Stator core and rotating electric machine

By aligning the radial direction of the teeth and the extending direction of the core back with the optimal magnetic properties of the electromagnetic steel sheets, the stator core achieves enhanced magnetic flux density and reduced iron loss, improving the performance of rotating electric machines.

JP7588599B2Active Publication Date: 2024-11-22NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021556181
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-15
Filing Date
2020-11-13
Publication Date
2024-11-22
Estimated Expiration
2040-11-13

AI Technical Summary

Technical Problem

Existing stator cores with split cores do not fully optimize magnetic properties, as previous technologies do not consider the composition and orientation of electromagnetic steel sheets effectively.

Method used

The stator core is configured with split cores made of electromagnetic steel sheets having specific chemical compositions and orientations, where the radial direction of the teeth and the extending direction of the core back align with the directions of excellent magnetic properties of the steel sheets, adhering to certain magnetic flux density and anisotropy ratios.

Benefits of technology

This configuration enhances the magnetic properties of the stator core, leading to improved magnetic flux density and reduced iron loss, allowing for increased torque and reduced copper loss in rotating electric machines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588599000007
    Figure 0007588599000007
  • Figure 0007588599000008
    Figure 0007588599000008
  • Figure 0007588599000009
    Figure 0007588599000009
Patent Text Reader

Abstract

The present invention is a stator core (21) provided with a plurality of divided cores (30). The plurality of divided cores (30) are configured by layering core pieces (40) comprising electrical steel sheets. The electrical steel sheets are predetermined electrical steel sheets. Both the radial direction of the teeth (41) and the direction of extension of the core backs (42) of the core pieces (40) of at least one divided core (30) among the plurality of divided cores (30) are arranged along a direction in which the electrical steel sheets have excellent magnetic characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stator core and a rotating electric machine, and in particular to a stator core including a plurality of split cores. This application claims priority based on Japanese Patent Application No. 2019-206648, filed on November 15, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] 2. Description of the Related Art A stator core (iron core) for a rotating electric machine is known in which a plurality of divided cores are arranged in a circumferential direction.

[0003] Patent Document 1 discloses that the motor's core is divided into laminated core pieces by a dividing surface, and the laminated core pieces are made of unidirectional or bidirectional magnetic steel sheets. The laminated core pieces are wound with windings via insulating parts, and the laminated core pieces are laminated with a determined direction of easy magnetization. With such a motor, the magnetic flux passing through the laminated core pieces always flows in the direction of easy magnetization of the directional magnetic steel sheets, and the change in the direction of the magnetic flux flowing in the pole teeth and gaps during rotation is reduced, thereby reducing iron loss, excitation current, cogging torque, induced voltage distortion, and torque ripple.

[0004] Patent Document 2 discloses a motor having a stator core in which a plurality of laminated cores having teeth extending in the radial direction are arranged in the circumferential direction. The laminated core has a plurality of plate-shaped core pieces laminated in the plate thickness direction. The core pieces are made of non-oriented electromagnetic steel sheets, and the rolling direction of the core pieces is inclined with respect to the radial direction. It is also disclosed that the laminated core is formed by laminating core pieces with the same inclination, and at least a pair of laminated cores adjacent in the circumferential direction have inclinations opposite to each other. Such a motor can reduce cogging torque and torque ripple. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 8-47185 [Patent Document 2] International Publication No. 2017 / 090571 Summary of the Invention [Problem to be solved by the invention]

[0006] However, neither Patent Document 1 nor Patent Document 2 considers electromagnetic steel sheets. For this reason, there is room for improvement in terms of improving the magnetic properties of the conventional stator core including a plurality of split cores.

[0007] An object of the present invention is to improve the magnetic characteristics of a stator core provided with a plurality of split cores. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention employs the following configuration. (1) A stator core according to one aspect of the present invention is a stator core including a plurality of split cores, the plurality of split cores being configured by laminating core pieces made of electromagnetic steel sheets, the electromagnetic steel sheets containing, by mass%, C: 0.0100% or less, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0%, S: 0.0100% or less, N: 0.0100% or less, Mn, One or more selected from the group consisting of Ni, Co, Pt, Pb, Cu, and Au: 2.50% to 5.00% in total, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0 The alloy contains 100% Mn, and when the Mn content (mass%) is [Mn], the Ni content (mass%) is [Ni], the Co content (mass%) is [Co], the Pt content (mass%) is [Pt], the Pb content (mass%) is [Pb], the Cu content (mass%) is [Cu], the Au content (mass%) is [Au], the Si content (mass%) is [Si], and the sol.Al content (mass%) is [sol.Al], the alloy satisfies the following formula (1) with the balance consisting of Fe and impurities, and when the B50 value in the rolling direction is B50L, the B50 value in the direction tilted at 45° from the rolling direction is B50D1, the B50 value in the direction tilted at 90° from the rolling direction is B50C, and the B50 value in the direction tilted at 135° from the rolling direction is B50D2, the alloy satisfies the following formula (2) and (4) Satisfy the formula, {100} <011> The X-ray random intensity ratio is 5 or more and less than 30, the plate thickness is 0.50 mm or less, and the core piece of at least one of the plurality of split cores has both the radial direction of the teeth and the extension direction of the core back aligned along the direction in which the magnetic properties of the electromagnetic steel sheet are excellent. ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0% ···(1) (B50D1+B50D2) / 2>1.7T ···(2) (B50D1+B50D2) / 2>1.1×(B50L+B50C) / 2...(4) Here, the magnetic flux density B50 is the magnetic flux density when excited with a magnetic field strength of 5000 A / m. (2) A stator core according to an aspect of the present invention is a stator core including a plurality of split cores, the plurality of split cores being configured by laminating core pieces made of electromagnetic steel sheets, the electromagnetic steel sheets containing, by mass%, C: 0.0100% or less, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0%, S: 0.0100% or less, N: 0.0100% or less, Mn, Ni, C One or more selected from the group consisting of O, Pt, Pb, Cu, and Au: 2.50% to 5.00% in total, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total and has a chemical composition that satisfies the following formula (1) when the Mn content (mass%) is [Mn], the Ni content (mass%) is [Ni], the Co content (mass%) is [Co], the Pt content (mass%) is [Pt], the Pb content (mass%) is [Pb], the Cu content (mass%) is [Cu], the Au content (mass%) is [Au], the Si content (mass%) is [Si], and the sol.Al content (mass%) is [sol.Al], with the balance consisting of Fe and impurities. When the B50 value in the rolling direction is B50L, the B50 value in the direction tilted at 45° from the rolling direction is B50D1, the B50 value in the direction tilted at 90° from the rolling direction is B50C, and the B50 value in the direction tilted at 135° from the rolling direction is B50D2, the following formulas (3) and (6) are satisfied, and <011> The X-ray random intensity ratio is 5 or more and less than 30, the plate thickness is 0.50 mm or less, and the core piece of at least one of the plurality of split cores has both the radial direction of the teeth and the extension direction of the core back aligned along the direction in which the magnetic properties of the electromagnetic steel sheet are excellent. ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0% ···(1) (B50D1+B50D2) / 2>(B50L+B50C) / 2...(3) (B50D1+B50D2) / 2>1.8T ···(6) (3)(1) above Or (2) The stator core described in may satisfy the following formula (5). (B50D1+B50D2) / 2>1.2×(B50L+B50C) / 2...(5) (4)(1) above Any one of items (3) to (3) The stator core described in It may contain one or more elements selected from the group consisting of 0.020% to 0.400% Sn and 0.020% to 0.400% Sb. (5) In the stator core described in (1) above, the direction in which the magnetic properties of the electromagnetic steel sheet are excellent may be a direction at an angle of 45° or 135° from the rolling direction of the electromagnetic steel sheet, the radial direction of the teeth may be along one of the directions at an angle of 45° or 135° from the rolling direction, and the extension direction of the core back may be along the other direction at an angle of 45° or 135° from the rolling direction. (6) In the stator core described in any one of (1) to (5) above, in all of the core pieces of the multiple split cores, both the radial direction of the teeth and the extension direction of the core back may be aligned along the direction in which the magnetic properties of the electromagnetic steel sheet are excellent. (7) In the stator core described in any one of (1) to (5) above, the multiple split cores each have a teeth portion, and among the multiple teeth portions, the width of the teeth portion along the direction in which the magnetic properties are superior may be narrower than the width of the teeth portion not along the direction in which the magnetic properties are superior. (8) In the stator core described in (7) above, the product of the width of the teeth portion and the magnetic flux density of the teeth portion when excited with a predetermined magnetic field strength may be approximately constant for each of the teeth portions of the multiple split cores. (9) A rotating electric machine according to one aspect of the present invention includes the stator core according to any one of (1) to (8) above. Effect of the Invention

[0009] According to the above-described aspects of the present invention, it is possible to improve the magnetic characteristics of a stator core including a plurality of split cores. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a diagram illustrating an example of a configuration of a rotating electric machine. [Diagram 2] FIG. 2 is a diagram illustrating an example of a configuration of a split core. [Diagram 3] FIG. 4 is a diagram showing an example of a configuration of a core piece. [Figure 4] 1 is a graph showing an example of the relationship between the B50 ratio and the angle from the rolling direction. [Diagram 5] 1 is a graph showing an example of the relationship between the W15 / 50 ratio and the angle from the rolling direction. [Figure 6] 1 is a graph showing an example of the relationship between the W15 / 100 ratio and the angle from the rolling direction. [Figure 7] FIG. 2 is a diagram showing an example of the relationship between the rolling direction and the direction in which the magnetic properties are the best. [Figure 8] FIG. 2 is a diagram for explaining a mold according to one embodiment of the present invention. [Figure 9] FIG. 4 is a diagram for explaining the width of a tooth portion. [Figure 10] 13A and 13B are diagrams for explaining a mold according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Examples of magnetic steel sheets used in split cores> First, the electromagnetic steel sheets used in the split cores of the embodiments described below will be described. Here, the chemical composition of the non-oriented electromagnetic steel sheet of this embodiment, which is an example of the electromagnetic steel sheet used for the split core of the embodiment, and the steel material used in its manufacturing method will be described. In the following description, "%" which is the unit of the content of each element contained in the non-oriented electromagnetic steel sheet or steel material of this embodiment means "mass%" unless otherwise specified. Also, in the numerical limit range described with "~" in between, the lower limit value and the upper limit value are included in that range. The numerical values indicated by "less than" or "exceeding" are not included in the numerical range. The non-oriented electromagnetic steel sheet and the steel material have a chemical composition in which ferrite-austenite transformation (hereinafter, α-γ transformation) can occur, and C: 0.0100% or less, Si: 1.50% to 4.00%, sol.Al: 0.0001% to 1.0%, S: 0.0100% or less, N: 0.0100% or less, one or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, Au: a total of 2.50% to 5.00%, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and one or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: a total of 0.0000% to 0.0100%, and the balance consists of Fe and impurities. Further, the contents of Mn, Ni, Co, Pt, Pb, Cu, Au, Si, and sol.Al satisfy predetermined conditions described later. Examples of the impurities include those contained in raw materials such as ores and scraps, and those contained in the manufacturing process.

[0012] <<C: 0.0100% or less>> C increases iron loss and causes magnetic aging. Therefore, the lower the C content, the better. Such a phenomenon is remarkable when the C content exceeds 0.0100%. For this reason, the C content is set to 0.0100% or less. The reduction of the C content also contributes to the uniform improvement of the magnetic properties in all directions within the plate surface. Although the lower limit of the C content is not particularly limited, it is preferably 0.0005% or more in view of the cost of decarburization treatment during refining.

[0013] <<Si: 1.50% to 4.00%>> Si increases the electrical resistance, reduces the eddy current loss, reduces the iron loss, or increases the yield ratio to improve the punching processability of the iron core. If the Si content is less than 1.50%, these effects cannot be fully obtained. Therefore, the Si content should be 1.50% or more. On the other hand, if the Si content exceeds 4.00%, the magnetic flux density decreases, the punching processability deteriorates due to an excessive increase in hardness, and cold rolling becomes difficult. Therefore, the Si content should be 4.00% or less.

[0014] <<sol.Al: 0.0001% - 1.0%>> sol.Al increases the electrical resistance, reduces the eddy current loss, and reduces the iron loss. sol.Al also contributes to an improvement in the relative magnitude of the magnetic flux density B50 with respect to the saturation magnetic flux density. Here, the magnetic flux density B50 is the magnetic flux density when excited with a magnetic field strength of 5000 A / m. If the sol.Al content is less than 0.0001%, these effects cannot be fully obtained. Also, Al has an effect of promoting desulfurization in steelmaking. Therefore, the sol.Al content should be 0.0001% or more. On the other hand, if the sol.Al content exceeds 1.0%, the magnetic flux density decreases, the yield ratio decreases, and the punching processability deteriorates. Therefore, the sol.Al content should be 1.0% or less.

[0015] <<S: 0.0100% or less>> S is not an essential element and is contained as an impurity in steel, for example. S inhibits the recrystallization and grain growth during annealing due to the precipitation of fine MnS. Therefore, the lower the S content, the better. The increase in iron loss and the decrease in magnetic flux density due to such inhibition of recrystallization and grain growth are significant when the S content exceeds 0.0100%. For this reason, the S content should be 0.0100% or less. Note that the lower limit of the S content is not particularly limited, but considering the cost of desulfurization treatment during refining, it is preferably 0.0003% or more.

[0016] <<N: 0.0100% or less>> Similar to C, N deteriorates magnetic properties. Therefore, the lower the N content, the better. Thus, the N content should be 0.0100% or less. Although the lower limit of the N content is not particularly limited, considering the cost of denitrification treatment during refining, it is preferably 0.0010% or more.

[0017] <<One or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, Au: total 2.50% - 5.00%>> Since these elements are necessary for causing α-γ transformation, it is necessary to contain these elements in a total amount of 2.50% or more. On the other hand, if it exceeds 5.00% in total, the cost will be high and the magnetic flux density may decrease. Therefore, the total amount of these elements should be 5.00% or less.

[0018] Also, as conditions under which α-γ transformation can occur, the following conditions should be further satisfied. That is, when the Mn content (mass%) is [Mn], the Ni content (mass%) is [Ni], the Co content (mass%) is [Co], the Pt content (mass%) is [Pt], the Pb content (mass%) is [Pb], the Cu content (mass%) is [Cu], the Au content (mass%) is [Au], the Si content (mass%) is [Si], and the sol.Al content (mass%) is [sol.Al], it is preferably satisfied with the following formula (1) in mass%. ([Mn] + [Ni] + [Co] + [Pt] + [Pb] + [Cu] + [Au]) - ([Si] + [sol.Al]) > 0% ···(1)

[0019] When the above formula (1) is not satisfied, α-γ transformation does not occur, so the magnetic flux density becomes low.

[0020] <<Sn: 0.000% - 0.400%, Sb: 0.000% - 0.400%, P: 0.000% - 0.400%>> Sn and Sb improve the crystal structure after cold rolling and recrystallization, and enhance the magnetic flux density. Therefore, these elements may be contained as needed, but excessive inclusion will embrittle the steel. Thus, both the Sn content and the Sb content should be 0.400% or less. Also, P may be contained to ensure the hardness of the steel sheet after recrystallization, but excessive inclusion will cause embrittlement of the steel. Therefore, the P content should be 0.400% or less. When further effects such as magnetic properties are to be imparted as described above, it is preferable to contain one or more selected from the group consisting of 0.020% to 0.400% Sn, 0.020% to 0.400% Sb, and 0.020% to 0.400% P.

[0021] <<One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: total 0.0000% to 0.0100%>> Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd react with S in the molten steel during casting of the molten steel to form precipitates of sulfide or oxysulfide or both. Hereinafter, Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd may be collectively referred to as "coarse precipitate-forming elements". The particle size of the precipitates of the coarse precipitate-forming elements is about 1 μm to 2 μm, which is much larger than the particle size (about 100 nm) of fine precipitates such as MnS, TiN, and AlN. For this reason, these fine precipitates adhere to the precipitates of the coarse precipitate-forming elements, and it becomes difficult to inhibit recrystallization and grain growth during intermediate annealing. In order to sufficiently obtain these effects, it is preferable that the total of these elements is 0.0005% or more. However, if the total of these elements exceeds 0.0100%, the total amount of sulfide or oxysulfide or both will be excessive, and recrystallization and grain growth during intermediate annealing will be inhibited. Therefore, the total content of the coarse precipitate-forming elements should be 0.0100% or less.

[0022] <<Crystal structure>> Next, the texture of the non-oriented electrical steel sheet of this embodiment will be described. The details of the manufacturing method will be described later, but the non-oriented electrical steel sheet of this embodiment has a chemical composition in which α-γ transformation can occur, and the structure is refined by rapid cooling immediately after the end of finish rolling in hot rolling, resulting in a structure in which {100} crystal grains have grown. As a result, the non-oriented electrical steel sheet of this embodiment has a {100} <011> The orientation concentration strength is 5 to 30, and the magnetic flux density B50 in the 45° direction to the rolling direction is particularly high. Thus, the magnetic flux density is high in a specific direction, but overall, a high magnetic flux density is obtained on average in all directions. <011> When the orientation concentration is less than 5, the magnetic flux density is reduced. <112> The intensity of the magnetic flux increases, and the magnetic flux density decreases overall. <011> Manufacturing methods that achieve an orientation integration strength of over 30 require thick hot-rolled sheets, which poses the problem of being difficult to manufacture.

[0023] {100} <011> The orientation integration strength can be measured by X-ray diffraction or electron backscatter diffraction (EBSD). Since the reflection angle of X-rays and electron beams from a sample differs for each crystal orientation, the crystal orientation strength can be determined from the reflection intensity of a randomly oriented sample. <011> The orientation accumulation strength is an X-ray random intensity ratio of 5 to 30. In this case, the crystal orientation may be measured by EBSD and a value converted into an X-ray random intensity ratio may be used.

[0024] <<Thickness>> Next, the thickness of the non-oriented electrical steel sheet of this embodiment will be described. The thickness of the non-oriented electrical steel sheet of this embodiment is 0.50 mm or less. If the thickness exceeds 0.50 mm, excellent high-frequency iron loss cannot be obtained. Therefore, the thickness is set to 0.50 mm or less.

[0025] <<Magnetic properties>> Next, the magnetic properties of the non-oriented electrical steel sheet of this embodiment will be described. When examining the magnetic properties, the value of B50, which is the magnetic flux density of the non-oriented electrical steel sheet of this embodiment, is measured. In the manufactured non-oriented electrical steel sheet, one side of the rolling direction cannot be distinguished from the other side. Therefore, in this embodiment, the rolling direction refers to both sides. If the value of B50 in the rolling direction is B50L, the value of B50 in a direction tilted 45° from the rolling direction is B50D1, the value of B50 in a direction tilted 90° from the rolling direction is B50C, and the value of B50 in a direction tilted 135° from the rolling direction is B50D2, then anisotropy of the magnetic flux density is observed, with B50D1 and B50D2 being the highest and B50L and B50C being the lowest.

[0026] Here, for example, when considering the distribution of magnetic flux density in all directions (0° to 360°) with the clockwise direction (or counterclockwise direction) as the positive direction, and the rolling direction is 0° (one direction) and 180° (the other direction), B50D1 has B50 values ​​at 45° and 225°, and B50D2 has B50 values ​​at 135° and 315°. Similarly, B50L has B50 values ​​at 0° and 180°, and B50C has B50 values ​​at 90° and 270°. The B50 value at 45° and the B50 value at 225° strictly match, and the B50 value at 135° and the B50 value at 315° strictly match. However, B50D1 and B50D2 may not strictly match because it may not be easy to make the magnetic properties the same during actual manufacturing. Similarly, the B50 value at 0° strictly matches the B50 value at 180°, and the B50 value at 90° strictly matches the B50 value at 270°, while B50L and B50C may not strictly match. In the non-oriented electrical steel sheet of this embodiment, the average values ​​of B50D1 and B50D2 and the average values ​​of B50L and B50C are used to satisfy the following formulas (2) and (3). (B50D1+B50D2) / 2>1.7T ···(2) (B50D1+B50D2) / 2>(B50L+B50C) / 2...(3)

[0027] In this way, when the magnetic flux density is measured, the average value of B50D1 and B50D2 is 1.7 T or more as shown in formula (2), and high anisotropy of the magnetic flux density is confirmed as shown in formula (3).

[0028] Furthermore, in addition to satisfying formula (1), it is preferable that the anisotropy of the magnetic flux density is higher than that of formula (3), as shown in the following formula (4). (B50D1+B50D2) / 2>1.1×(B50L+B50C) / 2...(4) Furthermore, it is preferable that the anisotropy of the magnetic flux density is higher, as shown in the following formula (5). (B50D1+B50D2) / 2>1.2×(B50L+B50C) / 2...(5) Furthermore, as shown in the following formula (6), it is preferable that the average value of B50D1 and B50D2 is 1.8T or more. (B50D1+B50D2) / 2>1.8T ···(6)

[0029] The above 45° is a theoretical value, and since it may not be easy to match it to 45° in actual manufacturing, it also includes angles that do not strictly match 45°. This also applies to the 0°, 90°, 135°, 180°, 225°, 270°, and 315°.

[0030] The magnetic flux density can be measured by cutting a 55 mm square sample from a direction at 45°, 0°, etc. with respect to the rolling direction and using a single sheet magnetic measurement device.

[0031] <<Manufacturing method>> Next, an example of a method for manufacturing the non-oriented electrical steel sheet of this embodiment will be described. When manufacturing the non-oriented electrical steel sheet of this embodiment, for example, hot rolling, cold rolling (first cold rolling), intermediate annealing (first annealing), skin pass rolling (second cold rolling), finish annealing (third annealing), stress relief annealing (second annealing), etc. are performed.

[0032] First, the above-mentioned steel material is heated and hot-rolled. The steel material is, for example, a slab produced by normal continuous casting. The rough rolling and finish rolling of the hot rolling are performed at a temperature in the γ region (Ar1 temperature or higher). In other words, the hot rolling is performed so that the finishing temperature of the finish rolling is Ar1 temperature or higher and the coiling temperature is more than 250°C and less than 600°C. As a result, the structure is refined by the transformation from austenite to ferrite by subsequent cooling. If cold rolling is then performed in the refined state, bulging recrystallization (hereinafter, bulging) is likely to occur, and it is possible to facilitate the growth of {100} crystal grains, which are usually difficult to grow.

[0033] Furthermore, when manufacturing the non-oriented electrical steel sheet of this embodiment, the temperature (finishing temperature) during the final pass of finish rolling is set to be equal to or higher than the Ar1 temperature, and the coiling temperature is set to be greater than 250°C and equal to or lower than 600°C. The crystal structure is refined by transforming from austenite to ferrite. By refining the crystal structure in this way, it is possible to make bulging more likely to occur through the subsequent cold rolling and intermediate annealing.

[0034] Thereafter, the hot-rolled steel sheet is coiled without annealing, pickled, and then cold-rolled. The reduction ratio in cold rolling is preferably 80% to 95%. If the reduction ratio is less than 80%, bulging is less likely to occur. If the reduction ratio exceeds 95%, {100} crystal grains tend to grow due to subsequent bulging, but the hot-rolled steel sheet must be thickened, which makes coiling of the hot roll difficult and operation difficult. The reduction ratio in cold rolling is more preferably 86% or more. If the reduction ratio in cold rolling is 86% or more, bulging is more likely to occur.

[0035] After the cold rolling is completed, intermediate annealing is performed. When manufacturing the non-oriented electrical steel sheet of this embodiment, intermediate annealing is performed at a temperature at which transformation to austenite does not occur. In other words, it is preferable that the intermediate annealing temperature is lower than the Ac1 temperature. By performing intermediate annealing in this manner, bulging occurs, and {100} crystal grains tend to grow. In addition, the time for intermediate annealing is preferably 5 seconds to 60 seconds.

[0036] After intermediate annealing, skin pass rolling is performed. As mentioned above, if skin pass rolling and annealing are performed in a state where bulging has occurred, the {100} grains will grow further from the part where bulging has occurred. This is because the {100} grains are further grown by skin pass rolling. <011> The crystal grains are less susceptible to distortion, and the {111} <112> The crystal grains have a tendency to accumulate distortion, and the {100} <011> The crystal grains are driven by the difference in strain {111} <112> This is to corrode the crystal grains. This corrode phenomenon, which occurs with the strain difference as the driving force, is called strain-induced grain boundary migration (hereinafter, SIBM). The reduction ratio of the skin pass rolling is preferably 5% to 25%. If the reduction ratio is less than 5%, the amount of strain is too small, so SIBM does not occur in the subsequent annealing, and the {100} <011> On the other hand, if the rolling reduction rate exceeds 25%, the amount of distortion becomes too large, and the {111} <112> Recrystallization nucleation (hereafter referred to as nucleation) occurs, in which new crystal grains are born from within the crystal grains. In this nucleation, most of the new grains have {111} <112> The magnetic properties are poor due to the crystal grains.

[0037] After the skin pass rolling, the steel is subjected to a final annealing in order to release the distortion and improve the workability. The final annealing is also performed at a temperature that does not cause the steel to transform into austenite, and the final annealing temperature is set to be lower than the Ac1 temperature. By performing the final annealing in this manner, the {100} <011> The grains are {111} <112> This erodes the crystal grains and improves the magnetic properties. In addition, the time required for the final annealing to reach a temperature of 600°C to Ac1 is set to within 1200 seconds. If the annealing time is too short, most of the distortion introduced by the skin pass remains, and warping occurs when punching complex shapes. On the other hand, if the annealing time is too long, the crystal grains become too coarse, causing large sagging during punching and resulting in poor punching precision.

[0038] After the finish annealing is completed, the non-oriented electrical steel sheet is subjected to forming processing, etc., to obtain a desired steel member. Then, in order to remove distortion, etc., caused by forming processing, etc. (e.g., punching) of the steel member made of the non-oriented electrical steel sheet, the steel member is subjected to stress relief annealing. In this embodiment, in order to generate SIBM below the Ac1 temperature and to make the crystal grain size coarse, the stress relief annealing temperature is set to, for example, about 800°C, and the stress relief annealing time is set to about 2 hours. The magnetic properties can be improved by stress relief annealing.

[0039] In the non-oriented electrical steel sheet (steel member) of this embodiment, the high B50 and excellent anisotropy of the formula (1) are obtained by performing finish rolling at an Ar1 temperature or higher mainly in the hot rolling process among the above-mentioned manufacturing methods. Furthermore, by setting the reduction rate in the skin pass rolling process to about 10%, even more excellent anisotropy of the formula (4) is obtained. In this embodiment, the Ar1 temperature is determined from the thermal expansion change of the steel material (steel plate) during cooling at an average cooling rate of 1°C / s. Also, in this embodiment, the Ac1 temperature is determined from the thermal expansion change of the steel material (steel plate) during heating at an average heating rate of 1°C / s.

[0040] As described above, a steel member made of the non-oriented electrical steel sheet of this embodiment can be manufactured.

[0041] Next, the non-oriented electrical steel sheet of this embodiment will be specifically described with reference to examples. The examples shown below are merely examples of the non-oriented electrical steel sheet, and the non-oriented electrical steel sheet is not limited to the examples below.

[0042] <<First Example>> Molten steel was cast to produce ingots with the compositions shown in Tables 1 and 2 below. Here, the left side of the formula represents the value of the left side of the formula (1) above. The produced ingots were then heated to 1150°C and hot-rolled to a plate thickness of 2.5 mm. After the finish rolling, the ingots were water-cooled and the hot-rolled steel plates were coiled. The temperature at the final pass of the finish rolling (finishing temperature) was 830°C, all of which were higher than the Ar1 temperature. For No. 108, which does not undergo γ-α transformation, the finishing temperature was 850°C. The coiling temperature was also set under the conditions shown in Table 1.

[0043] Next, the hot-rolled steel sheet was subjected to pickling to remove scale, and then rolled at the reduction ratio after cold rolling shown in Table 1. Then, intermediate annealing was performed at 700°C for 30 seconds in a non-oxidizing atmosphere. Next, the second cold rolling (skin pass rolling) was performed at the reduction ratio shown in Table 1.

[0044] Next, to examine the magnetic properties, a second cold rolling (skin pass rolling) was performed followed by a finish annealing at 800°C for 30 seconds, and a 55mm square sample was prepared by shearing, after which a stress relief annealing was performed at 800°C for 2 hours, and the magnetic flux density B50 was measured. The measurement samples were 55mm square samples taken in two different directions, 0° and 45° to the rolling direction. These two types of samples were then measured, and the magnetic flux densities B50 at 0°, 45°, 90°, and 135° to the rolling direction were designated B50L, B50D1, B50C, and B50D2, respectively.

[0045] [Table 1]

[0046] [Table 2]

[0047] The underlines in Tables 1 and 2 indicate conditions outside the scope of the present invention. Inventive examples No. 101 to No. 107, No. 109 to No. 111, and No. 114 to No. 130, all of which had good magnetic flux density B50 in both the 45° direction and the average magnetic flux density B50 for the entire circumference. However, No. 116 and No. 127 were slightly lower in magnetic flux density B50 because the coiling temperature was not appropriate. No. 129 and No. 130 had a low cold rolling reduction ratio, so their magnetic flux density B50 was slightly lower than that of No. 118, which had the same composition and coiling temperature. On the other hand, comparative example No. 108 had a high Si concentration, the value of the left side of the formula was 0 or less, and the composition did not undergo α-γ transformation, so all of the magnetic flux densities B50 were low. Comparative example No. 112 had a low skin pass rolling ratio, so the {100} <011> The strength was less than 5, and the magnetic flux density B50 was low in all cases. <011> The strength was over 30, which is outside the scope of the present invention. No. 113 had a drawback in that the thickness of the hot-rolled plate was as much as 7 mm, making it difficult to operate.

[0048] <<Second Example>> The molten steel was cast to produce an ingot with the composition shown in Table 3 below. The produced ingot was then heated to 1150°C and hot-rolled to a plate thickness of 2.5 mm. After finish rolling, the ingot was water-cooled and the hot-rolled steel plate was coiled. The finish temperature at the final pass of the finish rolling was 830°C, and all temperatures were higher than the Ar1 temperature.

[0049] Next, the hot-rolled steel sheet was pickled to remove scale, and cold-rolled to a thickness of 0.385 mm. Then, intermediate annealing was performed in a non-oxidizing atmosphere, and the intermediate annealing temperature was controlled so that the recrystallization rate was 85%. Next, a second cold rolling (skin pass rolling) was performed to a thickness of 0.35 mm.

[0050] Next, to examine the magnetic properties, a second cold rolling (skin pass rolling) was followed by a finish annealing at 800°C for 30 seconds, and a 55 mm square sample was prepared by shearing, after which a stress relief annealing was performed at 800°C for 2 hours, and the magnetic flux density B50 and iron loss W10 / 400 were measured. The magnetic flux density B50 was measured using the same procedure as in the first embodiment. On the other hand, the iron loss W10 / 400 was measured as the energy loss (W / kg) that occurred in the sample when a 400 Hz AC magnetic field was applied so that the maximum magnetic flux density was 1.0 T. The iron loss was the average value of the results measured at 0°, 45°, 90°, and 135° with respect to the rolling direction.

[0051] [Table 3]

[0052] [Table 4]

[0053] Nos. 201 to 214 are all examples of the invention, and all had good magnetic properties. In particular, Nos. 202 to 204 had higher magnetic flux density B50 than Nos. 201 and 205 to 214, and Nos. 205 to 214 had lower iron loss W10 / 400 than Nos. 201 to 204.

[0054] In the following description, the direction inclined by 45° from the rolling direction described in the description of <Examples of electromagnetic steel sheets used in split cores> will be referred to as an angle of 45° from the rolling direction, and the direction inclined by 135° from the rolling direction will be referred to as an angle of 135° from the rolling direction, as necessary. In addition, the direction inclined by θ° from the rolling direction will be referred to as a direction whose angle with the rolling direction is θ°, as necessary. In this way, the direction inclined by θ° from the rolling direction and the direction whose angle with the rolling direction is θ° have the same meaning.

[0055] The above non-oriented electrical steel sheet was newly developed by the present inventors, and has the best magnetic properties in two directions with angles of 45° and 135° from the rolling direction. On the other hand, the worst magnetic properties are in two directions with angles of 0° and 90° from the rolling direction. Here, the 45° and 135° are theoretical values, and it may not be easy to make them coincide with 45° and 135° in actual manufacturing. Therefore, if the directions with the best magnetic properties are the two directions with angles of 45° and 135° from the rolling direction in theory, the 45° and 135° in actual non-oriented electrical steel sheets may not strictly coincide with 45° and 135°. This is also true for the 0° and 90°. In addition, the magnetic properties of the two directions with the best magnetic properties are theoretically the same, but it may not be easy to make the magnetic properties of the two directions the same in actual manufacturing. Therefore, theoretically, if the magnetic properties of the two directions with the best magnetic properties are the same, the "same" includes cases where the magnetic properties are not strictly the same. This also applies to the two directions with the worst magnetic properties. Note that the clockwise angle is a positive angle.

[0056] <Stator core> The present inventors have considered constructing a stator core from a plurality of split cores so as to effectively utilize the properties of such non-oriented electrical steel sheets, and have found the embodiment described below. Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, unless otherwise specified, the electromagnetic steel sheet is the non-oriented electromagnetic steel sheet described in the section <Examples of electromagnetic steel sheets used in split cores>. In addition, in the following description, the term "being the same (matching)" in terms of length, direction, position, etc. includes not only being (strictly) the same (matching) but also being the same (matching) within a range that does not deviate from the gist of the invention (for example, within the range of error that occurs in the manufacturing process). In this embodiment, the rotating electric machine is an electric motor, specifically an AC electric motor, more specifically a synchronous electric motor, and even more specifically a permanent magnet field type electric motor, which is preferably used in, for example, electric vehicles.

[0057] Fig. 1 is a diagram showing an example of the configuration of a rotating electric machine 10. Fig. 1 is a diagram (plan view) of the rotating electric machine as viewed in a direction parallel to the axis of the rotating electric machine. The XYZ coordinate system shown in Fig. 1 indicates the relationship of directions in the figure. 1, the rotating electric machine 10 includes a stator 20 and a rotor 50. The stator 20 and the rotor 50 are housed in a case (not shown). The stator 20 is fixed to the case. In this embodiment, an inner rotor type rotating electric machine 10 is used in which the rotor 50 is located inside the stator 20. However, an outer rotor type rotating electric machine 10 in which the rotor 50 is located outside the stator 20 may also be used. Also, in this embodiment, the rotating electric machine 10 is a 10-pole, 12-slot three-phase AC motor. However, the number of poles, the number of slots, the number of phases, etc. can be changed as appropriate.

[0058] The stator 20 includes a stator core 21 and a coil (not shown). In the following description, the axial direction of stator core 21 (the direction along the central axis O of stator core 21 (Z-axis direction)) will be referred to as the axial direction as necessary. The radial direction of stator core 21 (the direction perpendicular to the central axis O of stator core 21) will be referred to as the radial direction as necessary. The circumferential direction of stator core 21 (the direction going around the central axis O of stator core 21) will be referred to as the circumferential direction as necessary.

[0059] The stator core 21 includes a plurality of split cores 30. Specifically, in the stator core 21 of this embodiment, twelve split cores 30 are arranged in the circumferential direction, i.e., in the direction rotating around the central axis O. The split cores 30 of this embodiment each have the same shape and size. Each split core 30 has a teeth portion 31 and a core back portion 32.

[0060] The windings of the stator 20 are wound around the teeth portions 31. The teeth portions 31 protrude radially inward from the core back portion 32. That is, the teeth portions 31 protrude radially toward the central axis O. The teeth portions 31 are arranged at equal intervals in the circumferential direction. In this embodiment, twelve teeth portions 31 are provided at intervals of an angle of 30° about the central axis O of the stator core 21. The windings of the stator 20 may be concentrated winding or distributed winding. The core back portion 32 is formed in an arc shape. The multiple split cores 30 are arranged in the circumferential direction, so that the core back portion 32 is formed in an annular shape as a whole.

[0061] Fig. 2 is a diagram showing an example of the configuration of the split core 30. Fig. 2 is a diagram (perspective view) showing one of the multiple split cores 30 included in the stator core 21 as viewed obliquely. The split core 30 is formed by stacking core pieces 40 made of electromagnetic steel sheets. Each core piece 40 is plate-like and has the same shape and size. By stacking the core pieces 40 in the plate thickness direction in the same orientation, the split core 30 has the same shape in the axial direction, i.e., along the central axis O.

[0062] Fig. 3 is a diagram showing an example of the configuration of a core piece 40. Fig. 3 is a plan view of one of the multiple core pieces 40 constituting the split core 30, viewed along the central axis O. As shown in Fig. 3, the core piece 40 has teeth 41 and a core back 42.

[0063] The teeth 41 constitute the teeth portion 31 of the split core 30 by stacking the core pieces 40. The teeth 41 have a teeth base 41a extending radially from the circumferential center of the core back 42 and a flange portion 41b located at the tip of the teeth base 41a. When the split core 30 is used to form the rotating electric machine 10, the flange portion 41b faces the rotor 50.

[0064] The core back 42 constitutes the core back portion 32 of the split core 30 by stacking the core pieces 40. The core back 42 has a convex portion 43a that protrudes in the circumferential direction at one circumferential end, and a concave portion 43b that is concave in the circumferential direction at the other circumferential end. The convex portion 43a and the concave portion 43b have mutually inverted shapes. When multiple split cores 30 are arranged in the circumferential direction, the convex portion 43a fits into the concave portion 43b of the adjacent core piece 40, and the concave portion 43b fits into the convex portion 43a of the adjacent core piece 40.

[0065] In the core piece 40, the radial direction of the tooth 41 and the extending direction of the core back 42 are perpendicular to each other. The radial direction of the tooth 41 is a direction parallel to the plate surface of the tooth 41 and along a line passing through the circumferential center of the tooth 41, as shown by the dashed line L1 in Fig. 3. Alternatively, the radial direction of the tooth 41 is a direction parallel to the plate surface of the tooth 41 and along a line connecting a position P that bisects the outer periphery length of the core back 42 and the center of the outer periphery circle of the core back 42. On the other hand, the extending direction of the core back 42 is a direction perpendicular to the radial direction of the teeth 41. That is, the extending direction of the core back 42 is a direction along a tangent to the outer periphery of the core back 42 at a position P between the dashed dotted line L1 and the outer periphery of the core back 42, as shown by the dashed dotted line L2 in Fig. 3. Alternatively, the extending direction of the core back 42 is a direction along a tangent to the outer periphery of the core back 42 at a position P that bisects the length of the outer periphery of the core back 42.

[0066] 1, the rotor 50 is disposed radially inside the stator core 21. The rotor 50 includes a rotor core 51, a plurality of permanent magnets 52, and a rotating shaft 60. The rotor core 51 is disposed coaxially with the stator core 21. The rotor core 51 has a generally annular (circular) shape. A plurality of permanent magnets 52 are fixed to the rotor core 51. In this embodiment, five sets (ten in total) of permanent magnets 52 are provided at intervals of an angle of 36° about the central axis O of the rotor core 51. A rotating shaft 60 is disposed within the rotor core 51. The rotating shaft 60 is fixed to the rotor core 51. In this embodiment, a surface magnet type motor is used as the permanent magnet field type motor, but an embedded magnet type motor may also be used.

[0067] Here, the core piece 40 is formed, for example, by punching out an electromagnetic steel sheet, which is a rolled plate-shaped base material (hoop). The electromagnetic steel sheet is the electromagnetic steel sheet described in the section <Examples of electromagnetic steel sheets used in split cores>. The ratios (B50 ratio, W15 / 50 ratio, W15 / 100 ratio) of the electromagnetic steel sheet described in the section <Examples of electromagnetic steel sheets used in split cores> to the known non-oriented electromagnetic steel sheet are shown in Table 5. All electromagnetic steel sheets have a thickness of 0.25 [mm]. As the known non-oriented electromagnetic steel sheet, a non-oriented electromagnetic steel sheet with W10 / 400 of 12.8 W / kg was used. W10 / 400 is the iron loss when the magnetic flux density is 1.0 T and the frequency is 400 Hz. In addition, the known non-oriented electromagnetic steel sheet has excellent magnetic properties only in the rolling direction. In the following description, the magnetic steel sheets described in the section <Examples of Magnetic Steel Sheets Used for Split Cores> will also be referred to as developed materials, as necessary. Also, known non-oriented magnetic steel sheets will also be referred to as conventional materials, as necessary.

[0068] [Table 5]

[0069] Here, B50 is the magnetic flux density when excited with a magnetic field strength of 5000 [A / m], and W15 / 100 is the iron loss when the magnetic flux density is 1.5 [T] and the frequency is 100 [Hz]. Here, the magnetic flux density and iron loss were measured using the method described in JIS C 2556:2015. In addition, Table 5 shows the average value for each angle from the rolling direction of the developed material, normalized by setting the average value for each angle from the rolling direction of the conventional material to 1.000 (= average value for each angle from the rolling direction of the developed material ÷ average value for each angle from the rolling direction of the conventional material). In this way, the values ​​in Table 5 are relative values ​​(dimensionless quantities).

[0070] From Table 5, the B50 of the developed material is 5.1% larger than the B50 of the conventional material. The W15 / 50 of the developed material is 12.0% smaller than the W15 / 50 of the conventional material. The W15 / 100 of the developed material is 13.5% smaller than the W15 / 100 of the conventional material. Thus, the developed material has a larger B50 and smaller iron loss than the conventional material.

[0071] Fig. 4 is a graph showing an example of the relationship between the B50 ratio and the angle from the rolling direction. Fig. 5 is a graph showing an example of the relationship between the W15 / 50 ratio and the angle from the rolling direction. Fig. 6 is a graph showing an example of the relationship between the W15 / 100 ratio and the angle from the rolling direction. Fig. 7 is a diagram showing an example of the relationship between the rolling direction RD and the direction in which the magnetic properties are the best. In the following description, the direction in which the magnetic properties are the best is referred to as the direction of easy magnetization as necessary. In Fig. 7, if the counterclockwise angle is a positive angle and the angle of the rolling direction RD is 0°, the directions of easy magnetization are ED1 and ED2. The magnetic properties of the four regions from the rolling direction RD to the direction in which the smaller angle from the rolling direction RD is 90° (the direction shown by the broken line in Fig. 7) are theoretically symmetrical.

[0072] Moreover, the B50 ratio, W15 / 50 ratio, and W15 / 100 ratio shown in Figures 4, 5, and 6 are values ​​normalized by the average value for each angle from the rolling direction of the conventional material, as in Table 5. In other words, the values ​​of the B50 ratio, W15 / 50 ratio, and W15 / 100 ratio shown in Figures 4, 5, and 6 are relative values ​​(dimensionless quantities). As shown in Fig. 4, for the developed material, the B50 ratio is largest when the angle from the rolling direction is 45°, and the B50 ratio decreases as the angle from the rolling direction approaches 0° and 90°. On the other hand, for the conventional material, the B50 ratio is smallest when the angle from the rolling direction is 45°.

[0073] As shown in Fig. 5 and Fig. 6, for the developed material, the W15 / 50 ratio and W15 / 100 ratio are largest when the angle from the rolling direction is 45°, and the W15 / 50 ratio and W15 / 100 ratio decrease as the angle from the rolling direction approaches 0° and 90°. On the other hand, in the conventional material, the W15 / 50 ratio and the W15 / 100 ratio are large when the angle from the rolling direction is 45° to 90°. As described above, the developed material has the best magnetic properties in the direction at an angle of 45° from the rolling direction (easy magnetic direction ED1) and in the direction at an angle of 135° from the rolling direction (easy magnetic direction ED2). On the other hand, the magnetic properties are the worst in the direction at an angle of 0° from the rolling direction (rolling direction RD) and in the direction at an angle of 90° from the rolling direction (direction perpendicular to the rolling direction RD).

[0074] The inventors came up with the idea that the magnetic properties of the entire stator core can be improved by producing core pieces from the developed material, which has better magnetic properties than conventional materials, and manufacturing a stator core with a split core by stacking the produced core pieces. In addition, the developed material has directions in which the magnetic properties are excellent at angles of 45° and 135° from the rolling direction, and the directions in which the magnetic properties are excellent are perpendicular to each other. Meanwhile, the core pieces also have the radial direction of the teeth and the extension direction of the core back perpendicular to each other. Therefore, the inventors came up with the idea that the direction in which the magnetic properties of the developed material are excellent can be matched with the radial direction of the teeth and the extension direction of the core back to produce the core pieces.

[0075] Based on this idea, the core pieces are configured so that the radial direction of the teeth is aligned along a direction that forms an angle of 45° from the rolling direction of the developed material, and the extension direction of the core back is aligned along a direction that forms an angle of 135° from the rolling direction of the developed material. Alternatively, the core pieces are configured so that the radial direction of the teeth is aligned along a direction that forms an angle of 135° from the rolling direction of the developed material, and the extension direction of the core back is aligned along a direction that forms an angle of 45° from the rolling direction of the developed material.

[0076] <Manufacturing method of stator core> Next, a manufacturing method of the stator core 21 including a process of producing the core pieces 40 from the developed material will be described. The manufacturing of the stator core 21 mainly includes a core piece producing process, a split core producing process, and a stator core producing process.

[0077] [Core piece production process] In the core piece production process, the developed material is punched out using a die to produce the core piece 40. Fig. 8 is a diagram for explaining a die for punching out the developed material. Fig. 8 is a schematic diagram (plan view) seen from a direction perpendicular to the plate surface of the developed material 80. Note that Fig. 8 also shows the rolling direction RD and directions (ED1, ED2) in which the magnetic properties are excellent for the developed material 80. The developed material 80 is in the shape of a strip with the rolling direction RD as the longitudinal direction. The developed material 80 is transported along the longitudinal direction by a transport device. Therefore, in the example shown in Fig. 8, the rolling direction RD is the same as the direction of transport by the transport device. Pilot holes 81 are provided at both ends in the width direction of the developed material 80 at intervals in the longitudinal direction.

[0078] First, the conveying device inserts a pilot into the pilot hole 81 and conveys the development material 80 a certain distance. Next, the press device punches out the conveyed development material 80 using a metal mold having a punch and a die, thereby generating core pieces 40. Here, a single punching by the press device generates multiple core pieces 40 each having the same shape and size.

[0079] The press machine punches out the developed material 80 so that the radial direction of the teeth of the core piece 40 and the extension direction of the core back are both in directions that provide excellent magnetic properties for the developed material 80. Specifically, as shown in Fig. 8, the die of the press machine is set so that the radial direction of the teeth (dash line L1) of the core piece 40 is along the direction at an angle of 45° from the rolling direction of the developed material 80 (along the easy magnetization direction ED1). Note that, since the radial direction of the teeth of the core piece 40 and the extension direction of the core back are perpendicular to each other, the extension direction of the core back is set so that the radial direction of the teeth is along the direction at an angle of 45° from the rolling direction of the developed material 80 (along the easy magnetization direction ED2)

[0080] Therefore, the core pieces 40 punched out by the press device have the radial direction of the teeth aligned along the direction at an angle of 45° from the rolling direction, and the extension direction of the core back aligned along the direction at an angle of 135° from the rolling direction. Note that in this embodiment, all of the core pieces 40 punched out by the press device are oriented in the same direction. Therefore, for all of the core pieces 40 punched out, the radial direction of the teeth aligned along the direction at an angle of 45° from the rolling direction, and the extension direction of the core back aligned along the direction at an angle of 135° from the rolling direction.

[0081] In addition, in Figure 8, a die is described that punches out core pieces 40 so that the radial direction of the teeth is along the direction at an angle of 45° from the rolling direction and the extension direction of the core back is along the direction at an angle of 135° from the rolling direction, but this is not limited to this case. For example, a die may be used for punching out core pieces 40A, 40B shown by the two-dot chain lines in Fig. 8 so that the radial direction of the teeth is aligned along a direction at an angle of 135° from the rolling direction and the extension direction of the core back is aligned along a direction at an angle of 45° from the rolling direction. In this case, the punched core pieces 40A, 40B have the radial direction of the teeth aligned along a direction at an angle of 135° from the rolling direction and the extension direction of the core back aligned along a direction at an angle of 45° from the rolling direction. Also, a die may be used for punching out core piece 40C shown by the two-dot chain line in Fig. 8 so that the core piece 40 shown by the solid line in Fig. 8 is rotated 180°. In this case, in the punched core piece 40C, like the core piece 40 shown by the solid line in Fig. 8, the radial direction of the teeth is aligned along the direction at an angle of 45° from the rolling direction, and the extension direction of the core back is aligned along the direction at an angle of 135° from the rolling direction.

[0082] 8 shows a die for punching out four core pieces 40 in a straight line along the width direction of the developed material 80, but the invention is not limited to this and may be a die for punching out five or more or three or less core pieces 40, or may be a die for punching out core pieces in a staggered pattern relative to a straight line. Also, the die may be a die for punching out two or more core pieces at once out of the core pieces 40, 40A to 40C in different orientations shown in FIG. 8.

[0083] [Split core production process] In the split core producing step, the core pieces 40 are stacked to produce the split cores 30. Specifically, the core pieces 40 punched out by a press machine in the core piece production process are all aligned so that they face the same direction, and then connected and stacked so that their plate surfaces are in contact with each other. To connect the core pieces 40, the plate surfaces of the core pieces 40 can be bonded together with an adhesive, or the core pieces 40 can be connected by crimping or welding in the stacking direction. The number of core pieces 40 to be stacked varies depending on the specifications or size of the stator core 21 to be manufactured. When manufacturing the stator core 21 of this embodiment, twelve split cores 30 are produced for one stator core 21.

[0084] As described above, the core pieces 40 have excellent magnetic properties in both the radial direction of the teeth and the extending direction of the core back, and the split cores 30 are stacked so that all the core pieces 40 face the same direction. Therefore, the split cores 30 in which the core pieces 40 are stacked can improve the magnetic properties of the teeth portion 31 and the core back portion 32.

[0085] [Stator core production process] In the stator core production process, the split cores 30 are arranged in the circumferential direction and connected to produce the stator core 21. Specifically, the core back portions 32 of the multiple split cores 30 produced in the split core production process are arranged to form a ring shape. At this time, adjacent split cores 30 are positioned by fitting the convex portions 43a and concave portions 43b of each core piece 40 together. To connect the split cores 30, the core back portions 32 of adjacent split cores 30 can be bonded together with an adhesive or by welding. When manufacturing the stator core 21 of this embodiment, the twelve split cores 30 are arranged in the circumferential direction and connected together. The stator core 21 can be manufactured by the above-described steps. When the manufactured stator core 21 is used to manufacture the stator 20 or the rotating electric machine 10, a known manufacturing method can be used.

[0086] <Example> Next, the magnetic properties were compared between a split core using core pieces made from the developed material and a split core using core pieces made from conventional materials. First, core pieces produced by punching out the developed material were stacked to produce a split core sample. The split core using the core pieces of the developed material in this manner is referred to as the split core of the invention example. The core pieces punched out of the developed material are referred to as the core pieces of the invention example. The split core of the invention example was produced by the method described in the above section <Method of manufacturing a stator core>. Note that in the core pieces of the invention example, the radial direction of the teeth is aligned along a direction at an angle of 45° from the rolling direction of the developed material, and the extension direction of the core back is aligned along a direction at an angle of 135° from the rolling direction of the developed material. Meanwhile, core pieces produced by punching out the conventional material were stacked to produce a split core sample. The split core using the core pieces of the conventional material in this way is referred to as the split core of the comparative example. The core pieces punched out from the conventional material are also referred to as the core pieces of the comparative example. The split core of the comparative example was produced by the method described in the above section <Method of manufacturing a stator core>. Note that in the core pieces of the comparative example, the radial direction of the teeth is aligned along a direction at an angle of 0° from the rolling direction of the conventional material, and the extension direction of the core back is aligned along a direction at an angle of 90° from the rolling direction of the conventional material.

[0087] The split core of the invention example and the split core of the comparative example have the following specifications. Outer diameter of stator core: 77.0 [mm], inner diameter of stator core: 40.0 [mm], height of stator core (laminated thickness): 45.0 [mm], thickness of core piece (electromagnetic steel sheet): 0.25 [mm], number of poles: 10, number of slots: 12 Here, Table 6 shows the ratio of magnetic flux density when excited at B50, that is, a magnetic field strength of 5000 [A / m], as a comparison of magnetic properties between the split core of the invention example and the split core of the comparative example.

[0088] [Table 6]

[0089] As shown in Table 6, when the magnetic flux density of the split core of the comparative example is taken as 1.000, the magnetic flux density of the split core of the invention example is 1.042. As can be seen from Table 6, the B50 of the split core of the invention example is 4.2% higher than the B50 of the split core of the comparative example. In this way, it was confirmed that the split core using core pieces made from the developed material has a higher magnetic flux density and improved magnetic properties compared to the split core using core pieces made from the conventional material.

[0090] By manufacturing a stator core (referred to as the stator core of the invention example) by circumferentially arranging the split cores of the invention example, which have a high magnetic flux density, the magnetic flux density can be made larger throughout the stator core than a stator core manufactured by circumferentially arranging the split cores of the comparative example (referred to as the stator core of the comparative example), thereby improving the magnetic characteristics. In addition, by applying the stator core of the example of the invention, which has a large magnetic flux density, to a rotary electric machine, it is possible to improve the torque compared to a rotary electric machine using the stator core of the comparative example. Furthermore, in a rotary electric machine using the stator core of the example of the invention, when outputting the same torque as a rotary electric machine using the stator core of the comparative example, it is possible to reduce the current flowing through the windings wound around the stator core of the example of the invention, thereby reducing copper loss.

[0091] As described above, according to this embodiment, the magnetic properties of the entire stator core including the split cores can be improved by using the developed electromagnetic steel sheet with excellent magnetic properties for the core pieces that make up the split cores. Also, according to this embodiment, for each core piece of all the split cores included in the stator core, both the radial direction of the teeth and the extension direction of the core back are aligned with the direction in which the magnetic properties of the developed electromagnetic steel sheet are excellent, so that the magnetic properties of the entire stator core can be further improved. In addition, since the magnetic properties are improved, magnetic saturation of the stator core can be suppressed even if the width of the teeth portion and the width of the core back portion are narrowed, so that the area of ​​the slots can be expanded and the space factor of the windings can be improved. In this embodiment, the superiority of the developed material over the conventional material that is a non-oriented electrical steel sheet has been described, but the developed material is also superior to the conventional material that is a bidirectional electrical steel sheet. Specifically, the developed material can reduce manufacturing costs compared to the conventional material that is a bidirectional electrical steel sheet. In addition, since the grain size of the steel sheet structure of the developed material is smaller than that of the conventional material that is a bidirectional electrical steel sheet, iron loss under high frequency conditions can be suppressed when the core pieces are laminated to form a split core.

[0092] <Modification> In the above-described embodiment, a case has been described in which for each core piece of all the split cores provided in the stator core, both the radial direction of the teeth and the extension direction of the core back are aligned along the direction in which the magnetic properties of the electromagnetic steel sheet of the developed material are excellent, but this is not limited to this case. In this modification, a case will be described in which the radial direction of the teeth and the extension direction of the core back of each core piece of at least one of the multiple split cores included in the stator core are sufficient as long as they are aligned with the direction in which the magnetic properties of the electromagnetic steel sheet of the developed material are excellent. In other words, the stator core of this modification is a mixture of split cores composed of core pieces in which the radial direction of the teeth and the extension direction of the core back are aligned with the direction in which the magnetic properties of the electromagnetic steel sheet of the developed material are excellent, and split cores composed of core pieces in which the radial direction of the teeth or the extension direction of the core back are not aligned with the direction in which the magnetic properties of the electromagnetic steel sheet of the developed material are excellent. In a stator core in which different types of split cores are mixed in this way, there are parts with good magnetic properties and parts with bad magnetic properties, which causes variation in the distribution of the magnetic properties of the stator core, and increases iron loss.

[0093] In this modification, when different types of split cores are mixed, the stator core is configured so that the width of the teeth portion whose radial direction is aligned with the direction of superior magnetic properties is narrower than the width of the teeth portion whose radial direction is not aligned with the direction of superior magnetic properties. Furthermore, in this modification, when different types of split cores are mixed, the stator core is configured so that the product of the width of the teeth portion of the split core and the magnetic flux density of the teeth portion when excited with a predetermined magnetic field strength is approximately constant for each tooth portion of all split cores. By configuring the stator core in this way, it is possible to reduce the variation in magnetic flux density and suppress iron loss even in a stator core that includes different types of split cores.

[0094] Fig. 9 is a diagram for explaining the width of the teeth. Fig. 9(a) is an example of teeth 31A that are parallel along the radial direction. In this example, the teeth 31A themselves are parallel along the radial direction. Fig. 9(b) is an example of teeth 31B in which the slots are parallel along the radial direction. In this example, the slots located between the teeth 31B adjacent in the circumferential direction are parallel along the radial direction. Here, the width of the teeth is the length in the circumferential direction of the stator core at the center of the straight-line area of ​​the teeth, which is determined for each of the two ends of the teeth in the circumferential direction of the stator core in a cross section of the stator core taken perpendicular to the axis of the stator core, by measuring the area of ​​the longest straight line among the straight lines constituting the ends of the teeth in the circumferential direction of the stator core.

[0095] In the example shown in Fig. 9(a), the straight line connecting positions 311 and 312 and the straight line connecting positions 313 and 314 form the teeth straight line region. In the example shown in Fig. 9(a), the center positions of the teeth straight line region are positions 321 and 322. Therefore, the width of teeth portion 31A shown in Fig. 9(a) is the distance TW between positions 321 and 322. In the example shown in Fig. 9(b), the straight line connecting positions 315 and 316 and the straight line connecting positions 317 and 318 form the teeth straight line region. In the example shown in Fig. 9(b), the center positions of the teeth straight line region are positions 323 and 324. Therefore, the width of teeth portion 31B shown in Fig. 9(b) is the distance TW between positions 323 and 324.

[0096] FIG. 9(a) shows an example of teeth 31A that are parallel along the radial direction, and therefore the width of teeth 31A is constant regardless of the radial position in the teeth linear region. On the other hand, in (b) of Figure 9, since the slot is an example of a tooth portion 31B that is parallel along the radial direction, the actual width of the tooth portion 31B varies depending on the radial location in the straight tooth region, and therefore the width of the tooth portion 31B is set to the distance TW between the above-mentioned positions 323 and 324 as a representative value.

[0097] In the above-described embodiment, the method described in the section <Method of manufacturing stator core> can be used to produce split cores in which the radial direction of the teeth is aligned with the direction in which the magnetic properties are excellent. Next, an example of a case where a split core is produced in which the radial direction of the teeth is not aligned with the direction of excellent magnetic properties will be described. Note that the same content as that described in the above section <Method of manufacturing a stator core> will be omitted as appropriate.

[0098] First, in the core piece production process, the developed material is punched out using a die to produce the core piece 90. Fig. 10 is a diagram for explaining a die used to punch out the developed material. The developed material 80 shown in Fig. 10 is the same electromagnetic steel sheet as the developed material 80 shown in Fig. 8. Fig. 10 shows the rolling direction RD and the directions (ED1, ED2) in which the magnetic properties are excellent for the developed material 80.

[0099] The press machine punches out the developed material 80 such that neither the radial direction of the teeth of the core piece 90 nor the extension direction of the core back are in a direction that provides superior magnetic properties for the developed material 80. Specifically, as shown in Fig. 10, the die of the press machine is set so that the radial direction of the teeth of the core piece 90 (dotted line L1) is aligned along a direction that forms an angle of 0° from the rolling direction of the developed material 80. Note that, since the radial direction of the teeth of the core piece 90 and the extension direction of the core back are perpendicular to each other, the extension direction of the core back is set so that it forms an angle of 90° from the rolling direction of the developed material 80 by aligning the radial direction of the teeth along a direction that forms an angle of 0° from the rolling direction of the developed material 80.

[0100] Therefore, in the core pieces 90 punched out by the press device, the radial direction of the teeth is along the direction at an angle of 0° from the rolling direction, and the extension direction of the core back is along the direction at an angle of 90° from the rolling direction. Note that in this modified example, the radial directions of the teeth of all the core pieces 90 punched out by the press device are in the same direction. Therefore, for all the core pieces 90 punched out, the radial direction of the teeth is along the direction at an angle of 0° from the rolling direction, and the extension direction of the core back is along the direction at an angle of 90° from the rolling direction. Next, the punched-out core pieces 90 are all aligned so that they are facing the same direction, and then connected and stacked so that the plate surfaces are in contact with each other, thereby producing a split core in which the radial direction of the teeth does not align with the direction of excellent magnetic properties.

[0101] Here, the core piece 90 shown in Fig. 10 and the core piece 40 shown in Fig. 8 are set to have different tooth widths. Specifically, the tooth width of the core piece 90 shown in Fig. 10 is set to be wider than the tooth width of the core piece 40 shown in Fig. 8. In other words, the tooth width of the core piece 40 shown in Fig. 8 is set to be narrower than the tooth width of the core piece 90 shown in Fig. 10. By constructing a stator core by mixing a split core in which core pieces 90 shown in Fig. 10 are laminated with a split core in which core pieces 40 shown in Fig. 8 are laminated, it is possible to configure the width of the teeth portion whose radial direction is aligned with the direction in which the magnetic properties are excellent to be narrower than the width of the teeth portion whose radial direction is not aligned with the direction in which the magnetic properties are excellent. By configuring the stator core in this way, it is possible to reduce the variation in magnetic flux density within the stator core.

[0102] In addition, in this modified example, when different types of split cores are mixed, the stator core is configured so that the product of the width of the teeth portion of the split core and the magnetic flux density of the teeth portion when excited with a predetermined magnetic field strength is approximately constant for each tooth portion of all the split cores. In the following, an example will be described in which the width of the teeth is determined so that the product of the width of the teeth and the magnetic flux density of the teeth is approximately constant for each tooth of all the split cores.

[0103] First, in a rotary electric machine to which the stator core is to be applied, when the width of all teeth is constant, the average magnetic flux density of the teeth is analyzed when the machine is operated under a specified operating condition (e.g., a specified torque). The average magnetic flux density of the teeth is the average of the maximum values ​​of the magnetic flux density at each location in each tooth. The average magnetic flux density can be obtained by performing an electromagnetic field analysis (numerical analysis) based on Maxwell's equations, or by measuring the induced voltage in the manufactured stator core using a search coil and integrating the induced voltage.

[0104] Next, the average magnetic field strength H [A / m] of the teeth is calculated from the average magnetic flux density of the teeth. The average magnetic field strength of the teeth can be calculated based on the relative permeability of the developed material. Next, the magnetic flux density B [T] of the teeth for each angle from the rolling direction when excited with the average magnetic field strength of the teeth is calculated based on the material properties of the developed material A. The magnetic flux density of the teeth for each angle from the rolling direction can be derived from the BH characteristics of the developed material at that angle from the rolling direction. In this modification, for a split core in which core pieces 40 shown in Fig. 8 are stacked, the magnetic flux density of the teeth is calculated at an angle of 45° from the rolling direction. Also, for a split core in which core pieces 90 shown in Fig. 10 are stacked, the magnetic flux density of the teeth is calculated at an angle of 0° from the rolling direction. As described above, for the developed material, the B50 ratio is largest when the angle from the rolling direction is 45°, and the B50 ratio decreases as the angles from the rolling direction approach 0° and 90°. Therefore, the magnetic flux density of the teeth at an angle of 45° from the rolling direction is calculated to be large, and the magnetic flux density of the teeth at an angle of 0° from the rolling direction is calculated to be small.

[0105] Next, an optimal width of the teeth is determined for each angle from the rolling direction. Specifically, the width of the teeth is determined based on the calculated magnetic flux density of the teeth for each angle from the rolling direction so that the product of the width of the teeth and the magnetic flux density of the teeth is approximately constant for each tooth. Therefore, in a split core in which core pieces 40 shown in FIG. 8 are stacked, the width of the teeth portion is calculated to be narrower, and in a split core in which core pieces 90 shown in FIG. 10 are stacked, the width of the teeth portion is calculated to be wider.

[0106] A die for punching out core piece 40 shown in Fig. 8 and a die for punching out core piece 90 shown in Fig. 10 are designed so as to achieve the optimal width of the teeth portion determined in this manner. The developed material is punched out with each of the designed dies to produce core piece 40 and core piece 90, respectively. By mixing split cores formed by stacking core pieces 40 shown in Figure 8 with split cores formed by stacking core pieces 90 shown in Figure 10 to construct a stator core, it is possible to construct a stator core so that the product of the width of the teeth portion of the split core and the magnetic flux density of the teeth portion when excited with a predetermined magnetic field strength is approximately constant for each tooth portion of all of the split cores.

[0107] In this way, in this modification, when different types of split cores are mixed, the stator core is configured so that the product of the width of the teeth of the split core and the magnetic flux density of the teeth when excited with a predetermined magnetic field strength is approximately constant for each tooth of all the split cores. Therefore, even in a stator core in which different types of split cores are mixed, the variation in magnetic flux density can be reduced and iron loss can be suppressed. Note that approximately constant does not necessarily mean that it is completely constant, but includes a range in which iron loss can be suppressed more than in the comparative example. Specifically, approximately constant means that the difference between the maximum value and the minimum value of the product of the width of the teeth and the magnetic flux density of the teeth is within a range of ±5%. For example, when the product of the width of the teeth and the magnetic flux density of the teeth is 1.5 [T], the product of the width of the teeth and the magnetic flux density of the teeth in each tooth is approximately within a range of 1.425 [T] to 1.575 [T] (within a range of ±5%).

[0108] In this modification, the case of analyzing the average magnetic flux density of the teeth when the motor is operated under a predetermined operating condition (e.g., a predetermined torque) has been described, but the predetermined operating condition can be selected as appropriate. For example, the operating condition with the highest operating time ratio among multiple assumed operating conditions may be set as the predetermined operating condition. The determined optimal width of the teeth may be further weighted based on the operating time ratio for each of the multiple operating conditions. In addition, in this modification, a stator core in which two types of split cores are mixed has been described, but the present invention is not limited to this case and can also be applied to a stator core in which three or more types of split cores are mixed.

[0109] Although the present invention has been described above in conjunction with various embodiments, the present invention is not limited to these embodiments, and modifications and the like are possible within the scope of the present invention. [Industrial Applicability]

[0110] According to the present invention, it is possible to improve the magnetic characteristics of a stator core having a plurality of split cores, and thus the present invention has high industrial applicability. [Explanation of symbols]

[0111] 10: Rotating electric machine 21: Stator core 30: Split core 31: Teeth section 32: Core back section 40: Core piece 41: Teeth 42: Coreback 50:Rota 51: Rotor core 52: Permanent magnet 60: Rotation axis

Claims

1. A stator core including a plurality of split cores, The plurality of split cores are formed by laminating core pieces made of electromagnetic steel sheets, The electromagnetic steel sheet is In mass percent, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. Al: 0.0001% to 1.0%, S: 0.0100% or less, N: 0.0100% or less, One or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, and Au: 2.50% to 5.00% in total, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total; When the Mn content (mass%) is [Mn], the Ni content (mass%) is [Ni], the Co content (mass%) is [Co], the Pt content (mass%) is [Pt], the Pb content (mass%) is [Pb], the Cu content (mass%) is [Cu], the Au content (mass%) is [Au], the Si content (mass%) is [Si], and the sol. Al content (mass%) is [sol. Al], the following formula (1) is satisfied, The balance has a chemical composition consisting of Fe and impurities, When the B50 value in the rolling direction is B50L, the B50 value in the direction tilted 45° from the rolling direction is B50D1, the B50 value in the direction tilted 90° from the rolling direction is B50C, and the B50 value in the direction tilted 135° from the rolling direction is B50D2, the following formulas (2) and (4) are satisfied, the X-ray random intensity ratio of {100}<011> is 5 or more and less than 30, and the sheet thickness is 0.50 mm or less, The core piece of at least one of the split cores includes A stator core, characterized in that both the radial direction of the teeth and the extending direction of the core back are aligned along the direction in which the magnetic properties of the electromagnetic steel sheets are excellent. ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0%...(1) (B50D1+B50D2) / 2>1.7T...(2) (B50D1+B50D2) / 2>1.1×(B50L+B50C) / 2...(4)

2. A stator core having a plurality of split cores, The plurality of split cores are formed by laminating core pieces made of electromagnetic steel sheets, The electromagnetic steel sheet is In mass percent, C: 0.0100% or less, Si: 1.50% to 4.00%, sol. Al: 0.0001% to 1.0%, S: 0.0100% or less, N: 0.0100% or less, One or more selected from the group consisting of Mn, Ni, Co, Pt, Pb, Cu, and Au: 2.50% to 5.00% in total, Sn: 0.000% to 0.400%, Sb: 0.000% to 0.400%, P: 0.000% to 0.400%, and One or more selected from the group consisting of Mg, Ca, Sr, Ba, Ce, La, Nd, Pr, Zn, and Cd: 0.0000% to 0.0100% in total; When the Mn content (mass%) is [Mn], the Ni content (mass%) is [Ni], the Co content (mass%) is [Co], the Pt content (mass%) is [Pt], the Pb content (mass%) is [Pb], the Cu content (mass%) is [Cu], the Au content (mass%) is [Au], the Si content (mass%) is [Si], and the sol. Al content (mass%) is [sol. Al], the following formula (1) is satisfied, The balance has a chemical composition consisting of Fe and impurities, When the B50 value in the rolling direction is B50L, the B50 value in the direction tilted at 45° from the rolling direction is B50D1, the B50 value in the direction tilted at 90° from the rolling direction is B50C, and the B50 value in the direction tilted at 135° from the rolling direction is B50D2, the following formulas (3) and (6) are satisfied, the X-ray random intensity ratio of {100}<011> is 5 or more and less than 30, and the sheet thickness is 0.50 mm or less, The core piece of at least one of the split cores includes A stator core, characterized in that both the radial direction of the teeth and the extending direction of the core back are aligned along the direction in which the magnetic properties of the electromagnetic steel sheets are excellent. ([Mn]+[Ni]+[Co]+[Pt]+[Pb]+[Cu]+[Au])-([Si]+[sol.Al])>0%...(1) (B50D1+B50D2) / 2>(B50L+B50C) / 2...(3) (B50D1+B50D2) / 2>1.8T...(6)

3. 3. The stator core according to claim 1, wherein the following formula (5) is satisfied: (B50D1+B50D2) / 2>1.2×(B50L+B50C) / 2...(5)

4. A stator core described in any one of claims 1 to 3, characterized in that it contains one or more elements selected from the group consisting of 0.020% to 0.400% Sn and 0.020% to 0.400% Sb.

5. The electromagnetic steel sheet is the directions having excellent magnetic properties are at angles of 45° and 135° from the rolling direction of the electrical steel sheet, The radial direction of the teeth is along either one of an angle of 45° and an angle of 135° from the rolling direction, 2. The stator core according to claim 1, wherein the extending direction of the core back is along the other of an angle of 45° or 135° from the rolling direction.

6. The plurality of split cores include A stator core as described in any one of claims 1 to 5, characterized in that in all of the core pieces of the split core, the radial direction of the teeth and the extension direction of the core back are both along the direction in which the magnetic properties of the electromagnetic steel sheet are excellent.

7. Each of the plurality of split cores has a teeth portion, A stator core as described in any one of claims 1 to 5, characterized in that, among the multiple tooth portions, the width of the tooth portions along the direction in which the magnetic properties are superior is narrower than the width of the tooth portions not along the direction in which the magnetic properties are superior.

8. 8. A stator core as described in claim 7, characterized in that the product of the width of the tooth portion and the magnetic flux density of the tooth portion when excited with a predetermined magnetic field strength is approximately constant for each tooth portion of the multiple split cores.

9. A rotating electric machine comprising the stator core according to claim 1 .

Citation Information

Patent Citations

  • Motor core

    JP1996047185A

  • Core for rotating machine and salient-pole type rotor core

    JP1996223830A

  • Electric motor

    JP2002320350A

  • Electromagnetic steel sheet, and manufacturing method of electromagnetic steel sheet

    JP2019178380A

  • Motor and method for manufacturing motor

    WO2017090571A1