Hyaluronic acid hydrogels with sustained antimicrobial activity
Polyarginine-filled HA hydrogels with specific cross-linking address the antimicrobial and stability issues of hyaluronic acid hydrogels, offering effective bacteriostatic properties and improved tissue regeneration.
Patent Information
- Application Number
- JP2021564802
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-02
- Filing Date
- 2020-04-30
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-04-30
AI Technical Summary
Hyaluronic acid hydrogels lack antimicrobial activity and have a short half-life, posing challenges in biomedical applications such as implant infections and tissue engineering.
Development of polyarginine-filled HA hydrogels that are cross-linked at the hydroxyl moieties, maintaining the carboxyl moieties negatively charged, providing long-term antimicrobial effects.
The hydrogels exhibit significant bacteriostatic activity against various pathogens, including ESKAPE pathogens, with sustained antimicrobial effects and minimal cytotoxicity, enhancing tissue regeneration and implant integration.
Smart Images

Figure 0007587524000010 
Figure 0007587524000011 
Figure 0007587524000012
Abstract
Description
[Technical field]
[0001] The present invention relates to hydrogels having antimicrobial activity. [Background technology]
[0002] The implantation of biomedical devices is frequently followed by excessive immune responses against the implant, as well as infections with bacteria, yeast, and fungi. Inflammation and infection can severely affect the function of the implants and even lead to their failure.
[0003] Thus, there is a significant need for solutions to avoid such infections following implantation of biomedical devices.
[0004] Hydrogels have several unique features, including similarity to the extracellular matrix of tissues, support for cell proliferation and migration, controlled release of drugs or growth factors, minimal mechanical stimulation to the surrounding tissue, and diffusion of nutrients that support cell viability and proliferation. As a result, hydrogels are promising materials in the field of tissue engineering.
[0005] Hyaluronic acid is widely used in the preparation of biomaterials for tissue engineering because it produces biomaterials that are easy to regenerate and affordable. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Biomed ResInt.2016; 2016:2475067 Summary of the Invention [Problem to be solved by the invention]
[0007] However, HA hydrogel itself has no activity against possible infections.Furthermore, the use of HA in tissue engineering is associated with a number of drawbacks, such as a short half-life and rapid turnover, which affect the benefits of its use in tissue engineering.
[0008] Thus, there is a critical need for new materials useful for biomedical device implantation or tissue engineering that are easy for physicians to manipulate, do not have too rapid a turnover, and have antimicrobial activity while being safe for patient treatment.
[0009] The present invention meets this need.
[0010] The present invention arose from the unexpected discovery by the inventors that it is possible to develop polyarginine-loaded HA hydrogels that provide long-term antimicrobial effects and can be easily deposited onto wound dressings and mesh prostheses to prevent infection, thus improving tissue regeneration and / or improving implant integration. [Means for solving the problem]
[0011] The present invention therefore relates to a hydrogel comprising hyaluronic acid (HA) or a derivative thereof and loaded with at least one positively charged antimicrobial peptide, wherein the HA or derivative thereof is crosslinked at the level of its hydroxyl moieties by a crosslinker, while the carboxyl moieties of the HA or derivative thereof remain free and the HA or derivative thereof remains negatively charged.
[0012] Another object of the invention is a method for preparing a hydrogel according to the invention, comprising the steps of: (a) mixing, under basic conditions, hyaluronic acid (HA) or a derivative thereof with a crosslinking agent that crosslinks HA at the level of its hydroxyl moieties while leaving the carboxyl moieties of HA or its derivative free and leaving HA or its derivative negatively charged; (b) depositing the mixture on a support and incubating it at room temperature for 48 to 72 hours to obtain a hydrogel; (c) recovering the hydrogel formed in step (b); (d) incubating the hydrogel in an aqueous buffer under conditions that allow for removal of crosslinker residues and swelling of the hydrogel; (e) loading the hydrogel obtained in step (d) with at least one positively charged antimicrobial peptide; (f) recovering the loaded hydrogel obtained in step (e); The present invention relates to a method comprising the steps of:
[0013] Yet another object of the invention relates to a hydrogel according to the invention, possibly obtainable by the process of preparation of the invention.
[0014] The present invention further relates to medical devices comprising a hydrogel according to the present invention. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram of the preparation process of hydrogels. [Diagram 2] FIG. 1 shows the construction between Parafilm and a glass slide. [Diagram 3] Figure 1 shows the bacterial growth in HA films pre-loaded and post-loaded with PAR. Bacterial growth was assessed after 24 hours by optical density (OD) measurements at 620 nm. PAR0 corresponds to HA films without PAR. 1mg / mL PAR was added to crosslinked HA 2.5%+BDDE 20% films (=post-loaded films). [Figure 4] Figure 2: Fabrication of free-standing HA hydrogels. A schematic procedure for hydrogel disc preparation (A) to obtain HA hydrogel discs of different sizes (B). [Diagram 5]Loading of PAR into HA hydrogel discs. (A) Schematic of PAR-FITC loading. (B) CLSM images of the resulting hydrogel disc (loaded with 0.5 mg / mL PAR30-FITC): 3D reconstruction (left) and transverse section in the Z-axis (right). [Figure 6] Figure 1 shows the results of loading different concentrations of PAR30-FITC into HA hydrogel discs for 3 and 24 h: (A) CLSM images and (B) graph quantifying PAR concentration at the center of the disc. [Figure 7] Figure 1. Loading of PAR-FITC into HA hydrogel discs. CSLM images of HA hydrogel discs loaded with three FITC-labeled PARs at 0.5 mg / mL (left) and graphs showing the resulting fluorescence profiles of the discs (right). [Figure 8] Figure 1. PAR mobility within HA hydrogels. HA disks were loaded with three different FITC-conjugated PARs at 0.5 mg / mL for 24 h and rinsed. FRAP experiments were then performed. (A) Comparison of the fluorescence recovery of the three PARs. (B) Determination of the diffusion coefficient D and fraction p of mobile molecules for the three PARs. [Figure 9] Figure 1 shows the antibacterial activity of PAR10, PAR30 and PAR200 loaded HA hydrogels in replicate incubations, where samples were rinsed and inoculated with fresh bacteria 24 hours after bacterial incubation. [Figure 10] 1 is a graph showing the antibacterial activity of PAR10-loaded HA hydrogels in replicate cultures. After 24 hours of bacterial culture, the samples were rinsed and inoculated with fresh bacteria. The graph shows bacterial growth in the presence of hydrogel discs loaded with different concentrations of PAR10. [Figure 11] 1 is a graph showing the antibacterial activity of PAR30-loaded HA hydrogels in replicate cultures. After 24 hours of bacterial culture, the samples were rinsed and inoculated with fresh bacteria. The graph shows bacterial growth in the presence of hydrogel discs loaded with different concentrations of PAR30. [Figure 12]1 is a graph showing the antibacterial activity of PAR200-loaded HA hydrogels in replicate cultures. After 24 hours of bacterial culture, the samples were rinsed and inoculated with fresh bacteria. The graph shows bacterial growth in the presence of hydrogel discs loaded with different concentrations of PAR200. [Figure 13] Cytotoxicity assay of PAR10-loaded and PAR30-loaded HA hydrogels. (A) After 24 hours, Balb / 3T3 cells show detachment / deformation on the underside of HA+PAR10 and HA+PAR30 disks (loaded at 0.05 mg / mL), while the periphery of the disks remains in good condition. (B) Good cell viability was confirmed by MTT test. (C) According to ISO10993, such reactivity (grade 2) is considered to be a mild reactivity without cytotoxic effect. [Figure 14] Figure 1: Evaluation of cell viability by MTT test. Balb / 3T3 cells were seeded in 24-well plates and placed in contact with HA hydrogel discs loaded or not loaded with PAR for 24 h. HA discs correspond to BDDE-crosslinked HA hydrogel discs without PAR, and HA+PAR corresponds to HA hydrogels loaded with different PAR concentrations (mg / mL). (A) Cell images after 24 h of direct in vitro cytotoxicity test. (B) Graph showing cell viability measured by MTT test. The dashed line corresponds to 70% viability (cytotoxicity limit). [Figure 15] Figure 1 shows the antibacterial activity of HA hydrogels loaded with PAR10, PAR30, and PAR200 in replicate cultures. Samples were inoculated with fresh bacteria every 24 hours of bacterial culture. The graph shows bacterial growth in the presence of hydrogel discs loaded with PAR10, PAR30, and PAR200 (loading concentrations shown). [Figure 16]1 is a graph showing the antibacterial activity of HA hydrogel discs and PAR-loaded hydrogel-coated meshes. The graph shows bacterial growth in the presence of hydrogel discs or hydrogel-coated meshes loaded with 0.05 mg / mL PAR10 or PAR30 (loading concentrations shown in mg / mL). Bacteria were incubated with the materials at 37° C. for 6 days, after which bacterial growth was assessed by measuring optical density. [Figure 17] 1 is a graph showing the antibacterial activity of HA hydrogels after autoclaving. The graph shows bacterial growth in the presence of hydrogel-coated polypropylene (PP) meshes loaded with 0.05 mg / mL and 0.1 mg / mL PAR30 and sterilized by autoclaving, compared to non-autoclaved samples. Bacteria were incubated with the materials for 24 hours at 37° C., after which bacterial growth was assessed by measuring optical density. [Figure 18] Figure 1 shows the antibacterial activity of HA hydrogels crosslinked with different % BDDE. The graph shows bacterial growth in the presence of HA hydrogel disks loaded with 0.05 and 0.1 mg / mL PAR30 and sterilized by autoclaving, compared to non-autoclaved samples. Bacteria were incubated with the materials for 24 hours at 37°C, after which bacterial growth was assessed by measuring optical density. [Figure 19] 1 is a graph showing the antibacterial activity of HA hydrogels loaded with positively charged antibacterial polypeptides. The graph shows bacterial growth in the presence of HA hydrogel disks loaded with 0.05 mg / mL and 0.1 mg / mL of polyarginine PAR30, polyornithine PLO30, and polylysine PLL30. Bacteria were incubated with the materials for 24 hours at 37° C., after which bacterial growth was assessed by measuring the optical density. [Figure 20] Confocal microscopy and percentage of PAR remaining after 72 hours, where HA discs were incubated with 0.5 mg.mL-1 of three different FITC-conjugated PARs for 24 hours. The discs were rinsed and then incubated in NaCl 1M for 72 hours. [Figure 21]Figure 1 shows spectrofluorometric quantification of PAR release after 72 hours in NaCl 1M. The graph represents the average of three independent experiments, and the error bars represent the standard deviation. HA discs were incubated with three different FITC-conjugated PARs at 0.5 mg.mL-1 for 24 hours. Discs were rinsed and then incubated in NaCl 1M for 72 hours. [Figure 22] Confocal microscopy images of disks showing the release of PARs before and after incubation with MH and DMEM, where HA disks were incubated with 0.5 mg.mL-1 of three different FITC-conjugated PARs for 24 h. Disks were rinsed and then incubated with MH or DMEM for 72 h. [Figure 23] Figure 1 shows the percentage of PAR released in MH. 100% represents the fluorescence intensity of the disks in Tris / NaCl. HA disks were incubated with 0.5 mg.mL-1 of three different FITC-conjugated PARs for 24 h. The disks were rinsed and then incubated in MH for 72 h. [Figure 24] Figure 1 shows the percentage of released PARs in DMEM, where 100% represents the fluorescence intensity of the discs in Tris / NaCl. The HA discs were incubated with 0.5 mg.mL-1 of three different FITC-conjugated PARs for 24 h. The discs were rinsed and then incubated in DMEM for 72 h. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hyaluronic Acid Hydrogel As used herein, the term "hydrogel" refers to a chemically crosslinked hydrogel that retains water.
[0017] The hydrogels of the present invention comprise hyaluronic acid (HA) or a derivative thereof.
[0018] As used herein, the term "hyaluronic acid (HA)," also known as hyaluronan, is a linear (unbranched) polysaccharide or non-sulfated glycosaminoglycan composed of repeating disaccharide units of N-acetylglucosamine and glucuronic acid (linked by β1-3 and β1-4 glycosidic bonds).
[0019] HA is usually expressed by the following formula (3):
[0020] [ka]
[0021] (wherein p is an integer between 2 and 25,000). It is of the following.
[0022] Hyaluronic acid (HA) is therefore a negatively charged polymer (also called a polyanion). Negatively charged polymers therefore exist with counterions in the form of salts. In the case of sodium hyaluronate, the counterion is sodium. Hyaluronic acid is degraded by hyaluronidase. The molecular weight (Mw) of hyaluronan represents the average of all molecules in a population and therefore the molecular mass average (molecular weight average). Hyaluronic acid (HA) is available in a wide range of molecular weights.
[0023] Thus, "a type of hyaluronic acid" refers to a particular hyaluronic acid having a particular molecular weight.
[0024] In a particular embodiment, the hyaluronic acid has a molecular weight of between 150 kDa and 3000 kDa, in particular between 160 kDa and 2900 kDa, between 170 kDa and 2800 kDa, between 180 kDa and 2700 kDa, between 190 kDa and 2670 kDa, between 200 kDa and 2600 kDa, between 300 kDa and 2500 kDa, between 400 kDa and 2400 kDa, between 500 kDa and 2300 kDa, between 600 kDa and 2200 kDa, between 700 kDa and 2100 kDa, between 750 kDa and 2000 kDa. a, between 760 kDa and 1900 kDa, between 770 kDa and 1800 kDa, between 780 kDa and 1700 kDa, between 790 kDa and 1600 kDa, between 800 kDa and 1500 kDa, between 805 kDa and 1400 kDa, between 810 kDa and 1300 kDa, between 815 kDa and 1200 kDa, between 820 kDa and 1100 kDa, between 821 kDa and 1000 kDa, between 822 kDa and 900 kDa, between 823 kDa and 850 kDa.
[0025] In one example, the hyaluronic acid has a molecular weight of 150 kDa and is provided in the form of sodium hyaluronate by Lifecore Biomed, USA.
[0026] In a preferred embodiment, the hyaluronic acid is hyaluronic acid having a molecular weight between 800 and 850 kDa.
[0027] In a preferred embodiment, the hyaluronic acid has a molecular weight of 823 kDa (HA 800 is called).
[0028] In another example, hyaluronic acid has a molecular weight of 2670 kDa (HA 2700 is called).
[0029] In certain embodiments, the hydrogel comprises more than one type of hyaluronic acid. Accordingly, in some embodiments, the hyaluronic acid comprises at least two types of hyaluronic acid, one of the at least two types of hyaluronic acid having a molecular weight between 800 and 850 kDa and the other of the at least two types of hyaluronic acid having a molecular weight between 100 and 2000 kDa, in particular a molecular weight of 150 kDa.
[0030] As used herein, the term "derivatives of hyaluronic acid" refers to chemically modified hyaluronic acid. More specifically, derivatives of hyaluronic acid can refer to hyaluronic acid that has been chemically modified to introduce chemical groups or to bind HA to a compound, which preferably allows crosslinking of HA with another compound or another HA compound or its derivative, particularly a compound with an amine group.
[0031] In some embodiments, derivatives of hyaluronic acid include, but are not limited to, HA modified with an aldehyde group (referred to as HA-CHO or HA-Ald), amine-modified hyaluronic acid (referred to as HA-NH2), HA containing a photoreactive vinylbenzyl group (referred to as HA-VB), HA modified with a methacrylate group (referred to as methacrylated HA), HA conjugated to tyramine (referred to as HA-tyramine), and HA conjugated to catechol (referred to as HA-catechol).
[0032] In the hydrogel of the present invention, HA or its derivatives is crosslinked by a crosslinker at the level of its hydroxyl moieties, while the carboxyl moieties of the HA or its derivatives remain free and the HA or its derivatives remain negatively charged.
[0033] By "crosslinking agent" herein is meant an agent that allows the formation of a covalent or ionic bond between two polymers, i.e., two HA molecules.
[0034] In the context of the present invention, the crosslinking agent crosslinks HA at the level of the hydroxyl moieties of HA, while the carboxyl moieties of HA remain free and the HA remains negatively charged.
[0035] By "carboxyl moieties that remain free" is meant herein that the crosslinker does not induce bond formation at the level of the carboxyl moieties of the HA, which therefore remain unmodified compared to the state before crosslinking.
[0036] Examples of crosslinkers targeting hydroxyl groups are well known to those skilled in the art and include butanediol diglycidyl ether (BDDE), divinyl sulfone (DVS), cyanogen bromide, and octenylsuccinic anhydride.
[0037] As one of ordinary skill in the art will appreciate, whether a cross-linking agent induces formation at a particular moiety may depend on the reaction conditions, particularly reactions under acidic or basic conditions.
[0038] "HA remains negatively charged" means herein that the overall charge of the HA after cross-linking is negative. In certain embodiments, all HA molecules remain negatively charged after cross-linking.
[0039] In certain embodiments, the cross-linking agent is butanediol diglycidyl ether (BDDE).
[0040] BDDE crosslinked HA is generally of the following formula (4):
[0041] [ka]
[0042] The hydrogels of the present invention typically have a high level of crosslinking.
[0043] Positively charged antimicrobial peptides The HA hydrogels of the present invention are loaded with at least one positively charged antimicrobial peptide.
[0044] By "loaded" herein is meant that the HA hydrogel is impregnated, contains, and / or bears at least one positively charged antimicrobial peptide without being covalently bound to the hydrogel, and thus the peptide may be released naturally from the hydrogel over time.
[0045] By "antimicrobial peptide" herein is meant a peptide that exhibits antiseptic, antibiotic, antibacterial, antiviral, antifungal, antiprotozoal, and / or antiparasitic activity.
[0046] Preferably, the antimicrobial peptide is an antibacterial peptide.
[0047] As used herein, the term "antimicrobial activity" encompasses bacteriostatic and / or bacteriocidal activity.
[0048] In one embodiment, the antibacterial and / or bacteriostatic activity is directed against at least one species of bacteria.
[0049] As used herein, "bactericidal activity" refers to the killing of bacteria, particularly at least one type of bacteria.
[0050] As used herein, "bacteriostatic activity" herein refers to preventing the growth of bacteria, but not necessarily killing them, in other words, bacteriostatic activity herein refers to inhibiting the growth of bacteria. As a result, bacteriostatic activity can be expressed, for example, as a percentage of inhibition of growth of at least one type of bacteria.
[0051] "Growth inhibition of at least one bacteria" in the context of the present invention may be greater than 70%, e.g., greater than 75%, greater than 80%, typically greater than 82%, 84%, 86%, 88%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%.
[0052] Consequently, in one embodiment, the antimicrobial peptides used in the context of the present invention have greater than 70% growth inhibition of at least one bacterium, more particularly greater than 75%, greater than 80%, typically greater than 82%, 84%, 86%, 88%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% growth inhibition of at least one bacterium.
[0053] "At least one bacterium" herein refers to at least 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or more species of bacteria.
[0054] In one embodiment, the at least one bacterium is an ESKAPE pathogen.
[0055] "ESKAPE pathogens" are a major cause of hospital-acquired infections worldwide and are described, for example, in Biomed Res Int. 2016; 2016:2475067. In one embodiment, the term "ESKAPE pathogen" refers to a bacterium selected from the group consisting of Enterococcus faecium, Staphylococcus aureus, Klebsiella pneumoniae, Acinetobacter baumannii, Pseudomonas aeruginosa, and Enterobacter species.
[0056] In one embodiment, the at least one bacterium is a gram positive or gram negative bacterium, preferably a gram positive bacterium.
[0057] In one embodiment, the Gram-negative bacterium is Pseudomonas aeruginosa, Acinetobacter baumannii, Stenotrophomonas maltophilia, Escherichia coli, Klebsiella pneumoniae, Enterobacter species or Legionella bacterium, preferably Escherichia coli or Pseudomonas aeruginosa.
[0058] In one embodiment, the Gram positive bacteria is a Staphylococcus, Micrococcus, or Enterococcus.
[0059] The bacteria of the genus "Staphylococcus" are stationary, non-spore-forming, catalase-positive, oxidase-negative, gram-positive cocci grouped in grape clusters. Observed in pus furuncles by Pasteur in 1879, staphylococci were named after Ogsten (1881), who isolated them in acute and chronic abscesses. Bacteria of the genus "Staphylococcus", such as Staphylococcus aureus, Staphylococcus epidermidis, Staphylococcus capitis, Staphylococcus caprae, Staphylococcus haemolyticus, Staphylococcus lugdunensis, Staphylococcus schleiferi, Staphylococcus simulans, and Staphylococcus warneri, are major pathogens of foreign body infections, e.g., prosthetic joint infections.
[0060] Accordingly, in one embodiment, the genus Staphylococcus is selected from Staphylococcus aureus, Staphylococcus epidermidis, Staphylococcus capitis, Staphylococcus caprae, Staphylococcus haemolyticus, Staphylococcus lugdunensis, Staphylococcus schleiferi, Staphylococcus simulans and Staphylococcus warneri, preferably Staphylococcus aureus, Staphylococcus epidermidis, and more preferably Staphylococcus aureus.
[0061] Bacteria of the genus "Micrococcus" are generally considered to be saprophytic or commensal organisms, but can become opportunistic pathogens, especially in hosts with a weakened immune system, such as HIV patients. Micrococcus normally resides in the skin microflora, and the genus is rarely associated with disease. However, in rare cases, pulmonary infections caused by Micrococcus have led to death in immunocompromised patients. Micrococcus may be involved in other infections, including recurrent bacteremia, septic shock, septic arthritis, endocarditis, meningitis, and cavitating pneumonia, especially in immunosuppressed patients.
[0062] In one embodiment, the Micrococcus is a Micrococcus luteus (M. luteus) bacterium.
[0063] Bacteria of the genus "Enterococcus" are the cause of serious clinical infections such as urinary tract infections, bacteremia, bacterial endocarditis, diverticulitis, and meningitis.
[0064] In one embodiment, the Enterococcus is a vancomycin-resistant Enterococcus, such as Enterococcus faecalis (E. faecalis) or Enterococcus faecium.
[0065] Bacteriostatic activity or % growth inhibition can be demonstrated, for example, by the antibacterial assays described herein below in the "Methods" section. Strains that can be used in such antibacterial assays can be, for example, Micrococcus luteus or Staphylococcus aureus.
[0066] Antimicrobial peptides as used in the context of the present invention are positively charged peptides.
[0067] By "positively charged" herein is meant that the overall charge of the peptide is positive.
[0068] Positively charged amino acids are well known to those of skill in the art and include lysine, arginine, histidine and ornithine.
[0069] Any positively charged antimicrobial peptide can be used in the context of the present invention.
[0070] In certain embodiments, the positively charged antimicrobial peptide has the following formula (2):
[0071] [ka]
[0072] (In the formula, n is an integer comprised between 2 and 250, in particular between 2 and 200, - R is selected from -NH2, -CH2-NH2 and -NH-C(NH)-NH2. It is a peptide.
[0073] A peptide of formula (2) consists of n repeating units, which may be identical or different. According to the present invention, the repeating units of the peptide of formula (2) have the formula -NH-CH(CH2-CH2CH2-R)-C(=O)-. For a particular repeating unit, R is as defined above and may therefore be different for each unit.
[0074] According to one preferred embodiment, the peptide of formula (2) consists of n repeating units, all R groups being identical.
[0075] According to a further embodiment, the peptide of formula (2) consists of n repeating units, the R groups being optionally different.
[0076] Of the n units, the peptide may contain i units of the formula -NH-CH(CH-CH-CH-NH)-C(=O)-, j units of the formula -NH-CH(CH-CH-CH-CH-NH)-C(=O)-, and k units of the formula -NH-CH(CH-CH-CH-NH-C(NH)-NH)-C(=O)-, where each i, j, and k is comprised between 0 and n, and i+j+k=n, with a random distribution of units or a distribution in blocks.
[0077] In one embodiment, "n" of the n repeating units having formula (2) is an integer comprised between 11 and 200 when R is selected from -NH2, -CH2-NH2, and -NH-C(NH)-NH2.
[0078] In a further embodiment, when R is selected from -NH2, -CH2-NH2 and -NH-C(NH)-NH2, preferably when R is selected from -CH2-NH2 and -NH-C(NH)-NH2, more preferably when R is -NH-C(NH)-NH2, n is an integer comprised between 11 and 99, for example n is an integer comprised between 11 and 95, between 15 and 95, between 15 and 90, between 15 and 85, between 15 and 80, between 15 and 75, between 20 and 95, between 20 and 90, between 20 and 85, between 20 and 80, between 20 and 75, between 25 and 95, between 25 and 90, between 25 and 85, between 25 and 80, between 25 and 75, between 28 and 74, between 28 and 72, between 30 and 70, for example 30, 50 and 70.
[0079] In a further embodiment, when R is selected from -NH2, -CH2-NH2 and -NH-C(NH)-NH2, preferably when R is selected from -CH2-NH2 and -NH-C(NH)-NH2, more preferably when R is -NH-C(NH)-NH2, n is an integer comprised between 11 and 49, for example n is an integer comprised between 11 and 45, between 15 and 45, between 20 and 40, between 21 and 39, between 22 and 38, between 23 and 37, between 24 and 36, between 25 and 35, between 26 and 34, between 27 and 33, between 28 and 32, between 29 and 31.
[0080] In one particular embodiment, when R is selected from -NH2, -CH2-NH2 and -NH-C(NH)-NH2, preferably when R is selected from CH2-NH2 and -NH-C(NH)-NH2, more preferably when R is -NH-C(NH)-NH2, n is an integer selected from the group consisting of 11, 15, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 45, 47, 50, 52, 54, 56, 58, 60, 62, 64, 66, 68, 70, 72, 74, 76, 78, 80, 82, 84, 86, 88, 90, 92, 94, 96, 98, preferably n is 30, 50 or 70.
[0081] In one particular embodiment, when R is selected from -NH2, -CH2-NH2 and -NH-C(NH)-NH2, preferably when R is selected from -CH2-NH2 and -NH-C(NH)-NH2, more preferably when R is -NH-C(NH)-NH2, n is an integer selected from the group consisting of 11, 15, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 45 and 49, preferably n is 30.
[0082] The "repeating unit" of formula (2), sometimes also referred to as "structural unit", refers herein to an amino acid or amino acid residue, where the amino acid is ornithine when R is -NH2, lysine when R is -CH2-NH2, or arginine when R is -HC(NH)-NH2. Thus, the "n repeating units of formula (2)" may also be referred to as "n amino acid residues of formula (2)", or more precisely, n ornithine residues when R is -NH2, n lysine residues when R is -CH2-NH2, or n arginine residues when R is -HC(NH)-NH2.
[0083] According to the above, in some embodiments, "n repeat units having formula (2)" may be referred to as "polyornithine having n ornithine residues" when R is -NH2, as "polylysine having n lysine residues" when R is -CH2-NH2, or as "polyarginine having n arginine residues" when R is -HC(NH)-NH2.
[0084] "Ornithine" is a non-proteinogenic amino acid that plays a role in the urea cycle. Polyornithine refers to a polymer whose structural unit is ornithine. Polyornithine refers to poly-L-, poly-D-, or poly-LD-ornithine. In the context of the present invention, polyornithine refers in particular to poly-L-ornithine (PLO).
[0085] "Arginine" and "lysine" are α-amino acids used in protein biosynthesis. Polyarginine and polylysine refer to polymers whose structural unit is arginine or lysine, respectively. Polyarginine or polylysine refers to poly-L-, poly-D- or poly-LD-arginine or -lysine. In the context of the present invention, polyarginine or polylysine refers in particular to poly-L-arginine (PAR) and poly-L-lysine (PLL), respectively.
[0086] In certain embodiments, the positively charged antimicrobial peptide is selected from the group consisting of polyarginine, polyornithine, and polylysine.
[0087] "Poly-L-ornithine", "poly-L-lysine" and "poly-L-arginine" are positively charged synthetic polymers that are produced in the form of a salt with a counterion, which can be selected from, but is not limited to, hydrochloride, hydrobromide, or trifluoroacetate.
[0088] In one example, the polyarginine is poly-L-arginine hydrochloride, CAS#26982-20-7.
[0089] In one example, the polyornithine is poly-L-ornithine hydrobromide with CAS#27378-49-0 or poly-L-ornithine hydrochloride with CAS#26982-21-8.
[0090] In one example, the polylysine is poly-L-lysine trifluoroacetate, poly-L-lysine hydrobromide with CAS#25988-63-0, or poly-L-lysine hydrochloride with CAS#26124-78-7.
[0091] Poly-L-ornithine, poly-L-lysine and poly-L-arginine with defined numbers of amino acid residues are commercially available, for example through Alamanda Polymers, USA.
[0092] In one example, poly-L-arginines (PAR), such as PAR10 (10 Arginines (R), Mw=2.1 kDa, PDI=1); PAR30 (30R, Mw=6.4 kDa, PDI=1.01); PAR50 (50 Arginines (R), Mw=9.6 kDa, PDI=1.03); PAR70 (70 Arginines (R), Mw=13.4 kDa, PDI=1.01), PAR100 (100R, Mw=20.6 kDa, PDI=1.05), and PAR200 (200R, Mw=40.8 kDa, PDI=1.06), were purchased from Alamanda Polymers, USA.
[0093] In another example, poly-L-ornithine (PLO), such as PLO30 (30R, Mw=5.9 kDa, PDI=1.03), PLO100 (100R, Mw=18.5 kDa, PDI=1.03), and PLO250 (250R, Mw=44.7 kDa, PDI=1.02), was purchased from Alamanda Polymers, USA.
[0094] In a further example, poly-L-lysine (PLL), such as PLL10 (10R, Mw=1.6 kDa), PLL30 (30R, Mw=5.4 kDa, PDI=1.02), PLL100 (100R, Mw=17.3 kDa, PDI=1.07), and PLL250 (250R, Mw=39.5 kDa, PDI=1.08), were purchased from Alamanda Polymers, USA.
[0095] Methods for obtaining polypeptides with n repeating units, such as polyarginine, polylysine, or polyornithine with n=30, are known to those skilled in the art and include ring-opening polymerization of α-amino acid N-carboxyanhydrides (NCAs) followed by purification. Usually, the polypeptides are purified after polymerization by precipitation in water or, for example, in an organic non-solvent, and after deprotection of the amino acid side chains, by dialysis. All water-soluble polymers are finally lyophilized.
[0096] In a particularly preferred embodiment, the positively charged antimicrobial peptide is polyarginine.
[0097] In a more particularly preferred embodiment, the polyarginine has the following formula (1):
[0098] [ka]
[0099] (wherein n is an integer between 2 and 100). It is of the following.
[0100] In a further embodiment, in formula (1), n is an integer comprised between 11 and 99, for example, n is an integer comprised between 11 and 95, between 15 and 95, between 15 and 90, between 15 and 85, between 15 and 80, between 15 and 75, between 20 and 95, between 20 and 90, between 20 and 85, between 20 and 80, between 20 and 75, between 25 and 95, between 25 and 90, between 25 and 85, between 25 and 80, between 25 and 75, between 28 and 74, between 28 and 72, between 30 and 70, for example 30, 50 and 70.
[0101] In further embodiments, n in formula (1) is an integer comprised between 11 and 49, for example, n is an integer comprised between 11 and 45, between 15 and 45, between 20 and 40, between 21 and 39, between 22 and 38, between 23 and 37, between 24 and 36, between 25 and 35, between 26 and 34, between 27 and 33, between 28 and 32, between 29 and 31.
[0102] In one particular embodiment, n in formula (1) is an integer selected from the group consisting of 11, 15, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 45, 47, 50, 52, 54, 56, 58, 60, 62, 64, 66, 68, 70, 72, 74, 76, 78, 80, 82, 84, 86, 88, 90, 92, 94, 96, 98; preferably, n is 30, 50 or 70.
[0103] In one particular embodiment, n in formula (1) is an integer selected from the group consisting of 11, 15, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 45 and 49, preferably, n is 30.
[0104] In a particularly preferred embodiment, the polyarginine has the following formula (1):
[0105] [ka]
[0106] (wherein n is 30) It is of the following.
[0107] In a particular embodiment, the hydrogel is loaded with a positively charged antimicrobial peptide of formula (2) as defined above, where n is n1, an integer comprised between 2 and 100, and at least one positively charged antimicrobial peptide of formula (2) as defined above, where n is n2, an integer comprised between 2 and 100, but different from n1.
[0108] In other words, in certain embodiments, the hydrogel is loaded with at least two positively charged antimicrobial peptides of formula (2), the peptides differing in size.
[0109] In certain embodiments, the hydrogel comprises a compound having the following formula (1):
[0110] [ka]
[0111] (wherein n is n1 and is an integer comprised between 2 and 250, in particular between 2 and 200). and the following formula (1)
[0112] [ka]
[0113] where n is n2, an integer comprised between 2 and 250, in particular between 2 and 200, and n2 is different from n1. It is filled with polyarginine.
[0114] In a more particular embodiment, the hydrogel is loaded with polyarginines of formula (1) of different sizes.
[0115] In another embodiment, the antimicrobial peptide is selected from catestatin, cateslitin, polyornithine, polylysine and their D or L isomers, nisin, defensin, melittin and magainin.
[0116] In a particular embodiment, the hydrogels of the invention are loaded with different positively charged antimicrobial peptides, as defined above, for example as a mixture of PAR10 and PAR200 or a mixture of PAR30 and PAR200.
[0117] Additional Compounds The hydrogels of the present invention may further comprise additional compounds, in particular, the hydrogels of the present invention may further comprise a pharma- ceutical active agent.
[0118] In the context of the present invention, the term "pharmaceutical active drug" refers to a compound or entity that alters, inhibits, activates, or otherwise affects biological events. This includes, but is not limited to, for example, anticancer substances, anti-inflammatory agents, immunosuppressants, modulators of cell-extracellular matrix interactions, including cell growth inhibitors, anticoagulants, antithrombotic agents, enzyme inhibitors, analgesics, antiproliferative agents, antifungal agents, cytostatic agents, growth factors, hormones, steroids, nonsteroidal substances, and antihistamines. Examples of symptom groups are, but are not limited to, analgesics, antiproliferative agents, antithrombotic agents, anti-inflammatory agents, antifungal agents, antibiotics, cytostatic agents, immunosuppressants, and growth factors, hormones, glucocorticoids, steroids, nonsteroidal substances, genetically or metabolically active agents for silencing and transfection, antibodies, peptides, receptors, ligands, and any pharmaceutically acceptable derivatives thereof. Specific examples from the above group are paclitaxel, estradiol, sirolimus, erythromycin, clarithromycin, doxorubicin, irinotecan, gentamicin, dicloxacillin, quinine, morphine, heparin, naproxen, prednisone, dexamethasone, cytokines, IL-4, IL-10, VEGF, fungizone, catestatin or cateslitin.
[0119] Method of preparation The present invention also relates to a method for preparing a hydrogel as defined above, comprising the steps of: (a) mixing, under basic conditions, hyaluronic acid (HA) or a derivative thereof, as defined above in the section "Hyaluronic acid hydrogel", with a crosslinker, as defined above in the section "Hyaluronic acid hydrogel", which crosslinks HA at the level of its hydroxyl moieties, while leaving the carboxyl moieties of HA or its derivative free and leaving HA or its derivative negatively charged; (b) depositing the mixture on a support and incubating it at room temperature for 48 to 72 hours to obtain a hydrogel; (c) recovering the hydrogel formed in step (b); (d) incubating the hydrogel in an aqueous buffer under conditions that allow for removal of crosslinker residues and swelling of the hydrogel; (e) loading the hydrogel obtained in step (d) with at least one positively charged antimicrobial peptide, as defined above in the "Positively charged antimicrobial peptide" section; (f) recovering the loaded hydrogel obtained in step (e); The present invention relates to a method comprising the steps of:
[0120] Mixing process (a) The mixing step (a) of the method of the present invention consists of mixing, under basic conditions, hyaluronic acid (HA) or a derivative thereof, as defined above in the section "Hyaluronic acid hydrogel", with a crosslinking agent, as defined above in the section "Hyaluronic acid hydrogel", which crosslinks HA at the level of its hydroxyl moieties, while leaving the carboxyl moieties of HA or its derivative free and leaving HA or its derivative negatively charged.
[0121] In a particular embodiment, the HA is hyaluronic acid having a molecular weight between 800 kDa and 850 kDa, in particular having a molecular weight of 823 kDa.
[0122] In a particular embodiment, the mixture of step (a) comprises between 1% (w / v) and 10% (w / v) of HA or a derivative thereof as defined above, more preferably between 2% (w / v) and 3% (w / v) of HA or a derivative thereof as defined above, and most preferably 2.5% (w / v) of HA or a derivative thereof as defined above.
[0123] In certain embodiments, the cross-linking agent is butanediol diglycidyl ether (BDDE).
[0124] In a particular embodiment, the mixture of step (a) comprises at least 10% (v / v) of a crosslinker as defined above, in particular BDDE, more preferably at least 20% (v / v) of a crosslinker, in particular BDDE. In a particular embodiment, the mixture of step (a) comprises between 10% (v / v) and 30% (v / v) of a crosslinker as defined above, in particular BDDE.
[0125] In a particular embodiment, the mixture of step (a) comprises 2% (w / v) to 3% (w / v) of HA or a derivative thereof and at least 10% (v / v) of a cross-linking agent, in particular BDDE, in particular at least 20% (v / v) of a cross-linking agent, in particular BDDE.
[0126] By "basic conditions" herein is meant reaction conditions with a pH greater than 7. Typically, the HA and crosslinker are mixed in a NaOH solution, particularly a 0.1 M to 0.3 M NaOH solution, more particularly a 0.25 M NaOH solution.
[0127] Deposition process (b) The deposition step (b) of the method of the invention consists in depositing the mixture obtained in step (a) on a support and incubating it at room temperature for 48 to 72 hours to obtain a hydrogel as defined above.
[0128] Any suitable support may be used, such as a petri dish, a glass slide, a well plate, parafilm, a medical compress, a mesh, or a medical prosthesis (polymeric, metal).
[0129] The support may be any suitable material such as polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE), polypropylene, acrylonitrile butadiene styrene (ABS), glass, Teflon, or metal, etc. In certain embodiments, the support is a material capable of maintaining a high pH.
[0130] The support can be pretreated before deposition of the mixture, for example it can be cleaned with, for example, a Hellmanex® (anionic detergent) solution and / or an HCl solution and / or a 70% alcohol solution and / or acetone and / or treated, for example by deposition of polyethyleneimine (PEI), to improve adhesion.
[0131] The mixture can be deposited on the support by any technique well known to those skilled in the art, such as drop deposition, pouring, pipetting, extrusion, spin coating, dipping, or 3D printing.
[0132] The mixture once deposited on the support is incubated at room temperature for a period ranging from 48 to 72 hours, preferably 72 hours, to obtain a hydrogel as defined above.
[0133] Recovery process (c) The hydrogel formed in step (b) is then recovered.
[0134] The recovery step (c) can be implemented by any technique well known to the person skilled in the art, for example by cutting the pieces of hydrogel, usually using a circle cutter, a scalpel, a precision cutting tool (physical or laser based) and a specific press cutter depending on the size required.
[0135] Incubation step (d) The incubation step (d) of the method of the present invention consists of incubating the hydrogel in an aqueous buffer under conditions that allow for the removal of crosslinker residues and for swelling of the hydrogel.
[0136] By "aqueous buffer" herein is meant an aqueous solution consisting of a mixture of a weak acid and its conjugate base, or vice versa. Examples of aqueous buffers include Tris / NaCl buffer (e.g., Tris 10 mM, NaCl 0.15 M, pH 7.4 buffer), PBS, or HEPES.
[0137] As used herein, aqueous buffers further include solutions comprised of water, such as distilled water.
[0138] "Removal of crosslinker residues" herein means that crosslinker molecules not involved in bonding are excluded from the hydrogel, such that preferably there are 0.01% or less free crosslinker molecules in the hydrogel after the incubation step.
[0139] By "swelling of the hydrogel" herein is meant that the hydrogel takes up water from the aqueous buffer in which it is incubated, preferably to a level such that the size of the hydrogel increases by at least 1.5-fold.
[0140] The incubation step is usually carried out for 1-5 min to 1 h. The incubation step may in particular comprise several incubations in different or the same buffer, usually a first incubation for 1-5 min and a second incubation for 1 h.
[0141] The hydrogel can typically be stored at 4° C. after the incubation step and before carrying out the filling step.
[0142] Filling process (e) The loading step (e) of the method of the invention consists in loading at least one positively charged antimicrobial peptide, as defined above in the section "Positively charged antimicrobial peptides", into the hydrogel obtained in step (d).
[0143] In a particular embodiment, the positively charged antimicrobial peptide is a polyarginine, in particular PAR30, as defined above in the "Positively charged antimicrobial peptides" section.
[0144] In a particular embodiment, the positively charged antimicrobial peptide is loaded in step (e) at a concentration of 0.05 mg / ml to 5 mg / ml, more particularly 0.05 mg / ml to 1 mg / ml.
[0145] The loading is preferably carried out at room temperature.
[0146] Loading of the positively charged antimicrobial peptide may be carried out for a period of 2 hours to 48 hours, in particular 3 hours to 24 hours, preferably 24 hours.
[0147] The loading step (e) can be followed by a washing step (e') in which the loaded hydrogel is washed with an aqueous buffer as defined above, in particular a Tris / NaCl buffer.
[0148] The filled hydrogel prepared by the method of the present invention may further comprise additional compounds as defined in the "Additional Compounds" section above. Such additional compounds can be added during the formation of the hydrogel or during the filling of the hydrogel. In particular, the additional compounds can be mixed with the HA before the addition of the crosslinker, mixed with the mixture of HA and crosslinker, or loaded after the crosslinking reaction, and can be loaded before or after loading the antimicrobial peptide.
[0149] The present invention further relates to a hydrogel possibly obtainable by the method of preparation defined above.
[0150] As will be clearly evident to one skilled in the art from the above disclosed methods of preparation, the hydrogels likely to be obtainable by the above defined methods of preparation have a high crosslinking level.
[0151] Medical Devices The present invention further relates to a medical device comprising a hydrogel as defined above.
[0152] By "medical device" herein is meant items such as catheters, stents, endotracheal tubes, hypotubes, filters such as for embolic protection, surgical instruments, and the like. Any device that is typically coated in the medical field can be used in the present invention. Furthermore, within the scope of the present invention, the term refers to any material, natural or artificial, that is inserted into a mammal. Specific medical devices that are particularly suitable for application of the hydrogels of the present invention include, but are not limited to, peripherally insertable central venous catheters, dialysis catheters, long-term tunneled central venous catheters, long-term non-tunneled central venous catheters, peripheral venous catheters, short-term central venous catheters, arterial catheters, pulmonary artery Swan-Ganz catheters, urinary catheters, artificial urinary sphincters, long-term urinary devices, urinary dilators, urinary stents, other urinary instruments, tissue-bound urinary devices, penile prostheses, vascular grafts, vascular catheter ports, vascular dilators, extravascular dilators, vascular stents, extravascular stents, wound drain tubes, hydrocephalus shunts, ventricular catheters, peritoneal catheters, pacemaker systems, miniature or temporary joint replacements, heart valves, cardiac assist devices, and the like, as well as artificial bones, artificial joints, and dental prostheses.
[0153] As used herein, the term "medical device" further encompasses wound dressings and mesh prostheses.
[0154] The term "wound dressing" refers to any pharma- ceutically acceptable wound dressing, such as: a) Films, including semipermeable or semiocclusive materials such as polyurethane copolymers, acrylamides, acrylates, paraffins, polysaccharides, cellophane, and lanolin. b) Hydrocolloids including carboxymethylcellulose, the protein component of gelatin, pectin, and complex polysaccharides including gum acacia, gum guar, and gum karaya, which are available in the form of flexible foams, which can alternatively be formulated with polyurethanes or, further alternatively, with adhesives such as polyisobutylene. c) Impregnated materials including pine mesh gauze, paraffin and lanolin coated gauze, polyethylene glycol coated gauze, knitted viscose, rayon, and polyester. d) Cellulose-like polysaccharides such as alginates, including calcium alginate, which may be formulated as fibrous nonwoven composites or spun into woven composites.
[0155] In certain embodiments, the wound dressing comprises a nonwoven or knitted fabric as a carrier material, the knitted or nonwoven fabric being made from natural or synthetic fibers.
[0156] "Mesh prosthesis" as used herein means a loosely woven sheet used as a permanent or temporary support for organs and other tissues during surgery. Mesh prostheses may typically be polypropylene mesh, polyethylene terephthalate mesh, polytetrafluoroethylene mesh, or polyvinylidene fluoride mesh.
[0157] In certain embodiments, the medical device is a wound dressing or a mesh prosthesis.
[0158] In certain embodiments, medical devices are coated and / or impregnated with the hydrogels of the present invention.
[0159] In particular, when the medical device is a wound dressing, the carrier material of the wound dressing is preferably coated or impregnated on one or more sides with a hydrogel.
[0160] The hydrogel may be applied to and / or included in the medical device by any method well known to those of skill in the art.
[0161] Typically, the hydrogel may be applied to and / or included in the medical device by dropwise deposition of a mixture of non-crosslinked HA and a crosslinker onto a material, or by immersing an absorbent material in a mixture of non-crosslinked HA and a crosslinker, or by coating the hydrogel with a dedicated instrument or by extrusion printing.
[0162] In a particular embodiment of the present invention, it is also indicated that the hydrogel according to the present invention is disposed in a container. It is particularly indicated that the hydrogel is packaged as sterile. In such a case, containers such as screw cap containers, resealable tubes, or consumable containers, such as tubes with safety caps, can be used. However, it may also be indicated that the hydrogel is disposed in a syringe used as original packaging. It is particularly indicated that the hydrogel in the syringe is sterile. In a particularly preferred embodiment, the hydrogel is included in a sterile original packaging as a ready-to-use kit, and is available together with a drug carrier or coating material, and optionally further medical aid. It may also be indicated that both the hydrogel and the drug carrier or coating material of the original packaging are available in the sterile original packaging of the kit package.
[0163] Any combination of the above embodiments is part of the present invention.
[0164] Throughout this application, the term "comprising" should be interpreted as embracing all specifically mentioned features as well as any additional, unspecified features. As used herein, use of the term "comprising" also discloses embodiments in which no features other than those specifically mentioned are present (i.e., "consisting of"). Moreover, the indefinite articles "a" or "an" do not exclude a plurality. The mere fact that certain measures are recited in mutually different dependent claims does not indicate that a combination of these measures cannot be used to advantage.
[0165] The present invention will now be described in more detail with reference to the following examples. All literature and patent documents cited in this specification are incorporated herein by reference. Although the present invention has been described and illustrated in detail in the preceding description, the examples should be considered as illustrative or exemplary, and not restrictive. EXAMPLES
[0166] Example 1 HA crosslinking and hydrogel deposition As a first step in the development of HA hydrogels, we evaluated several substrates and deposition techniques. The goal was to obtain a homogenous HA layer with a thickness of 10-100 μm.
[0167] To crosslink the films, we chose butanediol diglycidyl ether (BDDE), which is used in most of the market-leading HA hydrogels.
[0168] HA crosslinking with BDDE Preliminary experiments were performed by mixing 5% (v / v) and 10% (v / v) BDDE in a glass vial and crosslinking 2.5% (w / v) of 823 kDa HA dissolved in 0.1 M NaOH by stirring overnight. The reaction was carried out for 48 hours until no increase in solution viscosity was observed. The HA solution was observed before and after crosslinking.
[0169] Prior to crosslinking, all three solutions were liquid. After 24 hours, gelation of the HA solution with 10% BDDE was observed, and after 48 hours, both the 5% and 10% BDDE-containing solutions were crosslinked, while the HA without BDDE remained liquid.
[0170] HA hydrogels fabricated by droplet deposition, HA premixed with BDDE We chose HA 823 kDa, which appears to absorb more PAR30-rhodamine than other HAs.
[0171] We tested a method that consisted of dissolving 5% HA 823 kDa in NaOH 0.25 M and premixing it with BDDE 10% or 20%.
[0172] Deposition was examined on glass slides with a diameter of 12 mm.
[0173] The slides were first washed with a Hellmanex 2% solution, then with HCl 1M (both steps were followed by rinsing with demineralized water), then rinsed with ethanol 70% and dried. To improve HA adhesion, a layer of polyethyleneimine (PEI) was deposited on the slides by immersing them in a 0.5mg / ml PEI solution in water for 30 minutes.
[0174] The mixture was deposited on a prepared glass slide and the plate containing the slide was sealed to prevent the film from drying out (Figure 1). The cross-linking reaction was carried out for 48 h.
[0175] Dissolving HA in NaOH allows the HA concentration to be increased up to 5% without the solution becoming too viscous. Premixing BDDE with HA allows the use of less crosslinker.
[0176] Deposition of 25 μL of HA 5% BDDE 10% resulted in a homogenous layer with a thickness of approximately 800 μm. When 10 μL of HA 5%-BDDE 10% was deposited and spread on a slide, the film thickness decreased to approximately 250 μm. Finally, deposition of 5 μL of HA 5% BDDE 20% between two glass slides resulted in a film thickness of 50 μm.
[0177] Thus, deposition of HA premixed with BDDE can result in films of different thicknesses depending on the volume deposited and the deposition method.
[0178] Finally, we opted for HA 2.5% + 20% BDDE (premixed), depositing 10 μL between parafilm and a glass slide (Figure 2), which resulted in a homogenous film of approximately 100 μm.
[0179] PAR pre-fill vs post-fill Next, we tested the PAR-charged HA hydrogels for antibacterial activity. We evaluated them after loading with PAR (adding a 1 mg / mL solution of PAR onto the crosslinked HA film). The loaded PARs were of four different lengths: 10, 30, 150 and 200 residues. These are further referred to as PAR10, PAR30, PAR150 and PAR200. We also investigated the release of PAR from the loaded films after 24 hours.
[0180] Antibacterial activity was tested using cultures of Staphylococcus aureus (400 μL of bacterial suspension with initial optical density OD = 0.001 per well of a 24-well plate with or without HA, PAR-charged or non-charged slides). After 24 h, the OD at 620 nm was measured and bacterial viability on the surface was assessed using the BacLight Redox Sensor CTC Vitality Kit (Molecular Probes) as a fluorescent marker.
[0181] The results showed inhibition of bacterial growth on the films after loading with PAR (all lengths).
[0182] The inventors have determined that post-loading of the PAR is the most efficient method.
[0183] Example 2 Fabrication and characterization of free-standing HA hydrogels First, we established a procedure to fabricate thin hydrogel films by mixing 2.5% (w / v) 823 kDa HA and 20% (v / v) 1,4-butanediol diglycidyl ether (BDDE) in 0.25 M NaOH and depositing the solution between parafilm and a 12 mm diameter glass slide.
[0184] This technique yielded thin films of approximately 100 μm, but required the use of parafilm, which is temperature sensitive and may affect hydrogel formation.To circumvent the lack of reproducibility, we developed a new technique that allows us to fabricate free-standing hydrogels of different sizes that are resistant and easy to manipulate.
[0185] Construction of free-standing HA hydrogels To prepare such hydrogels, 1.5 mL of a well-mixed solution containing 2.5% HA and 20% BDDE in NaOH 0.25 M was poured into a 35 mm diameter Petri dish and allowed to crosslink for 72 h at room temperature.
[0186] The hydrogels were further cut into disks of required size using a circle cutter, for example, for experiments in 24-well plates, disks of 4 mm diameter were used.
[0187] The hydrogel discs were further rinsed with Tris 10 mM / NaCl 0.15 M buffer (pH=7.4) and could be stored at 4° C. for several weeks.
[0188] The schematic procedure for hydrogel disc preparation and the resulting discs of different sizes are shown in Figure 4. The resulting hydrogels can be easily manipulated with pliers or a spatula.
[0189] Example 3 PAR loading and emission characterization Loading of PAR into HA hydrogel discs To load the hydrogels with PAR, the disks were immersed in the PAR solution and incubated at room temperature. For 4 mm disks in a 24-well plate, 0.5 mL of PAR solution was used. The disks were then rinsed twice with Tris / NaCl buffer: one short rinse and one longer rinse (at least 1 h).
[0190] An example of the procedure and the resulting PAR30-FITC (PAR with 30 arginine residues and conjugated to FITC) loaded disks is shown in FIG.
[0191] We compared 3-hour vs. 24-hour loading of PAR30. The results showed that after 24 hours, PAR30 was more diffused to the center of the disk (FIG. 6). Therefore, 24-hour loading was selected for further experiments.
[0192] Next, we studied the packing of three different PARs, namely PAR10, corresponding to chains with 10 arginine residues, PAR30, corresponding to chains with 30 arginine residues, and PAR200, corresponding to chains with 200 arginine residues.
[0193] To visualize the loading and diffusion of PARs within the hydrogels, we again used fluorescently labeled PARs (PAR10-FITC, PAR30-FITC, PAR200-FITC).
[0194] The fluorescence profiles showed a more uniform distribution for PAR10 and PAR30 (Figure 7).
[0195] Next, we used the FRAP (fluorescence recovery after photobleaching) technique to study PAR mobility within the hydrogel (Figure 8). Qualitatively, PAR10 was the most mobile and PAR200 was the least mobile (Figure 8A). Quantitative parameters such as the diffusion coefficient were also determined (Figure 8B).
[0196] Stability of PAR-loaded hydrogels in Tris / NaCl buffer HA disks loaded with three different PARs (PAR10, corresponding to chains with 10 arginine residues, PAR30, corresponding to chains with 30 arginine residues, and PAR200, corresponding to chains with 200 arginine residues) were incubated for 48 h at room temperature or at 37°C. The results showed that there was no release of PAR-FITC under any condition, suggesting that the antimicrobial HA-PAR disks are stable in Tris / NaCl buffer even at high temperatures and are suitable for disk manipulation and transportation.
[0197] More specifically, the total amount of PAR contained in the hydrogel was estimated by incubation of hydrogels loaded with fluorescently labeled PAR in concentrated NaCl to promote PAR release. According to confocal microscopy images (Figure 20), after 72 h at 37 °C in NaCl 1M, the release of PAR10 was nearly complete, while the release of PAR30 and PAR200 was close to 80%. The percentage of PAR remaining in the hydrogel discs after 72 h of incubation was measured by image processing. 100% corresponds to the fluorescence intensity before release. The percentage of PAR remaining after NaCl 1M incubation was then measured to determine the value of released PAR. It was about 97%, 78%, and 78% for PAR10, PAR30, and PAR200, respectively. The incomplete release of PAR30 and PAR200 correlates with the low mobility shown by the FRAP experiments. The amount of released PAR-FITC was then quantified by measuring the fluorescence intensity of the supernatant by spectrofluorimetry and referencing a calibration curve.
[0198] As a result, 0.5 mg.mL -1 Disks incubated with PAR solution released approximately 212 μg PAR10-FITC, 157 μg PAR30-FITC, and 91 μg PAR200-FITC after 72 hours in NaCl 1M (FIG. 21). When the released amounts were normalized to 100%, 218 μg, 201 μg, and 117 μg of PAR10-FITC, PAR30-FITC, and PAR200-FITC were loaded, respectively. Since the volume of the disks was approximately 30 μL, the disks contained approximately 7.3 mg.mL of each.-1 PAR10, 6.7 mg.mL -1 of PAR30, and 3.9 mg.mL -1 It includes PAR200.
[0199] Release of PARs in bacterial and cell culture media Using 10 units, 30 units and 200 units of FITC-labeled PAR, we assessed its release from HA hydrogels at 37° C. in two different media.
[0200] We performed disk imaging after 24 h of incubation at 37°C in MH (Mueller-Hinton medium, bacterial culture medium) and DMEM (Dulbecco's modified Eagle medium + 10% FBS + antibiotics, cell culture medium). The results showed that the PAR release patterns were slightly different between MH and DMEM / FBS. In the latter, the release of PAR30 and PAR200 was higher than in MH.
[0201] More specifically, PAR release from hydrogels was examined in microbiological growth medium (MH) or cell culture medium (DMEM) for 72 hours. PAR-FITC-loaded hydrogels were placed in these media and incubated at 37°C, and PAR release was observed by confocal microscopy (Figure 22). PAR10 release in MH was faster compared to PAR30 and PAR200, which were released more slowly (Figure 23). In DMEM, all three PARs had almost similar release profiles and were completely released after 48 hours (Figure 24).
[0202] Example 4 Antibacterial efficacy versus in vitro cytotoxicity In preliminary experiments, we demonstrated the antibacterial activity of PAR10, PAR30 and PAR200 loaded into HA hydrogels at 1 mg / mL.
[0203] To study the antibacterial properties of PAR-loaded hydrogels in more detail, we performed replicate bacterial cultures (Figure 9) using hydrogel discs loaded with different concentrations of PAR10, PAR30, and PAR200.
[0204] PAR30 showed the longest antibacterial effect, remaining effective at 0.5 and 1 mg / mL (loading) even after repeated incubation for 8 days. PAR10 was effective for 8 days at 1 mg / mL, and PAR200 was effective for 7 days at 1 mg / mL (Figures 10-12).
[0205] Cytotoxicity Testing Direct in vitro cytotoxicity testing consists of putting the material in contact with cells for 24 hours and performing an MTT test to evaluate cell viability. According to ISO10993, the tested material should cover approximately 1 / 10 of the cell layer surface. This corresponds to approximately 5 mm of hydrogel discs per well of a 24-well plate.
[0206] We used 4 mm diameter disks that swelled to approximately 6 mm in diameter when placed in Tris-NaCl buffer.
[0207] After 24 h at 37 °C, the hydrogel discs were removed to perform the MTT test to measure cell metabolic activity, which often serves to estimate cell viability. The yellow, water-soluble MTT (3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide) is metabolically reduced in viable cells to a blue-purple insoluble formazan. The number of viable cells correlates with the intensity of the color, determined by photometry after dissolving the formazan in alcohol (from ISO 10993).
[0208] Therefore, disks, loaded with or without PAR, were sterilized and placed on top of a ∼80% confluent layer of Balb / 3T3 cells. For the MTT assay, cells were incubated for 2 h with cell culture medium containing 0.2 mg / mL MTT. The medium was then removed and the formazan was dissolved in DMSO. The absorbance of the resulting solution was measured at 570 nm using a spectrophotometer, and images were taken around and under the disk to assess cell morphology.
[0209] In the first experiment, hydrogels loaded with 0.05 mg / mL PAR10 and PAR30 (the lowest loading concentration showing antibacterial effect) appeared to be non-cytotoxic by ISO10993 criteria based on the quantitative MTT test results (good viability) and the qualitative reactivity gradation (reactivity limited to the lower region of the specimen) (Figure 13).
[0210] We confirmed these results and, in addition, performed cytotoxicity assays on hydrogels loaded with PAR10 and PAR30 0.1 mg / mL, which also appeared to be non-cytotoxic (Figure 14). As before, the reactive area was limited to the underside of the disc (data not shown) and cell viability was good (Figure 20B). However, the hydrogel loaded with PAR200 was classified as cytotoxic.
[0211] Remarkably, hydrogels loaded with 0.1 mg / mL PAR10 and PAR30 showed antibacterial efficacy for 2 and 4 days in repeated incubations (= fresh bacteria added daily), and in additional studies (Figure 15), these values were even higher (3 and 5 days).
[0212] Example 5 Deposition of HA hydrogel onto mesh materials In addition to establishing a procedure for fabricating free-standing hydrogel discs, the inventors attempted to deposit the hydrogel onto two materials used in clinical applications: a highly absorbent nonwoven fabric used for wound disinfection (Medicomp®) and a polypropylene mesh for hernia repair.
[0213] The HA-BDDE solution (50 μL or 100 μL) was deposited on 12 mm diameter pieces of fabric or mesh and allowed to crosslink. Medicomp® absorbed and retained 100 μL of hydrogel solution, while a volume of 50 μL was more suitable for the non-absorbent polypropylene mesh. However, both materials were able to retain the hydrogel after crosslinking and were easy to manipulate.
[0214] Confocal images were obtained of HA hydrogels loaded with PAR30-rhodamine deposited on Medicomp® fabric and polypropylene mesh. In these images, the fibers of the fabric or mesh are surrounded by the PAR30-rhodamine-labeled hydrogel. Some PAR30-rhodamine is also absorbed into the fibers.
[0215] With regard to antibacterial activity, hydrogel-covered mesh materials were compared to hydrogel discs and showed similar bacterial growth inhibition at low concentrations (Figure 16) for 6 days.
[0216] Example 6 Storage and sterilization The hydrogels (free-standing and deposited on mesh materials) can be kept at 4° C. for several days, dried, frozen, and sterilized by autoclaving (FIG. 17) without loss of antimicrobial activity.
[0217] Example 7 Crosslinking rate Low and high cross-linked (10% and 30% BDDE v / v) hydrogels loaded with PAR30 showed similar antibacterial activity after 24 h compared to 20% BDDE (Figure 18). However, they were more difficult to handle. The 10% BDDE hydrogel was very soft and elastic, while the 30% BDDE hydrogel was brittle and easily broke.
[0218] Example 8 Use of other positively charged antimicrobial polypeptides After 24 hours, HA hydrogels loaded with 0.05 mg / mL and 0.1 mg / mL polyornithine PLO30 and polylysine PLL30 showed similar antibacterial activity compared to hydrogels loaded with PAR30 (Figure 19).
[0219] Example 9 In vivo biocompatibility Ten 8-week-old male Wistar rats (body weight 300 g–400 g), provided by a certified breeding center (Charles River, France), were used in this study.
[0220] Animals were received at the CREFRE (US006 / CREFRE-Inserm / UPS / ENVT) animal supplier (No. A31555010 issued 17 December 2015). Approval was obtained according to the European Directive for performing animal experiments (DE86 / 609 / CEE; amended DE2003 / 65 / CE) and the procedure was submitted to the CREFRE Ethics Committee. A one-week acclimatization was observed. The animals were housed in double-level ventilated cages (two animals per cage, according to European standards). The animals were closely monitored (behaviour and food consumption) and weighed every week during the experiment. Ten rats received two round implants each (1 cm diameter), i.e. one implant on the left side and one on the right side. In total, there were five implantations of hydrogel deposited on the mesh material and processed for drying and autoclaving for each of the following conditions: The conditions were: i) HA-only hydrogel; ii) 0.1 mg.mL -1 HA hydrogel loaded with PAR10 at 0.05 mg.mL-1 HA hydrogel loaded with PAR30 at 0.1 mg.mL -1 The HA hydrogel was loaded with PAR30.
[0221] Rats were induced with isoflurane 4% and maintained at 2%. Each rat was placed prone on a heated pad. After shaving and scrubbing with betadine, two 20 mm dorsal incisions were made in the thoracic-lumbar region, one on the right and one on the left. One scaffold was inserted into a subcutaneous pocket on each side. All incisions were closed with Vicryl® 3-0. All rats were injected subcutaneously with buprenorphine (0.6 mg / kg) twice daily for 5 days. All animals survived the study period without adverse effects. Euthanasia was performed after 14 days. Animals were first anesthetized with an isoflurane device and mask, then slowly injected with an overdose of pentobarbital (150 mg / kg) by intraperitoneal route. After the animals had died, the implants, including the surrounding tissues, were explanted and collected to perform histology.
[0222] For histological analysis, samples were fixed in 4% formalin. Macroscopic sections were embedded in paraffin. 5 μm thick sections were stained with hematoxylin-eosin-saffron (HES). For each sample, a slide scan (NanoZoomer, Hamamatsu Photonics K.K.) was performed with the following criteria, followed by a microscopic optical analysis using the software NDP.view2 (Hamamatsu Photonics K.K., Massy, France). A semiquantitative evaluation of acute inflammation, chronic inflammation, fibroblastic reaction, edema, fibrosis, angiogenesis and periprosthetic histiocytic reaction was realized.
[0223] result Preliminary in vivo experiments were performed in rats (10 animals). Each rat received two implants of hydrogel-covered mesh (d=1 cm), one on the left side and one on the right side. All animals survived the study period without adverse effects and all animals gained weight in the normal manner.
[0224] After 14 days, the implants, including the surrounding tissue, were explanted and collected for histological analysis. Analysis showed inflammation in the tissue surrounding the implants, but there was no difference between the HA-only hydrogel and the HA-PAR hydrogel, suggesting that the addition of PAR did not promote or increase the inflammatory response.
[0225] conclusion In summary, we developed hyaluronic acid (HA) hydrogels that can be loaded with polyarginine (PAR) and provide long-lasting antibacterial effects. This effect depends on the concentration and length of the loaded PAR. PAR30 was identified as the most efficient in providing long-lasting antibacterial effects, and the antibacterial effects increased with PAR concentration.
[0226] Antimicrobial hydrogels can be deposited onto wound dressings and mesh prostheses and may help prevent infection, thus improving tissue regeneration and / or implant integration.
Claims
1. 1. A hydrogel comprising hyaluronic acid (HA) or a derivative thereof and loaded with at least one positively charged antimicrobial peptide, wherein the peptide is not covalently bound to the hydrogel, the HA or a derivative thereof is crosslinked at the level of its hydroxyl moieties by a crosslinker, while the carboxyl moieties of the HA or a derivative thereof remain free and the HA or a derivative thereof remains negatively charged, the derivative of hyaluronic acid is selected from the group consisting of aldehyde-modified HA, amine-modified hyaluronic acid, HA containing photoreactive vinylbenzyl groups, methacrylate-modified HA, tyramine-linked HA, and catechol-linked HA, and the positively charged antimicrobial peptide is selected from the group consisting of polyarginine, polyornithine, and polylysine.
2. 10. The hydrogel of claim 1, wherein the positively charged antimicrobial peptide is polyarginine.
3. The polyarginine is represented by the following formula (1): 【Chemistry 1】 (wherein n is an integer between 2 and 250).
3. The hydrogel of claim 2,
4. The polyarginine is represented by the following formula (1): 【Chemistry 2】 (wherein n is 30) 4. The hydrogel of claim 3,
5. 5. The hydrogel of claim 1, wherein the hyaluronic acid is hyaluronic acid having a molecular weight between 800 kDa and 850 kDa.
6. 6. The hydrogel of claim 1, wherein the crosslinker is butanediol diglycidyl ether (BDDE).
7. A method for preparing a hydrogel according to any one of claims 1 to 6, comprising the steps of: (a) mixing under basic conditions hyaluronic acid (HA) or a derivative thereof with a crosslinking agent that crosslinks HA at the level of its hydroxyl moieties while leaving the carboxyl moieties of the HA or derivative thereof free and negatively charged, the derivative of hyaluronic acid being selected from the group consisting of aldehyde-modified HA, amine-modified hyaluronic acid, HA containing photoreactive vinylbenzyl groups, methacrylate-modified HA, tyramine-linked HA, and catechol-linked HA; (b) depositing the mixture on a support and incubating it at room temperature for 48 to 72 hours to obtain a hydrogel; (c) recovering the hydrogel formed in step (b); (d) incubating the hydrogel in an aqueous buffer under conditions that allow for removal of crosslinker residues and swelling of the hydrogel; (e) loading the hydrogel obtained in step (d) with at least one positively charged antimicrobial peptide selected from the group consisting of polyarginine, polyornithine and polylysine, wherein said peptide is not covalently bound to said hydrogel; (f) recovering the loaded hydrogel obtained in step (e); The method includes:
8. 8. The method of claim 7, wherein the mixture of step (a) comprises 2% (w / v) to 3% (w / v) of HA or a derivative thereof and at least 10% (v / v) of a cross-linking agent.
9. 9. The method according to claim 7 or 8, wherein the cross-linking agent is butanediol diglycidyl ether (BDDE).
10. 10. The method of any one of claims 7 to 9, wherein the positively charged antimicrobial peptide is polyarginine.
11. 11. The method of any one of claims 7 to 10, wherein the positively charged antimicrobial peptide is loaded in step (e) at a concentration of 0.05 mg / ml to 1 mg / ml.
12. 12. The hydrogel according to claim 1, possibly obtained by the method of preparation according to any one of claims 7 to 11.
13. 13. A medical device comprising the hydrogel of any one of claims 1 to 6 or 12.
14. 14. The medical device of claim 13, wherein the medical device is a wound dressing or a mesh prosthesis.
Citation Information
Patent Citations
Emulsion breaking agent, and processing method of oil-containing aqueous solution
JP2016150334A
Liquid antibacterial agent composition, method for producing the same, and antibacterial treatment method