Laminated windows including different glass substrates having a low-E coating adjacent to a vehicle interior or building interior and / or methods for making same

A laminated window design with high-iron and low-iron glass substrates and an ITO-based coating on the inboard surface addresses the challenge of solar heat load and visibility, enhancing solar heat gain and reducing secondary heat transfer.

JP7588183B2Active Publication Date: 2024-11-21GUARDIAN GLASS LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023109158
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-04-26
Filing Date
2023-07-03
Publication Date
2024-11-21
Estimated Expiration
2038-04-24

AI Technical Summary

Technical Problem

Existing vehicle and marine glazing systems face challenges in reducing solar heat load while maintaining visible light transmission, as absorption solutions re-emit heat, and silver-based low-E coatings are costly and prone to damage.

Method used

A laminated window design with different glass substrates, where a high-iron absorption glass is on the outboard side and a low-iron transparent glass on the inboard side, combined with an ITO-based low-E coating on the inboard surface, enhances solar heat gain and reduces secondary heat transfer.

Benefits of technology

This design improves solar heat gain performance, reduces visible reflections, and maintains high visible transmission, while being durable and cost-effective compared to traditional solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588183000012
    Figure 0007588183000012
  • Figure 0007588183000013
    Figure 0007588183000013
  • Figure 0007588183000014
    Figure 0007588183000014
Patent Text Reader

Abstract

To provide a laminated glass window that absorbs more IR radiation.SOLUTION: A laminated vehicle window has different glass substrates and a low-emissivity (low-E) coating on an interior surface thereof, so that the low-E coating is to be located adjacently and exposed to the vehicle interior. In certain example embodiments, the low-E coating includes a transparent conductive oxide (TCO) layer of a material such as indium-tin-oxide (ITO). In certain example embodiments, the exterior glass substrate contains more iron and thus absorbs more IR radiation than the interior glass substrate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Certain exemplary embodiments of the present invention relate to laminated windows that may have different glass substrates. A low emissivity (Low-E) coating is provided on the inner surface of the window such that the Low-E coating is disposed adjacent to and exposed to the interior of a vehicle or building or the like. In certain exemplary embodiments, the outer / outboard and inner / inboard glass substrates of the window are laminated together. A Low-E coating, including a transparent conductive oxide (TCO) layer of a material such as indium tin oxide (ITO), is provided on the surface of the inner glass substrate facing and exposed to the vehicle / building interior. In certain exemplary embodiments, the outer glass substrate contains more iron than the inner glass substrate, and therefore absorbs more IR radiation. In certain exemplary embodiments, the Low-E coating may consist of or include a TCO layer, such as ITO, disposed between a first and a second dielectric layer, which may consist of or include silicon oxynitride, silicon nitride, and / or the like. The coating is durable enough to survive in exposed environments and also has a low enough hemispherical emissivity to enable the window to retain heat from inside the vehicle / building, thereby improving solar heat gain characteristics and / or reducing the likelihood of condensation on the coating. Summary of the Invention

[0002] For many years, vehicle, transportation, and marine glazing systems have sought to reduce the solar heat load transmitted through the glazing while maintaining a desired level of visible transmittance. The primary drivers for this have been passenger comfort, reduced air conditioning load, improved fuel economy, and reduced emissions.

[0003] Solutions often use tinted glass to reduce visible light transmission and mitigate solar heat gain in the vehicle interior. Such solutions are often called absorbing solutions because they absorb a portion of the solar spectrum, which is converted into direct heating of the glass / window assembly. Absorbing glass solutions are used in both laminated and monolithic applications, where all glass substrates are tinted. Such solutions have the advantage of reducing the directly transmitted solar energy while improving comfort. However, a major drawback of absorbing solutions is that the heat gained by the assembly is then re-emitted or re-radiated in all directions, thus transferring a portion of the heat to the interior space of the vehicle, thereby becoming a secondary source of undesirable heat. This effect of secondary heat is recognized and quantified by many standards for the calculation of solar load transmitted through glass windows, such as the NFRC Solar Heat Gain Coefficient (SHGC), or Tts (Total Solar Transmittance) according to ISO 13837. SF (G-factor, EN410-673 2011) and SHGC (NFRC-2001) values ​​are calculated from the full spectrum and can be measured with a spectrophotometer such as the Perkin Elmer 1050. In each case, these values ​​represent the sum of the direct solar transmittance component and the secondary re-radiated heat component. For example, a visible transmittance (T vis Most tinted / absorbent glass solutions with lower T typically exhibit a Tts or SHGC in the range of 53-65% compared to clear glass with a Tts or SHGC of around 80%. vis For absorbing solutions with Tts, the Tts can be even lower. For example, Tts in the range of 15-20% vis can result in a Tts or SHGC of around 40%.

[0004] Silver-based low-E coatings have also been used on vehicle windshields to improve solar heat rejection. Such silver-based low-E coatings are typically applied between the glass substrates of a laminated windshield. The advantage of silver-based low-E coatings is the fact that a significant portion of the solar energy is reflected by the window, rather than absorbed, thus mitigating most of the secondary heating. Thus, such reflective solutions typically have a comparable T vis They have a Tts approximately 8-15% lower than absorbing solutions. The disadvantages of these silver-based Low-E reflective solutions are primarily related to the cost and complexity of production at the manufacturing level. Silver-based Low-E coatings are typically soft and easily damaged during processing, and are also susceptible to damage from the heating processes used to strengthen or shape the glass. In addition, such reflective solutions also tend to significantly increase the visible reflection from one or both sides of the window, creating additional potential internal glare and undesirable outward-facing color effects. The appearance of such solutions is often quite noticeably different from the appearance of regular glass windows, and is perceived negatively in most cases.

[0005] In certain exemplary embodiments of the present invention, it has been found that applying a low-E coating having a TCO such as ITO with surface durability to the inner surface of a solar absorbing assembly improves the solar heat gain of the assembly. For example, an ITO-based coating having an emissivity of about 0.17-0.22 can provide a reduction in SHGC or Tts of at least about 0.05 (5%) absolute, more preferably at least about 0.10 (10%) absolute, compared to the absence of such a coating. Furthermore, in the case of laminated windows, it has been surprisingly found that using a hybrid including an absorbing tinted glass (e.g., a relatively high iron content glass) for the outboard glass substrate and a different low absorbing clear glass (e.g., a relatively low iron content glass) for the inboard glass substrate is advantageous in that having an ITO-based low-E coating on the surface of the inboard glass substrate facing the interior of the vehicle can further improve solar heat gain performance compared to when the same glass is used with the same coating for both substrates.

[0006] Thus, certain exemplary embodiments of the present invention relate to laminated windows (e.g., vehicle windows, marine vehicles, or building windows) having different glass substrates and an ITO-based low-emissivity (Low-E) coating on their inner surfaces such that the ITO-based Low-E coating is adjacent to and exposed to the vehicle or building interior. In certain exemplary embodiments, the outer / outboard and inner / inboard glass substrates of the window are laminated to each other via a laminating material such as polyvinyl butyral (PVB) or ethylene-vinyl acetate (EVA). In certain exemplary embodiments, the Low-E coating is not provided between the glass substrates. Instead, a Low-E coating, including a transparent conductive oxide (TCO) layer of a material such as indium tin oxide (ITO), is provided on the surface of the inner glass substrate facing and exposed to the vehicle or building interior. In certain exemplary embodiments of the present invention, the outer glass substrate contains more iron than the inner glass substrate, and therefore absorbs more IR radiation. Surprisingly, it has been found that this hybrid approach, including a relatively high iron absorbing glass substrate on the outboard side and a relatively low iron transparent glass substrate on the inboard side, when the Low-E coating is on the transparent inboard glass substrate facing the vehicle or building interior, results in a laminated window with improved solar heat gain performance compared to using the same glass for both the inboard and outboard glass substrates. In certain exemplary embodiments, the Low-E coating may consist of or include a TCO layer, such as ITO, disposed between a first dielectric layer and a second dielectric layer, which may consist of or include silicon oxynitride, silicon nitride, and / or the like. The coating is durable enough to survive in an exposed environment and also has a sufficiently low hemispherical emissivity so that the window can retain heat from the vehicle / building interior, thereby improving solar heat gain properties and / or reducing the possibility of condensation on the coating.

[0007] In certain exemplary embodiments, the ITO-based coating on at least one glass substrate may be heat treated (e.g., at a temperature of at least 580° C. for at least about 2 minutes, more preferably at least about 5 minutes) and heat strengthened and / or heat bent in this regard. Heat treatment may be used, for example, to activate the ITO-based coating and reduce its sheet resistance and emissivity, and / or may be used for heat strengthening and / or heat bending of the glass of the window. In certain exemplary embodiments of the present invention, following such heat treatment (HT), the ITO-based coating has a hemispherical emissivity of 0.40 or less (more preferably 0.30 or less, and most preferably 0.25 or less) and / or a sheet resistance (R s ).

[0008] In an exemplary embodiment of the invention, a window for a vehicle (e.g., a car, truck, train, bus, or boat) is provided, the window including first and second glass substrates laminated together via a polymer-inclusive interlayer, the first glass substrate configured to be positioned closer to an interior of the vehicle than the second glass substrate, and a multi-layer coating on the first glass substrate and configured to be positioned closer to and exposed to the interior of the vehicle, the multi-layer coating not being positioned between the first and second glass substrates, the coating having a sheet resistance (R s ), including a transparent conductive layer comprising indium tin oxide (ITO) disposed between and in direct contact with a first transparent dielectric layer and a second transparent dielectric layer, the first transparent dielectric layer being disposed between at least a first glass substrate and the transparent conductive layer comprising ITO, and the base glass composition of each of the first and second glass substrates being SiO 2 67-75%, Na 2 O 10~20%, CaO 5~15%, MgO 0~5%, Al 2 O 3 0~5%, K 2The second glass substrate contains 0 to 5% by weight of O, and the second glass substrate contains at least 0.25% more total iron (Fe 2 O 3 (represented as

[0009] In another exemplary embodiment of the invention, a window is provided, the window comprising: first and second glass substrates laminated together via a polymer-inclusive interlayer, the first glass substrate configured to be positioned closer to a vehicle or building interior than the second glass substrate; and a multi-layer coating on the first glass substrate and configured to be positioned closer to and exposed to the vehicle or building interior, the multi-layer coating being not disposed between the first glass substrate and the second glass substrate, the coating comprising a transparent conductive layer comprising indium tin oxide (ITO) disposed between and in direct contact with a first transparent dielectric layer and a second transparent dielectric layer, the first transparent dielectric layer being disposed between at least the first glass substrate and the transparent conductive layer comprising ITO, the base glass composition of each of the first and second glass substrates comprising: [Table 1] a first dielectric layer having a refractive index of 1.60 to 1.90 and a thickness of 10 to 120 nm, a layer including ITO having a thickness of 75 to 175 nm, and a second dielectric layer having a refractive index of 1.60 to 1.90 and a thickness of 10 to 120 nm, in order of increasing distance from the first glass substrate; s ) and a hemispherical emissivity of 0.30 or less, and the window has an SHGC value of 0.48 or less. These and other features and advantages may be better and more completely understood by reference to the following detailed description of the illustrative embodiments taken in conjunction with the drawings. [Brief description of the drawings]

[0010] [Figure 1] 1 is a cross-sectional view of a laminated window according to an exemplary embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view of a laminated window according to another exemplary embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view of a laminated window according to another exemplary embodiment of the present invention. [Figure 4] 1 is a cross-sectional view of a laminated window according to another exemplary embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Referring now in more detail to the accompanying drawings, like reference numerals refer to like parts throughout the several views.

[0012] Certain exemplary embodiments of the present invention relate to a laminated window (e.g., a vehicular window such as a vehicle windshield, a marine vehicle window such as on a boat, or a building window) having distinct glass substrates 1 and 2 and an ITO-based low-emissivity (Low-E) coating 20 on their inner surfaces such that the ITO-based Low-E coating 20 is positioned adjacent to and exposed to a vehicle or building interior (for illustrative purposes, a "vehicle interior" is shown in Figures 1-4). In certain exemplary embodiments, the exterior / outboard glass substrate 2 and the interior / inboard glass substrate 1 of the window are laminated together via a polymer-containing interlayer lamination material 3 such as polyvinyl butyral (PVB) or ethylene-vinyl acetate (EVA). In certain exemplary embodiments, no Low-E coating is provided between the glass substrate 1 and the glass substrate 2. Instead, a low-E coating 20, comprising a transparent conductive oxide (TCO) layer of a material such as indium tin oxide (ITO) 5, is provided on the surface of the inner glass substrate 1 that faces and is exposed to the vehicle or building interior. In certain exemplary embodiments of the invention, the outer glass substrate 2 contains more iron than the inner glass substrate 1, and therefore absorbs more IR radiation. Iron is an absorbing material in glass, and the more iron present, the more absorbing the glass is. Surprisingly, it has been found that this hybrid approach, including a relatively high iron absorbing glass substrate 2 on the outboard side and a relatively low iron transparent glass substrate 1 on the inboard side, when the Low-E coating 20 is on the transparent inboard glass substrate 1 facing the vehicle or building interior, results in a laminated window with improved solar heat gain performance compared to using the same glass for both the inboard and outboard glass substrates. In certain exemplary embodiments, the Low-E coating 20 may consist of or include a TCO layer, such as ITO 5, disposed between a first dielectric layer 9a and a second dielectric layer 9b, which may consist of or include silicon oxynitride, silicon nitride, and / or the like. The coating 20 is durable enough to survive in an exposed environment and also has a low enough hemispherical emissivity to enable the window to retain heat from the interior of the vehicle / building, thereby improving solar heat gain characteristics and / or reducing the likelihood of condensation on the coating 20.

[0013] In this specification, the total amount of iron present in glass substrates 1 and 2 is calculated according to standard practice as Fe 2 O 3 However, typically all of the iron in the glass is expressed in terms of Fe 2 O 3 Instead, iron is usually present in the ferrous state (Fe 2+ Even though not all of the ferrous state iron in the glass is in the form of FeO, it is possible to distinguish between the ferric state (represented herein as FeO) and the ferric state (Fe 3+ ) and ferrous iron (Fe 2+ , FeO) is a blue-green colorant, while ferric iron (Fe 3+ ) is a yellow-green colorant. Ferrous iron (Fe 2+ , FeO) is a strong colorant and introduces significant color into glass. Iron in the ferric state (Fe 3+) are also colorants, but iron in the ferric state tends to be a weaker colorant than its ferrous counterpart.

[0014] Glass substrates 1 and 2 in Figures 1-4 preferably utilize soda-lime-silica glass produced by the float process as their base composition / glass. In addition to the base composition / glass, a colorant portion is provided. An exemplary soda-lime-silica base glass for each of glass substrates 1 and 2 according to certain embodiments of the present invention includes the following base components, based on weight percent: [Table 2]

[0015] SO 3 Other minor components may also be included in the base glass, including various conventional refining aids such as fluoride and carbon. In certain embodiments, for example, the glasses described herein may be prepared using sodium sulfate (SO 4 ) as a refining agent. 3 % Na 2 O 3 , 5-dichloropropane, 1,2-trimethylsilane, 1,3-trimethylsilane, 1,4-trimethylsilane, 1,5-trimethylsilane, 1,6-trimethylsilane, 1,7-trimethylsilane, 1,8-trimethylsilane, 1,9 ... 2 O and about 6-12 wt.% CaO.

[0016] In addition to the base glass, the glass composition of each of the glass substrates 1 and 2 includes a colorant portion that includes iron, which is responsible for the coloring and absorption of the corresponding glass substrate 1 and 2. As mentioned above, the outer glass substrate 2 contains more iron, and therefore absorbs more radiation, than the inner glass substrate 1. Iron is an absorbing material in glass, and the more iron present, the more absorbent the glass is. In certain exemplary embodiments of the invention, the inner / inboard glass substrate 1 is a substantially transparent glass made of a relatively low iron glass, such that it is a low absorbing glass, with a total iron content of 0.001-0.20%, more preferably 0.001-0.15%, more preferably 0.005-0.12%, and most preferably 0.01-0.10% total iron (Fe 2 O 3 It should be noted that the percentage amounts of glass compositions herein are expressed as weight percent (%) of the total glass composition. In contrast, the exterior / outboard glass substrate 2 is a colored and / or tinted glass made of a relatively high iron content glass to be a highly absorbent glass, with a total iron content of at least 0.30%, more preferably at least 0.50%, even more preferably at least 0.60%, more preferably at least 0.70%, and most preferably at least 0.75% (Fe 2 O 3 In a preferred embodiment of the invention, the outboard glass substrate 2 contains at least 0.25% (more preferably at least 0.40%, even more preferably at least 0.50%, and most preferably at least 0.60%) more total iron than the inboard glass substrate 1. In a specific exemplary embodiment of the invention, the inboard glass substrate 1 has a visible transmittance (T vis ).

[0017] For example, in an exemplary embodiment of the invention, the outboard glass substrate 2 may be a green glass substrate such as SMGII or SMGIII available from Guardian Industries Corp., having a visible transmission of about 60-68% by a 2° observer with Illuminant A at a nominal thickness of 6 mm and containing a total iron content of about 0.70-0.95%, and the inboard glass substrate 1 may be a clear low iron glass substrate available from Guardian Industries Corp., having a visible transmission of about 80-91% by a 2° observer with Illuminant A at a nominal thickness of 6 mm and containing a total iron content of about 0.01-0.10%. In another exemplary embodiment of the present invention, the outboard glass substrate 2 may be a dark tinted glass substrate such as PrivaGuard available from Guardian Industries Corp., having a visible transmission of about 5-12% by a 2° observer with Illuminant A at a nominal thickness of 6 mm and containing about 1.4-1.7% total iron, and the inboard glass substrate 1 may be a clear glass substrate available from Guardian Industries Corp., having a visible transmission of about 80-91% by a 2° observer with Illuminant A at a nominal thickness of 6 mm and containing about 0.01-0.10% total iron. These examples apply to any of the embodiments shown in Figures 1-4.

[0018] For example, the transparent low iron inboard glass substrate 1 may be made of any of the low iron glass compositions described in any of U.S. Pat. Nos. 7,169,722, 7,144,837, 6,218,323, 5,030,594, 5,656,559, or 7,037,869, the disclosures of which are incorporated herein by reference, and the relatively high iron outboard glass substrate 2 may be made of any of the relatively high iron glass compositions described in any of U.S. Pat. Nos. 5,214,008, 4,792,536, 5,393,593, or 5,932,502, the disclosures of which are incorporated herein by reference.

[0019] In certain exemplary embodiments of the present invention, the low iron inboard glass substrate 1 may have a colorant portion (in terms of weight percent of the total glass composition) as set forth in the following table, where the materials set forth in Table 2 below are added to the base glass described above. [Table 3]

[0020] In certain exemplary embodiments of the present invention, the higher iron outboard glass substrate 2 may have a colorant portion (in terms of weight percent of the total glass composition) as set forth in the following table, where the materials set forth in Table 3 below are added to the base glass described above. [Table 4]

[0021] The glass substrates 1 and 2 may or may not be provided with other colorants.

[0022] It is noted that glasses according to certain exemplary embodiments of the present invention are often made by the known float process in which a tin bath is utilized. Thus, it will be understood by those skilled in the art that as a result of forming the glass on molten tin in certain exemplary embodiments, small amounts of tin or tin oxide may migrate into the surface area of ​​the glass on the side that was in contact with the tin bath during manufacture (i.e., typically, float glass may have a tin oxide concentration of 0.05 wt. % or more in the first few micrometers below the surface that was in contact with the tin bath).

[0023] In certain exemplary embodiments, the ITO-based coating 20 on at least the substrate 1 may be heat treated (e.g., at a temperature of at least 580° C. for at least about 2 minutes, more preferably at least about 5 minutes) and heat strengthened and / or heat bent in this regard. Heat treatment may be used, for example, to activate the ITO-based coating and reduce its sheet resistance and emissivity, and / or may be used for heat strengthening and / or heat bending of the glass of the window, such as in an autoclave. In certain exemplary embodiments of the present invention, following such heat treatment (HT), the ITO-based coating 20 has a hemispherical emissivity of 0.40 or less (more preferably 0.30 or less, more preferably 0.25 or less, and most preferably 0.20 or less) and / or a sheet resistance (R s ). The laminated window combines low sheet resistance and / or low emissivity with desirable visible transmittance. In certain exemplary embodiments of the invention, the visible transmittance (T vis ) is at least about 50%, more preferably at least about 60%, and even more preferably at least about 70%. Furthermore, in certain exemplary embodiments of the invention, the window has an exterior visible reflectance of 10% or less (more preferably 9% or less), and an interior visible reflectance of 10% or less (more preferably 9% or less). In certain exemplary embodiments of the invention, the window has an SHGC value of 0.75 (75%) or less, more preferably 0.50 (50%) or less, even more preferably 0.48 (48%) or less, and sometimes 0.30 (30%) or 0.27 (27%) or less.

[0024] The application of the low-E coating 20 on the inside of the non-absorbing or low absorbing glass 1 affects the solar heat gain of the system, which can be significantly improved by combining the coating 20 with the selective placement of the absorbing glass substrates 1 and 2. The application of the coating 20 in the locations shown in Figures 1-4 has at least the following advantages in the final assembly: minimal or reduced effect on the color of the system, so that it appears the same as an uncoated part to the naked eye, no significant increase in visible reflectance from both sides of the window, and in some cases a slight decrease, providing benefits with respect to internal veiling glare in certain exemplary embodiments. The durable hard coat 20 has essentially the same handling and processing durability as bare glass. Adding the coating 20 to a typical transparent laminate reduces the SHGC by about 6-7% absolute when both glass substrates are transparent and non-absorbing or low absorbing. If absorbing tinted glass is used instead of the clear glass, the improvement compared to the same tinted substrate without the coating is more, in the range of 7-10%. However, when the coating 20 is used on a hybrid laminate having a tinted absorbing outer glass substrate 2 and a low absorbing inner glass substrate 1, the SHGC reduces the overall T vis The emissivity is advantageously affected / reduced by about 1-2% absolute depending on the coating 20. It has been surprisingly found that the greater the solar absorption ratio between the glass substrates (the outer glass substrate 2 absorbs more radiation), the greater the SHGC effect. While designed to increase the U-value by reflecting IR energy back towards the interior space of the vehicle or building, this emissivity likewise selectively reduces secondary heat transfer to the interior surfaces which alters the typical energy balance seen without the coating 20.

[0025] FIG. 1 is a cross-sectional view of a laminated window according to an exemplary embodiment of the present invention. The exemplary embodiment of FIG. 1 includes a transparent, low absorbing, low iron glass substrate 1 supporting a multi-layer thin film low-E coating 20, and a more absorbing glass substrate 2 having a higher iron content. The glass substrates 1 and 2 are laminated together via a lamination interlayer 3 made of or including polyvinyl butyral (PVB) or ethylene-vinyl acetate (EVA), or the like. The coating 20 has a low hemispherical emissivity. In certain exemplary embodiments, the hemispherical emissivity of the coating 20 is 0.40 or less (more preferably 0.30 or less, more preferably 0.25 or less, and most preferably 0.20 or less). In certain exemplary embodiments, before and / or after heat treatment, the coating 20 has a sheet resistance (R s ). This is accomplished by providing a coating 20 having a thin transparent conductive oxide layer (TCO) 5 of the desired thickness, such as made of or including ITO. In the embodiment of FIG. 1, the TCO 5 is indium tin oxide (ITO).

[0026] With further reference to FIG. 1, the coating 20 may also be a silicon nitride (e.g., Si 3 N 4 The dielectric layers 9a and 9b preferably consist of or contain silicon nitride and / or silicon oxynitride, although one or both of these layers may also consist of silicon oxide (e.g., SiO 2 ) or titanium oxide (e.g., TiO 2), or other dielectric materials such as SiO 2 . Layer 9b may be both a silicon-containing barrier layer and a lower contact layer in contact with ITO 5. Both layers 9a and 9b are on the glass substrate 1 and in direct contact with ITO-containing layer 5 in certain exemplary embodiments of the present invention. Silicon nitride and / or silicon oxynitride layers 9a and 9b may be doped with about 1-10% Al, more preferably about 1-8% Al, in certain exemplary embodiments of the present invention. Transparent dielectric layers 9a and 9b, for example, when made of silicon oxynitride, are designed to have a refractive index (n, at 550 nm) of 1.60-1.90, more preferably 1.65-1.80, and most preferably 1.65-1.75. In the embodiment of FIG. 1, transparent low-E coating 20 may consist of or consist essentially of layers 9a, 5, and 9b, where layer 5 is a transparent conductive oxide and layers 9a, 9b are transparent dielectrics. However, in certain exemplary embodiments of the present invention, coating 20 may include another transparent dielectric layer, not shown, consisting of or including silicon nitride, silicon oxide, or silicon oxynitride, or the like, disposed between transparent glass substrate 1 and layer 9b.

[0027] 2 and 3 are cross-sectional views of a laminated window according to another exemplary embodiment of the present invention. The embodiment of FIGS. 2 and 3 is similar to the embodiment of FIG. 1 described above, except that in the embodiment of FIGS. 2-3, an additional protective overcoat layer 7 is provided within coating 20. Overcoat layer 7, in an exemplary embodiment of the present invention, is made of zirconium oxide (e.g., ZrO 2 or any other suitable stoichiometry), aluminum oxide, niobium oxide, titanium oxide, aluminum nitride, and / or aluminum oxynitride. Protective overcoat layer 7 is configured to be positioned adjacent to and exposed to the interior of a vehicle or building, as shown in Figures 2-3.

[0028] FIG. 4 is a cross-sectional view of a laminated window according to another exemplary embodiment of the present invention. The embodiment of FIG. 4 is the same as any of the embodiments of FIG. 1, FIG. 2, and / or FIG. 3 described above, except that in the embodiment of FIG. 4, an additional transparent dielectric layer 11 and an additional layer 13 are provided within coating 20. Layer 11 may be made of or include any of the materials described above for layers 9a and / or 9b, such as silicon nitride or silicon oxynitride. Layer 13 may be a transparent conductive oxide such as ITO in certain example exemplary embodiments, or alternatively, titanium oxide (e.g., TiO) having a refractive index of at least 2.15, and more preferably at least 2.20. 2 It may also be a high refractive index transparent dielectric layer of a material such as SiO 2 (or any other suitable stoichiometry).

[0029] The following table provides example physical thicknesses and example materials for the various layers 9a, 9b, 5, and 7 in the above-described embodiment of Figures 1-4. Other materials may have similar thicknesses. [Table 5]

[0030] In the example embodiment of Figure 1, layer 9b is made of silicon oxynitride doped with Al and is about 55 nm thick, ITO layer 5 is about 105 nm thick, and layer 9a is made of silicon oxynitride doped with Al and is about 60 nm thick. As noted above, other TCOs may be used in place of or in addition to ITO. For example, certain exemplary embodiments may incorporate an ITO / Ag / ITO sandwich in place of ITO layer 5.

[0031] Additionally or alternatively, in certain exemplary embodiments, a thin hydrophilic and / or photocatalytic coating may be applied over the top layer of coating 20. Such a layer may be anatase TiO 2, BiO, BiZr, BiSn, SnO, and / or any other suitable material. Such layers may also promote wetting and / or provide self-cleaning properties to the article.

[0032] As used herein, the terms "on" and "supported by" and the like should not be construed to mean that two elements are directly adjacent to one another unless expressly stated. In other words, a first layer may be "on" or "supported by" a second layer, even if there are one or more layers between the second layer.

[0033] The following examples according to various embodiments of the present invention were modeled with the following results: Example 1

[0034] Example 1 was a laminated vehicle window according to the embodiment of Figure 1 having a 2.5 mm thick clear low iron glass substrate 1 and a 4 mm thick green tinted higher iron glass substrate 2 laminated with a 0.76 mm thick Saflex™ R transparent PVB lamination layer 3. A coating 20 was provided on the surface of the inboard glass substrate 1 facing and exposed to the interior of the vehicle as shown in Figure 1. The coating 20 of Example 1 consisted of a 55 nm thick silicon oxynitride layer 9b, a 105 nm thick ITO layer 5, and a 60 nm thick silicon oxynitride layer 9a. In Example 1, the clear low iron inboard glass substrate 1 was coated with a SiO 2 coating having a thickness of about 71.69%, by weight percent. 2 , 13.70% Na 2 O, 9.35% CaO, 4.07% MgO, 0.41% Al 2 O 3 , 0.23% K 2 The base glass composition is composed of 0.001% total iron (Fe 2 O 3 0.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), 0.0013% chromium (Cr 2 O3 or other suitable stoichiometry), and 0.0007% erbium (Er 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of about 72.01% SiO 2 by weight percent. 2 , 13.69% Na 2 O, 8.29% CaO, 3.91% MgO, 0.72% Al 2 O 3 , 0.22% K 2 The base glass composition is composed of 0.01% total iron (Fe 2 O 3 0.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), and 0.0014% chromium (Cr 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of 70% visible transmittance, 8% exterior visible reflectance, 8% interior visible reflectance, and an SHGC value of 0.47 (47%) after heat treatment. Example 2

[0035] Example 2 differed from Example 1 in that in Example 2, both glass substrates 1 and 2 were low iron clear glass substrates and no coating 20 was provided. Thus, Example 2 was a laminated vehicle window according to the embodiment of Figure 1 having a pair of 3 mm thick clear low iron glass substrates 1 and 2 laminated together with a 0.76 mm thick Saflex™ R clear PVB lamination layer 3. In Example 2, both glass substrates 1 and 2 were, by weight percent, approximately 71.69% SiO 2 , 13.70% Na 2 O, 9.35% CaO, 4.07% MgO, 0.41% Al 2 O 3 , 0.23% K 2 The base glass composition is composed of 0.001% total iron (Fe 2 O 30.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), 0.0013% chromium (Cr 2 O 3 or other suitable stoichiometry), and 0.0007% erbium (Er 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of 89% visible transmittance, 8% exterior visible reflectance, 8% interior visible reflectance, and an SHGC value of 0.80 (80%) after heat treatment. Example 3

[0036] Example 3 differed from Example 1 in that in Example 3, both glass substrates 1 and 2 were relatively iron-rich green-tinted glass substrates. Thus, Example 3 was a laminated vehicle window according to the embodiment of FIG. 1 having a pair of 3 mm thick green-tinted relatively iron-rich glass substrates 1 and 2 laminated together with a 0.76 mm thick Saflex® R transparent PVB lamination layer 3. A coating 20 was provided on the surface of the inboard glass substrate 1 facing and exposed to the vehicle interior as shown in FIG. 1. The coating 20 in Example 3 was the same as that in Example 1. In Example 3, both glass substrates 1 and 2 were green-tinted and each contained, by weight percent, about 71.4% SiO 2 , 13.95% Na 2 O, 8.57% CaO, 4.05% MgO, 0.72% Al 2 O 3 , 0.21% K 2 The base glass composition is composed of 0.01% fluoride, 0.02% sodium hydroxide, and a small amount of mirabilite. 2 O 3 0.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), 0.0012% chromium (Cr 2 O 3 or other suitable stoichiometry), and 0.0001% erbium (Er 2 O 3or other suitable stoichiometry), and a colorant portion consisting of 67% visible transmittance, 7% exterior visible reflectance, 8% interior visible reflectance, and an SHGC value of 0.44 (44%) after heat treatment. Example 4

[0037] Example 4 differed from Example 1 in that in Example 4, both glass substrates 1 and 2 were low iron transparent glass substrates. Thus, Example 4 was a laminated vehicle window according to the embodiment of Figure 1 having a pair of 3 mm thick transparent low iron glass substrates 1 and 2 laminated together with a 0.76 mm thick Saflex™ R transparent PVB lamination layer 3. The coating 20 in Example 4 was the same as in Example 1 and in the same location as shown in Figure 1. In Example 4, both glass substrates 1 and 2 were coated with a coating of about 71.69% SiO 2 , by weight percent. 2 , 13.70% Na 2 O, 9.35% CaO, 4.07% MgO, 0.41% Al 2 O 3 , 0.23% K 2 The base glass composition is composed of 0.001% total iron (Fe 2 O 3 0.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), 0.0013% chromium (Cr 2 O 3 or other suitable stoichiometry), and 0.0007% erbium (Er 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of 86% visible transmittance, 9% exterior visible reflectance, 9% interior visible reflectance, and an SHGC value of 0.73 (73%) after heat treatment. Example 5

[0038] Example 5 was the same as Example 1, except that glass substrates 1 and 2 were reversed in position compared to Example 1. In other words, the positions of the clear glass substrate and the green glass substrate of Example 1 were swapped in Example 5, such that the clear glass was closer to the vehicle exterior and the green glass was closer to the vehicle interior in Example 5. The coating 20 remained on the inboard glass substrate in Example 5, and thus on the green glass substrate, in the position shown in FIG. 1 exposed to the vehicle interior. The window of Example 5 had a visible transmittance of 70%, an outside visible reflectance of 8%, an inside visible reflectance of 8%, and an SHGC value of 0.48 (48%) after heat treatment. Thus, surprisingly and unexpectedly, swapping the positions of the clear glass substrate and the tinted glass substrate in Examples 1 and 5 resulted in an approximately 1% lower SHGC value (compared to Example 5) when the clear glass substrate was closer to the vehicle interior in Example 1.

[0039] Comparing Example 1 with Examples 2-5 above, it can be seen that the use of low iron glass for the inboard substrate 1 and higher iron glass for the outboard substrate 2 (Example 1) combined with an ITO-based Low-E coating 20 on the surfaces exposed to the vehicle interior surprisingly resulted in a combination of acceptably high visible transmittance and low SHGC values. In particular, the SHGC value of Example 1 was lower than Examples 2 and 4-5. Surprisingly, swapping the positions of the clear and tinted glass substrates in Examples 1 and 5 resulted in about 1% lower SHGC values ​​(compared to Example 5) when the clear glass substrate in Example 1 was closer to the vehicle interior. The only difference between Example 1 and Example 5 was swapping the positions of the two glass substrates. Furthermore, while the SHGC value of Example 3 was acceptably low, the visible transmittance of Example 3 was poorer, below 70%. Thus, only Example 1 was able to achieve a combination of high visible transmittance and low SHGC. Example 6

[0040] Example 6 was a laminated vehicle window according to the embodiment of Figure 1 having a 2 mm thick clear low iron glass substrate 1 and a 5 mm thick dark tinted higher iron glass substrate 2 laminated with a 0.76 mm thick Saflex™ R transparent PVB lamination layer 3. A coating 20 was provided on the surface of the inboard glass substrate 1 facing and exposed to the vehicle interior as shown in Figure 1. The coating 20 in Example 6 was the same as in Example 1 and consisted of a 55 nm thick silicon oxynitride layer 9b, a 105 nm thick ITO layer 5, and a 60 nm thick silicon oxynitride layer 9a. In Example 6, the clear low iron inboard glass substrate 1 was coated with ... 2 , 13.70% Na 2 O, 9.35% CaO, 4.07% MgO, 0.41% Al 2 O 3 , 0.23% K 2 The base glass composition is composed of 0.001% total iron (Fe 2 O 3 0.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), 0.0013% chromium (Cr 2 O 3 or other suitable stoichiometry), and 0.0007% erbium (Er 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of about 71.78% SiO 2 by weight percent. 2 , 13.72% Na 2 O, 7.86% CaO, 3.95% MgO, 0.58% Al 2 O 3 , 0.19% K 2 The base glass composition is composed of 0 and a small amount of mirabilite, and has a total iron content of 1.60% (Fe 2 O 3 ), 0.02% cobalt (Co 3 O 4or other suitable stoichiometry), 0.01% chromium (Cr 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of 0.003% Se. The window of Example 6 had a visible transmittance of 13%, an exterior visible reflectance of 5%, an interior visible reflectance of 5%, and an SHGC value of 0.26 (26%) after heat treatment. Example 7

[0041] For purposes of comparison with Example 6, Example 7 differed from Example 6 in that the substrates were reversed. In other words, in Example 7, the clear low iron glass substrate was on the outboard side and the higher iron dark tinted glass substrate was on the inboard side. Thus, Example 7 was a laminated vehicle window having a 2 mm thick clear low iron glass substrate 2 and a 5 mm thick dark tinted higher iron glass substrate 1 laminated with a 0.76 mm thick Saflex® R transparent PVB lamination layer 3. The coating 20 was provided on the surface of the inboard glass substrate facing and exposed to the vehicle interior as shown in FIG. 1. The coating 20 in Example 7 was the same as that in Examples 1 and 6. In Example 7, the clear low iron inboard glass substrate 2 was coated with a coating of about 71.69% SiO 2 by weight percent. 2 , 13.70% Na 2 O, 9.35% CaO, 4.07% MgO, 0.41% Al 2 O 3 , 0.23% K 2 The base glass composition is composed of 0.001% total iron (Fe 2 O 3 0.0002% Cobalt (Co 3 O 4 or other suitable stoichiometry), 0.0013% chromium (Cr 2 O 3 or other suitable stoichiometry), and 0.0007% erbium (Er 2 O 3or other suitable stoichiometry), and a colorant portion consisting of about 71.78% SiO 2 by weight percent. 2 , 13.72% Na 2 O, 7.86% CaO, 3.95% MgO, 0.58% Al 2 O 3 , 0.19% K 2 The base glass composition is composed of 0 and a small amount of mirabilite, and has a total iron content of 1.60% (Fe 2 O 3 ), 0.02% cobalt (Co 3 O 4 or other suitable stoichiometry), 0.01% chromium (Cr 2 O 3 or other suitable stoichiometry), and a colorant portion consisting of 0.003% Se. The window of Example 7 had a visible transmittance of 13%, an exterior visible reflectance of 5%, an interior visible reflectance of 5%, and an SHGC value of 0.28 (28%) after heat treatment.

[0042] Comparing Examples 6 and 7, it was found surprisingly and unexpectedly that the SHGC value in Example 6 was lower compared to Example 7, where the only difference between the examples was the location of the corresponding substrates. In Example 6, the clear glass substrate was on the inboard side and the higher iron dark absorbing glass substrate was on the outboard side. In contrast, in Example 7, the clear glass substrate was on the outboard side and the higher iron dark absorbing glass substrate was on the inboard side. Thus, it can be seen that the use of low iron glass for the inboard substrate 1 and higher iron glass for the outboard substrate 2 (Example 6), combined with an ITO based Low-E coating 20 on the surfaces exposed to the vehicle interior, surprisingly resulted in a combination of desirable visible transmittance and a surprisingly low SHGC value (0.26 for Example 6 compared to 0.28 for Example 7).

[0043] Although the present invention has been described in connection with what are presently considered to be practical and preferred embodiments, it should be understood that the present invention is not limited to the disclosed embodiments, but rather is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims. For example, while the two glass substrates are preferably different in preferred embodiments of the present invention (see, e.g., Examples 1 and 5 above), in alternative embodiments of the present invention, glass substrates 1 and 2 may be the same or essentially the same, and / or both glass substrates may be either clear or tinted in certain alternative embodiments of the present invention (see, e.g., other examples above).

[0044] In an exemplary embodiment of the invention, a window for a vehicle (e.g., a car, truck, train, bus, or boat) is provided, the window including first and second glass substrates laminated together via a polymer-inclusive interlayer, the first glass substrate configured to be positioned closer to an interior of the vehicle than the second glass substrate, and a multi-layer coating on the first glass substrate and configured to be positioned closer to and exposed to the interior of the vehicle, the multi-layer coating not being positioned between the first and second glass substrates, the coating having a sheet resistance (R s ), including a transparent conductive layer comprising indium tin oxide (ITO) disposed between and in direct contact with a first transparent dielectric layer and a second transparent dielectric layer, the first transparent dielectric layer being disposed between at least a first glass substrate and the transparent conductive layer comprising ITO, and the base glass composition of each of the first and second glass substrates being SiO 2 67-75%, Na 2 O 10~20%, CaO 5~15%, MgO 0~5%, Al 2 O 3 0~5%, K 2 The second glass substrate contains 0 to 5% by weight of O, and the second glass substrate contains at least 0.25% more total iron (Fe 2 O3 (represented as

[0045] In the vehicle window described in the immediately preceding paragraph, the second glass substrate may contain at least 0.40% more total iron than the first glass substrate.

[0046] In the vehicle window according to either of the two paragraphs above, the second glass substrate may contain at least 0.50% (more preferably at least 0.60%) more total iron than the first glass substrate.

[0047] In the vehicle window according to any of the three paragraphs above, the first glass substrate may have a visible transmittance at a nominal thickness of 6 mm that is at least 10% (more preferably at least 15% and most preferably at least 20%) higher than the visible transmittance of the second glass substrate (illuminant A, 2° observer).

[0048] In the vehicle window described in any of the above four paragraphs, in certain embodiments, no Low-E coating is provided between the first glass substrate and the second glass substrate.

[0049] In the vehicle window described in any of the above five paragraphs, the first and second dielectric layers may be silicon-based and may include at least one of oxygen and nitrogen.

[0050] In the vehicle window according to any of the above six paragraphs, the first and second dielectric layers may each comprise silicon nitride and / or silicon oxynitride.

[0051] In the vehicle window described in any of the seven paragraphs above, the coating may further comprise an overcoat comprising a metal oxide, such as zirconium oxide, aluminum oxide, or aluminum oxynitride, which in a preferred embodiment consists of or comprises an oxide of zirconium.

[0052] In the vehicle window described in any of the above eight paragraphs, the coating may further include another dielectric layer (e.g., silicon nitride, silicon oxide, and / or silicon oxynitride) disposed between at least the first glass substrate and the first dielectric layer.

[0053] In the vehicle window according to any of the above nine paragraphs, the layer comprising ITO may have a refractive index (n) of 1.80 to 1.93.

[0054] In the vehicle window according to any of the ten paragraphs above, the coating may comprise, in order moving away from the first glass substrate, a first dielectric layer, the first dielectric layer may comprise silicon oxynitride and may have a refractive index of 1.60 to 1.90 and a thickness of 10 to 120 nm; a layer comprising ITO, the ITO comprising layer may have a thickness of 40 to 200 nm; and a second dielectric layer, the second dielectric layer may comprise silicon oxynitride and may have a refractive index of 1.60 to 1.90 and / or a thickness of 10 to 120 nm.

[0055] In the vehicle window according to any of the above eleven paragraphs, the coating may comprise, in order moving away from the first glass substrate, a first dielectric layer, which may comprise silicon oxynitride and may have a refractive index of 1.65 to 1.80 and a thickness of 40 to 85 nm; a layer comprising ITO, which may have a thickness of 75 to 175 nm; and a second dielectric layer, which may comprise silicon oxynitride and may have a refractive index of 1.65 to 1.80 and / or a thickness of 40 to 80 nm.

[0056] In the vehicle window according to any of the twelve paragraphs above, the tinting agent portion of the first glass substrate has a total iron content (Fe 2 O 3 and the colorant portion of the second glass substrate may comprise a total iron content (Fe 2 O 3 (represented as:

[0057] In the vehicle window according to any of the above thirteen paragraphs, the tinting agent portion of the first glass substrate has a total iron content (Fe 2 O 3 and the colorant portion of the second glass substrate may comprise a total iron content (Fe 2 O 3 (represented as:

[0058] In the vehicle window according to any of the above 14 paragraphs, the tinting agent portion of the first glass substrate has a total iron content (Fe 2 O 3 and the colorant portion of the second glass substrate may comprise a total iron content (Fe 2 O 3 (represented as:

[0059] In the vehicle window according to any of the above 15 paragraphs, the tinting agent portion of the first glass substrate has a total iron content (Fe 2 O 3 and the colorant portion of the second glass substrate may comprise a total iron content (Fe 2 O 3 (represented as:

[0060] In the vehicle window described in any of the above 16 paragraphs, the first glass substrate may be a clear glass substrate and the second glass substrate may be a tinted (e.g., green tinted and / or dark / black / gray tinted) glass substrate.

[0061] In the vehicle window described in any of the 17 paragraphs above, the polymer-containing interlayer may include PVB.

[0062] In any of the above 18 paragraphs, the vehicle window has a sheet resistance (R s), and / or a hemispherical emissivity of 0.30 or less.

[0063] In any of the above 19 paragraphs, the vehicle window has a sheet resistance (R s ), and / or a hemispherical emissivity of 0.20 or less.

[0064] In the vehicle window described in any of the above 20 paragraphs, the window may have an SHGC value of 0.48 or less.

[0065] In a vehicle window according to any of the above 21 paragraphs, the window may have a visible transmittance (Illuminant A, 2° observer) of at least 70% and / or a SHGC value of 0.48 or less.

[0066] In the vehicle window according to any of the above 22 paragraphs, at least the coating and the first glass substrate may be heat treated. The second glass substrate may also be heat treated during heat strengthening and / or during heat bending / lamination of the two glass substrates.

Claims

1. A vehicle window, comprising: A first and a second glass substrate laminated to each other via a polymer-containing interlayer, the first glass substrate being configured to be positioned closer to an interior of a vehicle than the second glass substrate; a multi-layer coating on the first glass substrate and configured to be positioned proximate to and exposed to a vehicle interior, wherein the multi-layer coating is not disposed between the first glass substrate and a second glass substrate; The coating has a sheet resistance (R s a transparent conductive layer comprising indium tin oxide (ITO) disposed between and in direct contact with a first transparent dielectric layer and a second transparent dielectric layer, the first transparent dielectric layer being disposed between at least the first glass substrate and the transparent conductive layer comprising ITO; The base glass composition of each of the first and second glass substrates comprises: [Table 1] The second glass substrate has a total iron content (Fe) that is at least 0.40% greater than that of the first glass substrate. 2 O 3 wherein the first glass substrate having a low total iron content is an inboard glass substrate and is less absorbing than the second glass substrate, which is an outboard glass substrate, so as to reduce the SHGC value of the vehicle window; A vehicle window, wherein the coating is formed to reduce the total solar transmittance (Tts) of the window by at least 5% absolute compared to if no coating was provided, while also ensuring that the window has a visible transmittance of at least 70% (Illuminant A, 2° observer).

2. 10. The vehicle window of claim 1, wherein the second glass substrate contains at least 0.50% more total iron than the first glass substrate.

3. 10. The vehicle window of claim 1, wherein the second glass substrate contains at least 0.60% more total iron than the first glass substrate.

4. 2. The vehicle window of claim 1, wherein the first glass substrate has a visible transmittance at a nominal thickness of 6 mm that is at least 10% higher than the visible transmittance of the second glass substrate (Illuminant A, 2° observer).

5. 2. The vehicle window of claim 1, wherein the first glass substrate has a visible transmittance at a nominal thickness of 6 mm that is at least 15% higher than the visible transmittance of the second glass substrate (Illuminant A, 2° observer).

6. 2. The vehicle window of claim 1, wherein the first glass substrate has a visible transmittance at a nominal thickness of 6 mm that is at least 20% greater than the visible transmittance of the second glass substrate (Illuminant A, 2° observer).

7. 2. The vehicle window of claim 1, wherein there is no Low-E coating between the first and second glass substrates.

8. 10. The vehicle window of claim 1, wherein the first and second transparent dielectric layers are silicon-based and contain at least one of oxygen and nitrogen.

9. 10. The vehicle window of claim 1, wherein the first and second transparent dielectric layers each comprise silicon nitride.

10. 10. The vehicle window of claim 1, wherein the first and second transparent dielectric layers each comprise silicon oxynitride.

11. 10. The vehicle window of claim 1, wherein the coating further comprises an overcoat comprising a metal oxide.

12. 12. The vehicle window of claim 11, wherein the overcoat comprises an oxide of zirconium.

13. 10. The vehicle window of claim 1, wherein the coating further comprises another dielectric layer disposed at least between the first glass substrate and the first transparent dielectric layer.

14. 2. The vehicle window of claim 1, wherein the layer comprising ITO has a refractive index (n) of 1.80 to 1.

93.

15. The coatings, in order of increasing distance from the first glass substrate, the first transparent dielectric layer comprising silicon oxynitride, having a refractive index between 1.60 and 1.90, and having a thickness between 10 and 120 nm; the layer comprising ITO, the layer comprising ITO having a thickness of 40 to 200 nm; 2. The vehicle window of claim 1, comprising: a second transparent dielectric layer comprising silicon oxynitride, having a refractive index of 1.60 to 1.90, and having a thickness of 10 to 120 nm.

16. The coatings, in order of increasing distance from the first glass substrate, the first transparent dielectric layer comprising silicon oxynitride, having a refractive index between 1.65 and 1.80, and having a thickness between 40 and 85 nm; a layer comprising ITO, the layer comprising ITO having a thickness of 75 to 175 nm; 2. The vehicle window of claim 1, comprising: a second transparent dielectric layer comprising silicon oxynitride, having a refractive index of 1.65 to 1.80, and having a thickness of 40 to 80 nm.

17. The colorant portion of the first glass substrate has a total iron content of 0.001 to 0.20% (Fe 2 O 3 and the colorant portion of the second glass substrate comprises a total iron content (Fe) of at least 0.30%. 2 O 3 2. The vehicle window of claim 1, comprising:

18. The colorant portion of the first glass substrate has a total iron content of 0.001 to 0.20% (Fe 2 O 3 and the colorant portion of the second glass substrate comprises a total iron content (Fe 2 O 3 2. The vehicle window of claim 1, comprising:

19. The colorant portion of the first glass substrate has a total iron content of 0.001 to 0.15% (Fe 2 O 3 ) and the colorant portion of the second glass substrate comprises a total iron content (Fe 2 O 3 2. The vehicle window of claim 1, comprising:

20. The colorant portion of the first glass substrate has a total iron content of 0.01 to 0.10% (Fe 2 O 3 ) and the colorant portion of the second glass substrate comprises a total iron content (Fe 2 O 3 2. The vehicle window of claim 1, comprising:

21. the colorant portion of the first glass substrate comprising: [Table 2] 10. The vehicle window of claim 1, wherein the tint portion of the second glass substrate comprises: [Table 3]

22. the colorant portion of the first glass substrate comprising: [Table 4] 10. The vehicle window of claim 1, wherein the tint portion of the second glass substrate comprises: [Table 5]

23. 2. The vehicle window of claim 1, wherein the first glass substrate is a clear glass substrate and the second glass substrate is a tinted glass substrate.

24. 10. The vehicle window of claim 1, wherein the polymer-containing interlayer comprises PVB.

25. The coating has a sheet resistance (R s 10. The vehicle window of claim 1, having a hemispherical emissivity of 0.30 or less.

26. The coating has a sheet resistance (R s 10. The vehicle window of claim 1, wherein the window has a hemispherical emissivity of 0.20 or less.

27. 10. The vehicle window of claim 1, wherein the window has an SHGC value of 0.48 or less.

28. The vehicle window of claim 1 , wherein at least the coating and the first glass substrate are heat treated.

29. A window, a first glass substrate and a second glass substrate laminated together via a polymer-inclusive interlayer, the first glass substrate configured to be positioned closer to a vehicle or building interior than the second glass substrate, the first glass substrate having a total iron content that is at least 0.40% less than the second glass substrate, the first glass substrate being an inboard glass substrate and being less absorbing than the second glass substrate; a multi-layer coating on the first glass substrate and configured to be positioned proximate to and exposed to a vehicle or building interior, wherein the coating is not positioned between the first glass substrate and a second glass substrate; the coating includes a transparent conductive layer comprising indium tin oxide (ITO) disposed between and in direct contact with a first transparent dielectric layer and a second transparent dielectric layer, the first transparent dielectric layer being disposed between at least the first glass substrate and the transparent conductive layer comprising ITO; The base glass composition of each of the first and second glass substrates comprises: [Table 6] No Low-E coating is provided between the first glass substrate and the second glass substrate; the first and second transparent dielectric layers are silicon-based and contain at least one of oxygen and nitrogen; the coatings, in order moving away from the first glass substrate, include: the first transparent dielectric layer, the first transparent dielectric layer having a refractive index of 1.60 to 1.90 and a thickness of 10 to 120 nm; a layer comprising ITO, the layer comprising ITO having a thickness of 75 to 175 nm; the second transparent dielectric layer, the second transparent dielectric layer having a refractive index of 1.60 to 1.90 and a thickness of 10 to 120 nm; The coating has a sheet resistance (R s ) and a hemispherical emissivity of 0.30 or less; A window, the window having an SHGC value of 0.48 or less.

30. 30. The window of claim 29, wherein the first and second transparent dielectric layers each comprise silicon oxynitride.

31. 30. The window of claim 29, wherein the coating further comprises an overcoat comprising an oxide of zirconium.

32. The coating has a sheet resistance (R s 30. The window of claim 29, having a hemispherical emissivity of 0.20 or less, and / or a hemispherical emissivity of 0.10 or less.

33. 30. The window of claim 29, wherein the window has a visible transmission (Illuminant A, 2 degree observer) of at least 70%.

Citation Information

Patent Citations

  • Laminated glass

    JP2002173346A

  • solar control glazing

    JP2007527353A

  • Products containing condensation prevention and / or low emissivity coatings and / or methods for manufacturing the same

    JP2015504035A

  • Heat treatable article with screen and / or inkjet printed coating thereon, and / or method of making the same

    US20140370209A1

  • Laminated glazing for solar control

    WO2016202799A1