Dissolving microcarriers for culturing cells and related methods - Patents.com
PGA microcarriers with controlled digestion byproducts address issues of oxygenation, nutrient supply, and enzyme damage in cell culture, facilitating efficient and low-stress cell recovery.
Patent Information
- Application Number
- JP2021573204
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-13
- Filing Date
- 2020-06-02
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-06-02
AI Technical Summary
Existing cell culture methods using microcarriers face challenges in oxygenation, nutrient supply, hydrodynamic stress, enzyme-induced cell damage, and inefficient cell recovery due to enzyme use and by-product effects.
The use of polygalacturonic acid (PGA) microcarriers crosslinked with divalent cations, which are digestible by chelating agents and enzymes, allowing for non-proteolytic cell separation and harvesting, with controlled digestion byproducts.
This approach enables efficient cell culture and harvesting with reduced damage, predictable separation, and minimal impact on cell health, using environmentally friendly and cost-effective methods.
Smart Images

Figure 0007588097000009 
Figure 0007588097000010 
Figure 0007588097000011
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority under 35 U.S.C. §120 of U.S. Provisional Patent Application No. 62 / 861,084, filed June 13, 2019, the contents of which are relied upon and incorporated herein by reference in its entirety.
[0002] This application is related to commonly-assigned U.S. patent application Ser. Nos. 14 / 899,394 and 15 / 579,739, and U.S. Patent Nos. 8,404,85 and 8,426,176, the contents of which are relied upon and incorporated herein by reference in their entireties. [Technical field]
[0003] The present disclosure relates generally to digestible substrates, and more particularly to digestible microcarriers that can be used, for example, for the isolation of proteins, cells, and viruses, and for diagnostic applications and cell culture, as well as methods of using the digestible substrates, and more particularly to methods of culturing and recovering cells, proteins, and viruses from the digestible substrates. [Background technology]
[0004] Microcarriers allow efficient cell scale-up in controlled bioreactors for therapeutic applications. In contrast to cell culture on flat surfaces where adherent cells reach high confluence and cell growth may therefore be limited by cell-cell contact inhibition, spherical microcarriers with their high surface area / volume ratio provide an attractive platform for efficient cell culture scale-up or expansion, allowing either harvested cells or conditioned media to be turned into the desired product.
[0005] A key imperative for cell culture is proper oxygenation and nutrient supply to the cells. Related challenges include agitation of the microcarriers to provide the necessary oxygen and nutrients without introducing sufficient hydrodynamic stress to damage the growing cells. Traditionally, agitation is achieved using impellers.
[0006] Further challenges include separating the microcarriers from the cells or conditioned medium. Enzymatic treatment can be used, for example, to harvest adherent cells, but the addition of enzymes can damage the cells. For example, proteolytic enzymes can non-selectively remove cell surface receptors.
[0007] Effective cell recovery from microcarriers often requires the use of concentrated enzymes, extended processing times, and successive centrifugation / filtration cycles that can have a detrimental effect on cell health and recovery. Additionally, concerns exist regarding potential by-products from microcarrier digestion and the impact such by-products may have on cell health and recovery. Summary of the Invention [Problem to be solved by the invention]
[0008] In view of the above, it would be advantageous to provide a cell growth surface comprising microcarriers with defined digestion by-products, as well as a method for effectively culturing and harvesting cells from the growth surface while controlling the digestion by-products. [Means for solving the problem]
[0009] According to an embodiment of the present disclosure, a cell culture article includes a substrate having polygalacturonic acid compounds crosslinked with divalent cations, the polygalacturonic acid compounds being selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof, the substrate being digestible by a digestive reagent into components including galacturonic acid monomers and divalent cations.
[0010] In another embodiment, a method for harvesting cultured cells from a soluble substrate is provided, comprising the steps of: separating the cultured cells from the substrate by digesting the substrate by exposing the substrate to (i) a chelating agent, (ii) an enzyme, or (iii) a chelating agent and an enzyme, the separation resulting in a harvest solution; and performing a series of washing and / or centrifugation cycles of the components of the harvest solution after the separation. The substrate comprises a polygalacturonic acid compound selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof, and an adhesive polymer on the surface of the polygalacturonic acid compound.
[0011] Additional features and advantages of the presently disclosed subject matter will be set forth in the following detailed description, and in part will be readily apparent to those skilled in the art from that description, or may be learned by practicing the presently disclosed subject matter as described herein, including the following detailed description, the claims, and the accompanying drawings.
[0012] It should be understood that both the foregoing summary and the following detailed description present embodiments of the presently disclosed subject matter and are intended to provide an overview or framework for understanding the nature and features of the presently disclosed subject matter as claimed. The accompanying drawings are included to provide a further understanding of the presently disclosed subject matter and are incorporated in and constitute a part of this specification. The drawings illustrate various embodiments of the presently disclosed subject matter and, together with the description, serve to explain the principles and operation of the presently disclosed subject matter. Additionally, the drawings and description are merely for illustrative purposes and are not intended to limit the scope of the claims in any way.
[0013] The following detailed description of specific embodiments of the present disclosure can be best understood when read in conjunction with the following drawings, where like structure is indicated with like reference numerals and in which: [Brief description of the drawings]
[0014] [Figure 1] Phase contrast image showing hMSC cells on externally crosslinked PGA microcarriers according to one embodiment. [Diagram 2] Phase contrast images showing hMSC cells on externally crosslinked PGA microcarriers according to further embodiments. [Diagram 3] Phase contrast image showing hMSC cells on externally crosslinked PGA microcarriers according to yet another embodiment. [Figure 4] Phase contrast images showing MRC5 and Vero cells on gelatin-coated PGA microcarriers, according to one embodiment. [Diagram 5] Graph of fold expansion of Vero cells on gelatin-coated dextran microcarriers and on gelatin-coated external crosslinked microcarriers. [Figure 6] Graph of fold expansion of MRC5 cells on gelatin-coated dextran microcarriers and on gelatin-coated externally crosslinked microcarriers. [Figure 7]Graph of hMSC cell fold expansion on gelatin-coated digestible microcarriers and on microcarriers with Corning Incorporated's Synthemax® II surface. [Figure 8] Phase contrast image showing monodisperse PGA beads made according to one embodiment [Figure 9] Phase contrast image showing MRC5 cells on externally crosslinked PGA microcarriers according to one embodiment. [Figure 10] Emulsification and internal gelation. Phase contrast images showing comparative microcarriers exhibiting a broad size distribution obtained by emulsification and internal gelation. [Figure 11] Phase contrast images of hMSC cells in serum-free medium after seeding on VN-grafted PGA microcarriers [Figure 12] Absorbance graph of PGA and digestion reagents using size exclusion chromatography (SEC) [Figure 13] Absorbance graph of PGA polymer digestion with pectinase and EDTA using SEC. [Figure 14] Mass spectrometry graph of PGA digestion in water [Figure 15] Graph of PGA microcarrier digestion using SEC [Figure 16] 1 is a flow diagram of a method for washing and centrifuging a cell suspension according to one or more embodiments. [Figure 17A] UV-VIS spectra of PGA and digesta from undiluted samples. [Figure 17B] UV-VIS spectra of PGA and digesta from diluted samples [Figure 17C] Graph of optical density of PGA and digesta at different wavelengths [Figure 17D] Graph of optical density of components from Figure 17C before and after various washes. [Figure 18] Synthemax II staining images of dissolving microcarriers [Figure 19]Graph of the fluorescence intensity of the stains in Figure 19 measured using a spectrophotometer [Figure 20] Image of anti-Synthemax II antibody staining of dissolving microcarriers [Figure 21] Image of dot blot analysis of soluble Synthemax II in digestion solution. [Figure 22A] A graph of the concentration of Vero cells based on different dilutions of the harvest solution. [Figure 22B] A graph of the concentration of Vero cells based on different dilutions of pectinase. [Figure 22C] A graph of the concentration of Vero cells based on different dilutions of EDTA. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Reference will now be made in more detail to various embodiments of the presently disclosed subject matter, some embodiments of which are illustrated in the accompanying drawings, in which the same reference numerals are used throughout to refer to the same or similar parts.
[0016] Disclosed are cell culture articles that promote cell attachment and proliferation. According to some embodiments, the disclosed cell culture articles allow for cell harvesting without the use of proteases. Exemplary cell culture articles are microcarriers, also referred to as beads or microbeads (collectively "microcarriers").
[0017] In an embodiment, the cell culture article is a smooth, transparent (or translucent) bead comprising a gel containing pectic acid, partially esterified pectic acid, or a salt thereof. The cell culture article may be spherical or substantially spherical and is formed by external gelation. The calcium content of the cell culture article can be adjusted to provide rapid cell harvest under gentle conditions that reduce damage to the cells. Molecules that promote adhesion of anchorage-dependent cells can be attached to the surface of the cell culture article by chemical bonding or physical adsorption.
[0018] In contrast to the external gelation route disclosed herein, microcarriers can be formed via emulsification and internal gelation, in which beads are formed by gelation of an aqueous solution of polygalacturonic acid (PGA) containing an insoluble calcium salt dispersed in an aqueous phase, which is emulsified within an oil phase (also called the continuous phase or dispersion medium).
[0019] In the case of internal gelation, crosslinking is achieved by the transfer of soluble divalent metal ions (e.g., Ca) from salts. 2+ or Mg 2+ The process is initiated by the addition of an oil-soluble acid, which releases an ester group. However, such a process requires a large amount of oil phase, as well as a significant amount of surfactant, to stabilize the emulsion. Vegetable oils can be used as the continuous phase, but beads prepared in this dispersion medium are difficult to rinse.
[0020] A further drawback of the internal gelation process is that some of the metal ion source (salt) may remain intact and manifest itself as inhomogeneity in the microcarrier, thereby impairing surface roughness and transparency. Furthermore, such left-over metal salts may be released over time during use of the microcarrier (which may be detrimental to cell culture) or may inhibit digestion of the microcarrier during cell harvesting.
[0021] The external gelation method of the present disclosure provides an inexpensive and environmentally friendly synthetic route to prepare highly transparent PGA microcarriers that are free of undesirable inclusions (second phases) and surface defects and that support the separation and harvesting of non-proteolytic cells. As defined herein, transparent microcarriers exhibit at least 90% transmittance across the visible spectrum from 390 to 700 nm, i.e., 90, 92, 94, 96, 98, 99, or 100% transmittance (including ranges between any of the foregoing values).
[0022] Additionally, embodiments can provide a uniform size distribution of microcarriers, which ensures faster and cleaner separation of the microcarriers from the supernatant during use. This can make medium exchange and final product separation more predictable, more reliable, and less expensive. In embodiments, the size of the microcarriers can be precisely tuned to different ranges, which allows customization of the bead settling rate to match different bioprocess needs without changing the material properties of the beads.
[0023] According to some embodiments, calcium cross-linked polygalacturonic acid (PGA) microcarriers are provided that can be dissolved using ethylenediaminetetraacetic acid (EDTA) and pectinase. Characterization of such PGA polymers and microcarriers, as well as dissociation agents and by-products, is discussed herein, and the effect of such components on subsequent cell growth is determined. Based on this, efficient PGA microcarriers and methods for culturing and harvesting cells using the PGA microcarriers have been determined.
[0024] The by-products of PGA microcarrier digestion (e.g., galacturonic acid monomers, calcium, EDTA, and pectinase) were characterized using size exclusion chromatography (SEC), electrospray ionization mass spectrometry (ESI-MS), and inductively coupled plasma mass spectrometry (ICP-MS). UV-Vis spectroscopy was used to confirm that these soluble components can be removed by the methods disclosed herein, including a series of washing and / or centrifugation cycles.
[0025] Additionally, as described below, analysis of the location of the "Synthemax" II coating on the microcarriers after lysis using an antibody against the "Synthemax" II peptide indicates that the majority of the "Synthemax" II for the PGA microcarriers of the present disclosure becomes soluble after bead digestion. In some embodiments, if a small residual amount of "Synthemax" II remains associated with the released cells, this level can be reduced by adding a protease (e.g., trypsin) to the harvest solution.
[0026] The effects of digestive juice components, pectinase, and EDTA on cell growth in 2D culture were analyzed by adding known concentrations of pectinase and EDTA back to the cells to identify the concentrations that had the least effect on cell growth. According to some embodiments, the method includes maintaining the concentration of EDTA at 1 mM or less and pectinase at 30 U / mL or less. Additionally, these components can be removed by washing and / or centrifugation or filtration before passaging or cryopreserving the cells.
[0027] Thus, embodiments disclosed herein provide microcarriers with reduced or eliminated digestive by-products. Additionally, knowledge or control of the by-products by the articles and methods herein may provide practitioners with increased knowledge and confidence in the use of PGA microcarriers and their biological and / or therapeutic implications.
[0028] Although some embodiments are directed to microcarriers, the substrate can take a variety of forms and is not limited to microcarriers or beads. In some embodiments, the substrate can take a form suitable for use in a packed bed bioreactor, for example, a foamed scaffold having a cylindrical, rectangular, triangular, or disc shape. Thus, according to embodiments, a dissolvable foamed scaffold for cell culture is provided. The dissolvable foamed scaffold comprises an ionotropically crosslinked polygalacturonic acid compound selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof. In some embodiments, the scaffold can comprise at least one first water-soluble polymer having surface activity.
[0029] PGA Polymer Polygalacturonic acid (PGA), or pectic acid, is a water-soluble biopolymer of pectin degradation found in ripe fruits and some vegetables. It is best known as a thickening agent in the food industry, but can also be used as a matrix or binder for drug, protein, and cell delivery in the pharmaceutical and biotechnology industries. The viscosity of the polymer depends on the molecular weight, degree of esterification, concentration, pH, and the presence of counterions in the solution. PGA polymers produce gels that are independent of sugar content, show little sensitivity to changes in pH, and require a defined amount of calcium or other divalent cations to control gelation. Microcarriers of PGA polymers can be made, for example, by dropping a solution of PGA into a calcium chloride bath, which results in rapid gelation of the droplets as spherical beads. Excess calcium chloride is removed from the microcarriers through a series of washing cycles before the microcarriers are coated with a cell adhesion-promoting substrate such as "Synthemax" II or denatured collagen.
[0030] PGA microcarriers can be destabilized by removing calcium ions using ethylenediaminetetraacetic acid (EDTA). PGA polymers can be further degraded using the enzyme pectinase, which hydrolyzes the linkages between monomer units, thus reducing the molecular weight of the PGA polymer and increasing its solubility. Generally, pectinases are associated with fruit ripening because they promote the softening of plant cell walls; therefore, pectinases have been issued a Generally Recognized As Safe (GRAS) notice by the FDA for use as a direct human food ingredient.
[0031] Microcarriers can be made using at least one ionotropically cross-linked polysaccharide, examples include pectic acid, also known as polygalacturonic acid (PGA), or a salt thereof, or partially esterified pectic acid, also known as pectinic acid (PE PGA), or a salt thereof.
[0032] Pectic acid can be formed by hydrolysis of certain pectin esters. Pectin is a cell wall polysaccharide that naturally has a structural role in plants. Major sources of pectin include citrus peels (e.g., lemon and lime peels) and apple peels. Pectin is a primarily linear polymer based on a 1,4-linked alpha-D-galacturonate backbone randomly interrupted by 1,2-linked L-rhamnose. The average molecular weight ranges from about 50,000 to about 200,000 daltons.
[0033] The polygalacturonic acid chains of pectin may be partially esterified, for example with methyl groups, and the free acid groups may be partially or completely neutralized with monovalent ions, such as sodium, potassium, or ammonium ions. Polygalacturonic acid partially esterified with methanol is called pectinic acid and its salts are called pectinates. The degree of methylation (DM) of high methoxyl (HM) pectin may be, for example, 60-75 mol %, and the degree of methylation of low methoxyl (LM) pectin may be, for example, 1-40 mol %.
[0034] In embodiments in which pectic acid is selected, the degree of esterification may be 40 mole % or less (e.g., 1, 5, 10, 20, 30 or 40 mole %, including ranges between any of the foregoing values). A higher degree of esterification may result in ineffective bead formation through ionotropic crosslinking. Without being bound by theory, it is believed that a minimum amount of free carboxylic acid groups (not esterified) is required to obtain the desired degree of ionotropic crosslinking.
[0035] In embodiments, the microcarrier beads are formed using LM pectin, such as polygalacturonic acid containing 20 mole % or less (e.g., 0, 5, 10, 15, or 20 mole %) methoxyl groups. Such polygalacturonic acid may have no or negligible methyl ester content, like pectinic acid. As used herein, pectinic acid and low methoxyl (LM) pectins, which have no or negligible methyl ester content, are collectively referred to as PGAs.
[0036] In an embodiment, the microcarrier beads were formed using a mixture of pectinic acid and pectinic acid. Pure pectinic acid and / or pectinic acid may be used. Blends with compatible polymers may also be used. For example, pectinic acid or pectinic acid may be mixed with polysaccharides such as dextran, substituted cellulose derivatives, alginic acid, starch, glycogen, arabinoxylan, agarose, etc. Glycosaminoglycans such as hyaluronic acid and chondroitin sulfate, or various proteins such as elastin, fibrin, silk fibroin, collagen and their derivatives may also be used. Other water-soluble synthetic polymers may also be blended with pectinic acid and / or pectinic acid. Non-limiting examples include polyalkylene glycols, poly(hydroxyalkyl(meth)acrylates), poly(meth)acrylamides and derivatives, poly(N-vinyl-2-pyrrolidone), polyvinyl alcohol, etc. Compatible polymers can be anionic, neutral, or cationic, provided their inclusion does not impair digestion of the microcarrier.
[0037] External ionotropic gelation External gelation, also called diffusion setting, involves the introduction of a hydrocolloid (PGA) solution into an ionic solution, where gelation occurs via the diffusion of ions into the hydrocolloid solution. In an embodiment, a negatively charged aqueous polysaccharide solution was dispensed dropwise into a solution of divalent cations such as calcium, magnesium, or barium to induce crosslinking of the PGA polymer. The crosslinks are ionic crosslinks, as opposed to covalent crosslinks, which allow for subsequent digestion of the crosslinked polymer.
[0038] According to embodiments, the PGA concentration in the hydrocolloid solution was in the range of 0.5 to 5% by weight, for example, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5% by weight (including ranges between any of the foregoing values).
[0039] Exemplary methods for forming droplets of hydrocolloid (PGA) solutions included syringe dripping or extrusion; jet break-up or milling, where beads are formed by a coaxial air stream that draws the droplets from a nozzle; electrostatic bead generation, where an electrostatic field is used to draw the droplets from a nozzle into a gelling bath; magnetically driven vibration; jet cutting, where beads are formed by a rotating cutting tool that cuts the jet into uniform cylindrical segments; and spinning disk atomization.
[0040] The droplets of the PGA solution may be spherical or substantially spherical and have an average diameter in the range of 10 to 500 micrometers, for example, 10, 20, 25, 50, 75, 100, 150, 200, 252, 300, 350, 400, 450, or 500 micrometers (including ranges between any of the foregoing values).
[0041] The gelling bath may include an aqueous solution of a divalent metal salt. In embodiments, the salt (e.g., calcium chloride) concentration in the gelling bath is at least 1% (w / v), such as 1, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20% (including ranges between any of the preceding values). If the calcium content is too low, the beads will exhibit insufficient stability due to too low crosslink density.
[0042] The aqueous solution may include an alcohol, such as ethanol, in a ratio of alcohol to water (v / v) ranging from 0 / 100 to 80 / 20, such as 0 / 100, 10 / 90, 20 / 80, 30 / 70, 40 / 60, 50 / 50, 60 / 40, 70 / 30, and 80 / 20.
[0043] In embodiments, some covalent cross-linking may occur, but the level of such cross-linking that is irreversible must be sufficiently low, e.g., less than about 10 mol % to 20 mol %, to maintain digestibility of the beads.
[0044] The microcarrier beads may be spherical or substantially spherical and have an average diameter in the range of 10 to 500 micrometers, e.g., 10, 20, 25, 50, 75, 100, 150, 200, 250, 300, 350, 400, 450, or 500 micrometers (including ranges between any of the aforementioned values). In embodiments, the coefficient of variation (CV) of the microcarrier beads, also referred to as the relative standard deviation, is less than 20%, e.g., 2, 5, 10, or 15% (including ranges between any of the aforementioned). In embodiments, the size range Δd5-d95 (the difference between d95 and d5, where d5 is the microcarrier diameter that is greater than the diameter of 5% of the microcarrier population and d95 is the microcarrier diameter that is greater than the diameter of 95% of the microcarrier population) is less than 25 micrometers, e.g., 10, 15, or 20 micrometers (including ranges between any of the aforementioned). In an embodiment, the size range Δd10-d90 (the difference between d90 and d10, where d10 is the microcarrier diameter larger than the diameter of 10% of the microcarrier population and d90 is the microcarrier diameter larger than the diameter of 90% of the microcarrier population) is less than 20 micrometers, for example 5, 10, or 15 micrometers (including ranges between any of the foregoing). In an embodiment, the range of radii of curvature from d5 to d95 (the difference between the radius of curvature of the microcarrier diameter larger than the diameter of 5% of the microcarrier population and the radius of curvature of the microcarrier diameter larger than the diameter of 95% of the microcarrier population) is less than 10 cm -1 Less than, for example, 2, 5, or 8 cm -1 (including any range therebetween).
[0045] Bead Size Control In embodiments, microcarrier beads can be manufactured within a specific narrow size range; that is, their size can be controlled. Controlling the size of microcarrier beads is important for several reasons. If there is a wide size distribution ranging from small to large microcarriers, the microcarriers with smaller sizes will remain in suspension much longer than the microcarriers with larger sizes. The exact settling time in the process will be much longer (due to the presence of small beads) or will be difficult to define. During use, more time is needed to ensure that the supernatant is removed from the microcarriers.
[0046] The narrow size distribution allows the beads to settle at a consistent rate, which allows for more predictable separation of the microcarriers from the supernatant during medium exchange or culture product separation. The size of the microcarriers can be fine-tuned to different ranges to control the settling rate. This allows for customization of the settling rate to suit different process needs. Size-controlled microcarriers have a uniform surface area, providing the same area available for cell seeding per microcarrier. This makes it easier to calculate the surface area available for cell seeding. In addition, the cells reach confluence at the same or similar times. As used herein, the terms "confluence" or "confluent" are used to indicate that the cells form a coherent layer on the growth surface where every cell is in contact with other cells, such that substantially all of the available growth surface is used. For example, "confluence" is defined as a state in which "all cells are in contact with other cells throughout their surroundings and no available substrate is left uncovered" (RI Freshney, Culture of Animal Cells-A Manual of Basic Techniques, Second Edition, Wiley-Liss, Inc. New York, NY, 1987, p. 363). Conventionally, the amount of growth surface covered by cells is referred to as the percentage of confluence. For example, a situation in which approximately half of the growth surface is covered with cells is referred to herein as 50% confluence, or alternatively, half confluence. Size-controlled microcarriers can be suspended under the same stirring conditions. This allows fine control of shear forces to balance good suspension of the microcarriers and conditions that cause less damage to the cells. Well-defined settling times for different populations of size-controlled microcarriers can facilitate separation during continuous cell culture and help prevent uneven cell growth on beads supplied at different times. For example, cells can be initially seeded on size-controlled microcarriers of 250 μm size.After the cells reach half confluence, size-controlled microcarriers of 350 μm size can be added to the bioreactor for bead-to-bead transfer. At the time of confluence of the 250 μm microcarriers, this size microcarrier can be removed by its own settling velocity or by filtration. Only beads with a size of 350 μm and half confluence are left in the bioreactor. Then, new 250 μm microcarriers can be added. After the 350 μm microcarriers reach confluence, they can be collected and new 350 μm microcarriers can be added. This process can ensure that all beads are removed when confluence is reached. In contrast, if the same size microcarriers are used to perform bead-to-bead transfer and continuous cell culture, the cells on the beads from the previous feed will remain in the bioreactor much longer than the cells on the beads from the later feed, which may result in a decrease in cell quality as a result of excessive confluence.
[0047] In an embodiment, a vibration encapsulation device was used to size-control the soluble microcarriers during production. Size-controlled beads were formed by passing them through a nozzle with a defined hole size, flow rate, and vibration frequency. The size of the resulting beads was narrowly controlled with a coefficient of variation of less than 10%.
[0048] Digestion of beads Non-proteolytic enzymes suitable for digesting microcarriers, harvesting cells, or both include pectinolytic enzymes, or pectinases, a heterogeneous group of related enzymes that hydrolyze pectic substances.
[0049] Cell harvesting involves contacting the cell-laden microcarriers with a solution containing a pectinase degrading enzyme or a mixture of pectinase and a divalent cation chelating agent.
[0050] An exemplary method for harvesting cultured cells includes culturing the cells on the surface of the microcarriers disclosed herein and contacting the cultured cells with a mixture of pectinase and a chelating agent to separate the cells from the microcarriers.
[0051] Pectinase (polygalacturonase) is an enzyme that breaks down complex pectin molecules into shorter molecules of galacturonic acid. Pectinase catalyzes the release of pectic oligosaccharides (POS) from polygalacturonic acid. Pectinases are produced by fungi, yeasts, bacteria, protozoa, insects, nematodes, and plants. Commercially available sources of pectinase are generally multienzymes, such as Novozyme Pectinex™ ULTRA SPL, a pectinolytic enzyme preparation produced from selected strains of Aspergillus aculeatus. Novozyme Pectinex™ ULTRA SPL primarily contains polygalacturonase (EC 3.2.1.15), pectin transeliminase (EC 4.2.2.2), and pectinesterase (EC:3.1.1.11). The EC designation is the Enzyme Commission's classification scheme for enzymes based on the chemical reaction they catalyze. Pectinases are known to hydrolyze pectin. They can attack methyl-esterified pectin or de-esterified pectin.
[0052] The concentration of pectin degrading enzyme in the digestion solution may be from 1 to 200 U, for example, 1, 2, 5, 10, 20, 50, 100, 150, or 200 U (including ranges between any of the foregoing).
[0053] Exemplary chelating agents include ethylenediaminetetraacetic acid (EDTA), cyclohexanediaminetetraacetic acid (CDTA), ethylene glycol tetraacetic acid (ETGA), citric acid, tartaric acid, etc. The concentration of the chelating agent in the digestion solution can be 1-200 mM, e.g., 10, 20, 50, 100, 150, or 200 mM. To prevent cytotoxic side effects, the concentration of the chelating agent in the digestion solution can be 10 mM or less, e.g., 1, 2, 5, or 10 mM (including ranges between any of the foregoing).
[0054] In embodiments, the total volume of the digestion solution comprising the pectin degrading enzyme and the chelating agent is less than 10 times the volume of the microcarriers, for example 1, 2, 4, 5, or 10 times the volume of the microcarriers (including ranges between any of the preceding values).
[0055] Depending on the digestion time, temperature, and amount of pectinolytic enzyme added, the degree of digestion of the beads can be selected or predetermined. It has been observed that cells detach from the microcarrier surface before the beads are completely digested. Thus, it is possible to harvest cells with or without complete digestion of the beads. In embodiments in which cells are harvested from partially digested microcarriers, separation of the cells from the remaining microcarriers can be achieved by one or more of filtration, decantation, centrifugation, and similar processes.
[0056] The beads are easily digested when the calcium content is less than 2 g / L of wet beads, e.g., less than 2, 1.5, 1, 0.8, or 0.5 g / L. If the calcium content of the beads at the harvest stage is greater than 1 g / L, greater amounts and / or concentrations of pectinolytic enzymes and divalent cation chelators can be used. The time required for complete digestion can be less than 1 hour, e.g., 10, 15, 30, or 45 minutes. As used herein, the term "complete digestion" refers to the time required for complete digestion as defined in the United States Pharmacopeia and National Formulary Section 788 (USP) entitled "Particulate Matter in Injections". <788> The digestion of microcarriers gives a microcarrier particle count according to the particle counting method described in the USP <788> A preparation complies with the test if the average number of particles present in the unit being tested does not exceed 25 particles per mL at 10 μm or greater and does not exceed 3 particles per mL at 25 μm or greater, as shown in Table 1. In an embodiment, the number of microcarrier particles for particles having a size of 10 μm or greater after digestion of the microcarrier is less than 10 particles, e.g., 0, 1, 2, 3, 4, 5, 6, 7, 8, or 9 (including any of the ranges between the foregoing). In an embodiment, the number of microcarrier particles for particles having a size of 25 μm or greater after digestion of the microcarrier is less than 1 particle, e.g., 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9 (including any of the ranges between the foregoing).
[0057] As defined herein, the volume of "wet beads" is the volume of the bead bed after decantation or centrifugation. The bead bed includes swollen beads and interstitial water (i.e., water present between the swollen beads). By measurement, the wet beads include 70% by volume of swollen beads and 30% by volume of interstitial water. The swollen beads include 99% water for a 1% PGA solution, 98% water for a 2% PGA solution, 97% water for a 3% PGA solution, etc.
[0058] As an example, microbeads prepared from 3% (w / v) PGA sol contain approximately 1.48 g / l calcium ions at equilibrium. Complete digestion of the microbeads in less than 10 minutes occurs with exposure to at least 10 mM EDTA and at least 50 U of enzyme using a 5-fold volume of digestion solution (relative to the volume of the beads).
[0059] cell adhesion Due to their hydrogel nature and negative charge, PGA beads do not readily support cell adhesion without specific treatment. To promote the adhesion of anchorage-dependent cells, the microbeads can be coated or otherwise surface treated. For example, PGA beads can be functionalized with moieties that promote cell adhesion, such as peptides containing the RGD sequence.
[0060] Further candidate peptides include those that contain amino acid sequences that are potentially recognized by proteins of the integrin family or that provide interactions with cellular molecules that can maintain cell adhesion. Examples include BSP, vitronectin, fibronectin, laminin, collagen types I and IV, denatured collagen (gelatin), and similar peptides, as well as mixtures thereof. Further exemplary peptides are the BSP and vitronectin (VN) peptides, which have the following sequences, respectively: Ac-Lys-Gly-Pro-Gln-Val-Thr-Arg-Gly-Asp-Val-Phe-Thr-Met-Pro-NH2 (SEQ ID NO: 1), and Ac-Lys-Gly-Gly-Asn-Gly-Glu-Pro-Arg-Gly-Asp-Thr-Tyr-Arg-Ala-Tyr-NH2 (SEQ ID NO: 2).
[0061] In embodiments, the microbeads are surface functionalized with recombinant proteins that promote cell adhesion, which can be grafted or applied as a coating. Exemplary recombinant proteins include fibronectin-like engineered proteins sold under the trade names ProNectin® and "ProNectin" plus, although other recombinant proteins that promote adhesion of anchorage-dependent cells can also be used. EXAMPLES
[0062] Example 1. 1% PGA microbeads crosslinked with 3% calcium.
[0063] Microbeads were prepared from a 1% by weight solution of polygalacturonic acid (PGA) by dissolving polygalacturonic acid sodium salt (Sigma catalog number #P3850) in water under constant stirring at 80-85 °C. The solution was filtered using a 20 micrometer polypropylene filter under vacuum to eliminate any particles in the suspension.
[0064] A gelling bath was generated in a separate beaker using 400 ml of 3% w / v calcium chloride water / ethanol (75 / 25 v / v) solution, stirred using a magnetic stirrer.
[0065] Droplets were generated by adding 25 ml of PGA solution to the gelling bath using a syringe equipped with a 30 gauge needle. A syringe pressure of approximately 2 bar was applied.
[0066] The beads were cured in a calcium chloride bath for 120 minutes and then washed four times with water. The calcium content in the beads was determined as described in Example 9. After four rinses, the calcium concentration was about 0.5-0.6 g / l of wet beads.
[0067] The beads were stored in sterile water in a sterile container at 4° C. prior to coating. The beads were very clear with no observable surface defects.
[0068] When contacted with 5 mM EDTA / 50 U pectinase at 25°C, the beads were completely dissolved within 5 min.
[0069] Example 2. 1% PGA microcarriers cross-linked with 12% calcium The procedure from Example 1 was repeated, except that the 3% w / v calcium chloride aqueous / ethanol (75 / 25 v / v) solution was replaced with a 12% w / v calcium chloride aqueous / ethanol (75 / 25 v / v) solution. After four rinses, the calcium concentration was about 0.5-0.6 g / l of the wet beads. The beads were very transparent with no observable surface defects.
[0070] When contacted with 5 mM EDTA / 50 U pectinase at 25°C, the beads were completely dissolved within 5 min.
[0071] Example 3. 1.5% PGA microcarriers cross-linked with 3% calcium The procedure from Example 1 was repeated, except that a 1.5 wt % solution of polygalacturonic acid and a pressure of 4 bar were used.
[0072] After four rinses, the calcium concentration was approximately 0.7-0.8 g / l of the wet beads. The beads were very transparent with no observable surface defects.
[0073] Example 4. 1.5% PGA microcarriers cross-linked with 12% calcium The procedure from Example 3 was repeated, except that a 12% w / v aqueous calcium chloride / ethanol (75 / 25 v / v) solution was used instead of the 3% w / v aqueous calcium chloride / ethanol (75 / 25 v / v) solution.
[0074] After four rinses, the calcium concentration was approximately 0.7-0.8 g / l of wet beads.
[0075] Example 5-a. 2% PGA microcarriers cross-linked with 3% calcium The procedure from Example 1 was repeated, except that a 2 wt% solution of polygalacturonic acid and a pressure of 5 bar were used. The PGA solution was preheated to 30°C and jetted at 30°C into a gelling bath maintained at 25°C.
[0076] After four rinses, the calcium concentration was approximately 0.9-1.0 g / L of the wet beads. The beads were very transparent with no observable surface defects.
[0077] Example 5-b. 3% PGA microcarriers cross-linked with 3% calcium The procedure from Example 1 was repeated, except that a 3 wt% solution of polygalacturonic acid and a pressure of 6 bar were used. The PGA solution was preheated to 40°C and jetted at 40°C into a gelling bath maintained at 25°C.
[0078] After four rinses, the calcium concentration was 1.48 g / l of the wet beads. The beads were very clear with no observable surface defects.
[0079] When contacted with 5 mM EDTA / 50 U pectinase at 25°C, the beads were completely dissolved within 10 min.
[0080] Example 6. 2% PGA microcarriers cross-linked with 12% calcium The procedure from Example 5-a was repeated, except that a 12% w / v calcium chloride aqueous / ethanol (75 / 25 v / v) solution was used.
[0081] After four rinses, the calcium concentration was approximately 0.9-1.0 g / l of wet beads.
[0082] Example 7. PGA beads coated with 0.1% gelatin crosslinked with glutaraldehyde.
[0083] A 0.1% pig skin gelatin solution was prepared by first soaking 0.5 g (Type A) of pig skin (Sigma #G1890) in 20 ml of water, then adding 480 ml of heated water (60°C-80°C).
[0084] Ten milliliters of PGA beads prepared according to Examples 1-6 were collected by centrifugation, to which 10 mL of porcine gelatin solution was added. The resulting mixture was gently shaken and incubated at 25° C. for 60 minutes. The supernatant was removed, and the beads were washed once with water.
[0085] To crosslink the gelatin coating, 100 ml of 0.05% glutaraldehyde solution, prepared from a 25% stock solution (Sigma C5882), was added to the bead bed and incubated with gentle shaking for 1 hour at 23° C. The beads were then rinsed three times with water and stored in a sterile container at 4° C.
[0086] Example 8. PGA beads with "Synthemax" II-SC synthetic copolymer surface Approximately 9 ml of swollen beads prepared according to Example 1 were placed in a 50 ml plastic centrifuge tube. 36 ml of a 0.25 mg / ml aqueous solution of adhesion-promoting peptide was added to the beads to form a Corning Incorporated "Synthemax" II-SC surface. The tube was gently shaken and placed at 40° C. for 30 minutes to functionalize the beads with the synthetic copolymer. After cooling, the functionalized beads were washed three times with deionized water. The beads were stored in a sterile container in water at 4° C.
[0087] Example 9. Calcium titration To quantify calcium content, 1 ml of PGA beads was digested by combining with 10 ml of 5 mM EDTA / 50 U pectinase solution. The suspension was shaken vigorously and left at 25° C. for 1 h with gentle shaking until digestion was complete.
[0088] The calcium content of the beads was quantified by inductively coupled plasma optical emission spectrometry (Axial ICP-OES, Varian720 ES tool). Samples to be analyzed were prepared by diluting 100 μl of the solution containing the digested beads with 9.9 ml of 1% HNO3. A calibration curve was constructed using solutions of known calcium concentration, prepared from a 1 g / l aqueous standard solution diluted with HNO3 as was done for each sample.
[0089] Example 10-a. Static culture of hMSCs using peptide copolymer-coated microcarriers Beads prepared according to Example 2 and with a "Synthemax" II-SC copolymer surface according to Example 8 were cleaned with 70% ethanol / water, rinsed twice with phosphate buffered saline (dPBS) and then with MesenCult™-XF complete medium (MC-XF). Bone marrow-derived mesenchymal stem cell (hMSC) cultures were performed in MC-XF in 24-well ULA plates under static conditions. Cells were seeded at 100k cells / well. Cells were harvested from the microcarriers by treatment with 50U pectinase / 5mM EDTA for 5 min. Cell morphology 2 days after seeding is shown in Figure 1. Cell morphology 4 days after seeding is shown in Figure 2.
[0090] Example 10-b. Static culture of hMSCs using gelatin-coated microcarriers Beads were prepared according to Example 4 and coated with gelatin according to Example 7. Figure 3 shows exemplary phase contrast images of human bone marrow-derived mesenchymal stem cells (hMSCs) attachment and proliferation 2 days after seeding at 100k cells / well in a 24-well plate.
[0091] Example 11. Growth of Vero cells on gelatin-coated PGA microcarriers Vero cells were cultured on gelatin-coated externally crosslinked 1% PGA microcarriers prepared according to Example 2 and coated according to Example 7 with continuous stirring.
[0092] The beads were first cleaned with 70% ethanol / water, rinsed twice with phosphate buffered saline (dPBS) and then with (IMDM+10% FBS+5ml penicillin streptomycin+5ml Glutamax™ medium).
[0093] Cell culture was performed in Corning Inc. disposable spinner flasks using IMDM supplemented with 10% FBS + 5ml penicillin streptomycin + 5ml "Glutamax" medium as the culture medium. Flasks were seeded with 1M Vero (p5) without agitation for 2 hours, followed by continuous agitation. The passage number designation (p#, in this example "p5") indicates the number (#) of growth and harvest cycles used to generate the cells (i.e., the number of divisions the cells had in culture).
[0094] Cell harvest on day 5 was performed using 10 mL of 50 U / ml pectinase, 5 mM EDTA.
[0095] Figure 4 shows exemplary phase contrast images of Vero cell attachment and proliferation 4 days after seeding. Fold expansion data is shown in Figure 5.
[0096] Example 12. Growth of MRC5 cells on gelatin-coated PGA microcarriers Human fetal lung fibroblast (MRC5) cells were cultured on gelatin-coated, externally crosslinked 1% PGA microcarriers prepared according to Example 2 and coated according to Example 7 with intermittent agitation.
[0097] The beads were first cleaned with 70% ethanol / water, rinsed twice with phosphate buffered saline (dPBS) and then with (IMDM+10% FBS+5ml penicillin streptomycin+5ml "Glutamax" medium).
[0098] Cell culture was performed in disposable spinner flasks from Corning Inc. using IMDM supplemented with 10% FBS + 5ml penicillin streptomycin + 5ml "Glutamax" medium as the culture medium. Flasks were seeded with 1M MRC5 cells (p4) without stirring overnight, followed by intermittent stirring (1 / 4 hour every 2 hours).
[0099] Cell harvest on day 5 was performed using 10 mL of 50 U / ml pectinase, 5 mM EDTA.
[0100] Figure 4 shows exemplary phase contrast images of MRC5 cell attachment and proliferation 4 days after seeding. Fold expansion data is shown in Figure 6.
[0101] The micrographs in Figure 4 show that Vero and MRC5 cells were able to attach to the PGA microcarriers and reach confluence.
[0102] Example 13. Growth of hMSC cells on peptide copolymer-coated microcarriers hMSC cells were prepared as described in Example 1 and cultured with continuous stirring on externally crosslinked PGA beads with a "Synthemax" II-SC copolymer surface according to Example 8.
[0103] The beads were first cleaned with 70% ethanol / water, rinsed twice with phosphate buffered saline (dPBS) and then with "MesenCult"-XF complete medium (MC-XF). Cells were seeded at 1M cells / flask and cell culture was performed in Corning Incorporated disposable spinner flasks using MC-XF.
[0104] Cells were harvested from the microcarriers on day 7 by treatment with 10 ml of 50 U pectinase / 5 mM EDTA for 5 minutes. Fold expansion data is shown in FIG.
[0105] Example 14. Growth of hMSC cells on peptide copolymer-coated microcarriers Expansion of hMSC cells under continuous agitation as described in Example 13 was repeated, except that externally crosslinked PGA beads prepared from a 2% PGA solution prepared as described in Example 5-a and with a Corning Synthemax II synthetic peptide copolymer surface as described in Example 8 were used. Fold expansion data is shown in FIG.
[0106] Example 15. Growth of hMSC cells on gelatin-coated microcarriers hMSC cells were prepared as described in Example 1 and cultured with continuous stirring on externally crosslinked PGA beads coated with gelatin as described in Example 7.
[0107] The beads were first cleaned with 70% ethanol / water, rinsed twice with phosphate buffered saline (dPBS) and then with "MesenCult"-XF complete medium (MC-XF). Cells were seeded at 1M cells / flask and cell culture was performed in Corning Incorporated disposable spinner flasks using MC-XF.
[0108] Cells were harvested from the microcarriers on day 7 by treatment with 10 ml of 50 U pectinase / 5 mM EDTA for 5 minutes. Fold expansion data is shown in FIG.
[0109] Example 16. Growth of hMSC cells on gelatin-coated microcarriers Expansion of hMSC cells under continuous stirring conditions was repeated as described in Example 15, except that externally crosslinked gelatin-coated PGA beads were used, prepared as described in Example 5-a, and coated with gelatin as described in Example 7. Fold expansion data is shown in FIG.
[0110] Example 17. Chemical stability of PGA microcarriers The chemical stability of the microcarrier beads was assessed by adding 1 ml of swollen beads to a plastic centrifuge tube containing 5 ml of Dulbecco's Phosphate Buffered Saline (dPBS) (1X). The tube was incubated at 37°C for 24 hours. The volume of the beads after 24 hours was comparable to the initial volume, indicating that the beads were not soluble in the phosphate buffer.
[0111] Example 18.
[0112] Monodisperse microcarrier beads were generated from a 1.5 wt% PGA solution using an electromagnetically driven laminar jet nozzle system (Nisco Engineering AG, Zurich, Switzerland). The system is equipped with a 100 μm nozzle. The frequency was set at 2.5 kHz and the amplitude was set at 100%. The flow rate of the generated solution was about 100 ml / hr by applying a pressure of about 3 psi (about 20.68 kPa).
[0113] The nozzle was positioned approximately 7.5 cm above the surface of the gelling bath (4 wt % CaCl2 solution in 50:50 v / v water / ethanol). The bath was continuously stirred (170 rpm).
[0114] The resulting microbeads had a mean diameter of 240±15 μm, corresponding to a coefficient of variation (CV) of 6.25%. This narrow size distribution is shown in Figure 9 (magnification: 4X).
[0115] The beads were gelatin coated and the gelatin coating crosslinked as described in Example 7, except that 50 ml of 0.05% glutaraldehyde solution was used instead of 100 ml.
[0116] Example 10-c. Static culture of MRC5 using gelatin-coated microcarriers Human fetal lung fibroblast (MRC5) cells were cultured under static conditions on gelatin-coated microbeads prepared according to Example 18. Cells were seeded at 100k cells / well in 24-well ULA plates using IMDM supplemented with 10% FBS as the culture medium. Cell morphology one day after seeding is shown in the phase contrast microscope image in FIG. 10.
[0117] Example 19. Grafting of vitronectin peptides onto PGA microcarriers Approximately 3 ml of swollen beads prepared according to Example 18 were placed in a 15 ml plastic centrifuge tube. 12 ml of an aqueous solution containing 200 mM N-ethyl-N'-(3-(dimethylamino)propyl)carbodiimide (EDC) and 50 mM N-hydroxysuccinimide (NHS) was added. The tube was gently agitated for 30 minutes at 23°C to activate the carboxylic acid groups in the PGA beads. The activated microcarriers were collected by centrifugation and rinsed three times with 10 ml of deionized water.
[0118] The rinsed microcarriers were resuspended in 12 ml of borate buffer (pH 9.2) containing 49 mg of vitronectin peptide (Ac-Lys-Gly-Pro-Gln-Val-Thr-Arg-Gly-Asp-Val-Phe-Thr-Met-Pro-NH2; Cat. No. 341587, available from American Peptide, Inc.) and the suspended microcarriers were allowed to react for 30 minutes with gentle agitation.
[0119] The peptide-conjugated microcarriers were collected by centrifugation and washed three times with 10 ml of PBS buffer, pH 7.4. Excess active esters were quenched by blocking with 12 ml of 1 M ethanolamine, pH 8.4, for 60 min.
[0120] The peptide-grafted and blocked microcarriers were collected and rinsed three times with PBS. After removing excess PBS, the microcarriers were rinsed twice with ethanol / water (70 / 30 v / v) and stored at 4 °C in a sterile container prior to cell culture.
[0121] Example 10-d. Static culture of hMSCs using VN-grafted microcarriers Human mesenchymal stem cells (hMSC 2637, p3) were cultured in static conditions on VN-grafted microcarrier beads prepared according to Example 19. Cells were seeded at 50k cells / well in 24-well ULA plates. Figure 12 is a phase contrast image showing hMSC cells in serum-free medium (Mesencult XF) 24 hours after seeding.
[0122] The data from Examples 10a-10d demonstrate that fully synthetic and gelatin-coated microcarriers support the attachment and proliferation of hMSCs, respectively.
[0123] Example 20. Generation of soluble microcarriers of different sizes using external gelation Polygalacturonic acid sodium salt was dissolved in water at 2%. External gelation was processed using a NISCO single nozzle vibrating encapsulation system. The beads were dropped into 4% CaCl2 dissolved in a 1:1 (v / v) mixture of ethanol and water. For the target size range, different nozzle sizes, flow rates, and vibration frequencies were used according to Table I.
[0124] [Table 1]
[0125] Example 21. Sedimentation time measurement and analysis To evaluate sedimentation rates, embodiments of microcarriers of different sizes were compared to three commercially available microcarriers: Cytodex®-1 (a cross-linked dextran-based microcarrier available from GE Healthcare Bio-Sciences, Pittsburgh, PA, USA), SoloHill® P102-1521 (a plastic cross-linked polystyrene microcarrier available from Pall Corporation, Port Washington, NY, USA), and Hillex® II (a modified polystyrene microcarrier available from Pall Corporation, Port Washington, NY, USA). These three commercially available microcarriers range from hydrogels to solid plastics and have densities ranging from 1.02 to 1.09. As described in more detail below, optical density (OD) was measured and used to determine the concentration of beads in the suspension. Microcarriers can block visible light due to obscuration. Generally, a low OD correlates with a low concentration of microcarriers in the suspension.
[0126] The method of measuring OD involves allowing the beads to settle in a cuvette in various stages. The light path used may have the bottom of the cuvette closed. The OD may change over the period of time that the microcarrier beads settle out of the solution. Generally, at the start of the measurement, the microcarrier beads are fully suspended in the solution and the light is blocked at the highest level. As the microcarrier beads begin to settle, the top of the suspension begins to become clear as the microcarrier beads move in the same direction, but the concentration of microcarrier beads in the light path remains relatively unchanged. As the microcarrier beads fall below the upper limit of the light path and begin to settle, the OD falls by half. When the microcarrier beads reach approximately the center of the light path, the time at which the microcarrier beads reach approximately the center of the light path is called t m For a fixed height of the total suspension and position in the light path, the faster the beads settle, the smaller they are. The settling velocity (defined herein as v m) is the distance that the microcarriers are from the top of the suspension to the center of the light path (herein l m The time it takes to travel (represented as t m can be estimated by This can be expressed in equation (1):
[0127]
number
[0128] In a population of microcarrier beads with non-uniform sizes, different settling velocities are expected for microcarrier beads of different sizes. Therefore, the settling velocity v m represents the media sedimentation velocity of the population.
[0129] The optical path has a width (l w ) and the microcarrier beads have a width l w The time it takes to move (t w If the population of microcarrier beads has a uniform sedimentation velocity (i.e., the microcarrier beads have a uniform size distribution), then the width of the light path, l, will be w and the settling velocity v m Using t w can be estimated as:
[0130]
number
[0131] If a population of microcarrier beads has a distribution of different sedimentation velocities (i.e. the microcarrier beads have a non-uniform size distribution), the fastest sedimenting microcarrier beads will reach the light path earlier than the slowest sedimenting microcarrier beads. As the fastest sedimenting microcarrier beads pass through the light path, a drop in OD will be observed, but a complete drop in OD will not be observed until the slowest sedimenting microcarrier beads have passed through the light path. A population of microcarrier beads with a distribution of different sedimentation velocities will have a longer t than a population of microcarrier beads with a uniform sedimentation rate. w Therefore, t w The shorter the OD, the more uniform the settling rate of the population of microcarrier beads and the more uniform the size distribution of the population of microcarriers. The above assumes that the beginning and end points of the change in OD can be determined, but it should be understood that such beginning and end points may be difficult to define. Thus, the slope of the change in OD can be used to represent the magnitude of variation in the settling rate of the population of microcarrier beads.
[0132] In practice, it is preferable to wait for all beads to completely separate from the supernatant to complete the sedimentation process. Therefore, the time to observe a complete drop in OD (represented herein as t) is more appropriate for estimating the final settling time. The final settling time can be determined using both the average settling time of a population of microcarrier beads and the variation in the settling time of a population of microcarrier beads. In a quantitative measurement, the final settling time is determined by the t m and t w or using the slope of the change in OD.
[0133] In this experiment, three types of commercially available microcarriers were rehydrated and suspended in DPBS solution. Dissolvable microcarriers (DMC) with three different sizes (250 μm, 350 μm, and 450 μm) were formed as described in experiment 1. Approximately 0.5 ml of loaded microcarriers were added to each cuvette. DPBS was then filled into the cuvette to a total volume of 3.5 ml. Just before measurement, the microcarriers were suspended by pipetting up and down 10 times. The OD was measured according to the method described above and measured at a wavelength of 400 nm. Other visible wavelengths can also be selected. The OD measurements were taken every 2.0 seconds. Because different types of microcarriers are formed from different materials, have different optical refractive indices, are different sizes, and have different optical clarity, the initial OD was used to normalize the measurements of each sample so that different samples can be compared.
[0134] The three sizes of DMC were compared with three commercially available microcarriers. The results showed that the 350 μm diameter DMC settled twice as fast as the 250 μm diameter DMC, and the 450 μm diameter DMC settled three times as fast as the 250 μm diameter DMC. By changing the size of the DMC, the settling rate could be matched to the media settling rate of three commercially available beads made of different materials and with different densities. Compared to the "Cytodex"-1 and "SoloHill" P102-1521 microcarriers, the DMCs with sizes of 250 μm and 350 μm showed comparable media settling rates but with much shorter t w As discussed in more detail in Example 21, the shorter t wThe steeper slope of the change in OD is a result of a smaller size distribution than the commercial microcarriers, providing a more consistent settling rate compared to the commercial microcarriers. Comparing the settling times t, DMC with sizes of 250 μm and 350 μm sediment faster than "Cytodex"-1 and "SoloHill" P102-1521 microcarriers, suggesting that DMC requires much less time to complete settling compared to the commercial microcarriers.
[0135] Example 21. Analysis of Microcarrier Size Distribution and Radius of Curvature The size distribution and radius of curvature of soluble microcarriers (DMC) formed according to the microcarriers with a target size of 250 μm in Example 20 were compared to three commercially available microcarriers: "Cytodex"-1, "SoloHill" P102-1521, and "Cytodex"-3 (a cross-linked dextran-based microcarrier available from GE Healthcare Bio-Sciences, Pittsburgh, PA, USA). The size of the microcarriers was determined using known optical microscopy techniques and software for analyzing images captured by an optical microscope. The radius of curvature was then calculated from the determined microcarrier size using equation (3):
[0136]
number
[0137] where K is the radius of curvature of the microcarrier and R is the radius of the microcarrier. For each type of microcarrier, Table II shows the size range d5-d95 (where d5 is the microcarrier diameter larger than the diameter of 5% of the microcarrier population and d95 is the microcarrier diameter larger than the diameter of 95% of the microcarrier population), the size range d10-d90 (where d10 is the microcarrier diameter larger than the diameter of 10% of the microcarrier population and d90 is the microcarrier diameter larger than the diameter of 95% of the microcarrier population), the size range Δd5-d95 (the difference between d95 and d5), the coefficient of variation for d5-d95, the size range Δd10-d90 (the difference between d90 and d10), and the coefficient of variation for d10-d90.
[0138] [Table 2]
[0139] For each type of microcarrier, Table III shows the average microcarrier diameter (d), the average radius of curvature (K), the radius of curvature at d5, the radius of curvature at d95, and the range of radii of curvature from d5 to d95 (the difference between the radius of curvature at d5 and the radius of curvature at d95).
[0140] [Table 3]
[0141] The data in Tables II and III show that the DMCs disclosed herein have a more uniform size distribution and a more uniform radius of curvature than the three commercially available microcarriers. As previously discussed, a uniform size distribution allows the beads to settle at a consistent rate, which allows for more predictable separation of the microcarriers from the supernatant during medium exchange or culture product separation. A uniform size distribution and uniform radius of curvature provides the same surface area available for seeding cells per microcarrier, allowing the cells to reach confluence in the same or similar time.
[0142] Example 22. Microcarrier particle number analysis The number of debris particles generated from dissolving microcarriers (DMC) formed according to the microcarriers described in Example 20 was compared to two commercially available microcarriers: "SoloHill" P102-1521 and "Cytodex"-3. Each type of microcarrier underwent multiple steps of washing before mixing to reduce particle counts to less than 2 particles per mL. For each type of microcarrier, approximately 1000 cm 2 A quantity of microcarriers was placed in separate Corning® 125 mL disposable spinner flasks (commercially available from Corning, Inc., Corning, NY, USA) and suspended in approximately 100 mL of Dulbecco's Phosphate Buffered Saline (DPBS). The two disposable spinner flasks were filled with DMC. The microcarriers were continuously stirred at room temperature at a speed of approximately 60 rpm for a total of six days. The DMC in one of the disposable spinner flasks was dissolved according to the methods described herein, while the DMC in the other disposable spinner flask did not dissolve. After stirring was completed, the microcarriers were separated from the DPBS and the particle count in the DPBS was determined according to the United States Pharmacopeia and National Formulary section 788 (USP) entitled "Particulate Matter in Injections." <788> ) was measured on a HIAC 9703+ particle counter (available from Beckman Coulter Life Sciences, Indianapolis, Indiana, USA). <788> A preparation complies with the test if the average number of particles present in the unit tested does not exceed 25 particles per mL at 10 μm or greater and does not exceed 3 particles per mL at 25 μm or greater, as shown in Table IV. Table IV shows the number of residual particles having a size of 25 μm or greater per mL of DPBS for each microcarrier containing non-soluble DMC and soluble DMC. Table V shows the number of residual particles having a size of 10 μm or greater per mL of DPBS for each microcarrier containing non-soluble DMC and soluble DMC.
[0143] [Table 4]
[0144] [Table 5]
[0145] As shown in Tables IV and V, when DMC was both soluble and insoluble, fewer DMC particles remained after agitation in the disposable spinner flask than after agitation of the other two commercially available microcarriers, even for particles with sizes greater than 10 μm and particles with sizes greater than 25 μm.
[0146] Comparative Example 1 Cultivation of Vero cells was repeated as described in Example 11, except that non-digestible "Cytodex"-3 substrate was used instead of PGA microcarriers. Trypsin was required to detach the cells from the surface of the "Cytodex"-3 beads. Fold expansion data is summarized in Figure 5. The expansion obtained using digestible microcarriers is comparable to that on "Cytodex"-3.
[0147] Comparative Example 2 The culture of MRC5 cells was repeated as described in Example 12, except that the non-digestible "Cytodex"-3 substrate was used instead of the PGA microcarriers. Trypsin was required to detach the cells from the surface of the "Cytodex" beads. The fold expansion data is summarized in Figure 6. The expansion obtained using the digestible microcarriers is comparable to that on "Cytodex"-3.
[0148] Comparative Example 3 11 is a phase contrast microscopy image of beads formed by internal gelation according to Example 1 of WO 2014 / 209865. The beads had an average diameter of 231±54 μm, which corresponds to a coefficient of variation (CV) of 23%.
[0149] The disclosed method provides an inexpensive and environmentally friendly route to prepare highly transparent PGA microcarriers that are free of undesirable inclusions and surface defects and support the separation and harvesting of non-proteolytic cells.
[0150] Characterization of by-products from PGA digestion To show the composition of the soluble microcarrier digestion, size exclusion chromatography (SEC) was used to separate the PGA polymer digestion by-products by their molecular weight. Figure 12 shows the results for each individual reagent (left) and a close-up of the data to better separate the PGA and salt peaks (right). As shown in Figure 12, each individual reagent was run as a control to determine the relative elution profile and retention time. From this, strong peaks for pectinase and EDTA were observed due to high absorbance at 214 nm. The PGA peak had the shortest retention time at 2.1 minutes, suggesting it had the highest molecular weight, and pectinase showed multiple peaks between 2.2 and 3.0 minutes consistent with a mixture of multiple enzyme components. There was some overlap between the lower molecular weight PGA peak and the pectinase peak, which may have prevented detection of the larger digestion fragments from PGA. Similarly, EDTA had a peak at 3.91 minutes due to its relatively low molecular weight of 292.17 daltons; this may have also masked the appearance of the PGA monomer and dimer peaks, which have expected molecular weights of 194.14 and 370.26 daltons, respectively.
[0151] To better illustrate the small molecule digestion by-products of PGA, an analysis of the digestion of PGA polymer with pectinase was first performed. Solutions of PGA polymer and pectinase were mixed without EDTA. As shown in Figure 13, new periodic peaks were generated at low molecular weights, most likely the result of different lengths of digested galacturonic acid oligomers, each separated by one residue. With longer digestion times, the new low molecular weight peaks became stronger, suggesting that PGA oligomers were continually digested into lower molecular weight oligomers. With longer times, the periodic peaks disappeared, and a strong low molecular weight peak appeared at 4.17 minutes. This retention time suggests that its molecular weight is lower than that of EDTA, and is likely to be a galacturonic acid monomer. Because the SEC mobile phase (e.g., Dulbecco's Phosphate Buffered Saline or DPBS) prevented the determination of the molecular weight and identity of each peak using mass spectrometry, a separate digestion solution was analyzed using electrospray ionization mass spectrometry. The results are shown in Figure 14. With increasing digestion time, an enhanced peak (m / z=193) was observed (Figure 14), supporting the SEC data that the PGA polymer is completely digested to monomer. Mass spectrometry (MS) data supports the rapid increase in the monomer peak below 15 minutes, but little change from 15 to 60 minutes. In contrast, the SEC analysis showed the greatest increase in the monomer peak after 10 minutes. While not wishing to be bound by theory, this suggests two potential explanations: (1) digestion occurs rapidly, and the different sample introduction methods used in the MS vs. SEC analyses may have introduced some lag in real time, and (2) MS peak intensity may not be as quantitatively sensitive to sample concentration as SEC absorbance.
[0152] Next, the degradation by-products of the PGA polymer were compared to those of the PGA microcarriers. When only EDTA was added, the microcarriers dissociated into PGA polymers. As shown in Figure 15, PGA peaks at approximately 2.10 min, and EDTA peaks at 3.91 and 4.03 min. When both pectinase and EDTA were added, dissociation of the microcarriers and digestion of the PGA polymer occurred simultaneously. An additional pectinase peak was observed between 2.2 and 3.0 min, with multiple periodic peaks after 3.5 min that weakened with increasing digestion time, and a single strong peak at 4.17 min corresponding to the PGA monomer (Figure 15). Unlike the SEC data from the PGA polymer, the peaks of the PGA oligomers could not be resolved between 3.85 and 4.10 min due to being hidden by the EDTA peak.
[0153] Calcium and EDTA concentrations To facilitate dissolution of PGA microcarriers, EDTA can be added to sequester and capture calcium ions, thereby destabilizing the polymer network and bead structure. Therefore, to better understand the expected amount of calcium ions released upon bead dissolution and the amount of EDTA required to sequester the released calcium ions, inductively coupled plasma mass spectrometry (ICP-MS) is combined with SEC. Samples were similarly prepared for both analyses, as described in the Methods section below. The calcium content measured by ICP-MS was 90-110 mg / L, or approximately 2.25-2.75 mM calcium ions in the digestion solution (data not shown). SEC data showed that the EDTA peak at 3.91 min was reduced by approximately 60% in the digestion solution containing 4 mM EDTA (data not shown). This is in good agreement with the ICP-MS results for the amount of calcium released. This data suggests that most of the calcium released from the dissolved microcarriers is bound to EDTA, with EDTA being in excess at 4 mM. It should be noted that existing digestion protocols may recommend 10 mM EDTA to ensure rapid digestion of the beads, however, according to embodiments of the present disclosure, much lower EDTA concentrations can be used to dissolve the beads, as evidenced by the data above.
[0154] Removal of soluble digestive components from harvested cells Soluble microcarrier digestion products include small PGA oligomers (monomers), EDTA, calcium, and pectinase. To demonstrate how these components can be separated from the cells, a series of wash and centrifugation cycles were used after harvesting according to some embodiments of the disclosed method. Cells were harvested from the lysed microcarriers by centrifugation, as described in the "Methods" section and shown in Figure 16, and 75% of the supernatant from each wash cycle was analyzed by UV-VIS spectroscopy. UV-VIS spectra of individual digestion solution reagents are shown in Figure 17A. Optical density (OD) at four different wavelengths was used to represent the characteristic spectra of the different components: 215 nm (typically used for general organics); 260 nm (typically used for DNA); 280 nm (typically used for proteins); and 400 nm in visible color. OD at 215 nm was inaccurate for undiluted samples due to oversaturation; therefore, a 1:10 dilution was used for quantitative comparison (Figure 17B). Each reagent had a unique combination of ODs at the four selected wavelengths, as shown in Figure 17C; the ratios between these ODs were used to identify each reagent in the digestion solution and further quantify their concentrations, as shown in Figure 17D. The OD values at each wavelength for the experimental samples corresponded to the additive ODs of the individual digestion reagents and PGA.
[0155] Furthermore, the drop in OD with each wash / centrifugation cycle is consistent with the theoretical 75% media reduction model, indicating that removal of digestion reagents and microcarrier by-products follows a similar dilution scheme and can be reduced through a series of wash cycles according to embodiments. Based on these results, and considering that the by-products are proteins (pectinases) and small water-soluble molecules (PGA oligomers, EDTA), tangential flow filtration or other commonly used cell purification methods will be able to remove these by-products.
[0156] Soluble by-products of dissolution of PGA microcarriers should be reduced or removed by washing. However, the ultimate fate of the adhesive substrate, Synthemax II (a synthetic peptide from the extracellular matrix protein (ECM), vitronectin), or denatured collagen was previously unknown. Therefore, residual peptides on cells were measured using anti-Synthemax II antibodies as a function of cell density. Briefly, human mesenchymal stem cells (hMSCs) were cultured at cell concentrations of 15 × 103, 30 × 103, and 40 × 103 per well. 3 , and 60×10 3 The cells were expanded to 60 × 10 cells per well and seeded on Synthemax II (S2) dissolving microcarriers (DMC). Denatured collagen (DC) DMC was seeded at 60 × 10 cells per well as a negative control. 3 DMCs were seeded with 1000 μg of cells. The cells were grown for 5 days and then harvested with a digestion solution of pectinase and EDTA. The digested cell suspension was immunostained with anti-"Synthemax" II antibody as described in the methods. Unseeded DMCs were also stained using the same method.
[0157] As shown in Figure 18, Synthemax II staining was evident in unseeded Synthemax II DMCs (NSM) when compared to negative control denatured collagen beads (NDC). Similarly, low background fluorescence was observed in cells harvested from DC DMCs (DC60). In contrast, fluorescence corresponding to Synthemax II immunodetection was observed in cells harvested from Synthemax II DMCs (S2 15, 30, and 60). Overall fluorescence signal increased with cell density; however, the amount of Synthemax II detected per cell was similar across the various conditions, based on quantitative fluorescence intensity measured using a spectrophotometer (Figure 19). Moreover, when fluorescence intensity was normalized to the total fluorescence of Synthemax II DMCs (lower graph in Figure 19), the amount of Synthemax II associated with harvested cells was 1-6% of the total Synthemax II present on the microcarriers before digestion.
[0158] According to some embodiments, the method of digesting the microcarriers can include a standard cell culture protease during digestion of the microcarriers to aid in the disruption of the cell-ECM network and promote a single cell suspension. To determine whether the addition of trypsin to the pectinase / EDTA digestion solution reduces the amount of "Synthemax" II associated with the harvested cells, several harvest conditions were compared: pectinase / EDTA (NSM PE), trypsin alone (NSM Trypsin), trypsin / pectinase / EDTA (NSM TPE), and trypsin first until the cells begin to detach from the beads, then pectinase / EDTA (NSM T+PE). Conditions were then immunostained with anti-"Synthemax" II antibody as previously done, and samples were visualized using a fluorescent microscope, as shown in FIG. 20. The use of trypsin during the cell harvesting process significantly reduced the fluorescence intensity corresponding to "Synthemax" II. Furthermore, pretreatment with trypsin followed by pectinase / EDTA solution resulted in less signal for "Synthemax" II compared to parallel treatment with trypsin / pectinase / EDTA.
[0159] Furthermore, mock digestion solutions were subjected to a series of centrifugation and washing cycles to determine whether soluble Synthemax II peptides could be detected in the DMC digestion solutions, as shown in FIG. 16. Based on dot blot analysis of anti-"Synthemax" II antibodies of samples from each washing cycle, "Synthemax" II was detected in the original digestion solution, wash 1, and wash 2 (FIG. 21). Trace amounts of "Synthemax" II were detected in wash 3, which was considered to be at the limit of detection of approximately 100 pg (5 μL blot at 20 ng / mL) based on serial dilutions of "Synthemax" II. These results confirm that soluble by-products of microcarrier dilution can be removed or reduced by washing, and that only small amounts of "Synthemax" II (<6%) are associated with the recovered cells.
[0160] Effect of digestive components on cell proliferation To demonstrate the effect of digestion by-products and reagents on subsequent cell growth, Vero cells on denatured collagen DMC were harvested and pelleted, the digestion solution was completely removed, and then reseeded in T75 flasks with fresh medium containing dilutions of the harvested digestion solution (1:5 to 1:100). Cell attachment and growth were monitored for several days. As shown in Figure 22A, Vero cell growth was significantly affected by the presence of low dilutions (1:5 to 1:10) of harvest solution, with mild inhibition of growth observed up to a 1:40 dilution. These results suggest that components that inhibit cell growth are present in the digestion solution. To further investigate the effect of pectinase and EDTA on the reseeding of Vero cells on DMC, pectinase (final concentrations of 10 to 100 U / mL) or EDTA (final concentrations of 1 to 5 mM) were spiked into disposable spinner flasks containing soluble microcarriers. Vero cells were then plated at 10,000 cells / cm. 2 Each spinner flask was then added at 100 μl for 30 min. Cells were harvested and quantified on day 3.
[0161] As shown in FIG. 22B, the presence of pectinase in the cell culture medium at a concentration of ≧40 U / mL resulted in a decrease in cell yield, with cell concentration only minimally affected (less than 10% decrease) at pectinase concentrations up to 30 U / mL. Thus, according to some embodiments, the digestion solution can be diluted more than 1:3 to minimize inhibition of cell growth due to pectinase. Similarly, EDTA had a large effect on cell growth, with concentrations of ≧2 mM affecting the integrity of DMC, which resulted in DMC dissolution (FIG. 22C). Thus, to minimize the effect of EDTA, according to some embodiments, the final concentration can be less than 1 mM.
[0162] Furthermore, addition of calcium chloride during cell reseeding failed to neutralize EDTA, and pre-equilibration of calcium chloride with cell suspensions containing EDTA prior to cell seeding had only a minor effect (data not shown). Based on these results, it would be recommended to remove the microcarrier digestion solution from the cells by centrifugation, filtration, or perfusion prior to reseeding, or to optimize microcarrier dissolution with low concentrations of pectinase and EDTA (e.g., 30 U / mL pectinase, 1 mM EDTA).
[0163] Thus, according to embodiments of this disclosure, as illustrated above, soluble components resulting from lysis of the microcarriers include: PGA monomers / oligomers, calcium, EDTA, pectinase, and surface coatings. These can be reduced or removed from the harvested cells through a series of wash / centrifugation cycles. Also, a small amount (1-6%) of residual Synthemax II coating remains associated with the harvested cells, which can be further reduced by using a protease (e.g., trypsin) during bead digestion. Furthermore, since the residual pectinase and EDTA used in digesting the microcarriers can adversely affect subsequent cell growth, methods can be used to remove or significantly reduce these components by centrifugation, filtration, or perfusion prior to cell passaging or long-term storage.
[0164] method For size exclusion chromatography, dissolved microcarriers were prepared as follows: 1 mL of concentrated digestion solution (400 U / mL pectinase ± 40 mM EDTA) was added to 1 mL of loaded hydrated DMC beads (or 1 mL of 1.75% PGA solution, containing a comparable amount of PGA material) diluted with 8 mL of Dulbecco's modified buffered saline (DPBS). A UPLC-PDA Waters Acquity H class instrument was used with the following settings: column = 4.6 x 150 mm, BEH 125 SEC (1.7 μm); column temperature = 30 °C; flow rate = 0.4 ml / min; mobile phase = 20 mM phosphate (pH 5); and injection = 10 μl.
[0165] For mass spectrometry, samples were prepared as for SEC and diluted in an acetonitrile / water mixture (1:9 v / v) to obtain a final dilution of 1:10,000. HPLC grade acetonitrile and water were purchased from FisherScientific. Electrospray ionization (ESI)-mass spectrometry (MS) experiments were performed using an Agilent 6560 ion mobility quadrupole time-of-flight system. The Agilent ion mobility system consists of a front funnel, a trapping funnel, a drift tube, and a rear funnel coupled to a Q-TOF mass spectrometer via a hexapole. Samples were directly injected into a Dual AJS (Agilent jet stream) ionization source at a flow rate of 5 μL / min for all ESI-MS experiments. The operating conditions were as follows: gas temperature: 300 °C, drying gas: 7 L / min, nebulizer pressure: 35 psi (approximately 241 kPa), sheath gas temperature: 275 °C, sheath gas flow rate: 12 L / min, VCap: 3500 V, and nozzle voltage: 2000 V. Data acquisition was collected in the mass range of 50-1700 m / z. All acquired mass spectra were accumulated and processed via MassHunter Workstation Software, version B.08.00.
[0166] For inductively coupled plasma mass spectrometry, samples were prepared as done for SEC and analyzed using an Agilent 7700s quadrupole inductively coupled plasma mass spectrometer (Q-ICP-MS) located in a class 1,000 clean room. Samples were diluted with high purity 1% HNO3 solution spiked with indium, used as an internal standard. Calcium was measured only in reaction mode (hydrogen). Sodium was measured in no gas mode (argon only) and collision mode (helium). Indium was measured in all three modes. Additional dilutions were made, if necessary, to keep the measured concentrations within the linear range of the calibration curve. The average concentrations of duplicate measurements were reported.
[0167] For the clearance study of dissolvable microcarrier by-products, human mesenchymal stem cells (hMSCs) (RoosterBio, Catalog No. MSC-001, 1 million cells) were cultured in a 200 cm2 tube in a 125 mL disposable spinner flask (Corning Catalog No. 3152) containing 50 mL of DMEM (Corning Catalog No. 15-018-CM) supplemented with 10% FBS (Corning Catalog No. 35-074-CV) and 2 mM L-glutamine (Corning Catalog No. 25-005). 2 Cells were cultured on Corning "Synthemax" II soluble microcarriers (Corning Cat. No. 4988). Dual spinner flasks without cells were used as mock controls. Cells attached to the microcarriers under intermittent agitation (3 cycles of 5 min at 30 rpm and 6 h at 0 rpm; Wheaton Micro-Stir Platform Cat. No. W900701-A); continuous agitation at 35 rpm and half-medium changes on days 3 and 5 were used to promote cell growth until day 7.
[0168] To harvest the cells from the lysed microcarriers, the contents of each spinner flask were transferred to a 50 mL conical tube and the beads were allowed to settle. The supernatant was removed and the cultures were washed twice with 20 mL of DPBS. A digestion solution consisting of 50 U / mL pectinase (Sigma, Cat. No. P2611) / 5 mM EDTA (Corning, Cat. No. 46-034-CI) in DPBS mixed 1:1 with 1× TrypLE was added to a final concentration of 10 cm 2 100μl / mL. Microcarrier digestion was checked by microscope after 10 minutes. The tubes were then centrifuged at 259×g for 5 minutes. After centrifugation, 75% of the supernatant was removed and measured in a UV-Vis spectrophotometer (Laxco UV-vis, model number: Alpha-1106). The absorbance of the samples was measured either undiluted or diluted by adding 100μl (30× dilution) or 300μl (10× dilution) in 3000μl of DPBS to ensure accurate measurements within the detection limits. DPBS was used for both the dilution medium and baseline. All samples were scanned from 200nm to 500nm. The same volume of DPBS was then used to resuspend the remaining liquid (mock sample) or the cell pellet and centrifuged again. This process was repeated for a total of four DPBS wash / centrifugation steps.
[0169] For immunostaining of hMSCs after DMC lysis, human mesenchymal stem cells were seeded onto 10 mg of soluble microcarriers per well of a ULA 6-well plate (Corning catalogue no. 3471) and cells were allowed to attach and grow on the microcarriers until the desired cell density (15,000-60,000 cells / well) was achieved. To harvest the cells, the microcarriers were transferred to a 15 mL tube, the spent culture medium was removed and washed with DPBS. The wash solution was discarded and a harvesting solution containing 50 U / mL pectinase and 5 mM EDTA was added to each suspension. Complete bead digestion was observed after 10 min. For cell harvesting using trypsin, pectinase, and EDTA, 2 mL of a mixture of 0.125% trypsin, 5 mM EDTA, and 50 U / mL pectinase was added; whereas for incubation with trypsin followed by treatment with pectinase and EDTA, 1 mL of trypsin 0.25% was added and incubated for 5 minutes, then 1 mL of 5 mM EDTA and 50 U / mL pectinase was added to the reaction for an additional 5 minutes. Released cells were pelleted at 300×g for 2 minutes and resuspended in 1 mL of DPBS.
[0170] For cell fixation and immunostaining, the cell pellet was resuspended in 500 μL of 4% formaldehyde and incubated at room temperature for 10 min. Cells were pelleted, washed with DPBS, and resuspended in 250 μL of primary antibody solution (anti-SynthemaxII polyclonal antibody in DPBS, 1:1000 dilution). Primary antibody was incubated at room temperature for 45 min. Cells were washed with 1 mL of DPBS and resuspended in 250 μL of secondary antibody solution (anti-rabbit Alexa 488 in DPBS, 1:500) at room temperature in the dark for 45 min. Cells were washed twice with 1 mL of DPBS and then resuspended in 200 μL of DPBS for fluorescence microscopy at 488 nm. Alternatively, 100 μL of stained cells (or beads) were transferred to a 96-well plate and fluorescence intensity was quantified using a spectrophotometer. Unseeded Synthemax II and denatured collagen beads were stained using the same protocol for microscopy, and the remaining beads were then dissolved in 2 mL of pectinase / EDTA harvesting solution for fluorescence measurements.
[0171] For the dot blot analysis to detect soluble "Synthemax" II, "Synthemax" II soluble microcarriers (250 mg) were hydrated in water according to standard protocols. The water was removed and replaced with 30 mL of digestion solution containing 100 U / mL pectinase and 10 mM EDTA in DPBS. After 10 min, the dissolved bead solution was spun at 125 x g for 10 min. The supernatant was discarded, leaving only 2 mL. This remaining solution was diluted and mixed with 12 mL of DPBS (wash 1). After a second centrifugation cycle, the supernatant was removed, leaving only 1 mL, and 13 mL of DPBS was added (wash 2). This sequence was repeated two more times.
[0172] A sample of each wash was collected and mixed with an equal volume of SDS-PAGE running buffer, and 5 μL was dotted onto a nitrocellulose membrane. Similarly, serial dilutions of the "Synthemax" II peptide were blotted as controls for concentration comparison. After drying the blotted samples, the membrane was saturated with 5% milk powder in TBS-Tween buffer for 30 min, washed, incubated with anti-"Synthemax" II antibody (diluted 1:1000 in TBS Tween) for 2 h, washed, and incubated with anti-rabbit secondary antibody conjugated with peroxidase for 1 h. After a final wash, the "Synthemax" II peptide was visualized using ECL substrate.
[0173] For growth of Vero cells in the presence of digestion solution reagent, Vero cells were cultured in 125 mL disposable spinner flasks at 1 cm 2 Cells were seeded in denatured collagen DMC at 10,000 cells per well for 3-5 days. Cells were harvested and cultures were centrifuged to completely remove the harvest solution. Cells were re-seeded in T-75 flasks in culture medium containing dilutions of the harvest solution (from 1:2 to 1:100 dilution). Cells were cultured in T-flasks for 5-6 days. Images of cells were captured daily. Adherent cells were quantified at the end of the culture period using a ViCell automated cell counter.
[0174] To determine the effect of pectinase and EDTA on cell growth on microcarriers, pectinase (10–100 U / mL final concentration) or EDTA (1–5 mM final concentration) was spiked into each spinner flask prior to the addition of cells (10,000 cells / cm). 2 ). Cells were continuously mixed during the cell attachment and cell proliferation phases. Images of the DMC were captured daily. Cells were harvested and quantified on days 3 or 5.
[0175] Exemplary Implementations Below are descriptions of various aspects of implementations of the disclosed subject matter. Each aspect may include one or more of various features, characteristics, or advantages of the disclosed subject matter. The implementations are intended to describe some aspects of the disclosed subject matter and should not be considered a comprehensive or exhaustive description of all possible implementations.
[0176] Aspect 1 is directed to a cell culture article comprising a substrate comprising a polygalacturonic acid compound crosslinked with a divalent cation, the polygalacturonic acid compound being selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof, the substrate being digestible by a digestive reagent into components comprising galacturonic acid monomers and divalent cations.
[0177] Aspect 2 is directed to the article of aspect 1, wherein the substrate is spherical or substantially spherical.
[0178] Example 3 is directed to the article of example 2, wherein the substrate comprises a diameter between 10 and 500 micrometers.
[0179] Aspect 4 is directed to the article of any of aspects 1 to 3, wherein the divalent cation concentration is in the range of 0.5 to 2 g / l of substrate.
[0180] Aspect 5 is directed to the article of aspect 4, wherein the divalent cation is selected from the group consisting of calcium, magnesium, and barium.
[0181] Example 6 is directed to the article of any of Examples 1 to 5, further comprising an adhesive polymer on a surface of the substrate.
[0182] Example 7 is directed to the article of example 6, wherein the adhesive polymer comprises a polypeptide.
[0183] Example 8 is directed to the article of example 6 or example 7, wherein the adhesive polymer is grafted or coated onto a surface of the substrate.
[0184] Aspect 9 is directed to the article of any of aspects 1 to 8, wherein the polygalacturonic acid compound is ionotropically crosslinked.
[0185] Aspect 10 is directed to the article of any of aspects 1 to 9, wherein the digestive reagent comprises at least one of EDTA and an enzyme.
[0186] Example 11 is directed to the article of example 10, wherein the enzyme is a pectinase.
[0187] Example 12 is directed to the article of any of Examples 6-8, wherein at least a portion of the adhesive polymer is soluble upon digestion of the substrate.
[0188] Example 13 is directed to the article of example 12, wherein the portion of the adhesive polymer that is soluble is at least about 40%, at least about 50%, at least about 60%, at least about 70%, at least about 80%, at least about 90%, or at least about 95%.
[0189] Aspect 14 is directed to a method of culturing cells, the method comprising contacting cells with a cell culture medium having a cell culture article according to any of aspects 1 to 13, and culturing the cells in the medium.
[0190] Aspect 15 is directed to a method of harvesting cultured cells, the method comprising: culturing cells on a surface of the cell culture article of any of aspects 1 to 13; and contacting the cultured cells with a mixture of pectinase and a chelating agent to separate the cells from the cell culture article.
[0191] Example 16 is directed to the method of example 15, wherein the chelating agent comprises EDTA.
[0192] Aspect 17 is directed to a method of harvesting cultured cells from a soluble substrate, the method comprising: separating the cultured cells from the substrate by digesting the substrate by exposing the substrate to (i) a chelating agent, (ii) an enzyme, or (iii) a chelating agent and an enzyme, whereby separation results in a harvest solution; and performing a series of washing and / or centrifugation cycles of the components of the harvest solution after separation, whereby the substrate comprises a polygalacturonic acid compound selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof, and an adhesive polymer on a surface of the polygalacturonic acid compound.
[0193] Example 18 is directed to the method of example 17, wherein the enzyme comprises a non-proteolytic enzyme.
[0194] Aspect 19 is directed to the method of aspect 18, wherein the non-proteolytic enzyme is selected from the group consisting of pectinase and pectinase.
[0195] Aspect 20 is directed to a method according to any of aspects 17 to 19, wherein the step of digesting the soluble substrate comprises exposing the soluble substrate to between about 1 U / mL and about 200 U / mL of enzyme, or between about 1 U / mL and about 50 U / mL, or between about 1 U / mL and about 30 U / mL, or less than about 30 U / mL of enzyme.
[0196] Aspect 21 is directed to a method of any of aspects 17 to 20, comprising exposing the dissolvable foam scaffold to a chelating agent at a concentration of less than about 10 mM, less than about 9 mM, less than about 8 mM, less than about 7 mM, less than about 6 mM, less than about 5 mM, less than about 4 mM, less than about 3 mM, less than about 2 mM, or less than about 1 mM.
[0197] Example 22 is directed to the method of any of Examples 17 to 21, wherein the chelating agent is EDTA.
[0198] Example 23 is directed to a method according to any of Examples 17 to 22, wherein after digestion, at least a portion of the adhesion polymer is soluble.
[0199] Example 24 is directed to the method of example 23, wherein the portion of the adhesive polymer that is soluble is at least about 40%, at least about 50%, at least about 60%, at least about 70%, at least about 80%, at least about 90%, or at least about 95%.
[0200] Example 25 is directed to the method of example 23 or example 24, further comprising removing the insoluble portion of the adhesion polymer by adding a protease to the harvesting solution.
[0201] Example 26 is directed to the method according to example 25, wherein the protease is trypsin.
[0202] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to a (a) "divalent cation" includes instances having two or more such "divalent cations" unless the context clearly dictates otherwise.
[0203] The terms "include" and "includes" are meant to be inclusive and not exclusive, but include but are not limited to.
[0204] "Optional" or "optionally" means that a subsequently described event, circumstance, or component may or may not occur, and the description includes instances when the event, circumstance, or component occurs and instances when it does not occur.
[0205] Ranges can be expressed herein as from "about" one particular value, and / or to "about" another particular value. When such a range is expressed, examples include from the one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, for example by use of the antecedent "about," it will be understood that the particular value forms another aspect. Moreover, it will be understood that the endpoints of each of the ranges are significant both in relation to the other endpoint, and independently of the other endpoint.
[0206] Unless otherwise expressly stated, it is in no way intended that any method described herein be construed as requiring that its steps be performed in a particular order. Thus, unless a method claim actually recites the order in which its steps are to be followed or the claim or specification specifically states that the steps are to be limited to a particular order, no particular order is intended to be inferred. Any single or multiple features or aspects recited in any one claim may be combined or permuted with other recited features or aspects recited in any other claim.
[0207] It should also be noted that enumerations herein refer to components that are "configured" or "adapted" to function in a particular way. In this regard, such components are "configured" or "adapted" to embody certain properties or function in a particular way, and such enumerations are structural enumerations rather than enumerations of intended uses. More specifically, references herein to the way in which a component is "configured" or "adapted" refer to the existing physical state of the component and, therefore, should be interpreted as an explicit enumeration of the structural features of that component.
[0208] Although various features, elements, or steps of particular embodiments may be disclosed using the transitional phrase "comprising," it should be understood that alternative embodiments are implied, including those that may be described using the transitional phrases "consisting of" or "consisting essentially of." Thus, for example, implicit alternative embodiments of a hydrocolloid solution comprising pectinic acid and water include embodiments in which the hydrocolloid solution consists of pectinic acid and water and embodiments in which the hydrocolloid solution consists essentially of pectinic acid and water.
[0209] It will be apparent to those skilled in the art that various modifications and variations can be made to the technology of the present invention without departing from the spirit and scope of the present disclosure. Since modifications, combinations, subcombinations, and variations of the disclosed embodiments incorporating the spirit and essence of the technology of the present invention may occur to those skilled in the art, the technology of the present invention should be construed as including all those within the scope of the appended claims and their equivalents.
[0210] Preferred embodiments of the present invention will be described below in detail.
[0211] EMBODIMENT 1 A cell culture article, comprising: 1. A substrate comprising a polygalacturonic acid compound cross-linked with a divalent cation, the polygalacturonic acid compound being selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof. Including, the substrate is digestible by a digestion reagent into components comprising galacturonic acid monomers and the divalent cations; Goods.
[0212] EMBODIMENT 2 2. The article of embodiment 1, wherein the substrate is spherical or substantially spherical.
[0213] EMBODIMENT 3 3. The article of embodiment 2, wherein the substrate comprises a diameter of 10 to 500 micrometers.
[0214] EMBODIMENT 4 4. The article of any one of claims 1 to 3, wherein the divalent cation concentration is in the range of 0.5 to 2 g / l of the substrate.
[0215] EMBODIMENT 5 5. The article of claim 4, wherein the divalent cation is selected from the group consisting of calcium, magnesium, and barium.
[0216] EMBODIMENT 6 6. The article of any one of the preceding claims, further comprising an adhesive polymer on the surface of the substrate.
[0217] EMBODIMENT 7 The article of embodiment 6, wherein the adhesive polymer comprises a polypeptide.
[0218] EMBODIMENT 8 8. The article of claim 6 or 7, wherein the adhesive polymer is grafted or coated onto the surface of the substrate.
[0219] EMBODIMENT 9 9. The article of any one of the preceding claims, wherein the polygalacturonic acid compound is ionotropically crosslinked.
[0220] EMBODIMENT 10 10. The article of any one of the preceding claims, wherein the digestive reagent comprises at least one of EDTA and an enzyme.
[0221] EMBODIMENT 11 11. The article of embodiment 10, wherein the enzyme is a pectinase.
[0222] EMBODIMENT 12 9. The article of any of claims 6 to 8, wherein at least a portion of the adhesive polymer becomes soluble upon digestion of the substrate.
[0223] EMBODIMENT 13 13. The article of embodiment 12, wherein the portion of the adhesive polymer that becomes soluble is at least about 40%, at least about 50%, at least about 60%, at least about 70%, at least about 80%, at least about 90%, or at least about 95%.
[0224] EMBODIMENT 14 14. A method for culturing cells, comprising contacting cells with a cell culture medium having a cell culture article according to any one of embodiments 1 to 13, and culturing the cells in the medium.
[0225] EMBODIMENT 15 1. A method for harvesting cultured cells, the method comprising: Culturing cells on the surface of the cell culture article according to any one of claims 1 to 13; and contacting the cultured cells with a mixture of pectinase and a chelating agent to separate the cells from the cell culture article. A method comprising:
[0226] EMBODIMENT 16 16. The method of embodiment 15, wherein the chelating agent comprises EDTA.
[0227] EMBODIMENT 17 1. A method for harvesting cultured cells from a soluble substrate, the method comprising: separating the cultured cells from the substrate by digesting the substrate by exposing the substrate to (i) a chelating agent, (ii) an enzyme, or (iii) a chelating agent and an enzyme, the separation resulting in a harvest solution; and performing a series of washing and / or centrifugation cycles of the components of the collection solution after said separating step. Including, the substrate comprises a polygalacturonic acid compound selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof, and an adhesive polymer on the surface of the polygalacturonic acid compound; method.
[0228] EMBODIMENT 18 18. The method of embodiment 17, wherein the enzyme comprises a non-proteolytic enzyme.
[0229] EMBODIMENT 19 19. The method of embodiment 18, wherein the non-proteolytic enzymes are selected from the group consisting of pectinolytic enzymes and pectinases.
[0230] EMBODIMENT 20 20. The method of any of embodiments 17 to 19, wherein the step of digesting the soluble substrate comprises exposing the soluble substrate to between about 1 U / mL and about 200 U / mL of the enzyme, or between about 1 U / mL and about 50 U / mL, or between about 1 U / mL and about 30 U / mL, or less than about 30 U / mL of the enzyme.
[0231] EMBODIMENT 21 21. The method of any of embodiments 17 to 20, comprising exposing the dissolvable foam scaffold to the chelating agent at a concentration of less than about 10 mM, less than about 9 mM, less than about 8 mM, less than about 7 mM, less than about 6 mM, less than about 5 mM, less than about 4 mM, less than about 3 mM, less than about 2 mM, or less than about 1 mM.
[0232] EMBODIMENT 22 22. The method of any one of embodiments 17 to 21, wherein the chelating agent is EDTA.
[0233] EMBODIMENT 23 23. The method according to any of embodiments 17 to 22, wherein after digestion, at least a portion of said adhesive polymer becomes soluble.
[0234] EMBODIMENT 24 24. The method of embodiment 23, wherein the portion of the adhesive polymer that becomes soluble is at least about 40%, at least about 50%, at least about 60%, at least about 70%, at least about 80%, at least about 90%, or at least about 95%.
[0235] EMBODIMENT 25 25. The method of embodiment 23 or 24, further comprising removing the insoluble portion of the adhesion polymer by adding a protease to the harvesting solution.
[0236] EMBODIMENT 26 26. The method of embodiment 25, wherein the protease is trypsin.
Claims
1. 1. A method for harvesting cultured cells from a dissolvable substrate, the method comprising: separating the cultured cells from the substrate by exposing the substrate to (i) a chelating agent, or (ii) a chelating agent and an enzyme to digest the substrate, the chelating agent being EDTA at a concentration of 1 mM or less, the separation resulting in a harvest solution; and performing a series of washing and / or centrifugation cycles of the components of the collection solution after said separating step. Including, the substrate comprises a polygalacturonic acid compound selected from at least one of pectinic acid, partially esterified pectinic acid, partially amidated pectinic acid, and salts thereof, and an adhesive polymer on a surface of the polygalacturonic acid compound; method.
2. 2. The method of claim 1, wherein the enzyme comprises a non-proteolytic enzyme selected from the group consisting of pectin degrading enzymes and pectinases.
3. The method of claim 1 or 2, wherein after digestion, at least a portion of the adhesive polymer becomes soluble.
4. The method of claim 3, further comprising removing the insoluble portion of the adhesive polymer by adding a protease to the harvesting solution.
Citation Information
Patent Citations
Culture of pluripotent stem cells on microcarriers
JP2012509085A
Enriched medium for hutc growth
JP2016501026A
Cell culture articles and methods thereof
JP2016523086A
Digestible substrate for cell culture
JP2018520662A
Methods and systems for harvesting cells
US20140030805A1