Method for grinding a workpiece

A two-step grinding process with controlled water supply and feed rates addresses the challenge of grinding hard substrates by reducing load and wear on the wheel, ensuring efficient and high-quality processing.

JP7588494B2Active Publication Date: 2024-11-22DISCO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020184622
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-04
Publication Date
2024-11-22
Estimated Expiration
2040-11-04

AI Technical Summary

Technical Problem

Existing grinding methods for hard substrates like silicon carbide or sapphire face challenges with the grinding wheel failing to bite into the workpiece, leading to increased grinding load and spindle current values, and excessive wear of the grinding wheel, especially when processing multiple sheets.

Method used

A method involving a two-step grinding process with controlled grinding water supply and feed rates, using different grain sizes for rough and finish grinding, and adjusting water amounts to prevent excessive wear and promote self-sharpening of the grinding wheel.

Benefits of technology

The method effectively reduces grinding load while preventing excessive wear on the grinding wheel, maintaining high processing quality and reducing the frequency of wheel replacements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588494000001
    Figure 0007588494000001
  • Figure 0007588494000002
    Figure 0007588494000002
  • Figure 0007588494000003
    Figure 0007588494000003
Patent Text Reader

Abstract

To provide a grinding method for a workpiece, which can prevent excessive consumption of a grinding stone and, at the same time, can reduce a grinding load as well.SOLUTION: A grinding method for a workpiece, for thinning the workpiece to a finished thickness using a grinding device, includes: a first grinding step 1001 of grinding the workpiece to a predetermined thickness by grinding and feeding a rough grinding unit while supplying a first amount of grinding water with which consumption of a grinding stone can be suppressed; and a second grinding step 1002 of, after the first grinding step 1001, grinding the workpiece to the finished thickness by grinding and feeding the rough grinding unit while supplying a second amount of grinding water decreased from the first amount of grinding water to increase consumption of the grinding stone to promote autogenous cutting edge, and then promoting dressing of the grinding stone to prepare for a process for a next workpiece.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for grinding a workpiece. [Background technology]

[0002] Grinding devices have been used to thin workpieces such as wafers on which semiconductor devices are formed (see, for example, Patent Documents 1 and 2). The above-mentioned grinding devices have a problem that when grinding hard substrates such as silicon carbide (SiC) and sapphire, the grinding wheel does not bite into the workpiece, especially at the beginning of processing, which increases the grinding load and makes it easy for the current value of the spindle to increase.

[0003] Therefore, if the grinding device reduces the amount of grinding water, the wear of the grinding wheel increases, promoting self-sharpening and reducing the grinding load. However, when processing multiple pieces continuously, the grinding device is not preferable because the wear of the grinding wheel increases, which increases the cost and the frequency of replacing the grinding wheel.

[0004] Also, a grinding device has been proposed that reduces the amount of grinding water at the start of processing to make it easier for the grinding wheel to bite into the workpiece (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-24041 A [Patent Document 2] JP 2017-56523 A [Patent Document 3] JP 2014-124690 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, if glazing has occurred due to the processing of the previous workpiece, even if the amount of grinding water is reduced at the start of processing when the grinding load is greatest, the grinding wheel will not bite into the workpiece, and the grinding load will increase, making it difficult to suppress the increase in the spindle current value.

[0007] An object of the present invention is to provide a method for grinding a workpiece, which can reduce the grinding load while preventing excessive wear of the grinding wheel. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems and achieve the object, the present invention provides a method for grinding a workpiece to thin the workpiece to a finish thickness using a grinding device including a holding table for holding the workpiece, a grinding unit having a spindle on which a grinding wheel having grinding wheels arranged in an annular shape for grinding the workpiece held on the holding table is mounted and a motor for rotating the spindle, a grinding feed unit for moving the grinding unit toward and away from the holding table, a grinding water supply unit for supplying grinding water to an upper surface of the workpiece held on the holding table in an adjustable flow rate, and a control unit for controlling each unit, the method comprising: a first grinding step for grinding the workpiece to a predetermined thickness by feeding the grinding unit while supplying grinding water at a first amount of grinding water capable of suppressing wear of the grinding wheel; and a second amount of grinding water supplied after the first grinding step, the second amount of grinding water being reduced from the first amount of grinding water to increase wear of the grinding wheel and promote self-sharpening. A grinding feed rate at which the grinding unit approaches the holding table is reduced below a grinding feed rate in the first grinding step. and a second grinding step in which the grinding unit is fed to grind the workpiece to a finishing thickness, facilitating the sharpening of the grinding wheel and preparing for the processing of the next workpiece.

[0009] In the method for grinding a workpiece, the grinding unit includes a rough grinding unit using a grinding wheel with a coarse grain size, and a finish grinding unit using a grinding wheel with a fine grain size to grind the workpiece ground by the rough grinding unit, and the first grinding step and the second grinding step may be performed in the rough grinding unit. In the method for grinding a workpiece, in the first grinding step, the grinding feed speed of the grinding unit may be reduced stepwise. Effect of the Invention

[0010] The method for grinding a workpiece of the present invention has the effect of preventing excessive wear of the grinding wheel while also reducing the grinding load. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a perspective view showing an example of the configuration of a grinding device used in the method for grinding a workpiece according to the first embodiment. [Diagram 2] FIG. 2 is a perspective view of a workpiece to be processed by the method for grinding a workpiece according to the first embodiment. [Diagram 3] FIG. 3 is a cross-sectional view that typically shows the configuration of a grinding unit, a holding table, and a grinding water supply unit of the grinding apparatus shown in FIG. [Figure 4] FIG. 4 is a flowchart showing the flow of the method for grinding a workpiece according to the first embodiment. [Diagram 5] FIG. 5 is a diagram showing changes in the amount of grinding water and the spindle current value in the method for grinding a workpiece shown in FIG. [Figure 6] FIG. 6 is a diagram showing changes in the amount of grinding water and the spindle current value in Comparative Example 1. [Figure 7] FIG. 7 is a diagram showing changes in the amount of grinding water and the spindle current value in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.

[0013] [Embodiment 1] A method for grinding a workpiece according to a first embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a perspective view showing a configuration example of a grinding device used in the method for grinding a workpiece according to the first embodiment. FIG. 2 is a perspective view of a workpiece to be processed in the method for grinding a workpiece according to the first embodiment. FIG. 3 is a cross-sectional view showing a schematic configuration of a grinding unit, a holding table, and a grinding water supply unit of the grinding device shown in FIG. 1. FIG. 4 is a flowchart showing the flow of the method for grinding a workpiece according to the first embodiment. FIG. 5 is a diagram showing changes in the amount of grinding water and the spindle current value in the method for grinding a workpiece shown in FIG. 4.

[0014] (Workpiece) The method for grinding a workpiece according to the first embodiment is a grinding method for thinning a workpiece 200 shown in Fig. 2 using a grinding device 1 shown in Fig. 1. The workpiece 200 to be processed by the method for grinding a workpiece according to the first embodiment is a wafer such as a disk-shaped semiconductor wafer having a silicon substrate 201, or an optical device wafer having a substrate 201 made of sapphire, SiC (silicon carbide), or the like. In the first embodiment, the disk-shaped substrate 201 of the workpiece 200 is made of a material harder than silicon, such as sapphire or SiC (silicon carbide).

[0015] 2, the workpiece 200 has devices 204 formed in each of a plurality of regions partitioned by a plurality of planned division lines 203 intersecting (orthogonal in the first embodiment) on a surface 202 of a substrate 201. The devices 204 are, for example, integrated circuits such as ICs (Integrated Circuits) or LSIs (Large Scale Integrations), image sensors such as CCDs (Charge Coupled Devices) or CMOSs ​​(Complementary Metal Oxide Semiconductors), or MEMS (Micro Electro Mechanical Systems). A protective member 210 is attached to the surface 202 side of the substrate 201 of the workpiece 200, and the surface 202 side is suction-held to the holding surface 71 via the protective member 210, and a back surface 205 on the back side of the surface 202 is ground.

[0016] Next, a grinding device 1 shown in Fig. 1 used in the grinding method of the workpiece according to the embodiment 1 will be described. The grinding device 1 is a processing device that grinds the back surface 205 of the workpiece 200. As shown in Fig. 2, the grinding device 1 mainly includes an apparatus main body 2, a rough grinding unit 3 (corresponding to a grinding unit), a finish grinding unit 4 (corresponding to a grinding unit), a grinding feed unit 5, a turntable 6, a plurality of holding tables 7 (three in the embodiment 1) installed on the turntable 6, cassettes 8 and 9, an alignment unit 10, a transport unit 11, a cleaning unit 12, a carry-in / out unit 13, and a control unit 100.

[0017] The turntable 6 is a disk-shaped table provided on the upper surface of the device body 2, and is rotatable in a horizontal plane and driven to rotate at a predetermined timing. On the turntable 6, for example, three holding tables 7 are arranged at equal intervals, for example, at a phase angle of 120 degrees. These three holding tables 7 have a holding table structure with a vacuum chuck connected to a suction source 72 on a holding surface 71, and the workpiece 200 is placed on the holding surface 71 and suction-holds the workpiece 200. During grinding, these holding tables 7 are rotated in a horizontal plane by a rotary drive mechanism around an axis parallel to the vertical direction, i.e., the Z-axis direction. In this way, the holding table 7 has a holding surface 71 that holds the workpiece 200 and is rotatable around the axis.

[0018] The holding table 7 is moved in sequence to the carry-in / out area 301 , the rough grinding area 302 , the finish grinding area 303 , and back to the carry-in / out area 301 by the rotation of the turntable 6 .

[0019] The loading / unloading area 301 is an area where the workpiece 200 is loaded and unloaded onto the holding table 7, the rough grinding area 302 is an area where the rough grinding unit 3 performs rough grinding (corresponding to grinding) of the workpiece 200 held on the holding table 7, and the finish grinding area 303 is an area where the finish grinding unit 4 performs finish grinding (corresponding to grinding) of the workpiece 200 held on the holding table 7.

[0020] The rough grinding unit 3 is a grinding unit that is equipped with a grinding wheel 32 for rough grinding, which has grinding stones 31 for rough grinding arranged in an annular shape for roughly grinding the workpiece 200 held on the holding table 7, and that roughly grinds the back surface 205 of the workpiece 200 held on the holding surface 71 of the holding table 7 in the rough grinding region 302. The finish grinding unit 4 is equipped with a grinding wheel 42 for finish grinding, which has grinding stones 41 for finish grinding the workpiece 200 held on the holding table 7 arranged in an annular shape for finish grinding the workpiece 200 held on the holding table 7, and that finish grinds the back surface 205 of the workpiece 200 held on the holding surface 71 of the holding table 7 in the finish grinding region 303.

[0021] For this reason, the rough grinding unit 3 is a grinding unit that uses a grinding wheel 32 for rough grinding, and the finish grinding unit 4 is a grinding unit that uses a grinding wheel 42 to finish grind the workpiece 200 that has been roughly ground by the rough grinding unit 3. Since the grinding units 3 and 4 have substantially the same configuration, the same parts will be denoted by the same reference numerals in the following description.

[0022] As shown in FIG. 1, the rough grinding unit 3 and the finish grinding unit 4 have a spindle 33 to which the grinding wheels 32, 42 are attached at the lower end, and a motor 34 that rotates the spindle 33 around an axis parallel to the vertical direction (also called the Z-axis direction). As shown in FIG. 3, the grinding wheels 32, 42 have an annular base 35 and a plurality of grinding wheels 31, 41 fixed to the lower surface of the annular base 35. The grinding wheels 31, 41 are arranged in the circumferential direction on the outer edge of the lower surface of the annular base 35. The grinding wheels 31, 41 are made of abrasive grains fixed with a bond. The abrasive grains of the grinding wheel 31 of the grinding wheel 32 are coarser (i.e., larger) than the abrasive grains of the grinding wheel 41 of the grinding wheel 42, and the abrasive grains of the grinding wheel 41 of the grinding wheel 42 are finer than the abrasive grains of the grinding wheel 31 of the grinding wheel 32.

[0023] The spindle 33 is accommodated in the spindle housing 36 so as to be rotatable about an axis parallel to the Z-axis direction perpendicular to the holding surface 71, and is rotated about the axis by the motor 34 attached to the spindle housing 36. The spindle 33 is formed in a cylindrical shape, and as shown in FIG. 3, a wheel mount 37 for mounting the grinding wheels 32, 42 is provided at the lower end. The wheel mount 37 protrudes from the lower end of the spindle 33 in the outer circumferential direction over the entire circumference, and the planar shape of the outer circumferential surface is formed into a circle. The upper surface of the annular base 35 is overlapped on the lower surface of the wheel mount 37, and the grinding wheels 32, 42 are fixed by bolts (not shown). The spindle 33 and the wheel mount 37 are arranged in positions that are coaxial with each other.

[0024] The grinding units 3, 4 rotate the spindle 33 and the grinding wheels 32, 42 around their axes using the motor 34 and supply grinding water to the back surface 205 of the workpiece 200 held on the holding table 7 in the grinding areas 302, 303 while the grinding feed unit 5 moves the grinding wheels 31, 41 closer to the holding table 7 at a predetermined feed speed, thereby rough-grinding or finish-grinding the back surface 205 of the workpiece 200.

[0025] Moreover, in the first embodiment, the grinding units 3 and 4 are provided with a current value measuring sensor 38 that measures the current value (hereinafter, referred to as the spindle current value) of the current flowing through the motor 34 when the spindle 33 rotates about its axis. The current value measuring sensor 38 outputs the measurement result to the control unit 100. Note that the spindle current value increases when the grinding load (which refers to the load that hinders the rotation of the grinding wheels 32 and 42) of the grinding units 3 and 4 increases, and decreases when the grinding load decreases.

[0026] The grinding units 3 and 4 each include a grinding water supply unit 14 shown in Fig. 3. The grinding water supply unit 14 supplies grinding water to the back surface 205 of the workpiece 200, which is the upper surface of the workpiece held on the holding table 7, in a manner that allows the flow rate of the grinding water to be adjustable. As shown in Fig. 3, the grinding water supply unit 14 includes a grinding water supply source 141, a grinding water supply passage 142, and a grinding water supply nozzle 143. The grinding water supply source 141 supplies grinding water to the grinding water supply passage 142 and the grinding water supply nozzle 143.

[0027] The grinding water supply passage 142 includes an intra-spindle passage 144 extending along the axis at the center of the spindle 33, an intra-mount passage 145 communicating with the intra-spindle passage 144 and extending from the intra-spindle passage 144 toward the outer periphery of the wheel mount 37 and opening at the lower surface of the wheel mount 37, and an intra-base passage 146 communicating with the intra-mount passage 145 and opening at the inner circumferential surface of the annular base 35 of the grinding wheels 32, 42. The intra-spindle passage 144 is a passage provided in the spindle 33, the intra-mount passage 145 is a passage provided in the wheel mount 37, and the intra-base passage 146 is a passage provided in the annular base 35. The grinding water supply passage 142 supplies grinding water supplied from the grinding water supply source 141 through passages 144, 145, and 146 in sequence, and supplies the grinding water to the inner surface of the annular base 35 of the grinding wheels 32, 42, thereby supplying grinding water to the grinding wheels 31, 41 and the workpiece 200 that grind the workpiece 200.

[0028] The grinding water supply nozzle 143 is disposed below the lower surface of the grinding wheel 32, 42 of the grinding unit 3, 4, and is disposed inside the multiple grinding wheels 31, 41 of the grinding wheel 32, 42 of the grinding unit 3, 4 during grinding. The grinding water supply nozzle 143 is disposed below the lower surface of the grinding wheel 32, 42 of the grinding unit 3, 4, and extends from the center of the grinding wheel 32, 42 of the grinding unit 3, 4 during grinding toward the center of the holding surface 71 of the holding table 7 located at the processing position (i.e., the grinding wheels 31, 41 located at the processing position), and supplies grinding water supplied from the grinding water supply source 141 to the grinding wheels 31, 41 located at the processing position. The grinding wheels 31, 41 located at the processing position are the grinding wheels 31, 41 located at the center of the holding surface 71 of the holding table 7 among the multiple grinding wheels 31, 41 rotating around the axis.

[0029] In addition, in embodiment 1, the grinding water supply unit 14 is equipped with a flow rate adjustment valve 147 that controls the flow rate of grinding water (equivalent to the amount of grinding water) supplied to the grinding water supply passage 142, and a flow rate adjustment valve 148 that controls the flow rate of grinding water supplied to the grinding water supply nozzle 143.

[0030] The grinding feed unit 5 moves the grinding units 3, 4 in the Z-axis direction to move the grinding units 3, 4 away from and towards the holding table 7. In the first embodiment, the grinding feed unit 5 is provided on an erected column 21 erected from one end of the device body 2 in the Y-axis direction parallel to the horizontal direction. The grinding feed unit 5 includes a well-known ball screw provided rotatably about its axis, a well-known motor for rotating the ball screw about its axis, and a well-known guide rail for supporting the spindle housings 36 of the grinding units 3, 4 movably in the Z-axis direction.

[0031] In addition, in embodiment 1, the rough grinding unit 3 and the finish grinding unit 4 are arranged in parallel with a horizontal gap between the axis that is the center of rotation of the grinding wheels 32, 42 and the axis that is the center of rotation of the holding table 7, and the grinding wheels 31, 41 pass over the center of the back surface 205 of the workpiece 200 held on the holding table 7.

[0032] The cassettes 8 and 9 are containers having a plurality of slots for accommodating the workpiece 200. The cassettes 8 and 9 accommodate the workpiece 200 before and after grinding. The alignment unit 10 is a table on which the workpiece 200 removed from the cassettes 8 and 9 is temporarily placed and its center is aligned.

[0033] Two transport units 11 are provided. Each of the two transport units 11 has a suction pad that suctions the workpiece 200. One of the transport units 11 suctions and holds the workpiece 200 before grinding that has been aligned by the alignment unit 10, and carries it onto the holding table 7 located in the carry-in / out area 301. The other transport unit 11 suctions and holds the workpiece 200 after grinding that is held on the holding table 7 located in the carry-in / out area 301, and carries it out to the cleaning unit 12.

[0034] The cleaning unit 12 cleans the workpiece 200 after grinding, and removes contamination such as grinding debris adhering to the ground back surface 205. The carry-in / out unit 13 is, for example, a robot pick equipped with a U-shaped hand 131, and adsorbs and holds the workpiece 200 with the U-shaped hand 131 and transports it. Specifically, the carry-in / out unit 13 takes out the workpiece 200 before grinding from the cassettes 8, 9 and transports it to the alignment unit 10, and takes out the workpiece 200 after grinding from the cleaning unit 12 and transports it into the cassettes 8, 9.

[0035] The grinding apparatus 1 also includes a thickness measuring device (not shown) that measures the thickness of the workpiece 200 held on the holding table 7 in the rough grinding area 302 and the finish grinding area 303. The thickness measuring device outputs the measurement result to the control unit 100.

[0036] The control unit 100 controls each of the above-mentioned constituent units constituting the grinding apparatus 1. In other words, the control unit 100 causes the grinding apparatus 1 to execute a grinding operation on the workpiece 200. The control unit 100 is a computer having an arithmetic processing device having a microprocessor such as a CPU (central processing unit), a storage device having a memory such as a ROM (read only memory) or a RAM (random access memory), and an input / output interface device.

[0037] The arithmetic processing device of the control unit 100 performs arithmetic processing according to a computer program stored in the storage device, and outputs control signals for controlling the grinding device 1 to the above-mentioned components of the grinding device 1 via the input / output interface device. The control unit 100 is also connected to a display unit constituted by a liquid crystal display device or the like for displaying the status and images of the machining operation, and an input unit used by an operator to register machining content information, etc. The input unit is constituted by at least one of a touch panel provided on the display unit, a keyboard, etc.

[0038] The grinding device 1 having the above-mentioned configuration performs rough grinding and finish grinding in order on the workpiece 200 by controlling each component unit with the control unit 100, thereby performing a processing operation to thin the workpiece 200. In the first embodiment, the grinding device 1 starts the processing operation when the operator places cassettes 8, 9, each containing the workpiece 200 with the protective member 210 attached to the surface 202 thereof with the protective member 210 facing downward, the processing conditions are registered in the control unit 100, and the control unit 100 receives an instruction to start the processing operation from the operator.

[0039] In the processing operation, the grinding device 1 rotates the spindle 33 of each of the grinding units 3 and 4 about its axis at a rotation speed determined by the processing conditions, and causes the carry-in / out unit 13 to take out one workpiece 200 from the cassette 8 and carry it out to the alignment unit 10. The grinding device 1 causes the alignment unit 10 to align the center of the workpiece 200, and carries the front surface 202 side of the workpiece 200 aligned by the transport unit 11 onto the holding table 7 located in the carry-in / out area 301. At this time, the workpiece 200 carried into the holding table 7 is positioned coaxially with the holding table 7.

[0040] In the processing operation, the grinding device 1 sucks and holds the front surface 202 side of the workpiece 200 on the holding table 7 in the carry-in / out area 301 via the protective member 210, rotates the turntable 6, and moves the holding table 7 holding the workpiece 200 in the carry-in / out area 301 to the rough grinding area 302. In the processing operation, the grinding device 1 roughly grinds the workpiece 200 while rotating the holding table 7 about its axis by the rough grinding unit 3 while supplying grinding water, rotates the turntable 6, and moves the holding table 7 holding the workpiece 200 after the rough grinding to the finish grinding area 303. The grinding device 1 finishes grinding the workpiece 200 while rotating the holding table 7 about its axis by the finish grinding unit 4 while supplying grinding water, rotates the turntable 6, and moves the holding table 7 holding the workpiece 200 after the finish grinding and having stopped rotating about its axis to the carry-in / out area 301.

[0041] In the processing operation, the grinding device 1 transports the workpiece 200 after the finish grinding from the holding table 7 in the carry-in / out area 301 to the cleaning unit 12, cleans it in the cleaning unit 12, and stores it in the cassettes 8 and 9. In the processing operation, the grinding device 1 transports the workpiece 200 after the finish grinding to the holding table 7 in the carry-in / out area 301 that does not hold the workpiece 200 after the finish grinding every time the turntable 6 rotates, transports the workpiece 200 from the holding table 7 in the carry-in / out area 301 that holds the workpiece 200 after the finish grinding to the cleaning unit 12, and then transports the workpiece 200 before grinding. When the grinding device 1 performs the rough grinding and the finish grinding on all the workpieces 200 in the cassettes 8 and 9, the processing operation is completed. Next, a method for grinding the workpiece will be described.

[0042] (Method of grinding a workpiece) The grinding method of the workpiece according to the first embodiment is a grinding method for thinning the workpiece 200 to a predetermined finish thickness 206 (shown in FIG. 2) using the grinding device 1 described above, and in the first embodiment, the grinding method is carried out in the rough grinding unit 3. Therefore, in the first embodiment, the predetermined finish thickness 206 is the thickness of the workpiece 200 after rough grinding by the rough grinding unit 3, and does not necessarily match the thickness of the workpiece 200 after finish grinding.

[0043] 4, the method for grinding a workpiece according to the first embodiment includes a first grinding step 1001 and a second grinding step 1002. That is, in the first embodiment, the first grinding step 1001 and the second grinding step 1002 are performed in the rough grinding unit 3.

[0044] (First grinding step) The first grinding step 1001 is a step in which the rough grinding unit 3 is fed for grinding while supplying the grinding wheel 31 with a first grinding water amount 401 (shown in FIG. 5) that is a flow rate capable of suppressing wear of the grinding wheel 31. The predetermined thickness is a thickness that is thicker than the finishing thickness 206, and is appropriately determined depending on the type of the workpiece 200, the type of the grinding wheel 31 of the rough grinding unit 3, etc.

[0045] In the grinding apparatus 1, the grinding water supply unit 14 supplies the grinding water of the first grinding water amount 401 to the grinding stone 31 of the grinding wheel 32 of the rough grinding unit 3, while the grinding feed unit 5 moves the rough grinding unit 3 close to the workpiece 200 held on the holding table 7 in the rough grinding area 302, and the grinding stone 31 of the rough grinding unit 3 comes into contact with the workpiece 200 to start the rough grinding process and the first grinding step 1001, and the workpiece 200 is gradually thinned. Note that the first grinding water amount 401 in the first grinding step 1001 is the sum of the flow rate of the grinding water supplied to the grinding water supply passage 142, which is the amount of grinding water, and the flow rate of the grinding water supplied to the grinding water supply nozzle 143, which is the amount of grinding water. In addition, the first grinding water volume 401 is equivalent to the amount of water (flow rate) when a conventionally used rough grinding unit 3 roughly grinds the workpiece 200, i.e., when a conventionally used grinding device grinds the workpiece 200.

[0046] Thus, in the first grinding step 1001, the grinding water supply unit 14 supplies the first grinding water amount 401 equivalent to that of the conventional method to the grinding wheel 31 of the grinding wheel 32 of the rough grinding unit 3, thereby suppressing wear of the grinding wheel 31 of the rough grinding unit 3. The first grinding water amount 401 capable of suppressing wear of the grinding wheel 31 is the same amount of water (flow rate) as when the conventionally used rough grinding unit 3 roughly grinds the workpiece 200, i.e., when the conventionally used grinding device grinds the workpiece 200.

[0047] 5 indicates time, the vertical axis on the right side indicates the amount of grinding water supplied to the rough grinding unit 3, and the vertical axis on the left side indicates the spindle current value of the rough grinding unit 3. The dotted line in Fig. 5 indicates the change in the amount of grinding water supplied to the rough grinding unit 3, and the solid line in Fig. 5 indicates the change in the spindle current value of the rough grinding unit 3.

[0048] In the first embodiment, in the first grinding step 1001, the grinding feed speed of the rough grinding unit 3, which the grinding feed unit 5 brings closer to the holding table 7, is reduced stepwise in accordance with the thickness of the workpiece 200. In the first grinding step 1001 in the first embodiment, the grinding feed speed of the rough grinding unit 3 by the grinding feed unit 5 is reduced in three steps, but in the present invention, the steps for reducing the grinding feed speed are not limited to three steps.

[0049] 5, in the first grinding step 1001, the grinding device 1 suppresses wear of the bond of the grinding wheel 31 of the rough grinding unit 3, so that self-sharpening is not promoted, and glazing gradually occurs due to the influence of grinding chips, and the spindle current value of the rough grinding unit 3 gradually increases. In the first grinding step 1001, as shown in FIG. 5, the grinding device 1 maintains the amount of grinding water at the first grinding water amount 401, and thins the workpiece 200 to a predetermined thickness.

[0050] (Second grinding step) The second grinding step 1002 is a step in which, after the first grinding step 1001, a second grinding water volume 402 is supplied which is less than the first grinding water volume 401, increases wear on the grinding wheel 31, and promotes self-sharpening, while the rough grinding unit 3 is fed to grind the workpiece 200 to the finishing thickness 206, thereby promoting sharpening of the grinding wheel 31, and preparing for rough grinding of the next workpiece 200.

[0051] In the second grinding step 1002, the grinding device 1 reduces the grinding feed rate of the rough grinding unit 3 by the grinding feed unit 5 to a value lower than the grinding feed rate in the first grinding step 1001, and controls the flow rate regulating valves 147 and 148 to reduce the amount of grinding water supplied by the grinding water supply unit 14 to the grinding stone 31 of the grinding wheel 32 of the rough grinding unit 3 to a second grinding water amount 402 lower than the first grinding water amount 401, as shown in FIG. 5. This promotes self-sharpening, in which the bond of the grinding stone 31 of the rough grinding unit 3 is worn and the abrasive grains are separated from the bond. In the second grinding step 1002, the grinding stone 31 of the rough grinding unit 3, which was becoming dull due to grinding chips in the first grinding step 1001, is sharpened so that it can be roughly ground with new abrasive grains by promoting self-sharpening.

[0052] For this reason, in the second grinding step 1002, the grinding device 1 promotes self-sharpening of the grinding wheel 31 of the rough grinding unit 3 and sharpens the grinding wheel, so that the grinding load is lower than in the first grinding step 1001 and the spindle current value is lowered as shown in Fig. 5. In the second grinding step 1002, when the grinding device 1 thins the workpiece 200 to the finishing thickness 206, it stops the grinding feed of the rough grinding unit 3 by the grinding feed unit 5, and then moves the rough grinding unit 3 away from the holding table 7 by the grinding feed unit 5, thereby completing the second grinding step 1002 and completing the rough grinding of the workpiece 200.

[0053] Then, the grinding device 1 sequentially performs a first grinding step 1001 and a second grinding step 1002 in the rough grinding unit 3 on the next workpiece 200 (hereinafter referred to as the n+1th workpiece, where n is a natural number) held on the holding table 7 that is next positioned in the rough grinding region 302 by the rotation of the turntable 6. At this time, since the grinding wheel 31 of the rough grinding unit 3 has been sharpened when the previous workpiece 200 (hereinafter referred to as the nth workpiece) was subjected to the second grinding step 1002, when the first grinding step 1001 is performed on the n+1th workpiece 200, the grinding wheel 31 bites into the workpiece 200 immediately after the start of the first grinding step 1001, and the grinding load does not rise abruptly, and as shown in FIG. 5, the spindle current value does not rise abruptly temporarily, but gradually rises in the same manner as when the nth workpiece 200 is ground. FIG. 5 shows the case where n=1.

[0054] As described above, the grinding method of the workpiece according to the first embodiment sets the amount of grinding water in the second grinding step 1002 in the latter half of grinding the workpiece 200 to the second grinding water amount 402, which is reduced from the first grinding water amount 401 in the first grinding step 1001, to promote the self-sharpening of the grinding wheel 31. For this reason, the grinding method of the workpiece according to the first embodiment can start rough grinding of the next workpiece 200 in a state where the workpiece is sufficiently sharpened, and the grinding wheel 31 is likely to bite into the workpiece 200 at the start of rough grinding of the n+1th workpiece 200, and the grinding load at the start of rough grinding of the n+1th workpiece 200, which is likely to be applied, can be suppressed, thereby preventing an increase in the spindle current value at the start of rough grinding of the n+1th workpiece 200.

[0055] Furthermore, in the grinding method for a workpiece according to the first embodiment, the amount of grinding water in the first grinding step 1001 in the first half of grinding the workpiece 200 is set to a first grinding water amount 401 that is equivalent to that in the conventional method and is higher than the second grinding water amount 402, thereby suppressing wear of the grinding wheel 31 in the first grinding step 1001, and reducing the amount of grinding water to the second grinding water amount 402 in the second half when glazing progresses, thereby increasing wear and promoting spontaneous sharpening. For this reason, the grinding method for a workpiece according to the first embodiment can reduce the grinding load while preventing excessive wear of the grinding wheel 31.

[0056] In addition, the grinding method of the workpiece according to the first embodiment uses a grinding device 1 that performs rough grinding and finish grinding, and thus promotes self-sharpening by reducing the amount of grinding water in the second grinding step 1002 of the rough grinding unit 3. The grinding method of the workpiece according to the first embodiment performs grinding using the grinding wheel 31 in which self-sharpening is promoted in the second grinding step 1002, and can intentionally roughen the back surface 205, which is the grinding surface of the workpiece 200 after rough grinding by the rough grinding unit 3, more than in the case where the amount of grinding water is kept constant from the start to the end of grinding or in the conventional method in which the amount of grinding water is increased in the latter half of grinding compared to the first half of grinding (this is equivalent to scratching the surface to make it rougher). For this reason, the grinding method of the workpiece according to embodiment 1 uses a grinding device 1 which performs rough grinding and finish grinding. Therefore, when grinding with a grinding wheel 42 for finish grinding, which has a finer abrasive grain size, the grinding stone 41 of the grinding wheel 42 for finish grinding easily bites into the grinding wheel 42 due to the unevenness of the back surface 205 of the workpiece 200, and wear is also accelerated, so that grinding with reduced grinding load can be achieved even with the grinding wheel 42 for finish grinding, which has a harder time biting into the grinding wheel 42 for finish grinding.

[0057] As a result, the method for grinding a workpiece according to the first embodiment has the effect of preventing excessive wear of the grinding wheel 31 while also realizing a reduction in the grinding load.

[0058] Furthermore, since the grinding method of the workpiece according to embodiment 1 uses a grinding device 1 that performs rough grinding and finish grinding, even if the back surface 205 of the workpiece 200 is roughened by the rough grinding unit 3, the surface roughness of the back surface 205 of the workpiece 200 can be reduced by the finish grinding, so that the processing quality of the workpiece 200 can be maintained high while reducing the grinding load.

[0059] Next, the applicants of the present invention confirmed the effects of the method for grinding a workpiece according to the first embodiment. In the confirmation, the spindle current value was measured when the nth workpiece 200 and the (n+1)th workpiece 200 were roughly ground by the rough grinding unit 3 in Comparative Example 1 shown in Fig. 6 and Comparative Example 2 shown in Fig. 7. In the confirmation, n=1. Fig. 6 is a diagram showing the changes in the amount of grinding water and the spindle current value in Comparative Example 1. Fig. 7 is a diagram showing the changes in the amount of grinding water and the spindle current value in Comparative Example 2.

[0060] 6 and 7, similar to Fig. 5, the horizontal axis indicates time, the vertical axis on the right indicates the amount of grinding water supplied to the rough grinding unit 3, and the vertical axis on the left indicates the spindle current value of the rough grinding unit 3. In Fig. 6 and 7, the dotted lines indicate changes in the amount of grinding water supplied to the rough grinding unit 3, and the solid lines indicate changes in the spindle current value of the rough grinding unit 3.

[0061] In Comparative Example 1, the amount of grinding water during rough grinding by the rough grinding unit 3 is maintained at the first grinding water amount 401, and other conditions are the same as those of the first embodiment (i.e., the amount of grinding water is not increased or decreased from the first grinding water amount 401 from immediately after the start of rough grinding to the end of the rough grinding). In Comparative Example 2, the amount of grinding water immediately after the start of rough grinding of the n+1th workpiece 200 is set to the second grinding water amount 402, and thereafter is maintained at the first grinding water amount 401, and other conditions are the same as those of the first embodiment (corresponding to the method shown in the above-mentioned Patent Document 3) (i.e., the amount of grinding water immediately after the start of rough grinding is less than that in the latter half of the rough grinding, and the amount of grinding water in the latter half of the rough grinding is greater than that in the first half of the rough grinding).

[0062] According to FIG. 6, in Comparative Example 1, the grinding water amount 401 was maintained to suppress wear of the grinding wheel 31, so that the grinding wheel 31 was clogged, and the spindle current value temporarily increased at the start of rough grinding of the n+1th workpiece 200. According to FIG. 7, in Comparative Example 2, in the latter half of the rough grinding, the grinding water amount was changed to the second grinding water amount 402, which was reduced from the first grinding water amount 401 used in the first half of the grinding, to suppress wear of the grinding wheel 31. In this way, the grinding load was further increased, and the spindle current value temporarily increased at the start of rough grinding of the n+1th workpiece 200. Therefore, according to FIG. 6 and FIG. 7, it was clear that in Comparative Example 1 and Comparative Example 2, the grinding load temporarily increased at the start of rough grinding of the n+1th workpiece 200. A temporary and sudden increase in the grinding load is undesirable because it can easily cause scratches or damage to the grinding wheel 31 and the workpiece 200.

[0063] In contrast to Comparative Example 1 and Comparative Example 2, in the first embodiment, as shown in Fig. 5, it was clear that the spindle current value did not rise temporarily and the grinding load did not rise temporarily at the start of rough grinding of the n+1th workpiece 200. Therefore, it was clear that the grinding load at the start of rough grinding of the n+1th workpiece 200 can be suppressed by setting the amount of grinding water in the second grinding step 1002 in the latter half of grinding the workpiece 200 to the second grinding water amount 402 that is reduced from the first grinding water amount 401 in the first grinding step 1001, thereby promoting the self-sharpening of the grinding wheel 31.

[0064] The present invention is not limited to the above embodiment. That is, various modifications can be made without departing from the gist of the present invention. In the first embodiment, the grinding water supply unit 14 includes a flow rate adjustment valve 147 for controlling the flow rate of grinding water (corresponding to the amount of grinding water) supplied to the grinding water supply passage 142, and a flow rate adjustment valve 148 for controlling the flow rate of grinding water supplied to the grinding water supply nozzle 143. However, the grinding water supply unit 14 may include at least one of the grinding water supply passage 142 and the flow rate adjustment valve 147, or the grinding water supply nozzle 143 and the flow rate adjustment valve 148. When changing the amount of grinding water from the first grinding water amount 401 to the second grinding water amount 402, both the flow rate adjustment valve 147 and the flow rate adjustment valve 148 are adjusted in the first embodiment, but only one of them may be adjusted. [Explanation of symbols]

[0065] 1 Grinding equipment 3 Rough grinding unit 4 Finish grinding unit 5 Grinding feed unit 7 Holding Table 14 Grinding water supply unit 31,41 Grinding wheel 32,42 Grinding wheels 33 Spindle 34 Motor 100 Control Unit 200 Workpiece 205 Back side (top side of workpiece) 206 Finishing thickness 401 First grinding water volume 402 Second grinding water volume 1001 First grinding step 1002 Second grinding step

Claims

1. A holding table for holding the workpiece; a grinding unit having a spindle on which a grinding wheel having grinding stones arranged in an annular shape for grinding the workpiece held on the holding table is mounted, and a motor for rotating the spindle; a grinding feed unit for moving the grinding unit toward and away from the holding table; a grinding water supply unit that supplies grinding water to an upper surface of the workpiece held on the holding table in a manner that allows the flow rate of the grinding water to be adjusted; A grinding method for thinning a workpiece to a finish thickness using a grinding apparatus including a control unit for controlling each unit, the method comprising: a first grinding step of grinding the workpiece to a predetermined thickness by feeding the grinding unit while supplying a first amount of grinding water capable of suppressing wear of the grinding wheel; a second grinding step in which, after the first grinding step is performed, a second grinding water amount is supplied which is less than the first grinding water amount, which increases wear of the grinding wheel and promotes self-sharpening, while a grinding feed speed at which the grinding unit approaches the holding table is slower than the grinding feed speed of the first grinding step, the grinding unit is fed, and the workpiece is ground to a finishing thickness, promoting the sharpening of the grinding wheel, and preparing for processing the next workpiece; A method for grinding a workpiece, comprising:

2. The grinding unit comprises: a coarse grinding unit using a coarse grinding wheel; a finish grinding unit that uses a grinding wheel having a fine grain size to grind the workpiece ground by the rough grinding unit; 2. The method for grinding a workpiece according to claim 1, wherein the first grinding step and the second grinding step are performed in the rough grinding unit.

3. A method for grinding a workpiece as described in claim 1 or claim 2, characterized in that in the first grinding step, the grinding feed speed of the grinding unit is gradually reduced.

Citation Information

Patent Citations

  • Method of grinding thin sheet-shaped workpiece, and double-head surface grinding machine

    JP2012210697A

  • Method for grinding semiconductor wafer

    JP2012222123A

  • Grinding method and grinding device

    JP2014124690A

  • Surface grinding method of work-piece

    JP2015160249A

  • Grinding method

    JP2015196226A