Compositions and films containing polylactic acid polymers, polyvinyl acetate polymers, and plasticizers
A composition of semi-crystalline PLA, PVAc, and a plasticizer with a nucleating agent addresses crystallinity and mechanical issues in PLA polymers, enhancing properties for applications like pressure-sensitive adhesive tapes.
Patent Information
- Application Number
- JP2022164470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-12-22
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2035-12-14
AI Technical Summary
Existing polylactic acid (PLA) polymers face challenges in achieving optimal crystallinity and mechanical properties, particularly when combined with polyvinyl acetate (PVAc) polymers, leading to issues such as plasticizer migration and inadequate mechanical performance.
A composition comprising semi-crystalline PLA, PVAc with a glass transition temperature (Tg) of at least 25°C, a plasticizer, and optionally amorphous PLA, along with a nucleating agent, is formulated to enhance crystallization and mechanical properties, with specific ratios and additives to prevent plasticizer migration.
The composition achieves improved mechanical properties, including high tensile strength, flexibility, and resistance to plasticizer migration, making it suitable for applications like pressure-sensitive adhesive tapes.
Smart Images

Figure 0007588626000008 
Figure 0007588626000009 
Figure 0007588626000010
Abstract
Description
[Technical field]
[0001] (overview) In one embodiment, a composition is described that includes a semi-crystalline polylactic acid polymer, a polyvinyl acetate polymer having a glass transition temperature (Tg) of at least 25° C., a plasticizer, and optionally an amorphous polylactic acid polymer.
[0002] In another embodiment, a composition is described that includes a semicrystalline polylactic acid polymer, a polyvinyl acetate polymer having a Tg of at least 25° C., a plasticizer, a nucleating agent, and optionally an amorphous polylactic acid polymer.
[0003] In some embodiments, the polyvinyl acetate polymer is present in an amount of at least 15 or 20 wt %, based on the total amount of the polylactic acid polymer, the polyvinyl acetate polymer, and the plasticizer. In some embodiments, the plasticizer is present in an amount ranging from 5 to 35 wt %, based on the total amount of the polylactic acid polymer, the polyvinyl acetate polymer, and the plasticizer. In some embodiments, the semicrystalline polylactic acid polymer contains at least 90 wt % polymerized units of L-lactide and less than 10, 9, 8, 7, 6, 5, 4, 3, or 2 wt % of D-lactide and / or meso-lactide. In preferred embodiments, the composition has a net melting endotherm, ΔH, in the second heating scan, greater than 10, 11, 12, 13, 14, or 15 J / g and less than 40 J / g. nm2 Further, the composition preferably has a Tg of less than 30°C, 25°C or 20°C.
[0004] In another embodiment, a film comprising such a composition is described. The film preferably has a net melting endotherm, ΔH, in the first heating scan, greater than 10, 11, 12, 13, 14, or 15 J / g and less than 40 J / g. nm1 Further, the film preferably has a Tg of less than 30°C, 25°C or 20°C.
[0005] In another embodiment, an article, such as a tape or sheet, is described that includes a film described herein and a layer of pressure sensitive adhesive disposed on the film. [Brief description of the drawings]
[0006] [Figure 1] 1 is a representative DSC profile of a composition containing a nucleating agent that exhibits a sharp crystallization peak exotherm during cooling. [Diagram 2] 1 is a representative DSC profile of a composition without a nucleating agent that did not exhibit a crystallization peak exotherm during cooling. [Diagram 3] FIG. 13 is a diagram showing the results of dynamic viscoelasticity measurement in Example 12. [Figure 4] FIG. 13 is a diagram showing the results of dynamic viscoelasticity measurement in Example 16. Summary of the Invention
[0007] (Detailed Description) The compositions described herein include polylactic acid ("PLA") polymers. Lactic acid is a renewable raw material obtained by bacterial fermentation of corn starch or cane sugar and is therefore considered a natural, or in other words "biomass" material. Lactic acid has two optical isomers, L-lactic acid (also known as (S)-lactic acid) and D-lactic acid (also known as (R)-lactic acid), as shown below: [ka]
[0008] Polyester polycondensation of lactic acid produces polylactic acid polymer.
[0009] More commonly, lactic acid is usually converted to cyclic lactide monomer, and the lactide is ring-opening polymerized, as shown below: [ka]
[0010] The resulting polymeric material is commonly referred to as a polylactide polymer.
[0011] The degree of crystallinity, and therefore many important properties, is controlled primarily by the ratio of D and / or meso-lactide to L cyclic lactide monomers used. Similarly, in polymers prepared by direct polyester polycondensation of lactic acid, the degree of crystallinity is controlled primarily by the ratio of polymerized units derived from D-lactic acid to those derived from L-lactic acid.
[0012] The compositions and films described herein typically include a semi-crystalline PLA polymer, either alone or in combination with an amorphous PLA polymer. Both semi-crystalline and amorphous PLA polymers typically include a high concentration of polymerized units derived from L-lactic acid (e.g., L-lactide) along with a low concentration of polymerized units derived from D-lactic acid (e.g., D-lactide).
[0013] Semicrystalline PLA polymers typically contain at least 90, 91, 92, 93, 94, or 95 wt% polymerized units derived from L-lactic acid (e.g., L-lactide) and no more than 10, 9, 8, 7, 6, or 5 wt% polymerized units derived from D-lactic acid (e.g., D-lactide and / or meso-lactide). In yet other embodiments, semicrystalline PLA polymers contain at least 96 wt% polymerized units derived from L-lactic acid (e.g., L-lactide) and no more than 4, 3, or 2 wt% polymerized units derived from D-lactic acid (e.g., D-lactide and / or meso-lactide). Similarly, compositions and films contain even lower concentrations of polymerized units derived from D-lactic acid (e.g., D-lactide and / or meso-lactide), depending on the concentration of semicrystalline PLA polymer in the composition or film. For example, if the composition comprises 15 wt% semi-crystalline PLA containing about 2 wt% D-lactide and / or meso-lactide, the composition comprises about 0.3 wt% D-lactide and / or meso-lactide. The compositions and films typically comprise no more than 9, 8, 7, 6, 5, 4, 3, 2, 1.5, 1.0, 0.5, 0.4, 0.3, 0.2, or 0.1 wt% polymerized units derived from D-lactic acid (e.g., D-lactide and / or meso-lactide). Suitable examples of semi-crystalline PLA include Natureworks™ Ingeo™ 4042D and 4032D. These polymers have been described in the literature as having a molecular weight Mw of about 200,000 g / mol, an Mn of about 100,000 g / mol, and a polydispersity of about 2.0.
[0014] The composition may further comprise an amorphous PLA polymer blended with the semi-crystalline PLA. Amorphous PLA typically comprises 90 wt% or less of polymerized units derived from L-lactic acid and more than 10 wt% of polymerized units derived from D-lactic acid (e.g., D-lactide and / or meso-lactide). In some embodiments, the amorphous PLA comprises at least 80 or 85 wt% of polymerized units derived from L-lactic acid (e.g., L-lactide). In some embodiments, the amorphous PLA comprises 20 or 15 wt% or less of polymerized units derived from D-lactic acid (e.g., D-lactide and / or meso-lactide). Suitable amorphous PLA includes Natureworks™ Ingeo™ 4060D grade. This polymer has been described in the literature to have a molecular weight Mw of about 180,000 g / mol.
[0015] The PLA polymer is preferably a "film grade" polymer having a melt flow rate (measured according to ASTM D1238) of 25, 20, 15, or 10 g / min or less at 210°C and a mass of 2.16 kg. In some embodiments, the PLA polymer has a melt flow rate of less than 10 or 9 g / min at 210°C. The melt flow rate is related to the molecular weight of the PLA polymer. The PLA polymer typically has a weight average molecular weight (Mw) of at least 50,000 g / mol, 75,000 g / mol, 100,000 g / mol, 125,000 g / mol, 150,000 g / mol, as determined by gel permeation chromatography using polystyrene standards. In some embodiments, the molecular weight (Mw) is less than 400,000 g / mol, 350,000 g / mol, or 300,000 g / mol.
[0016] PLA polymers typically have a tensile strength in the range of about 25-150 MPa, a tensile modulus in the range of about 1000-7500 MPa, and a tensile elongation in the range of at least 3, 4, or 5 to about 15%. In some embodiments, the tensile strength of the PLA polymer is at least 30, 40, or 50 MPa. In some embodiments, the tensile strength of the PLA polymer is no more than 125, 100, or 75 MPa. In some embodiments, the tensile modulus of the PLA polymer is at least 1500, 2000, or 2500 MPa. In some embodiments, the tensile modulus of the PLA polymer is no more than 7000, 6500, 6000, 5500, 5000, or 4000 MPa. Such tensile and elongation properties may be determined by ASTM D882 and are typically reported by the manufacturer or supplier of such PLA polymer.
[0017] PLA polymers generally have a glass transition temperature, Tg, in the range of about 50-65° C., which can be determined by differential scanning calorimetry (DSC) as described in the Examples below.
[0018] Semi-crystalline PLA polymers typically have a melting point in the range of 140-175° C. PLA polymers, which typically include semi-crystalline PLA alone or in combination with amorphous PLA polymers, can be melt processed at temperatures of 180, 190, 200, 210, 220, or 230° C.
[0019] The compositions typically include semi-crystalline PLA polymer or a blend of semi-crystalline PLA and amorphous PLA in an amount of at least 40, 45, or 50 wt %, based on the total weight of the PLA polymer, polyvinyl acetate polymer, and plasticizer, and the total amount of PLA polymer is typically no more than 90, 85, 80, 75, or 70 wt % of the total weight of the PLA polymer, polyvinyl acetate polymer, and plasticizer.
[0020] When the composition comprises a blend of semi-crystalline PLA and amorphous PLA, the amount of semi-crystalline PLA is typically at least 10, 15, or 20 wt% based on the total weight of the PLA polymer, the polyvinyl acetate polymer, and the plasticizer. In some embodiments, the amount of amorphous PLA polymer ranges from 10, 15, 25, or 30 wt% to 50, 55, or 60 wt% based on the total weight of the PLA polymer, the polyvinyl acetate polymer, and the plasticizer. The amount of amorphous PLA polymer may exceed the amount of crystalline polymer.
[0021] The composition further comprises a polyvinyl acetate polymer having a Tg of at least 25, 30, 35 or 40° C. The Tg of polyvinyl acetate is typically no greater than 50 or 45° C.
[0022] The polyvinyl acetate polymer typically has a weight or number average molecular weight (as determined by size exclusion chromatography using polystyrene standards) of at least 50,000 g / mol, 75,000 g / mol, 100,000 g / mol, 125,000 g / mol, 150,000 g / mol, 175,000 g / mol, 200,000 g / mol, 225,000 g / mol, or 250,000 g / mol. In some embodiments, the molecular weight (Mw) is no greater than 1,000,000 g / mol, 750,000 g / mol, 500,000 g / mol, 450,000 g / mol, 400,000 g / mol, 350,000 g / mol, or 300,000 g / mol. In some embodiments, the molecular weight of the polyvinyl acetate polymer exceeds the molecular weight of the PLA polymer. Polyvinyl acetate polymer is 10 to 50 mPa * % in ethyl acetate at 20° C. in the range of 0.15 to 1.0 s.
[0023] Polyvinyl acetate polymers are typically homopolymers. However, the polymer may contain a relatively low concentration of repeat units derived from other comonomers, provided that the Tg of the polyvinyl acetate polymer is within the aforementioned range. Other comonomers include, for example, acrylic monomers such as acrylic acid and methyl acrylate, vinyl monomers such as vinyl chloride and vinyl pyrrolidone, and C2-C8 alkylene monomers such as ethylene. The total concentration of repeat units derived from other comonomers in the polyvinyl acetate polymer is typically 10, 9, 8, 7, 6, or 5 wt % or less. In some embodiments, the total concentration of repeat units derived from other comonomers in the polyvinyl acetate polymer is typically 4, 3, 2, 1, or 0.5 wt % or less. The polyvinyl acetate polymer is usually hydrolyzed to a low level. The polymerized units of the polyvinyl acetate polymer that are hydrolyzed to vinyl alcohol units are usually 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, or 0.5 mol % or less of the polyvinyl acetate polymer.
[0024] Polyvinyl acetate polymers are commercially available from a variety of sources, including Wacker under the trade name VINNAPAS™. Prior to combination with PLA, such polyvinyl acetate polymers are often in the form of a solid powder (e.g., white) or colorless beads. In some embodiments, the polyvinyl acetate polymer (e.g., a powder prior to combination with the PLA polymer) is not water-redispersible.
[0025] A single polyvinyl acetate polymer or a combination of two or more polyvinyl acetate polymers can be utilized.
[0026] The total amount of polyvinyl acetate polymer present in the compositions described herein is at least about 10 wt%, and typically no more than about 50, 45, or 40 wt%, based on the total weight of the PLA polymer, the polyvinyl acetate polymer, and the plasticizer. In some embodiments, the concentration of polyvinyl acetate polymer is present in an amount of at least 15 or 20 wt%.
[0027] In some embodiments, the compositions have a Tg of less than 30, 29, 28, 27, 26, 25, 24, 23, 22, 21, or 20° C. and exhibit no plasticizer migration when aged for 24 hours at 80° C. (according to the test method described in the Examples), a property that results from the inclusion of a polyvinyl acetate polymer.
[0028] The composition further comprises a plasticizer. The total amount of plasticizer in the composition typically ranges from about 5 wt % to about 35, 40, 45, or 50 wt %, based on the total weight of the PLA polymer, the polyvinyl acetate polymer, and the plasticizer.
[0029] A variety of plasticizers capable of plasticizing PLA have been described in the art. Plasticizers are generally liquid at 25° C. and typically have a molecular weight ranging from about 200 g / mol to 10,000 g / mol. In some embodiments, the molecular weight of the plasticizer is 5,000 g / mol or less. In other embodiments, the molecular weight of the plasticizer is 4,000, 3,000, 2,000, or 1,000 g / mol or less. Various combinations of plasticizers can be utilized.
[0030] The plasticizer preferably contains one or more alkyl or aliphatic ester or ether groups. Typically, multifunctional esters and / or ethers are preferred. These include alkyl phosphate esters, dialkyl ether diesters, tricarboxylate esters, epoxidized oils and esters, polyesters, polyglycol diesters, alkyl alkyl ether diesters, aliphatic diesters, alkyl ether monoesters, citrate esters, dicarboxylate esters, vegetable oils and their derivatives, and esters of glycerin. Such plasticizers are generally free of aromatic groups and halogen atoms and are expected to be biodegradable. Such plasticizers are usually C2-C 10 The alkyl group further comprises a straight or branched alkyl end group having a carbon chain length of
[0031] In one embodiment, the plasticizer is a bio-based citric acid plasticizer represented by the following formula (I): [ka] (I) (In the formula, R are independently alkyl groups, which may be the same or different; R' is H or (C1-C 10 ) an acyl group).
[0032] R is typically independently C1 to C 10 In some embodiments, R is a straight chain or branched alkyl group having a carbon chain length of C2 to C8 or C2 to C4. In some embodiments, R' is acetyl. In other embodiments, at least one R is a branched alkyl group having a carbon chain length of C5 or greater. In some embodiments, the branched alkyl group has a carbon chain length of 8 or less.
[0033] Representative citric acid plasticizers include, for example, triethyl citrate, acetyl triethyl citrate, tributyl citrate, acetyl tributyl citrate, trihexyl citrate, acetyl trihexyl citrate, trioctyl citrate, acetyl trioctyl citrate, butyryl trihexyl citrate, acetyl tris-3-methylbutyl citrate, acetyl tris-2-methylbutyl citrate, acetyl tris-2-ethylhexyl citrate, and acetyl tris-2-octyl citrate.
[0034] In another embodiment, the plasticizer comprises a polyethylene glycol backbone and an ester alkyl end group. The molecular weight of the polyethylene glycol portion is typically at least 100, 150, or 200 g / mol, and not more than 1,000 g / mol. In some embodiments, the polyethylene glycol portion has a molecular weight of not more than 900, 800, 700, or 600 g / mol. Examples include polyethylene glycol (400) di-ethylhexanoate, available under the trade name "TegMeR™ 809" from Hallstar (Chicago, IL), and tetraethylene glycol di-ethylhexanoate, available under the trade name "TegMeR™ 804" from Hallstar (Chicago, IL).
[0035] In some embodiments, the plasticizer compound typically has little or no hydroxyl groups. In some embodiments, the wt% percent of hydroxyl groups relative to the total weight of the plasticizer compound is 10, 9, 6, 7, 6, 5, 4, 3, 2, 1 wt% or less. In some embodiments, the plasticizer compound does not contain hydroxyl groups. Thus, in this embodiment, the plasticizer is not glycerol or water.
[0036] Nucleating agents may also be present in the PLA composition to accelerate the crystallization rate.Suitable nucleating agents include, for example, inorganic minerals, organic compounds, salts of organic acids and imides, particulate crystalline polymers with melting points above the processing temperature of PLA, and combinations of two or more of the foregoing.Suitable nucleating agents typically have an average particle size of at least 25 nanometers, or at least 0.1 micrometers.Combinations of two or more different nucleating agents may also be used.
[0037] Examples of useful nucleating agents include, for example, talc (hydrated magnesium silicate - H2Mg3(SiO3)4 or Mg3Si4O 10(OH)2), silica (SiO2), titania (TiO2), alumina (Al2O3), zinc oxide, saccharin sodium salt, calcium silicate, sodium benzoate, calcium titanate, aromatic sulfonate derivatives, boron nitride, copper phthalocyanine, phthalocyanine, saccharin sodium salt, isotactic polypropylene, polybutylene terephthalate, etc.
[0038] When an organic nucleating agent is present, it is typically at a concentration ranging from at least 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.15 or 0.2 wt % to about 1, 2, 3, 4 or 5 wt %, based on the total weight of the composition. The concentration may be higher when the nucleating agent is an inorganic oxide filler such as silica, alumina, zinc oxide and talc.
[0039] In one embodiment, the nucleating agent may be characterized as a salt of a phosphorus-containing aromatic organic acid, such as zinc phenylphosphonate, magnesium phenylphosphonate, disodium 4-tert-butylphenyl phosphonate, and sodium diphenylphosphinate.
[0040] One preferred nucleating agent is zinc phenylphosphonate, which has the following formula: [ka] and is available from Nissan Chemical Industries, Ltd. under the trade name "Ecopromote."
[0041] In some embodiments, inorganic fillers can be used to prevent the film layer or roll from blocking or sticking during storage and transportation. Inorganic fillers include clays or minerals, with or without surface modification. Examples include talc, diatomaceous earth, silica, mica, kaolin, titanium dioxide, perlite, and wollastonite.
[0042] Organic biomaterial fillers include various forest and agricultural products, modified or not. Examples include cellulose, wheat, starch, modified starch, chitin, chitosan, keratin, cellulosic materials from agricultural products, gluten, flour and guar gum. The term "flour" generally refers to a composition having a protein-containing fraction and a starch-containing fraction derived from one and the same plant source, where the protein-containing fraction and the starch-containing fraction are not separated from each other. Typical proteins present in flour are globulins, albumins, glutenins, secalins, prolamins, glutelins. In typical embodiments, the composition contains little or no organic biomaterial fillers, such as flours. Thus, the concentration of organic biomaterial fillers (e.g., flours) is typically less than 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 wt% of the total composition.
[0043] The compositions and films may optionally contain one or more conventional additives, such as, for example, antioxidants, stabilizers, UV absorbers, lubricants, processing aids, antistatic agents, colorants, impact resistance aids, fillers, matting agents, flame retardants (e.g., zinc borate), pigments, and the like.
[0044] When the film is a monolithic film, the thickness of the film is typically at least 10, 15, 20, or 25 micrometers (1 mil) to 500 micrometers (20 mils) thick. In some embodiments, the thickness of the film is no greater than 400, 300, 200, 150, or 50 micrometers. Films may be in the form of individual sheets, particularly at thicknesses greater than 20 mils. (E.g., thinner) films may be in the form of roll goods.
[0045] When the film is a film layer of a multi-layer film, the multi-layer film typically has the thickness described above. However, the thickness of the film layer may be less than 10 micrometers. In one embodiment, the film layer comprising the composition described herein is an outer surface layer or in other words a skin layer. A second film layer is disposed on the skin layer. The second film layer typically has a different composition from the skin layer.
[0046] In preparing the compositions described herein, the PLA, PVAc, plasticizer, nucleating agent, etc. are heated (e.g., 180-250° C.) and thoroughly mixed using any suitable means known to those of skill in the art. For example, the compositions may be mixed using a mixer (e.g., a Brabender), extruder, kneader, etc.
[0047] After mixing, the composition may be formed (e.g., cast) into a film using known film-forming techniques, taking into account the scale of the process and the equipment available. In some embodiments, the PLA composition is fed into a press and then compressed and solidified to form individual PLA film sheets. In other embodiments, the PLA composition can be extruded through a die onto a casting roll maintained at a suitable cooling temperature to form a continuous length of PLA film. In some embodiments, the casting roll temperature is preferably maintained between 80-120° C. during film extrusion to allow the PLA film to crystallize on the casting roll.
[0048] The PLA compositions and films described herein can be used in a variety of products. In some embodiments, PLA films have similar or better properties than polyvinyl chloride (PVC) films and can therefore be used in place of PVC films.
[0049] The films and compositions can have a variety of properties that are determined by the test methods described in the examples.
[0050] The films and compositions typically have a glass transition temperature ranging from about -20°C, -15°C, or -10°C to 40°C, below the Tg of both the PLA polymer and the polyvinyl acetate polymer. In some embodiments, the films and compositions have a glass transition temperature of at least -5, -4, -3, -2, -1, or 0°C. In some embodiments, the films and compositions have a glass transition temperature of less than 35°C, or 30°C, or 25°C. In some embodiments, the films and compositions have a glass transition temperature of less than 20°C, 19°C, or 18°C.
[0051] The films and compositions typically have a melting temperature T of at least about 150° C. or 155° C. to about 165° C. or 170° C. m1 Or T m2 Furthermore, the composition may have a crystallization peak temperature Tc in the range of 100°C to 120°C.
[0052] The net melting endotherm is the melting endotherm energy minus the crystallization exotherm energy (as described in more detail in the Examples below). The net melting endotherm of the composition (i.e., taken from a mini-kneader that has not been melt-pressed into a film) is determined by a second heat scan, while the net melting endotherm of the film (e.g., melt-pressed) is determined by a first heat scan. According to U.S. Pat. No. 6,005,068, a PLA film is considered non-crystalline if it exhibits a net melting endotherm of less than about 10 J / g. In preferred embodiments, such as when the composition and film contain a nucleating agent, the net melting enthalpy of the composition and film, ΔH nm2 and ΔH nm1 are greater than 10, 11, 12, 13, 14, or 15 J / g and less than 40, 39, 38, 37, 36, or 35 J / g, respectively.
[0053] In one embodiment, the film has a Tg of −10 to 30° C. and a net endotherm of melting ΔH of greater than 10 J / g and less than 40 J / g, as described above. nm1Such films are flexible at room temperature and have relatively high mechanical properties, such as modulus, when heated to high temperatures, as shown by the dynamic mechanical analysis (DMA) results in FIG. 3. In this embodiment, the film has a tensile storage modulus of at least 10 MPa, and typically less than 10,000 MPa, in the temperature range of −40° C. to 125° C. when heated at a rate of 2° C. / min (i.e., the tensile storage modulus does not drop below 10 MPa when heated at a rate of 2° C. / min to −40° C. to 125° C.). In some embodiments, the film has a tensile storage modulus, as determined by dynamic mechanical analysis, of at least 5, 6, 7, 8, 9, or 10 MPa in the temperature range of 25° C. to 80° C. when heated at a rate of 2° C. / min. In contrast, when the film has a very low net melting endotherm, as shown in FIG. 4, mechanical properties such as modulus dramatically decreased when the temperature was increased above room temperature, 23° C.
[0054] The films can be evaluated using standard tensile tests, as further described in the Examples below. The tensile strength of the film is typically at least 5 or 10 MPa, and is typically less than the tensile strength of the PLA and polyvinyl acetate polymers utilized to make the film. In some embodiments, the tensile strength is no greater than 34, 33, 32, 31, or 30 MPa. The elongation of the film typically exceeds the elongation of the PLA and polyvinyl acetate polymers utilized to make the film. In some embodiments, the elongation is at least 30, 40, or 50%. In other embodiments, the elongation is at least 100%, 150%, 200%, 250%, or 300%. In some embodiments, the elongation is no greater than 600% or 500%. The tensile modulus of the film is typically at least 50, 100, or 150 MPa. In some embodiments, the tensile modulus is at least 200, 250, or 300 MPa. In some embodiments, the tensile modulus is no greater than 750 MPa or 650 MPa.
[0055] The PLA-based films described herein are suitable for use as a backing for pressure-sensitive adhesive tapes or sheets.
[0056] The PLA-based film may be subjected to conventional surface treatments to improve adhesion with adjacent pressure-sensitive adhesive layers, including, for example, exposure to ozone, exposure to flame, exposure to high electric shock, ionizing radiation treatments, and other chemical or physical oxidation treatments.
[0057] Various pressure-sensitive adhesives can be applied to the PLA-based film, such as natural or synthetic rubber-based pressure-sensitive adhesives, acrylic pressure-sensitive adhesives, vinyl alkyl ether pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, polyamide pressure-sensitive adhesives, urethane pressure-sensitive adhesives, and styrene block copolymer pressure-sensitive adhesives. Pressure-sensitive adhesives generally have a viscosity of 3×10 at a frequency of 1 Hz, which can be measured by dynamic viscoelasticity measurement at room temperature (25° C.). 6 It has a storage modulus (E') of less than dynes / cm.
[0058] The pressure sensitive adhesives may be organic solvent based, water-based emulsion, hot melt, heat activated, as well as actinic radiation (eg, electron beam, ultraviolet) cured pressure sensitive adhesives.
[0059] The acrylic pressure sensitive adhesive can be produced by radical polymerization techniques such as solution polymerization, bulk polymerization, or emulsion polymerization. The acrylic polymer can be of any type, such as random copolymer, block copolymer, or graft polymer. The polymerization can be carried out using any of the commonly used polymerization initiators and chain transfer agents.
[0060] The acrylic pressure sensitive adhesives include polymerized units that are one or more (meth)acrylate ester monomers derived from (e.g., non-tertiary) alcohols containing from 1 to 14 carbon atoms, preferably an average of 4 to 12 carbon atoms. Examples of monomers include esters of non-tertiary alcohols such as ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 1-hexanol, 2-hexanol, 2-methyl-1-pentanol, 3-methyl-1-pentanol, 2-ethyl-1-butanol; 3,5,5-trimethyl-1-hexanol, 3-heptanol, 1-octanol, 2-octanol, isooctyl alcohol, 2-ethyl-1-hexanol, 1-decanol, 2-propylheptanol, 1-dodecanol, 1-tridecanol, 1-tetradecanol, and the like, with either acrylic or methacrylic acid.
[0061] The acrylic pressure sensitive adhesives include polymerized units that are one or more low Tg (meth)acrylate monomers, i.e., the (meth)acrylate monomers have a T of 0° C. or less when reacted to form a homopolymer. g In some embodiments, the low Tg monomer has a T of -5°C or lower, or -10°C or lower. g The Tg of these homopolymers is often -80°C or higher, -70°C or higher, -60°C or higher, or -50°C or higher.
[0062] The low Tg monomer may have the formula:
[0063] H2C=CR 1 C(O)OR 8 (In the formula, R 1 is H or methyl, R 8 is an alkyl having 1 to 22 carbons, or a heteroalkyl having 2 to 20 carbons and 1 to 6 heteroatoms selected from oxygen or sulfur. The alkyl or heteroalkyl group can be linear, branched, cyclic, or a combination thereof.
[0064] Representative low Tg monomers include, for example, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, n-pentyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-methylbutyl acrylate, 2-ethylhexyl acrylate, 4-methyl-2-pentyl acrylate, n-octyl acrylate, 2-octyl acrylate, isooctyl acrylate, isononyl acrylate, decyl acrylate, isodecyl acrylate, lauryl acrylate, isotridecyl acrylate, octadecyl acrylate, and dodecyl acrylate.
[0065] Low Tg heteroalkyl acrylate monomers include, but are not limited to, 2-methoxyethyl acrylate and 2-ethoxyethyl acrylate.
[0066] In a typical embodiment, the acrylic pressure sensitive adhesive includes polymerized units that are at least one low Tg monomer having an alkyl group containing 6 to 20 carbon atoms. In some embodiments, the low Tg monomer has an alkyl group containing 7 or 8 carbon atoms. Representative monomers include, but are not limited to, esters of (meth)acrylic acid and alcohols derived from renewable resources, such as 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, and 2-octyl (meth)acrylate.
[0067] The acrylic pressure sensitive adhesives typically include at least 50, 55, 60, 65, 70, 75, 80, 85, 90 or more wt % of polymerized units that are monofunctional alkyl (meth)acrylate monomers having a Tg less than 0° C., based on the total weight of polymerized units (i.e., excluding inorganic fillers or other additives).
[0068] The acrylic pressure sensitive adhesive may further comprise at least one high Tg monomer, i.e., the (meth)acrylate monomer has a Tg greater than 0° C. when reacted to form a homopolymer. High Tg monomers more typically have a Tg greater than 5° C., 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., or 40° C. High Tg monofunctional alkyl (meth)acrylate monomers include, for example, t-butyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, stearyl methacrylate, phenyl methacrylate, cyclohexyl methacrylate, isobornyl acrylate, isobornyl methacrylate, norbornyl (meth)acrylate, benzyl methacrylate, 3,3,5 trimethylcyclohexyl acrylate, cyclohexyl acrylate, N-octylacrylamide, and propyl methacrylate, or combinations.
[0069] The acrylic pressure sensitive adhesive may further comprise polymerized units of a polar monomer. Exemplary polar monomers include, for example, acid functional monomers (e.g., acrylic acid), hydroxyl functional (meth)acrylate monomers, nitrogen-containing monomers (e.g., acrylamide), and combinations thereof. In some embodiments, the acrylic pressure sensitive adhesive comprises at least 0.5, 1, 2, or 3 wt %, and typically no more than 10 wt %, polymerized units of a polar monomer, such as acrylamide.
[0070] The pressure-sensitive adhesive may further include one or more suitable additives as required. Examples of additives are crosslinkers (e.g., multifunctional (meth)acrylate crosslinkers, epoxy crosslinkers, isocyanate crosslinkers, melamine crosslinkers, aziridine crosslinkers, etc.), tackifiers (e.g., phenol-modified terpenes and rosin esters such as glycerol esters of rosin and pentaerythritol esters of rosin, and C5 and C9 hydrocarbon tackifiers), thickeners, plasticizers, fillers, antioxidants, UV absorbers, antistatic agents, surfactants, leveling agents, colorants, flame retardants, and silane coupling agents.
[0071] The pressure sensitive adhesive layer can be disposed on the film by a variety of common coating methods, including roller coating, flow coating, dip coating, spin coating, spray coating, knife coating, die coating, and printing.
[0072] The adhesive may be applied directly to the PLA films described herein or may be transfer coated using a release liner.
[0073] The following examples are provided to illustrate further features and embodiments of the present invention. All parts are by weight unless otherwise specified.
[0074] material PLAs, Ingeo 4032D ("4032") and Ingeo 4060D ("4060"), were purchased from Natureworks, LLC. Polyvinyl acetate "PVAc" was obtained from Wacker under the trade name "Vinnapas™ UW4FS". Ecopromote nucleating agent was obtained from Nissan Chemical Industrials (Japan).
[0075] Commercially available plasticizers used include Citroflex A4 (Vertellus Performance Materials), PEG 400 di-ethylhexonate and tetraethylene glycol di-ethylhexonate ester plasticizers available from Hallstar under the tradenames "TegMer 809" and "TegMer 804", respectively, and a polyester plasticizer (polymeric adipate with a molecular weight of 3200) available from Eastman under the tradename "Admex 6995".
[0076] Sample preparation - Melt mixing DSM Xplore(trademark) 15cm 3 Samples were prepared by mixing PLA, PVAc, plasticizer and nucleating agent in a twin screw mini-kneader at 100 RPM and 200°C for 10 minutes, then opening the valve of the mixing chamber to collect the sample. The kneaded samples were subjected to aging tests at 80°C and DSC characterization, and were melt pressed into films for tensile testing.
[0077] Aging test The kneaded samples (0.2 grams) were placed in scintillation vials, sealed to prevent the plasticizer from evaporating during the aging test, and aged in an oven at 80° C. for 24 hours. The sample surfaces were then inspected to see if there was any plasticizer migration after aging at 80° C. Samples with wet or oily surfaces were considered to have failed, and samples with dry surfaces were considered to have passed.
[0078] DSC - Differential Scanning Calorimetry The glass transition temperature, crystallization temperature, melting temperature, etc. of each sample were measured according to ASTM D3418-12 using a TA Instruments Differential Scanning Calorimeter unless otherwise specified. Each sample (4-8 mg) was heated from -60 to 200°C at 10°C / min in the first heating scan, held for 2 minutes to erase the thermal history, then cooled to -60°C at 10°C / min in the first cooling scan, and heated to 200°C at 10°C / min in the second heating scan. The second heating scan was used to determine the Tg of the compositions and films. Various parameters were obtained from the DSC as defined below: T g - ASTM D3418-12 T mg This refers to the intermediate temperature of the second heating scan. T c - ASTM D3418-12 T pc This refers to the crystallization peak temperature of the first cooling scan, which is described as "crystallization peak temperature of the first cooling scan." T m1 and T m2 -ASTM D3418-12, T pm The melting peak temperatures of the first and second heating scans are indicated as
[0079] The ability of a composition to crystallize is determined by the net melting endotherm ΔH associated with the crystalline material formed during the second cooling scan, calculated using the following formula: nm2 was determined by calculating
[0080] ΔH nm2 = ΔH m2 -ΔH cc2 (In the formula, ΔH m2 is the mass normalized enthalpy of the melting endotherm of the second heating scan, and ΔH cc2 is the mass-normalized enthalpy of the crystallization exotherm of the second heating scan (as described in Section 11 of ASTM D3418-12). For compositions containing a nucleating agent, ΔH cc2 was not detected, so ΔHnm2 = ΔH m2 It was.
[0081] Net heat of melting absorption ΔH nm1 is related to the degree of crystallinity in films (prepared, for example, by melt pressing). nm1 was calculated using the following formula: ΔH nm1 = ΔH m1 -ΔH cc1 (In the formula, ΔH m1 is the mass-normalized enthalpy of the melting endotherm of the first heating scan, and ΔH cc1 is the mass-normalized enthalpy of crystallization exotherm for the first heating scan (as described in Section 11 of ASTM D3418-12). For films containing nucleating agents, ΔH cc1 was not detected, so ΔH nm1= ΔH m1 It was.
[0082] The absolute value of the enthalpy associated with the amount of heat released and absorbed (i.e., ΔH m1、 ΔH m2 , ΔH cc1、 and ΔH cc2 was used in the calculation.
[0083] Melt Press The compounded samples were placed between two Teflon sheets with a 10 mil thick spacer between them. The Teflon sheets were sandwiched between two metal sheets. The metal sheets with the sample between them were placed between the platens of a hydraulic press (available from Carver) and the platens were heated to 340° F. Each sample was preheated with no pressure for 8 minutes and then pressed at 300 pounds per square inch for 5 minutes. The metal plates were then removed from the Carver press and allowed to cool. The melt pressed films were subjected to DSC characterization and tensile testing.
[0084] Tensile Test Melt pressed samples were cut into 0.5 inch wide strips. Tensile testing was performed at room temperature using an Instron 4501 tensile tester. The initial grip distance was 1 inch and the pull rate was 1 inch / min or 100% strain / min. Test results were reported as the average of 3-5 sample replicates. Tensile strength (nominal), modulus and percent elongation at break were determined as described in ASTM D882-10, 11.3 and 11.5.
[0085] Dynamic Mechanical Analysis (DMA) Dynamic Mechanical Analysis (DMA) was performed to evaluate the physical properties of the films as a function of temperature using a film tensile fixture available from TA Instruments as "DMA Q800." Samples were heated from a temperature of -40°C to 140°C at a rate of 2°C / min, a frequency of 1 rad / sec, and a tensile strain of 0.1%.
[0086] 180° peel strength test method A 0.5 inch wide by 6 inch long strip of adhesive was laminated onto a stainless steel panel using a roller. Dwell time in a CTH (constant temperature and humidity) chamber conditioned at 23°C / 50% RH was 10 minutes. Peel strength measurements were made at 12 in / min (approximately 30 cm / min) using a 180° peel mode. Data was recorded as the average of six measurements.
[0087] The wt% of each of the components used in the compositions of the examples and controls (designated "C") are shown in Table 1. For example, Example 8 contains 70 wt% PLA4032, 15 wt% PVAc, and 15 wt% Citroflex A4, based on the total weight of the polylactic acid polymer, polyvinyl acetate polymer, and plasticizer. Example 8 further contained 0.2 wt% Ecopromote, based on the total weight of the composition. The Tg and aging results of the compositions are also reported in Table 1 as follows: [Table 1]
[0088] As shown in Table 1, Comparative Examples C1, C4, and C5 passed the aging test, while Comparative Examples C2, C3, C6, and C7 failed the aging test. The Tg of the sample can be reduced to 25° C. (as shown by Comparative Example C5) but still pass the aging test above 25° C. (as shown by Comparative Examples C6 and C7). If the composition contained PLA, a plasticizer, and PVAc, the Tg can be reduced to below 25° C. and pass the aging test.
[0089] The respective wt% of the components used in the compositions of the examples and controls (designated "C") and the DSC results are shown in Table 2 below: [Table 2]
[0090] A representative DSC profile of the composition of Example 12 is shown in Figure 1. The DSC profile shows a sharp crystallization peak exotherm during cooling. As shown in Figure 2, the composition of Example 16 does not show any crystallization during cooling.
[0091] The respective wt% of the components used in the compositions to prepare the melt pressed film examples and the control example (designated "C"), as well as the DSC and tensile test results of these films, are shown in Table 3 below: [Table 3]
[0092] The Tg of the films in Table 3, if measured by DSC, would also be the same as the compositions in Table 2. Examples 12 and 16 were tested according to the dynamic mechanical properties measurements described above. The results of Example 12 are shown in Figure 3 and the results of Example 16 are shown in Figure 4.
[0093] Example 22 (EX-22) A strip of the film of Example 17 containing 44.8 wt% PLA4032, 35 wt% PVAc, 20 wt% Citroflex A4, and 0.2 wt% Ecopromote was overlaminated at room temperature with a 1 mil thick polyacrylate pressure sensitive adhesive derived from 97 wt% isooctyl acrylate and 3 wt% acrylamide, with a weight average molecular weight of about 1,000,000 g / mol. The 180° peel strength was then measured to be 25 oz / in. During the peel test, it was observed that the polyacrylate adhesive bonded well to the PLA-based backing and the adhesive peeled cleanly from the stainless steel panel.
Claims
1. a semicrystalline polylactic acid polymer; a polyvinyl acetate polymer having a Tg of at least 25° C.; a plasticizer comprising a polyfunctional ester or a polyfunctional ether; an optional amorphous polylactic acid polymer; The composition includes the polyvinyl acetate polymer is present in an amount ranging from 10 to 50 wt %, based on the total amount of the polylactic acid polymer, the polyvinyl acetate polymer, and the plasticizer; the plasticizer is present in an amount ranging from 5 to 35 wt %, based on the total amount of polylactic acid polymer, polyvinyl acetate polymer, and plasticizer; The composition does not exhibit plasticizer migration when aged at 80° C. for 24 hours. film.
2. The plasticizer comprises an alkyl or aliphatic ester group or an ether group, and 2 ~C 10 2. The film of claim 1, further comprising a linear or branched alkyl end group having a carbon chain length of:
3. 10. The film of claim 1, wherein the polyvinyl acetate polymer has a molecular weight in the range of 75,000 g / mol to 500,000 g / mol.
4. When the polyvinyl acetate polymer is dissolved in a 10% ethyl acetate solution at 20° C., the polyvinyl acetate polymer has a viscosity of 10 to 50 mPa * 2. The film of claim 1 having a viscosity in the range of s.
5. The film of any one of claims 1 to 4, wherein the polylactic acid polymer is present in an amount ranging from 40 to 80 wt %, based on the total amount of polylactic acid polymer, polyvinyl acetate polymer and plasticizer.
6. The film of any one of claims 1 to 5, wherein the polylactic acid polymer has a melt flow rate of 25 g / min or less at 210°C.
7. The film of any one of claims 1 to 6, wherein the polylactic acid polymer has a Tg in the range of 50 to 65°C.
8. The film of any one of claims 1 to 7, wherein the film has a tensile modulus of from 50 MPa to 700 MPa.
9. The film according to any one of claims 1 to 8, wherein the film has a tensile storage modulus, as determined by dynamic viscoelasticity measurement, of at least 10 MPa in the temperature range of -40°C to 125°C when heated at a rate of 2°C / min.
10. The film according to any one of claims 1 to 9, wherein the film has a tensile storage modulus, as determined by dynamic viscoelasticity measurement, of at least 5 MPa in a temperature range of 25°C to 80°C when heated at a rate of 2°C / min.
11. The film of any one of claims 1 to 10, further comprising an antioxidant, a stabilizer, a UV absorber, a colorant, a filler, or a pigment.
12. The film of any one of claims 1 to 11 having a tensile elongation of from 50% to 600%.
13. 13. The film of claim 12 having a tensile elongation of at least 150%.
14. The film of any one of claims 1 to 13 having a tensile modulus of at least 200 MPa.
15. An article comprising the film of any one of claims 1 to 14 and a layer of pressure sensitive adhesive disposed on the film.
Citation Information
Patent Citations
The lactide biodegradable thermoplastic plastic
JP1992504731A
Melt-stable lactide polymer films and methods for their production
JP1995504227A
Polymer composition having biodegradability and shrink film
JP1997151310A
Biodegradable resin composition
JP2011006615A
Heat-shrinkable laminated polylactic acid film, molding using the film, heat-shrinkable label, and container which uses the molding or to which the label is attached
JP2011136428A