amorphous transition metal dichalcogenide films, monolayer amorphous boron carbon nitride films, or heteroatom-doped films or alloys.

[0060] FIG. 7 is a schematic diagram illustrating a device according to various embodiments that includes a substrate and a monolayer amorphous carbon (MAC) film overlying the substrate, with an inset showing the amorphous-like atomic arrangement.

[0061] Various embodiments may relate to devices in which the amorphous carbon film covers the entire substrate. Various embodiments may find use, for example, as a carbon coating. The monolayer amorphous carbon film can also act as a defect-free diffusion barrier (i.e., permeation barrier) to prevent oxidation and corrosion of the underlying substrate. The amorphous carbon film may reduce or prevent galvanic corrosion of the substrate due to its electrical insulating properties.

[0062] Table 1 below lists some of the features and associated benefits / advantages of various embodiments of the present invention. [Table 1] JPEG0007587210000002.jpg147165JPEG0007587210000003.jpg104165

[0063] [Structural advantages of monolayer amorphous carbon (MAC)]

[0064] The atomic structure of MAC is a two-dimensional (2D) disordered sp 2 It may be a continuous network of carbon (C) atoms (homogeneous), whereas conventional polycrystalline graphene may contain ordered crystalline domains separated by grain boundaries (heterogeneous). In MAC, the ratio of hexagonal carbon rings to non-hexagonal carbon rings may be less than 1, i.e., around 0.6. Advantages of MAC may include:

[0065] 1.Corrosion / oxidation resistance

[0066] Grain boundaries in polycrystalline graphene barrier films can act as special weak points, leading to inhomogeneities in the structure and susceptibility to corrosion by reactive atmospheres (e.g., oxygen, moisture), which can reduce the barrier properties of the barrier film and even accelerate the corrosion process. However, MAC can provide a homogeneous atomic structure and inhibit oxygen and moisture reactions, forming an effective and stable barrier against harsh environments. Figure 8 shows optical images (left) of graphene-encapsulated copper after 4 months of aging in ambient atmosphere and (right) of monolayer amorphous carbon (MAC)-encapsulated copper according to various embodiments after 4 months of aging in ambient atmosphere. It can be seen from Figure 8 that monolayer amorphous carbon (MAC)-encapsulated copper shows higher oxidation resistance compared to graphene-encapsulated copper.

[0067] 2.Thermal stability

[0068] At high temperatures, grain boundary sliding occurs in polycrystalline barrier films (e.g., tantalum (Ta), molybdenum (Mo), chromium (Cr), titanium nitride (TiN), etc.), which destabilizes the structure and causes the barrier film to lose its functionality. Copper (Cu) ions can diffuse through the grain boundaries. In contrast, MAC has shown thermal stability at temperatures above 700°C due to its homogeneous structure. Therefore, MAC may have great potential as an effective barrier for components operating at higher temperatures (e.g., as a diffusion barrier for interconnects). The homogeneous structure of MAC may contribute to its chemical stability and chemical inertness.

[0069] 3.Adjustable structure

[0070] Depending on the synthesis conditions, the structure of MACs can be tuned from fully amorphous to nanocrystalline, allowing for a wide range of tailoring of structure, properties and performance according to end-use requirements.

[0071] 4. Mechanical stability

[0072] MACs exhibit very high fracture toughness (in x, y, and z directions) due to their amorphous-like atomic structure with no grain boundaries, which can result in a crack arrest phenomenon when folded. In contrast, in crystalline equivalents (e.g., polycrystalline graphene), cracks can propagate along preferred crystal orientations or grain boundaries, reducing the fracture toughness of the material. Figure 9 shows an optical image (left) showing crack propagation along the grain boundaries of graphene after indentation, and an optical image (right) of a monolayer amorphous carbon (MAC) film according to various embodiments showing no crack propagation after indentation.

[0073] MAC can also exhibit high plasticity, with deformations of more than 5% without fracture. This is also very important for obtaining high fracture toughness. No significant plasticity has been observed in conventional films. FIG. 10A shows an atomic force microscopy (AFM) image (top) of a crosslinked monolayer amorphous carbon (MAC) film according to various embodiments after an indentation is made in the film, and a graph (bottom) of height (in nanometers (i.e., nm)) as a function of distance (in nanometers (i.e., nm)) showing the corresponding height profile showing the indentation peak after the AFM is released from the monolayer amorphous carbon (MAC) film. Figure 10B shows another atomic force microscopy (AFM) image (top) of a bridged monolayer amorphous carbon (MAC) film according to various embodiments after a second indentation has been made in the film (to the right of the first indentation) and a graph (bottom) of height (in nanometers (i.e., nm)) as a function of distance (in nanometers (i.e., nm)) showing a corresponding height profile showing the second indentation peak after the AFM has left the monolayer amorphous carbon (MAC) film. Figure 10C shows a three-dimensional atomic force microscopy (AFM) image of a bridged monolayer amorphous carbon (MAC) film according to various embodiments having two indentations.

[0074] In flexible OLED, TFT, and other wearable electronic devices that are often subjected to repeated stress and bending, high fracture toughness can be essential to enhance the durability and performance of the barrier films according to various embodiments. On the other hand, bending of conventional inorganic polycrystalline barrier films (e.g., aluminum oxide (Al2O3), silicon nitride (SiN), zirconium oxide (ZrO2)) can cause cracks, which act as a source of moisture / oxygen leakage and limit the barrier's useful life.

[0075] 11 shows an optical image (left) of a bubble test in which some holes are covered by a monolayer amorphous carbon (MAC) film according to various embodiments and gas is injected to cause the monolayer amorphous carbon (MAC) film to form a ridge, respectively, and an atomic force microscopy (AFM) image (right) showing the ridge of the monolayer film after removal from the high pressure gas chamber. The ridge of the MAC film remains even after 24 hours, which may indicate the effectiveness of the MAC film as a barrier material.

[0076] 5. Atomically thin

[0077] A single layer MAC may have a thickness of about 0.4 nm on the growth substrate and relax to 0.6 nm after transfer, making the MAC an atomically thin barrier film against metal diffusion for interconnects or an oxygen / moisture barrier for OLEDs and TFTs. The atomically thin barrier film can be important in providing effective protection while minimizing the impact on the performance of the underlying substrate (conductivity of Cu interconnects). Even when multi-layer MAC films are required, the thickness can be in the range of 1 nm to 3 nm, preserving the ultra-thin character of the barrier film.

[0078] In contrast, existing diffusion barriers (e.g., titanium nitride (TiN) or tantalum nitride (TaN)) can lose their barrier function at thicknesses less than 2-3 nm due to film non-uniformity and lack of continuity. The large thicknesses required for these conventional films can adversely affect the flexibility of OLED displays, as displays containing these films face limitations in their critical bend radius to prevent cracking.

[0079] 6.High transparency

[0080] The transparency of the barrier film can be crucial to maintaining the transparency of the OLED display while protecting the underlying material from the ambient atmosphere. Conventional displays have traditionally used glass as a barrier. However, glass cannot be applied to flexible and foldable OLED displays due to its rigidity. Furthermore, with regard to inorganic barrier materials (e.g., aluminum oxide (Al2O3), silicon oxide (SiO2), etc.), the minimum thickness for such barrier materials to effectively block moisture results in a significant decrease in the transparency of the device.

[0081] In contrast, MAC films can have a very high transparency of about 98.1% at a wavelength of 550 nm. FIG. 12 shows a plot of transmittance (in percent (i.e. %)) as a function of wavelength (in nanometers (i.e. nm)) illustrating the transmittance spectrum of a single atomic layer amorphous carbon (MAC) according to various embodiments. FIG. 12 shows that MAC has a high transmittance of about 98.1% at a wavelength of 550 nm, approaching 99% in the infrared spectrum. This transparency is higher than graphene, which has a theoretical maximum of 97.7% at all visible wavelengths. The slight absorption of MAC can be attributed to its homogeneous atomic structure. When a few layers (e.g. 5-10 layers) of MAC are applied as a moisture barrier, an overall transparency difference of about 2-4% can be expected compared to a multi-layer graphene barrier.

[0082] 7. Thermal conductivity and electrical insulation

[0083] MAFs can be electrically insulating as well as highly thermally conductive. Theoretical predictions suggest that no significant degradation of thermal conductivity occurs in monolayer amorphous materials. MACs have been shown to be electrically insulating with sheet resistances of about 100 GΩ / □.

[0084] [Advantages of MAC processing technology]

[0085] MACs may be synthesized by laser chemical vapor deposition (LCVD), which can be integrated with existing semiconductor processing techniques. LCVD is an industrially scalable process that can achieve high-throughput, large-area barrier films. Furthermore, LCVD is an ultrafast technique, and the entire surface of a substrate can be covered with MAC in less than 60 seconds. LCVD is more efficient than the widely used atomic layer deposition (ALD) process.

[0086] Furthermore, MAC can be synthesized at low temperatures below 300 °C. This may mean that barrier films can be grown directly on Cu interconnects, as the low temperatures required correspond to silicon-based technologies. Also, the cost of MAC growth may be significantly lower compared to graphene, which can consume large amounts of energy when grown by thermal chemical vapor deposition at temperatures of about 1000 °C. Further reduction of the synthesis temperature (e.g., below 150 °C) may enable MAC to be grown directly on polymer substrates used in OLEDs and flexible electronics.

[0087] Graphene as a barrier film does not have to be grown directly on the polymer substrate or on the copper interconnects and may need to be transferred from the growth substrate, however this transfer may require a polymethylmethacrylate (PMMA) support layer that may affect the performance of the barrier film and the underlying device by introducing undesirable contaminants at the interface of the barrier film and the underlying device.

[0088] In contrast, MAC films are mechanically stable, making free-standing films achievable. Thus, free-standing MAC films can be transferred onto substrates without the use of a polymer support layer. As a result, barrier films can be formed without residues. Furthermore, integration with existing roll-to-roll transfer techniques can be possible to facilitate large-area barrier films for OLED and flexible displays.

[0089] Formation of a more effective barrier may generally require multiple layers. However, uniform multi-layer graphene can be difficult to produce. Currently, multi-layer graphene formation may only be achieved using a layer-by-layer transfer process, which is highly inefficient. In contrast, with MAC, a well-defined number of layers (e.g., 1-100 layers) can be synthesized by LCVD, allowing the thickness of the barrier film to be carefully tailored for a specific application.

[0090] Furthermore, MAC can be grown on any substrate, including metals such as copper, gold, tungsten, titanium, aluminum, nickel, etc., and insulators such as silicon oxide, strontium titanate (SrTiO3), glass, boron nitride (BN), etc. LCVD can enable the growth of complex geometries, allowing complete coverage of the interconnect for effective barrier properties.

[0091] The adhesion that can be achieved between the film and the substrate by direct growth of MAC is 10 J / m 2 It is stronger than CVD graphene, which has only a moderate adhesive strength (up to 200 J / m 2 Strong adhesion is necessary to prevent any membrane separation defects and interfacial failure that would lead to a loss of barrier properties.

[0092] MAC growth has been performed on copper (Cu) lines as an interdiffusion barrier. MAC is grown directly on thin Cu interconnects using LCVD without damaging the underlying layers. Furthermore, it has been shown that MAC can act as a protective / interdiffusion barrier layer, as evidenced by penetration, corrosion and acidity tests.

[0093] Copper interconnects (30 nm high, 200 nm wide) were fabricated on silicon oxide (SiO2) wafers using electron beam lithography followed by electron beam evaporation of copper (Cu). MAC is grown on the copper interconnects using laser-assisted CVD. FIG. 13A shows a scanning electron microscope image of a copper (Cu) interconnect after a monolayer amorphous carbon (MAC) film is grown on the copper interconnect using laser chemical vapor deposition according to various embodiments. FIG. 13B shows an atomic force microscopy (AFM) image of a copper (Cu) interconnect after a monolayer amorphous carbon (MAC) film is grown on the copper interconnect using laser chemical vapor deposition according to various embodiments. FIG. 13C shows a plot of Raman intensity (arbitrary units (i.e., au)) as a function of wavenumber (in 1 / cm units of / centimeter) according to various embodiments, showing the Raman spectrum with D and G bands of a monolayer amorphous carbon (MAC) / copper (Cu) interconnect.

[0094] SEM and AFM images shown in Figures 13A and 13B show that the shape and surface of the copper (Cu) interconnects remain pristine and smooth after LCVD growth. Furthermore, Figures 13A and 13B also confirm the feasibility of LCVD for direct growth of MAC, and that the growth of MAC can be realized based on existing semiconductor processing techniques. The Raman spectrum taken from the Cu interconnects shows D and G bands, which indicate that MAC (sp 2 These Raman features are consistent based on data collected from several locations, indicating the uniformity of the MAC film grown on the Cu interconnect.

[0095] It was also found that monolayer amorphous carbon (MAC) is highly permeable to protons (H+), but its permeability to deuterons (which have a radius roughly twice as large) is reduced by more than an order of magnitude, indicating that MAC can be impermeable to ions or molecules larger than protons. Based on the measurements, MAC can be expected to be an excellent barrier to gases (oxygen, air, etc.) and moisture (H2O), as well as an excellent interdiffusion barrier to metals and semiconductors (e.g., copper (Cu), cobalt (Co), silicon (Si), etc.).

[0096] A copper (Cu) wiring coated with MAC and one without any coating were compared. Liquid (filter) The barrier performance of MAC on Cu can be evaluated by exposing it to ammonium persulfate (APS). Figure 14A shows atomic force microscopy (AFM) images of bare copper (Cu) traces before (left) and after (middle and right) exposure to ammonium persulfate (APS). Figure 14A shows that the bare Cu traces underwent severe corrosion after exposure to APS solution. The height profile of the bare Cu traces decreased from ~30 nm to ~8.0 nm, and the root mean square (rms) roughness increased from 1.8 nm to 6.5 nm.

[0097] In contrast, the MAC-coated Cu interconnects remained smooth and uncorroded even after exposure to APS. Figure 14B shows atomic force microscopy (AFM) images of a copper (Cu) interconnect coated with monolayer amorphous carbon (MAC) according to various embodiments before exposure to ammonium persulfate (APS) (left) and after exposure to ammonium persulfate (APS) (middle and right). The height profile and rms roughness of the MAC-coated Cu interconnects remained almost unchanged, measuring 29.3 nm and 1.7 nm, respectively.

[0098] Acid corrosion tests were also performed on bare Cu traces, graphene-coated Cu traces, and MAC-coated Cu traces. The samples were exposed to nitric acid. FIG. 15 shows scanning electron microscope (SEM) images of various embodiments of a copper (Cu) foil coated with monolayer amorphous carbon (MAC) (left) and graphene-coated copper (Cu) foil (center) after exposure to acid, as well as a plot (right) comparing the copper (Cu) ion loss (in parts per million (i.e., ppm)) of a standard copper (Cu) electrode, a graphene-coated (Cu) electrode, and various embodiments of a copper (Cu) electrode coated with monolayer amorphous carbon (MAC). The SEM images in FIG. 15 show that the MAC-coated copper foil formed significantly less copper oxide after the corrosion test compared to the graphene-coated foil. As shown in the plot, the MAC-coated copper electrode lost about 7 times less copper ions during acid corrosion tests compared to the standard (bare) copper electrode and the graphene-coated electrode. These results clearly demonstrate that the MAC acts as an effective barrier layer on Cu wires / interconnects to protect them from chemicals.

[0099] As highlighted above, various embodiments may relate to devices that include one or more layers of a monolayer amorphous film (MAF), such as one or more layers of a monolayer amorphous carbon (MAC) film, on a semiconductor or polymer substrate. Depending on the permeation and mechanical requirements of the barrier, there may be any number of layers of the MAC film, selected, for example, from 1 to 10 layers.

[0100] Various embodiments may relate to devices with one or more layers of MAF as part of a multi-layer barrier, e.g., aluminum oxide (Al2O3) / MAC / silicon (Si). Various embodiments may relate to devices with composite barrier films including one or more monolayers followed by a thin barrier layer of another material (such as Al2O3). This may allow for a much thinner overall barrier to achieve the same barrier performance requirements.

[0101] Direct growth of thin MAC (1-10 layers) barrier films on OLED or TFT polymer substrates can result in strong interfacial adhesion between the barrier layer and the flexible substrate. Strong interfacial adhesion can allow higher bending of the device (radius less than 1 mm) while preventing cracking or delamination of the MAC barrier film, allowing for excellent flexibility while maintaining the original barrier performance. Furthermore, the plasticity (>5%) and high fracture toughness of MAC can greatly increase the durability of the barrier film in flexible devices, so that even if the barrier film develops minor cracks / fractures (due to accidents), it can still be repeatedly stressed without causing any film fracture, thus preventing catastrophic damage to the barrier film and its impact on the performance of the flexible device. The LCVD process can also result in strong interfacial adhesion of the MAC with the substrate. In flexible applications, the barrier layer can delaminate under induced strain, leading to film fracture and device failure. Strong interfacial adhesion of the MAC with the surface on which it is synthesized can be very important. Furthermore, the MAC can act as a strong adhesion layer for subsequent film deposition. Therefore, MAFs such as MAC films can address a critical failure mechanism in flexible electronics.

[0102] A defect-free, atomically stitched, continuous MAF barrier layer can be grown directly on the target substrate, effectively blocking the penetration of water or oxygen molecules. Various embodiments can help to avoid the existing drawback of pinhole defects in state-of-the-art ALD-deposited inorganic barrier films, which lead to moisture penetration through the defects and reduced barrier performance. The defect / pinhole-free, densely packed atomic structure of the MAC would have no preferential sites for moisture or oxygen penetration. This would allow the water vapor transmission rate (WVTR) to be increased to 10 -5 g m -2 ·day -1 Less than (graphene 10 -3 ~10 -1 g m -2 ·day -1 (at least two orders of magnitude higher than 10 -4 cc·m -2 ·day -1 Suitable barrier films can be formed that are expected to remain below 100 nm. The MAC as an interdiffusion barrier can also enable the growth of subsequent high quality barrier layers, as high temperature PECVD / ALD deposition of oxide barriers is possible without diffusion damage to the underlying substrate (silicon oxide (SiO2), polyethylene terephthalate (PET), etc.).

[0103] A MAC interdiffusion barrier layer can be present between two metal contacts such as gate metal stacks (Aluminum (Al), Titanium (Ti), Tantalum (Ta), Copper (Cu), Nickel (Ni), Gold (Au), Chromium (Cr), etc.) to prevent interdiffusion and commonly observed alloying between metal contacts at high operating temperatures (>450°C). Furthermore, the breakdown of SiO2 / metal contacts due to interdiffusion at high temperatures can also be prevented by inserting a MAC barrier layer.

[0104] The high thermal stability (>700°C) and thermal conductivity of the MAC barrier layer may allow for thinner Cu interconnects. The MAC barrier layer may allow for higher current densities that cause heat to pass. The MAC barrier layer is thermally conductive, so it can provide stability by thermal diffusion and ensure that excessively high temperatures are not reached. Conventional interdiffusion barrier layers may be thermally insulating, so they cannot dissipate heat, which leads to the breakdown of the diffusion barrier.

[0105] The electrical insulating properties of the MAC barrier layer can also prevent shorting of the thin Cu interconnects.

[0106] Heat spreaders can be important to regulate the peak temperature of transistors and thus improve device performance currently limited by localized thermal loads. The high thermal conductivity of the electrically insulating MAC diffusion barrier layer can enable efficient thermal management of high power density devices. Thus, the MAC can fulfill the requirements as a heat spreader, which is important for nanoelectronics due to the high power densities in the transistors. The MAC barrier layer may be in direct contact with the semiconductor active layer and may be suitable to act as a heat dissipation layer.

[0107] Various embodiments may relate to the MAF as a potential barrier layer for applications such as diffusion barrier layers for metal interconnects (Cu) in integrated circuits (ICs) of electronic components and microelectronic devices, or as gas and moisture barrier layers for ambient sensitive applications such as organic light emitting diodes (OLEDs) and other flexible electronic components, or in high temperature oxidation resistant components.

[0108] Various embodiments may relate to MAFs, including but not limited to MAC films. Other MAFs of various configurations may be synthesized using LCVD to form single elemental to multi-component composite films for various barrier applications.

[0109] Embodiments may include, but are not limited to, the following.

[0110] (A) An electronic device comprising a substrate comprising a suitable semiconductor material or a suitable polymeric material, and a barrier comprising one or more layers of an atomically monolayer amorphous film overlying the substrate, wherein the barrier is configured to inhibit or reduce the permeation of moisture or gas from the environment into the substrate.

[0111] (B) The electronic device of claim (A), wherein the one or more monolayer amorphous films are a monolayer amorphous carbon film, an amorphous boron nitride film, a monolayer amorphous molybdenum disulfide film, a monolayer amorphous tungsten disulfide film, a monolayer amorphous borophene film, a monolayer amorphous transition metal dichalcogenide film, a monolayer amorphous boron nitride carbon film, or a film or alloy doped with a heteroatom.

[0112] (C) The electronic device according to statement (A) or (B), wherein each of the one or more monoatomic amorphous films has a thickness selected from the range of 0.4 nm to 1 nm.

[0113] (D) The electronic device of any one of statements (A) to (C), wherein the one or more monoatomic amorphous films form a stack.

[0114] (E) The electronic device of any one of statements (A) to (D), further comprising a protective layer over the substrate.

[0115] (F) The electronic device of statement (E), wherein the protective layer comprises an oxide or a polymer.

[0116] (G) The electronic device of statement (F), wherein the oxide is aluminum oxide or hafnium oxide.

[0117] (H) The electronic device of statement (F), wherein the polymer is Parylene C.

[0118] (I) The electronic device of any one of statements (E) through (H), wherein the one or more monoatomic amorphous films are between the protective layer and the substrate.

[0119] (J) The electronic device of any one of statements (E) through (H), wherein the protective layer is between the one or more amorphous films and the substrate.

[0120] (K) The electronic device of any one of statements (A) through (J), wherein the electronic device is an organic light emitting diode or a thin film transistor.

[0121] (L) sp present in the one or more monoatomic layer amorphous films 3 / sp 2 The electronic device of any one of statements (A) through (K), wherein the bonding ratio is 0.1 or less.

[0122] (M) The oxygen permeation amount of the one or more monoatomic layer amorphous films is 10 -4 cc·m -2 ·day -1 and the water vapor permeability of the one or more monoatomic amorphous films is less than 10 -5 g m -2 ·day -1 The electronic device of any one of statements (A) through (L),

[0123] (N) A method of forming an electronic device, the method comprising forming a barrier comprising one or more layers of an atomically monolayer amorphous film over a substrate, the substrate comprising a suitable semiconductor material or a suitable polymeric material, the barrier configured to inhibit or reduce permeation of moisture or gas from the environment into the substrate.

[0124] (O) The method of statement (N), wherein the one or more monolayer amorphous films are formed on the substrate by a chemical vapor deposition process.

[0125] (P) The method of statement (O), wherein the chemical vapor deposition process is a laser chemical vapor deposition process.

[0126] (Q) The method of statement (O) or statement (P), wherein the temperature at which the chemical vapor deposition process is carried out is any suitable temperature below 300° C.

[0127] (R) The method of statement (N), wherein the one or more monoatomic amorphous films are formed as free-standing films prior to being transferred to the substrate.

[0128] (S) An electronic device comprising a first device structure comprising a conductive material, a second device structure comprising a further conductive or semiconducting material, and a barrier between the first device structure and the second device structure comprising one or more monoatomic layer amorphous films, the barrier being configured to inhibit or reduce interdiffusion between the first device structure and the second device structure.

[0129] (T) The electronic device of statement (S), wherein the conductive material is a metal, a metal alloy, a doped metal oxide, or a conductive carbon.

[0130] (U) The electronic device of statement (T), wherein the metal is copper or cobalt.

[0131] (V) The electronic device of any one of statements (S) to (U), wherein the additional conductive material is a metal, a metal alloy, a doped metal oxide, or a conductive carbon.

[0132] (W) The electronic device of any one of statements (S) to (V), wherein the semiconductor material is silicon.

[0133] (X) The electronic device of any one of statements (S) through (W), wherein the electronic device is a transistor, a diode, a memory device, an electromechanical device, an integrated circuit chip, a microprocessor, or an electronic detection device.

[0134] (Y) The electronic device of any one of statements (S) to (X), wherein the first device structure is an interconnect and the second device structure is a substrate.

[0135] (Z) The electronic device of any one of statements (S) to (X), wherein the first device structure is a first interconnect and the second device structure is a second interconnect.

[0136] (AA) sp present in the one or more monoatomic layer amorphous films 3 / sp 2 The electronic device of any one of statements (S) through (Z), wherein the bonding ratio is 0.1 or less.

[0137] (AB) A circuit arrangement comprising an electronic device described in any one of descriptions (S) to (AA).

[0138] (AC) A method of forming an electronic device, the method comprising forming a first device structure comprising a conductive material, forming a second device structure comprising a further conductive or semiconducting material, and forming a barrier between the first device structure and the second device structure comprising one or more layers of a monoatomic layer amorphous film, the barrier being configured to inhibit or reduce interdiffusion between the first device structure and the second device structure.

[0139] (AD) The method of claim (AC), wherein after forming the one or more monolayer amorphous films on the second device structure, the first device structure is formed on the one or more monolayer amorphous films, such that the one or more monolayer amorphous films are between the first device structure and the second device structure.

[0140] (AE) The method of statement (AC) or statement (AD), wherein the one or more monolayer amorphous films are formed by a chemical vapor deposition process.

[0141] (AF) The method according to statement (AE), wherein the chemical vapor deposition process is a laser chemical vapor deposition process.

[0142] (AG) The method of statement (AE) or statement (AF), wherein the temperature at which the chemical vapor deposition process is carried out is any suitable temperature below 300° C.

[0143] (AH) The method of claim (AC), wherein the one or more monolayer amorphous films are formed as free-standing films prior to being transferred onto the second device structure.

[0144] Although the present invention has been shown and described in detail with reference to specific embodiments, it will be understood by those skilled in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the invention as defined by the appended claims. The scope of the present invention is therefore defined by the appended claims, and all changes that come within the meaning and range of equivalence of the claims are intended to be embraced therein.

Claims

1. a substrate comprising a suitable semiconductor material or a suitable polymeric material; a barrier comprising one or more monolayer amorphous films overlying the substrate, each of the one or more monolayer amorphous films being an atomically thick layer having a thickness selected from the range of 0.4 nm to 1 nm, the one or more monolayer amorphous films having an sp 3 / sp 2 bonding ratio of 0.1 or less; An electronic device comprising: an electronic device, wherein each of said one or more monoatomic amorphous films is continuous and free of grain boundaries such that said barrier is configured to inhibit or reduce the permeation of moisture or gas from the environment into said substrate, and said one or more monoatomic amorphous films have a water vapor transmission rate of less than 10 −5 g·m −2 ·day −1 .

2. 2. The electronic device of claim 1, wherein the one or more monolayer amorphous films are a monolayer amorphous carbon film, an amorphous boron nitride film, a monolayer amorphous borophene film, or a monolayer amorphous boron carbon nitride film.

3. 3. The electronic device of claim 1, wherein the one or more monoatomic amorphous films form a stack.

4. The electronic device of claim 1 , further comprising a protective layer over the substrate.

5. The electronic device of claim 4 , wherein the protective layer comprises an oxide or a polymer.

6. The electronic device of claim 5 , wherein the oxide is aluminum oxide or hafnium oxide.

7. The electronic device of claim 5 or 6, wherein the polymer is Parylene C.

8. 8. The electronic device of claim 4, wherein the one or more monoatomic amorphous films are between the protective layer and the substrate.

9. 8. The electronic device of claim 4, wherein the protective layer is between the amorphous film or films and the substrate.

10. 10. The electronic device of claim 1, wherein the electronic device is an organic light emitting diode or a thin film transistor.

11. The organic light emitting diode, A first electrode; A second electrode; an organic light-emitting layer between the first electrode and the second electrode; Equipped with 11. The electronic device of claim 10, wherein the substrate is the second electrode or the organic light-emitting layer, and the barrier is disposed on the second electrode or on the organic light-emitting layer.

12. The thin film transistor, A semiconductor layer; a dielectric layer overlying the semiconductor layer; a gate electrode overlying the dielectric layer; a drain electrode and a source electrode at least partially embedded in the semiconductor layer and on a first surface of the dielectric layer; Equipped with 12. The electronic device of claim 10 or 11, wherein the gate electrode is on a second surface of the dielectric layer opposite the first surface.

13. The thin film transistor, A gate electrode; a dielectric layer overlying the gate electrode; a drain electrode and a source electrode on or above said dielectric layer; a semiconductor layer overlying the drain electrode and the source electrode; Equipped with 12. An electronic device according to claim 10 or 11, wherein the semiconductor layer is the substrate and the barrier is on or above the substrate.

14. The one or more monoatomic layer amorphous films are -4 C.C.M. -2 ・day -1 14. The electronic device of claim 1, having an oxygen permeation of less than 100 nm.

15. An electronic device as described in any one of claims 1 to 14, wherein the barrier is configured to inhibit or reduce penetration of the moisture or gas from the environment into the substrate by blocking ions or molecules larger than a proton.

16. 1. A method of forming an electronic device, the method comprising: forming a barrier on a substrate comprising one or more monolayer amorphous films, each of the one or more monolayer amorphous films being an atomically thick layer having a thickness selected from the range of 0.4 nm to 1 nm, and the one or more monolayer amorphous films having an sp3 / sp2 bonding ratio of 0.1 or less; the substrate comprises a suitable semiconductor material or a suitable polymeric material; wherein each of the one or more layers of monolayer amorphous films is continuous and free of grain boundaries such that the barrier is configured to inhibit or reduce the permeation of moisture or gas from the environment into the substrate, and the one or more layers of monolayer amorphous films have a water vapor transmission rate of less than 10 −5 g·m −2 ·day −1 .

17. 17. The method of claim 16, wherein the one or more monolayer amorphous films are formed on the substrate by a chemical vapor deposition process.

18. The method of claim 17 , wherein the chemical vapor deposition process is a laser chemical vapor deposition process.

19. 19. The method of claim 17 or 18, wherein the temperature at which the chemical vapor deposition process is carried out is any suitable temperature below 300°C.

20. 20. The method of any one of claims 16 to 19, wherein the one or more monoatomic amorphous films are formed as free-standing films prior to being transferred to the substrate.

21. 21. The method of any one of claims 16 to 20, wherein the electronic device is an organic light emitting diode or a thin film transistor.

22. The organic light emitting diode, A first electrode; A second electrode; an organic light-emitting layer between the first electrode and the second electrode; Equipped with 22. The method of claim 21, wherein the substrate is the second electrode or the organic light-emitting layer, and the barrier is disposed on the second electrode or on the organic light-emitting layer.

23. The thin film transistor, A semiconductor layer; a dielectric layer overlying the semiconductor layer; a gate electrode overlying the dielectric layer; a drain electrode and a source electrode at least partially embedded in the semiconductor layer and on a first surface of the dielectric layer; Equipped with 23. The method of claim 21 or 22, wherein the gate electrode is on a second side of the dielectric layer opposite the first side.

24. The thin film transistor, A gate electrode; a dielectric layer overlying the gate electrode; a drain electrode and a source electrode on or above said dielectric layer; a semiconductor layer overlying the drain electrode and the source electrode; Equipped with 23. The method of claim 21 or 22, wherein the semiconductor layer is the substrate and the barrier is on the substrate.

25. A method according to any one of claims 16 to 24, wherein the barrier is configured to inhibit or reduce permeation of the moisture or gas from the environment to the substrate by blocking ions or molecules larger than a proton.

26. a first device structure comprising a conductive material; a second device structure comprising a further conductive or semiconductive material; and a barrier between the first device structure and the second device structure and composed of one or more monoatomic amorphous films in contact with both device structures, the one or more monoatomic amorphous films being each a monoatomic layer having a thickness selected from a range of 0.4 nm to 1 nm, and the one or more monoatomic amorphous films having an sp 3 / sp 2 bond ratio of 0.1 or less; An electronic device comprising: each of the one or more monoatomic amorphous films is continuous and free of grain boundaries such that the barrier is configured to inhibit or reduce interdiffusion between the first device structure and the second device structure; An electronic device, wherein the first device structure is an interconnect and the second device structure is a substrate or a further interconnect.

27. 27. The electronic device of claim 26, wherein the conductive material is a metal, a metal alloy, a doped metal oxide, or a conductive carbon.

28. 28. The electronic device of claim 27, wherein the metal is copper or cobalt.

29. 29. The electronic device of any one of claims 26 to 28, wherein the further conductive material is a metal, a metal alloy, a doped metal oxide, or conductive carbon.

30. 30. The electronic device of any one of claims 26 to 29, wherein the semiconductor material is silicon.

31. 31. The electronic device of any one of claims 26 to 30, wherein the electronic device is a transistor, a diode, a memory device, an electromechanical device, an integrated circuit chip, a microprocessor, or an electronic sensing device.

32. A circuit arrangement comprising an electronic device according to any one of claims 26 to 31.

33. 1. A method of forming an electronic device, the method comprising: forming a first device structure comprising a conductive material; forming a second device structure comprising a further conductive or semiconductive material; forming a barrier between the first device structure and the second device structure, the barrier being comprised of one or more monolayer amorphous films therein, the one or more monolayer amorphous films being each a monoatomic thick layer having a thickness selected from the range of 0.4 nm to 1 nm, and the one or more monolayer amorphous films having an sp 3 / sp 2 bonding ratio of 0.1 or less; Equipped with each of the one or more monoatomic amorphous films is continuous and free of grain boundaries such that the barrier is configured to inhibit or reduce interdiffusion between the first device structure and the second device structure; The method, wherein the first device structure is an interconnect and the second device structure is a substrate or a further interconnect.

34. 34. The method of claim 33, wherein after forming the one or more monolayer amorphous films on the second device structure, the first device structure is formed on the one or more monolayer amorphous films, such that the one or more monolayer amorphous films are between the first device structure and the second device structure.

35. 35. The method of claim 33 or 34, wherein the one or more monolayer amorphous films are formed by a chemical vapor deposition process.

36. 36. The method of claim 35, wherein the chemical vapor deposition process is a laser chemical vapor deposition process.

37. 37. The method of claim 35 or 36, wherein the temperature at which the chemical vapor deposition process is carried out is any suitable temperature below 300°C.

38. 38. The method of any one of claims 33 to 37, wherein the one or more monoatomic amorphous films are formed as free-standing films before being transferred onto the second device structure.

Citation Information

Patent Citations

  • Semiconductor device

    JP2012033908A

  • Encapsulation method for organic electrical devices

    JP2012519936A

  • barrier coating

    JP2017511955A

  • Two-dimensional amorphous carbon coatings and methods for stem cell growth and differentiation - Patent Application 20070122997

    JP2020510590A

  • Semiconductor device

    US20120001170A1