Composite oxide powder, method for producing composite oxide powder, method for producing solid electrolyte body, and method for producing lithium ion secondary battery

A refined composite oxide powder with a cubic garnet structure and specific doping improves ionic conductivity, addressing the limitations of conventional solid electrolytes and enhancing battery performance.

JP7587220B2Active Publication Date: 2024-11-20FUJI SHIKISO +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020052231
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-24
Publication Date
2024-11-20
Estimated Expiration
2040-03-24

AI Technical Summary

Technical Problem

Conventional solid electrolytes for lithium ion secondary batteries have limitations in ionic conductivity and need further improvements to meet the demands for higher capacity and downsizing.

Method used

A composite oxide powder composed of lithium (Li), lanthanum (La), zirconium (Zr), and oxygen (O) with a cubic garnet type crystal structure, doped with gallium (Ga) and refined to a 50% diameter of 1000 nm or less, and a pyrochlore phase content of 10% by mass or less, is produced using a specific manufacturing process involving blending, firing, pulverization, and heat-treatment in organic solvents.

Benefits of technology

The resulting solid electrolyte body exhibits high ionic conductivity and density, enhancing the performance of lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587220000003
    Figure 0007587220000003
  • Figure 0007587220000004
    Figure 0007587220000004
  • Figure 0007587220000005
    Figure 0007587220000005
Patent Text Reader

Abstract

To provide a composite oxide powder capable of producing a solid electrolyte having high density and high ionic conductivity, and a method for producing the same.SOLUTION: A composite oxide powder comprises lithium (Li), lanthanum (La), zirconium (Zr), and oxygen (O), and is composed of particles having a cubic garnet-type crystal structure, in which the particles further contain only gallium (Ga) as a dopant element, and the composite oxide powder has a 50% diameter (D50) of 1000 nm or less in the volume particle size distribution and a pyrochlore phase content of 10 mass% or less.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite oxide powder, a method for producing the composite oxide powder, a method for producing a solid electrolyte body, and a method for producing a lithium ion secondary battery. [Background technology]

[0002] Lithium-ion secondary batteries are used as power sources for portable devices such as mobile phones and personal computers, as well as batteries for environmentally friendly vehicles (electric vehicles, etc.) and power storage systems for natural energy generation (wind power generation, etc.) In recent years, the demand for lithium-ion secondary batteries has been increasing due to the spread of portable devices and growing interest in environmental issues.

[0003] Lithium ion secondary batteries are required to have a high energy density. They are also required to operate safely and stably to prevent accidents such as fire. In this context, all-solid-state lithium ion secondary batteries that use solid electrolytes instead of liquid electrolytes have attracted attention. Most liquid electrolytes use flammable organic solvents. Therefore, lithium ion secondary batteries with liquid electrolytes cannot eliminate the risk of fire and are prone to leakage. In addition, there is a problem that the lithium (Li) component in the negative electrode grows in a dendritic shape during repeated charging and discharging, causing a short circuit between the positive electrode and the negative electrode. In contrast, batteries with solid electrolytes do not have such problems and are superior in terms of safety and reliability.

[0004] Garnet-type composite oxides have been proposed as solid electrolytes for all-solid-state lithium-ion secondary batteries. For example, Patent Document 1 discloses a stoichiometric composition of L 7+x A x G 3-x ZrO 12 [Wherein, L is Li + , Na + or K +A is an alkali metal ion selected from the group consisting of A, a divalent metal cation, G, a trivalent metal cation, 0≦x≦3, and O may be partially or completely replaced by a divalent anion (claim 1 of Patent Document 1). Patent Document 1 also discloses a solid ionic conductor having a garnet-like crystal structure having a stoichiometric composition of Li7La3Zr2O 12 It is described that the compound has an improved ionic conductivity compared to the compounds of the prior art, and can be used as a solid electrolyte for batteries having very high energy density (claim 6,

[0023] and

[0031] of Patent Document 1).

[0005] Patent Document 2 discloses an all-solid-state lithium secondary battery (claim 1 of Patent Document 2) that includes a positive electrode, a negative electrode, and a solid electrolyte containing ceramics having a garnet-type or garnet-like crystal structure composed of Li, La, Zr, and O. Patent Document 2 also describes that Li-La-Zr ceramics are excellent in lithium resistance and lithium ion conductivity, and are useful as a solid electrolyte for all-solid-state secondary batteries (

[0039] of Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 5634865 [Patent Document 2] JP 2010-45019 A Summary of the Invention [Problem to be solved by the invention]

[0007] There is a demand for batteries to be smaller and have higher capacity, and there is a demand for further improvements in the properties of solid electrolytes, particularly in ionic conductivity. However, the conventional solid electrolytes disclosed in Patent Documents 1 and 2 have room for improvement in order to meet this demand.

[0008] The present inventors have thoroughly investigated the production conditions for producing a cubic garnet-type composite oxide powder and have found that it is possible to obtain a fine powder with few heterogeneous phases, and that by using this powder, a dense solid electrolyte body having high ionic conductivity can be produced.

[0009] The present invention has been completed based on these findings, and an object of the present invention is to provide a composite oxide powder capable of producing a dense solid electrolyte body with high ionic conductivity, and a method for producing the same. Another object of the present invention is to provide a method for producing a solid electrolyte body and a lithium ion secondary battery using the composite oxide powder. [Means for solving the problem]

[0010] The present invention encompasses the following aspects (1) to (13). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."

[0011] (1) A composite oxide powder containing lithium (Li), lanthanum (La), zirconium (Zr), and oxygen (O) and composed of particles having a cubic garnet-type crystal structure, The particles further comprise only gallium (Ga) as a dopant element; The composite oxide powder has a 50% diameter (D50) in its volumetric particle size distribution of 1000 nm or less, and a content of the pyrochlore phase of 10 mass % or less.

[0012] (2) The composite oxide powder of (1) above, having a 50% diameter (D50) of 600 nm or less.

[0013] (3) The particles have the formula: Li 7-3x Ga x La3Zr2O 12 The composite oxide powder according to (1) or (2) above, having a basic composition represented by the following formula (where 0.1≦x≦0.5).

[0014] (4) The composite oxide powder according to any one of the above (1) to (3), wherein the particles further contain at least one dopant element selected from the group consisting of aluminum (Al), magnesium (Mg) and niobium (Nb).

[0015] (5) The composite oxide powder according to any one of the above (1) to (4), wherein the composite oxide powder has a half-width of a peak of a (211) diffraction line in an X-ray diffraction (XRD) profile of 0.50° or less.

[0016] (6) A method for producing a composite oxide powder according to any one of the above (1) to (5), comprising the following steps: preparing at least a lithium (Li) source, a lanthanum (La) source, a zirconium (Zr) source, and gallium (Ga) as raw materials; blending and mixing the ingredients to form a mixture; A step of calcining the mixture to obtain a calcined product; A step of pulverizing the fired product to obtain a pulverized product; and The pulverized material is subjected to a heat treatment to obtain a heat-treated material, The method according to claim 1, wherein the calcined product is pulverized in an organic solvent using a bead mill.

[0017] (7) The method according to (6) above, wherein lithium carbonate (Li2CO3) is used as the lithium (Li) source.

[0018] (8) The method according to (6) or (7) above, wherein when the raw materials are mixed, a lithium (Li) source is mixed in an amount of 1 to 20% by mass in excess of the stoichiometric composition of the garnet-type crystal structure.

[0019] (9) Any of the above methods (6) to (8), wherein, in firing the mixture, the mixture is subjected to a first firing at a temperature of 700 to 1000°C and then a second firing at a temperature of 900 to 1100°C.

[0020] (10) The method according to any one of the above (6) to (9), wherein the organic solvent is at least one selected from the group consisting of alcohol-based solvents, ketone-based solvents, ester-based solvents, glycol ether-based solvents, hydrocarbon-based solvents, ether-based solvents, glycol-based solvents, and amine-based solvents.

[0021] (11) The method according to (10) above, wherein the organic solvent is isopropyl alcohol (IPA) and / or toluene.

[0022] (12) A method for producing a solid electrolyte body, comprising the steps of: Providing a composite oxide powder; A step of forming the composite oxide powder into a molded body; and The molded body is sintered to obtain a sintered body, The method for preparing the composite oxide powder comprises producing the composite oxide powder by any one of the methods (6) to (11) above.

[0023] (13) A method for producing a lithium ion secondary battery, comprising the steps of: A step of preparing at least an exterior material, a positive electrode, a negative electrode, and a solid electrolyte body; and The positive electrode and the negative electrode are disposed in the exterior material so as to face each other, and a solid electrolyte body is disposed between the positive electrode and the negative electrode, The method for preparing the solid electrolyte body includes producing the solid electrolyte body by the method described above in (12). Effect of the Invention

[0024] According to the present invention, there are provided a composite oxide powder capable of producing a dense solid electrolyte body having high ionic conductivity, and a method for producing the same. [Brief description of the drawings]

[0025] [Figure 1] FIG. 2 is a diagram showing an X-ray diffraction profile of the fired product. [Diagram 2] FIG. 2 is an enlarged view showing an X-ray diffraction profile of the fired product. [Diagram 3]FIG. 2 is a view showing an SEM image of a fired product. [Figure 4] FIG. 2 is a view showing an SEM image of a fired product. [Diagram 5] FIG. 1 shows an SEM image of a pulverized product. [Figure 6] FIG. 2 is a diagram showing X-ray diffraction profiles of the fired product, the crushed product, and the heat-treated product. [Figure 7] FIG. 2 is a graph showing the particle size distribution of a heat-treated product (composite oxide powder). [Figure 8] FIG. 2 is a photograph showing the appearance of a sintered body (solid electrolyte body). [Figure 9] FIG. 1 is a diagram showing a Nyquist plot of the AC impedance of a sintered body (solid electrolyte body). [Figure 10] FIG. 2 is a diagram showing X-ray diffraction profiles of the fired product, the crushed product, and the heat-treated product. [Figure 11] FIG. 1 shows SEM images of a fired product and a heat-treated product. [Figure 12] FIG. 2 is a graph showing the particle size distribution of a heat-treated product (composite oxide powder). [Figure 13] FIG. 1 is a diagram showing a Nyquist plot of the AC impedance of a sintered body (solid electrolyte body). [Figure 14] FIG. 2 is a diagram showing an SEM image of a fracture surface of a sintered body (solid electrolyte body). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described below. However, the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.

[0027] Composite Oxide Powder The composite oxide powder of the present embodiment is composed of particles containing lithium (Li), lanthanum (La), zirconium (Zr), and oxygen (O) and having a cubic garnet-type crystal structure. The particles further contain only gallium (Ga) as a dopant element. Furthermore, the composite oxide powder has a 50% diameter (D50) in its volumetric particle size distribution of 1000 nm or less, and a pyrochlore phase content of 10 mass% or less.

[0028] Tetragonal and cubic crystal structures are known as crystal structures of garnet-type complex oxides. Among these, cubic garnet-type complex oxides are characterized by high lithium ion conductivity, excellent chemical stability, and a wide potential window. In addition, by using lithium (Li), lanthanum (La), zirconium (Zr), and oxygen (O) as the constituent elements of the complex oxide, the crystal structure becomes more stable and has excellent lithium resistance. Therefore, the complex oxide powder of this embodiment is useful as a solid electrolyte material for various applications, including lithium ion secondary batteries. In this specification, the term "particle" refers to individual grains, and the term "powder" refers to an aggregate of multiple particles that exhibits fluidity as a whole.

[0029] The particles constituting the complex oxide powder further contain only gallium (Ga) as a dopant element. In other words, the complex oxide powder (particles) contains lithium (Li), lanthanum (La), zirconium (Zr), gallium (Ga), and oxygen (O), with the remainder being unavoidable impurities. Here, unavoidable impurities refer to components that are inevitably mixed in during the manufacturing process and have a content of 5000 ppm or less. By replacing the elements constituting the particles (Li, etc.) with gallium (Ga), the properties of the complex oxide powder, such as ionic conductivity and sinterability, are further improved.

[0030] The particles constituting the composite oxide powder are represented by the formula: Li 7-3x Ga x La3Zr2O 12It is preferable that the basic composition has a stoichiometric composition (Li7La3Zr2O) of a garnet-type structure having lithium (Li), lanthanum (La), zirconium (Zr) and oxygen (O) as constituent elements. 12 LLZO) doped with gallium (Ga). This basic composition (stoichiometric composition) stabilizes the crystal structure of the composite oxide powder, and the ionic conductivity is further increased. In addition, by increasing the amount of gallium (Ga) x to a certain extent, the effect of gallium doping can be fully exerted. However, excessive inclusion of gallium may actually deteriorate the characteristics. Therefore, the amount of gallium x is preferably 0.1≦x≦0.5, and more preferably 0.2≦x≦0.4. Note that the composition of the particles does not need to be strictly stoichiometric. Due to the deviation in the composition during the blending of raw materials and the inclusion of impurities, a deviation of about ±10% is allowed. In addition, the composite oxide powder does not exclude the inclusion of components other than the particles having a garnet structure. Examples of such components include additives such as sintering aids.

[0031] The composite oxide powder of this embodiment has a 50% diameter (D50) in its volumetric particle size distribution of 1000 nm or less. By refining the composite oxide powder in this way, the sintered body (solid electrolyte body) made using this composite oxide powder becomes dense and the bulk resistance and grain boundary resistance become small. These combine to significantly increase the ionic conductivity of the sintered body (solid electrolyte body). D50 is preferably 750 nm or less, more preferably 600 nm or less, and even more preferably 500 nm or less. The lower limit of D50 is not particularly limited. However, D50 may be 200 nm or more, or 400 nm or more.

[0032] The composite oxide powder of the present embodiment has a pyrochlore phase content of 10% by mass or less. Here, the pyrochlore phase is a heterogeneous phase having a composition represented by the formula: La2Zr2O7. The lithium (Li) atoms constituting the garnet-type structure have a high vapor pressure and are highly reactive with water. Therefore, when the composite oxide powder is produced, the lithium (Li) atoms are easily released from the raw materials or the processed products through volatilization or dissolution in water. When the lithium (Li) is released, a large amount of the pyrochlore phase (La2Zr2O7) is generated in the composite oxide powder. This pyrochlore phase has a low ionic conductivity. Therefore, when a large amount of the pyrochlore phase is generated, the ionic conductivity of the composite oxide powder is deteriorated. By suppressing the content of the pyrochlore phase in the composite oxide powder to a low level, the ionic conductivity is excellent. The content of the pyrochlore phase is preferably 10% by mass or less, more preferably 5% by mass or less. The content may be 0% by mass.

[0033] The particles constituting the composite oxide powder may further contain at least one dopant element selected from the group consisting of aluminum (Al), magnesium (Mg) and niobium (Nb). By replacing the elements constituting the particles (Li, La, Zr and O) with the above-mentioned dopant elements, the properties of the composite oxide powder, such as ionic conductivity and sinterability, may be improved. However, excessive inclusion of the dopant element may rather deteriorate the properties. Therefore, the content of the dopant element is set to Li7La3Zr2O 12 The molar ratio to (LLZO) is preferably from 0.1 to 0.5, and more preferably from 0.2 to 0.3.

[0034] The composite oxide powder preferably has a peak half-width of the (211) diffraction line in its X-ray diffraction (XRD) profile of 0.50° or less. The garnet-type structure shows two strong peaks in the X-ray diffraction profile, a (211) diffraction line and a (420) diffraction line. For example, when CuKα is used as a radiation source, the (211) diffraction line appears near 2θ=16.7°, and the (420) diffraction line appears near 2θ=30.8°. Therefore, the half-width of the (211) diffraction line can be used as an index of the crystallinity of the garnet structure. The composite oxide powder with a small peak half-width of the (211) diffraction line has excellent crystallinity and even more excellent ionic conductivity. The peak half-width is preferably 0.40° or less, more preferably 0.30° or less. The peak half-width is typically 0.05° or more, more typically 0.10° or more.

[0035] Method for producing composite oxide powder The method for producing the composite oxide powder of this embodiment includes the following steps: a step of preparing at least a lithium (Li) source, a lanthanum (La) source, a zirconium (Zr) source, and a gallium (Ga) source as raw materials (raw material preparation step), a step of blending and mixing these raw materials to form a mixture (raw material mixing step), a step of firing this mixture to form a fired product (firing step), a step of pulverizing this fired product to form a pulverized product (pulverization step), and a step of heat-treating this pulverized product to form a heat-treated product (heat treatment step). When pulverizing the fired product, the fired product is pulverized in an organic solvent using a bead mill. Details of each step are described below.

[0036] <Raw material preparation process> In the raw material preparation step, at least a lithium (Li) source, a lanthanum (La) source, a zirconium (Zr) source, and a gallium (Ga) source are prepared as raw materials. Known ceramic raw materials can be used as raw materials. Examples of such raw materials include metal oxides, metal hydroxides, carbonates, nitrates, organometallic compounds, and / or metals. However, metal oxides, metal hydroxides, carbonates, and / or hydrates thereof, which are inexpensively available and easy to handle, are preferred. For example, lithium carbonate (Li2CO3), lithium hydroxide (LiOH), and / or lithium oxide (Li2O) can be used as the lithium (Li) source. Also, lanthanum carbonate (La2(CO3)3), lanthanum hydroxide (La(OH)3), and / or lanthanum oxide (La2O3) can be used as the lanthanum (La) source. Zirconium oxide (ZrO2) can be used as the zirconium (Zr) source. Gallium oxide (Ga2O3) can be used as the gallium (Ga) source.

[0037] It is preferable to use lithium carbonate (Li2CO3) as the lithium (Li) source. By using lithium carbonate (Li2CO3), the garnetization reaction proceeds more in the subsequent firing process than when lithium hydroxide (LiOH) is used, and a fired product or composite oxide powder with fewer impurities can be obtained. Furthermore, lithium carbonate (Li2CO3) is less hygroscopic than lithium hydroxide (LiOH) and is easier to handle.

[0038] <Raw material mixing process> In the raw material mixing process, the prepared raw materials are mixed and blended to form a mixture. The blending ratio should be such that a composite oxide powder of the desired composition is obtained. For example, the basic composition (Li 7-3x Ga x La3Zr2O 12When preparing a garnet-type composite oxide of Li, Ga, La and Zr, the atomic ratio of Li, Ga, La and Zr should be 7-3x:x:3:2. However, as described later, it is preferable to mix an excess of Li in anticipation of the volatilization of Li during the firing process. Mixing can be performed by a known method used in the field of ceramics manufacturing. Examples of mixing devices include a mortar, a mortar and pestle machine, a Henschel mixer, a ball mill and a vibration mill. Mixing can be performed by either or both of a wet method and a dry method.

[0039] When mixing the raw materials, it is preferable to mix the lithium (Li) source in an amount of 1 to 20 mass% in excess of the stoichiometric composition of the garnet-type crystal structure. Lithium (Li) has a high vapor pressure and is a component that is easily volatilized in the subsequent firing process. If the fired product becomes lithium (Li) deficient due to volatilization, the pyrochlore phase (La2Zr2O7), which causes deterioration of ionic conductivity, is likely to be formed. Therefore, in order to compensate for the lithium (Li) volatilization in the firing process, it is preferable to mix the lithium (Li) source in excess in the mixing process. If the amount of excess is too small, the volatilization of lithium (Li) is not sufficiently compensated. On the other hand, if the amount of excess is too large, a different phase containing an excess of lithium (Li) may be formed in the fired product. Therefore, the amount of excess is preferably 1 to 20 mass%, more preferably 5 to 15 mass%, and even more preferably 6 to 10 mass%.

[0040] <Firing process> In the firing step, the mixture is fired (calcined) to produce a fired product (calcined product). Firing is performed to generate a garnet-type composite oxide by thermally decomposing the raw materials and promoting the reaction between the raw materials. For example, when carbonates or hydroxides are used as raw materials, carbon dioxide gas and moisture are removed in the early stage of firing. After that or at the same time, the components in the raw materials react with each other to generate a garnet-type composite oxide. In order to promote the thermal decomposition and reaction of the raw materials, it is desirable to perform firing at a relatively high temperature for a long time. The firing temperature is preferably 700°C or higher, more preferably 800°C or higher, and even more preferably 900°C or higher. In addition, the holding time of firing is preferably 6 hours or more, more preferably 8 hours or more, and even more preferably 10 hours or more. On the other hand, if firing proceeds excessively, the grain growth of the fired product proceeds too much, which may make it difficult to grind in the subsequent grinding step. Therefore, the firing temperature is preferably 1200°C or lower, more preferably 1150°C or lower, and even more preferably 1100°C or lower. The retention time is preferably 16 hours or less, more preferably 14 hours or less, and even more preferably 12 hours or less.

[0041] The firing atmosphere is not particularly limited as long as a garnet-type composite oxide can be obtained. However, an oxygen-containing atmosphere such as air or an oxygen atmosphere is preferred, and air is particularly preferred. Furthermore, firing may be performed by a known method used in the field of ceramics manufacturing. For example, the raw material mixture may be placed in a crucible or setter, and fired in that state in a firing furnace. A known furnace may be used as the firing furnace.

[0042] The mixture may be fired only once, but it is preferable to fire it several times, for example, twice. By firing it several times, the garnetization reaction of the mixture proceeds more. Therefore, the crystallinity of the fired product is excellent, and the generation of impurity phases is suppressed. When firing the mixture, it is particularly preferable to perform the first firing at a temperature of 700 to 1000°C, and then the second firing at a temperature of 900 to 1100°C. When firing is performed several times, the holding time for each firing may be within the above-mentioned range (e.g., 16 hours or less).

[0043] <Crushing process> In the grinding process, the obtained fired product is ground to obtain a ground product. When grinding the fired product, a bead mill is used to grind the fired product in an organic solvent. The bead mill is a device for grinding and dispersing inorganic powders, and is composed of a grinding chamber and a rotor (agitator) provided in the grinding chamber. A large number of grinding media are filled in the gap between the inner wall of the grinding chamber and the rotor. Small diameter beads made of ceramics such as zirconium oxide are used as the grinding media. When grinding is performed in a wet manner, a grinding solvent is introduced into the grinding chamber together with the treated powder. During grinding, the treated powder is introduced into the grinding chamber and the rotor is rotated at high speed. When the rotor is rotated at high speed, the beads are agitated. As a result, the beads collide with other beads, the inner wall of the grinding chamber, and the rotor at high speed. As a result, strong impact forces and shear forces are applied to the treated powder between the beads and between the beads and the inner wall of the grinding chamber, which causes the treated powder to be ground. Compared to other grinding devices such as ball mills, the diameter of the grinding media in the beer mill is small and moves at high speed. Therefore, it is an effective method for finely pulverizing the treated powder.

[0044] There are two types of pulverization using a bead mill: dry pulverization and wet pulverization. In this embodiment, wet pulverization is performed in an organic solvent. The treated powder is finer in wet pulverization than in dry pulverization. This is because agglomeration of the treated powder is unavoidable in dry pulverization, and impact and shear forces are not effectively applied to each particle during pulverization. In addition, even in wet pulverization, pulverization in water is not preferable. This is because the lithium (Li) component contained in the fired product, which is the treated powder, dissolves in water and escapes. A method of drying the entire amount of the treated powder after pulverization is also possible, but in that case, the lithium (Li) component segregates in the pulverized product after drying, making it impossible to obtain a garnet-type composite oxide with a uniform composition. In contrast, by performing bead mill pulverization in an organic solvent, it is possible to prevent the lithium (Li) component from dissolving from the pulverized product, and to obtain a fine pulverized product with a uniform composition.

[0045] The organic solvent may be an alcohol solvent such as methanol, ethanol, butanol, hexanol, benzyl alcohol, or isopropyl alcohol (IPA); a ketone solvent such as acetone, methyl ethyl ketone, methyl isobutyl ketone, or cyclohexanone; an ester solvent such as methyl acetate, ethyl acetate, or butyl acetate; a glycol ether solvent such as propylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, 3-methoxy-3-methyl-1-butanol, or diethylene glycol monobutyl ether; benzene, toluene, xylene, cyclohexane, methylcyclohexane, ethyl At least one selected from the group consisting of hydrocarbon solvents such as cyclohexane, mineral oil, normal paraffin, and isoparaffin, ether solvents such as 1,3-dioxolane, 1,4-dioxane, and tetrahydrofuran, glycol solvents such as ethylene glycol, diethylene glycol, propylene glycol, and polyethylene glycol, and amine solvents such as monoethanolamine, diethanolamine, triethanolamine, n-methyl-2-pyrrolidone, 2-amino-2-methyl-1-propanol, and N,N-dimethylformamide is preferred, and isopropyl alcohol (IPA) and / or toluene are particularly preferred. Water, which is highly hydrophilic, may dissolve lithium (Li) and destroy the crystallinity of LLZO constituting the fired product, but the above-mentioned organic solvents are highly hydrophobic, so lithium (Li) is less likely to dissolve, making it easier to maintain the crystallinity of LLZO.

[0046] <Heat treatment process> In the heat treatment step, the obtained pulverized material is heat-treated to obtain a heat-treated material. The pulverized material after the pulverization step contains crystal distortion caused by the pulverization process. The pulverized material containing crystal distortion has low crystallinity and is inferior in properties such as ion conductivity. By restoring the crystallinity in the heat treatment step, a composite oxide powder with fine and high properties can be obtained. In order to restore the crystallinity, it is effective to perform a long-term heat treatment at a certain high temperature. Therefore, the heat treatment temperature is preferably 200°C or higher, more preferably 300°C or higher, and even more preferably 400°C or higher. In addition, the holding time of the heat treatment is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 1.5 hours or more. On the other hand, if the heat treatment is performed excessively, the grain growth of the pulverized material may progress, and the obtained composite oxide powder may become coarse. Therefore, the heat treatment temperature is preferably 1000°C or lower, more preferably 900°C or lower, and even more preferably 800°C or lower. In addition, the holding time is preferably 4 hours or less, more preferably 3 hours or less, and even more preferably 2 hours or less. The heat treatment atmosphere is not particularly limited as long as the garnet structure is maintained, but is preferably an oxygen-containing atmosphere such as air or an oxygen atmosphere, and more preferably air.

[0047] According to the method of the present embodiment, it is possible to produce an excellent composite oxide powder that is fine, has few heterogeneous phases, and has high crystallinity. By using such an excellent composite oxide, it is possible to produce a solid electrolyte that is dense and has high ionic conductivity.

[0048] Manufacturing method of solid electrolyte body The method for producing the solid electrolyte body of this embodiment includes the following steps: a step of preparing a composite oxide powder (composite oxide powder preparation step), a step of molding the composite oxide powder into a molded body (molding step), and a step of firing the molded body into a sintered body (main firing step). When preparing the composite oxide powder, the composite oxide powder is produced by the above-mentioned method. Each step will be described in detail below.

[0049] <Composite oxide powder preparation process> First, the composite oxide powder is prepared by the above-mentioned method.

[0050] <Forming process> In the molding step, the obtained composite oxide powder is molded into a molded body. The molding may be performed by a known method used in the field of ceramics manufacturing, such as press molding and doctor blade method.

[0051] <Main firing process> In the firing step, the obtained molded body is fired (fired) to form a sintered body. The firing may be performed by a known method used in the field of ceramics manufacturing. For example, the molded body is held at 1000 to 1300°C for 10 to 20 hours. However, it is preferable to fire the molded body while it is embedded in LLZO powder. This can prevent the lithium (Li) component from volatilizing from the molded body.

[0052] If necessary, the obtained sintered body may be processed by a known method used in the field of ceramics manufacturing, for example, polishing, grinding or cutting the sintered body.

[0053] In this manner, a solid electrolyte body can be obtained. This solid electrolyte body is dense and has excellent ionic conductivity, and is therefore useful as a solid electrolyte body for lithium ion secondary batteries, oxygen sensors, or electric double layer capacitors.

[0054] Manufacturing method of lithium-ion secondary battery The method for producing a lithium ion secondary battery of this embodiment includes the following steps: preparing at least an exterior material, a positive electrode, a negative electrode, and a solid electrolyte body, and disposing the positive electrode and the negative electrode in the exterior material so as to face each other, and disposing the solid electrolyte body between the positive electrode and the negative electrode. When preparing the solid electrolyte body, the solid electrolyte body is produced by the above-mentioned method.

[0055] Known materials used in lithium ion secondary batteries can be used for the exterior material, positive electrode, and negative electrode. For example, a container made of metal or resin can be used for the exterior material. In addition, a positive electrode can be used in which a positive electrode active material made of manganese oxide, lithium manganese composite oxide, lithium nickel composite oxide, or lithium cobalt composite oxide is applied to a positive electrode current collector. In addition, a negative electrode can be used in which a negative electrode active material made of metallic lithium or a lithium compound is applied to a negative electrode current collector.

[0056] The lithium ion secondary battery of this embodiment includes a solid electrolyte body that is dense and has excellent ionic conductivity, and therefore has high output. EXAMPLES

[0057] The present embodiment will be described in more detail with reference to the following examples, but the present invention is not limited to the following examples.

[0058] [Experimental Example 1] In Experimental Example 1, starting materials for Al-doped LLZO were mixed and fired to produce a fired product. Here, the effects of the type of starting materials and firing conditions were investigated.

[0059] (1) Preparation of fired products Example 1-1 (reference example) <Raw material mixing process> As starting materials, powders of lithium carbonate (Li2CO3), lanthanum oxide (La2O3), zirconium oxide (ZrO2) and aluminum oxide (Al2O3) were prepared. 6.25 Al 0.25 La3Zr2O 12 The starting materials were blended so that the lithium source (lithium carbonate) was in excess of 6 mass% relative to the starting materials. The blended starting materials were then mixed in an alumina mortar. Isopropyl alcohol (IPA) was added to the starting materials during mixing.

[0060] <Firing process> The obtained mixture was placed in an alumina crucible and fired (pre-fired) to obtain a fired product (pre-fired product). At this time, firing was carried out once under the conditions of 1000 °C × 12 hours.

[0061] Example 1-2 (Reference Example) Firing was carried out twice during the firing process. Otherwise, a fired product was prepared in the same manner as in Example 1-1.

[0062] Example 1-3 (Reference Example) During the raw material mixing process, lithium hydroxide monohydrate (LiOH·H2O) was used instead of lithium carbonate (Li2CO3) as the lithium source. Otherwise, a fired product was prepared in the same manner as in Example 1-1.

[0063] Example 1-4 (Reference Example) Firing was carried out twice during the firing process. Otherwise, a fired product was prepared in the same manner as in Example 1-3.

[0064] (2) Evaluation For Examples 1-1 to 1-4, various properties were evaluated as follows.

[0065] <X-ray Diffraction> The obtained fired product was analyzed by powder X-ray diffraction to identify the crystal phase in the fired product. The analysis conditions were as follows.

[0066] - X-ray diffractometer: Bruker D2 Phaser - Radiation source: CuKα radiation - Tube voltage: 30 kV - Tube current: 10 mA - Scan speed: 2.4° / min - Scan range (2θ): 10 to 70°

[0067] <SEM Observation> The fired product was observed using a scanning electron microscope (SEM; SIRION manufactured by FEI). The observation was carried out under the conditions of 2000 times or 20000 times magnification.

[0068] (3) Evaluation Results X-ray diffraction patterns of the fired products of Examples 1-1 to 1-4 are shown in Figures 1 and 2. Figure 2 is an enlarged view of Figure 1. In Figures 1 and 2, the "◯" marks indicate the diffraction lines of the cubic garnet phase (LLZO), the "▽" marks indicate the diffraction lines of the pyrochlore phase (La2Zr2O7), and the "×" marks indicate the diffraction lines of the impurity phase.

[0069] As shown in FIG. 1, in all samples (Example 1-1 to Example 1-4), cubic garnet-type compounds (marked with "◯" in the figure) were formed as the main phase. Samples (Example 1-1 and Example 1-3) that were fired once contained impurity phases (marked with "X" in the figure). On the other hand, in samples (Example 1-2 and Example 1-4) that were fired twice, in addition to narrowing the XRD peak and reducing background noise, the impurity phases (marked with "X" in the figure) disappeared, and a small amount of pyrochlore phase (marked with "▽" in the figure) was formed. The impurity phases (marked with "X" in the figure) are phases that contain excess lithium (Li), and it is presumed that the pyrochlore phase was formed by the volatilization of lithium (Li) by the second firing. Therefore, in order to obtain a single cubic garnet phase by firing twice, it is considered appropriate to set the excess amount of lithium (Li) source added at the time of blending to about 8 mass%. In addition, the sample (Example 1-2) that used lithium carbonate (Li2CO3) as the lithium (Li) source had a smaller amount of impurity phase than the sample (Example 1-4) that used lithium hydroxide monohydrate (LiOH·H2O).

[0070] SEM photographs of Examples 1-2 and 1-4 are shown in Figures 3 and 4. The influence of the microstructure due to the difference in the lithium (Li) source was observed from the SEM photographs. Specifically, the sample using lithium carbonate (Li2CO3) (Example 1-2) showed a structure in which angular particles of about 10 μm in size were fused on the surface (Figure 3). In contrast, the sample using lithium hydroxide monohydrate (LiOH·H2O) (Example 1-4) showed a structure in which small spherical particles of 2 to 3 μm in diameter were fused (Figure 4). It is thought that Example 1-2 has a shape that more closely reflects the characteristics of cubic crystals. The details of the reason for the difference in the microstructure are unknown, but it is thought to be related to the melting points of the lithium sources (Li2CO3: 723°C, LiOH: 462°C).

[0071] From these results, it is considered preferable to use lithium carbonate (Li2CO3) as the lithium (Li) source, set the excess amount of lithium (Li) added (mixture amount) to about 6 mass%, and perform firing twice at 1000°C for 12 hours in order to produce a cubic garnet-type LLZO compound with high purity.

[0072] [Experimental Example 2] In Experimental Example 2, Al-doped LLZO was sintered and crushed and heat-treated to produce a composite oxide powder, and the effects of the crushing and heat-treatment conditions were investigated.

[0073] (1) Preparation of composite oxide powder Example 2-1 (Comparative Example) <Crushing process> The fired product obtained in Example 1-2 of Experimental Example 1 was pulverized in water (H2O) using a wet bead mill. The pulverization conditions were as follows: pulverization chamber capacity: 1.2 L, pulverization media: zirconia beads (0.8 mmφ), bead filling rate: 80 volume %, agitator tip speed: 10 m / sec, flow rate: 1500 mL / min. The pulverization solvent (water) was added in an amount (20 L) that was 20 mass % of the fired product. The pulverization time was 0.5, 1.0, or 2.0 hours. Thus, a pulverized product was obtained. When pulverized in water (H2O), the pulverized product was considerably aggregated after 2.0 hours of pulverization, so pulverization was not performed for more than 2.0 hours.

[0074] <Heat treatment process> The resulting pulverized material was subjected to a heat treatment at 700°C for 4 hours to obtain a composite oxide powder.

[0075] Example 2-2 (reference example) The fired product was pulverized in isopropyl alcohol (IPA) for 0.5, 1.0, 2.0 or 4.0 hours, and heat-treated at 400° C. for 2 hours. Other than that, the composite oxide powder was produced in the same manner as in Example 2-1.

[0076] Example 2-3 (reference example) The fired product was pulverized in toluene for 4.0 hours and heat-treated under the conditions of 400 °C for 2 hours. Otherwise, the composite oxide powder was prepared in the same manner as in Example 2-1.

[0077] (2) Evaluation For Examples 2-1 to 2-3, the evaluation of various properties was conducted as follows.

[0078] <X-ray Diffraction> The obtained pulverized product and composite oxide powder were analyzed by powder X-ray diffraction method to identify the crystal phase. The analysis conditions were the same as those in Experimental Example 1.

[0079] <Particle Size Distribution> The particle size distribution of the composite oxide powder was determined by optical particle size distribution measurement. The measurement was carried out as follows. That is, the powder sample was put into pure water and dispersed with an ultrasonic disperser for 5 minutes, and then measured using a laser diffraction particle size distribution analyzer (manufactured by Shimadzu Corporation, SALD-1100).

[0080] <SEM Observation> The pulverized product and composite oxide powder were observed using a scanning electron microscope (SEM; manufactured by FEI, SIRION).

[0081] (3) Evaluation Results

[0082] For Example 2-1 and Example 2-2, the SEM photographs of the pulverized product are shown in FIGS. 5(a) to (f). Here, each of (a), (b), and (c) is an SEM photograph of the sample (Example 2-2) pulverized in isopropyl alcohol (IPA) for 0.5, 1.0, or 2.0 hours. Also, each of (d), (e), and (f) is an SEM photograph of the sample (Example 2-1) pulverized in water (H2O) for 0.5, 1.0, or 2.0 hours.

[0083] As shown in Figures 5(a)-(f), the sample (Example 2-2) ground in isopropyl alcohol (IPA) was ground to particles of approximately 1 μm or less after 0.5 hours of treatment (Figure 5(a)). By increasing the treatment time to 1.0 and 2.0 hours, the grinding appears to have progressed further (Figures 5(b) and (c)). In contrast, the sample (Example 2-1) ground in water (H2O) was ground to about 1 μm, but the particle size was somewhat larger than when ground in IPA. Aggregation of the ground particles was also observed (Figures 5(d)-(f)).

[0084] FIG. 6 shows the X-ray diffraction patterns of the fired product, pulverized product and heat-treated product (composite oxide powder) for Examples 2-1 to 2-3.

[0085] As shown in Figure 6, the diffraction lines of the sample (Example 2-1) ground in water (H2O) are shifted to the higher angle side in the ground product, indicating that the crystal lattice has contracted. In addition, peaks of impurity phases (marked with "x" in the figure) are visible. In the heat-treated product obtained by heat-treating this ground product, the shift to higher angles disappears, but the peak due to the pyrochlore phase (marked with "▽" in the figure) becomes larger. It is believed that when ground in water (H2O), the heat treatment produced the pyrochlore phase from the LLZO crystals from which lithium (Li) had dissolved. In fact, it has been confirmed that the water (H2O) used as the solvent exhibits strong alkalinity after grinding, which supports the dissolution of lithium (Li).

[0086] In the sample (Example 2-2) ground in isopropyl alcohol (IPA), the diffraction angle (2θ) of the (211) diffraction line was 16.74° in the fired state, whereas the diffraction angle was 16.58° in the ground state. This indicates that the peak shifted to a lower angle side and the lattice expanded due to grinding. No new impurities were generated. In the composite oxide powder in which the impurities were heat-treated, the diffraction angle of the (211) diffraction line was 16.68°, and the peak shift was mitigated. Although the generation of the pyrochlore phase was confirmed, the content ratio estimated from the peak intensity ratio of the X-ray diffraction was only about 3 mass%. Furthermore, the peak half-width of the (211) diffraction line was 0.25°.

[0087] The sample (Example 2-3) ground in toluene for 4 hours retains the cubic garnet structure. The diffraction lines are shifted slightly to the lower angle side, which indicates that the crystal lattice is expanded. By subjecting the ground material to heat treatment at 400°C for 2 hours, the shift in the diffraction lines disappeared, and impurity phases such as pyrochlore were not produced by grinding in toluene.

[0088] From the above results, it is believed that when the grinding process is performed using water (H2O) as a solvent, the lithium (Li) ions in LLZO dissolve into the water, causing the crystal lattice to shrink. It is also believed that even with the subsequent heat treatment, the lithium (Li) ions do not completely return to the crystal lattice, and the dissolved lithium (Li) ions crystallize as a pyrochlore phase (La2Zr2O7). In contrast, when the grinding process is performed in an organic solvent such as isopropyl alcohol (IPA) or toluene, the crystal lattice expands slightly after grinding, and returns to its original shape by heat treatment. Although the detailed mechanism is unknown, it is believed that the role of the solvent in the fine-graining process is important.

[0089] For Example 2-2, which was prepared by pulverization in IPA, the particle size distribution of the heat-treated product (pulverization for 2 hours + heat treatment at 700°C for 4 hours) is shown in Figure 7. The 50% diameter (D50) was 0.4 μm, and approximately 80% of the particles had a particle diameter of 1 μm or less.

[0090] [Experimental Example 3] In Experimental Example 3, a composite oxide powder was prepared from Al-doped LLZO, which was then molded and sintered to prepare a sintered body (solid electrolyte body). The sinterability and ionic conductivity were then evaluated.

[0091] (1) Preparation of sintered body Example 3-1 (reference example) <Raw material mixing process> As starting materials, lithium carbonate (Li2CO3), lanthanum oxide (La2O3), and zirconium oxide (ZrO2) powders were prepared. Formula: Li 7-3x Al x La3Zr2O 12 The starting materials were blended so that the aluminum (Al) doping amount x was 0.3 and the excess amount of the lithium source (lithium carbonate) was 10 mass% in the composition represented by the formula (1). The blended starting materials were then mixed in an alumina mortar. Isopropyl alcohol (IPA) was added to the starting materials during mixing.

[0092] <Firing process> The resulting mixture was placed in an alumina crucible and fired to produce a fired product. The firing was performed once at 900°C for 12 hours and once at 1035°C for 12 hours.

[0093] <Crushing process> The obtained fired product was pulverized in isopropyl alcohol (IPA) using a wet bead mill. Zirconia beads (0.8 mmφ) were used as the pulverization medium. The pulverization time was 4.0 hours. As a result, a pulverized product was obtained.

[0094] <Heat treatment process> The obtained pulverized material was subjected to a heat treatment. The heat treatment was carried out under the conditions of 400°C x 2 hours. As a result, a composite oxide powder was obtained. The obtained composite oxide powder had a particle size of 0.3 to 0.5 μm (D50 was 0.41 μm).

[0095] <Forming process> The obtained composite oxide powder was press-molded. The molding was carried out using a die with a diameter of 17 mm under the condition of 200 MPa. As a result, a disk-shaped molded body was obtained.

[0096] <Main firing process> The obtained molded body was placed in an alumina crucible in a state of being embedded in LLZO powder, and this was subjected to main firing. The main firing was carried out under the conditions of 1150 °C or 1250 °C × 12 hours. As a result, a sintered body was obtained.

[0097] Example 3-2 (Reference example) The pulverization time was set to 3 hours, and the heat treatment was carried out under the conditions of 800 °C × 3 hours. Otherwise, the composite oxide powder and the sintered body were produced in the same manner as in Example 3-1.

[0098] Example 3-3 (Comparative example) The fired product was not subjected to pulverization treatment and heat treatment. Otherwise, the composite oxide powder and the sintered body were produced in the same manner as in Example 3-1. The obtained composite oxide powder had a particle size of 1 to 10 μm.

[0099] Example 3-4 (Comparative example) The starting materials were blended so that the aluminum (Al) doping amount x was 0.25. Otherwise, the composite oxide powder and the sintered body were produced in the same manner as in Example 3-3. The obtained composite oxide powder had a particle size of 1 to 10 μm. (2) Evaluation For Examples 3-1 to 3-4, the evaluation of various properties was carried out as follows.

[0100] <X-ray diffraction> The obtained fired product and pulverized product were analyzed by powder X-ray diffraction method to identify the crystal phase. The analysis conditions were the same as those in Experimental Example 1.

[0101] <Appearance observation> The appearance of the sintered body was observed visually.

[0102] <Sintered body density> The dimensions (diameter, thickness) and mass of the sintered body were measured, and the density was calculated. Also, the theoretical density of LLZO (5.14 g / cm3 ) was used to calculate the relative density.

[0103] <Ionic conductivity> The ionic conductivity of the sintered body was measured by the AC impedance method. First, both sides of the sintered body were polished, and gold was evaporated by sputtering to prepare a measurement sample. The measurement was performed at room temperature using an impedance analyzer (Solartron, 1260A).

[0104] (3) Evaluation results 8 shows external photographs of the sintered bodies of Examples 3-1 to 3-4 produced at a firing temperature of 1250° C. Example 3-1 was almost white, but Examples 3-2, 3-3, and 3-4 were colored with a beige color in that order.

[0105] For Examples 3-1 to 3-4, the density and relative density of the sintered bodies produced at firing temperatures of 1150° C. or 1250° C. are shown in Table 1. As shown in Table 1, when compared at the same firing temperature, Examples 3-1 and 3-2, which used fine particles as the raw material, have higher density and are sintered more densely than Examples 3-3 and 3-4, which used particles with a particle size of several μm as the raw material.

[0106] [Table 1]

[0107] Figure 9 shows the Nyquist plot of the AC impedance of the sintered bodies produced at a sintering temperature of 1250°C for Examples 3-1 to 3-4. As shown in Figure 9, in Examples 3-1 and 3-2, in which finely divided powder was sintered, the semicircle on the left side (high frequency side) is smaller due to bulk resistance compared to Examples 3-3 and 3-4. This shows that the bulk ionic conductivity is improved by sintering the finely divided powder. The bulk ionic conductivity calculated from the impedance results was 3.8 x 10 in Example 3-1. -4 Scm -1 , 4.7 × 10 in Example 3-2 -4 Scm -1 In Example 3-3, the -4Scm -1 , 2.8 × 10 in Example 3-4 -4 Scm -1 It was.

[0108] 9, the second semicircle due to the grain boundary resistance is clearly seen in Examples 3-3 and 3-4, whereas the second semicircle is not clearly seen in Examples 3-1 and 3-2. This shows that the grain boundary resistance is smaller in Examples 3-1 and 3-2.

[0109] [Experimental Example 4] In Experimental Example 4, the starting materials for Ga-doped LLZO were mixed and fired to produce a fired product, which was then pulverized and heat-treated to produce a composite oxide powder.

[0110] (1) Preparation of composite oxide powder Example 4-1 (Working Example) <Raw material mixing process> As starting materials, powders of lithium carbonate (Li2CO3), lanthanum oxide (La2O3), zirconium oxide (ZrO2) and gallium oxide (Ga2O3) were prepared. Formula: Li 7-3x Ga x La3Zr2O 12 The starting materials were blended so that the amount of gallium (Ga) x was 0.3 and the amount of excess lithium source (lithium carbonate) added was 10 mass% in the composition represented by the formula (1). The blended starting materials were then mixed in an alumina mortar. Isopropyl alcohol (IPA) was added to the starting materials during mixing.

[0111] <Firing process> The resulting mixture was placed in an alumina crucible and fired to produce a fired product. The firing was performed once at 900°C for 12 hours, after which the fired mixture was crushed and wet mixed, and then fired once at 1035°C for 12 hours. This resulted in Li 6.1 Ga 0.3 La3Zr2O 12 Ga-LLZO powder (sintered product) of the following composition was obtained.

[0112] <Crushing process> The obtained Ga-LLZO powder was pulverized. The pulverization was carried out in isopropyl alcohol (IPA) using a wet bead mill. Zirconia beads (0.8 mmφ) were used as the pulverization medium, and the pulverization time was 4.0 hours. After pulverization, the powder was dried to obtain finely divided Ga-LLZO-S (pulverized material).

[0113] <Heat treatment process> The obtained Ga-LLZO-S was subjected to a heat treatment under the conditions of 800°C x 2 hours to obtain a composite oxide powder.

[0114] Example 4-2 (Working Example) The heat treatment was carried out under the conditions of 400° C.×2 hours, except for that, the composite oxide powder was produced in the same manner as in Example 4-1.

[0115] Example 4-3 (Comparative example) The pulverized material was not subjected to heat treatment, but otherwise the same procedure as in Example 4-1 was followed to produce a composite oxide powder.

[0116] Example 4-4 (Comparative Example) The calcined product was not crushed or heat-treated. Otherwise, a composite oxide powder was prepared in the same manner as in Example 4-1.

[0117] (2) Evaluation For Examples 4-1 to 4-4, the various characteristics were evaluated in the same manner as for Examples 2-1 to 2-3.

[0118] (3) Evaluation results X-ray diffraction patterns for Examples 4-1 to 4-4 are shown in FIG. 10. As shown in FIG. 10, all samples showed diffraction patterns of a cubic garnet crystal structure. Diffraction lines (▼ in the figure) derived from the pyrochlore phase (La2Zr2O7) were only slightly observed in the 800°C heat-treated sample (Example 4-1). In the crushed sample (Example 4-3), the diffraction lines were shifted to the lower angle side. This indicates lattice expansion. In addition, the width of the diffraction lines was broad in the crushed sample (Example 4-3) and the 400°C heat-treated sample (Example 4-2). This indicates that the crystal grains were refined. On the other hand, in the 800°C heat-treated sample (Example 4-1), the width of the diffraction lines was somewhat narrower due to the growth of crystallites.

[0119] SEM photographs of the fired product (Example 4-4) and the product heat-treated at 400°C (Example 4-2) are shown in Figures 11(a) and (b), respectively. Here, Figure 11(a) shows an SEM photograph at a magnification of 1000 times, and Figure 11(b) shows an SEM photograph at a magnification of 10,000 times. In the fired product (Example 4-4), the particle diameter is about 10 μm, whereas in the sample (Example 4-2) in which the fired product was treated in a bead mill and then heat-treated at 400°C, the particles were pulverized to 1 μm or less.

[0120] The particle size distribution measurement results for the 400°C heat treated material (Example 4-2) are shown in Figure 12. The average particle size D50 was 0.56 μm (560 nm). The particle size distribution showed two peaks near 0.3 μm and 2 μm. Since no single particles larger than 1 μm were observed in the SEM photograph, it is believed that the peak near 2 μm was due to aggregation of fine particles.

[0121] [Experimental Example 5] In Experimental Example 5, a sintered body (solid electrolyte body) was produced by molding and sintering a sintered or heat-treated Ga-doped LLZO (composite oxide powder) in the Ga-doped LLZO. The sinterability and ionic conductivity were then evaluated.

[0122] (1) Preparation of sintered body Example 5-1 (Working Example) A sintered body was produced using the 400°C heat-treated product (Example 4-2) produced in Experimental Example 4. The sintered body was produced as follows. First, the heat-treated product was press-molded into a disk shape with a diameter of about 20 mm and a thickness of 1.5 mm. Next, the obtained molded body was placed in an alumina crucible while embedded in the mother powder, and this was subjected to main sintering. The main sintering was performed under the conditions of 1250°C x 12 hours. As a result, a sintered body was obtained.

[0123] Example 5-2 (Comparative Example) A sintered body was produced in the same manner as in Example 5-1, except that the fired product (Example 4-4) was used instead of the product heat-treated at 400° C.

[0124] (2) Evaluation For Examples 5-1 and 5-2, the various properties were evaluated in the same manner as for Examples 3-1 to 3-4.

[0125] (3) Evaluation results The density and ionic conductivity of the sintered bodies for Examples 5-1 and 5-2 are shown in Table 2. The results of Examples 3-2 and 3-4 obtained for Al-doped LLZO are also shown in Table 2. Regardless of whether the fired product or the heat-treated product was used as the raw material, the Ga-doped LLZO (Examples 5-1 and 5-2) had higher sintered body density and ionic conductivity than the Al-doped LLZO (Examples 3-2 and 3-4).

[0126] [Table 2]

[0127] The impedance Nikeis plots for Examples 5-1 and 5-2 are shown in FIG. 13 together with the results of Examples 3-2 and 3-4. The sintered body (Example 5-2) made from the Ga-doped LLZO sintered material drew a smaller semicircle than the sintered body (Example 3-4) made from the Al-doped LLZO sintered material, and it was found to have a higher conductivity. The sintered body (Example 5-1) made from the Ga-doped heat-treated material showed an even higher conductivity than the sintered body (Example 5-2) made from the sintered material. No components thought to be grain boundary resistance were observed in the Nikeis plots for either the sintered body made from the Ga-doped heat-treated material (Example 5-1) or the sintered body made from the Al-doped heat-treated material (Example 3-2).

[0128] SEM photographs of the fracture surfaces of the sintered bodies for Examples 5-1 and 5-2 are shown in Figures 14(a) and (b). In the sintered body made from the fired product (Example 5-2), particles with a diameter of several tens of μm were densely sintered, but grain boundaries were observed between the particles and relatively large holes of about 5 to 10 μm in size were also observed (Figure 14(a)). In contrast, the sintered body made from the 400°C heat-treated product (Example 5-1) was extremely densely sintered, with the exception of closed pores of a few μm or less in size, and almost no grain boundaries were observed (Figure 14(b)).

Claims

1. A composite oxide powder comprising particles having a cubic garnet-type crystal structure, the composite oxide powder comprising lithium (Li), lanthanum (La), zirconium (Zr), and oxygen (O), The particles further comprise only gallium (Ga) as a dopant element; The composite oxide powder has a 50% diameter (D50) in its volume particle size distribution of 1000 nm or less and a pyrochlore phase content of 10 mass % or less, The particles are composite oxide powders having a basic composition represented by the formula Li 7-3x Ga x La 3 Zr 2 O 12 (where 0.1≦x≦0.3).

2. The composite oxide powder according to claim 1, having a 50% diameter (D50) of 600 nm or less.

3. The composite oxide powder according to claim 1 or 2, wherein the composite oxide powder has a half-width of a peak of a (211) diffraction line in an X-ray diffraction (XRD) profile of 0.50° or less.

4. A method for producing the composite oxide powder according to any one of claims 1 to 3, comprising the following steps: providing at least a lithium (Li) source, a lanthanum (La) source, and a zirconium (Zr) source as raw materials; blending and mixing the ingredients to form a mixture; A step of calcining the mixture to obtain a calcined product; A step of pulverizing the fired product to obtain a pulverized product; and The pulverized material is subjected to a heat treatment to obtain a heat-treated material, The method according to claim 1, wherein the calcined product is pulverized in an organic solvent using a bead mill.

5. As the lithium (Li) source, lithium carbonate (Li 2 CO 3 5. The method of claim 4, wherein

6. The method according to claim 4 or 5, wherein when the raw materials are mixed, a lithium (Li) source is mixed in an excess amount of 1 to 20 mass % with respect to the stoichiometric composition of the garnet-type crystal structure.

7. The method according to any one of claims 4 to 6, wherein, when the mixture is fired, the mixture is subjected to a first firing at a temperature of 700 to 1000 ° C., and further subjected to a second firing at a temperature of 900 to 1100 ° C.

8. The method according to any one of claims 4 to 7, wherein the organic solvent is at least one selected from the group consisting of alcohol-based solvents, ketone-based solvents, ester-based solvents, glycol ether-based solvents, hydrocarbon-based solvents, ether-based solvents, glycol-based solvents, and amine-based solvents.

9. The method of claim 8, wherein the organic solvent is isopropyl alcohol (IPA) and / or toluene.

10. A method for producing a solid electrolyte body, comprising the steps of: Providing a composite oxide powder; A step of forming the composite oxide powder into a molded body; and The molded body is sintered to obtain a sintered body, The method for preparing the composite oxide powder comprises preparing the composite oxide powder by the method according to any one of claims 4 to 9.

11. A method for producing a lithium ion secondary battery, comprising the steps of: A step of preparing at least an exterior material, a positive electrode, a negative electrode, and a solid electrolyte body; and The positive electrode and the negative electrode are disposed in the exterior material so as to face each other, and a solid electrolyte body is disposed between the positive electrode and the negative electrode, 11. The method of claim 10, wherein the solid electrolyte body is prepared by the method of claim 10.

Citation Information

Patent Citations

  • Oxide ceramic composite solid electrolyte and preparation method and application thereof

    CN109755637A

  • Multi-doping pomegranate-shaped solid electrolyte material and preparation method thereof

    CN109888374A

  • Multistage verticallyymoving observation tower

    JP1981034865A

  • All-solid lithium secondary battery, and method of manufacturing the same

    JP2010045019A

  • Material for solid electrolyte

    JP2014170734A