Method for extracting lithium from an electric battery containing solid metallic lithium
The method addresses the inefficiencies in recovering solid metallic lithium from lithium metal polymer batteries by orienting and heating the assemblies to melt lithium under controlled conditions, using gravity and compression to enhance recovery while minimizing risks and contamination.
Patent Information
- Application Number
- JP2021546244
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-15
- Filing Date
- 2020-02-07
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-02-07
AI Technical Summary
Current methods are inadequate for efficiently recovering solid metallic lithium from lithium metal polymer batteries, posing risks of short circuits and uncontrollable reactions during recycling.
A method involving specific orientation and heating of battery assemblies to melt metallic lithium, combined with gravity-driven extraction and optional compression, using inert gases or denser liquids to manage short circuits and enhance recovery.
Facilitates safe and efficient recovery of solid metallic lithium by minimizing short circuit risks and controlling chemical reactions, increasing yield and reducing contamination.
Smart Images

Figure 0007587510000001 
Figure 0007587510000002 
Figure 0007587510000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for extracting lithium from batteries containing solid metallic lithium.
[0002] The field of the invention is that of solid-state lithium metal based batteries, in particular that of lithium metal polymer batteries, and even more particularly that of the recycling of these batteries. [Background technology]
[0003] Solid-state lithium metal-based batteries are known, such as for example Lithium Metal Polymer (LMP®) batteries. These batteries are increasingly used, for example, in electric vehicles or charging stations. The number of LMP® batteries has therefore been growing for several years.
[0004] It is believed that LMP® batteries do not have an infinite lifespan and that these batteries need to be recycled. Currently, even at the end of their life, LMP® batteries still contain solid metallic lithium that can be reused in other batteries or in other fields, and their value is not significant.
[0005] However, there is currently no technology that can effectively recover solid metallic lithium from batteries.
[0006] The aim of the present invention is to overcome this drawback. Another object of the invention is to propose a method for recovering solid metallic lithium from an assembly of at least one electric energy storage cell.
[0007] Another object of the invention is to propose a method for recovering solid metallic lithium from an assembly of at least one electric energy storage cell in a simple manner.
[0008] Another object of the present invention is to propose a method for recovering solid metallic lithium from an assembly of at least one electrical energy storage cell in an efficient manner, while limiting and managing the effects of potential short circuits during recycling. DISCLOSURE OF THEINVENTION
[0009] First solution proposed by the present invention According to a first solution, the invention makes it possible to achieve at least one of these objectives by means of a method for extracting lithium from an assembly of at least one cell of an electric battery containing solid metallic lithium, such as a lithium metal polymer battery, said method comprising the following steps: positioning the assembly in an orientation such that a first edge of the assembly from which one or more negative electrodes extend is opposite the first edge and below a second edge of the assembly from which one or more positive electrodes extend; heating the assembly to a temperature equal to or above the melting temperature of the solid metallic lithium, referred to as the processing temperature; The method comprises the steps of:
[0010] The method according to the invention proposes to recover lithium from a battery containing solid lithium by treating, individually or together, the cells which constitute said battery.
[0011] In addition, the method according to the invention proposes to recover metallic lithium (preferably in solid form) from an assembly of at least one cell in which lithium is in liquid state, by heating said assembly of cells to a processing temperature higher than the melting temperature of solid metallic lithium. Once melted, the metallic lithium will naturally drain, in whole or in part, from each cell under the effect of gravity.
[0012] The method according to the invention therefore allows a simple and less complicated recovery of solid metallic lithium.
[0013] Furthermore, the method according to the invention proposes a particular orientation of each cell with a minimum inclination so that a first edge from which the negative electrode extends is located below the level of a second edge opposite the first edge and from which the positive electrode extends. Such an orientation of each cell makes it possible, on the one hand, to facilitate the flow of molten lithium from the cell by gravity and, on the other hand, to avoid contact between the molten lithium and the positive electrode or the current collector of the positive electrode, which could cause an electrical short circuit or an electric arc, which could cause a fire.
[0014] In this application, an "electrical energy storage cell" refers to at least one a negative electrode formed by or including a layer of solid metallic lithium; A positive electrode and a solid electrolyte, particularly comprising a lithium salt, disposed between the positive electrode and the negative electrode; The positive electrode current collector and "assembly" means an assembly comprising:
[0015] In this application, "solid metallic lithium" means Pure metallic lithium, or A combination of at least one metallic lithium alloy, or A combination of pure metallic lithium and at least one metallic lithium alloy may include.
[0016] When "solid metallic lithium" includes a combination of different forms of lithium, such as those set forth above, having different melting temperatures, the heating step may include: the lowest temperature of the different melting temperatures, and Preferably, the highest temperature of the different melting temperatures The cell assembly is then heated to a processing temperature above.
[0017] According to a non-limiting example embodiment, the processing temperature is 180.5° C. or higher.
[0018] According to one example embodiment, the processing temperature is up to a maximum temperature, for example 300°C.
[0019] The assembly may comprise a single or only one cell. The assembly may comprise several cells assembled, or in particular stacked, in an assembly direction, which may be perpendicular to the plane formed by each cell.
[0020] In particular, the assembly can accommodate a battery having cells connected in series.
[0021] According to a preferred embodiment, the positioning step may involve vertical positioning of the assembly of cells with the first edge downwards.
[0022] Thus, the gravity flow of molten lithium from each cell is improved. In addition, the risk of contact between the molten lithium and the positive electrode(s) is reduced, i.e., eliminated.
[0023] Preferably, the step of heating the assembly of cells can be carried out under inert gas. The method according to the invention therefore reduces the risk of accidents, in particular the risk of fire.
[0024] In addition, the method according to the invention makes it possible to avoid the formation of contaminating compounds that may be produced by undesired or uncontrolled physicochemical reactions during the extraction of lithium.
[0025] By way of non-limiting example, the inert gas may be or include any one of the following gases: helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe), and radon (Rn).
[0026] According to another embodiment, the step of heating the assembly of cells can be performed under vacuum.
[0027] According to a particularly advantageous feature, the method according to the invention can also comprise a step of charging the assembly of cells before the extraction step, said extraction step being applied to said charged assembly.
[0028] The fact of charging one or more cells and carrying out the extraction step on the charged cells makes it possible to increase the lithium extraction yield: in fact, the charging of the cells makes it possible to displace lithium ions towards the negative electrode, thus increasing the recoverable amount of lithium.
[0029] Each cell can be charged individually or by charging an assembly of cells.
[0030] According to a particularly advantageous embodiment, the extraction stage may also comprise a step of compressing the assembly of cells.
[0031] Thus, molten lithium is evacuated from each cell, increasing the amount of recovered lithium. The compression step can be performed continuously throughout the extraction phase, with each cell being partially or totally compressed for the entire duration of the extraction phase.
[0032] Alternatively, the compression step can be carried out separately, once or several times, during the extraction phase, which in this case includes moments during which the assembly of cells is not subjected to compression.
[0033] Advantageously, the compression step can be performed by sweeping the surface of the assembly of cells from the second edge to the first edge, thereby exerting compression on said surface of the assembly, so that the molten lithium is gradually conveyed / guided towards the first edge from which the negative electrode or electrodes extend, thereby increasing the amount of lithium recovered and reducing the risk of contact between the lithium and the positive electrode or electrodes.
[0034] For example, the compression step can be performed by passing the assembly of cells between two rollers.
[0035] According to another example, the compression step can be performed by a compression roller that compresses the assembly of cells against a bearing surface.
[0036] Compression can be applied in successive passes, each pass sweeping the surface of the cell assembly starting from the second edge to the first edge.
[0037] Between the compression rollers, the gap between each compression roller and the bearing surface can correspond to the thickness of the cell assembly minus the thickness of the solid metallic lithium layer or layers, allowing compression to be applied while the solid lithium still remains within the cell assembly.
[0038] The gap between the two compression rollers, or between the compression roller and the bearing surface, respectively, can be reduced with successive passes so as to still apply compression to the assembly of cells.
[0039] The passing speed, or more generally the sweep speed, of each compression roller between the compression rollers can be comprised between a few mm and a few tens of mm per second.
[0040] Furthermore, the method according to the invention may comprise the step of removing at least one electrical connector, also known as a "crimp connector", from at least one cell prior to the extraction stage. This allows for easy handling of the assembly of the cells.
[0041] Furthermore, the method according to the invention may comprise, prior to the extraction stage, a step of removing excess material of at least one of the assemblies of cells, in particular at the level of each edge.
[0042] According to another aspect of the same invention, an installation is proposed for extracting lithium from an assembly of at least one cell of an electric battery containing solid metallic lithium, such as a lithium metal polymer battery, said installation comprising: means for positioning the assembly in an orientation such that a first edge of the assembly from which one or more negative electrodes extend is opposite the first edge and below a second edge of the assembly from which one or more positive electrodes extend; heating means configured to heat the assembly to a processing temperature above the melting temperature of the solid metallic lithium; Equipped with.
[0043] In general, the facility comprises means, not described in detail herein for the sake of brevity, configured to implement at least one of any combination of the above mentioned features.
[0044] In particular, the heating means may comprise an oven. Advantageously, the oven may be filled with an inert gas or placed under vacuum.
[0045] The installation according to the invention may also comprise means for compressing the assembly of cells. The compression means may comprise at least one roller.
[0046] In particular, the compression means may comprise a single roller which compresses the assembly of cells against a bearing surface. The bearing surface may be heated to accelerate the temperature rise of the assembly of cells.
[0047] Alternatively, the compression means may comprise two rollers between which the assembly of cells passes.
[0048] In general, the compression means may be arranged to apply continuous compression throughout the extraction stage.
[0049] Alternatively, the compression means may be configured to apply compression discontinuously over time, once or several times during the extraction phase, in which case the extraction phase includes moments during which the assembly of cells is not subjected to compression.
[0050] Advantageously, the compression step can be configured to apply a constant or variable compression from the second edge to the first edge, either gradually or by sweeping over the surface of the cell assembly, so that the molten lithium is gradually conveyed / guided towards the lowered first edge, increasing the amount of lithium recovered and reducing the risk of contact between the lithium and the positive electrode(s).
[0051] When one or two compression rollers are used, compression can be applied to the cell assembly by successive passes. Each pass applies compression by sweeping over the surface of the cell assembly from the second edge to the first edge. At the end of each pass, compression can be stopped by withdrawing the roller or by withdrawing the roller from the bearing surface to return to the second edge and begin a new pass.
[0052] The distance between the rollers, respectively between the compression roller and the bearing surface, can be reduced between successive passes, in particular between two successive passes.
[0053] The method according to the invention can be carried out to process an assembly of several cells, in particular an assembly of several cells which form a battery pack and are connected to one another in parallel within said battery pack.
[0054] At least two assemblies of cells can be aligned side-by-side, for example in a direction parallel to the first edge, without overlapping.
[0055] In this case, compression can be applied to at least two assemblies of cells by one and the same compression means, ie a set of rollers or one roller cooperating with a bearing surface.
[0056] The second solution proposed by the present invention According to a second solution, the invention makes it possible to achieve at least one of these objectives by means of a method for extracting lithium from an assembly of at least one cell of an electric battery containing solid metallic lithium, such as a lithium metal polymer battery, said method comprising the following steps: positioning the assembly in an orientation such that a first edge of the assembly from which one or more negative electrodes extend is opposite the first edge and above a second edge of the assembly from which one or more positive electrodes extend; immersing the assembly of cells in a liquid that is denser and more electrically insulating than liquid lithium; heating the assembly to a temperature equal to or above the melting temperature of the solid metallic lithium, referred to as the processing temperature; The method comprises the steps of:
[0057] The method according to the invention proposes to recover lithium from a lithium-containing battery by treating, individually or together, the cells which constitute said battery.
[0058] In addition, the method according to the invention proposes to recover metallic lithium from at least one assembly of cells in which lithium has been brought into liquid state, by heating said assembly of cells to a processing temperature higher than the melting temperature of solid metallic lithium. Once melted, metallic lithium is naturally discharged from each cell under the effect of density differences. The method according to the invention therefore allows a simple and less complicated recovery of solid metallic lithium.
[0059] Furthermore, the method according to the invention proposes a particular orientation of each cell with a minimum inclination so that the first edge from which the negative electrode extends is located above the height of the second edge opposite the first edge from which the positive electrode extends. Such an orientation of each cell makes it possible, on the one hand, to facilitate the flow of molten lithium from the cell due to density differences, and, on the other hand, to avoid contact between the molten lithium and the positive electrode or the current collector of the positive electrode, which can cause an electrical short circuit, which can cause a fire. In addition, immersion of the assembly of cells in a liquid makes it possible to improve the dissipation of calories from the cell, especially during a short circuit, thus significantly limiting its effects.
[0060] In this application, an "electrical energy storage cell" refers to at least one a negative electrode formed by or including a layer of solid metallic lithium; A positive electrode and a solid electrolyte, particularly comprising a lithium salt, disposed between the positive electrode and the negative electrode; The positive electrode current collector and "assembly" means an assembly comprising:
[0061] In this application, "density" means the ratio between the mass density of the liquid in question and the mass density of water.
[0062] In this application, "solid metallic lithium" means Pure metallic lithium, or A combination of at least one metallic lithium alloy, or A combination of pure metallic lithium and at least one metallic lithium alloy may include.
[0063] When "solid metallic lithium" includes a combination of different forms of lithium, such as those set forth above, having different melting temperatures, the heating step may include: the lowest of the different melting temperatures, or preferably the highest of the different melting temperatures, or For example, a combination of different temperatures or an entire temperature gradient extending from a first edge to a second edge. The cell assembly is then heated to a processing temperature above.
[0064] According to a non-limiting example embodiment, the processing temperature is 180.5° C. or higher when utilizing pure metallic lithium.
[0065] According to one example embodiment, the processing temperature is up to a maximum temperature, for example 300°C.
[0066] The assembly may comprise a single or only one cell. The assembly may comprise several cells assembled, or in particular stacked, in an assembly direction, which may be perpendicular to the plane formed by each cell.
[0067] In particular, the assembly can accommodate a battery having cells connected in series.
[0068] According to a preferred embodiment, the positioning step may involve vertical positioning of the assembly of cells with the first edge positioned upwards.
[0069] Thus, the flow of molten lithium out of each cell due to density differences is improved. In addition, the risk of contact between the molten lithium and the positive electrode(s) is reduced, i.e., eliminated.
[0070] Preferably, the immersion step is carried out by immersing the cell assembly completely in the liquid.
[0071] The method according to the invention therefore reduces the risk of accidents, in particular the risk of fire.In addition, the method according to the invention makes it possible to avoid the formation of contaminating compounds that may be produced by undesired or uncontrolled physicochemical reactions during the extraction of lithium, in particular by controlling the processing temperature and the density of the liquid so as to be able to extract only lithium or lithium alloys.
[0072] According to a particularly advantageous feature, the method according to the invention can also comprise a step of charging the assembly of cells before the extraction step, said extraction step being applied to said charged assembly.
[0073] The fact of charging one or more cells and carrying out the extraction step on the charged cells makes it possible to increase the lithium extraction yield: in fact, the charging of the cells makes it possible to displace lithium ions towards the negative electrode, thus increasing the recoverable amount of lithium.
[0074] Each cell can be charged individually or by charging an assembly of cells.
[0075] According to a particularly advantageous embodiment, the extraction stage may also comprise a step of compressing the assembly of cells.
[0076] Thus, molten lithium is pumped out of each cell, increasing the amount of lithium recovered and the reaction rate of the process.
[0077] The compression step can be performed continuously throughout the extraction phase, with each cell being partially or totally compressed for the entire duration of the extraction phase.
[0078] Alternatively, the compression step can be carried out separately, once or several times, during the extraction phase, which in this case includes moments during which the assembly of cells is not subjected to compression.
[0079] Advantageously, the compression step can be performed by sweeping the surface of the assembly of cells from the second edge to the first edge, thereby exerting compression on said surface of the assembly, so that the molten lithium is gradually conveyed / guided towards the first edge from which the negative electrode or electrodes extend, thereby increasing the amount of lithium recovered and reducing the risk of contact between the lithium or lithium alloy and the positive electrode or electrodes.
[0080] For example, the compression step can be performed by passing the assembly of cells between two rollers.
[0081] According to another example, the compression step can be performed by a compression roller that compresses the assembly of cells against a bearing surface.
[0082] The compression step can be applied in successive passes, each pass sweeping the surface of the assembly of cells starting from the second edge to the first edge.
[0083] Between the compression rollers, the gap between each compression roller and the bearing surface can correspond to the thickness of the cell assembly minus the thickness of the solid metallic lithium layer or layers, allowing compression to be applied while the solid lithium still remains within the cell assembly.
[0084] The gap between the two compression rollers, also called platens, respectively between the compression roller and the bearing surface, can be reduced with successive passes so as to still apply compression to the assembly of cells.
[0085] The passing speed, or more generally the sweep speed, between the compression rollers or between the respective compression rollers cooperating with the platen may be comprised between a few mm and several tens of mm per second.
[0086] Furthermore, the method according to the invention may comprise the step of removing at least one electrical connector, also known as a "crimp connector", from the cell prior to the extraction stage. This allows for easy handling of the assembly of the cells.
[0087] Furthermore, the method according to the invention may comprise, prior to the extraction stage, a step of removing excess material of at least one of the assemblies of cells, in particular at the level of each edge.
[0088] According to another aspect of the same invention, an installation is proposed for extracting lithium from an assembly of at least one electric battery cell containing solid metallic lithium, such as a lithium metal polymer battery, said installation comprising: means for positioning the assembly in an orientation such that a first edge of the assembly from which one or more negative electrodes extend is opposite the first edge and above a second edge of the assembly from which one or more positive electrodes extend; an oven filled with a liquid that is denser and more electrically insulating than liquid lithium; heating means configured to heat the assembly to a processing temperature above the melting temperature of the solid metallic lithium; Equipped with.
[0089] In general, the facility comprises means, not described in detail herein for the sake of brevity, configured to implement at least one of any combination of the above mentioned features.
[0090] The liquid may be a natural or synthetic oil, comprising the following physicochemical properties: Hydrophobic and non-reactive towards lithium, Electrical insulation, Higher density than lithium, - Thermally stable even above the melting point of lithium, i.e. 180.5℃ Highest possible flash point and autoignition point.
[0091] The installation according to the invention may also comprise means for compressing the assembly of cells. The compression means may comprise at least one roller.
[0092] In particular, the compression means may comprise a single roller which compresses the assembly of cells against a bearing surface. The bearing surface may be heated to accelerate the temperature rise of the assembly of cells.
[0093] Alternatively, the compression means may comprise two rollers between which the assembly of cells passes.
[0094] In general, the compression steps can be arranged to apply continuous compression throughout the extraction stage.
[0095] Alternatively, the compression means may be configured to apply compression discontinuously over time, once or several times during the extraction phase, in which case the extraction phase includes moments during which the assembly of cells is not subjected to compression.
[0096] Advantageously, the compression means may be configured to apply a constant or variable compression from the second edge to the first edge, either gradually or by sweeping over the surface of the assembly of cells, so that the molten lithium is gradually conveyed / guided towards the lowered first edge, increasing the amount of lithium recovered and reducing the risk of contact between the lithium and the positive electrode(s).
[0097] When one or two compression rollers are used, compression can be applied to the cell assembly by successive passes. Each pass applies compression by sweeping over the surface of the cell assembly from the second edge to the first edge. At the end of each pass, compression can be stopped by withdrawing the roller or by withdrawing the roller from the bearing surface to return to the second edge and begin a new pass.
[0098] The distance between the rollers, respectively between the compression roller and the bearing surface, can be reduced between successive passes, in particular between two successive passes.
[0099] The method according to the invention can be carried out to process an assembly of several cells, in particular an assembly of several cells which form a battery pack and are connected to one another in parallel within said battery pack.
[0100] At least two assemblies of cells can be aligned side-by-side, for example in a direction parallel to the first edge, without overlapping.
[0101] In this case, compression can be applied to at least two assemblies of cells by one and the same compression means, ie a set of rollers or one roller cooperating with a bearing surface. [Brief description of the drawings]
[0102] Other advantages and features will become apparent from a consideration of the detailed description of the embodiments, which is by no means limiting, and from the accompanying drawings. [Figure 1] 1 is a schematic diagram of an example of a non-limiting embodiment of a cell in the sense of the present invention; [Diagram 2] FIG. 2 is a schematic diagram of an example of a non-limiting embodiment of an assembly of cells in the sense of the present invention. [Diagram 3] FIG. 2 is a schematic diagram of a first non-limiting embodiment example of the method according to the invention, which is compatible with the first proposed solution. [Figure 4] FIG. 2 is a schematic diagram of a second non-limiting embodiment example of the method according to the invention, which is compatible with the first proposed solution. [Diagram 5] FIG. 2 is a schematic diagram of an example of a non-limiting embodiment of an installation according to the invention, which is compatible with the first solution proposed. [Figure 6] FIG. 2 is a schematic diagram of a first non-limiting embodiment example of the method according to the invention, which is compatible with the second proposed solution. [Figure 7]FIG. 4 is a schematic diagram of a second non-limiting embodiment example of the method according to the invention, which is compatible with the second proposed solution. [Figure 8] FIG. 2 is a schematic diagram of an example of a non-limiting embodiment of an installation according to the invention, which is compatible with the second proposed solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0103] It is fully understood that the embodiments described below are in no way limiting. Variations of the present invention may be envisaged that include only a selection of features described below, if this selection of features, apart from the other features described, confers a technical advantage or is sufficient to distinguish the present invention over the prior art. This selection includes at least one, preferably functional feature, without structural details or including only a portion of the structural details, if only this portion confers a technical advantage or is sufficient to distinguish the present invention over the prior art.
[0104] In the figures, elements that are common to several figures retain the same reference numbers. In this application, "density" means the ratio between the mass density of the liquid in question and the mass density of water.
[0105] The liquid may be a natural or synthetic oil, comprising the following physicochemical properties: Hydrophobic and non-reactive towards lithium, Electrical insulation, Higher density than lithium, - Thermally stable even above the melting point of lithium, i.e. 180.5℃ Highest possible flash point and autoignition point.
[0106] FIG. 1 is a schematic diagram of an example of a non-limiting embodiment of a cell in the sense of the invention, regardless of which of the two proposed solutions is implemented.
[0107] The cell 100 shown in FIG. 1 includes a negative electrode 102 formed by or including a layer of solid metallic lithium.
[0108] The cell 100 also includes a positive electrode 104. The positive electrode 104 is generally formed by a layer of a composite material based on a polymer and an active material.
[0109] A layer of solid electrolyte 106 is disposed between the anode 102 and the cathode 104. The layer of solid electrolyte 106 can include, for example, a lithium salt.
[0110] The cell 100 also includes a current collector 108 on the side of the positive electrode 104. The current collector 108 is typically made from aluminum.
[0111] Conventionally, the negative electrode 102 of the cell 100 extends beyond the other elements of the cell 100 on a first edge 110 of the cell 100, here to the right in the figure, and the positive electrode 104 and / or current collector 108 of the cell 100 (said current collector 108 is connected to the positive electrode 104) extends beyond the other elements of the cell 100 on a second edge 112 opposite the first edge 110. In the illustrated example, only the current collector 108 extends beyond the assembly 100 on its second edge 112, here to the left in the figure. In other examples, the extension may include only the positive electrode 104, or also the positive electrode 104 and the current collector 108.
[0112] It will be appreciated that the cell 100 shown in Fig. 1 is a very simplified version of a realization, given as a non-limiting example: a cell in the sense of the present invention may comprise other layers than those shown, or more layers, or layers whose composition differs from the composition given here as a non-limiting example.
[0113] FIG. 2 is a schematic diagram of a non-limiting embodiment example of an assembly of cells in the sense of the invention, regardless of which of the two proposed solutions is implemented.
[0114] The cell assembly 200 shown in FIG. 2 comprises one or more cells in the sense of the present invention.
[0115] In particular, the cell assembly 200 comprises several identical cells 100 i assembled in a direction 202 perpendicular to the plane of the layer of each cell 100 1 ~100 n and includes.
[0116] Each cell 100 i may be identical to the cell 100 of FIG. 1. In addition, between two adjacent cells 100 i ~100 i+1 (i < n), a positive electrode 204 i , and a current collector 206 connected thereto i are arranged.
[0117] Example of an embodiment according to the first proposed solution FIG. 3 is a schematic diagram of an example of a first non-limiting embodiment of a method according to the invention that conforms to the proposed first solution.
[0118] The method 300 shown in FIG. 3 includes a first optional step 302 during which the electrical connectors of the cell assembly, in particular current concentrators also known as "crimp connectors", are removed.
[0119] During an optional step 304, excess material, in particular solid metallic lithium, at the height of each side edge of the cell assembly is removed.
[0120] The method 300 then includes a step 306 of extracting metallic lithium from the cells.
[0121] The extraction phase 306 includes a step 308 of positioning the assembly of cells in an orientation in which a first edge from which one or more negative electrodes extend is at a lower height than a second edge from which one or more positive electrodes and current collectors extend. In particular, step 308 positions the assembly of cells in a vertical orientation, i.e., parallel to the gravity vector, with one or more negative electrodes extending downward from the edge. Preferably, but by no means limiting, the assembly of cells is maintained in this orientation throughout the entire extraction phase 306.
[0122] The extraction stage 306 also includes a step 310 of heating the assembly of cells to a processing temperature above the melting temperature of the solid metallic lithium present in the assembly of cells, for example a temperature of 180.5° C. This temperature causes melting of the solid metallic lithium and extraction of the solid metallic lithium from each cell by natural drainage under the influence of gravity. Preferably, but by no means limiting, the assembly of cells is maintained at this temperature throughout the entire extraction stage 306.
[0123] Advantageously, the heating step is carried out in a sealed enclosure filled with an inert gas.
[0124] The extraction stage 306 may also include an optional step 312 of compressing the assembly of cells to flush the molten lithium from each cell. Compression may be performed continuously throughout all or part of the extraction stage 306. Alternatively, the compression step 312 may be repeated several times discontinuously during the extraction stage 306. Preferably, the compression step 312 is performed by applying compression gradually or by sweeping over the surface of the assembly of cells, starting from the second edge from which the one or more positive electrodes extend and moving toward the first edge from which the one or more negative electrodes extend.
[0125] FIG. 4 is a schematic diagram of another non-limiting embodiment example of the method according to the invention, which is compatible with the first solution proposed.
[0126] The method 400 shown in FIG. 4 includes all the steps of the method 300 of FIG.
[0127] Method 400 also includes a step 402 of recharging the treated cells prior to the steps of method 300.
[0128] Each cell can be partially or fully recharged. The fact of charging each cell makes it possible to increase the amount of lithium available for extraction, since recharging causes the migration of lithium ions to the negative electrode of the cell.
[0129] FIG. 5 is a schematic diagram of an example of a non-limiting embodiment of an installation according to the invention, which is compatible with the first solution proposed.
[0130] The installation 500 shown in FIG. 5 can be used to implement the methods according to the invention, in particular the methods 300 and 400 of FIGS.
[0131] The facility 500 allows for the extraction and recovery of some or all of the lithium from a battery cell containing solid metallic lithium, such as, for example, the cell 100 of FIG. 1, or from an assembly of cells, such as the assembly 200 of FIG.
[0132] The equipment 500 includes an oven 502, filled with an inert gas or under vacuum, configured to heat the cells to a processing temperature above the melting temperature of the solid metallic lithium present in the cells, e.g., 180.5°C or 181°C.
[0133] The fixture 500 comprises a pair of jaws 504 for holding the cell 100 or cell assembly 200 in a vertical, or at least inclined, position in which the first edge 110 is positioned below the level of the second edge 112. Each jaw 504 is movably mounted on a vertical rail 506 to displace the cell or cell assembly 200 vertically.
[0134] The apparatus 500 also comprises a pair of rollers 508 having a gap between them corresponding to the thickness of the cell 100 or cell assembly 200 minus the thickness of the solid layer of metallic lithium. The pair of rollers are positioned such that, when the jaws 504 are displaced upwards, the cell 100, respectively the cell assembly 200, passes between the rollers 508, starting from the second edge 112. The rollers thus apply a progressive compression to the cell 100, respectively the cell assembly 200, starting from the second edge 112 and moving towards the first edge 110.
[0135] The equipment also includes a container 510 for collecting the molten metallic lithium that flows out of each cell under the influence of gravity. The container 510 must be inert to lithium.
[0136] Example of an embodiment according to the second proposed solution FIG. 6 is a schematic diagram of a non-limiting embodiment example of a method according to the invention, which is compatible with the second proposed solution.
[0137] The method 600 shown in FIG. 6 includes a first optional step 602 during which the electrical connectors, also known as "crimp connectors," of each battery cell are removed.
[0138] During optional step 604, excess material at the height of each side edge of the assembly of cells is removed.
[0139] The method 600 then includes the step 606 of extracting metallic lithium from the cell.
[0140] The extraction phase 606 includes a step 608 of positioning the cell assembly in an orientation in which a first edge 110, from which one or more negative electrodes 102 extend, is at a higher vertical height than a second edge 112, from which one or more positive electrodes 104 and current collectors extend. In particular, step 608 positions the cell assembly in a vertical orientation, i.e., parallel to the gravity vector, with one or more negative electrodes 102 extending upward from the edge. Preferably, but by no means limiting, the cell assembly is maintained in this orientation throughout the extraction phase 606.
[0141] The extraction stage 606 includes a step 609 of immersing the assembly of cells in a liquid 850 (see FIG. 8). For example, in the embodiment shown in FIG. 8, the liquid 850 is a natural or synthetic oil, such as paraffin oil, that includes the following physicochemical properties: Hydrophobic and non-reactive towards lithium, Electrical insulation, Higher density than lithium, - Thermally stable even above the melting point of lithium, i.e. 180.5℃ The flash point must be as high as possible, e.g. above 600°C, but at least above the processing temperature of the cell, as well as the autoignition point.
[0142] The immersion step 609 is performed by immersing the cell assembly 200 in the liquid 850 such that the liquid 850 completely covers the cell assembly 200 .
[0143] This immersion step 609 is particularly advantageous in promoting significant heat exchange between the cell and the liquid 850, which limits the risk of overheating the cell during a short circuit and the elimination of generated calories, and improves the heating rate.
[0144] The extraction stage 606 also includes a step 610 of heating the assembly of cells to a processing temperature above the melting temperature of the solid metallic lithium present in the assembly of cells, for example a temperature of 180.5° C. In the embodiment presented, the liquid 850 is heated by an oven, which transfers heat to the assembly of cells. Once the melting temperature of lithium is exceeded, the temperature causes the melting of the solid metallic lithium and its extraction from each cell by natural drainage under the influence of gravity. Preferably, but by no means limiting, the assembly of cells is maintained at this temperature throughout the extraction stage 606. The processing temperature must not exceed the decomposition temperature of the liquid 850, specific for each liquid 850, above which the liquid 850 decomposes. In other words, the liquid 850 changes properties when it exceeds a threshold temperature, so that the aforementioned properties are no longer fulfilled. Ideally, the decomposition temperature of the liquid must be higher than +40° C. relative to the melting temperature of lithium (for example, + 30 ℃~+60℃).
[0145] Thus, the method for extracting lithium from a battery allows for limiting the effects of a short circuit potential by flowing the lithium through the first edge 110 from which one or more negative electrodes 102 extend, and allows for controlling short circuits by immersing the cell assembly in a liquid that does not react with lithium and improving the dissipation of calories from the cell assembly, particularly during a short circuit.
[0146] The extraction stage 606 may also include an optional step 612 of compressing the assembly of cells to accelerate the extraction of the molten lithium from each cell. Compression may be performed continuously throughout all or part of the extraction stage 606. Alternatively, the compression step 612 may be repeated several times discontinuously during the extraction stage 606. Preferably, the compression step 612 is performed by applying compression gradually or by sweeping over the surface of the assembly of cells, starting from the second edge 112 from which one or more positive electrodes 104 extend and moving toward the first edge 110 from which one or more negative electrodes 102 extend.
[0147] FIG. 7 is a schematic diagram of another non-limiting embodiment example of the method according to the invention, which is compatible with the second proposed solution.
[0148] The method 700 shown in FIG. 7 includes all the steps of the method 600 of FIG.
[0149] Method 700 also includes a step 702 of recharging one or more cells that were processed prior to the steps of method 600.
[0150] Each cell can be partially or fully recharged. The fact of charging each cell makes it possible to increase the amount of lithium available for extraction, since recharging causes the migration of lithium ions to the negative electrode of the cell, improving the amount of lithium extracted as well as the kinetics of operation.
[0151] FIG. 8 is a schematic diagram of a non-limiting embodiment example of an installation according to the invention, which is compatible with the second solution proposed.
[0152] The installation 800 shown in FIG. 8 can be used to implement the methods according to the invention, in particular the methods 600 and 700 of FIGS.
[0153] The facility 800 allows for the extraction and recovery of some or all of the lithium from a battery cell containing solid metallic lithium, such as, for example, the cell 100 of FIG. 1, or from an assembly of cells, such as the assembly 200 of FIG.
[0154] The equipment 800 comprises an oven 802 filled with a liquid 850 configured to heat the cells to a processing temperature above the melting temperature of the solid metallic lithium present in the cells, for example 180.5° C. or 181° C. In the embodiment presented, the liquid 850 is heated by the oven 802 and transfers heat to the assembly of cells.
[0155] The fixture 800 comprises a pair of jaws 804 for holding a cell 100 or cell assembly 200 in a vertical, or at least inclined, position where a first edge 110 is positioned above the level of a second edge 112. Each jaw 804 is movably mounted on a vertical rail 806 to displace the cell 100 or cell assembly 200 vertically.
[0156] The liquid 850 completely covers the cell assembly such that the first edge 110 is below the level of the liquid 850 .
[0157] The apparatus 800 also comprises a pair of rollers 808 having a gap between them corresponding to the thickness of the cell 100 or assembly of cells 200 minus the thickness of one or more solid layers of metallic lithium. The pair of rollers are positioned such that, when the jaws 804 are displaced upwards, the cell 100, respectively the assembly of cells 200, passes between the rollers 808, starting from the second edge 112. The rollers thus apply progressive compression to the cell 100, respectively the cell assembly 200, starting from the second edge 112 and moving towards the first edge 110.
[0158] Of course, the invention is not limited to the examples detailed above. For example, the composition of an electric battery cell containing solid metallic lithium may differ from that shown in FIG.
[0159] In addition, the apparatus according to the present invention may include apparatus other than that shown in Figures 5-7, such as means for disconnecting electrical connectors from the cells, means for cutting off excess portions of one or each of the edges, etc.
[0160] For example, jaws 504 and 804, respectively, may be fixed and rollers 508 and 808, respectively, may be movable, and may compress the assembly of cells from top to bottom and bottom to top, respectively, according to an embodiment.
[0161] In addition, it is possible to use a single oven and several pairs of rollers dedicated to one cell or assembly of cells.
[0162] A pair of rollers can operate to process several adjacent assemblies of cells simultaneously.
[0163] As an example, step 609 can be performed by submerging the cell 100 or cell assembly 200 in the liquid 850, or by filling the oven 802 with the liquid 850 such that the liquid 850 covers the cell assembly 200, the cell 100, respectively.
[0164] It should be noted that the orientation of the first edge 110 of the assembly from which the negative electrode or electrodes 102 extend is a function of the density of the fluid in which the cell 100 or the assembly of cells 200 is immersed. If the fluid is a gas, which is covered by the first solution proposed by the present invention, the first edge 110 is located below the second edge 112 from which the positive electrode or electrodes 104 extend, since the gas has a lower density than lithium. If the fluid is a liquid, which is covered by the second solution proposed by the present invention, which is denser than lithium, the first edge 110 is located above the second edge 112.
[0165] If the fluid is a liquid less dense than lithium, the orientation of the first edge 110 will be below the second edge 112, as shown in the first embodiment.
[0166] In addition, the direction of compression of the cells 100 by the rollers 508, 808, respectively, is more favorable to compress the cells from the second edge 112 to the first edge 110. Thus, depending on the density of the fluid, the direction of compression is not the same, as can be seen in the examples shown in Figures 5 and 8.
[0167] The first edge 110 can be characterized by the fact that it defines the side to which the lithium must flow once it is in a liquid state.
Claims
1. A method (300, 400) for extracting lithium from an assembly (200) of at least one cell (100) of an electric battery containing solid metallic lithium, in order to melt and drain the metallic lithium wholly or partially from each cell under the influence of gravity, said method (300, 400) comprising the following steps: positioning (308) the assembly (200) in an orientation such that a first edge (110) of the assembly (200) from which one or more negative electrodes (102) extend is opposite (112) to the first edge (110) and below a second edge (112) of the assembly (200) from which one or more positive electrodes (104) extend; heating (310) the assembly to a temperature equal to or above the melting temperature of the solid metallic lithium, referred to as the processing temperature; The method (300, 400) includes an extraction step (306) including:
2. 2. The method (300, 400) of claim 1, wherein the positioning step (308) comprises vertically positioning the assembly of cells (200) with the first edge (110) below.
3. 3. The method (300, 400) according to claim 1 or 2, characterized in that the step (310) of heating the assembly (200) of cells is carried out under inert gas.
4. 3. The method (300, 400) according to claim 1 or 2, characterized in that the step (310) of heating the assembly (200) of cells is carried out under vacuum.
5. The method (400) according to any one of claims 1 to 4, further comprising a step (402) of charging the assembly (200) of cells prior to the extraction step (306), characterized in that the extraction step (306) is applied to the charged assembly (200).
6. The method (300, 400) according to any one of the preceding claims, characterized in that the extraction stage (306) further comprises the step (312) of compressing the assembly of cells (200).
7. 7. The method (300, 400) of claim 6, wherein the compressing step (312) applies compression to the surface of the assembly (200) by sweeping the surface of the assembly (200) from the second edge (112) to the first edge (110).
8. The method (300, 400) according to any one of the preceding claims, characterized in that it comprises a step (302) of removing at least one electrical connector from at least one cell (100) prior to said extraction stage (306).
9. An apparatus (500) for extracting lithium from an assembly (200) of at least one cell (100) of an electric battery containing solid metallic lithium, said apparatus (500) comprising: a means (504) for positioning the assembly (200) in an orientation such that a first edge (110) of the assembly (200) from which one or more negative electrodes (102) extend is opposite the first edge (110) and below a second edge (112) of the assembly from which one or more positive electrodes (104) extend; heating means (502) configured to heat the assembly (200) to a processing temperature equal to or higher than the melting temperature of the solid metallic lithium; The facility (500).
10. 10. Installation (500) according to claim 9, characterized in that said heating means comprise an oven (502) filled with inert gas.
11. Installation (500) according to claim 9 or 10, characterized in that it comprises means (508) of compression of said assembly (200) of cells.
12. 12. Installation (500) according to claim 11, characterized in that said compression means comprise two rollers (508) between which the assembly of cells passes.
Citation Information
Patent Citations
Method for recovering lithium, cobalt and other metal
JP2012112027A
Method of recovering valuable metals from wasted batteries and system for the same
KR101883100B1
Solid-state battery and regeneration method therefor
WO2012035631A1