Ceramic Electronic Components

The ceramic electronic component addresses the bonding challenge of low ionization tendency conductors by using oxide interface protrusions with a constricted and wide configuration to enhance bonding reliability between the element body and external electrode.

JP7587445B2Active Publication Date: 2024-11-20TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021036609
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-08
Publication Date
2024-11-20
Estimated Expiration
2041-03-08

AI Technical Summary

Technical Problem

Conventional ceramic electronic components face challenges in bonding external electrodes containing low ionization tendency conductors, such as copper, to the element body or glass frit, which are oxides, resulting in low bonding reliability.

Method used

The ceramic electronic component features an interface protrusion on the external electrode side, made of oxide, with a constricted and wide portion configuration, enhancing the anchoring effect and facilitating strong bonding with the element body.

Benefits of technology

This configuration improves the bonding reliability between the element body and external electrode, even with conductors like copper, by increasing the anchoring effect and ensuring firm bonding through oxide interface protrusions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587445000007
    Figure 0007587445000007
  • Figure 0007587445000008
    Figure 0007587445000008
  • Figure 0007587445000009
    Figure 0007587445000009
Patent Text Reader

Abstract

To provide a ceramic electronic component in which an element body and an external electrode join with each other strongly.SOLUTION: The ceramic electronic component includes: an element body in which a ceramic layer and an internal electrode layer are laminated; and an external electrode electrically connected to at least an end of the internal electrode layer. At least a part of the joint interface of the external electrode and the ceramic layer has an interface protruding part on the external electrode side, and the interface protruding part is formed of an oxide.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic electronic component having external electrodes. [Background technology]

[0002] As shown in Patent Document 1, there is known a ceramic electronic component that includes an element body containing a ceramic component and an external electrode formed on the outer surface of the element body. Fired electrodes are widely used as the external electrodes of ceramic electronic components, and can be formed by applying a conductive paste containing a conductor powder and a glass frit to the surface of the element body and firing it.

[0003] However, in the conventional technology disclosed in Patent Document 1, it is difficult to bond external electrodes that contain an element with low ionization tendency, such as copper, as a conductor to the element body or glass frit, which is an oxide. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 4-171912 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above circumstances, and has an object to provide a ceramic electronic component having high bonding reliability between the element body and external electrodes. [Means for solving the problem]

[0006] In order to achieve the above object, a ceramic electronic component according to the present invention comprises: an element body in which ceramic layers and internal electrode layers are laminated; an external electrode electrically connected to at least one end of the internal electrode layer, At least a part of a joint boundary between the external electrode and the ceramic layer has an interface protrusion on the external electrode side, The interfacial protrusion is a ceramic electronic component made of an oxide.

[0007] The ceramic electronic component according to the present invention has high bonding reliability between the element body and the external electrodes. The reasons for this are believed to be as follows.

[0008] In the present invention, at least a portion of the bonding boundary between the external electrode and the ceramic layer has an interface protrusion on the external electrode side. The interface protrusion is also made of an oxide. Therefore, the interface protrusion included in the external electrode is easily bonded to the element body including the dielectric layer which is an oxide, and as a result, the element body and the external electrode can be firmly bonded to each other, thereby improving the bonding reliability.

[0009] The bonding reliability can be determined, for example, by the rate of change in capacitance due to an air-tank thermal shock test. α After the test, the capacitance C β The rate of change (C β / C α ) is higher, the joint reliability is higher. Also, the higher the joint strength, the higher the joint reliability.

[0010] The external electrodes may contain at least one selected from the group consisting of Cu, a Cu alloy, Ag, and an Ag alloy as a main component.

[0011] Copper and other metals used as conductors for the external electrodes have a low ionization tendency and are therefore relatively resistant to oxidation. In other words, copper is a metal that does not easily bind with oxygen. In contrast, the ceramic components contained in the element body are oxides. The glass frit contained in the external electrodes is also an oxide. For this reason, in conventional technology, it is difficult to join an external electrode that contains an element with a low ionization tendency, such as copper, as a conductor to the element body or glass frit, which are oxides.

[0012] In contrast, according to the present invention, even if the conductor of the external electrode contains an element that is difficult to oxidize, such as copper, the interface protrusions can firmly join the element body and the external electrode.

[0013] The interface protrusion portion is A narrow section and It is preferable that the external electrode has a wide portion adjacent to the narrow portion and wider than the narrow portion, the wide portion being located on the inner side of the external electrode relative to the narrow portion.

[0014] As a result, the interface protrusion exerts an anchor effect on the external electrode due to the constricted portion formed by the narrow portion and the wide portion, thereby improving the reliability of the bond between the element body and the external electrode.

[0015] Preferably, within a length of 100 μm of the junction boundary between the element body and the external electrode, there are two or more interface protrusions, each having a constriction formed by the narrow portion and the wide portion.

[0016] This allows the element body and the external electrodes to be bonded more firmly.

[0017] Of the interface protrusions, the angle θ of the constricted portion, which is the smallest angle, preferably satisfies 20°≦θ≦140°.

[0018] When the angle θ is within the above range, the external electrode is more easily inserted into the narrowed portion of the interface protrusion than when the angle θ is below the above range, and the anchor effect is enhanced. Also, when the angle θ is within the above range, the external electrode is more easily sandwiched between the narrow and wide portions of the interface protrusion than when the angle θ is above the above range, and the anchor effect is enhanced. Therefore, by having the angle θ fall within the above range, the anchor effect of the interface protrusion is enhanced, and the bond between the element body and the external electrode is stronger.

[0019] The width of the narrow portion is Tn, When the width of the wide portion is Tw, The Tw / Tn at the interface protrusion is preferably 2 or more.

[0020] When Tw / Tn satisfies the above range, the external electrode easily fits into the narrowed portion of the interface protrusion, and the external electrode is easily sandwiched between the narrow and wide portions of the interface protrusion, resulting in a stronger anchor effect. Therefore, when Tw / Tn satisfies the above range, the anchor effect of the interface protrusion is enhanced, and the bond between the element body and the external electrode is stronger.

[0021] Preferably, at least a portion of said oxide is a glass.

[0022] At least a part of the oxide constituting the interface protrusion is glass, which increases the fluidity of the interface protrusion. This makes it easier for the interface protrusion to wet the conductor of the external electrode and the surface of the element body facing the external electrode. In addition, since the glass contained in the interface protrusion is an oxide, it is easy to bond with the element body including the dielectric layer, which is also an oxide. This makes it possible to bond the element body and the external electrode more firmly.

[0023] The interface protrusion contains at least two types selected from B, Si and Zn as main components.

[0024] This makes it easier for the interface protrusions to be vitrified, and for the reasons described above, the element body and the external electrodes can be bonded more firmly.

[0025] The ceramic layer may contain a perovskite type compound represented by ABO3 as a main component.

[0026] The perovskite compound represented by ABO3 is (Ba 1-a-b Sr a Ca b ) m (Ti 1-c-d Zr c Hf d)It is a perovskite-type compound represented by O3, and may satisfy the formula of 0.94 < m < 1.1, 0 ≦ a ≦ 1, 0 ≦ b ≦ 1, 0 ≦ c ≦ 1, and 0 ≦ d ≦ 1.

[0027] Let the linear expansion coefficient of the ceramic layer be α, Let the linear expansion coefficient of the external electrode be β, When the linear expansion coefficient of the interface protrusion is δ, The magnitude relationship of α, β, and δ preferably satisfies β > α > δ.

[0028] The interface protrusion has a low linear expansion coefficient. By providing such an interface protrusion on the surface of the external electrode on the ceramic layer side, the components constituting the external electrode tighten the interface protrusion with thermal stress during cooling at the time of baking. As a result, the element body and the external electrode can be joined more firmly.

Brief Description of the Drawings

[0029] [Figure 1] FIG. 1 is a schematic cross-sectional view of a multilayer ceramic capacitor according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of part II of FIG. 1. [Diagram 3] FIG. 3 is an enlarged view of part III of FIG. 2. [Figure 4] FIG. 4 is an enlarged view of part III of FIG. 2. [Diagram 5] FIG. 5 is an enlarged view of part III of FIG. 2. [Figure 6] FIG. 6 is an enlarged view of part III of FIG. 2. [Figure 7] FIG. 7 is an enlarged view of part VII of FIG. 2. [Figure 8] FIG. 8 is an enlarged view of a main part of a schematic cross-sectional view of a multilayer ceramic capacitor according to another embodiment of the present invention.

Modes for Carrying Out the Invention

[0030] First embodiment ​​The overall configuration of a multilayer ceramic capacitor will be described as an embodiment of a ceramic electronic component according to the present invention. Fig. 1 shows a cross-sectional view of a typical multilayer ceramic capacitor 2.

[0031] The multilayer ceramic capacitor 2 has dielectric layers (ceramic layers) 10 and internal electrode layers 12 that are substantially parallel to a plane including the X-axis and Y-axis, and has an element body 4 in which the dielectric layers 10 and the internal electrode layers 12 are alternately stacked along the Z-axis direction (stacking direction).

[0032] Here, "substantially parallel" means that most of the portions are parallel, but there may be some portions that are not parallel, and the dielectric layers 10 and the internal electrode layers 12 may be slightly uneven or inclined.

[0033] 1, the end face in the X-axis direction of the element body 4 is flat, in other words, the dielectric layer 10 and the internal electrode layer 12 are laminated so as to be flush with each other. However, the end face in the X-axis direction of the element body 4 may have a non-flat portion. Also, the dielectric layer 10 and the internal electrode layer 12 may not be flush with each other, and may be laminated in a state in which, for example, part of the dielectric layer 10 is scraped off or part of the internal electrode layer 12 protrudes.

[0034] In this embodiment, the X-axis, Y-axis, and Z-axis are perpendicular to each other.

[0035] In this embodiment, the term “inner side” refers to the side closer to the center of the multilayer ceramic capacitor 2 , and the term “outer side” refers to the side away from the center of the multilayer ceramic capacitor 2 .

[0036] In this embodiment, one of the alternately stacked internal electrode layers 12 is electrically connected to the inside of the external electrode 6 formed on the outside of one end in the X-axis direction of the element body 4. The other of the alternately stacked internal electrode layers 12 is electrically connected to the inside of the external electrode 6 formed on the outside of the other end in the X-axis direction of the element body 4.

[0037] In this embodiment, the shape and dimensions of the element body 4 are not particularly limited. The shape may be, for example, an elliptical columnar shape, a columnar shape, or other prismatic shapes. The length L0 of the element body 4 in the X-axis direction may be, for example, 0.4 to 5.7 mm. The length W0 of the element body 4 in the Y-axis direction may be, for example, 0.2 to 5.0 mm. The length T0 of the element body 4 in the Z-axis direction may be, for example, 0.2 to 2.0 mm.

[0038] The thickness of the dielectric layer 10 is not particularly limited. For example, the thickness Td of the dielectric layer 10 sandwiched between the internal electrode layers 12 is preferably 30 μm or less, more preferably 15 μm or less, and still more preferably 10 μm or less.

[0039] The number of stacked dielectric layers 10 is not particularly limited, but is preferably 20 or more, and more preferably 50 or more.

[0040] The material of the dielectric layer 10 is not particularly limited, but in this embodiment, the dielectric layer 10 mainly contains a perovskite-type compound represented by ABO3.

[0041] The main component of the dielectric layer 10 is a component contained in the dielectric layer 10 in an amount of 80% by mass or more.

[0042] The perovskite-type compound represented by ABO3 is, for example, a perovskite-type compound represented by (Ba 1-a-b Sr a Ca b ) m (Ti 1-c-d Zr c Hf d )O3, and may satisfy the formula of 0.94 < m < 1.1, 0 ≤ a ≤ 1, 0 ≤ b ≤ 1, 0 ≤ c ≤ 1, and 0 ≤ d ≤ 1.

[0043] m indicates the element ratio of the A site and the B site, for example, 0.94 < m < 1.1.

[0044] a indicates the element ratio of Sr, for example, 0 ≤ a ≤ 1, and preferably 0 ≤ a < 1.

[0045] b represents the element ratio of Ca and satisfies 0≦b≦1, and preferably satisfies 0≦b<1.

[0046] c represents the element ratio of Zr and satisfies 0≦c≦1, and preferably satisfies 0≦c<1.

[0047] d indicates the element ratio of Hf, and is 0≦d≦1, and preferably 0≦d<1.

[0048] The element ratio of oxygen (O) in the above composition formula may deviate slightly from the stoichiometric composition.

[0049] In addition to these main components, the dielectric layer 10 according to the present embodiment may contain auxiliary components such as Mn compounds, Mg compounds, Cr compounds, Ni compounds, rare earth element compounds, Si compounds, Li compounds, B compounds, V compounds, etc. The types and combinations of the auxiliary components and the amounts added are not particularly limited.

[0050] The conductive material contained in the internal electrode layer 12 is not particularly limited, but is preferably Ni, Ni-based alloy, Cu or Cu-based alloy, Ag or Ag-based alloy, Pd or Pd-based alloy, etc. In addition, Ni, Ni-based alloy, Cu or Cu-based alloy, Ag-Pd-based alloy, etc. may contain various trace components such as P at about 0.1 mass % or less. In this embodiment, the internal electrode 12 may contain Ni or Ni alloy as a main component. In addition, when Ni or Ni alloy is the main component, it may contain one or more subcomponents selected from Mn, Cu, Cr, etc.

[0051] The main component of the internal electrode layer 12 is a component contained in the internal electrode layer 12 at 90 mass % or more.

[0052] The internal electrode layer 12 may be formed using a commercially available electrode paste. The thickness of the internal electrode layer 12 may be appropriately determined depending on the application, etc. For example, the thickness Te of each internal electrode layer 12 may be set to 3.0 μm or less.

[0053] The external electrode 6 of this embodiment is formed on the element body 4 so as to be electrically connected to at least a portion of the internal electrode layer 12 .

[0054] The external electrode 6 according to this embodiment includes at least a conductor 61 .

[0055] There is no particular limitation on the components constituting the conductor 61 contained in the external electrode 6. For example, known conductive materials such as Ni, Cu, Sn, Ag, Pd, Au, or alloys of these may be used. In this embodiment, the conductor 61 may contain at least one selected from the group consisting of Cu, a Cu alloy, Ag, and an Ag alloy as a main component.

[0056] The main component of the conductor 61 is a component that is contained in the conductor 61 at 90 mass % or more other than the coating layer such as plating or conductive resin.

[0057] In addition, when the conductor 61 contains Cu, it may also contain elements such as Al, Ni, Ag, Pd, Sn, Zn, P, Fe, and Mn.

[0058] The thickness Le of the external electrode 6 is not particularly limited, but is, for example, 10 to 200 μm.

[0059] In this embodiment, the external electrode 6 may have a nonmetallic component 62 or a void (not shown). The nonmetallic component 62 may be the same component as the interface protrusion 16 described below, but may be a portion not present on at least a part of the surface on the dielectric layer 10 side. The nonmetallic component 62 may have the same composition as the interface protrusion 16, or may have a different composition. For example, the presence of glass (nonmetallic component 62) containing SiO2 or the like in a region of the external electrode 6 other than the vicinity of the interface with the dielectric layer 10 can suppress composition deviation of the interface protrusion 16.

[0060] Fig. 2 is an enlarged view of part II in Fig. 1. As shown in Fig. 2, in the multilayer ceramic capacitor according to this embodiment, at least a part of a junction boundary 46 between the external electrode 6 and the dielectric layer 10 has an irregular interface protrusion 16 on the external electrode 6 side. In other words, the interface protrusion 16 is formed by biting into the interior of the external electrode 6.

[0061] The interface protrusions 16 according to this embodiment are made of an oxide. Therefore, the interface protrusions 16 included in the external electrode 6 are easily bonded to the element body 4 including the dielectric layer 10, which is an oxide, and as a result, the element body 4 and the external electrode 6 can be firmly bonded to each other.

[0062] At least a part of the oxide constituting the interface protrusion 16 according to this embodiment is glass, which increases the fluidity of the interface protrusion 16. This makes it easier for the interface protrusion 16 to wet the conductor 61 of the external electrode 6 and the surface of the element body 4 facing the external electrode 6. In addition, since the glass contained in the interface protrusion 16 is an oxide, it is easy to bond with the element body 4 including the dielectric layer 10, which is also an oxide. This makes it possible to bond the element body 4 and the external electrode 6 more firmly.

[0063] The interface protrusions 16 contain at least two types selected from B, Si, and Zn as main components, and more preferably contain at least Si and B as main components. This makes the interface protrusions 16 more likely to vitrify, and allows the element body 4 and the external electrodes 6 to be bonded more firmly.

[0064] "The interface protrusion 16 contains at least two types selected from B, Si and Zn as main components" means that in the interface protrusion 16, when the total of elements other than oxygen is 100 molar parts, the total of at least two types selected from B, Si and Zn accounts for 90 molar parts or more.

[0065] In this embodiment, when the total amount of B, Si and Zn contained in the interface protrusion 16 is taken as 1 molar part, the interface protrusion 16 preferably contains 0.15 to 0.82 molar parts of B, and more preferably contains 0.28 to 0.70 molar parts of B.

[0066] In this embodiment, when the total amount of B, Si, and Zn contained in interface protrusion 16 is taken as 1 molar part, interface protrusion 16 preferably contains 0.07 to 0.60 molar parts of Si, and more preferably contains 0.10 to 0.35 molar parts.

[0067] In this embodiment, when the total amount of B, Si and Zn contained in interface protrusion 16 is taken as 1 molar part, interface protrusion 16 preferably contains 0.10 to 0.61 molar parts of Zn, and more preferably contains 0.15 to 0.46 molar parts.

[0068] The interface protrusion 16 may contain elements constituting the dielectric composition 10, elements constituting the internal electrode layer 12, and elements constituting the conductor 61, in addition to B, Si, and Zn.

[0069] The interface protrusions 16 in this embodiment have a shape that provides an anchor effect. The "shape that provides an anchor effect" means that the interface protrusions 16 do not spread thinly along the outer surface of the dielectric layer 10 (YZ plane), but rather spread three-dimensionally from the outer surface of the dielectric layer 10 toward the inside of the external electrode 6 (i.e., toward the outside in the X-axis direction) as shown in FIG.

[0070] The interface protrusion 16 according to this embodiment may or may not have a constricted portion 16c, but preferably has the constricted portion 16c. Here, the constricted portion 16c refers to a portion formed by a narrow portion 16a having a narrow width and a wide portion 16b which is wider than the narrow portion 16a and is provided adjacent to the narrow portion 16a on the inner side of the external electrode 6 (outside in the X-axis direction) than the narrow portion 16a.

[0071] Even if there is no constricted portion 16c like interface protrusion 160, as long as there is one or more interface protrusions 160 and these interface protrusions 160 are inclined in at least one of the Y-axis direction and the Z-axis direction, the anchor effect can be exhibited. For example, the inclination angle formed by the end face in the X-axis direction of element body 4 (YZ plane) and interface protrusion 160 is preferably 20° or more and 140° or less.

[0072] Furthermore, even if the interface protrusion 16 does not have a constricted portion 16c in the XZ cross section of FIG. 2, it may have a constricted portion 16c in the YZ cross section.

[0073] The interface protrusion 16 will be described with reference to Figures 3 to 6 which are enlarged views of part III in Figure 2. As shown in Figure 4, the interface protrusion 16 has a constricted portion 16c in the X-axis direction.

[0074] 3 and 4, the interface protrusion 16 has a narrow portion 16a that is narrow in the Z-axis direction (stacking direction), and a wide portion 16b that is wider in the Z-axis direction than the narrow portion, located outward in the X-axis direction of the interface protrusion 16 that is continuous with the narrow portion 16a. In other words, the interface protrusion 16 has the narrow portion 16a and the wide portion 16b that is provided adjacent to the narrow portion 16a on the inner side of the narrow portion 16a. The narrow portion 16a and the wide portion 16b form a constriction 16c.

[0075] The interface protrusions 16 are provided intermittently on the end surface in the X-axis direction of the element body 4 so as to ensure the connection between the conductor 61 and the internal electrode layer 12. In other words, the interface protrusions 16 are generally not provided in the portion where the end of the internal electrode layer 12 in the X-axis direction is connected to the conductor 61.

[0076] However, when observing the XZ cross section, there may be a portion near the end face in the X-axis direction of the element body 4 where the interface protrusion 16 covers the end portion in the X-axis direction of some of the internal electrode layers 12. Since each internal electrode layer 12 exists not only along the X-axis direction but also along the Y-axis direction, if there is a portion at the end portion in the Y-axis direction of each internal electrode layer 12 where the interface protrusion 16 is not provided, the internal electrode layer 12 and the conductor 61 can be electrically connected at that portion. In other words, even if the end portion of the internal electrode layer 12 is partially covered by the interface protrusion 16, the electrical connection between each internal electrode layer 12 and the conductor 61 can be ensured.

[0077] The connection interface between the external electrode 6 and the internal electrode layer 12 is indicated by a joint boundary 46 , but it does not have to be clear. For example, the end of the internal electrode layer 12 may extend into the interior of the interface protrusion 16 .

[0078] In addition, as shown in FIG. 1, when the external electrode 6 is formed across from the end face of the element body 4 in the X-axis direction to the end face of the element body 4 in the Z-axis direction, the interface protrusion 16 may be formed not only on the end face in the X-axis direction but also on the end face in the Z-axis direction.

[0079] Such a shape of the interface protrusion 16 having the constricted portion 16c can be realized, for example, by applying a paste for the narrow portion containing small grain size oxide particles (hereinafter referred to as "small oxide particles") that form the narrow portion 16a to the end face in the X-axis direction of the element body 4, and then applying and baking a paste for the wide portion containing large grain size oxide particles (hereinafter referred to as "large oxide particles") that form the wide portion 16b on top of the narrow portion paste.

[0080] Alternatively, the interface protrusions 16 can be formed by applying an interface protrusion paste containing interface protrusion particles having a desired shape to the end face in the X-axis direction of the element body 4 and baking it. "Interface protrusion particles" are particles that become the interface protrusions 16 after baking on the element body 4.

[0081] It is preferable that a predetermined number or more of the interface protrusions 16 having the constricted portions 16c are present within a predetermined length Lz in the Z-axis direction of the junction boundary 46 between the element body 4 and the external electrode 6. Specifically, in a cross section (XZ cross section) including the vicinity of the interface between the element body 4 and the external electrode 6, if the predetermined length Lz of the junction boundary 46 is 100 μm, it is preferable that two or more interface protrusions 16 having the constricted portions 16c are present, and more preferably 10 or more interface protrusions 16 having the constricted portions 16c are present. There is no particular upper limit on the number of interface protrusions 16 having the constricted portions 16c, but from the viewpoint of ensuring electrical connection between the internal electrode layer 12 and the external electrode 6, it is preferable that the number is 15 or less.

[0082] The predetermined length Lz is the distance between two points on the junction boundary 46 between the element body 4 and the external electrode 6. Therefore, when there are irregularities on the junction boundary 46 between the element body 4 and the external electrode 6, the predetermined length Lz is not the length of the irregularities, but two points on the irregularities are determined, and the distance between the two points is set as the predetermined length Lz.

[0083] It is preferable that an average of 0.5 or more interface protrusions 16 having constrictions 16c are present per dielectric layer 10, and it is more preferable that one or more interface protrusions 16 are present per dielectric layer 10.

[0084] There is no particular limitation on the method for controlling the number of interface protrusions 16 having constrictions 16c. The number of interface protrusions 16 having constrictions 16c can be controlled, for example, by changing the content of small oxide particles contained in the paste for narrow portions, large oxide particles contained in the paste for wide portions, or particles for interface protrusions contained in the paste for interface protrusions. In addition, the number of interface protrusions 16 having constrictions 16c tends to increase when the mass ratio of the content of small oxide particles to the content of large oxide particles is reduced.

[0085] As shown in FIG. 5, the angle θ of the narrow portion 16c, which is the smallest angle formed by a tangent 16aL of the narrow portion 16a and a tangent 16bL of the wide portion 16b, preferably satisfies 20°≦θ≦140°, and more preferably satisfies 20°≦θ≦120°.

[0086] When the angle θ is within the above range, the external electrode 6 (the conductor 61 and the non-metallic component 62, etc.) can easily enter the constricted portion 16c of the interface protrusion 16, and the anchor effect is enhanced, compared to when the angle θ is below the above range. When the angle θ is within the above range, the external electrode 6 can easily be sandwiched between the narrow portion 6a and the wide portion 6b of the interface protrusion 16, and the anchor effect is enhanced, compared to when the angle θ is above the above range. Therefore, when the angle θ is within the above range, the anchor effect of the interface protrusion 16 is enhanced, and the bond between the element body 4 and the external electrode 6 is stronger.

[0087] There is no particular limitation on the method for controlling the angle θ. For example, the angle θ can be controlled by changing the ratio (Dw / Dn) of the average particle size (Dw) of the large oxide particles to the average particle size (Dn) of the small oxide particles contained in the paste for the narrow width portion. If Dw / Dn is large, the angle θ tends to be small.

[0088] Alternatively, the angle θ may be controlled by using interface protrusion particles contained in the interface protrusion paste that have a constriction of a desired angle.

[0089] 6, when the width of narrow portion 16a is Tn and the width of wide portion 16b is Tw, Tw / Tn is preferably 2 or more, and more preferably 2.5 or more. There is no particular upper limit to Tw / Tn, but from the viewpoint of ensuring the strength of interface protrusion 16, Tw / Tn is preferably 4 or less.

[0090] When Tw / Tn satisfies the above range, the external electrode 6 easily fits into the constricted portion 16c of the interface protrusion 16, and the external electrode 6 is easily sandwiched between the narrow portion 16a and the wide portion 16b of the interface protrusion 16, and the anchor effect is enhanced, compared to when Tw / Tn is below the above range. Therefore, with Tw / Tn in the above range, the anchor effect of the interface protrusion 16 is enhanced, and the bond between the element body 4 and the external electrode 6 is stronger.

[0091] The method of controlling Tw / Tn is not particularly limited. For example, the ratio (Dw / Dn) of the average particle size (Dw) of large oxide particles to the average particle size (Dn) of small oxide particles contained in the paste for narrow width portion is changed. If Dw / Dn is large, Tw / Tn tends to be large.

[0092] Alternatively, Tw / Tn may be controlled by making the particles for interface protrusions contained in the paste for interface protrusions have a constriction with a desired Tw / Tn.

[0093] When the linear expansion coefficient of the dielectric layer 10 is α, the linear expansion coefficient of the external electrode 6 is β, and the linear expansion coefficient of the interface protrusion portion 16 is δ, it is preferable that the magnitude relationship between α, β, and δ is β>α>δ.

[0094] The interface protrusions 16 have a low coefficient of linear expansion. By providing such interface protrusions 16 on the surface of the external electrode 6 facing the dielectric layer 10, the components constituting the external electrode 6 tighten the interface protrusions 16 with thermal stress during cooling after baking. This allows the element body 4 and the external electrode 6 to be joined more firmly.

[0095] For example, the linear expansion coefficient α of BaTiO3, which is the main component of the dielectric layer 10, is 9.4 ppm / °C. The linear expansion coefficient β of Cu used in the external electrodes 6 is 17.5 ppm / °C. Furthermore, the linear expansion coefficient δ of the glass constituting the interface protrusion 16 is 2.8 to 9.0 ppm / °C.

[0096] The structure of the interfacial protrusion 16 can be analyzed by cross-sectional observation using a SEM (scanning electron microscope) or a STEM (scanning transmission electron microscope), etc. Specifically, when observing the cross section of the external electrode 6 using a backscattered electron image of an SEM or a HAADF image of a STEM, the conductor 61, which is often denser than the interfacial protrusion 16, the nonmetallic component 62, and the voids 63, can often be recognized as a bright contrast area, while the interfacial protrusion 16, the nonmetallic component 62, the voids 63, etc. can often be recognized as a dark contrast area.

[0097] The composition of the interface protrusion 16 can be measured by performing component analysis with an EPMA (electron probe microanalyzer) during cross-sectional observation. It is preferable to perform component analysis at least three or more locations and calculate the composition of the interface protrusion 16 from the average value of the measurement results. In this embodiment, when performing component analysis with an EPMA, an EDS (energy dispersive spectrometer) or a WDS (wavelength dispersive spectrometer) can be used as the X-ray spectrometer.

[0098] In the above, the present embodiment has been described with a focus on the shape of the interface protrusion 16, but hereinafter, the shape of the conductor 61 will be described with a focus on the shape of the conductor 61.

[0099] Fig. 7 is an enlarged view of part VII in Fig. 2. Fig. 7 shows two interface protrusions 161 and 162. As shown in Fig. 7, between adjacent interface protrusions 161 and 162, the distance between interface protrusions 161 and 162 is narrower between wide portion 161b and wide portion 162b, but the distance between interface protrusions 161 and 162 is wider between narrow portions 162a and 162b.

[0100] Thus, in the region between adjacent interface protrusions 161 and 162, an inter-narrow region 61a is likely to be formed in which the conductor 61 widens in the Z-axis direction toward the bond boundary 46, i.e., toward the inside in the X-axis direction. In such inter-narrow region 61a, the conductor 61 widens in the Z-axis direction and is sandwiched inward in the X-axis direction by the wide portions 161b and 162b, so that the bond between the element body 4 and the external electrode 6 can be strengthened and the bond reliability can be improved.

[0101] Next, an example of a method for manufacturing the multilayer ceramic capacitor 1 shown in FIG. 1 will be described.

[0102] First, a paste for dielectric layer is prepared in order to manufacture a green sheet that will constitute the dielectric layer 10 shown in FIG. 1 after firing.

[0103] The dielectric layer paste is usually composed of an organic solvent-based paste obtained by kneading a dielectric powder with an organic vehicle, or a water-based paste.

[0104] The raw materials for the dielectric powder can be appropriately selected from the composite oxides or various compounds that become oxides, such as carbonates, hydroxides, and organometallic compounds, that will form the dielectric layer 10 described above, and can be used by mixing them.

[0105] The organic vehicle is a binder dissolved in an organic solvent. The binder used in the organic vehicle is not particularly limited, and may be appropriately selected from various common binders such as acrylic, ethyl cellulose, butyral, etc.

[0106] The organic solvent used is not particularly limited, and may be appropriately selected from various organic solvents such as alcohol, methyl ethyl ketone, acetone, toluene, terpineol, and butyl carbitol depending on the method to be used, such as a sheet method or a printing method.

[0107] The dielectric layer paste may contain additives selected from various dispersants, plasticizers, dielectrics, subcomponent compounds, glass frits, and the like, as necessary.

[0108] Examples of the plasticizer include phthalates such as dioctyl phthalate and benzyl butyl phthalate, adipic acid, phosphates, and glycols.

[0109] Next, an internal electrode layer paste for forming the internal electrode layer 12 shown in FIG. 1 is prepared. The internal electrode layer paste is prepared by kneading the conductive material made of the various conductive metals or alloys described above with the organic vehicle described above. Instead of the conductive material, an oxide or an organometallic compound can also be used. The oxide and organometallic compound described above become the conductive material after firing. The internal electrode layer paste may contain ceramic powder (for example, barium titanate powder or calcium strontium zirconate powder) as a co-material, if necessary. The co-material has the effect of suppressing sintering of the conductive powder during the firing process.

[0110] Using the dielectric layer paste and internal electrode layer paste prepared above, as shown in FIG. 1, green sheets which become the dielectric layers 10 after firing and internal electrode pattern layers which become the internal electrode layers 12 after firing are alternately laminated to produce a green laminate which becomes the element body 4 after firing.

[0111] Specifically, first, a green sheet is formed on a carrier sheet (for example, a PET film) as a support by a doctor blade method, etc. After being formed on the carrier sheet, the green sheet is dried.

[0112] Next, an internal electrode pattern layer is formed on the surface of the green sheet formed above using the internal electrode layer paste, to obtain a green sheet having an internal electrode pattern layer. Then, the obtained green sheets having the internal electrode pattern layer are alternately laminated to obtain a green laminate.

[0113] The method for forming the internal electrode pattern layer is not particularly limited, but examples include a printing method, a transfer method, etc. Green sheets having internal electrode pattern layers may be laminated via an adhesive layer.

[0114] The obtained green laminate is cut to a predetermined size to form a green chip. The green chip may be solidified by solidification and drying to remove the plasticizer. The green chip after solidification and drying may be placed in a barrel container together with media and a polishing solution, and barrel polished by a horizontal centrifugal barrel machine or the like. The green chip after barrel polishing is washed with water and dried. Solidification and drying and barrel polishing are not necessarily performed.

[0115] The dried green chip is subjected to a binder removal step, a firing step, and an annealing step as required, to obtain the element body 4 shown in FIG.

[0116] The binder removal conditions are a temperature rise rate of preferably 5 to 300° C. / hour, a holding temperature of preferably 180 to 400° C., and a temperature holding time of preferably 0.5 to 24 hours. The binder removal atmosphere is air or a reducing atmosphere.

[0117] The holding temperature during firing is preferably 1200 to 1350° C., more preferably 1220 to 1300° C., and the holding time is preferably 0.5 to 8 hours, more preferably 1 to 3 hours.

[0118] The firing atmosphere is preferably a reducing atmosphere, and the atmospheric gas may be, for example, a humidified mixed gas of N2 and H2.

[0119] In addition, the oxygen partial pressure during firing may be appropriately determined depending on the type of conductive material in the internal electrode layer paste. When a base metal such as Ni or a Ni alloy is used as the conductive material, the oxygen partial pressure in the firing atmosphere is set to 10 -14 ~10 -10 It is preferable that the pressure is set to MPa.

[0120] After firing in a reducing atmosphere, it is preferable to anneal the element body 4. The annealing is a treatment for reoxidizing the dielectric layer 10, which can significantly extend the IR life (high temperature load life), thereby improving reliability.

[0121] The oxygen partial pressure in the annealing atmosphere is 10 -9 ~10 -5 It is preferable to set the oxygen partial pressure to 10 -9 By setting the pressure to be equal to or higher than MPa, the re-oxidation of the dielectric layer 10 can be carried out efficiently.

[0122] The holding temperature during annealing is preferably 950 to 1150° C. By holding the temperature at 950° C. or higher, the dielectric layer 10 can be easily oxidized sufficiently, and the IR (insulation resistance) and IR life can be easily improved.

[0123] Other annealing conditions include a temperature retention time of preferably 0 to 20 hours and a temperature drop rate of preferably 50 to 500° C. / hour. As the annealing atmospheric gas, for example, humidified N2 gas or the like is preferably used.

[0124] In the above-mentioned binder removal treatment, firing and annealing, N2 gas or mixed gas can be humidified using, for example, a wetter, etc. In this case, the water temperature is preferably about 5 to 75°C.

[0125] The debinding, firing and annealing may be carried out in succession or independently.

[0126] Next, a paste for the narrow portion containing small oxide particles and a paste for the wide portion containing large oxide particles are applied to both end faces in the X-axis direction of the element body 4, respectively, and then the paste for the narrow portion and the paste for the wide portion are dried and baked to form an interface protrusion portion 16 having a constriction portion 16c on the external electrode 6 side of the junction boundary 46.

[0127] The narrow section paste may be prepared in the same manner as the internal electrode layer paste described above, except that it contains at least the metal powder constituting the conductor 61 and the above-mentioned small oxide particles. The wide section paste may be prepared in the same manner as the internal electrode layer paste described above, except that it contains at least the metal powder constituting the conductor 61 and the above-mentioned large oxide particles.

[0128] The content of small oxide particles in the paste for the narrow portion is preferably less than the content of large oxide particles in the paste for the wide portion in terms of mass ratio. This makes it easier to form the interface protrusion 16 having the constricted portion 16c. Specifically, the content of small oxide particles in the paste for the narrow portion relative to the content of large oxide particles in the paste for the wide portion is preferably 0.5 or less in terms of mass ratio, and more preferably 0.25 to 0.4.

[0129] The composition of the small oxide particles and the composition of the large oxide particles are preferably the same as the composition of the desired interface protrusions 16 .

[0130] The average particle size Dn of the small oxide particles is preferably approximately equal to the width Tn of the narrow portion 16a, and the average particle size Dw of the large oxide particles is preferably approximately equal to the width Tw of the wide portion 16b. In other words, Dw / Dn is preferably approximately equal to the desired Tw / Tn.

[0131] There is no particular limitation on the method of applying the paste for the narrow width portion to the element body 4, and examples of the method include dipping, printing, coating, etc. After being applied, the paste for the wide width portion is dried.

[0132] Next, the paste for the wide portion is applied on top of the paste for the narrow portion in the same manner as the paste for the narrow portion, and then dried.

[0133] Next, the narrow portion paste and the wide portion paste are baked. The baking conditions for the narrow portion paste and the wide portion paste are not particularly limited, and for example, they are baked by holding at 700°C to 1000°C for 0.1 to 3 hours in a humidified N2 or dry N2 atmosphere.

[0134] Even in this case, the conductor 61 and the internal electrode layer 12 can be electrically connected. This is because the internal electrode layer 12 is made of a metal and the dielectric layer 10 is an oxide, so small oxide particles, which are oxides, are less likely to wet the internal electrode layer 12 and more likely to wet the dielectric layer 10. For this reason, the small oxide particles gather in large numbers on the dielectric layer 10. Therefore, the small oxide particles are less likely to obstruct the electrical connection between the conductor 61 and the internal electrode layer 12.

[0135] In addition, the large oxide particles are less wettable by the conductor 61, but are more wettable by the small oxide particles. Therefore, the large oxide particles tend to be present near the small oxide particles, and as a result, the large oxide particles and the small oxide particles tend to form the interface protrusions 16 having the constricted portions 16c.

[0136] By the above-mentioned baking process of the paste for the narrow portion and the paste for the wide portion, the small oxide particles contained in the paste for the narrow portion form the narrow portion 16a, and the large oxide particles contained in the paste for the wide portion form the wide portion 16b, thereby obtaining an interface protrusion portion 16 having a constricted portion 16c.

[0137] In the above, the narrow portion paste and the wide portion paste are baked at the same time, but the wide portion paste may be baked after the narrow portion paste is baked.

[0138] Next, the outer external electrode paste is applied, as necessary, to the outside of the portion where the wide section paste is baked, dried, and baked. The outer external electrode paste may be prepared in the same manner as the above-mentioned internal electrode layer paste, except that it contains at least the metal powder constituting the conductor 61. The outer external electrode paste may contain a non-metallic component 62 such as glass frit in addition to the above-mentioned metal powder.

[0139] In this embodiment, the paste for the outer external electrode may or may not be applied, but by applying the paste for the outer external electrode, the thickness of the paste for the narrow portion and the paste for the wide portion can be made thinner, and the interface protrusion portion 16 having the constricted portion 16c can be more reliably provided at the junction boundary 46 between the element body 4 and the external electrode 6.

[0140] Furthermore, if necessary, a covering layer is formed by plating or the like on the outside of the portion where the wide portion paste is baked. That is, the external electrode 6 is formed by baking the narrow portion paste and the wide portion paste, baking the outer external electrode paste, and forming a covering layer by plating or the like.

[0141] The multilayer ceramic capacitor 2 thus manufactured is mounted on a printed circuit board by soldering or the like, and is used in various electronic devices.

[0142] The multilayer ceramic capacitor 2 according to this embodiment can improve the bonding reliability between the element body 4 and the external electrode 6. The reason for this is believed to be as follows. In this embodiment, at least a portion of the bonding boundary 46 between the external electrode 6 and the dielectric layer 10 has an interface protrusion 16 on the external electrode 6 side, and the interface protrusion 16 is made of an oxide. For this reason, the interface protrusion 16 included in the external electrode 6 is easily bonded to the element body 4 including the dielectric layer 10 which is an oxide, and as a result, the element body 4 and the external electrode 6 can be firmly bonded to each other.

[0143] Furthermore, according to this embodiment, even if the conductor 61 of the external electrode 6 contains an element that is difficult to oxidize, such as Cu, the element body 4 and the external electrode 6 can be firmly joined by the interface protrusion 16 having an anchor effect.

[0144] Furthermore, the interface protrusion 16 having the constricted portion 16c exhibits an anchor effect due to the constricted portion 16c, and therefore the element body 4 and the external electrode 6 can be joined together more firmly.

[0145] Furthermore, since at least a part of the oxide constituting the interface protrusion 16 is glass, the fluidity of the interface protrusion 16 is increased. This makes it easier for the interface protrusion 16 to wet the conductor 61 of the external electrode 6 and the surface of the element body 4 facing the external electrode 6. In addition, since the glass contained in the interface protrusion 16 is an oxide, it is easy to bond with the element body 4 including the dielectric layer 10, which is also an oxide. Therefore, the element body 4 and the external electrode 6 can be bonded more firmly.

[0146] Furthermore, when the linear expansion coefficient of the dielectric layer 10 is α, the linear expansion coefficient of the external electrode 6 is β, and the linear expansion coefficient of the interface protrusion portion 16 is δ, it is preferable that the magnitude relationship between α, β, and δ is β>α>δ.

[0147] Thus, it is preferable that the interface protrusions 16 according to this embodiment have a low linear expansion coefficient. By providing such interface protrusions 16 on the surface of the external electrode 6 facing the dielectric layer 10, the components constituting the external electrode 6 tighten the interface protrusions 16 with thermal stress when cooling after baking. This allows the element body 4 and the external electrode 6 to be joined more firmly.

[0148] [ Second embodiment ] The multilayer ceramic capacitor according to this embodiment is similar to the multilayer ceramic capacitor according to the first embodiment, except for the following points.

[0149] Fig. 8 is an enlarged view of the same portion as part II in Fig. 1. As shown in Fig. 8, the element body 4 according to this embodiment may have a boundary layer 14 at the end of the dielectric layer 10 in the X-axis direction. The boundary layer 14 may be provided so as to be in contact with the internal electrode layer 12.

[0150] That is, in this embodiment, at least a part of the joint boundary 46 between the external electrode 6 and the boundary layer 14 may have the interface protrusion 16 on the external electrode 6 side.

[0151] The boundary layer 14 discontinuously covers the end face in the X-axis direction of the element body 4 so as to ensure the connection between the external electrode 6 and the internal electrode layer 12. That is, the boundary layer 14 is partially discontinued at the portion where the end of the internal electrode layer 12 in the X-axis direction is connected to the external electrode 6.

[0152] When observing the XZ cross section, there may be a portion near the end face in the X-axis direction of the element body 4 where the boundary layer 14 covers the end portion in the X-axis direction of some of the internal electrode layers 12. The internal electrode layers 12 exist not only along the X-axis direction but also along the Y-axis direction, and as long as the end portion of each internal electrode layer 12 penetrates the boundary layer 14 at least partially in the Y-axis direction and is electrically connected to the external electrode 6, the electrical connection between each internal electrode layer 12 and the external electrode 6 can be ensured even if the end portion of the internal electrode layer 12 is partially covered by the boundary layer 14.

[0153] The boundary layer 14 according to this embodiment contains A-site elements and B-site elements as main components.

[0154] "The boundary layer 14 contains A-site elements and B-site elements as main components" means that in the boundary layer 14, the total of the A-site elements and the B-site elements accounts for 90 parts by mole or more when the total of the elements other than oxygen is 100 parts by mole.

[0155] The A-site element contained in the boundary layer 14 is not particularly limited, but may be Ba. The B-site element contained in the boundary layer 14 is not particularly limited, but may be Ti.

[0156] In this embodiment, when the total of Ba and Ti contained in the boundary layer 14 is taken as 1 molar part, the boundary layer 14 preferably contains 0.27 to 0.40 molar parts of Ba. In this case, the linear expansion coefficient γ of the boundary layer 14 tends to be in the range of 13.0 ppm / °C to 14.5 ppm / °C. In this embodiment, it is more preferable that the boundary layer 14 is BaTi2O5.

[0157] When the linear expansion coefficient of the dielectric layer 10 is α and the linear expansion coefficient of the external electrode 6 is β, the magnitude relationship between α, β and γ is preferably β>γ>α.

[0158] For example, the linear expansion coefficient γ of BaTi2O5 constituting the boundary layer 14 is 13.3 ppm / °C.

[0159] Furthermore, when the linear expansion coefficient of the internal electrode layers 12 is σ, the magnitude relationship between α, β, γ and σ preferably satisfies β>γ>σ>α.

[0160] The structure of the boundary layer 14 can be analyzed by cross-sectional observation using an SEM or STEM. The composition of the boundary layer 14 can be measured by component analysis using an EPMA during cross-sectional observation. It is preferable to perform component analysis at least three or more locations and calculate the composition of the boundary layer 14 from the average value of the measurement results.

[0161] The boundary layer 14 can be formed by baking the narrow section paste and the wide section paste at high temperature, adding Ti-rich compounds such as BaTi2O5 and TiO2 to the narrow section paste and the wide section paste and baking them, or by using a boundary layer paste, and it is preferable to use a boundary layer paste. The boundary layer 14 may be formed by ceramic coating using various deposition methods without using a paste.

[0162] When a high-temperature baking process is adopted, the holding temperature is preferably 800° C. to 1000° C., and the holding time is preferably 0.1 to 3 hours. The boundary layer 14 is formed by baking the paste for narrow portions and the paste for wide portions at a higher temperature than in a normal baking process, or by baking the paste for narrow portions and the paste for wide portions for a longer period of time.

[0163] When using a boundary layer paste, the boundary layer 14 can be formed by applying and baking the boundary layer paste to the end face in the X-axis direction of the green chip before firing, or to the end face in the X-axis direction of the element body 4 after firing.

[0164] In this case, the paste for the boundary layer contains the powder for the boundary layer, a binder, and a solvent, and may further contain a dispersant, a plasticizer, etc., as necessary. The powder for the boundary layer is obtained by mixing starting materials such as BaO powder and TiO2 powder in a predetermined ratio, calcining the mixture, and pulverizing the mixture.

[0165] The boundary layer paste can be applied to the green chip or element body 4 by a dipping method, various printing methods such as screen printing, application methods using a dispenser, spraying methods using a spray, etc. The boundary layer paste is applied to at least the end face in the X-axis direction, and may also be applied to a part of the end face in the Z-axis direction. In this case, the average length Lr (average thickness) of the boundary layer 14 can be adjusted by controlling the amount of the boundary layer paste applied.

[0166] When the paste for the boundary layer is applied to the element body 4, the paste for the boundary layer is dried after application and baked at a temperature of 700°C to 1000°C for 0.1 to 3 hours to form the boundary layer 14. In this case, the baking of the paste for the boundary layer may be performed simultaneously with the baking of the paste for the narrow portion and the paste for the wide portion. The average length Lr of the boundary layer 14 is also affected by the conditions of the baking process. If the temperature during the baking process is set low or the holding time is shortened, the average length Lr tends to become smaller (the average thickness becomes thinner). In addition to the above, the average length Lr can also be affected by the thickness of the paste for the boundary layer. When the paste for the boundary layer is applied to the green chip, the paste for the boundary layer is baked when the green chip is fired.

[0167] When the boundary layer 14 is formed using a paste, it is preferable to subject the element body 4 to wet barrel polishing before applying the paste and / or after baking the paste. In the wet barrel polishing, the ceramic component (dielectric layer 10 or boundary layer 14) is selectively polished rather than the end of the internal electrode layer 12, and the end of the internal electrode layer 12 is easily exposed on the outermost surface of the end face 4a. In other words, the electrical connection of the internal electrode layer 12 to the external electrode 6 is improved by the wet barrel polishing.

[0168] In this embodiment, for example, a paste for boundary layers is applied to the fired element body 4, a paste for narrow portions is applied thereon, a paste for wide portions is applied thereon, and a paste for outer external electrodes is applied thereon, and the paste for boundary layers, paste for narrow portions, paste for wide portions, and paste for outer external electrodes are simultaneously baked. The baking temperature is not particularly limited, but is 800 to 1000°C.

[0169] Even in this case, electrical continuity can be established between the external electrode 6 and the internal electrode layer 12. This is because, after the conductive material of the internal electrode layer 12 reacts with the conductor of the external electrode 6, the glass component constituting the interface protrusion 16, the BaTi2O5 constituting the boundary layer 14, and the ABO3 constituting the dielectric layer 10 react with each other, so that oxides due to the boundary layer paste are unlikely to be formed at the end of the internal electrode layer 12 in the X-axis direction.

[0170] In this embodiment, the presence of the boundary layer 14 makes it possible to effectively prevent thermal stress from occurring at the interface between the external electrode 6 and the dielectric layer 10 due to cooling after baking, or thermal shock during manufacture or use. The reason for this is believed to be as follows.

[0171] In this embodiment, the dielectric layer 10 contains a perovskite compound represented by ABO3 as a main component, and the element body 4 has a boundary layer 14 containing an A-site element and a B-site element at a predetermined molar ratio at an end of the dielectric layer 10. For this reason, it is believed that the dielectric layer 10 and the boundary layer 14 are easily mutually diffused, and the dielectric layer 10 and the boundary layer 14 are firmly bonded to each other.

[0172] Furthermore, it is believed that the content of the B-site elements in the boundary layer 14 is greater than the content of the A-site elements, and therefore the external electrode 6 and the boundary layer 14 are firmly bonded to each other.

[0173] In this embodiment, the dielectric layer 10 and the boundary layer 14 are firmly bonded in this manner, and the external electrode 6 and the boundary layer 14 are also firmly bonded, so that the element body 4 and the external electrode 6 are firmly bonded. Note that the high bond strength can be confirmed, for example, by a tensile strength test.

[0174] Furthermore, since the conductor 61 of the baked electrode layer 6a of the external electrode 6 contains at least one selected from the group consisting of Cu, a Cu alloy, Ag, and an Ag alloy as a main component, the linear expansion coefficient γ of the boundary layer 14 is smaller than the linear expansion coefficient β of the external electrode 6 and larger than the linear expansion coefficient α of the dielectric layer 10. In this embodiment, the provision of such a boundary layer 14 can reduce thermal stress occurring at the interface between the external electrode 6 and the dielectric layer 10, and it is believed that the bonding strength between the dielectric layer 10 and the external electrode 6 can be further increased.

[0175] Furthermore, when the internal electrode layer 12 contains Ni or a Ni alloy as a main component, the relationship of the linear expansion coefficient α of the dielectric layer 10, the linear expansion coefficient γ of the boundary layer 14, and the linear expansion coefficient σ of the internal electrode layer 12 is γ>σ>α. In this embodiment, the boundary layer 14 is provided so as to contact the internal electrode layer 12. Therefore, the boundary layer 14 having a linear expansion coefficient close to the internal electrode layer 12 contacts the internal electrode layer 12, and the effect of suppressing peeling between the dielectric layer 10 and the internal electrode layer 12 near the surface of the element body 4 is enhanced.

[0176] Although an embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention.

[0177] For example, the ceramic electronic component of the present invention is not limited to a multilayer ceramic capacitor, but can be applied to other ceramic electronic components, such as any electronic component having a ceramic layer and an external electrode, including a disc capacitor, a bandpass filter, a multilayer three-terminal filter, a piezoelectric element, a PTC thermistor, an NTC thermistor, and a varistor.

[0178] For example, in the above, an interface protrusion 16 having a constricted portion was formed using a paste for a narrow portion and a paste for a wide portion, but the interface protrusion 16 may also be formed using a paste for an interface protrusion containing particles for the interface protrusion of the desired shape.

[0179] Specifically, instead of the paste for narrow portions and the paste for narrow portions, a paste for interface protrusions containing particles for interface protrusions is applied to both end faces in the X-axis direction of the element body 4 and baked to form the interface protrusions 16. This paste for interface protrusions may be prepared in the same manner as the paste for internal electrode layers described above, except that it contains at least the metal powder constituting the conductor 61 and particles for interface protrusions.

[0180] Incidentally, the "particles for interface protrusions" are particles that become the interface protrusions 16 after baking, and preferably satisfy the desired angle θ and Tw / Tn.

[0181] The manufacturing method involves applying a paste for the interface protrusions to the end face in the X-axis direction of the element body 4, drying it, and then baking it.

[0182] As a result, the interface protrusion particles contained in the interface protrusion paste become interface protrusions 16.

[0183] In this embodiment, the dielectric layers 10 and the internal electrode layers 12 are laminated in the Z-axis direction, but the lamination direction may be the X-axis direction or the Y-axis direction. In that case, the external electrode 6 may be formed in accordance with the exposed surface of the internal electrode layer 12. Furthermore, the element body 4 does not have to be a laminate, and may be a single layer. Furthermore, the internal electrode layer 12 may be drawn to the outer surface of the element body 4 via a through-hole electrode, in which case the through-hole electrode and the external electrode 6 are electrically connected. EXAMPLES

[0184] The present invention will be described in more detail below by way of examples of the present invention, but the present invention is not limited to these examples.

[0185] [ Experiment 1 ] < Sample No. 1 > BaTiO3 powder was prepared as the main raw material of the dielectric powder. Next, 1.6 molar parts of MgCO3 powder, 1.0 molar parts of Dy2O3 powder, 0.4 molar parts of MnCO3 powder, 0.06 molar parts of V2O5 powder, and 2.0 molar parts of SiO2 powder were weighed out as auxiliary components relative to 100 molar parts of the main raw material. These powders of the auxiliary components were wet mixed in a ball mill, dried, and calcined to obtain calcined powders of the auxiliary components.

[0186] Next, 100 parts by mass of the main raw material of the dielectric powder, the calcined powder of the secondary component obtained above, 7 parts by mass of acrylic resin, 4 parts by mass of butyl benzyl phthalate (BBP) as a plasticizer, and 80 parts by mass of methyl ethyl ketone as a solvent were mixed in a ball mill to form a paste, thereby obtaining a paste for the dielectric layer.

[0187] Separately from the above, 56 parts by weight of Ni particles, 40 parts by weight of terpineol, 4 parts by weight of ethyl cellulose (molecular weight 140,000), and 1 part by weight of benzotriazole were kneaded using a three-roll mill to form a paste, thereby preparing a paste for internal electrode layers.

[0188] Then, the dielectric layer paste prepared above was used to form a green sheet on a PET film, and the internal electrode layer paste was screen-printed to form a green sheet.

[0189] A plurality of green sheets were laminated and pressure-bonded to form a green laminate, and the green laminate was cut to a predetermined size to obtain a green chip.

[0190] Next, the obtained green chip was subjected to a binder removal treatment, sintering and annealing under the following conditions to obtain a sintered body (element body 4).

[0191] The binder removal treatment conditions were a holding temperature of 260° C. and an atmosphere of air.

[0192] The firing conditions were as follows: holding temperature: 1250°C. The atmospheric gas was a humidified N2+H2 mixed gas with an oxygen partial pressure of 10 -9 The pressure was adjusted to be less than MPa.

[0193] The annealing conditions were: holding temperature: 1050°C, atmospheric gas: humidified N2 gas (oxygen partial pressure: 10 -8 MPa or less).

[0194] A wetter was used to humidify the atmospheric gas during firing and annealing.

[0195] Next, small oxide particles and large oxide particles composed of B2O3-SiO2-ZnO were prepared. The ratio (Dw / Dn) of the average particle size (Dw) of the large oxide particles to the average particle size (Dn) of the small oxide particles was set to 2.8. Then, a paste for narrow portions containing Cu as metal powder and the above-mentioned small oxide particles was prepared. Also, a paste for wide portions containing Cu as metal powder and the above-mentioned large oxide particles was prepared.

[0196] The content of small oxide particles in the paste for the narrow width portion relative to the content of large oxide particles in the paste for the wide width portion was set to a mass ratio of 0.44.

[0197] The paste for the narrow portion was applied to both end faces in the X-axis direction of the element body 4 by dipping and dried, and the paste for the wide portion was applied thereon by dipping, dried, and baked at 800°C.

[0198] In this manner, a capacitor sample 2 (multilayer ceramic capacitor 2) having external electrodes 6 formed thereon was obtained.

[0199] The size of the element body 4 of the obtained capacitor sample 2 was L0×W0×T0=2.0 mm×1.25 mm×1.25 mm. The number of dielectric layers 10 sandwiched between the internal electrode layers 12 was 80.

[0200] The obtained capacitor sample was cut parallel to the XZ plane, and the obtained cross section was mirror-polished and then photographed by SEM. In addition, elemental analysis was performed by EPMA on the interface protrusion 16 part of the cross section of the obtained multilayer ceramic capacitor, and it was confirmed that the elemental composition of the small oxide particles and the large oxide particles was roughly the same as the elemental composition of the interface protrusion 16.

[0201] In a cross section (XZ cross section) including the vicinity of the interface between the element body 4 and the external electrode 6, 10 locations were photographed so as to include a predetermined length Lz (100 μm), and the number of "interface protrusions 16" and "interface protrusions 16 having constrictions 16c" per predetermined length Lz of the bond boundary 46 in each photograph was counted to determine the presence or absence, and the average number was calculated. As a result, it was confirmed that sample No. 1 was provided with "interface protrusions 16 having constrictions 16c," and that an average of 2.8 "interface protrusions 16 having constrictions 16c" were formed per predetermined length Lz (100 μm).

[0202] In addition, the average thickness Td of the dielectric layer 10 sandwiched between the internal electrode layers 12, the average thickness Te of the internal electrode layers 12, the average length Lr of the boundary layer 14, and the average thickness Le of the external electrode 6 were measured. Each was measured at 10 locations and the average value was calculated. The results are shown below.

[0203] Average thickness Td of the dielectric layer 10 sandwiched between the internal electrode layers 12: 10 μm Average thickness Te of the internal electrode layer 12: 1.5 μm Average length of boundary layer 14 Lr: 8.2 μm Average thickness of external electrode 6 Le: 89 μm

[0204] The linear expansion coefficient α of the dielectric layer 10, the linear expansion coefficient β of the external electrode 6, the linear expansion coefficient δ of the interface protrusions 16, the tensile strength test, and the 85° C. thermal shock tensile strength test of the obtained capacitor sample 2 were performed by the following methods.

[0205] Linear expansion coefficient The linear expansion coefficients of α, β, and δ were measured by thermomechanical analysis in air at temperatures ranging from 20 to 400° C. after preparing sintered bodies and glasses according to the compositions. The magnitude relationship of sample number 1 was β>α>δ.

[0206] Air tank thermal shock test In the air-bath thermal shock test, the test sample (capacitor sample) was held in an air bath at -55°C for 30 minutes, then held in an air bath at 150°C for 30 minutes, and this was repeated 1000 times. In this test, pass / fail was judged based on the rate of change in capacitance, and the capacitance C before the test was α After the test, the capacitance C β The rate of change (C β / C α ) was 0.9 (90%) or more, samples were deemed to have passed, and samples with a value less than 0.9 were deemed to have failed. For sample number 1, the above test was carried out on 80 samples, and the proportion of samples that failed (NG proportion) was calculated. The results are shown in Table 1.

[0207] < Sample No. 2 > For sample number 2, a capacitor sample was obtained in the same manner as sample number 1, except that an external electrode paste containing Cu as the metal powder and substantially no oxide was used instead of the "narrow portion paste and wide portion paste." The presence or absence of "interface protrusion 16" and "interface protrusion 16 having constriction 16c" in external electrode 6 was determined, and an air-tank thermal shock test was performed. The results are shown in Table 1.

[0208] < Sample No. 3 > For sample number 3, a capacitor sample was obtained in the same manner as sample number 1, except that instead of the "wide portion paste," an external electrode paste containing Cu as the metal powder and substantially no oxide was used, and the presence or absence of "interface protrusion 16" and "interface protrusion 16 having constriction 16c" in the external electrode 6 was determined, and an air-tank thermal shock test was performed. The results are shown in Table 1.

[0209] [Table 1]

[0210] From Table 1, it was confirmed that the results of the air-tank thermal shock test were better in the cases where the interfacial protrusions 16 were present (sample numbers 1 and 3) than in the case where the interfacial protrusions 16 were not present (sample number 2). Therefore, it is considered that the bonding reliability is higher in the cases where the interfacial protrusions 16 were present (sample numbers 1 and 3) than in the case where the interfacial protrusions 16 were not present (sample number 2).

[0211] Furthermore, it was confirmed from Table 1 that the results of the air-tank thermal shock test were better when interface protrusion 16 had constricted portion 16c (sample number 1) than when interface protrusion 16 did not have constricted portion 16c (sample number 3). Therefore, it is considered that the bonding reliability is higher when interface protrusion 16 has constricted portion 16c (sample number 1) than when interface protrusion 16 does not have constricted portion 16c (sample number 3).

[0212] [ Experiment 2 ] < Sample No. 1 > The above sample No. 1 was subjected to a liquid bath thermal shock test by the following method.

[0213] Liquid bath thermal shock test In the liquid bath thermal shock test, the thermal cycle is performed in a liquid bath instead of an air bath. When using a liquid bath, the test sample is subjected to a steeper temperature change than when using an air bath, so the bonding reliability of the test sample can be evaluated under more severe conditions than in the air bath test. Specifically, for sample number 1, the test sample was held in a -55°C liquid bath for 30 minutes per cycle, and then held in a 150°C liquid bath for 30 minutes, and this was repeated 1000 cycles. The pass / fail of the liquid bath thermal shock test was determined based on the rate of change in capacitance, as in the air bath thermal shock test. For sample number 1, the above test was performed on 80 samples, and the ratio of samples that failed (NG rate) was calculated. The results are shown in Table 2.

[0214] < Sample No. 11 > For sample number 11, a capacitor sample was obtained in the same manner as sample number 1, except that an interface protrusion paste containing interface protrusion particles was used instead of the narrow portion paste and the wide portion paste, and a liquid bath type thermal shock test was performed. The results are shown in Table 2. The total mass of the small oxide particles and large oxide particles in sample number 1 was equal to the mass of the interface protrusion particles in sample number 11.

[0215] For sample number 11, it was confirmed by SEM observation and elemental analysis by EPMA that the surface of the external electrode 6 facing the dielectric layer 10 was provided with an interface protrusion 16 having a constricted portion 16c.

[0216] < Sample No. 12 > For sample number 12, instead of the paste for the narrow width portion and the paste for the wide width portion, the paste for the interface protrusion portion used in sample number 11 was applied and dried, and then the paste for the outer external electrode was applied, dried, and baked. Except for this, a capacitor sample was obtained in the same manner as sample number 1, and a liquid bath type thermal shock test was performed. The results are shown in Table 2. The paste for the outer external electrode contained Cu as a metal powder, and further contained glass frit.

[0217] For sample number 12, it was confirmed by SEM observation and elemental analysis by EPMA that the surface of the external electrode 6 facing the dielectric layer 10 was provided with an interface protrusion 16 having a constricted portion 16c.

[0218] [Table 2]

[0219] From Table 2, it was confirmed that the liquid bath type thermal shock test was better when the paste for the narrow portion and the paste for the wide portion were used (sample number 1) than when the paste for the interface protrusions was used (sample numbers 11 and 12). Therefore, it is considered that the joining reliability is higher when the paste for the narrow portion and the paste for the wide portion were used (sample number 1) than when the paste for the interface protrusions was used (sample numbers 11 and 12).

[0220] [ Experiment 3 ] For sample numbers 21 and 22, capacitor samples were obtained in the same manner as sample number 1, except that the mass ratio of small oxide particles contained in the paste for the narrow portion to the large oxide particles contained in the paste for the wide portion was changed as shown in Table 3, and an air-tank type thermal shock test and a liquid-tank type thermal shock test were performed. The results are shown in Table 3.

[0221] [Table 3]

[0222] From Table 3, it was confirmed that when the average number of interfacial protrusions 16 having constrictions 16c per 100 μm length in the Z-axis direction of the bonded boundary 46 is 2.8 or more (sample numbers 1 and 22), the results of the liquid bath thermal shock test are better than when the average number is 0.6 (sample number 1). Therefore, when the average number of interfacial protrusions 16 having constrictions 16c per 100 μm length in the Z-axis direction of the bonded boundary 46 is 2.8 or more (sample numbers 1 and 22), it is considered that the bond reliability is higher than when the average number is 0.6 (sample number 1).

[0223] [ Experiment 4 ] <Sample No. 1> For the above sample number 1, 10 locations were photographed including a predetermined length Lz (100 μm) in a cross section (XZ cross section) including the vicinity of the interface between the element body 4 and the external electrode 6, and Tw / Tn of the interface protrusion 16 having the constriction 16c with the largest Tw per predetermined length Lz of the bond boundary 46 in each photograph was obtained, and the average value was calculated. The results are shown in Table 4.

[0224] For the above sample number 1, 10 locations were photographed including a predetermined length Lz (100 μm) in a cross section (XZ cross section) including the interface between the element body 4 and the external electrode 6, and the angle θ of the interface protrusion 16 having the narrowed portion 16c with the smallest angle θ per predetermined length Lz of the bond boundary 46 in each photograph was measured and the average value was calculated. The results are shown in Table 4.

[0225] < Samples No. 31 and 32 > For sample numbers 31 and 32, capacitor samples were obtained in the same manner as sample number 1, except that the ratio (Dw / Dn) of the average particle size of large oxide particles (Dw) to the average particle size of small oxide particles (Dn) was changed, and then "calculation of the average Tw / Tn of interface protrusions 16 having constrictions 16c with the largest Tw in a predetermined length (100 μm) in the Z-axis direction of bond boundary 46," "calculation of the average angle θ of interface protrusions 16 having constrictions 16c with the smallest angle θ in a predetermined length (100 μm) in the Z-axis direction of bond boundary 46," and liquid bath thermal shock tests were performed. The results are shown in Table 4.

[0226] [Table 4]

[0227] From Table 4, it was confirmed that when the specified Tw / Tn was 2.66 or more (sample numbers 1 and 31), the results of the liquid bath thermal shock test were better than when the Tw / Tn was 1.95 (sample number 32). Therefore, when the specified Tw / Tn was 2.66 or more (sample numbers 1 and 31), it is considered that the bonding reliability is higher than when the Tw / Tn was 1.95 (sample number 32).

[0228] From Table 4, it was confirmed that when the predetermined angle θ was 108° or less (sample numbers 1 and 31), the results of the liquid bath thermal shock test were better than when the angle θ was 117° (sample number 32). Therefore, when the predetermined angle θ was 108° or less (sample numbers 1 and 31), it is considered that the bonding reliability is higher than when the angle θ was 117° (sample number 32).

[0229] [ Experiment 5 ] For sample number 41, a capacitor sample was prepared in the same manner as sample number 1, except that the composition of the main component of dielectric layer 10 was as shown in Table 5, and an air-tank thermal shock test was performed. The results are shown in Table 5.

[0230] For sample number 41, it was confirmed by SEM observation and component analysis by EPMA that the surface of the external electrode 6 facing the dielectric layer 10 was provided with an interface protrusion 16 having a constricted portion 16c.

[0231] [Table 5]

[0232] From Table 5, the composition of the main component of the dielectric layer 10 is (Ca 0.7 Sr 0.3 )(Ti 0.04 Zr 0.96It was confirmed that the air-chamber thermal shock test was also favorable when the main component of the dielectric layer 10 was (Ca 0.7 Sr 0.3 )(Ti 0.04 Zr 0.96 It is believed that high bonding reliability was obtained even when the material was O3 (sample number 41).

[0233] [ Test 6 ] For sample numbers 51 to 53, capacitor samples were prepared in the same manner as sample number 1, except that the compositions of the large oxide particles and the small oxide particles were as shown in Table 6, and an air-tank thermal shock test was performed. The results are shown in Table 6.

[0234] For sample numbers 51 to 53, the obtained capacitor samples were cut parallel to the XZ plane, and the cross sections obtained were mirror-polished and then photographed by SEM. In addition, elemental analysis was performed by EPMA, and it was confirmed that the interface protrusions 16 having constrictions 16c were provided on the surface of the external electrode 6 facing the dielectric layer 10. It was also confirmed that the elemental composition of the small oxide particles and large oxide particles was roughly consistent with the elemental composition of the interface protrusions 16 having constrictions 16c.

[0235] [Table 6]

[0236] From Table 6, it was confirmed that the results of the air-tank thermal shock test were good when the interface protrusion 16 having the constricted portion 16c contained at least two of the main components selected from B, Si, and Zn (sample numbers 1, 51 to 53). Therefore, it is considered that high bonding reliability was obtained when the interface protrusion 16 having the constricted portion 16c contained at least two of the main components selected from B, Si, and Zn (sample numbers 1, 51 to 53). [Explanation of symbols]

[0237] 2. Multilayer ceramic capacitor (capacitor sample) 4... Element body 6... External electrode 61... Conductor 61a... Area between narrow width parts 62… Non-metallic components 10... Dielectric layer (ceramic layer) 12… Internal electrode layer 14… Boundary layer 16,160,161,162… Interface protrusion 16a,161a,162a… Narrow part 16aL… Tangent to narrow section 16b, 161b, 162b... Wide section 16bL… Tangent of wide part 16c... waist

Claims

1. an element body in which ceramic layers and internal electrode layers are laminated; an external electrode electrically connected to at least one end of the internal electrode layer, At least a part of a joint boundary between the external electrode and the ceramic layer has an interface protrusion on the external electrode side, the interface protrusion portion is made of an oxide, The linear expansion coefficient of the ceramic layer is defined as α, The linear expansion coefficient of the external electrode is β, When the linear expansion coefficient of the interface protrusion is δ, A ceramic electronic component in which the magnitude relationship between α, β, and δ is β>α>δ.

2. 2. The ceramic electronic component according to claim 1, wherein the external electrodes contain, as a main component, at least one selected from the group consisting of Cu, a Cu alloy, Ag, and an Ag alloy.

3. The interface protrusion portion is A narrow section and 3. The ceramic electronic component according to claim 1, further comprising: a wide portion that is adjacent to the narrow portion and is wider than the narrow portion, the wide portion being located closer to the inner side of the external electrode than the narrow portion.

4. 4. The ceramic electronic component according to claim 3, wherein there are two or more interfacial protrusions having a constriction formed by the narrow portion and the wide portion within a length of 100 μm of the joint boundary between the element body and the external electrode.

5. 5. The ceramic electronic component according to claim 3, wherein an angle θ of the constricted portion formed by a tangent line of the narrow width portion and a tangent line of the wide width portion satisfies 20°≦θ≦140°.

6. The width of the narrow portion is Tn, When the width of the wide portion is Tw, 6. The ceramic electronic component according to claim 3, wherein Tw / Tn at the interface protrusion is 2 or more.

7. 7. The ceramic electronic component according to claim 1, wherein at least a part of the oxide is glass.

8. 8. The ceramic electronic component according to claim 1, wherein the interface protrusions contain at least two kinds selected from the group consisting of B, Si and Zn as main components.

9. The ceramic layer is made of ABO 3 9. The ceramic electronic component according to claim 1, comprising, as a main component, a perovskite type compound represented by the following formula:

10. The ABO 3 The perovskite compound represented by the formula (Ba 1-a-b Sr a Ca b ) m (Ti 1-c-d Zr c Hf d ) O 3 and satisfying formulae: 0.94<m<1.1, 0≦a≦1, 0≦b≦1, 0≦c≦1, and 0≦d≦1.

Citation Information

Patent Citations

  • Ceramic capacitor

    JP1992171912A

  • Laminated ceramic electronic component and manufacture of the same

    JP2001035739A

  • Dielectric ceramic composition and layered ceramic capacitor

    JP2002164247A

  • Ceramic electronic component

    JP2010161175A

  • Multilayer ceramic electronic component and method for manufacturing same

    WO2014097701A1