Electrical steel strip or sheet for high frequency electric motor applications with improved polarization and low magnetic losses
A specifically composed and processed non-oriented electrical steel strip achieves high polarization and low magnetic losses, addressing the limitations of existing materials for high-efficiency electric machines.
Patent Information
- Application Number
- JP2021524159
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-08
- Filing Date
- 2019-11-07
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2039-11-07
AI Technical Summary
Existing non-oriented electrical steel strips and sheets fail to achieve high polarization values at high frequencies while maintaining low magnetic losses, which are essential for next-generation high-efficiency electric machines.
A non-oriented electrical steel strip with a specific composition (3.2-3.4% Si, 0.85-1.1% Al, 0.07-0.2% Mn, 0.01-0.04% P, 0.0003-0.0030% S, 0.0005-0.0025% N, 0.0010-0.0050% C, 0.0015-0.0040% Ti, up to 0.05% Nb+Mo+V, and 0.01-0.08% Cr) is produced through a process involving hot rolling, cold rolling, and a final heat treatment in a high-hydrogen atmosphere to achieve specific electrical resistance of 0.62-0.65 μΩm at 50°C.
The solution results in improved polarization and reduced magnetic losses at both low and high frequencies, with enhanced magnetic permeability, making it suitable for high-frequency applications in electric motors and generators.
Smart Images

Figure 0007587497000001 
Figure 0007587497000002 
Figure 0007587497000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel strip or sheet having a composition of 3.2 to 3.4 Si, 0.85 to 1.1 Al, 0.07 to 0.2 Mn, 0.01 to 0.04 P, 0.0003 to 0.0030 S, 0.0005 to 0.0025 N, 0.0010 to 0.0050 C, 0.0015 to 0.0040 Ti, 0.01 to 0.08 Cr, a total of up to 0.05 Nb+Mo+V, a total amount of up to 1.0 wt% of the balance Fe, and unavoidable impurities (all values are in weight percent). The present invention relates to a non-oriented electrical steel strip or sheet, characterized in that the non-oriented electrical steel strip or sheet has a specific electrical resistivity of 0.62 to 0.65 μΩm at 50° C., a manufacturing process thereof, and its use in iron cores of rotating electrical machines, in particular electric motors, for example electric vehicles or hybrid vehicles, and generators. [Background technology]
[0002] Non-oriented (NO) electrical steel strips or sheets are used to increase the magnetic flux of the iron cores of rotating electrical machines, i.e., motors and generators. The next generation of high-efficiency electrical machines, such as electric motors with high speed rotation for electric vehicles, require a specific type of NO electrical steel strips or sheets that have low magnetic losses at high frequencies and high magnetic polarization or induction with high magnetic permeability.
[0003] Components manufactured from electrical steel strips or sheets of this type now require the above mentioned magnetic properties which often cannot be met by the NO electrical steel strip or sheet types available today. Non-oriented electrical steel strips and their manufacturing processes are already known from the prior art.
[0004] EP 2612942 discloses a non-oriented electrical steel strip or sheet made of steel containing, apart from iron and unavoidable impurities, 1.0-4.5% by weight of Si, max. 2.0% by weight of Al, max. 1.0% by weight of Mn, max. 0.01% by weight of C, max. 0.01% by weight of N, max. 0.012% by weight of S, 0.1-0.5% by weight of Ti and 0.1-0.3% by weight of P, in which the ratio of Ti content / P content satisfies, in each case in % by weight, 1.0≦Ti content / P content≦2.0. The non-oriented electrical steel strip or sheet, and the parts for electrical applications manufactured from such steel sheets or strips, show improved strength and at the same time good magnetic properties. The NO electrical steel strip or sheet according to EP 2612942 is produced by cold rolling a hot rolled steel strip made of a steel having the above-mentioned composition to obtain a cold rolled steel strip, which is then subjected to a final heat treatment. The low frequency polarizability and mechanical properties of the electrical steel strip or sheet according to EP 2612942 still need to be improved.
[0005] EP 2840157 discloses a non-oriented electrical steel strip or sheet, particularly for electrical applications, made from a steel containing, apart from iron and unavoidable impurities, 2.0-4.5% by weight Si, 0.03-0.3% by weight Si, max. 2.0% by weight Al, max. 1.0% by weight Mn, max. 0.01% by weight C, max. 0.01% by weight N, max. 0.001% by weight S and max. 0.015% by weight P, in which ternary Fe-Si-Zr precipitates are present in the structure of the electrical steel strip or sheet. EP 2840157 also discloses a manufacturing process for such electrical steel strip and sheet, including a final heat treatment. The polarizability at low electric field strength and the mechanical properties of the electrical steel strip according to EP 2840157 still need to be improved.
[0006] WO 00 / 65103 discloses a process for producing a non-oriented electrical steel strip, in which an intermediate steel containing less than 0.06% by weight C, 0.03-2.5% by weight Si, less than 0.4% by weight Al, 0.05-1% by weight Mn and less than 0.02% by weight S is hot rolled to obtain a hot rolled steel strip having a thickness of less than 3.5 mm, followed by pickling and rolling after pickling to obtain a cold rolled steel strip having a thickness of 0.2-1 mm. The mechanical and magnetic properties of the electrical steel strip according to WO 00 / 65103 can be improved as well. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] European Patent No. 2612942 [Patent Document 2] European Patent No. 2840157 [Patent Document 3] WO 00 / 65103 Summary of the Invention [Problem to be solved by the invention]
[0008] In view of the prior art, it is an object of the present invention to provide a non-oriented electrical steel strip or sheet, and components for electrical applications manufactured from such a steel strip or sheet, which exhibits very high polarization values at relatively high frequencies of 400 Hz, 700 Hz and 1000 Hz at relatively low modulation ranges of 100-20 A / m, and at the same time low magnetic losses.
[0009] Furthermore, a process was to be provided for producing such NO magnetic steel strip or sheet which, as a result of a final heat treatment adapted to the indicated alloy, exhibits particularly low magnetic losses at both low and relatively high frequencies in combination with improved polarization values in the low modulation range. [Means for solving the problem]
[0010] These objectives are: Si of 3.2 to 3.4; Al, 0.85 to 1.1; Mn 0.07-0.18; P of 0.01 to 0.04, S of 0.0003 to 0.0030, N of 0.0005 to 0.0025, C of 0.0010 to 0.0050, Ti 0.0015~0.0040 0.01 to 0.08 Cr, Nb+Mo+V up to 0.05 in total, The balance of Fe and unavoidable impurities up to a total amount of 1.0% by weight (All values are in weight %) and has a specific electrical resistivity of 0.62 to 0.65 μΩm at 50° C. This is achieved by the non-oriented electrical steel strip or steel sheet of the present invention.
[0011] Further, the object of the present invention is to (A) providing a hot rolled and hot strip annealed non-oriented electrical steel strip or sheet with a thickness of 1.5 to 2.5 mm, preferably by a conventional production route by a continuous casting plant or by thin slab production; (B) cold rolling the electromagnetic steel strip or steel sheet obtained from step (A) to a thickness of 0.255 to 0.31 mm to obtain a cold rolled steel strip; (C) a process step of final heat treatment of the cold rolled steel strip obtained from step (B) to obtain a non-oriented electrical steel strip or sheet; (D) a process step of cooling the final heat treated cold rolled steel strip obtained from step (C) to a lower temperature of 500°C at a normal average cooling rate of 1 K / s to 10 K / s in a non-oxidizing atmosphere, in particular with a relatively high hydrogen content of more than 70%; A process for producing a non-oriented electrical steel strip or sheet according to the present invention, comprising at least This is achieved by a process in which the cold-rolled steel strip obtained from step (B) is first heated in step (C) to a temperature of 860-940°C, preferably 880-920°C, at a heating rate of at least 40 K / s and subsequently to a temperature of 1050-1070°C at a heating rate of 3-20 K / s, by components manufactured from such electrical steel strip or sheet, as well as by the use of this non-oriented electrical steel strip or sheet in the cores of rotating electrical machines, in particular electric motors, e.g. electric or hybrid vehicles, and generators.
[0012] The non-oriented electrical steel strip or sheet of the invention has an improved polarization J in the range of 100-200 A / m and an improved magnetic permeability in the range of 0.8-1.2 T. At the same time, the magnetic losses, both at low frequencies, for example 50 Hz, and at high frequencies, for example 400-1000 Hz, are reduced compared to the materials of the prior art. This behavior is achieved according to the invention by precisely adapted alloy compositions and specially adapted heat treatments during manufacture.
[0013] The present invention relates to Si of 3.20 to 3.40, preferably Si of 3.25 to 3.35; 0.85 to 1.1 Al, preferably 0.95 to 1.05 Al, Mn of 0.07 to 0.18, preferably Mn of 0.14 to 0.16, P of 0.01 to 0.04, preferably P of 0.015 to 0.02, S of 0.0003 to 0.0030, preferably S of 0.0005 to 0.002; N of 0.0005 to 0.0025, preferably N of 0.001 to 0.002; C of 0.0010 to 0.0050, preferably C of 0.0015 to 0.0025, 0.0015 to 0.0040 Ti, preferably 0.0017 to 0.0035 Ti, 0.01 to 0.08 Cr, preferably 0.02 to 0.06, particularly preferably 0.02 to 0.04 Cr; Nb+Mo+V up to 0.05 in total, The balance of Fe and unavoidable impurities totaling up to 1.0% by weight (All values are in weight %) and has a specific electric resistivity of 0.62 to 0.65 μΩm at 50°C.
[0014] For the purposes of the present invention, inevitable impurities are, for example, C, S, N, Ti, Cr, Ni, Cu, As, Pb and Bi.
[0015] The non-oriented electrical steel strip or sheet of the present invention has a specific electrical resistivity of 0.62 to 0.65 μΩm at 50° C. Methods for determining the specific electrical resistivity are known per se to those skilled in the art. For example, a method for determining the specific electrical resistivity by a four-point measurement according to DIN EN 60404-13:2008-05 “Magnetic materials-part 13: Methods of measurement of resistivity, density and stacking factor of electrical steel strip and sheet” is known per se to those skilled in the art.
[0016] A relatively high specific electrical resistivity reduces eddy current losses that occur as the frequency increases, thereby reducing magnetic losses.
[0017] For the purposes of the present invention, electrical steel strip means that the material according to the invention is present in the form of a steel strip, i.e. the length of the steel strip is significantly greater than its width. For the purposes of the present invention, electrical steel sheet means that the material according to the invention is present in the form of steel sheets, the width and length of these sheets being not limited in terms of size, other than by the width and length of the steel strip from which they are preferably obtained. In a preferred embodiment, the electrical steel sheet according to the present invention is obtained from the electrical steel strip according to the present invention by cutting or stamping. The electrical steel sheet according to the present invention can be made into a shape suitable for use, for example, in the stator or rotor of an electric motor.
[0018] Furthermore, the present invention provides a non-oriented electrical steel strip or sheet according to the present invention, in which the total content of C, S, N and Ti is 0.0090% by weight or less.
[0019] The non-oriented electrical steel strip or sheet according to the invention has a final thickness of 0.255 to 0.31 mm. For the purposes of the present invention, "final thickness" means the thickness of the non-oriented electrical steel strip or sheet after cold rolling, i.e. in the form in which it is subsequently used, for example, also for electric motors.
[0020] The present invention further preferably provides a non-oriented electrical steel strip or sheet according to the invention, during the manufacture of which a heat treatment step is carried out at a maximum temperature of 1050-1070°C, preferably 1055-1065°C. This particular manufacturing method provides a corresponding electrical steel strip or sheet with an improved polarization J of 100-200 A / m and an improved magnetic permeability in the range of 0.8-1.2 T. At the same time, the magnetic losses are reduced both at low frequencies, for example 50 Hz, and at high frequencies, for example 400-1000 Hz, in comparison with the materials of the prior art.
[0021] For example, the present invention provides a non-oriented electrical steel strip or sheet according to the present invention, which has, at a polarization P of 1.5 T and at 50 Hz, a loss value of 2.3 W / kg or less in any case for a steel sheet thickness of 0.280 to 0.310 mm and a loss value of 2.2 W / kg or less in any case for a steel sheet thickness of 0.255 to 0.280 mm.
[0022] The present invention preferably provides a non-oriented electrical steel strip or sheet according to the invention, which at a polarization P of 1.0 T and at 400 Hz has in each case loss values of less than or equal to 14.2 W / kg for sheet thicknesses of 0.280 to 0.310 mm and in each case loss values of less than or equal to 13.55 W / kg for sheet thicknesses of 0.255 to 0.280 mm.
[0023] The present invention preferably provides a non-oriented electrical steel strip or sheet according to the invention, which at a polarization P of 1.0 T and at 700 Hz has in each case loss values of less than or equal to 33 W / kg for a steel sheet thickness of 0.280 to 0.310 mm and in each case loss values of less than or equal to 31.5 W / kg for a steel sheet thickness of 0.255 to 0.280 mm.
[0024] The invention preferably provides a non-oriented electrical steel strip or sheet according to the invention, which at a polarization P of 1.0 T and at 1000 Hz has in each case loss values of less than or equal to 58 W / kg for a steel sheet thickness of 0.280 to 0.310 mm and in each case loss values of less than or equal to 55 W / kg for a steel sheet thickness of 0.255 to 0.280 mm.
[0025] Furthermore, in the non-oriented electrical steel strip or sheet of the present invention, the ratio of the polarization J at 50 Hz and 100 A / m to the magnetic losses P at 1 T and 400 Hz is particularly advantageous, i.e. high. This ratio is expressed by the following formula (1): 100*J 100A / m、50Hz / P 1.0T、400Hz (1) The present invention preferably provides a non-oriented electrical steel strip or sheet according to the invention, in which the ratio of the polarization J at 50 Hz and 100 A / m to the magnetic loss P at 1 T and 400 Hz times 100 is at least 6.8, preferably at least 7.0.
[0026] Furthermore, in the non-oriented electrical steel strip or sheet according to the invention, the ratio of the polarization J at 400 Hz and 100 A / m to the magnetic loss P at 1 T and 400 Hz is advantageous, i.e. high, by a factor of 100. This ratio is expressed by the following formula (2): 100*J 100A / m 400Hz / P 1.0T 400Hz (2) The present invention preferably provides a non-oriented electrical steel strip or sheet according to the invention, in which the ratio of the polarization J at 400 Hz and 100 A / m to the magnetic losses P at 1 T and 400 Hz is at least 6.0, preferably at least 6.1.
[0027] Furthermore, the non-oriented electrical steel strip or sheet according to the invention preferably has a polarization J of at least 1.53 T at a modulation of 2500 A / m, at least 1.63 at 5000 A / m and / or at least 1.75 at 10000 A / m, in each case with a sheet thickness of 0.280 to 0.310 mm, and a polarization J of at least 1.52 T at a modulation of 2500 A / m, at least 1.62 at 5000 A / m and / or at least 1.75 at 10000 A / m, in each case with a sheet thickness of 0.255 to 0.280 mm.
[0028] The present invention also provides (A) providing a hot rolled and hot strip annealed non-oriented electrical steel strip or sheet with a thickness of 1.5 to 2.5 mm by a conventional production route, preferably by a continuous casting plant; (B) cold rolling the electromagnetic steel strip or steel sheet obtained from step (A) to a thickness of 0.255 to 0.310 mm to obtain a cold rolled steel strip; (C) a process step of final heat treatment of the cold rolled steel strip obtained from step (B) to obtain a non-oriented electrical steel strip or sheet; (D) a process step of cooling the final heat treated cold rolled steel strip obtained from step (C) to a lower temperature of 500°C at a normal average cooling rate of 1 K / s to 10 K / s in a non-oxidizing atmosphere, in particular with a relatively high hydrogen content of more than 70%; A process for producing a non-oriented electrical steel strip or sheet according to the present invention, comprising at least The cold rolled steel strip obtained from step (B) is in step (C) first heated to a temperature of 860-940°C, preferably 880-920°C, at a heating rate of at least 40 K / s and subsequently heated to a temperature of 1050-1070°C, preferably 1055-1065°C, at a heating rate of 3-20 K / s. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The individual steps of the process of the present invention are described in detail below.
[0030] Step (A) of the process of the present invention comprises providing a hot rolled non-oriented electrical steel strip or sheet with a thickness of 1.5 to 2.5 mm, preferably by the conventional production route by continuous casting plants or by thin slab production.
[0031] The hot rolled non-oriented electrical steel strip or sheet provided in step (A) of the process of the present invention has the composition described above. The provision of the hot rolled non-oriented electrical steel strip in step (A) of the process of the present invention is preferably carried out by the conventional production route by continuous casting plants or by thin slab production.
[0032] The production of the hot-rolled steel strip provided according to the invention can be carried out largely conventionally, for which purpose a steel melt having a composition corresponding to that defined according to the invention is first melted and cast to obtain an intermediate material, which in the case of conventional production can be a slab or a thin slab.
[0033] The intermediate material thus produced can then be brought to an intermediate material temperature of 1020-1300° C. For this purpose, the intermediate material is reheated if necessary or maintained at the respective target temperature using the heat of casting.
[0034] The intermediate material thus heated can then be hot rolled to obtain a hot rolled steel strip having a thickness typically between 1.5 and 2.5 mm, the hot rolling being carried out in a manner known per se starting at an initial hot rolling temperature of the finishing series between 1000 and 1150°C and ending at a final hot rolling temperature between 700 and 920°C, in particular between 780 and 850°C.
[0035] The resulting hot-rolled steel strip can then be cooled to a reeling temperature and wound into coils. The reeling temperature is ideally selected so as to avoid problems during the subsequent cold rolling. In practice, the reeling temperature is for this purpose, for example, below 700°C.
[0036] The hot-rolled electrical steel strip or sheet obtained from step (A) can be used directly in step (B) of the process of the invention. In a preferred embodiment of the process of the invention, the invention provides a process according to the invention, in which in step (A') after step (A), i.e. before step (B), a heat treatment in a bell furnace is carried out at a temperature of 700-800 ° C, preferably at a temperature of 720-760 ° C. Thus, the hot-rolled and hot-strip-annealed non-oriented electrical steel strip or sheet is provided for step (B) in a preferred embodiment, preferably by conventional production routes by continuous casting plants or by thin slab production, with a thickness of 1.5-2.5 mm.
[0037] Step (B) of the process of the present invention involves cold rolling the electrical steel strip or sheet obtained from step (A) to a thickness of 0.255-0.310 mm to obtain a cold rolled steel strip.
[0038] Step (B) of the process of the present invention can generally be carried out by any method known to those skilled in the art.
[0039] The cold rolled steel strip obtained from step (B) can be transferred directly to step (C) of the process of the present invention.
[0040] Step (C) of the process of the present invention comprises a final heat treatment of the cold rolled steel strip obtained from step (B) to obtain a non-oriented electrical steel strip or sheet, in which the cold rolled steel strip obtained from step (B) is first heated in step (C) to a temperature of 860-940°C, preferably 880-920°C, at a heating rate of at least 40 K / s and subsequently heated to a temperature of 1050-1070°C, preferably 1055-1065°C, at a heating rate of 3-20 K / s.
[0041] The final heat treatment in step (C) of the process of the present invention comprises at least the two sub-steps mentioned and may be subject to additional heating and / or cooling steps.
[0042] The cold rolled steel strip obtained from step (B) is first heated in step (C) to a temperature of 860-940° C., preferably 880-920° C., at a heating rate of at least 3-20 K / s.
[0043] Step (C) of the process according to the invention can in principle be carried out in any apparatus known to the person skilled in the art, in particular in continuous furnaces, particularly preferably in horizontal continuous furnaces.
[0044] In a preferred embodiment of the process of the invention, step (C) is carried out at low strip tension. This has the advantage that only small forces are applied to the cold rolled strip during the heat treatment step, so that the anisotropy of the magnetic losses in the longitudinal and transverse directions remains very low. The invention therefore preferably provides that step (C) is carried out at a tension of 10 N / mm 2 The process of the present invention is provided, which is carried out at the following strip tensions:
[0045] Step (C) of the process of the invention is preferably carried out in a reducing atmosphere. It is particularly preferred that step (C) of the process of the invention is carried out in a heat treatment atmosphere containing at least 70% by volume, in particular at least 85% by volume, of hydrogen. Apart from hydrogen, nitrogen may also be present in the heat treatment atmosphere. Nitrogen leads to a decrease in the magnetic properties as a result of nitridation of the surface.
[0046] Step (C) of the process of the invention is preferably carried out at a low dew point. Step (C) of the process of the invention is preferably carried out at a dew point below -10°C, particularly preferably below -20°C.
[0047] Step (D) of the process of the invention comprises cooling the final heat treated cold rolled steel strip obtained from step (C) at a typical average cooling rate between 1 K / s and 10 K / s, in particular in a non-oxidizing atmosphere containing a relatively high proportion of hydrogen, more than 70%, down to a lower temperature of 500° C.
[0048] After step (D) of the process of the invention, the non-oriented electrical steel strip according to the invention is in principle in a form which can be used in the applications described. The non-oriented electrical steel strip obtained from step (D) may be subjected to further process steps, such as cleaning, winding, cutting and / or stamping of the electrical steel sheet.
[0049] Therefore, the present invention also provides the above-mentioned inventive non-oriented electrical steel strip or sheet, having a suitable composition and produced by the process according to the present invention comprising at least process steps (A) to (D) as described above.
[0050] The invention also provides components for electrical applications, in particular cores of rotating electrical machines, in particular electric motors, for example electric or hybrid vehicles, and generators, manufactured from the non-oriented electrical steel strip or sheet according to the invention. The corresponding processes for manufacturing such components, for example stamping, cutting, laser cutting, adhesive bonding, etc., are known per se to the person skilled in the art.
[0051] The present invention also provides the use of the non-oriented electrical steel strip or sheet according to the invention in the cores of rotating electrical machines, in particular electric motors, for example electric or hybrid vehicles, and generators.
[0052] According to the invention, the magnetic losses P can be determined by any method known to the person skilled in the art, in particular by means of an Epstein frame, in accordance with DIN EN 60404-2:2009-01:Magnetic material-part 2:Methods of measurement of the magnetic properties of electrical steel strip and sheet by means of an Epstein frame", in which a suitable magnetic steel sheet is cut into longitudinal and transverse strips and measured as a mixed specimen in an Epstein frame.
[0053] The non-oriented electrical steel strip described herein has an anisotropy of magnetic loss values at 1.5 T and 50 Hz of less than 20% in the longitudinal and transverse directions.
[0054] [Example] The following examples serve to illustrate the invention. The steel compositions used are given in Table 1. [Table 1]
[0055] Examples 10-20 and 22-33 according to the invention as well as comparative test pieces V1-V9 and V21 were produced. For this purpose, after melting the compositions according to table 1, the slabs obtained in each case were hot rolled and (optionally) subjected to a hot-rolled strip bell furnace heat treatment at 740 ° C and pickled. This material was subsequently cold rolled to a final thickness of 0.255-0.310 mm (see tables 2 and 3) and then subjected to a final heat treatment. Comparative test pieces V1-V9 and V21 as well as examples 10-20 and 22-33 according to the invention were final heat treated at the heat treatment temperatures indicated in tables 2 and 3. The thicknesses obtained are likewise indicated in tables 2 and 3.
[0056] In each case the specific magnetic properties were determined for the specimens after the final heat treatment: J 100A / m 50Hz, J 100A / m 400Hz, J 2500A / m, J 5000A / m, J 10000A / m, P1.5T 50Hz, P1.0T 400Hz, P1.0T 700Hz and P1.0T 1000Hz. In addition, the following ratios were determined: J 100A / m、50Hz / P 1.0T 400Hz (1) J 100A / m 400Hz / P 1.0T 400Hz (2) [Table 2] [Table 3] [Industrial Applicability]
[0057] The non-oriented electrical steel strip or sheet of the present invention exhibits improved polarization at 100-200 A / m, improved permeability at 0.8-1.2 T, and at the same time reduced magnetic losses at low frequencies of 50 Hz and high frequencies of 400-1000 Hz, and can therefore be advantageously used in rotating electrical machines, in particular electric motors and generators.
Claims
1. A non-oriented electrical steel strip or sheet having the following composition (all values are in weight percent): Si from 3.20 to 3.40; Al from 0.85 to 1.10, Mn between 0.07 and 0.18; P between 0.01 and 0.04; S of 0.0003 to 0.0030, N between 0.0005 and 0.0025; C between 0.0010 and 0.0050; Ti from 0.0015 to 0.0040, 0.01 to 0.08 Cr, Nb+Mo+V in total up to 0.05; Less than 1% by weight of unavoidable impurities, and The balance is Fe; It has a specific electrical resistivity of 0.62 to 0.65 μΩm at 50° C. A non-oriented electrical steel strip or sheet, characterized in that the ratio of polarization at 50 Hz and 100 A / m to magnetic loss at 1 T and 400 Hz (polarization / magnetic loss) is 100 times at least 6.
8.
2. 2. The non-oriented electrical steel strip or sheet according to claim 1, characterized in that the ratio of the polarization at 400 Hz and 100 A / m to the magnetic loss at 1 T and 400 Hz (polarization / magnetic loss) times 100 is at least 6.
0.
3. In each case, with a steel sheet thickness of 0.280 to 0.31 mm, the loss values are 2.3 W / kg or less at 1.5 T polarization J and 50 Hz; 14.2 W / kg or less at 1.0 T polarization and 400 Hz; 33 W / kg or less at 1.0 T polarization and 700 Hz; and 58 W / kg or less at 1.0 T polarization and 1000 Hz, 3. The non-oriented electrical steel strip or sheet according to claim 1 or 2, characterized in that in each case with a steel sheet thickness of 0.255 to 0.280 mm, it has loss values of 2.2 W / kg or less at a polarization J of 1.5 T and 50 Hz; 13.6 W / kg or less at a polarization J of 1.0 T and 400 Hz; 32 W / kg or less at a polarization J of 1.0 T and 700 Hz; and 55 W / kg or less at a polarization J of 1.0 T and 1000 Hz.
4. 4. A non-oriented electrical steel strip or sheet according to claim 1, characterized in that it has a final thickness of 0.255 to 0.31 mm.
5. 5. The non-oriented electrical steel strip or sheet according to claim 1, wherein the total of C, S, N and Ti is 0.0090% by weight or less.
6. In each case with a steel sheet thickness of 0.280 to 0.31 mm, the polarization J at a modulation of 2500 A / m is at least 1.53 T; the polarization J at a modulation of 5000 A / m is at least 1.63; and / or the polarization J at a modulation of 10000 A / m is at least 1.75 T, 6. A non-oriented electrical steel strip or sheet according to claim 1 , characterized in that the polarization J at a modulation of 2500 A / m is at least 1.52 T; the polarization J at a modulation of 5000 A / m is at least 1.62; and / or the polarization J at a modulation of 10000 A / m is at least 1.75, in each case with a steel sheet thickness of 0.255 to 0.280 mm.
7. A process for producing a non-oriented electrical steel strip or sheet according to any one of claims 1 to 6, comprising the steps of: (A) providing a hot rolled and hot strip annealed steel strip or sheet having a thickness of 1.5 to 2.5 mm; (B) cold rolling the steel strip or the steel sheet obtained from step (A) to a thickness of 0.255 to 0.31 mm to obtain a cold rolled steel strip or a cold rolled steel sheet; (C) a process step of subjecting the cold rolled steel strip or the cold rolled steel sheet obtained from step (B) to a final heat treatment; (D) a process step of cooling the final heat treated cold rolled steel strip or sheet obtained from step (C) in a non-oxidizing atmosphere at a normal average cooling rate of 1 K / s to 10 K / s to a lower limit temperature of 500° C.; At least 13. A process according to claim 12, characterized in that the cold rolled steel strip or sheet obtained from step (B) is in step (C) first heated to a temperature of 860-940°C with a heating rate of at least 40 K / s and subsequently heated to a temperature of 1050-1070°C with a heating rate of 3-20 K / s.
8. Step (C) is 10 N / mm 2 8. The process according to claim 7, characterized in that it is carried out with a strip tension of:
9. 9. The process according to claim 7 or 8, characterized in that step (C) is carried out in a heat treatment atmosphere containing at least 70% by volume of hydrogen.
10. 10. The process according to any one of claims 7 to 9, characterized in that step (C) is carried out at a dew point of -10°C or less.
11. Process according to any one of claims 7 to 10, characterised in that the hot rolled and hot strip annealed steel strip or sheet is provided for step (B) with a thickness of 1.5 to 2.5 mm.
12. 12. The process according to any one of claims 7 to 11, characterized in that step (A) is carried out by the conventional production route by continuous casting plants or by thin slab production.
13. 13. The process according to any one of claims 7 to 12, characterized in that step (D) is carried out in a non-oxidizing atmosphere containing a relatively high hydrogen content, more than 70%.
14. The process according to any one of claims 7 to 13, characterized in that the initial heating in step (C) is at a temperature of from 880 to 920°C.
15. A part for electrical applications made of the non-oriented electrical steel strip or sheet according to any one of claims 1 to 6.
16. 16. The part for electrical applications according to claim 15, which is an iron core of a rotating electrical machine, an electric motor of an electric or hybrid vehicle, or a generator.
17. 7. Use of the non-oriented electrical steel strip or sheet according to any one of claims 1 to 6 in an iron core of a rotating electrical machine, an electric motor of an electric or hybrid vehicle, or a generator.
Citation Information
Patent Citations
Non-grain oriented electrical steel or sheet metal, component produced from same and method for producing non-grain oriented electrical steel or sheet metal
EP2612942A1
Non-grain oriented electrical steel or sheet metal, component produced from same and method for producing non-grain oriented electrical steel or sheet metal
EP2840157A1
Nonoriented silicon steel sheet with minimal magnetic anisotropy and high magnetic flux density, and its manufacture
JP2001049402A
Nonoriented silicon steel sheet low in core loss and producing method therefor
JP2001158948A
Non-oriented silicon steel sheet for rotating machine and production method thereof
JP2003253404A