Battery

The battery design with an insulating layer between the current collector and electrode material addresses reliability and energy density issues by ensuring flush side surfaces and precise area adjustment, resulting in a highly reliable battery with enhanced energy density and simplified manufacturing.

JP7588327B2Active Publication Date: 2024-11-22PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021566782
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-04-14
Publication Date
2024-11-22
Estimated Expiration
2040-04-14

AI Technical Summary

Technical Problem

Existing battery technologies face challenges in achieving high reliability and energy density due to difficulties in precisely controlling the area of the positive and negative electrode active material layers, leading to issues such as metal precipitation, dendrite growth, and uneven compression during manufacturing, which increases equipment costs and reduces volumetric energy density.

Method used

The battery design includes an insulating layer between the current collector and the electrode active material layer, ensuring the side surfaces of the insulating and electrode layers are flush, allowing for precise adjustment of the insulating layer area by cutting, thereby preventing exposure of the electrode material and reducing the positive electrode area, thus suppressing dendrite growth and enhancing reliability while increasing energy density.

Benefits of technology

This design results in a highly reliable battery with improved volumetric energy density by minimizing the positive electrode area, preventing short circuits, and ensuring uniform compression of layers, while simplifying the manufacturing process and reducing equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588327000001
    Figure 0007588327000001
  • Figure 0007588327000002
    Figure 0007588327000002
  • Figure 0007588327000003
    Figure 0007588327000003
Patent Text Reader

Abstract

The present disclosure provides a battery which has high reliability. A battery (50) according to the present disclosure is provided with an electrode layer (10), a counter electrode layer (20) that is arranged so as to face the electrode layer (10), and a solid electrolyte layer (30) that is positioned between the electrode layer (10) and the counter electrode layer (20). The electrode layer (10) comprises a collector (11), an electrode active material layer (12) that is positioned between the collector (11) and the solid electrolyte layer (30), and an insulating layer (13) that is positioned between the collector (11) and the electrode active material layer (12) at an end of the electrode layer (10); the counter electrode layer (20) comprises a counter electrode active material layer (22) that is arranged so as to face the electrode active material layer (12); the electrode active material layer (12) has a region that does not overlap with the insulating layer (13) when viewed in plan; and a lateral surface of the insulating layer (13) and a lateral surface of the electrode active material layer (12) are flush with each other.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to batteries. [Background technology]

[0002] Patent Documents 1 and 2 disclose batteries equipped with insulating members. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2012 / 164642 [Patent Document 2] JP 2016-207286 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the prior art, there is a need for improved battery reliability. Therefore, an object of the present disclosure is to provide a highly reliable battery. [Means for solving the problem]

[0005] A battery according to one aspect of the present disclosure includes an electrode layer, a counter electrode layer disposed opposite the electrode layer, and a solid electrolyte layer located between the electrode layer and the counter electrode layer, the electrode layer having a current collector, an electrode active material layer disposed between the current collector and the solid electrolyte layer, and an insulating layer disposed between the current collector and the electrode active material layer at an end of the electrode layer, the counter electrode layer having a counter electrode active material layer disposed opposite the electrode active material layer, the electrode active material layer having a region that does not overlap with the insulating layer in a planar view, and a side surface of the insulating layer and a side surface of the electrode active material layer are flush with each other. Effect of the Invention

[0006] According to the present disclosure, a highly reliable battery can be provided. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic top view showing an example of a battery according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an example of a battery according to a comparative example. [Figure 4] FIG. 4 is a schematic cross-sectional view showing another example of a battery according to a comparative example. [Diagram 5] FIG. 5 is a flowchart illustrating a method for manufacturing the battery according to the first embodiment. [Figure 6A] FIG. 6A is a schematic diagram showing an example of a current collector on which insulating layers according to the first embodiment are stacked. [Figure 6B] FIG. 6B is a schematic diagram showing another example of the current collector on which the insulating layer according to the first embodiment is laminated. [Figure 6C] FIG. 6C is a schematic diagram showing another example of the current collector on which the insulating layer according to the first embodiment is laminated. [Figure 7A] FIG. 7A is a schematic cross-sectional view showing an example of a laminated electrode plate according to the first embodiment. [Figure 7B] FIG. 7B is a schematic cross-sectional view showing another example of the laminated electrode plate according to the first embodiment. [Figure 7C] FIG. 7C is a schematic cross-sectional view showing another example of the laminated electrode plate according to the first embodiment. [Figure 8] FIG. 8 is a diagram for illustrating a cutting step in the manufacturing method of the battery according to the first embodiment. [Figure 9] FIG. 9 is a schematic cross-sectional view showing an example of a battery according to Modification 1 of Embodiment 1. As shown in FIG. [Figure 10] FIG. 10 is a schematic cross-sectional view showing another example of the battery according to the first modification of the first embodiment. [Figure 11] FIG. 11 is a diagram illustrating a cutting step in the battery manufacturing method according to the first modification of the first embodiment. [Figure 12]FIG. 12 is a schematic cross-sectional view showing an example of a battery according to the second embodiment. [Figure 13] FIG. 13 is a schematic cross-sectional view showing another example of the battery according to the second embodiment. [Figure 14] FIG. 14 is a flowchart illustrating a method for manufacturing a battery according to the second embodiment. [Figure 15] FIG. 15 is a schematic cross-sectional view showing an example of a multilayer electrode plate according to the second embodiment. [Figure 16] FIG. 16 is a schematic cross-sectional view showing an example of a laminated electrode plate according to a first modification of the second embodiment. [Figure 17] FIG. 17 is a schematic cross-sectional view showing an example of a multilayer electrode plate according to a first modification of the second embodiment. [Figure 18] FIG. 18 is a diagram for illustrating a current collector stacking step and a cutting step in the battery manufacturing method according to the first modification of the second embodiment. [Figure 19] FIG. 19 is a schematic cross-sectional view showing an example of a laminated electrode plate having an insulating layer according to Modification 2 of Embodiment 2. As shown in FIG. [Figure 20] FIG. 20 is a schematic cross-sectional view showing an example of a laminated electrode plate having no insulating layer according to Modification 2 of Embodiment 2. As shown in FIG. [Figure 21] FIG. 21 is a schematic cross-sectional view showing an example of a multilayer electrode plate according to the second modification of the second embodiment. [Figure 22] FIG. 22 is a schematic cross-sectional view showing another example of a laminated electrode plate according to the second modification of the second embodiment. [Diagram 23] FIG. 23 is a schematic cross-sectional view showing an example of a battery according to Modification 2 of Embodiment 2. As shown in FIG. [Figure 24] FIG. 24 is a schematic cross-sectional view showing another example of the battery according to Modification 2 of Embodiment 2. As shown in FIG. [Diagram 25] FIG. 25 is a schematic cross-sectional view showing an example of a battery according to the third embodiment. [Figure 26] FIG. 26 is a schematic cross-sectional view showing another example of the battery according to the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] (Findings on which this disclosure is based) When manufacturing a battery such as an all-solid-state battery having a solid electrolyte layer containing a solid electrolyte, the area of ​​the negative electrode active material layer is generally made larger than the area of ​​the positive electrode active material layer. This is for the purpose of stabilizing the performance of the battery by making the capacity of the negative electrode active material layer larger than the capacity of the positive electrode active material layer and suppressing the precipitation of metal derived from metal ions not incorporated in the negative electrode active material layer, thereby improving the reliability of the battery. In addition, it is also for the purpose of improving the reliability of the battery by suppressing the electric field concentration at the end of the negative electrode active material layer and suppressing dendrite growth (precipitation of metal) at the end. In addition, when the area of ​​the negative electrode active material layer is increased, for example, a solid electrolyte layer is disposed around the positive electrode active material layer disposed opposite to it. As a result, the positive electrode active material layer is not in contact with the end of the current collector which is easily peeled off, so that the reliability is also improved by suppressing the exposure of the positive electrode active material layer even if the end of the current collector is peeled off.

[0009] However, it is difficult to manufacture a battery by precisely controlling the area of ​​the positive electrode active material layer and the area of ​​the negative electrode active material layer. Alternatively, in order to ensure reliability, it is necessary to form the positive electrode active material layer while taking into consideration the dimensional accuracy when forming the positive electrode active material layer. Therefore, there is a problem that the positive electrode active material layer becomes small and the volume energy density of the battery decreases. In addition, in order to increase the dimensional accuracy of the positive electrode active material layer, there is a concern that the number of steps such as inspection and the equipment cost will increase.

[0010] In view of this, the present disclosure provides a highly reliable battery, particularly a highly reliable battery having an increased energy density.

[0011] An outline of one aspect of the present disclosure is as follows.

[0012] A battery according to one aspect of the present disclosure includes an electrode layer, a counter electrode layer disposed opposite the electrode layer, and a solid electrolyte layer located between the electrode layer and the counter electrode layer, the electrode layer having a current collector, an electrode active material layer disposed between the current collector and the solid electrolyte layer, and an insulating layer disposed between the current collector and the electrode active material layer at an end of the electrode layer, the counter electrode layer having a counter electrode active material layer disposed opposite the electrode active material layer, the electrode active material layer having a region that does not overlap with the insulating layer in a planar view, and a side surface of the insulating layer and a side surface of the electrode active material layer are flush with each other.

[0013] As a result, there is a region at the end of the electrode layer where the current collector, the insulating layer, and the electrode active material layer are laminated in this order. Therefore, even if the current collector peels off at the end of the current collector where peeling is likely to occur, exposure of the electrode active material layer is suppressed, and damage or short circuit caused by contact between the electrode active material layer and other members is unlikely to occur. Therefore, the reliability of the battery can be improved.

[0014] In addition, since the side surface of the insulating layer and the side surface of the electrode active material layer are flush with each other, the area of ​​the insulating layer can be easily adjusted by cutting the insulating layer and the electrode active material layer together, for example. Therefore, although the presence of the insulating layer suppresses the exchange of electrons between the electrode active material layer and the current collector, forming a region in which the electrode active material layer does not easily function as an electrode, the region can be minimized by adjusting the area of ​​the insulating layer. Therefore, the volumetric energy density of the battery can be increased.

[0015] Furthermore, for example, the electrode layer may be a positive electrode layer, and the counter electrode layer may be a negative electrode layer.

[0016] As a result, the electrode active material layer in the region overlapping with the insulating layer in plan view, i.e., the positive electrode active material layer, does not receive electrons directly from the current collector, so the positive electrode active material layer in this region does not function as an electrode. Therefore, the effect of substantially reducing the area of ​​the positive electrode active material layer is obtained. As a result, the area of ​​the positive electrode active material layer is likely to be substantially smaller than the area of ​​the counter electrode active material layer of the negative electrode layer, i.e., the area of ​​the negative electrode active material layer. Therefore, the capacity of the negative electrode active material layer is likely to be larger than the capacity of the positive electrode active material layer, so that the precipitation of metal derived from metal ions not incorporated into the negative electrode active material layer is suppressed, and the reliability of the battery can be further improved.

[0017] For example, the insulating layer may include a resin.

[0018] This allows the resin contained in the insulating layer to have an anchor effect by penetrating into the current collector and the electrode active material layer, thereby improving the bonding between the insulating layer and the current collector and the electrode active material layer, and suppressing peeling between the insulating layer and the current collector and the electrode active material layer.

[0019] For example, the insulating layer may include a metal oxide.

[0020] This makes the insulating layer hard, so that even if the insulating layer is formed thin during battery production, the insulating layer is less likely to deform when stacked with other layers, and a thin insulating layer of uniform thickness can be formed.

[0021] Furthermore, for example, the insulating layer may be located in a region that is 1 mm or less in length from the outer periphery of the electrode active material layer in a plan view.

[0022] This makes it possible to confine the area in which the electrode active material layer is less likely to function as an electrode due to the presence of the insulating layer to a range within a certain distance from the outer periphery of the electrode active material layer, thereby increasing the volumetric energy density of the battery.

[0023] For example, the insulating layer may have a thickness of 5 μm or less.

[0024] This makes the insulating layer located between the current collector and the electrode active material layer thinner. Therefore, even when a high-pressure press is performed on each layer of the battery stacked on the current collector for the purpose of increasing the volumetric energy density of the battery, the insulating layer can reduce the effect of the press on each layer, and each layer, such as the electrode active material layer, can be compressed uniformly. As a result, the possibility of each layer being compressed non-uniformly and peeling off can be reduced. Therefore, a highly reliable battery can be realized while increasing the energy density.

[0025] Furthermore, for example, the side surfaces of the solid electrolyte layer, the current collector, the electrode active material layer, the counter electrode active material layer, and the insulating layer may each be exposed.

[0026] This allows each layer that contributes to the charge / discharge performance of the battery to be present all the way to the ends of the battery, thereby increasing the volumetric energy density of the battery.

[0027] Furthermore, for example, a side surface of the electrode layer, a side surface of the counter electrode layer, and a side surface of the solid electrolyte layer may be flush with each other.

[0028] As a result, there are no steps or unevenness on the side surfaces of the layers of the battery. Therefore, there is no space that does not contribute to the charge / discharge performance of the battery, which is formed by the unevenness, and the substantial decrease in the energy density of the battery can be suppressed. Therefore, the volumetric energy density of the battery can be increased.

[0029] Furthermore, for example, the electrode active material layer and the counter electrode active material layer may have the same shape and position in a plan view.

[0030] This makes it possible to reduce the capacity difference between the counter electrode active material layer and the electrode active material layer, thereby maximizing the capacity of the counter electrode active material layer or the electrode active material layer.

[0031] In addition, when the electrode layer is a positive electrode layer and the counter electrode layer is a negative electrode layer, the positive electrode active material layer and the negative electrode active material layer have the same shape and position in a plan view, and the insulating layer is located at the end of the positive electrode layer, so that the positive electrode active material layer at the position facing the end of the negative electrode active material layer is unlikely to function as an electrode. As a result, electric field concentration at the end of the negative electrode active material layer is suppressed, and dendrite growth at the end is suppressed. Therefore, the reliability of the battery is improved.

[0032] Also, for example, a side surface of the battery may be inclined with respect to the stacking direction in a direction such that an area of ​​the counter electrode layer is larger than an area of ​​the electrode layer in a plan view.

[0033] As a result, the side surface of the solid electrolyte layer is also inclined with respect to the stacking direction on the side surface of the battery, so that the side surface of the solid electrolyte layer is larger than when the side surface is not inclined. As a result, the distance between the electrode layer and the counter electrode layer separated by the solid electrolyte layer on the side surface of the battery is longer. Therefore, the electrode layer and the counter electrode layer are less likely to come into contact with each other, and short circuits are suppressed.

[0034] Also, for example, the side surface of the battery may be a cut surface.

[0035] Since the side surface that becomes the end of the battery is cut, the area of ​​the insulating layer can be adjusted by the cutting position to reduce the area of ​​the region where the electrode active material layer does not function as an electrode due to the presence of the insulating layer, and the volumetric energy density of the battery can be increased. In addition, since the side surface of the battery is a cut surface, the side surface of the electrode layer, the side surface of the counter electrode layer, and the side surface of the solid electrolyte layer can be easily made flush with each other.

[0036] Also, for example, the shape of the cut surface may be rectangular or trapezoidal.

[0037] As a result, the ends of the cut surfaces are straight lines. Therefore, there is no space that does not contribute to the charge / discharge performance of the battery formed due to the ends not being straight lines, and the substantial decrease in the energy density of the battery can be suppressed. Therefore, the energy density of the battery can be increased.

[0038] Furthermore, for example, the insulating layer may be provided on the outer periphery of the electrode layer in a plan view and may be frame-shaped.

[0039] This provides the effect of providing an insulating layer at any position on the outer periphery of the electrode layer.

[0040] For example, the solid electrolyte layer may include a solid electrolyte having lithium ion conductivity.

[0041] This makes it possible to improve the reliability of a lithium ion battery that includes a solid electrolyte.

[0042] Hereinafter, the embodiment will be described in detail with reference to the drawings.

[0043] The embodiments described below are all comprehensive or specific examples. The numerical values, shapes, materials, components, arrangement positions and connection forms of the components shown in the following embodiments are merely examples and are not intended to limit the present disclosure.

[0044] Furthermore, in this specification, terms indicating the relationship between elements, such as parallel and flush, terms indicating the shape of elements, such as flat and rectangular, and numerical ranges are not expressions that only express a strict meaning, but are expressions that include a substantially equivalent range, for example, a difference of about a few percent.

[0045] In addition, the drawings are not necessarily strict illustrations. In the drawings, the same reference numerals are used for substantially the same configurations, and duplicated explanations are omitted or simplified.

[0046] In this specification and the drawings, the x-axis, y-axis, and z-axis indicate the three axes of a three-dimensional Cartesian coordinate system. In each embodiment, the z-axis direction is the stacking direction of the battery. The positive direction of the z-axis is the upper side in the z-axis direction, and the negative direction of the z-axis is the lower side in the z-axis direction. In this specification, "planar view" means the case where the battery is viewed along the z-axis. In this specification, "thickness" means the length of each layer in the stacking direction.

[0047] In this specification, the terms "upper" and "lower" in the battery configuration do not refer to the upper direction (vertically upper) and lower direction (vertically lower) in absolute spatial recognition, but are used as terms defined by a relative positional relationship based on the stacking order in the stacking configuration. The terms "upper" and "lower" are applied not only to the case where two components are arranged with a gap between them and another component is present between the two components, but also to the case where two components are arranged in close contact with each other and the two components are in contact with each other.

[0048] (Embodiment 1) Hereinafter, there will be described a battery according to embodiment 1. The battery according to embodiment 1 is a unit cell including one electrode active material layer and one counter electrode active material layer.

[0049] [composition] First, the configuration of the battery according to the first embodiment will be described with reference to the drawings. Fig. 1 is a schematic top view showing an example of the battery according to the present embodiment. Fig. 2 is a cross-sectional view taken along the line II-II in Fig. 1.

[0050] 1 and 2, a battery 50 according to the present embodiment includes an electrode layer 10, a counter electrode layer 20 disposed opposite the electrode layer 10, and a solid electrolyte layer 30 located between the electrode layer 10 and the counter electrode layer 20. That is, the battery 50 has a structure in which the electrode layer 10, the solid electrolyte layer 30, and the counter electrode layer 20 are laminated in this order.

[0051] The electrode layer 10 has a current collector 11, an electrode active material layer 12 located between the current collector 11 and the solid electrolyte layer 30, and an insulating layer 13 located between the current collector 11 and the electrode active material layer 12 at an end of the electrode layer 10 in a planar view. The current collector 11 and the electrode active material layer 12 have the same shape and are located at the same position in a planar view.

[0052] The counter electrode layer 20 has a current collector 21 and a counter electrode active material layer 22 located between the current collector 21 and the solid electrolyte layer 30 .

[0053] The battery 50 is, for example, an all-solid-state battery. The side of the battery 50 is parallel to the stacking direction. The side of the battery 50 is a flat plane. In other words, the side of the electrode layer 10, the side of the counter electrode layer 20, and the side of the solid electrolyte layer 30 are in a state without steps and are located on the same flat plane. That is, the side of the electrode layer 10, the side of the counter electrode layer 20, and the side of the solid electrolyte layer 30 are flush with each other. Note that the side is a surface that extends from the end of the main surface in a direction intersecting with the main surface when a plane perpendicular to the stacking direction is taken as the main surface in each component of the battery 50. Also, at the end of the electrode layer 10 in a direction perpendicular to the stacking direction, the side of the insulating layer 13, the side of the electrode active material layer 12, and the side of the current collector 11 are flush with each other. Also, at the end of the counter electrode layer 20 in a direction perpendicular to the stacking direction, the side of the counter electrode active material layer 22 and the side of the current collector 21 are flush with each other. That is, at the end of the battery 50 in the direction perpendicular to the stacking direction, the side surfaces of the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 are flush with each other and form the same flat plane. As a result, there are no steps or unevenness on the side surfaces of the layers of the battery 50, and no space that does not function as a battery due to unevenness is formed, thereby improving the substantial volumetric energy density of the battery 50. In addition, since the side surfaces of the layers can be made flush by cutting the layers together, the area of ​​the insulating layer 13 can be easily adjusted when manufacturing the battery 50.

[0054] The side surface of the battery 50 is, for example, a cut surface. Specifically, the side surface of the battery 50 is a surface formed by cutting with a blade such as a cutter, and is, for example, a surface having a cut mark such as a fine groove. In this way, since the cut surface is formed on the battery 50, the position where the insulating layer 13 is formed can be adjusted, so that the area of ​​the part that does not contribute to the charge / discharge performance of the battery 50 (the part where the insulating layer 13 is formed, details will be described later) can be reduced, and the volume energy density can be improved. In addition, since it is a cut surface, the side surface of the electrode layer 10, the side surface of the counter electrode layer 20, and the side surface of the solid electrolyte layer 30 can be easily made to be flush with each other. The cut mark may be smoothed by polishing or the like. The shape of the cut surface is not limited, but in the case of the battery 50, it is rectangular.

[0055] In the battery 50, the side surfaces of the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 are exposed. As a result, the layers that contribute to the charge / discharge performance of the battery 50 are present up to the ends of the battery 50, improving the volumetric energy density of the battery 50.

[0056] In the battery 50, the current collector 11, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 have the same shape and are located at the same positions in a plan view. The current collector 11, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 each have a rectangular shape in a plan view, but are not particularly limited thereto and may be a circular, elliptical, polygonal, or the like.

[0057] The current collector 11 is in contact with the lower surfaces of the electrode active material layer 12 and the insulating layer 13, and covers the lower surfaces of the electrode active material layer 12 and the insulating layer 13. The insulating layer 13 is laminated on the end portion of the current collector 11 in a plan view. The thickness of the current collector 11 is, for example, 5 μm or more and 100 μm or less.

[0058] Known materials can be used as the material of the current collector 11. For example, a foil, plate, or mesh made of copper, aluminum, nickel, iron, stainless steel, platinum, gold, or an alloy of two or more of these metals is used for the current collector 11.

[0059] The electrode active material layer 12 is laminated above the current collector 11 so as to cover the insulating layer 13 on the current collector 11. The lower surface of the electrode active material layer 12 is also in contact with the current collector 11. The upper surface of the electrode active material layer 12 is in contact with the solid electrolyte layer 30. The electrode active material layer 12 and the counter electrode active material layer 22 face each other with the solid electrolyte layer 30 interposed therebetween. The electrode active material layer 12 has a region that does not overlap with the insulating layer 13 in a planar view. Moreover, the electrode active material layer 12 and the counter electrode active material layer 22 have the same shape and position in a planar view. The thickness of the electrode active material layer 12 is, for example, 5 μm or more and 300 μm or less. The material used for the electrode active material layer 12 will be described later.

[0060] As described above, the insulating layer 13 is located between the current collector 11 and the electrode active material layer 12. The upper surface and the inner side surface in a plan view of the insulating layer 13 are in contact with the electrode active material layer 12. The insulating layer 13 is in contact with the electrode active material layer 12 at the end of the electrode layer 10 in a plan view. The side surface of the insulating layer 13 and the side surface of the electrode active material layer 12 are flush with each other. The lower surface of the insulating layer 13 is in contact with the current collector 11. Moreover, the insulating layer 13 overlaps with the counter electrode active material layer 22 in a plan view.

[0061] In the illustrated example, the insulating layer 13 is located on the outer periphery of the electrode layer 10 in a plan view and has a frame shape. That is, the insulating layer 13 is located between the current collector 11 and the electrode active material layer 12 at all ends of the electrode layer 10 in a direction perpendicular to the stacking direction.

[0062] The insulating layer 13 includes, for example, at least one of a resin and a metal oxide. Examples of the resin include a silicone resin, an epoxy resin, an acrylic resin, and a polyimide resin. The resin may be a thermosetting resin or an ultraviolet-curing resin. When the insulating layer 13 includes a resin, the bonding between the insulating layer 13 and the current collector 11 and the electrode active material layer 12 can be improved by an anchor effect in which the resin bites into the current collector 11 and the electrode active material layer 12. Examples of the metal oxide include silicon oxide, titanium oxide, and aluminum oxide. When the insulating layer 13 includes a metal oxide, the insulating layer 13 becomes hard. Therefore, even if the insulating layer 13 is formed thin during the manufacture of the battery 50, the insulating layer 13 is unlikely to deform when stacked with other layers, and a thin insulating layer 13 with a uniform thickness can be formed.

[0063] The thickness of the insulating layer 13 is thinner than that of the electrode active material layer 12, for example, sufficiently thinner than that of the electrode active material layer 12. Since the thickness of the insulating layer 13 is thinner than that of the electrode active material layer 12, even when a high pressure press treatment is performed when laminating the electrode active material layer 12, etc., the influence of the insulating layer 13 can be reduced, so that the electrode active material layer 12, etc. can be easily compressed uniformly. The thickness of the insulating layer 13 is, for example, 5 μm or less from the viewpoint of easily compressing the electrode active material layer 12, etc., even when a high pressure press treatment is performed when laminating the electrode active material layer 12, etc. From the viewpoint of the battery characteristics, the thickness of the insulating layer 13 may be 2 μm or less, or may be 1 μm or less. The insulating layer 13 is, for example, completely insulating, but may have slight conductivity depending on the required battery characteristics depending on the constituent material and thickness of the insulating layer 13.

[0064] From the viewpoint of the effective area contributing to power generation, i.e., from the viewpoint of volumetric energy density, the insulating layer 13 is located in a region having a length of 1 mm or less from the outer periphery of the electrode active material layer 12 in a plan view. From the viewpoint of volumetric energy density, the width of the insulating layer 13 when the insulating layer 13 is formed in a frame or line shape is, for example, 1 mm or less, and may be 0.5 mm or less, or may be 0.1 mm or less. The width of the insulating layer 13 is changed, for example, depending on the desired battery characteristics.

[0065] The current collector 21 is in contact with the upper surface of the counter electrode active material layer 22 and covers the upper surface of the counter electrode active material layer 22. The thickness of the current collector 21 is, for example, 5 μm or more and 100 μm or less. As the material of the current collector 21, the material of the current collector 11 described above can be used.

[0066] The counter electrode active material layer 22 is laminated on the solid electrolyte layer 30, and is disposed opposite the electrode active material layer 12. The upper surface of the counter electrode active material layer 22 contacts the current collector 21. The thickness of the counter electrode active material layer 22 is, for example, 5 μm or more and 300 μm or less. The material used for the counter electrode active material layer 22 will be described later.

[0067] The solid electrolyte layer 30 is located between the electrode active material layer 12 and the counter electrode active material layer 22. The solid electrolyte layer 30 has a thickness of, for example, 5 μm or more and 150 μm or less.

[0068] The solid electrolyte layer 30 includes at least a solid electrolyte, and may include a binder material as necessary. The solid electrolyte layer 30 may include a solid electrolyte having lithium ion conductivity.

[0069] As the solid electrolyte, known materials such as lithium ion conductors, sodium ion conductors, or magnesium ion conductors can be used. As the solid electrolyte, for example, a solid electrolyte material such as a sulfide solid electrolyte, a halogen-based solid electrolyte, or an oxide solid electrolyte is used. As the sulfide solid electrolyte, in the case of a material capable of conducting lithium ions, for example, a compound consisting of lithium sulfide (Li2S) and diphosphorus pentasulfide (P2S5) is used. As the sulfide solid electrolyte, a sulfide such as Li2S-SiS2, Li2S-B2S3, or Li2S-GeS2 may be used, and a sulfide obtained by adding at least one of Li3N, LiCl, LiBr, Li3PO4, and Li4SiO4 as an additive to the above sulfide may be used.

[0070] As an oxide solid electrolyte, materials that can conduct lithium ions include, for example, Li7La3Zr2O 12(LLZ), Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP) or (La,Li)TiO3(LLTO) are used.

[0071] As the binder material, for example, elastomers are used, and organic compounds such as polyvinylidene fluoride, acrylic resin, or cellulose resin may also be used.

[0072] In the present embodiment, of the electrode layer 10 including the electrode active material layer 12 and the counter electrode layer 20 including the counter electrode active material layer 22, one is a positive electrode layer including a positive electrode active material layer, and the other is a negative electrode layer including a negative electrode active material layer.

[0073] The positive electrode active material layer contains at least a positive electrode active material, and may contain at least one of a solid electrolyte, a conductive assistant, and a binder material, as necessary.

[0074] As the positive electrode active material, a known material capable of absorbing and releasing (inserting and desorbing, or dissolving and depositing) lithium ions, sodium ions, or magnesium ions can be used. As the positive electrode active material, in the case of a material capable of extracting and inserting lithium ions, for example, lithium cobalt oxide composite oxide (LCO), lithium nickel oxide composite oxide (LNO), lithium manganese oxide composite oxide (LMO), lithium-manganese-nickel composite oxide (LMNO), lithium-manganese-cobalt composite oxide (LMCO), lithium-nickel-cobalt composite oxide (LNCO), or lithium-nickel-manganese-cobalt composite oxide (LNMCO) can be used.

[0075] The solid electrolyte may be the above-mentioned solid electrolyte material. The conductive assistant may be, for example, a conductive material such as acetylene black, carbon black, graphite, or carbon fiber. The binder may be the above-mentioned binder material.

[0076] The negative electrode active material layer contains at least a negative electrode active material, and may contain at least one of a solid electrolyte, a conductive assistant, and a binder material, as in the positive electrode active material layer, if necessary.

[0077] As the negative electrode active material, a known material capable of occluding and releasing (inserting and desorbing, or dissolving and precipitating) lithium ions, sodium ions, or magnesium ions can be used. As the negative electrode active material, in the case of a material capable of extracting and inserting lithium ions, for example, a carbon material such as natural graphite, artificial graphite, graphite carbon fiber, or resin-baked carbon, metallic lithium, a lithium alloy, or an oxide of lithium and a transition metal element can be used.

[0078] In manufacturing a battery, as described above, it is common to make the area of ​​the negative electrode active material layer larger than the area of ​​the positive electrode active material layer in a plan view in order to improve reliability. Furthermore, by arranging the end of the negative electrode active material layer on the outer side of the end of the positive electrode active material layer, it is possible to suppress the electric field concentration at the end of the negative electrode active material layer and suppress dendrite growth (metal deposition).

[0079] Here, comparative batteries 950 and 950a in which the area of ​​the negative electrode active material layer is larger than the area of ​​the positive electrode active material layer in a plan view will be described. Figures 3 and 4 are schematic cross-sectional views showing examples of comparative batteries.

[0080] 3, the battery 950 includes a positive electrode layer 910, a negative electrode layer 920, and a solid electrolyte layer 930 located between the positive electrode layer 910 and the negative electrode layer 920. The positive electrode layer 910 includes a current collector 911 and a positive electrode active material layer 912 located between the current collector 911 and the solid electrolyte layer 930. The negative electrode layer 920 includes a current collector 921 and a negative electrode active material layer 922 located between the current collector 921 and the solid electrolyte layer 930. The solid electrolyte layer 930 covers the side surfaces of the positive electrode active material layer 912 and the negative electrode active material layer 922, and is in contact with the current collector 911 and the current collector 921. In the battery 950, the area of ​​the negative electrode active material layer 922 is larger than the area of ​​the positive electrode active material layer 912 in a plan view, and the end of the negative electrode active material layer 922 is located outside the end of the positive electrode active material layer 912. In this manner, in the battery 950, the area of ​​the negative electrode active material layer 922 is made larger than the area of ​​the positive electrode active material layer 912, thereby suppressing metal deposition. In addition, since the solid electrolyte layer 930 is present at the end of the battery 950, even if the current collector 911 and the current collector 921 are peeled off from the end, the positive electrode active material layer 912 and the negative electrode active material layer 922 are suppressed from being exposed.

[0081] The region 2C where the positive electrode active material layer 912 and the negative electrode active material layer 922 exist functions as a battery. On the other hand, the region 2A where neither the positive electrode active material layer 912 nor the negative electrode active material layer 922 exists does not function as a battery. In addition, the region 2B where the negative electrode active material layer 922 exists but the positive electrode active material layer 912 does not exist does not function as a battery. The region 2B is a region corresponding to the area difference between the positive electrode active material layer 912 and the negative electrode active material layer 922. As the region 2B and the region 2A become wider in plan view, the ratio of the region that does not contribute to power generation in the battery 950 increases, and the volumetric energy density of the battery 950 decreases. On the other hand, as the region 2B becomes narrower in plan view, the alignment accuracy required in the manufacturing process such as the process of stacking each layer becomes higher, and there is a concern that the number of processes such as inspection and the equipment cost will increase due to the required accuracy becoming higher.

[0082] In addition, the types and numbers of layers other than the current collectors 911 and 921 present in the thickness direction are different in the regions 2A, 2B, and 2C. That is, the region 2A has only one layer of the solid electrolyte layer 930, the region 2B has two layers of the negative electrode active material layer 922 and the solid electrolyte layer 930, and the region 2C has three layers of the positive electrode active material layer 912, the negative electrode active material layer 922, and the solid electrolyte layer 930. In an all-solid-state battery made of powder materials, in order to form a good interface between the powder materials (for example, an interface with good bonding between the powder materials and low grain boundary resistance), that is, to improve the reliability of the battery, and to improve the volumetric energy density by high packing, a high-pressure pressing process may be included in the manufacturing process. At this time, the types and numbers of the layers constituting the regions 2A, 2B, and 2C are different, and the ease of compression of each layer is also different. Therefore, when the entire battery 950 is pressed, the degree of compression is different in each region, that is, there is a concern that it is not compressed uniformly. For example, in regions 2A and 2B, compression is insufficient compared to region 2C, and there is concern that the layers may peel off, resulting in reduced reliability.

[0083] That is, there are problems in that battery 950 is difficult to manufacture and reliability is not sufficiently improved. Moreover, region 2A, which is the only layer in the thickness direction that is solid electrolyte layer 930, is a portion that does not particularly contribute to the basic charge / discharge performance of the battery, so that from the viewpoint of improving the volumetric energy density, it is preferable that region 2A is small.

[0084] Also, the battery 950a shown in FIG. 4 includes a positive electrode layer 910a having a current collector 911a and a positive electrode active material layer 912a, a negative electrode layer 920a having a current collector 921a and a negative electrode active material layer 922a, and a solid electrolyte layer 930a. The battery 950a is different from the battery 950 in that the solid electrolyte layer 930a does not cover the side surface of the negative electrode active material layer 922a. The battery 950a does not have a region where neither the positive electrode active material layer 912 nor the negative electrode active material layer 922 is present, as in the region 2A, but has a region 3A where the positive electrode active material layer 912a is not present. Therefore, the region 3A does not contribute to power generation, and the same problem as the region 2B occurs in the region 3A of the battery 950a.

[0085] On the other hand, the battery 50 includes, as described above, an electrode layer 10, a counter electrode layer 20 disposed opposite the electrode layer 10, and a solid electrolyte layer 30 located between the electrode layer 10 and the counter electrode layer 20. The electrode layer 10 includes a current collector 11, an electrode active material layer 12 located between the current collector 11 and the solid electrolyte layer 30, and an insulating layer 13 located between the current collector 11 and the electrode active material layer 12 at an end of the electrode layer 10 in a planar view. The electrode active material layer 12 has a region that does not overlap with the insulating layer 13 in a planar view. The side surface of the insulating layer 13 and the side surface of the electrode active material layer 12 are flush with each other. Furthermore, the side surfaces of the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 are flush with each other.

[0086] As a result, since the insulating layer 13 is present between the current collector 11 and the electrode active material layer 12 at the end of the current collector 11 where peeling is likely to occur, exposure of the electrode active material layer 12 is suppressed even if the current collector 11 peels off, and damage or short circuit caused by contact between the electrode active material layer 12 and other members is less likely to occur, thereby improving the reliability of the battery 50.

[0087] Since the side surfaces of the current collector 11, insulating layer 13, electrode active material layer 12, solid electrolyte layer 30, counter electrode active material layer 22, and current collector 21 are flush with each other, the area of ​​the insulating layer 13 can be easily adjusted by cutting each layer together, for example, to manufacture the battery 50. Therefore, although the presence of the insulating layer 13 suppresses the exchange of electrons between the electrode active material layer 12 and the current collector 11, forming a region in which the electrode active material layer 12 does not easily function as an electrode, the region can be minimized by adjusting the area of ​​the insulating layer. This allows the volumetric energy density of the battery to be increased.

[0088] In addition, since the insulating layer 13 is located between the current collector 11 and the electrode active material layer 12, the electrode active material layer 12 is also present on the insulating layer 13. Therefore, even when a high-pressure press treatment is performed, all regions are more likely to be compressed uniformly than, for example, a case in which a solid electrolyte layer is present on the side surface of the electrode active material layer 12 as in the battery according to the comparative example described above. Therefore, peeling of each layer of the battery 50 is less likely to occur, and the high-pressure press treatment can improve the reliability and volumetric energy density of the battery 50.

[0089] In the battery 50, for example, the electrode layer 10 including the electrode active material layer 12 is a positive electrode layer including a positive electrode active material layer, and the counter electrode layer 20 including the counter electrode active material layer 22 is a negative electrode layer including a negative electrode active material layer. In this case, since electrons do not directly reach the positive electrode active material layer (electrode active material layer 12) in contact with the insulating layer 13 from the current collector 11, the positive electrode active material layer in the region 1A shown in FIG. 1 and FIG. 2 does not function as an electrode. On the other hand, the positive electrode active material layer in the region 1B functions as an electrode. Therefore, in the battery 50, the region 1A does not function as a battery, and the region 1B functions as a battery. In the battery 50, the areas of the positive electrode active material layer and the negative electrode active material layer (counter electrode active material layer 22) are the same in plan view, but since the positive electrode active material layer in the region 1A does not function as an electrode, an effect of substantially reducing the area of ​​the positive electrode active material layer in plan view is obtained. That is, in the battery 50, even if the areas of the positive electrode active material layer and the negative electrode active material layer in a plan view are the same, metal deposition is suppressed.

[0090] In addition, since the positive electrode active material layer and the negative electrode active material layer have the same shape and position in a plan view and the insulating layer 13 is located at the end of the positive electrode layer (electrode layer 10), the positive electrode active material layer at the position facing the end of the negative electrode active material layer does not easily function as an electrode. As a result, electric field concentration at the end of the negative electrode active material layer is suppressed, and dendrite growth at the end is suppressed. Therefore, the reliability of the battery 50 is improved.

[0091] Furthermore, in manufacturing the battery 50, since the actual area of ​​the positive electrode active material layer can be adjusted by the insulating layer 13, there is no need to precisely form the positions and areas of the positive electrode active material layer and the negative electrode active material layer. Therefore, the battery 50 can be easily manufactured. For example, the battery 50 can be easily manufactured by cutting a laminate in which the positive electrode layer (electrode layer 10), the solid electrolyte layer 30, and the negative electrode layer (counter electrode layer 20) are laminated in a region including the insulating layer 13.

[0092] [Manufacturing method] Next, a method for manufacturing the battery according to the present embodiment will be described. Note that the method for manufacturing the battery 50 described below is one example, and the method for manufacturing the battery 50 is not limited to the following example.

[0093] The manufacturing method of the battery 50 includes an insulating layer laminating step, a power generating element laminating step, a cutting step, and a current collector laminating step. Each step will be described in detail below.

[0094] (1) Insulation layer lamination process First, the insulating layer lamination step will be described below. Fig. 5 is a flow chart for explaining the method for manufacturing the battery according to this embodiment.

[0095] In the insulating layer lamination step, an insulating layer 13 is laminated on at least one surface of a current collector 11. Specifically, first, a current collector 11 is prepared (step S11 in FIG. 5). Then, an insulating layer 13 is laminated on at least one surface of the prepared current collector 11 (step S12 in FIG. 5). For example, the insulating layer 13 is formed on the upper surface of the current collector 11, thereby laminating the insulating layer 13 on the current collector 11.

[0096] 6A, 6B, and 6C are schematic diagrams showing an example of a current collector 11 on which an insulating layer 13 is laminated. FIG. 6A (a) is a top view showing an example of a current collector 11 on which an insulating layer 13 is laminated, and FIG. 6A (b) is a cross-sectional view taken along the line VIa-VIa in FIG. 6A (a). The insulating layer 13 is formed in a lattice shape, for example, as shown in FIG. 6A. FIG. 6B is a top view showing another example of a current collector 11 on which an insulating layer 13 is laminated. Although a cross-sectional view is not shown in FIG. 6B, the current collector 11 on which an insulating layer 13 is laminated shown in FIG. 6B has a cross-sectional structure similar to that shown in FIG. 6A (b). The insulating layer 13 may be formed in a stripe shape as shown in FIG. 6B. By laminating the insulating layer 13 in such a relatively simple planar shape having a long portion such as a lattice or stripe, the insulating layer 13 can be easily formed on the current collector 11. Furthermore, in a cutting step described later, the insulating layer 13 is divided along the longitudinal direction of the insulating layer 13, so that the battery 50 can be easily formed with the insulating layer 13 formed along the end portion of the battery 50. In Figures 6A and 6B, rectangular regions 1E and 1F depicted by dotted lines correspond to the size of one battery 50. In this manner, the insulating layers 13 may be laminated on the current collector 11 so that the current collector 11 can be divided into a plurality of batteries in a later manufacturing step.

[0097] Fig. 6C(a) is a top view showing yet another example of the current collector 11 on which the insulating layer 13 is laminated, and Fig. 6C(b) is a cross-sectional view taken along line VIc-VIc in Fig. 6C(a). As shown in Fig. 6C, the lattice-shaped insulating layer 13 having a plurality of types of patterns (e.g., lattice spacing) may be formed on the current collector 11.

[0098] In this way, the insulating layer 13 is laminated in a lattice or stripe pattern, and in a cutting process described later, the insulating layer 13 is divided along the longitudinal direction of the lattice or stripe of the insulating layer 13, so that it is possible to simultaneously manufacture a plurality of batteries 50 each having the same shape or different shapes, thereby improving the manufacturing efficiency of the batteries 50.

[0099] Various processes can be considered for the method of forming the insulating layer 13, but from the viewpoint of mass production, for example, a coating process is used. For example, in a continuous process such as a roll-to-roll method, a coating material in which an insulating substance (e.g., a metal oxide) is dispersed in a solvent as the material of the insulating layer 13 is applied onto the current collector 11 by a high-precision coating method such as a gravure roll method or an inkjet method, and the coating is dried to evaporate the solvent, thereby obtaining the insulating layer 13. This allows the insulating layer 13 to be laminated thinly, so that a thin insulating layer 13 with a uniform thickness is formed. Therefore, when a high-pressure press process is performed to laminate other layers in the power generating element lamination process described later, the insulating layer 13 is less likely to be affected, and the other layers are easily compressed uniformly. In addition, by using such a high-precision coating method, the precision of the area of ​​the electrode active material layer 12 that is substantially effective as an electrode is improved.

[0100] When a resin is used as the material of insulating layer 13, a solution in which the resin is dissolved or dispersed may be applied onto current collector 11, or an ultraviolet curable resin or a thermosetting resin may be applied onto current collector 11 and then cured. The formation of insulating layer 13 is not limited to a continuous process such as a roll-to-roll method, and may be a batch process in which insulating layer 13 is formed for each current collector 11.

[0101] The solvent used to form the insulating layer 13 may be a general organic solvent or aqueous solvent capable of dispersing or dissolving a metal oxide or a resin.

[0102] (2) Power generating element stacking process Next, the power generating element lamination step will be described. In the power generating element lamination step, the power generating element section 40 in which the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are laminated in this order, and the current collector 11 on which the insulating layer 13 is laminated in the insulating layer lamination step are laminated so that the electrode active material layer 12 covers the insulating layer 13. In this manner, in the power generating element lamination step, a covering structure in which the electrode active material layer 12 covers the insulating layer 13 is formed. In the power generating element lamination step, the power generating element section 40 is formed, for example, by sequentially laminating the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 on the current collector 11. Specifically, the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are laminated in this order on the current collector 11 on which the insulating layer 13 is laminated (steps S13, S14, and S15 in FIG. 5). For example, the electrode active material layer 12 is laminated on the current collector 11 on which the insulating layer 13 is laminated so as to cover the insulating layer 13, and further the solid electrolyte layer 30 and the counter electrode active material layer 22 are laminated in this order. Furthermore, if necessary, the electrode active material layer 12, the solid electrolyte layer 30 and the counter electrode active material layer 22 laminated in steps S13, S14 and S15 are subjected to a high pressure press treatment (step S16 in FIG. 5). Furthermore, if necessary, the electrode active material layer 12, the solid electrolyte layer 30 and the counter electrode active material layer 22 laminated in steps S13, S14 and S15 are subjected to a heat treatment. As a result, a laminated electrode plate in which the power generating element section 40 is laminated on the current collector 11 on which the insulating layer 13 is laminated is obtained.

[0103] 7A, 7B, and 7C are schematic cross-sectional views showing examples of a laminated electrode plate according to the present embodiment. As shown in Fig. 7A, in a laminated electrode plate 41, a power generating element section 40 in which an electrode active material layer 12, a solid electrolyte layer 30, and a counter electrode active material layer 22 are laminated in this order is laminated on a current collector 11 on which an insulating layer 13 is laminated. The laminated electrode plate 41 is formed so that the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 have the same area and position in a plan view. In addition, the upper surface of the counter electrode active material layer 22 is exposed.

[0104] The structure of the laminated electrode plate 41 is not limited to this example. For example, as shown in Fig. 7B, the laminated electrode plate 41a is formed such that the side and upper surface of the electrode active material layer 12 are covered with the solid electrolyte layer 30, and the side and upper surface of the solid electrolyte layer 30 are covered with the counter electrode active material layer 22. As a result, the electrode active material layer 12 is covered with the solid electrolyte layer 30, and therefore, in the power generating element lamination step, the occurrence of a short circuit due to contact between the electrode active material layer 12 and the counter electrode active material layer 22 is suppressed.

[0105] 7C, the laminated electrode plate 41b is formed so that the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 have smaller areas in this order in plan view. In plan view, the counter electrode active material layer 22 is located inside the solid electrolyte layer 30, and the solid electrolyte layer 30 is located inside the electrode active material layer. Since the counter electrode active material layer 22 is designed to be located inside the solid electrolyte layer 30, even if the stacking position in plan view is shifted when stacking the counter electrode active material layer 22, the solid electrolyte layer 30 suppresses the occurrence of a short circuit due to contact between the electrode active material layer 12 and the counter electrode active material layer 22.

[0106] The laminated electrode plate in this embodiment may have any of the structures of laminated electrode plates 41, 41a, and 41b, and may have a structure other than that of laminated electrode plates 41, 41a, and 41b, so long as the structure is such that a power generating element part 40 is laminated on a collector 11 on which an insulating layer 13 is laminated.

[0107] The electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 constituting the power generating element section 40 are each formed in this order, for example, by a wet coating method. By using the wet coating method, the power generating element section 40 can be easily laminated on the current collector 11. As the wet coating method, a coating method such as a die coating method, a doctor blade method, a roll coater method, a screen printing method, or an inkjet method can be used, but the wet coating method is not limited to these methods.

[0108] When the wet coating method is used, a coating process is carried out in which materials for forming the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 (the materials for the positive electrode active material layer, the solid electrolyte layer 30, and the negative electrode active material layer described above) are appropriately mixed with a solvent to obtain a slurry.

[0109] The solvent used in the coating process may be a known solvent used in producing a known all-solid-state battery (for example, a lithium-ion all-solid-state battery).

[0110] The slurry of each layer obtained in the paint forming process is applied to the collector 11 on which the insulating layer 13 is formed in the order of the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22. At this time, the next layer may be applied after the layer coating of the layer that has been applied first is finished, or the layer coating of the next layer may be started during the layer coating of the layer that has been applied first. In other words, steps S13, S14, and S15 may be performed simultaneously in parallel. After the slurry of each layer is applied in sequence and all layers are coated, for example, a heat treatment to remove the solvent and binder material, and a high-pressure press treatment to promote the filling of the material of each layer are performed. Note that the heat treatment and high-pressure press treatment may be performed for each layer coating. In other words, step S16 may be performed between steps S13, S14, and S15. The heat treatment and the high-pressure press treatment may be performed for each coating layer of the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22, or may be performed separately after coating lamination of any two layers and after coating lamination of one layer, or may be performed collectively after coating lamination of all three layers. For the high-pressure press treatment, for example, a roll press or a flat plate press is used. At least one of the heat treatment and the high-pressure press treatment may not be performed.

[0111] By carrying out the layered coating method in this manner, it is possible to improve the bonding strength and reduce the interface resistance at the interfaces of the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22. It is also possible to improve the bonding strength and reduce the grain boundary resistance in the powder materials used in the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22. That is, good interfaces are formed between the layers of the power generating element section 40 and between the powder materials inside each layer.

[0112] The insulating layer lamination step and the power generating element lamination step may be carried out in a single continuous process such as a roll-to-roll method.

[0113] (3) Cutting process and current collector lamination process Next, the cutting step and the current collector lamination step will be described. FIG. 8 is a diagram for explaining the cutting step in the manufacturing method of the battery according to the present embodiment. In the cutting step, the current collector 11 on which the power generating element part 40 is laminated in the power generating element lamination step, that is, the laminated electrode plate 41, 41a or 41b, is cut in a lump in the lamination direction at the position where the insulating layer 13 is divided (step S17 in FIG. 5). As shown in FIG. 8, the laminated electrode plate 41 is cut, for example, by a blade or laser light at the positions of the dashed lines C1, C2, C3 and C4 where the insulating layer 13 is arranged. At the positions of the dashed lines C1, C2, C3 and C4, the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30 and the counter electrode active material layer 22 are laminated in this order, and these are cut in a lump. This makes it unnecessary to laminate each layer of the power generating element part 40 in the shape after cutting, and therefore the battery 50 can be easily manufactured. For example, when the insulating layer 13 is laminated in a lattice or stripe pattern having long portions as shown in Figures 6A, 6B, and 6C in plan view, the current collector 11 on which the power generating element section 40 is laminated is cut all at once along the long direction of the lattice or stripe of the insulating layer 13. This results in a battery 50 in which the insulating layer 13 is located over the entire end area on the cut surface side of the manufactured battery 50.

[0114] Next, in the current collector lamination step, a current collector 21 is laminated as an additional current collector on the surface of the power generating element section 40 of the laminated electrode plate 41 after being cut in the cutting step opposite to the current collector 11 side (the surface perpendicular to the lamination direction of the power generating element section 40 on which the current collector 11 is not laminated) (step S18 in FIG. 5). Specifically, the current collector 21 is joined to the upper surface of the exposed counter electrode active material layer 22 of the cut laminated electrode plate 41 by a press process or the like. The press process is performed, for example, at a pressure lower than the high-pressure press process in step S16. As a result, the battery 50 shown in FIG. 2 and FIG. 3 is obtained.

[0115] The cutting step and the current collector lamination step may be reversed in order. That is, the current collector 21 may be laminated on the surface of the laminated electrode plate 41 before being cut in the cutting step, opposite the current collector 11 side of the power generating element section 40, and then the laminated electrode plate 41 on which the current collector 21 is laminated may be cut in the lamination direction at a position where the insulating layer 13 is to be divided. In addition, in the current collector lamination step, a conductive substrate or a housing may be laminated as an additional current collector instead of the current collector 21 on the surface of the power generating element section 40 opposite the current collector 11 side.

[0116] Thus, the manufacturing method of the battery 50 includes a cutting step of cutting the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 at positions where they are stacked. As a result, the side surfaces of the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 are exposed at the end in the direction perpendicular to the stacking direction. Note that after cutting, a sealing member or the like that covers the side surfaces may be disposed to protect the exposed side surfaces. In other words, when the side surfaces are covered with another member such as a sealing member, the side surfaces of all layers may not be exposed.

[0117] In this way, by including a cutting step of cutting the positions where the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are stacked, the ends of each of the current collector 11, the insulating layer 13, the electrode active material layer 12, the solid electrolyte layer 30, the counter electrode active material layer 22, and the current collector 21 in a direction perpendicular to the stacking direction are exposed.

[0118] (4) Effects, etc. As described above, the manufacturing method of the battery 50 according to the present embodiment includes an insulating layer lamination step, a power generating element lamination step, a cutting step, and a current collector lamination step. In the insulating layer lamination step, the insulating layer 13 is laminated on at least a part of one surface of the current collector 11. In the power generating element lamination step, the power generating element part 40 in which the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are laminated in this order, and the current collector 11 on which the insulating layer 13 is formed are laminated so that the electrode active material layer 12 covers the insulating layer 13. In the cutting step, the current collector 11 on which the power generating element part 40 is laminated is cut in the lamination direction at a position where the insulating layer 13 is divided. In the current collector lamination step, the current collector 21 is laminated on the surface of the power generating element part 40 opposite to the current collector 11 side before or after cutting in the cutting step.

[0119] As a result, the current collector 11 on which the power generating element section 40 is laminated is cut all at once in the lamination direction at the position for dividing the insulating layer 13. Therefore, it is not necessary to laminate each layer of the power generating element section 40 in the shape after cutting, and the battery 50 can be easily manufactured.

[0120] In addition, since the current collector 11 on which the power generating element portion 40 is laminated is cut in the lamination direction at the position where the insulating layer 13 is divided, a battery is manufactured in which the insulating layer 13 is laminated on the end of the current collector 11 in a plan view. Furthermore, since the electrode active material layer 12 is laminated so as to cover the insulating layer 13 laminated on the current collector 11, the current collector 11, the insulating layer 13, and the electrode active material layer 12 are laminated in this order at the end of the current collector 11 of the manufactured battery 50. Therefore, even if the current collector 11 peels off at the end of the current collector 11 where peeling is likely to occur, the insulating layer 13 is exposed, so that the exposure of the electrode active material layer 12 is suppressed. As a result, damage or short circuit due to contact between the electrode active material layer 12 and other members is less likely to occur. Therefore, a highly reliable battery can be manufactured.

[0121] Moreover, the dimensions of the insulating layer 13 can be determined simply by adjusting the cutting position. Therefore, although the presence of the insulating layer 13 suppresses the exchange of electrons between the electrode active material layer 12 and the current collector 11 and forms a region in which the electrode active material layer 12 does not easily function as an electrode, the region can be minimized by adjusting the dimensions of the insulating layer 13. Therefore, a battery 50 with a high volumetric energy density can be easily manufactured.

[0122] In addition, when the electrode active material layer 12 is a positive electrode active material layer and the counter electrode active material layer 22 is a negative electrode active material layer, the insulating layer 13 is laminated on the end of the current collector 11, so that electrons from the current collector 11 do not reach the end of the positive electrode active material layer (electrode active material layer 12), and the function of the positive electrode active material layer at the end as an electrode is suppressed. That is, the substantial area of ​​the positive electrode active material layer in a planar view is reduced. In addition, since the power generating element section 40 is cut in the lamination direction, the positive electrode active material layer and the negative electrode active material layer (counter electrode active material layer 22) have the same shape and position in a planar view, and also the same area. Therefore, the substantial area (area functioning as an electrode) of the positive electrode active material layer is narrower than that of the negative electrode active material layer, and is located inside the negative electrode active material layer in a planar view. As a result, the deposition of metal in the negative electrode active material layer is suppressed as described above. Therefore, the reliability of the manufactured battery 50 is further improved.

[0123] Moreover, by cutting in the stacking direction, the current collector 11 (for example, laminated electrode plates 41, 41a or 41b) on which the power generating element parts 40 are stacked is cut all at once, and a battery is obtained in which an insulating layer is stacked on the end part of the current collector 11. Therefore, it is not necessary to stack the positive electrode active material layers and the negative electrode active material layers having different areas for each unit cell individually, and therefore the battery 50 can be manufactured easily and with high production efficiency.

[0124] In the absence of the insulating layer 13, even if the current collector 11 on which the power generating element section 40 is laminated is cut in one go, the electrode active material layer 12 is also laminated on the end of the current collector 11, so that when the end of the current collector 11 is peeled off, the exposure of the electrode active material layer 12 cannot be suppressed, and a battery is manufactured in which there is no substantial difference in area between the electrode active material layer 12 and the counter electrode active material layer 22. Therefore, even if the battery can be easily manufactured, the reliability of the battery is reduced, so it is difficult to adopt this as a manufacturing method. On the other hand, in the manufacturing method according to the present embodiment, as described above, the current collector 11 on which the power generating element section 40 is laminated is cut in one go at the position where the insulating layer 13 is divided. Therefore, by cutting the current collector 11 on which the power generating element section 40 is laminated in one go, in addition to being able to easily manufacture a battery, it is possible to suppress the exposure of the electrode active material layer 12, reduce the area of ​​the electrode active material layer 12 that functions as an electrode, and adjust the area of ​​the insulating layer 13. In this way, by combining the current collector lamination process of laminating the insulating layer 13 onto the current collector 11 with the cutting process of cutting the current collector 11 on which the power generating element section 40 is laminated at a position to divide the insulating layer 13, it is possible to easily manufacture a battery that is both highly reliable and has a high volumetric energy density.

[0125] (5) Other manufacturing methods The method for manufacturing the battery according to the present embodiment is not limited to the above-mentioned example, and may be, for example, the manufacturing method shown below.

[0126] First, a current collector 11 is prepared in the shape shown in Figures 2 and 3. Then, an insulating layer 13 is laminated on the current collector 11 in the shape shown in Figures 2 and 3 using a coating process or the like. An electrode active material layer 12 and a solid electrolyte layer 30 are laminated in this order on the entire surface of the current collector 11 on which the insulating layer 13 is laminated, by lamination coating, to obtain an electrode plate.

[0127] 2 and 3 is prepared. Then, the counter electrode active material layer 22 and the solid electrolyte layer 30 are laminated in this order on the entire surface of the current collector 21 by layer coating to obtain a counter electrode plate.

[0128] Next, the obtained electrode plate and counter electrode plate are stacked so that the respective solid electrolyte layers 30 are in contact with each other. The stacked body is pressed from both sides in the stacking direction using a plate press, thereby obtaining a battery 50.

[0129] In addition, the battery 50 may be formed by forming a laminate by stacking the insulating layer 13 and the power generating element section 40 on a base separate from the current collector, and, if necessary, cutting the laminate in the stacking direction at a position to divide the insulating layer 13, and then sandwiching the obtained laminate between the current collector 11 and the current collector 21.

[0130] [Variation 1] The following describes Modification 1 of Embodiment 1. In the following description of Modification 1 of Embodiment 1, differences from Embodiment 1 will be mainly described, and descriptions of commonalities will be omitted or simplified.

[0131] Fig. 9 is a schematic cross-sectional view showing an example of a battery according to this modification. As shown in Fig. 9, battery 51 differs from battery 50 of the first embodiment in that the side surface of battery 51 is inclined with respect to the stacking direction.

[0132] The battery 51 includes an electrode layer 10a, a counter electrode layer 20a disposed opposite the electrode layer 10a, and a solid electrolyte layer 30a located between the electrode layer 10a and the counter electrode layer 20a.

[0133] The electrode layer 10a includes a current collector 11a, an electrode active material layer 12a located between the current collector 11a and the solid electrolyte layer 30a, and an insulating layer 13a located between the current collector 11a and the electrode active material layer 12a at an end of the electrode layer 10a. The counter electrode layer 20a includes a current collector 21a, and a counter electrode active material layer 22a located between the current collector 21a and the solid electrolyte layer 30a.

[0134] The side surface 51s connecting the two main surfaces perpendicular to the stacking direction of the battery 51 is inclined with respect to the stacking direction in a direction in which the area of ​​the counter electrode layer 20a in a plan view is larger than the area of ​​the electrode layer 10a. In other words, the side surface 51s is inclined with respect to the stacking direction in a direction in which the width of the counter electrode layer 20a is larger than the width of the electrode layer 10a in a cross section of the battery 51 cut in the stacking direction. That is, in the battery 51, the area of ​​the main surface 22s of the counter electrode active material layer 22a on the electrode active material layer 12a side is larger than the area of ​​the main surface 12s of the electrode active material layer 12a on the counter electrode active material layer 22a side. Also, when viewed from the stacking direction, the main surface 12s is located inside the main surface 22s. In the battery 50a, for example, the electrode layer 10a including the electrode active material layer 12a is a positive electrode layer including a positive electrode active material layer, and the counter electrode layer 20a including the counter electrode active material layer 22a is a negative electrode layer including a negative electrode active material layer. In this case, the area of ​​the negative electrode active material layer in a plan view becomes larger than the area of ​​the positive electrode active material layer, so that metal deposition is suppressed in the battery 50a.

[0135] In addition, since the side surface 51s of the solid electrolyte layer 30 is also inclined with respect to the stacking direction, the exposed surface of the solid electrolyte layer 30 becomes larger, and the distance between the electrode active material layer 12a and the counter electrode active material layer 22a on the side surface 51s becomes longer. As a result, the electrode active material layer 12a and the counter electrode active material layer 22a are less likely to come into contact with each other, and short circuits are suppressed.

[0136] All of the side surfaces 51s of the battery 51, including side surfaces 51s not shown, are inclined with respect to the stacking direction, and the area of ​​the main surface 22s is larger than the area of ​​the main surface 12s. All of the side surfaces 51s of the battery 51 do not have to be inclined with respect to the stacking direction, as long as at least one side surface 51s is inclined with respect to the stacking direction.

[0137] Fig. 10 is a schematic cross-sectional view showing another example of a battery according to this modification. As shown in Fig. 10, a battery 52 includes an electrode layer 10b, a counter electrode layer 20b, and a solid electrolyte layer 30b. The electrode layer 10b includes a current collector 11b, an electrode active material layer 12b, and an insulating layer 13b. The counter electrode layer 20b includes a current collector 21b and a counter electrode active material layer 22b. In the battery 52, one side surface 52s is inclined with respect to the stacking direction in a direction in which the area of ​​the counter electrode layer 20b in a plan view is larger than the area of ​​the electrode layer 10b.

[0138] The batteries 51 and 52 are manufactured, for example, by cutting the battery 50 according to the first embodiment in a direction inclined with respect to the stacking direction. The batteries 51 and 52 may also be manufactured by cutting the battery 50 in a cutting step in the manufacturing method thereof in a direction inclined with respect to the stacking direction. That is, the side surfaces 51s and 52s may be cut surfaces. The shape of the cut surface is trapezoidal in the case of the battery 51, and rectangular in the case of the battery 52.

[0139] FIG. 11 is a diagram for explaining the cutting step in the manufacturing method of the battery according to this modification. As shown in FIG. 11, the batteries 51 and 52 are manufactured by cutting in a direction inclined at an angle θ from the stacking direction in the above-mentioned cutting step. The angle θ may be determined based on the width of the insulating layer formed and the desired battery characteristics. The angle θ is, for example, smaller than 45 degrees. The angle θ may be 30 degrees or less. Also, when the angle θ is zero degrees, a battery 50 is manufactured. For example, when the thickness of the battery is 0.1 mm and the width of the insulating layer from the side surface of the battery is 0.1 mm, if the angle of the cut surface is larger than 45 degrees, the insulating layer is removed by cutting, and the effect of the insulating layer cannot be obtained.

[0140] (Embodiment 2) Next, a battery according to embodiment 2 will be described. The battery according to embodiment 2 is a stacked type battery in which unit cells are stacked. In the following description, differences from embodiment 1 will be mainly described, and descriptions of commonalities will be omitted or simplified as appropriate.

[0141] [composition] First, the configuration of the battery according to the second embodiment will be described with reference to the drawings. Fig. 12 is a schematic cross-sectional view showing an example of the battery according to the present embodiment. As shown in Fig. 12, the battery 100 has a structure in which unit cells, which are structured without the current collector 21 in the battery 50 according to the first embodiment, are stacked.

[0142] The battery 100 includes a plurality of batteries 50a and a current collector 21. The battery 50a has a structure including a counter electrode layer 23 that does not include the current collector 21 of the counter electrode layer 20 in the battery 50. That is, the battery 50a includes an electrode layer 10, a counter electrode layer 23 that is disposed opposite the electrode layer 10 and is composed of a counter electrode active material layer 22, and a solid electrolyte layer 30 that is located between the electrode layer 10 and the counter electrode layer 23.

[0143] In the battery 100, the multiple batteries 50a are stacked such that the current collector 11 of one of the adjacent batteries 50a faces the counter electrode active material layer 22 of the other. This results in a structure in which the function of the current collector 11 is shared by the adjacent batteries 50a. In addition, the current collector 21 is stacked on the counter electrode active material layer 22 of the battery 50a stacked at the top. This results in the battery 100 being a series-stacked battery. This makes it possible to realize a series-stacked high-voltage battery 100 that exhibits the same effects as the battery 50 according to the first embodiment.

[0144] 12, the number of stacked batteries 50a is five, but may be two to four, or may be six or more. Battery 50b, which is the uppermost stacked unit cell, is composed of battery 50a and current collector 21, and has the same stacking configuration and shape as battery 50 according to embodiment 1.

[0145] The side of the battery 100 is, for example, a cut surface. The side of the battery 100 is a flat plane. In other words, the side of the plurality of batteries 50a and the current collector 21 are flush with each other. On the side of the battery 100, each layer may be exposed, or a sealing member or the like may be provided. FIG. 13 is a schematic cross-sectional view showing another example of the battery according to the present embodiment. As shown in FIG. 13, the battery 100a has a structure in which the side of the battery 100 is covered with a sealing member 60. That is, the side of each layer constituting the battery 100a is covered with the sealing member 60. As a result, the side of each layer in the battery 100a is not exposed, and therefore the strength of the battery 100a is increased, and the reliability of the battery 100a is improved.

[0146] The sealing member 60 of the battery 100a is formed, for example, by placing the battery 100 so that the side surface of the battery 100 faces upward, and applying the sealing member to the side surface from above using a dispenser or the like. The material of the sealing member 60 may be a known material for a sealing member for a battery (for example, a lithium ion solid-state battery).

[0147] [Manufacturing method] Next, a method for manufacturing the battery according to the present embodiment will be described. Note that the method for manufacturing the battery 100 described below is one example, and the method for manufacturing the battery 100 is not limited to the following example.

[0148] The manufacturing method of the battery 100 includes an insulating layer laminating step, a power generating element laminating step, a cutting step, and a current collector laminating step, similar to the manufacturing method of the battery 50. Each step will be described in detail below.

[0149] (1) Insulation layer lamination process First, the insulating layer lamination step will be described with reference to a flowchart of FIG 14, which is a flow chart for explaining the method for manufacturing the battery according to the present embodiment.

[0150] In the insulating layer lamination step, first, a plurality of current collectors 11 are prepared (step S21 in FIG. 14). Then, an insulating layer 13 is laminated only on one surface of each of the prepared plurality of current collectors 11 (step S22 in FIG. 14). In steps S21 and S22, a method similar to steps S11 and S12 described above can be used. As a result, a plurality of current collectors 11 on which insulating layers 13 are laminated can be obtained, for example, as shown in FIGS. 6A, 6B, and 6C.

[0151] (2) Power generating element stacking process Next, the power generating element lamination step will be described. In the manufacturing method according to the present embodiment, the power generating element lamination step includes a first laminate formation step and a first laminate lamination step. In the first laminate formation step, a plurality of laminated electrode plates (for example, laminated electrode plates 41, 41a or 41b shown in FIG. 7A, FIG. 7B and FIG. 7C) are formed by laminating a power generating element part 40 on each of a plurality of current collectors 11 on which an insulating layer 13 is laminated so that the electrode active material layer 12 covers the insulating layer 13. Specifically, the electrode active material layer 12, the solid electrolyte layer 30 and the counter electrode active material layer 22 are laminated in this order on each of the plurality of current collectors 11 on which the insulating layer 13 is laminated (steps S23, S24 and S25 in FIG. 14). Furthermore, as necessary, the electrode active material layer 12, the solid electrolyte layer 30 and the counter electrode active material layer 22 laminated in steps S23, S24 and S25 are subjected to high pressure pressing (step S26 in FIG. 14). Furthermore, if necessary, a heat treatment is performed on each of the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 laminated in steps S23, S24, and S25. In steps S23, S24, S25, and S26, the same method as in steps S13, S14, S15, and S16 described above may be used.

[0152] Next, in the first laminate lamination step, a plurality of laminate plates are laminated so that the positions of the insulating layers 13 of the plurality of laminate plates formed in the first laminate formation step overlap in a plan view (step S27 in FIG. 14). As a result, a multilayer plate in which a plurality of laminate plates are laminated is formed. FIG. 15 is a schematic cross-sectional view showing an example of a multilayer plate according to the present embodiment. FIG. 15 shows a multilayer plate 45 in which laminate plates 41 are laminated. As shown in FIG. 15, in the first laminate lamination step, a plurality of laminate plates 41 are laminated so that one of the counter electrode active material layers 22 of the adjacent laminate plates 41 faces the other current collector 11. For example, a pressing process is performed to press the stacked plurality of laminate plates 41 from both sides in the stacking direction, thereby joining the plurality of laminate plates 41 to each other to form a multilayer plate 45. In the multilayer electrode plate 45, of the adjacent laminated electrode plates 41, the current collector 11 of the upper laminated electrode plate 41 and the counter electrode active material layer 22 of the lower laminated electrode plate 41 are in contact with each other.

[0153] If the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are subjected to high-pressure pressing when forming the laminated electrode plate 41, high-pressure pressing is not required in the pressing process when forming the multilayer electrode plate 45. For example, the pressure of the pressing process for joining the laminated electrode plates 41 together in step S27 is lower than the pressure of the high-pressing process in step S26. This allows the multilayer electrode plate 45 to be formed without destroying the interface formed in the first laminate formation process.

[0154] (3) Cutting process and current collector lamination process Next, the cutting step and the current collector lamination step will be described. In the cutting step, the multilayer electrode plate 45, that is, the current collector 11 on which the power generating element section 40 is laminated in the power generating element lamination step, is cut in a lump in the lamination direction at the position where the insulating layer 13 is divided (step S28 in FIG. 14). As shown in FIG. 15, for example, the multilayer electrode plate 45 is cut by a blade or laser light at the positions of the dashed lines C5, C6, C7, and C8 where the insulating layer 13 is arranged. At the positions of the dashed lines C5, C6, C7, and C8, a plurality of laminated electrode plates 41 are laminated, and these are cut in a lump. In this way, by cutting a plurality of laminated electrode plates 41 in a lump, it is not necessary to manufacture and then laminate unit cells having the shape after cutting, so that the number of times the power generating element section 40 is laminated in the power generating element lamination step is significantly reduced. Therefore, a laminated battery can be efficiently manufactured.

[0155] Next, in the current collector lamination step, a current collector 21 is laminated as an additional current collector on the surface of the power generating element section 40 opposite to the current collector 11 in the multilayer electrode plate 45 after being cut in the cutting step (step S29 in FIG. 14). Specifically, in the cut multilayer electrode plate 45, the current collector 21 is joined by pressing or the like to the surface of the power generating element section 40 opposite to the current collector 11 in the multilayer electrode plate 41 in which no other multilayer electrode plate 41 is laminated on the surface opposite to the current collector 11 in the power generating element section 40. In the example shown in FIG. 15, the current collector 21 is joined onto the exposed counter electrode active material layer 22 on the upper surface of the uppermost laminate electrode plate 41. This results in the battery 100 shown in FIG. 12 being obtained.

[0156] The cutting step and the current collector stacking step may be performed in reverse order. That is, current collector 21 may be stacked on the surface of power generating element section 40 of multilayer electrode plate 45 before cutting in the cutting step opposite current collector 11, and then multilayer electrode plate 45 on which current collector 21 is stacked may be cut in the stacking direction at a position where insulating layer 13 is to be divided.

[0157] In this manner, by using the battery manufacturing method according to the present embodiment, a direct stack type high voltage battery 100 can be manufactured.

[0158] [Variation 1] The following describes Modification 1 of Embodiment 2. In the following description of Modification 1 of Embodiment 2, differences from Embodiments 1 and 2 will be mainly described, and descriptions of commonalities will be omitted or simplified.

[0159] A manufacturing method of the battery according to this modification will be described. The manufacturing method of the battery according to this modification is different from the manufacturing method of the battery according to the second embodiment in that, instead of the laminated electrode plate 41, a laminated electrode plate 42 is formed in which a power generating element part 40 is laminated on the surface of the current collector 11 on which the insulating layer 13 is not laminated.

[0160] In the battery manufacturing method according to this modification, the insulating layer laminating step is the same as the insulating layer laminating step according to the second embodiment (steps S21 and S22 in FIG. 14).

[0161] The power generating element lamination step in this modification includes a second laminate formation step and a second laminate lamination step. FIG. 16 is a schematic cross-sectional view showing an example of a laminated electrode plate according to this modification. As shown in FIG. 16, in the second laminate formation step, a plurality of laminated electrode plates 42 are formed by laminating a power generating element part 40 on each of a plurality of current collectors 11 on which an insulating layer 13 is laminated, so that the counter electrode active material layer 22 faces the surface of the current collector 11 on which the insulating layer 13 is not laminated. Specifically, the counter electrode active material layer 22, the solid electrolyte layer 30, and the electrode active material layer 12 are laminated in this order on the surface of the current collector 11 on which the insulating layer 13 is not laminated, thereby forming the laminated electrode plate 42. In laminating the counter electrode active material layer 22, the solid electrolyte layer 30, and the electrode active material layer 12, a method similar to that of the above-mentioned steps S15, S14, and S13 may be used. Furthermore, as required, a high-pressure press treatment is performed on each of the stacked counter electrode active material layer 22, solid electrolyte layer 30, and electrode active material layer 12. The high-pressure press treatment may be performed using a method similar to that of step S16 described above. Furthermore, as required, a heat treatment is performed on each of the stacked counter electrode active material layer 22, solid electrolyte layer 30, and electrode active material layer 12.

[0162] Next, in the second laminate lamination step, the multiple laminate plates 42 are laminated so that the positions of the insulating layers 13 of the multiple laminate plates 42 formed in the second laminate formation step overlap in a plan view. FIG. 17 is a schematic cross-sectional view showing an example of a multilayer plate according to this modified example. As shown in FIG. 17, in the second laminate lamination step, the multiple laminate plates 42 are laminated so that the electrode active material layer 12 of one of the adjacent laminate plates 42 covers the insulating layer 13 of the other. For example, the multiple laminate plates 42 are joined together by pressing the stacked multiple laminate plates 42 from both sides in the lamination direction to form a multilayer plate 46. In the multilayer plate 46, the current collector 11 and the insulating layer 13 of the upper laminate plate 42 of the adjacent laminate plates 42 are in contact with the electrode active material layer 12 of the lower laminate plate 42. As a result, in the multi-layer electrode plate 46, a covering structure is formed in which the electrode active material layer 12 of the lower laminated electrode plate 42 covers the insulating layer 13 of the upper laminated electrode plate 42 among the adjacent laminated electrode plates 42.

[0163] Next, the collector lamination step and the cutting step are performed. FIG. 18 is a diagram for explaining the collector lamination step and the cutting step in the manufacturing method of the battery according to this modified example. As shown in FIG. 18, the current collector 11a on which the insulating layer 13 is laminated is laminated as an additional current collector on the multilayer electrode plate 46. The current collector 11a on which the insulating layer 13 is laminated has the same shape and material as the current collector 11 on which the insulating layer 13 is laminated, for example, formed in the insulating layer lamination step. As shown in FIG. 18, the multilayer electrode plate 46 and the current collector 11a on which the insulating layer 13 is laminated are laminated so that the electrode active material layer 12 of the multilayer electrode plate 46 covers the insulating layer 13 laminated on the current collector 11a. In addition, the multilayer electrode plate 46 and the current collector 11a on which the insulating layer 13 is laminated are laminated so that the insulating layer 13 of each of the multiple laminated electrode plates 42 and the insulating layer 13 laminated on the current collector 11a overlap in a plan view. Specifically, in the multilayer electrode plate 46, among the multiple laminated electrode plates 42, a collector 11a having an insulating layer 13 laminated thereon by pressing or the like is joined to the surface opposite the current collector 11 of the power generating element section 40 of a laminated electrode plate 42 on which no other laminated electrode plate 42 is laminated on the surface opposite the current collector 11 of the power generating element section 40.

[0164] Next, in the cutting step, the multilayer electrode plate 46, i.e., the current collector 11 on which the power generating element part 40 is laminated, is cut in the lamination direction at a position where the insulating layer 13 is divided, as shown in FIG. 18. Specifically, for example, at the positions of the dashed lines C9, C10, C11, and C12 where the insulating layer 13 is arranged, the multilayer electrode plate 46 on which the current collector 11a is laminated is cut by a blade or laser light, etc. At the positions of the dashed lines C9, C10, C11, and C12, a plurality of laminated electrode plates 42 are laminated, and these are cut in a lump. In this manner, a stacked type battery 101 in which a plurality of unit cells are stacked is obtained. The battery 101 is a series stacked type battery like the battery 100. In the battery 101, the insulating layer 13 stacked on the current collector 11 located at the top or bottom in the lamination direction is exposed.

[0165] The cutting step and the current collector lamination step may be performed in reverse order.

[0166] In this way, by using the battery manufacturing method according to this modified example, a direct stack type high voltage battery 101 can be manufactured.

[0167] [Variation 2] The following describes Modification 2 of Embodiment 2. In the following description of Modification 2 of Embodiment 2, differences from Embodiments 1 and 2 will be mainly described, and descriptions of commonalities will be omitted or simplified.

[0168] A method for manufacturing a battery according to this modification will be described. The method for manufacturing a battery according to this modification differs from the method for manufacturing a battery according to the second embodiment in that a power generating element unit 40 is laminated on both sides of a current collector 11 having insulating layers 13 laminated on both sides.

[0169] First, in the insulating layer lamination step, insulating layers 13 are laminated on both sides of a current collector 11. The positions of the insulating layers 13 laminated on both sides are the same in a plan view. The method of laminating the insulating layers 13 on the current collector 11 may be the same as the method of steps S11 and S12 described above. For example, an insulating layer 13 is laminated on the surface of the current collector 11 on which the insulating layer 13 is not laminated, as shown in FIG. 6A, 6B, or 6C.

[0170] Next, a power generating element lamination step is performed. FIG. 19 is a schematic cross-sectional view showing an example of a laminated electrode plate having an insulating layer according to this modification. FIG. 20 is a schematic cross-sectional view showing an example of a laminated electrode plate having no insulating layer according to this modification. FIG. 21 is a schematic cross-sectional view showing an example of a multi-layered electrode plate according to this modification. In the power generating element lamination step according to this modification, for example, a laminated electrode plate 43a having an insulating layer 13 as shown in FIG. 19 and a laminated electrode plate 43b having no insulating layer 13 as shown in FIG. 20 are formed. The electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are laminated and coated in this order on one surface of the current collector 11 having the insulating layer 13 laminated on both surfaces, to form a laminated electrode plate 43a. That is, the power generating element part 40 is laminated on one surface of the current collector 11 having the insulating layer 13 laminated on both surfaces such that the electrode active material layer 12 of the power generating element part 40 covers the insulating layer 13. In the laminated electrode plate 43a, a coating structure in which the electrode active material layer 12 coats the insulating layer 13 is formed.

[0171] Also, for example, a current collector 25 having the same shape as the current collector 11 in a plan view is prepared, and the counter electrode active material layer 22, the solid electrolyte layer 30, and the electrode active material layer 12 are laminated and coated in this order on one surface of the current collector 25, to form a laminated electrode plate 43b.

[0172] The stacking of the power generating element parts 40 of the laminated electrode plates 43a and 43b may be performed using the same methods as those in steps S13, S14, and S15 described above. Furthermore, as necessary, the stacked electrode active material layers 12, solid electrolyte layers 30, and counter electrode active material layers 22 are each subjected to a high-pressure press treatment. Furthermore, as necessary, the stacked electrode active material layers 12, solid electrolyte layers 30, and counter electrode active material layers 22 are each subjected to a heat treatment.

[0173] 21, the laminated electrode plates 43a and the laminated electrode plates 43b are alternately stacked such that the electrode active material layers 12 of the laminated electrode plates 43b cover the insulating layers 13 of the laminated electrode plates 43a, thereby forming a multilayer electrode plate 47. In forming the multilayer electrode plate 47, the laminated electrode plates 43a and the laminated electrode plates 43b are alternately stacked such that the positions of the insulating layers 13 of the multiple laminated electrode plates 43a overlap in a plan view. The stacked laminated electrode plates 43a and the laminated electrode plates 43b are pressed from both sides in the stacking direction, thereby joining the laminated electrode plates 43a and the laminated electrode plates 43b, thereby forming the multilayer electrode plate 47.

[0174] FIG. 22 is a schematic cross-sectional view showing another example of the laminated electrode plate according to this modified example. For example, instead of forming the laminated electrode plate 43a and the laminated electrode plate 43b, a laminated electrode plate 43c shown in FIG. 22 may be formed. First, the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22 are laminated and coated in this order on both sides of the current collector 11, on both sides of which the insulating layer 13 is laminated, so that the electrode active material layer 12 covers the insulating layer 13, to form a laminate in which the power generating element part 40 is laminated on both sides of the current collector 11. In laminating the electrode active material layer 12, the solid electrolyte layer 30, and the counter electrode active material layer 22, each layer may be laminated and coated in sequence on one side of the current collector 11, or the same layer may be laminated and coated on both sides of the current collector 11 at the same time. Then, the obtained laminate is laminated on the current collector 25 to form the laminated electrode plate 43c. The laminated electrode plate 43c has a structure in which one laminated electrode plate 43a and one laminated electrode plate 43b are laminated, and may be formed by laminating one laminated electrode plate 43a and one laminated electrode plate 43b. Next, a multi-layer electrode plate 47 is formed by laminating a plurality of laminated electrode plates 43c.

[0175] The multilayer electrode plate 47 has a structure in which the current collector 11 on which the insulating layer 13 is laminated, two power generation element parts 40, and a current collector 25 are laminated. The multilayer electrode plate 47 also has a structure in which the current collector 11 is sandwiched between the two power generation element parts 40 so that the electrode active material layer 12 covers the insulating layers 13 laminated on both sides of the current collector 11, and one of the two power generation element parts 40 is sandwiched between the current collector 11 on which the insulating layer 13 is laminated and the current collector 25. As will be described in detail later, the current collector 21 is laminated on the other of the two power generation element parts 40 located at the top, on the opposite side to the current collector 11.

[0176] In this modification, the multilayer electrode plate 47 has three sets of alternately stacked laminated electrode plates 43a and laminated electrode plates 43b, but may have one or more sets or two or less sets, or may have four or more sets. When the multilayer electrode plate 47 is composed of one set of laminated electrode plates 43a and laminated electrode plates 43b, the multilayer electrode plate 47 has the same configuration as the laminated electrode plate 43c.

[0177] Next, a cutting step is performed. In the cutting step, the multilayer electrode plate 47, that is, the current collector 11 in which the current collector 25 and the two power generating element parts 40 are laminated in the power generating element lamination step, is cut in a lump in the lamination direction at a position where the insulating layer 13 is divided. As shown in Fig. 21, for example, the multilayer electrode plate 47 is cut with a blade or laser light at the positions of the dashed lines C13, C14, C15, and C16 where the insulating layer 13 is arranged. At the positions of the dashed lines C13, C14, C15, and C16, a plurality of laminated electrode plates 43a and a plurality of laminated electrode plates 43b are laminated, and these are cut in a lump.

[0178] Next, a collector lamination step is performed. In the collector lamination step, a current collector 21 is laminated as an additional current collector on the surface of the multilayer electrode plate 47 after cutting in the cutting step on which the current collector 11 of the power generating element part 40 is not laminated. Specifically, in the cut multilayer electrode plate 47, among the multiple laminate electrode plates 43a, the laminate electrode plate 43b is not laminated on the surface opposite to the current collector 11 of the power generating element part 40, and the current collector 21 is joined by pressing or the like to the surface opposite to the current collector 11 of the power generating element part 40 of the laminate electrode plate 43a. FIG. 23 is a schematic cross-sectional view showing an example of a battery according to this modified example. Through such a collector lamination step, a battery 102 shown in FIG. 23 is obtained.

[0179] The cutting step and the current collector lamination step may be performed in reverse order.

[0180] 23, the battery 102 includes a plurality of batteries 50c and a current collector 21. The battery 50c includes a current collector 25, two counter electrode active material layers 22 disposed opposite each other above the current collector 25, two solid electrolyte layers 30 disposed opposite each other between the two counter electrode active material layers 22, two electrode active material layers 12 disposed opposite each other between the two solid electrolyte layers 30, a current collector 11 disposed between the two electrode active material layers 12, and insulating layers 13 disposed between the current collector 11 and the two electrode active material layers 12 and stacked on ends of the current collector 11 in a plan view.

[0181] In the battery 102, the multiple batteries 50c are stacked such that the current collector 25 of one of the adjacent batteries 50c and the counter electrode active material layer 22 of the other face each other. This results in a structure in which the function of the current collector 25 is shared by the adjacent batteries 50c. In addition, the current collector 21 is stacked on the counter electrode active material layer 22 of the battery 50c stacked on the top. The battery 102 has a structure in which the electrode active material layer 12 is stacked on both sides of the current collector 11, and the counter electrode active material layer 22 is stacked on both sides of the current collector 25. This results in the battery 102 being a parallel stacked battery. In order to extract current, the current collector 21 and the current collector 25 are electrically connected by a lead or the like, and the current collectors 11 are electrically connected to each other by a lead or the like, thereby functioning as a parallel stacked battery. In the example shown in FIG. 23, the number of stacked batteries 50c is three, but it may be one to two or less, or it may be four or more.

[0182] In the battery 50c, the portion consisting of the upper current collector 21, the counter electrode active material layer 22, the solid electrolyte layer 30, the electrode active material layer 12, the insulating layer 13, and the current collector 11 has the same layered configuration and shape as the battery 50 according to the first embodiment.

[0183] The side of the battery 102 is a cut surface formed by the above-mentioned manufacturing method. The side of the batteries 50b and the current collector 21 are flush with each other. That is, a single flat plane is formed on the side of the battery 102. On the side of the battery 102, each layer may be exposed, or a sealing member or the like may be provided. FIG. 24 is a schematic cross-sectional view showing another example of the battery according to this modification. As shown in FIG. 24, the battery 102a has a structure in which the side of the battery 102 is covered with the sealing members 60a and 60b. The side of the battery 102 covered by the sealing member 60a and the side of the battery 102 covered by the sealing member 60b are arranged opposite to each other. Covering the side of the battery 102. Also, in the battery 102a, the entire side of the battery 102a is not covered by the sealing member 60a or 60b. For example, in order to connect a lead for extracting electricity as described above, sealing member 60a does not cover the exposed portion of current collector 25, and sealing member 60b does not cover the exposed portion of current collector 11.

[0184] In this way, by using the battery manufacturing method according to this modification, it is possible to manufacture a parallel-stacked, high-capacity battery 102 that exhibits the same effects as the battery 50 according to the first embodiment.

[0185] (Embodiment 3) The following describes embodiment 3. In the following description of embodiment 3, differences from embodiments 1 and 2 will be mainly described, and descriptions of commonalities will be omitted or simplified.

[0186] Fig. 25 is a cross-sectional view showing a schematic configuration of a battery according to the present embodiment. As shown in Fig. 25, the battery 104 includes a plurality of the batteries 50 according to the first embodiment, and has a structure in which the plurality of batteries 50 are stacked. The plurality of batteries 50 are stacked such that one electrode layer 10 and the other counter electrode layer 20 of adjacent batteries 50 in the stacking direction face each other. In other words, the battery 104 is a series-stacked battery. As a result, a high-voltage battery 104 can be realized by using the battery 50 according to the first embodiment.

[0187] The side surface of the battery 104 is a flat plane, in other words, the side surfaces of each of the multiple batteries 50 are flush with each other. Note that the multiple batteries 50 may be stacked with a shift in the direction perpendicular to the stacking direction in order to connect leads or the like.

[0188] The battery 104 is manufactured by stacking a plurality of batteries 50, for example, such that one electrode layer 10 and the other counter electrode layer 20 of adjacent batteries 50 in the stacking direction face each other. Alternatively, in a laminated electrode plate 41 (see FIG. 7A ) before being cut, a current collector 21 may be stacked on the side opposite to the current collector 11 of the power generating element section 40, and a plurality of laminated electrode plates 41 each having the current collector 21 stacked thereon may be stacked, and then the laminated electrode plates 41 may be cut in the stacking direction at a position to divide the insulating layer 13, thereby manufacturing the battery 104.

[0189] When the battery 50 is stacked, the two current collectors 11 and 21 are adjacent to each other. However, the battery may be one in which one of the adjacent current collectors 11 and 21 is missing.

[0190] Also, Fig. 26 is a cross-sectional view showing a schematic configuration of another example of the battery according to this modification. As shown in Fig. 26, the battery 105 includes a plurality of batteries 51 according to the modification 1 of the embodiment 1, and has a structure in which the plurality of batteries 51 are stacked. The plurality of batteries 51 are stacked such that one electrode layer 10a and the other counter electrode layer 20a of the batteries 51 adjacent to each other in the stacking direction face each other. In other words, the battery 105 is a series-stacked battery. As a result, a high-voltage battery 105 can be realized by using the battery 51 according to the modification 1 of the embodiment 1.

[0191] Although the battery 104 and the battery 105 are serially stacked batteries, they may be parallel stacked batteries having a structure in which the electrode layers or counter electrode layers of adjacent cells face each other. In the parallel stacked batteries, a high capacity battery can be realized.

[0192] By stacking the batteries 50 or 51, which are single cells, in this manner, a high-capacity or high-voltage battery that can achieve the same effects as the batteries 50 or 51 can be realized.

[0193] (Other embodiments) Although the battery and the manufacturing method thereof according to the present disclosure have been described based on the embodiments, the present disclosure is not limited to these embodiments. As long as they do not deviate from the gist of the present disclosure, various modifications conceivable by those skilled in the art to the embodiments and other forms constructed by combining some of the components in the embodiments are also included in the scope of the present disclosure.

[0194] In the above embodiment, the battery is composed of a current collector, an insulating layer, an electrode active material layer, a solid electrolyte layer, and a counter electrode active material layer, but is not limited thereto. For example, within the range of the battery characteristics, a bonding layer or the like for reducing electrical resistance and improving bonding strength may be provided between each layer of the battery.

[0195] In the above embodiment, the battery includes an insulating layer located between the current collector and the electrode active material layer at the end of the electrode layer, but may further include a second insulating layer located between the current collector and the counter electrode active material layer at the end of the counter electrode layer. In this case, the length of the second insulating layer from the outer periphery of the electrode active material layer in a plan view may be shorter than the length of the insulating layer from the outer periphery of the electrode active material layer. This prevents the counter electrode active material layer from being exposed even if the end of the current collector on the counter electrode active material layer side peels off, and the second insulating layer is narrower than the insulating layer in a plan view, so that the area of ​​the electrode active material layer is substantially smaller than the area of ​​the counter electrode active material layer.

[0196] In the above embodiment, the insulating layer is located on the outer periphery of the electrode layer in a plan view and has a frame shape, but is not limited thereto. For example, in a battery, there may be a region on the outer periphery of the electrode layer where no insulating layer is provided.

[0197] In addition, for example, in the above embodiment, when the battery is surrounded by a case or a substrate, and a part of the case or the substrate functions as a current collector, a current collector on the counter electrode active material layer side of the battery may not be provided. In other words, the counter electrode layer may be composed of a counter electrode active material layer.

[0198] In the above embodiment, the current collector, the electrode active material layer, the solid electrolyte layer, and the counter electrode active material layer have the same shape and position in a plan view, but this is not limited thereto. At least one of the current collector, the electrode active material layer, the solid electrolyte layer, and the counter electrode active material layer may have a different shape or position in a plan view. For example, the current collector may have a terminal portion for connecting to a lead or the like, which protrudes from the end of the electrode active material layer in a plan view. In other words, the current collector may have a region disposed outside the electrode active material layer in a plan view.

[0199] In the above embodiment, the power generating element is formed by sequentially stacking the electrode active material layer, the solid electrolyte layer, and the counter electrode active material layer on the current collector in the power generating element stacking step, but this is not limited thereto. For example, the power generating element may be formed by sequentially stacking the electrode active material layer, the solid electrolyte layer, and the counter electrode active material layer on a sheet-like substrate in the power generating element stacking step, and the formed power generating element may be removed from the substrate and stacked on the current collector.

[0200] Furthermore, the above-described embodiment can be modified, replaced, added, omitted, and the like in various ways within the scope of the claims or their equivalents. [Industrial Applicability]

[0201] The battery according to the present disclosure can be used, for example, as a secondary battery such as an all-solid-state battery for use in various electronic devices or automobiles. [Explanation of symbols]

[0202] 10, 10a, 10b electrode layer 11, 11a, 11b, 21, 21a, 21b, 25 Current collector 12, 12a, 12b electrode active material layer 12s, 22s main surface 13, 13a, 13b Insulating layer 20, 20a, 20b, 23 Counter electrode layer 22, 22a, 22b Counter electrode active material layer 30, 30a, 30b solid electrolyte layer 40 Electric element 41, 41a, 41b, 42, 43a, 43b, 43c Laminated plates 45, 46, 47 Multilayer Plates 50, 50a, 50b, 50c, 51, 52, 100, 100a, 101, 102, 102a, 104, 105 battery 51s, 52s side 60, 60a, 60b Sealing member

Claims

1. A positive electrode layer; a negative electrode layer disposed opposite the positive electrode layer; a solid electrolyte layer located between the positive electrode layer and the negative electrode layer; Equipped with The positive electrode layer is A current collector; a positive electrode active material layer located between the current collector and the solid electrolyte layer; an insulating layer located between the current collector and the positive electrode active material layer at an end of the positive electrode layer, The negative electrode layer is a negative electrode active material layer disposed opposite the positive electrode active material layer, the positive electrode active material layer has a region that does not overlap with the insulating layer in a plan view, a side surface of the insulating layer and a side surface of the positive electrode active material layer are flush with each other, a side surface of the insulating layer is flush with a side surface of the current collector; the positive electrode active material layer does not protrude beyond the negative electrode active material layer in a plan view, The insulating layer includes a resin. battery.

2. A positive electrode layer; a negative electrode layer disposed opposite the positive electrode layer; a solid electrolyte layer located between the positive electrode layer and the negative electrode layer; Equipped with The positive electrode layer is A current collector; a positive electrode active material layer located between the current collector and the solid electrolyte layer; an insulating layer located between the current collector and the positive electrode active material layer at an end of the positive electrode layer, The negative electrode layer is a negative electrode active material layer disposed opposite the positive electrode active material layer, the positive electrode active material layer has a region that does not overlap with the insulating layer in a plan view, a side surface of the insulating layer and a side surface of the positive electrode active material layer are flush with each other, the positive electrode active material layer does not protrude beyond the negative electrode active material layer in a plan view, The insulating layer includes a resin. battery.

3. In a plan view, the positive electrode active material layer and the negative electrode active material layer have the same shape and position.

3. The battery of claim 1 or 2.

4. A battery, A positive electrode layer; a negative electrode layer disposed opposite the positive electrode layer; a solid electrolyte layer located between the positive electrode layer and the negative electrode layer; Equipped with The positive electrode layer is A current collector; a positive electrode active material layer located between the current collector and the solid electrolyte layer; an insulating layer located between the current collector and the positive electrode active material layer at an end of the positive electrode layer, The negative electrode layer is a negative electrode active material layer disposed opposite the positive electrode active material layer, the positive electrode active material layer has a region that does not overlap with the insulating layer in a plan view, a side surface of the insulating layer and a side surface of the positive electrode active material layer are flush with each other, a side surface of the insulating layer is flush with a side surface of the current collector; the positive electrode active material layer does not protrude beyond the negative electrode active material layer in a plan view, A side surface of the battery is inclined with respect to the stacking direction in a direction in which an area of ​​the negative electrode layer is larger than an area of ​​the positive electrode layer in a plan view. battery.

5. A battery, A positive electrode layer; a negative electrode layer disposed opposite the positive electrode layer; a solid electrolyte layer located between the positive electrode layer and the negative electrode layer; Equipped with The positive electrode layer is A current collector; a positive electrode active material layer located between the current collector and the solid electrolyte layer; an insulating layer located between the current collector and the positive electrode active material layer at an end of the positive electrode layer, The negative electrode layer is a negative electrode active material layer disposed opposite the positive electrode active material layer, the positive electrode active material layer has a region that does not overlap with the insulating layer in a plan view, a side surface of the insulating layer and a side surface of the positive electrode active material layer are flush with each other, A side surface of the battery is inclined with respect to the stacking direction in a direction in which an area of ​​the negative electrode layer is larger than an area of ​​the positive electrode layer in a plan view. battery.

6. The insulating layer includes a metal oxide. The battery of any one of claims 1 to 5.

7. the insulating layer is located in a region having a length from an outer periphery of the positive electrode active material layer of 1 mm or less in a plan view; The battery of any one of claims 1 to 6.

8. The thickness of the insulating layer is 5 μm or less. The battery of any one of claims 1 to 7.

9. a side surface of each of the solid electrolyte layer, the current collector, the positive electrode active material layer, the negative electrode active material layer, and the insulating layer is exposed; 9. The battery of claim 1 .

10. A side surface of the positive electrode layer, a side surface of the negative electrode layer, and a side surface of the solid electrolyte layer are flush with each other.

10. The battery of claim 1.

11. The side surface of the battery is a cut surface; The battery of any one of claims 1 to 10.

12. The shape of the cut surface is rectangular or trapezoidal. The battery of claim 11.

13. The insulating layer is provided on the outer periphery of the positive electrode layer in a plan view and has a frame shape.

13. The battery of claim 1.

14. The solid electrolyte layer contains a solid electrolyte having lithium ion conductivity.

14. The battery of claim 1.

Citation Information

Patent Citations

  • Lithium-ion secondary battery

    JP2008262791A

  • Nonaqueous electrolyte battery and method for manufacturing nonaqueous electrolyte battery

    JP2013093241A

  • Electrode and battery

    JP2016207286A

  • Bipolar lamination type all-solid type lithium secondary battery and method for manufacturing the same

    JP2017168429A

  • Method for manufacturing all-solid battery

    JP2019139921A