Metal / resin composite structure, method for manufacturing metal / resin composite structure, and engine mount member
A polyamide resin composition with talc enhances bonding strength in metal/resin composites by controlling crystallization during injection molding, addressing the weakness of conventional methods and enabling high-temperature applications.
Patent Information
- Application Number
- JP2020058514
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-27
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Conventional methods for joining resin and metal parts, such as injection bonding, do not achieve sufficient bonding strength, particularly at high temperatures, limiting their application in components like engine mount brackets.
A metal/resin composite structure is created by using a polyamide resin composition containing talc, with specific component units and ratios, applied to a metal member with a fine uneven surface, enhancing bonding strength through controlled crystallization and fluidity during injection molding.
The method results in a strong, durable composite structure with improved bonding strength, suitable for high-temperature applications like engine mount brackets, maintaining integrity under vibration and thermal stress.
Smart Images

Figure 0007587349000003 
Figure 0007587349000004 
Figure 0007587349000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal / resin composite structure, a method for manufacturing a metal / resin composite structure, and an engine mount member. [Background technology]
[0002] 2. Description of the Related Art Techniques for joining resin members and metal members are in demand in a wide range of industrial fields, such as automobiles, communication devices, home appliances, and industrial equipment.
[0003] As a technique for joining a resin member and a metal member, a so-called "injection joining method" has been proposed, in which a resin material is injected into a metal member inserted into a mold to join the resin member and the metal member.
[0004] For example, a technique has been disclosed in which a resin member such as polybutylene terephthalate resin (hereinafter referred to as "PBT") or polyphenylene sulfide resin (hereinafter referred to as "PPS") is injection bonded to a surface-roughened metal member (see, for example, Patent Document 1). In addition, a method has been disclosed in which polyamide resin such as PA6 or PA66 is injection molded onto a surface-roughened metal member by further developing the metal surface roughening treatment technique (Patent Documents 2 to 4). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-216425 A [Patent Document 2] JP 2006-315398 A [Patent Document 3] JP 2007-182071 A [Patent Document 4] International Publication No. 2008 / 081933 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the bonding strength of the composite structures of a resin member and a metal member obtained by the methods shown in Patent Documents 2 to 4 was still not at a sufficient level.
[0007] For example, when conventional composite structures are applied to powertrain parts that require high rigidity at high temperatures, such as an engine mount bracket, which is a part inside an automobile engine room and is one of the parts that supports the engine, the bonding strength at high temperatures may not yet be at a sufficient level, leaving room for improvement.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a metal / resin composite structure in which a resin member made of a polyamide resin composition is firmly joined and fixed to a metal member, a manufacturing method thereof, and an engine mount member. [Means for solving the problem]
[0009] The present invention relates to the following metal / resin composite structure, a method for manufacturing a metal / resin composite structure, and an engine mount member.
[0010] The metal / resin composite structure of the present invention is a metal / resin composite structure having a metal member having a concave-convex structure on a surface thereof and a resin member bonded to the surface of the metal member having the concave-convex structure, the resin member being made of a polyamide resin composition containing a polyamide resin (A) and a talc (B), the polyamide resin (A) containing a component unit (a1) derived from a dicarboxylic acid and a component unit (a2) derived from a diamine, the component unit (a1) derived from a dicarboxylic acid containing a component unit derived from terephthalic acid, the component unit (a2) derived from a diamine containing a component unit derived from a linear aliphatic diamine having 4 to 15 carbon atoms and a component unit derived from a branched aliphatic diamine having 4 to 18 carbon atoms, and the content of the talc (B) is 0.1 to 5 mass % relative to the polyamide resin composition.
[0011] The engine mount member of the present invention includes the metal / resin composite structure of the present invention.
[0012] The method for producing a metal / resin composite structure of the present invention includes the steps of 1) placing a metal member having a concave-convex structure on its surface in an injection molding die, and 2) injecting the molten polyamide resin composition onto the surface of the metal member having the concave-convex structure, solidifying it, and joining a resin member. Effect of the Invention
[0013] According to the present invention, it is possible to provide a metal / resin composite structure in which a resin member made of a polyamide resin composition is firmly joined and fixed to a metal member, a method for producing the same, and an engine mount member. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is an external view showing a schematic example of the structure of the metal / resin composite structure of the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a method for measuring ten-point roughness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventors have found that a polyamide resin (A) containing a component unit derived from a branched aliphatic diamine has good fluidity during molding. On the other hand, a resin composition containing such a polyamide resin does not have sufficient bonding strength with a metal member having a concave-convex structure.
[0016] In response to this, the present inventors have discovered that by combining talc (B) with a polyamide resin (A) containing a component unit derived from a branched aliphatic diamine, it is possible to significantly increase the bonding strength between a metal member and a resin member while maintaining fluidity during molding.
[0017] The reason for this is not clear, but is presumed to be as follows. That is, since the polyamide resin (A) contains a component unit derived from a branched aliphatic diamine, it exhibits good fluidity during molding, but the crystallization rate is slow. Therefore, it hardly crystallizes during injection molding, but is likely to crystallize after injection molding. As a result, the amount of cure shrinkage on the metal member after injection molding is large, and gaps are likely to occur at the interface between the metal member and the resin member, which tends to reduce the bonding strength. In response to this, by blending a specified amount of talc (B) with polyamide resin (A), crystallization can be moderately advanced even during injection molding. This reduces the amount of cure shrinkage (on the metal member) after injection molding is completed, making it difficult for gaps to form at the interface between the metal member and the resin member, and increasing the bonding strength.
[0018] Furthermore, by further adding a polyamide resin (C) having a lower heat of fusion (ΔH) (crystallinity) than the polyamide resin (A), the fluidity and crystallization rate of the resin composition during injection molding can be well balanced, making it even more difficult for gaps to form at the interface between the metal member and the resin member, and further increasing the bonding strength.
[0019] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0020] 1.Metal / resin composite structure FIG. 1 is an external view showing a schematic example of the structure of a metal / resin composite structure 100 according to the present embodiment.
[0021] As shown in FIG. 1, a metal / resin composite structure 100 according to this embodiment has a metal member 110 having an uneven structure on its surface, and a resin member 120 joined to the metal member 110.
[0022] 1-1. Metallic parts 110 The metal member 110 has a fine uneven structure on at least a part of the surface to be bonded to the resin member 120 .
[0023] (material) The metal material constituting the metal member 110 is not particularly limited, and may be, for example, iron, high-tensile steel, stainless steel, aluminum, aluminum alloy, magnesium, magnesium alloy, copper, copper alloy, titanium, titanium alloy, etc. These may be used alone or in combination of two or more. Among them, from the viewpoint of light weight and high strength, aluminum (simple aluminum) and aluminum alloy are preferred, and aluminum alloy is more preferred. Also, from the viewpoint of high strength, iron and high-tensile steel are preferred. As the aluminum alloy, alloy numbers 1050, 1100, 2014, 2024, 3003, 5052, 6061, 6063, and 7075 specified in JIS H4000 are preferably used.
[0024] The shape of the metal member 110 is not particularly limited as long as it can be bonded to the resin member 120, and may be, for example, a flat plate, a curved plate, a rod, a tube, a block, etc. Furthermore, the surface 111 to be bonded to the resin member 120 is not particularly limited, and may be a flat surface or a curved surface.
[0025] It is preferable that the metal member 110 is processed into a predetermined shape by plastic processing such as cutting and pressing, punching, milling, polishing, electrical discharge machining, and other processes to remove material, and then subjected to a roughening process, which will be described later. If the processed metal member 110 has an oxide film (rust) on its surface due to being left in the open air for a long period of time, it is preferable to remove the oxide film (rust) by polishing or chemical processing.
[0026] (Uneven structure) It is preferable that the metal member 110 has a fine uneven structure including a plurality of protrusions at least on the surface 111 that contacts the resin member 120. This can improve the bonding strength between the metal member 110 and the resin member 120.
[0027] The center-to-center distance (pitch) of the plurality of convex portions constituting the fine uneven structure is not particularly limited as long as it is sufficient to bond the metal member 110 and the resin member 120 well, but is preferably 5 nm to 500 μm. When the center-to-center distance of the plurality of convex portions is 5 nm or more, the concave portions between the convex portions are appropriately large, so that the polyamide resin composition can easily penetrate into the concave portions during bonding, and the bonding strength between the metal member 110 and the resin member 120 can be further improved. In addition, when the center-to-center distance of the plurality of convex portions is 500 μm or less, the concave portions do not become too large, so that the occurrence of gaps at the metal-resin interface of the metal / resin composite structure 100 can be further suppressed. As a result, the intrusion of moisture and the like through the gaps at the interface between the metal and the resin can be further suppressed, so that the decrease in bonding strength can be further suppressed when the metal / resin composite structure is used under high temperature and high humidity. From the same viewpoint, the center-to-center distance of the plurality of convex portions is more preferably 5 μm to 250 μm. The center-to-center distance of a plurality of protrusions is the average value of the distances between the center of one protrusion and the center of an adjacent protrusion.
[0028] The center-to-center distance of the multiple protrusions can be measured by removing the resin member from the metal / resin composite structure by mechanical peeling, solvent cleaning, or the like, and observing the surface of the exposed metal member 110 using an electron microscope or laser microscope, or a surface roughness measuring device.
[0029] Specifically, a concave-convex structure in which the center-to-center distance of multiple protrusions is less than 0.5 μm can be observed by an electron microscope, and a concave-convex structure in which the center-to-center distance of multiple protrusions is 0.5 μm or more can be observed by a laser microscope or a surface roughness measuring device. For example, in a photograph of the surface of the metal member 110 taken by an electron microscope or a laser microscope, 50 convex portions are arbitrarily selected, and the center-to-center distance of each of these convex portions is measured. Then, all the measured values of the center-to-center distance of the convex portions are added up, and the sum is divided by 50 (average) to determine the "center-to-center distance of multiple convex portions."
[0030] The average value of the ten-point average roughness (Rz) over an evaluation length of 4 mm of the surface 111 of the metal member 110 having a fine uneven structure is not particularly limited, but is preferably greater than 2 μm, more preferably greater than 2 μm and not greater than 50 μm, and even more preferably greater than 2.5 μm and not greater than 45 μm.
[0031] The average value of the ten-point mean roughness (Rz) can be measured in accordance with JIS B0601 (ISO 4287). Specifically, as described below, the ten-point mean roughness (Rz) on a total of six straight line sections, consisting of three arbitrary straight line sections parallel to each other and three arbitrary straight line sections perpendicular to the above, is measured, and the average of these is taken as the average value of Rz (see Figure 2 described below).
[0032] The average length of the roughness curve element (RSm) of the surface 111 having a fine uneven structure of the metal member 110 is preferably 0.5 to 500 μm. In particular, from the viewpoint of bonding strength, it is preferable that the center-to-center distance of a plurality of convex portions is less than 0.5 μm and the average length of the roughness curve element (RSm) is 0.5 to 500 μm. The average length of the roughness curve element can be measured according to JIS B0601 (ISO 4287) as described above.
[0033] 1-2. Resin member 120 The resin member 120 is a molded product of a polyamide resin composition.
[0034] The polyamide resin composition contains a polyamide resin (A) and talc (B).
[0035] 1-2-1. Polyamide resin (A) The polyamide resin (A) contains a component unit (a1) derived from a dicarboxylic acid and a component unit (a2) derived from a diamine.
[0036] [Component unit (a1) derived from dicarboxylic acid] The component unit (a1) derived from a dicarboxylic acid is not particularly limited, but from the viewpoint of facilitating enhancement of crystallinity, it is preferable for the component unit (a1) to contain a component unit derived from terephthalic acid.
[0037] The content of the component unit derived from terephthalic acid is not particularly limited, but is preferably 20 to 100 mol% based on the total number of moles of the component unit (a1) derived from dicarboxylic acid. If the content of the component unit is 20 mol% or more, the crystallinity and mechanical strength of the polyamide resin (A) are easily improved. From the same viewpoint, the content of the component unit is more preferably 50 to 100 mol%.
[0038] The component unit (a1) derived from a dicarboxylic acid may further contain a component unit derived from a dicarboxylic acid other than the above, within a range that does not impair the effects of the present invention. Examples of the other dicarboxylic acid include aromatic dicarboxylic acids other than terephthalic acid (e.g., naphthalenedicarboxylic acid, isophthalic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid), and aliphatic dicarboxylic acids having 4 to 20 carbon atoms.
[0039] The total content of component units derived from other dicarboxylic acids (the total content of component units derived from aromatic dicarboxylic acids other than terephthalic acid, component units derived from alicyclic dicarboxylic acids, and component units derived from aliphatic dicarboxylic acids having 4 to 20 carbon atoms) is preferably 0 to 80 mol%, more preferably 0 to 50 mol%.
[0040] [Diamine-derived component unit (a2)] The diamine-derived component unit (a2) is not particularly limited, but from the viewpoint of increasing the fluidity during injection molding (to an extent that does not impair the mechanical strength of the resulting molded article), it is preferable for the diamine-derived component unit (a2) to contain a linear aliphatic diamine-derived component unit and a branched aliphatic diamine-derived component unit.
[0041] The linear aliphatic diamine is preferably a linear aliphatic diamine having 4 to 15 carbon atoms. Examples of linear aliphatic diamines having 4 to 15 carbon atoms include 1,4-butanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine. Among them, 1,6-hexanediamine, 1,9-nonanediamine, and 1,10-decanediamine are preferred, and 1,6-hexanediamine is more preferred. These aliphatic diamines may be used alone or in combination of two or more.
[0042] The content of the component unit derived from a linear aliphatic diamine is preferably 20 to 80 mol% based on the total content of the component unit derived from a linear aliphatic diamine and the component unit derived from a branched aliphatic diamine. When the content of the component unit is 20 mol% or more, the crystallization rate is not too slow, so that the crystallinity and mechanical strength of the polyamide resin (A) are easily increased appropriately. When the content of the component unit is 80 mol% or less, the crystallization rate of the polyamide resin (A) is not too high, so that the fluidity during molding is not easily impaired. From the same viewpoint, the content of the component unit derived from a linear aliphatic diamine is more preferably 30 to 60 mol% based on the total content.
[0043] The branched aliphatic diamine is preferably a branched aliphatic diamine having 4 to 18 carbon atoms. Examples of branched aliphatic diamines having 4 to 18 carbon atoms include 2-methyl-1,5-pentanediamine, 2-methyl-1,8-octanediamine, 2-methyl-1,6-hexanediamine, 2-methyl-1,7-heptanediamine, 2-methyl-1,9-nonanediamine, and 2-methyl-1,10-decanediamine. Among them, 2-methyl-1,8-octanediamine and 2-methyl-1,5-pentanediamine are preferred, and 2-methyl-1,5-pentanediamine is more preferred. These aliphatic diamines may be one type or two or more types. For example, the diamine-derived component unit (a2) preferably contains at least one of a component unit derived from 2-methyl-1,8-octanediamine and a component unit derived from 2-methyl-1,5-pentanediamine.
[0044] The content of the component units derived from the branched aliphatic diamine is preferably 20 to 80 mol% based on the total content of the component units derived from the linear aliphatic diamine and the component units derived from the branched aliphatic diamine. When the content of the component units is 20 mol% or more, the crystallization rate of the polyamide resin (A) tends to be appropriately slowed, and the flowability during molding tends to be improved. When the content of the component units is 80 mol% or less, the crystallinity and mechanical strength of the polyamide resin (A) are unlikely to be impaired. From the same viewpoint, the content of the component units derived from the branched aliphatic diamine is more preferably 40 to 70 mol% based on the total.
[0045] The total of the component units derived from a linear aliphatic diamine and the component units derived from a branched aliphatic diamine is preferably 60 to 100 mol %, more preferably 70 to 100 mol %, and even more preferably 100 mol %, based on the total number of moles of the component units (a2) derived from diamine.
[0046] The diamine-derived component unit (a2) may further contain other diamine-derived component units within the range not impairing the effects of the present invention. Examples of other diamines include aromatic diamines and alicyclic diamines. The total content of the other diamine-derived component units may be 5 mol% or less based on the total number of moles of the diamine-derived component units (b).
[0047] Examples of such polyamide resin (A) include polyamide resins containing, as the component units (a1) derived from a dicarboxylic acid, component units derived from terephthalic acid; and, as the component units (a2) derived from a diamine, component units derived from 1,6-hexanediamine and component units derived from 2-methyl-1,5-pentanediamine or 2-methyl-1,8-octanediamine.
[0048] [Physical Properties] The heat of fusion (ΔH) of the polyamide resin (A) measured by a differential scanning calorimeter (DSC) is preferably higher than that of the polyamide resin (C) described below. Specifically, the heat of fusion (ΔH) of the polyamide resin (A) is preferably higher than 20 J / g. When the heat of fusion (ΔH) of the polyamide resin (A) is higher than 20 J / g, the crystallinity is not too low, so that the heat resistance is easily increased. From the same viewpoint, the heat of fusion (ΔH) of the polyamide resin (A) is more preferably 30 to 130 J / g.
[0049] The melting point (Tm) of the polyamide resin (A) measured by a differential scanning calorimeter (DSC) is preferably 280 to 340° C. When the melting point (Tm) of the polyamide resin (A) is 280° C. or higher, the mold releasability, mechanical strength, heat resistance, etc. are not easily impaired, and when it is 340° C. or lower, there is no need to make the molding temperature excessively high, so molding processability is easily obtained. The melting point (Tm) of the polyamide resin (A) is more preferably 290 to 320° C.
[0050] The glass transition temperature (Tg) of the polyamide resin (A) measured by a differential scanning calorimeter (DSC) is preferably from 70 to 170° C., and more preferably from 128 to 155° C. When the glass transition temperature (Tg) of the polyamide resin (A) is within the above range, heat resistance is less likely to be impaired.
[0051] The heat of fusion (ΔH), melting point (Tm) and glass transition temperature (Tg) of the polyamide resin (A) can be measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of polyamide resin (A) is sealed in a measuring aluminum pan and heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it is held at 350°C for 3 minutes and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 5 minutes, it is heated a second time to 360°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating is the melting point (Tm) of polyamide resin (A), and the transition point corresponding to the glass transition is the glass transition temperature (Tg). The heat of fusion (ΔH) is calculated from the area of the exothermic peak of crystallization during the first heating process in accordance with JIS K7122.
[0052] The heat of fusion (ΔH), melting point (Tm) and glass transition temperature (Tg) of the polyamide resin (A) can be adjusted by the composition of the dicarboxylic acid and diamine.
[0053] The polyamide resin (A) preferably has an intrinsic viscosity [η] of 0.5 to 2.0 dl / g, as measured in 96.5% sulfuric acid at 25°C. When the polyamide resin (A) has an intrinsic viscosity [η] of 0.5 dl / g or more, the mechanical strength (toughness, etc.) of the resulting resin member (molded product) is easily increased sufficiently, and when the intrinsic viscosity [η] is 2.0 dl / g or less, the fluidity during molding is not easily impaired. From the same viewpoint, the polyamide resin more preferably has an intrinsic viscosity [η] of 0.80 to 1.15 dl / g. The intrinsic viscosity [η] can be adjusted by the amount of terminal blocking of the polyamide resin (A), etc.
[0054] The intrinsic viscosity of the polyamide resin (A) can be measured in accordance with JIS K6810-1977. Specifically, 0.5 g of polyamide resin (A) is dissolved in 50 ml of 96.5% sulfuric acid solution to prepare a sample solution. The number of seconds it takes for this sample solution to flow down is measured using an Ubbelohde viscometer under conditions of 25±0.05° C., and the obtained value can be applied to the following formula to calculate the viscosity. [η]=ηSP / [C(1+0.205ηSP)]
[0055] In the above formula, each algebra or variable represents the following: [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl)
[0056] ηSP is calculated by the following formula: ηSP=(t-t0) / t0 t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds)
[0057] From the viewpoint of thermal stability during compounding or molding, the polyamide resin (A) may have at least a part of the molecular terminal groups capped with a terminal capping agent. When the molecular terminal is a carboxyl group, the terminal capping agent is preferably a monoamine, and when the molecular terminal is an amino group, the terminal capping agent is preferably a monocarboxylic acid.
[0058] Examples of monoamines include aliphatic monoamines such as methylamine, ethylamine, propylamine, and butylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; Examples of monocarboxylic acids include aliphatic monocarboxylic acids having 2 to 30 carbon atoms, such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, oleic acid, and linoleic acid; aromatic monocarboxylic acids, such as benzoic acid, toluic acid, naphthalene carboxylic acid, methylnaphthalene carboxylic acid, and phenyl acetic acid; and alicyclic monocarboxylic acids, such as cyclohexane carboxylic acid. The aromatic monocarboxylic acid and the alicyclic monocarboxylic acid may have a substituent at the cyclic structure portion.
[0059] The content of polyamide resin (A) is preferably 20 to 99% by mass based on the polyamide resin composition. When the content of polyamide resin (A) is 20% by mass or more, the properties of polyamide resin (A) are easily obtained. From the same viewpoint, the content of polyamide resin (A) is more preferably 35 to 80% by mass based on the polyamide resin composition.
[0060] 1-2-2. Talc (B) Talc (B) can appropriately increase the crystallization speed of the polyamide resin (A), thereby increasing the bonding strength between the metal member 110 and the resin member 120.
[0061] Talc (B) generally contains hydrous magnesium silicate (SiO2: 58-64%, MgO: 28-32%, Al2O3: 0.5-5%, Fe2O3: 0.3-5%) as its main component.
[0062] The average particle size of the talc (B) is not particularly limited, but is preferably 1 to 15 μm. When the average particle size of the talc is within the above range, the talc is easily dispersed in the polyamide resin (A) without impairing the fluidity of the polyamide resin composition. From the same viewpoint, the average particle size of the talc is more preferably 1 to 7.5 μm.
[0063] The average particle size of the talc (B) can be measured by a laser diffraction method, for example, a laser diffraction method using a Shimadzu particle size distribution analyzer SALD-2000A manufactured by Shimadzu Corporation.
[0064] The content of talc (B) is preferably 0.1 to 5% by mass relative to the polyamide resin composition. When the content of talc is 0.1% by mass or more, the polyamide resin (A) can be appropriately crystallized during injection molding, so that the amount of curing shrinkage due to crystallization of the polyamide resin (A) after the end of injection molding can be reduced. As a result, gaps are less likely to occur between the surface 111 of the metal member 110 (specifically, between the multiple convex portions constituting the uneven structure) and the resin member 120, and the bonding strength can be further increased. When the content of talc (B) is 5% by mass or less, the polyamide resin (A) is not excessively crystallized during injection molding, so that the fluidity is less likely to be impaired, and poor conformity of the polyamide resin composition to the fine uneven structure of the surface 111 of the metal member 110 (poor filling between the multiple convex portions constituting the fine uneven structure) can be further suppressed. From the same viewpoint, the content of talc (B) is preferably 0.1 to 3.5% by mass relative to the polyamide resin composition.
[0065] The content of the talc (B) is preferably 0.02 to 11 parts by mass, and more preferably 0.1 to 7 parts by mass, per 100 parts by mass of the total of the polyamide resin (A) and the talc (B).
[0066] 1-2-3.Other ingredients The polyamide resin composition may further contain other components other than those described above, within the scope of not impairing the effects of the present invention. Examples of other components include polyamide resins (C) other than the polyamide resin (A), fibrous inorganic fillers (D), lubricants (E), and other additives (e.g., colorants, antioxidants, heavy metal deactivators (chelating agents), flame retardant assistants, ultraviolet absorbers, heat stabilizers, antistatic agents, antibacterial agents, antifogging agents, antiblocking agents, nucleating agents, dispersants, thickeners, foaming agents, pigments, dyes, organic fillers, etc.). Among these, polyamide resins (C) other than the polyamide resin (A), fibrous inorganic fillers (D), and lubricants (E) are preferred.
[0067] (Polyamide resin (C)) The heat of fusion (ΔH) of the polyamide resin (C) is preferably lower than the heat of fusion (ΔH) of the polyamide resin (A). Specifically, the heat of fusion (ΔH) of the polyamide resin (C) measured by a differential scanning calorimeter (DSC) is preferably 0 to 5 J / g. When the heat of fusion (ΔH) of the polyamide resin (C) is 5 J / g or less, the crystallinity of the resin composition can be reduced, so that the amount of curing shrinkage on the metal member 110 can be further reduced, and the bonding strength with the metal member 110 can be further increased. From the same viewpoint, the heat of fusion (ΔH) of the polyamide resin (C) is more preferably 0 J / g. In addition, the polyamide resin (C) is preferably an amorphous resin.
[0068] The difference in heat of fusion (ΔH) between the polyamide resin (C) and the polyamide resin (A) is not particularly limited, but is preferably 20 J / g or more. When the difference in heat of fusion (ΔH) is 20 J / g or more, it is easy to adjust the crystallization rate of the polyamide resin composition during injection molding. From the same viewpoint, the difference in heat of fusion (ΔH) between the polyamide resin (C) and the polyamide resin (A) may be more preferably 30 to 130 J / g, and further preferably 30 to 60 J / g. The heat of fusion (ΔH) of the polyamide resin (C) can be measured by the same method as described above.
[0069] The polyamide resin (C) is not particularly limited as long as the heat of fusion (ΔH) satisfies the above range, but contains component units (c1) derived from a dicarboxylic acid and component units (c2) derived from a diamine.
[0070] [Component unit (c1) derived from dicarboxylic acid] The component unit (c1) derived from a dicarboxylic acid is not particularly limited, but from the viewpoint of adjusting the crystallinity, it is preferable that the component unit (c1) contains a component unit derived from isophthalic acid.
[0071] The content of the component unit derived from isophthalic acid is not particularly limited, but is preferably 20 to 100 mol% based on the total number of moles of the component unit (c1) derived from dicarboxylic acid. If the content of the component unit is 20 mol% or more, the crystallinity of the polyamide resin (A) is easily increased. From the same viewpoint, the content of the component unit is more preferably 50 to 100 mol%.
[0072] The component unit (c1) derived from a dicarboxylic acid may further include a component unit derived from a dicarboxylic acid other than the above. Examples of the other dicarboxylic acid include aromatic dicarboxylic acids other than isophthalic acid (such as terephthalic acid), alicyclic dicarboxylic acids (such as cyclohexanedicarboxylic acid), and aliphatic dicarboxylic acids having 4 to 20 carbon atoms. Among them, terephthalic acid is preferred from the viewpoint of good affinity with the polyamide resin (A).
[0073] The molar ratio of the component units derived from isophthalic acid to the component units derived from terephthalic acid in the component units (c) derived from dicarboxylic acid is preferably isophthalic acid-derived component units / terephthalic acid-derived component units=60 / 40 to 100 / 0. By appropriately lowering the crystallization rate of the polyamide resin (C), the balance between the fluidity during molding and the crystallization rate can be adjusted when combined with the polyamide resin (A).
[0074] In addition, the content of component units derived from isophthalic acid in the component units (c1) derived from dicarboxylic acids constituting the polyamide resin (C) is preferably greater than the content of component units derived from isophthalic acid in the component units (a1) derived from dicarboxylic acids constituting the polyamide resin (A).
[0075] The total content of component units derived from other dicarboxylic acids is preferably from 0 to 80 mol %, and more preferably from 0 to 50 mol %.
[0076] [Diamine-derived component unit (c2)] The diamine-derived component unit (c2) is not particularly limited, but preferably contains an aliphatic diamine-derived component unit.
[0077] The aliphatic diamine is preferably an aliphatic diamine having 4 to 15 carbon atoms. From the viewpoint of appropriately adjusting the crystallization rate by combining with the polyamide resin (A), the aliphatic diamine having 4 to 15 carbon atoms is preferably a linear aliphatic diamine. The linear aliphatic diamine is the same as described above, and is preferably 1,6-hexanediamine. The diamine-derived component unit (c2) does not need to include a branched aliphatic diamine-derived component unit.
[0078] The content of the component units derived from linear aliphatic diamine is preferably 40 to 100 mol% based on the total number of moles of the component units (c2) derived from diamine. When the content of the component units is 40 mol% or more, the crystallization rate is easily slowed, and when it is 100 mol% or less, heat resistance is easily maintained. From the same viewpoint, the content of the component units is more preferably 60 to 100 mol% based on the total number of moles of the component units (c2) derived from diamine.
[0079] [Physical Properties] Since the polyamide resin (C) is an amorphous resin, the melting point (Tm) is not observed.
[0080] The glass transition temperature (Tg) of the polyamide resin (C) is not particularly limited, but is equal to the glass transition temperature (Tg) of the polyamide resin (A), and can be, for example, 90 to 130°C.
[0081] The intrinsic viscosity [η] of the polyamide resin (C) is not particularly limited, but is lower than the intrinsic viscosity [η] of the polyamide resin (A), and is, for example, 0.50 to 1.50 dl / g, preferably 0.50 to 0.90 dl / g.
[0082] The melting point (Tm), glass transition temperature (Tg), and intrinsic viscosity [η] can be measured by the same methods as described above.
[0083] The content of polyamide resin (C) is not particularly limited, but may be 0 to 30% by mass relative to the polyamide resin composition. If the content of polyamide resin (C) is a certain amount or more, the crystallization rate is likely to be delayed, and if it is 30% by mass or less, the heat resistance is unlikely to be impaired. From the same viewpoint, the content of polyamide resin (C) may be 0 to 20% by mass relative to the polyamide resin composition.
[0084] The content of polyamide resin (C) may be 0 to 60% by mass based on the total of polyamide resin (C) and polyamide resin (A). When the content of polyamide resin (C) is a certain amount or more, the crystallinity of the resin composition can be lowered, and the amount of cure shrinkage on the metal member 110 during injection molding can be further reduced. When the content of polyamide resin (C) is 60% by mass or less, the crystallinity of the resulting resin composition is unlikely to be impaired, and the mechanical strength and heat resistance of the molded product are unlikely to be impaired. From the same viewpoint, the content of polyamide resin (C) may be more preferably 1 to 40% by mass, and further preferably 5 to 40% by mass based on the total of polyamide resin (C) and polyamide resin (A).
[0085] (Fiber-like inorganic filler (D)) The fibrous inorganic filler (D) can impart high mechanical strength to the resin member 120 which is a molded product of the polyamide resin composition.
[0086] Examples of the fibrous inorganic filler (D) include glass fiber, carbon fiber, wollastonite, potassium titanate whiskers, calcium carbonate whiskers, aluminum borate whiskers, magnesium sulfate whiskers, zinc oxide whiskers, milled fiber, and cut fiber. Of these, one type may be used alone, or two or more types may be used in combination. Among these, glass fiber and wollastonite are preferred, and glass fiber is more preferred, because they are easy to increase the mechanical strength of the resin member 120.
[0087] The average fiber length of the fibrous inorganic filler (D) may be, for example, 1 μm to 20 mm, preferably 5 μm to 10 mm, from the viewpoints of moldability of the resin composition and mechanical strength and heat resistance of the resulting molded product. The aspect ratio of the fibrous inorganic filler (D) may be, for example, 5 to 2000, preferably 30 to 600.
[0088] The average fiber length and average fiber diameter of the fibrous inorganic filler (D) can be measured by the following method. 1) The resin composition is dissolved in a hexafluoroisopropanol / chloroform solution (0.1 / 0.9% by volume), and then filtered to obtain a filtrate. 2) The filtrate obtained in 1) is dispersed in water, and the fiber length (Li) and fiber diameter (di) of each of 300 randomly selected fibers are measured using an optical microscope (magnification: 50x). The number of fibers with fiber length Li is designated as qi, and the weight average length (Lw) is calculated based on the following formula, which is the average fiber length of the fibrous filler. Weight average length (Lw) = (Σqi × Li 2 ) / (Σqi×Li) Similarly, the number of fibers having a fiber diameter Di is taken as ri, and the weight average diameter (Dw) is calculated based on the following formula, and this is taken as the average fiber diameter of the fibrous filler. Weight average diameter (Dw)=(Σri×Di 2 ) / (Σri×Di)
[0089] The content of the fibrous inorganic filler (D) is not particularly limited, but is preferably 0 to 75 mass % relative to the polyamide resin composition, more preferably more than 0 mass % and not more than 75 mass %, and even more preferably 15 to 60 mass %.
[0090] (Lubricant (E)) The lubricant (E) can improve the flowability and kneading processability during molding of the polyamide resin composition, and the releasability from a mold.
[0091] The lubricant (E) is not particularly limited, but is a metal salt of a medium-chain fatty acid having 8 to 10 carbon atoms or a long-chain fatty acid having 12 or more carbon atoms.
[0092] Examples of fatty acids include octylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, behenic acid, montanic acid, sebacic acid, and ricinoleic acid, with montanic acid, 12-hydroxystearic acid, and behenic acid being preferred.
[0093] Examples of metal salts include lithium, sodium, potassium, magnesium, calcium, barium, zinc and aluminum salts, preferably calcium, magnesium, zinc, aluminum and lithium salts.
[0094] Examples of such metal salts of fatty acids include calcium 12-hydroxystearate, zinc 12-hydroxystearate, magnesium 12-hydroxystearate, aluminum 12-hydroxystearate, lithium 12-hydroxystearate, calcium behenate, zinc behenate, magnesium behenate, lithium behenate, calcium montanate, zinc montanate, magnesium montanate, aluminum montanate, and lithium montanate. These may be used alone or in combination of two or more.
[0095] The content of the lubricant (E) is, for example, 0 to 10% by mass, preferably 0.1 to 8% by mass, based on the polyamide resin composition. When the content of the lubricant (E) is a certain amount or more, the flowability is improved, and the kneading and moldability are likely to be improved, while when the content is a certain amount or less, the kneading processability of the resin composition is unlikely to be impaired.
[0096] When two or more lubricants (E) are contained, the content of the metal salt of montanic acid in the entire lubricant (E) is 20 to 100 mass%, preferably 30 to 100 mass%, more preferably 50 to 100 mass%, thereby increasing the bonding strength of the metal / resin composite structure.
[0097] (Physical Properties of Polyamide Resin Composition) The injection flow length (L / t) of the polyamide resin composition varies depending on the composition, but is preferably, for example, 18 mm or more, and more preferably 20 to 30 mm. When the flow length (L / t) is at least a certain level, the composition has excellent flowability, and therefore, when joined to the metal member 110, the polyamide resin composition is easily filled without gaps between the convex portions of the uneven structure on the surface 111 of the metal member 100. The flow length can be measured by injection molding using a bar flow mold.
[0098] The flow length of the polyamide resin composition can be adjusted by the composition of polyamide resins (A) and (C) and their content ratio, the content of talc (B) and fibrous inorganic filler (D), etc. In order to increase the flow length, it is preferable to increase the content of branched aliphatic diamine in polyamide resin (A) or add polyamide resin (C), for example.
[0099] (Method of producing polyamide resin composition) The polyamide resin composition can be produced by a known resin kneading method, for example, a method of mixing the above-mentioned components using a Henschel mixer, a V blender, a ribbon blender, or a tumbler blender, or a method of mixing and then melt-kneading the components using a single-screw extruder, a multi-screw extruder, a kneader, or a Banbury mixer, and then granulating or pulverizing the components.
[0100] 1-3.Physical properties The metal / resin composite structure 100 of this embodiment has a metal member 110 having a fine uneven structure on its surface, and a resin member 120 made of a polyamide resin composition firmly bonded to the surface having the fine uneven structure.
[0101] Specifically, the tensile shear strength of the joint surface between the metal member 110 and the resin member 120 is preferably 40 MPa or more, more preferably 45 MPa or more, and even more preferably 47 to 70 MPa.
[0102] Furthermore, the fracture surface after the measurement of the tensile shear strength is preferably in the form of fracture of the base material. Base material fracture is defined as a fracture form in which residual resin is observed over 80% by area or more of the interface of the metal / resin joint.
[0103] The bond strength can be measured by a tensile test under the conditions of 23°C, 60mm distance between chucks, and 10mm / min tensile speed. Specifically, a special jig is attached to a tensile tester, and the breaking load (N) of the metal / resin composite structure is measured under the above conditions. The breaking load (N) is then divided by the area of the metal / resin bonded portion to calculate the bond strength (tensile shear strength) (MPa).
[0104] The bonding strength can be adjusted by the composition of the polyamide resin composition, particularly the type and content of polyamide resin (A), talc (B), and polyamide resin (C). In order to increase the bonding strength, it is preferable to adjust the composition so that the flowability during injection molding is increased and the composition is appropriately crystallized during injection molding. From the viewpoint of appropriate crystallization during injection molding, it is preferable to appropriately increase the content of talc (B), and from the viewpoint of increasing the flowability, it is preferable to increase the content of branched aliphatic diamine in polyamide resin (A) or add polyamide resin (C).
[0105] 2. Manufacturing method of metal / resin composite structure The manufacturing method of the metal / resin composite structure 100 of this embodiment is not particularly limited, but may include, for example, 1) a step of placing a metal member 110 having a concave-convex structure on its surface in an injection molding die, and 2) a step of injecting a molten polyamide resin composition onto the surface of the metal member 110 having the concave-convex structure, solidifying it, and joining the resin member 120.
[0106] Regarding step 1) First, a metal member 110 having an uneven structure on at least a portion of its surface is prepared.
[0107] The method for obtaining the metal member 110 having a fine uneven structure is not particularly limited, and may be, for example, a method using laser processing as disclosed in Japanese Patent No. 4020957; a method of immersing a metal member in an aqueous solution of an inorganic base such as NaOH and / or an aqueous solution of an inorganic acid such as HCl or HNO3; a method of treating a metal member by an anodization method as disclosed in Japanese Patent No. 4541153; a displacement crystallization method in which etching is performed with an acid-based etching agent, preferably an acid-based etching agent aqueous solution containing an inorganic acid, ferric ions, cupric ions, and if necessary, manganese ions, aluminum chloride hexahydrate, sodium chloride, etc., as disclosed in International Publication No. 2015-8847; a method of immersing a metal member in an aqueous solution of one or more selected from hydrazine hydrate, ammonia, and a water-soluble amine compound as disclosed in International Publication No. 2009 / 31632 (hereinafter, sometimes referred to as the NMT method), and a hot water treatment method as disclosed in Japanese Patent Publication No. 2008-162115.
[0108] Among these methods, the etching method can be arbitrarily selected depending on the type of metal used in the metal material and the distance between the centers of the multiple convex portions. From the viewpoint of the bonding strength between the metal member 110 and the resin member 120, however, in this embodiment, the substitution crystallization method and the NMT method are preferred.
[0109] Then, the mold is opened, and the prepared metal member 110 having a concave-convex structure is placed in the cavity portion (space portion) within the mold.
[0110] Regarding step 2) Then, the polyamide resin composition is injected into the cavity of the mold so that at least a portion of the polyamide resin composition is in contact with the surface having the fine uneven structure of the metal member 110. Thereafter, the polyamide resin composition is cooled and solidified, and the metal member 110 and the resin member 120 are joined together.
[0111] The temperature of the injection molding die is not particularly limited as long as it is a temperature at which the polyamide resin composition can be melted to a state suitable for injection molding, and may be, for example, 100 to 250°C.
[0112] After injection and pressure holding, the mold is cooled, then opened, and ejected using an ejector pin if necessary, to obtain the metal / resin composite structure 100.
[0113] As the mold, a known injection molding mold, for example, a mold for high speed heat cycle molding (RHCM, heat & cool molding) or a core-back mold for foam molding can be used.
[0114] 3. Applications of metal / resin composite structures The metal / resin composite structure 100 according to the present embodiment has high productivity and a high degree of freedom in shape control, and therefore can be applied to a variety of applications.
[0115] Furthermore, the metal / resin composite structure 100 according to this embodiment has high heat resistance, mechanical properties, friction resistance, sliding properties, airtightness, and watertightness, and is therefore suitable for use in applications that correspond to these properties.
[0116] Examples of such applications include vehicle structural parts, vehicle mounted items, housings for electronic devices, housings for home appliances, structural parts, machine parts, various automotive parts, parts for electronic devices, household applications such as furniture and kitchenware, medical equipment, building material parts, and other structural and exterior parts.
[0117] Specifically, the following parts are designed to support parts where resin alone does not have enough strength. In the case of vehicles, examples include instrument panels, console boxes, doorknobs, door trim, shift levers, pedals, glove boxes, bumpers, bonnets, fenders, trunks, doors, roofs, pillars, seats, steering wheels, ECU boxes, electrical components, engine peripheral parts, drive and gear peripheral parts, intake and exhaust system parts, and cooling system parts. In addition, examples of building materials and furniture include glass window frames, handrails, curtain rails, chests of drawers, closets, bookshelves, desks, and chairs. In addition, examples of precision electronic parts include connectors, relays, and gears. In addition, examples of transport containers include transport containers, suitcases, and trunks.
[0118] In addition, by combining the high thermal conductivity of the metal member 110 with the insulating properties of the resin member 120, the material can be used in components for devices that require optimal heat management design, such as various home appliances. Specific examples of such applications include home appliances such as refrigerators, washing machines, vacuum cleaners, microwave ovens, air conditioners, lighting equipment, electric water heaters, televisions, clocks, ventilating fans, projectors, and speakers, as well as electronic information devices such as personal computers, mobile phones, smartphones, digital cameras, tablet PCs, portable music players, portable game consoles, chargers, and batteries.
[0119] Other uses include toys, sports equipment, shoes, sandals, bags, tableware such as forks, knives, spoons, and plates, stationery such as ballpoint pens, mechanical pencils, files, and binders, cooking utensils such as frying pans, pots, kettles, spatulas, ladles, slotted ladles, whisks, and tongs, parts for lithium-ion secondary batteries, and robots.
[0120] In addition, the metal / resin composite structure 100 according to the present embodiment has excellent mechanical properties and abrasion resistance because the resin member 120 contains polyamide, and is therefore very useful as a sliding part for dynamic applications such as gears, bushes, and door checker arms.
[0121] Moreover, the metal / resin composite structure 100 according to this embodiment is useful as a bracket constituting an engine mount member that supports an engine (vibrating member) on a supporting member in a vibration-proof manner. An engine mount member in which a polyamide resin composition is integrally molded on an insert fastening metal fitting formed on a bracket for fixing to a vibrating member and / or a supporting member, or a metal reinforcing rib embedded in the bracket body for strength improvement, is obtained by forming a fine uneven surface on the surface of the fastening metal fitting or the metal reinforcing rib, and then insert molding the polyamide resin composition. The engine mount member according to this embodiment has a bracket that exhibits high bonding strength and heat resistance, and has high vibration characteristics, so that it can effectively withstand vibrations of an engine, etc. EXAMPLES
[0122] The present invention will now be described with reference to examples, which should not be construed as limiting the scope of the present invention.
[0123] 1. Metallic parts <Preparation of surface-treated metal member (M-1)> An aluminum plate (thickness: 2.0 mm) of alloy number 6063 specified in JIS H4000 was cut into a length of 45 mm and a width of 18 mm. The aluminum plate was immersed in an alkaline etching agent (sodium hydroxide: 15 mass%, zinc oxide: 3 mass%) at 30°C for 3 minutes (hereinafter sometimes abbreviated as "alkaline etching agent treatment"), and then immersed in nitric acid; 30 mass% at 30°C for 1 minute, and the alkaline etching agent treatment was repeated once more. Next, the obtained aluminum alloy plate was immersed in an acid etching agent (sulfuric acid: 4.1 mass%, ferric chloride: 3.9 mass%, cupric chloride: 0.2 mass%) at 30°C for 5 minutes and etched by shaking. Next, ultrasonic cleaning was performed with running water (in water, 1 minute) and dried to obtain a surface-treated metal member (M-1).
[0124] The surface properties of the obtained surface-treated metal member (M-1) were as follows: Center distance between multiple protrusions: 95μm Average element length Rsm: 104μm Rz of six straight sections: 19.2μm, 20.8μm, 18.5μm, 18.2μm, 18.4μm, 19.6μm Average Rz value: 19μm Etching rate: 2.9% by mass
[0125] <Preparation of surface-treated metal member (M-2)> The aluminum plate with alloy number A6063 changed to alloy number A5052 was etched in an acid-based etching solution (sulfuric acid: 8.2 mass%, ferric chloride: 7.8 mass% (Fe 3+ : 2.7% by mass, Cupric chloride: 0.4% by mass (Cu 2+ The metal member was immersed in a solution of 0.2% by mass of copper foil and the balance of ion-exchanged water for 80 seconds and etched by shaking. The metal member was then ultrasonically cleaned in running water (in water for 1 minute) and dried to obtain a surface-treated metal member (M-2).
[0126] The surface properties of the obtained surface-treated metal member (M-2) were as follows: Center distance between multiple protrusions: 92μm Element average length Rsm: 96.8μm Rz of six straight sections: 17.8μm, 18.1μm, 19.6μm, 17.8μm, 17.2μm, 18.0μm Average Rz value: 18.1μm Etching rate: 2.6% by mass
[0127] The surface properties (center-to-center distance between a plurality of protrusions and surface roughness) of the surface-treated metal member were measured by the following method.
[0128] (Center distance between multiple protrusions) The interval period of the surface-treated metal member was measured with a laser microscope (Keyence VK-X100). Specifically, 50 convex portions were arbitrarily selected from a photograph obtained by photographing the surface of the metal member, and the center-to-center distance between adjacent convex portions was measured. All the measured center-to-center distances were added up and divided by 50 to obtain the "center-to-center distance between multiple convex portions."
[0129] (Surface roughness) The surface roughness of the surface-treated metal parts was measured using a surface roughness measuring device "Surfcom 1400D (Tokyo Seimitsu Co., Ltd.)," and the etching rate was calculated from the ten-point average roughness (Rz) on the six straight lines shown in Figure 2, the average element length (Rsm), and the mass ratio of the metal parts before and after the etching treatment. The measurement conditions were as follows. ·Stylus tip radius: 5μm Reference length: 0.8 mm Evaluation length: 4mm ·Measurement speed: 0.06mm / sec The measurements were taken along three randomly selected parallel lines on the surface of the metal part, plus three randomly selected perpendicular lines to the first three lines, for a total of six lines, and the average value was calculated (see Figure 2).
[0130] 2. Constituents of polyamide resin composition (1) Polyamide resin <Polyamide resin (PA-1)> 1,6-hexanediamine 1312g (11.3 mol), 2-methyl-1,5-pentanediamine 1312g (11.3 mol), terephthalic acid 3655g (22.0 mol), sodium hypophosphite 5.5g (5.2×10- 2 mol) and 640 ml of ion-exchanged water were charged into a 1-liter reactor, and after replacing with nitrogen, the mixture was heated at 250°C and 35 kg / cm 2 The reaction was carried out for 1 hour under the above conditions. The molar ratio of 1,6-hexanediamine to 2-methyl-1,5-pentanediamine was 50:50. After 1 hour had elapsed, the reaction product produced in the reactor was transferred to a pressurized water supply system connected to the reactor and maintained at a pressure of about 10 kg / cm. 2 The mixture was extracted into a receiver set at a low temperature to obtain a polyamide precursor having an intrinsic viscosity [η] of 0.15 dl / g. The polyamide precursor was then dried and melt-polymerized at a cylinder temperature of 330°C using a twin-screw extruder to obtain a polyamide resin (PA-1).
[0131] The composition of the obtained polyamide resin (PA-1) is as follows: the content of the component units derived from terephthalic acid in the component units derived from dicarboxylic acid was 100 mol%, the content of the component units derived from 1,6-hexanediamine in the component units derived from diamine was 50 mol%, and the content of the component units derived from 2-methyl-1,5-pentanediamine was 50 mol%. The intrinsic viscosity [η] of the polyamide resin (PA-1) was 0.9 dl / g, the melting point Tm was 300°C, the glass transition temperature was 140°C, and the heat of fusion (ΔH) was 45 J / g.
[0132] <Polyamide resin (PA-2)> 2800g (24.1 mol) of 1,6-hexanediamine, 1390g (8.4 mol) of terephthalic acid, 2581g (15.5 mol) of isophthalic acid, 109.5g (0.9 mol) of benzoic acid, 5.7g of sodium hypophosphite monohydrate and 545g of distilled water were placed in an autoclave with a capacity of 13.6L and substituted with nitrogen. Stirring was started at 190°C, and the internal temperature was raised to 250°C over 3 hours. At this time, the internal pressure of the autoclave was raised to 3.02MPa. After the reaction was continued for 1 hour, the mixture was released into the air from a spray nozzle installed at the bottom of the autoclave and the low-order condensation product was extracted. After that, the low-order condensation product was cooled to room temperature, pulverized to a particle size of 1.5mm or less with a pulverizer, and dried at 110°C for 24 hours. The water content of the obtained low-order condensate was 3000 ppm, and the intrinsic viscosity [η] was 0.14 dl / g. Next, this low-order condensate was melt-polymerized in a twin-screw extruder with a screw diameter of 30 mm and L / D=36 at a barrel setting temperature of 330°C, a screw rotation speed of 200 rpm, and a resin supply rate of 6 kg / h to obtain a polyamide resin (PA-2).
[0133] The composition of the obtained polyamide resin (PA-2) is as follows: the content of the component units derived from terephthalic acid in the component units derived from dicarboxylic acid was 70 mol%, the content of the component units derived from isophthalic acid was 30 mol%, and the content of the component units derived from 1,6-hexanediamine in the component units derived from diamine was 100 mol%. The intrinsic viscosity [η] of the polyamide resin (PA-2) was 0.9 dl / g, the melting point (Tm) was 330°C, the glass transition temperature (Tg) was 125°C, and the heat of fusion (ΔH) was 50 J / g.
[0134] <Polyamide resin (PA-3)> 2800g (24.1 mol) of 1,6-hexanediamine, 2581g (15.5 mol) of terephthalic acid, 1390g (8.4 mol) of isophthalic acid, 109.5g (0.9 mol) of benzoic acid, 5.7g of sodium hypophosphite monohydrate and 545g of distilled water were placed in an autoclave with a capacity of 13.6L and substituted with nitrogen. Stirring was started at 190°C, and the internal temperature was raised to 250°C over 3 hours. At this time, the internal pressure of the autoclave was raised to 3.02MPa. After the reaction was continued for 1 hour, the mixture was released into the air from a spray nozzle installed at the bottom of the autoclave and the low-order condensation product was extracted. After that, the low-order condensation product was cooled to room temperature, pulverized to a particle size of 1.5mm or less with a pulverizer, and dried at 110°C for 24 hours. The water content of the obtained low order condensate was 3000 ppm, and the intrinsic viscosity [η] was 0.14 dl / g. Next, this low-order condensate was melt-polymerized in a twin-screw extruder with a screw diameter of 30 mm and L / D=36 at a barrel setting temperature of 330°C, a screw rotation speed of 200 rpm, and a resin supply rate of 6 kg / h to obtain a polyamide resin (PA-3).
[0135] The composition of the obtained polyamide resin (PA-3) is as follows: the content of the component units derived from terephthalic acid in the component units derived from dicarboxylic acid was 30 mol%, the content of the component units derived from isophthalic acid was 70 mol%, and the content of the component units derived from 1,6-hexanediamine in the component units derived from diamine was 100 mol%. The intrinsic viscosity [η] of the polyamide resin (PA-3) was 0.65 dl / g, no melting point (Tm) was observed, the glass transition temperature (Tg) was 125°C, and the heat of fusion (ΔH) was 0 J / g.
[0136] The compositions and physical properties of the polyamide resins (PA-1) to (PA-3) are shown in Table 1.
[0137] [Table 1]
[0138] The intrinsic viscosity [η], melting point (Tm), glass transition temperature (Tg) and heat of fusion (ΔH) of the polyamide resin were measured by the following methods.
[0139] [Intrinsic viscosity [η]] According to JIS K6810-1977, 0.5 g of polyamide resin was dissolved in 50 ml of 96.5% sulfuric acid solution to prepare a sample solution. The flow time of the obtained sample solution was measured using an Ubbelohde viscometer under the condition of 25±0.05°C. The measurement results were applied to the following formula to calculate the intrinsic viscosity [η] of the polyamide resin. [η]=ηSP / [C(1+0.205ηSP)] ηSP=(t-t0) / t0 [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl) t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds)
[0140] [Melting point (Tm), glass transition temperature (Tg), heat of fusion (ΔH)] The melting point (Tm), glass transition temperature (Tg) and heat of fusion (ΔH) of the polyamide resin were measured using a differential scanning calorimeter (DSC220C type, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of polyamide resin was sealed in an aluminum pan for measurement and set in the differential scanning calorimeter. Then, it was heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it was held at 360°C for 3 minutes and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 5 minutes, it was heated a second time to 360°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating was taken as the melting point (Tm) of the polyamide resin, and the transition point corresponding to the glass transition was taken as the glass transition temperature (Tg). The heat of fusion ΔH was calculated from the area of the exothermic peak of crystallization in the first heating process in accordance with JIS K7122.
[0141] (2) Talc Talc: average particle size 6μm
[0142] (3) Fibrous inorganic filler Glass fiber: Nippon Electric Glass Co., Ltd. ECS03T-251H (glass fiber with an average fiber diameter of 10.5 μm)
[0143] (4) Lubricants Calcium Montanate
[0144] 3. Fabrication and evaluation of metal / resin composite structures [Examples 1 to 5 and Comparative Examples 1 to 7] (Preparation of Pellets of Polyamide Resin Composition) The polyamide resin, talc (B), glass fiber (D) and lubricant (E) shown in Table 2 were mixed in the ratios shown in Table 2 in a 30 mmφ vented twin-screw extruder with a barrel temperature set at 335°C, and pelletized in a pelletizer to obtain pellets of the composition.
[0145] (injection molding) Next, the small dumbbell metal insert mold was attached to an injection molding machine J55AD manufactured by Japan Steel Works, Ltd. Next, the mold was heated to 160°C, and then the surface-treated metal member shown in Table 2 was placed in the mold.
[0146] The pellets of the polyamide resin composition prepared above were dried for 24 hours under conditions of 110°C and 10 Torr (1330 Pa), and then placed in a hopper of the injection unit of the injection molding machine. Then, injection molding was carried out under conditions of a cylinder temperature of 335°C, a mold temperature of 150°C, an injection speed of 40 mm / sec, a holding pressure of 90 MPa, and an injection holding pressure time of 8 seconds, to obtain a metal / resin composite structure.
[0147] The bonding strength and fluidity of the obtained metal / resin bonded bodies were evaluated by the following methods.
[0148] (Joining strength) Using a tensile testing machine Model 1323 (manufactured by Aiko Engineering Co., Ltd.), a dedicated jig was attached to the tensile testing machine, and the breaking load (N) of the metal / resin composite structure was measured at room temperature (23°C) under the conditions of a chuck distance of 60 mm and a tensile speed of 10 mm / min. The breaking load (N) was then divided by the area of the metal / resin bonded portion to calculate the bond strength (tensile shear strength) (MPa).
[0149] (Flow length test (injection flowability)) A bar flow mold with a width of 10 mm and a thickness of 0.5 mm was used, and injection was performed under the following conditions, and the flow length (mm) of the resin within the mold was measured. Injection molding machine: Sodick Plastech Co., Ltd., Tupearl TR40S3A Injection pressure setting: 2000kg / cm 2 Cylinder temperature setting: 335℃ Mold temperature: 150℃
[0150] The evaluation results of Examples 1 to 5 and Comparative Examples 1 to 7 are shown in Table 2.
[0151] [Table 2]
[0152] As shown in Table 2, the metal / resin composite structures of Examples 1 to 5, which contain polyamide resin (A) and a predetermined amount of talc (B), have high bonding strength. In addition, the polyamide resin compositions of Examples 1 to 5 have good flowability during injection molding.
[0153] In particular, it is clear that the bonding strength of the metal / resin composite structure is further increased by further including the polyamide resin (C) (comparison between Examples 1 and 3).
[0154] In contrast, the metal / resin composite structures of Comparative Examples 1, 2 and 6 not containing the polyamide resin (A) and the metal / resin composite structures of Comparative Examples 3 and 4 not containing talc all have low bonding strength. [Industrial Applicability]
[0155] According to the present invention, it is possible to provide a metal / resin composite structure in which a resin member made of a polyamide resin composition is firmly joined and fixed to a metal member, a method for producing the same, and an engine mount member. [Explanation of symbols]
[0156] 100 Metal / resin composite structure 110 Metallic parts 111 Surface (joint surface) 120 Resin parts
Claims
1. A metal / resin composite structure having a metal member having a concave-convex structure on a surface thereof and a resin member joined to the concave-convex structure-having surface of the metal member, The resin member is made of a polyamide resin composition containing a polyamide resin (A), a talc (B), and a polyamide resin (C), The polyamide resin (A) contains a component unit (a1) derived from a dicarboxylic acid and a component unit (a2) derived from a diamine, The component unit (a1) derived from a dicarboxylic acid includes a component unit derived from terephthalic acid, The diamine-derived component unit (a2) is a component unit derived from a linear aliphatic diamine having 4 to 15 carbon atoms and a component unit derived from a branched aliphatic diamine having 4 to 18 carbon atoms. Including, The average particle size of the talc (B) is 6 to 15 μm, and The content of the talc (B) is 0.1 to 0.35% by mass relative to the polyamide resin composition, The polyamide resin (C) has a lower heat of fusion (ΔH) as measured by a differential scanning calorimeter than the polyamide resin (A), The uneven structure has a plurality of protrusions, The center-to-center distance of the plurality of protrusions is 5 nm to 500 μm. Metal / resin composite structure.
2. The component units derived from the branched aliphatic diamine include at least one of a component unit derived from 2-methyl-1,8-octanediamine and a component unit derived from 2-methyl-1,5-pentanediamine. The metal / resin composite structure according to claim 1 .
3. The component units derived from the linear aliphatic diamine include component units derived from 1,6-hexanediamine, The component units derived from the branched aliphatic diamine include component units derived from 2-methyl-1,5-pentanediamine. The metal / resin composite structure according to claim 1 or 2.
4. The heat of fusion (ΔH) of the polyamide resin (C) is 0 to 5 J / g. The metal / resin composite structure according to any one of claims 1 to 3.
5. The polyamide resin (C) contains a component unit (c1) derived from a dicarboxylic acid and a component unit (c2) derived from a diamine, The dicarboxylic acid-derived component unit (c1) includes an isophthalic acid-derived component unit, The diamine-derived component unit (c2) includes a carbon atom-derived aliphatic diamine-derived component unit. The metal / resin composite structure according to any one of claims 1 to 4.
6. The dicarboxylic acid-derived component unit (c1) may further include a terephthalic acid-derived component unit, the molar ratio of the component units derived from isophthalic acid to the component units derived from terephthalic acid is such that the component units derived from isophthalic acid / the component units derived from terephthalic acid is 60 / 40 to 100 / 0; The metal / resin composite structure according to claim 5 .
7. The content of the polyamide resin (C) is 1 to 40 mass% based on the total content of the polyamide resin (C) and the polyamide resin (A). The metal / resin composite structure according to any one of claims 1 to 6.
8. The polyamide resin composition further contains a fibrous inorganic filler. The metal / resin composite structure according to any one of claims 1 to 7.
9. The content of the fibrous inorganic filler is more than 0% by mass and 75% by mass or less with respect to the polyamide resin composition. The metal / resin composite structure according to claim 8.
10. The metal member includes one or more selected from iron, high-tensile steel, stainless steel, aluminum, aluminum alloy, magnesium, magnesium alloy, copper, copper alloy, titanium, and titanium alloy; The metal / resin composite structure according to any one of claims 1 to 9.
11. The metal / resin composite structure according to any one of claims 1 to 10, Engine mounting parts.
12. A method for producing a metal / resin composite structure according to any one of claims 1 to 10, comprising: 1) placing a metal member having a textured structure on a surface thereof in an injection molding die; 2) injecting the molten polyamide resin composition onto the surface of the metal member having the uneven structure and solidifying the composition to bond the resin member; Including, The uneven structure has a plurality of protrusions, The center-to-center distance of the plurality of protrusions is 5 nm to 500 μm. A method for manufacturing a metal / resin composite structure.
Citation Information
Patent Citations
Polyamide composition
JP2000212436A
Connecting joint for aluminum alloy pipe and its manufacturing method
JP2004216425A
Composite of aluminum alloy and resin, and its manufacturing method
JP2006315398A
Composite of aluminum alloy and resin and production method thereof
JP2007182071A
Metal / resin composite structure and method for producing metal / resin composite structure