Anticorrosive coating material, anticorrosive coating layer, and anticorrosive method for concrete structures
A (meth)acrylate monomer and hydrophobic silica-based coating addresses the durability and application challenges of sulfuric acid-resistant concrete coatings, offering a single-layer solution with enhanced resistance and ease of use.
Patent Information
- Application Number
- JP2022559132
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-30
- Filing Date
- 2021-10-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-10-25
AI Technical Summary
Existing methods for repairing and protecting concrete structures from sulfuric acid corrosion, such as those found in sewers and hot spring areas, are cumbersome and lack durability, requiring multiple layers of resin application and prolonged curing times.
A novel anticorrosion coating material containing (meth)acrylate monomer and hydrophobic silica with a specific particle size range, which forms a thick, thixotropic coating that can be applied in a single layer, enhancing sulfuric acid resistance and durability.
The coating material allows for easy application and rapid curing, providing excellent sulfuric acid resistance and durability, extending the service life of concrete structures in corrosive environments.
Smart Images

Figure 0007588654000001 
Figure 0007588654000002 
Figure 0007588654000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an anticorrosive coating material, an anticorrosive coating layer, and a method for preventing corrosion of a concrete structure. [Background technology]
[0002] In sewers and hot spring areas, hydrogen sulfide is generated by the influence of microorganisms and volcanic gases, and when water is present, sulfuric acid is produced. In such places, corrosion of concrete structures becomes a problem. When hardened cement such as concrete comes into contact with sulfuric acid, it reacts with the calcium hydroxide in the concrete to produce gypsum dihydrate, and further, ettringite is produced, causing the concrete to expand and deteriorate. As a method for repairing deteriorated parts caused by sulfuric acid, a method is carried out in which the deteriorated parts are removed by a water jet, the cross section is repaired or the unevenness is adjusted, and then a resin lining is applied. As repair materials used for this, a material in which a polymer is mixed with granulated blast furnace slag (Patent Document 1), a material made of alumina cement (Patent Documents 2 and 3), and a cement mortar in which a large amount of fine powder such as granulated blast furnace slag or silica fume is mixed (Patent Document 4) are used. In addition, a material using alumina cement and fine powder of blast furnace slag, in which alumina cement particles of 5 μm or less are 25% by weight or less and which contains a lithium salt (Patent Document 5), and a material containing 0.5 to 4 parts by mass of a water-soluble organic compound having an alkali metal salt of sulfonic acid as a substituent relative to 100 parts by mass of cement (Patent Document 6) have been proposed.
[0003] In addition, known resin components used for the resin lining include epoxy resin, bisphenol-based unsaturated polyester resin, HET acid-based unsaturated polyester resin, bisphenol-based vinyl ester resin, novolac-based vinyl ester resin, brominated bisphenol-based vinyl ester resin, silicone resin, polyurethane resin, polyurea resin, acrylic resin, etc. (Non-Patent Document 1).
[0004] In the method of repairing concrete with cement-based materials and then lining it with resin, it is common to apply multiple layers of resin lining, such as applying a primer, an intermediate coat, and a top coat. Depending on the type of resin, there are cases where the intermediate coat and top coat are applied twice, and many processes are required to finally form the resin layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 03-290348 [Patent Document 2] JP 2003-89565 A [Patent Document 3] JP 2004-292245 A [Patent Document 4] JP 2000-128618 A [Patent Document 5] JP 2002-293603 A [Patent Document 6] JP 2003-292362 A [Non-patent literature]
[0006] [Non-Patent Document 1] Japan Sewage Works Agency (ed.), "Manual for Corrosion Prevention and Corrosion Prevention Technology for Sewage Concrete Structures," published by the Sewerage Works Management Center, pp. 68-69, December 2017 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an anticorrosive coating material which is easy to repair concrete structures deteriorated by sulfuric acid or the like and which has excellent durability, an anticorrosive coating layer using the anticorrosive coating material, and a method for preventing corrosion of concrete structures using the anticorrosive coating material. [Means for solving the problem]
[0008] The present inventors have conducted intensive research and found that the above-mentioned problems can be solved by a corrosion-resistant coating material containing a (meth)acrylate monomer and hydrophobic silica having a predetermined average particle size, and have thus completed the present invention. [1] A composition comprising a (meth)acrylate monomer and a hydrophobic silica, The anticorrosive coating material, wherein the hydrophobic silica has an average particle size of 1 to 100 nm. [2] The corrosion-resistant coating material according to the above [1], wherein the hydrophobic silica is at least one of silica hydrophobized with an organosilane represented by the following general formula (1) and silica hydrophobized with an organosilane represented by the following general formula (2): R 1 x SiCl y H 4-x-y (1) In general formula (1), R 1 represents an alkyl group, x represents an integer of 1 to 3, y represents an integer of 0 to 3, and x+y≦4. (R 2 z H 3-z Si)2NR 3 (2) In general formula (2), R 2 represents hydrogen, an alkyl group, an alkenyl group, or a halogenated alkyl group; R 3 represents hydrogen, an alkyl group, or an alkali metal element; and z represents an integer of 1 to 3. [3] The hydrophobic silica includes silica hydrophobized with a first organosilane represented by the general formula (1) and silica hydrophobized with a second organosilane represented by the general formula (1) different from the first organosilane; In the general formula (1), R 1 is an alkyl group represented by the following general formula (3), and R of the second organosilane is 1 3. The corrosion-resistant coating material according to claim 2, wherein: C s H 2s+1 (3) In the general formula (3), s represents an integer of 1 to 5. C t H 2t+1 (4) In the general formula (4), t represents an integer of 6 to 12. [4] The corrosion-protective coating material according to any one of the above [1] to [3], wherein the (meth)acrylate monomer contains a di(meth)acrylate having a bisphenol A skeleton. [5] The corrosion-resistant coating material according to the above [4], wherein the di(meth)acrylate monomer having a bisphenol A skeleton is a di(meth)acrylate having a bisphenol A skeleton represented by the following general formula (5): [ka] In general formula (5), R 4 and R 4 ' represents a hydrogen atom or a methyl group, and R 5 and R 5 "1'" represents an alkylene group which may have a substituent, and m and n each represent an integer of 1 to 20. [6] The anticorrosive coating material according to any one of the above [1] to [5], which is a two-component type comprising a first anticorrosive coating material containing a polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica, and a second anticorrosive coating material containing a decomposition accelerator for accelerating decomposition of the polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica. [7] The corrosion-protective coating material according to any one of the above [1] to [6], which has a viscosity at 25°C of 1700 to 15000 mPa·s and a thixotropy index at 25°C of 3.0 or more. [8] The corrosion-protective coating material according to any one of the above [1] to [7], having a viscosity in the range of 0 to 25°C of 1700 to 15000 mPa s and a thixotropy index in the range of 0 to 25°C of 3.0 or more. [9] A corrosion-resistant coating layer comprising a base adjustment layer made of a hardened alumina cement composition containing alumina cement, a pozzolanic substance, and an aggregate, and a corrosion-resistant coating layer made of a hardened alumina cement composition according to any one of the above [1] to [8] on the base adjustment layer.
[10] The corrosion-protective coating layer according to the above item [9], further comprising a primer formed of a cured product of a primer composition containing a (meth)acrylate monomer, disposed between the surface adjustment layer and the corrosion-protective coating layer.
[11] The corrosion-protective coating layer according to the above
[10] , wherein the (meth)acrylate monomer contained in the primer composition contains a di(meth)acrylate having a bisphenol A skeleton.
[12] The corrosion-protective coating layer according to the above
[11] , wherein the di(meth)acrylate having a bisphenol A skeleton contained in the primer composition is a di(meth)acrylate having a bisphenol A skeleton represented by the following general formula (5): [ka] In general formula (5), R 4 and R 4 ' represents a hydrogen atom or a methyl group, and R 5 and R 5 "1'" represents an alkylene group which may have a substituent, and m and n each represent an integer of 1 to 20.
[13] The corrosion-resistant coating layer according to any one of the above
[10] to
[12] , wherein the porosity of the surface adjustment layer is 5 to 40 volume %, and in a region of the surface adjustment layer adjacent to the primer, the voids of the surface adjustment layer are filled with a cured product of the primer composition.
[14] A method for protecting a concrete structure from corrosion, comprising the steps of assembling a formwork, pouring an alumina cement composition containing alumina cement, a pozzolanic substance and an aggregate into the formwork to form a base adjustment layer, removing the formwork, and applying a corrosion-resistant coating material described in any one of [1] to [8] above to form a corrosion-resistant coating material layer on the base adjustment layer.
[15] The method for protecting a concrete structure according to the above item
[14] , further comprising the step of applying a primer composition containing a (meth)acrylate monomer to the base adjustment layer to form a primer, wherein the corrosion-protective coating material is applied to the primer. Effect of the Invention
[0009] According to the present invention, it is possible to provide an anticorrosive coating material which is easy to repair concrete structures deteriorated by sulfuric acid or the like and which has excellent durability, an anticorrosive coating layer using the anticorrosive coating material, and a method for protecting concrete structures using the anticorrosive coating material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Anti-corrosion coating material] The anticorrosive coating material of the present invention contains a (meth)acrylate monomer and hydrophobic silica having an average particle size of 1 to 100 nm. The hydrophobic silica is silica whose surface has been hydrophobized using a treatment agent. By hydrophobizing the surface of the silica, it becomes easy to disperse the silica in the anticorrosive coating material, and this makes it possible to enhance the thickening and thixotropic effects of the silica. As a result, it becomes easy to apply the anticorrosive coating material thick. The anticorrosive coating material of the present invention can be applied to a thickness of 400 μm or more by, for example, applying it once using a roller. By using a (meth)acrylate monomer in the anticorrosive coating material, it is possible to improve the sulfuric acid resistance and durability of the anticorrosive coating material. In addition, it also becomes easy to form a thick film of the anticorrosive coating material.
[0011] (Hydrophobic Silica) The average particle size of the hydrophobic silica in the anticorrosive coating material of the present invention is 1 to 100 nm. If the average particle size of the hydrophobic silica is less than 1 nm, it may be difficult to disperse the hydrophobic silica in the anticorrosive coating material. If the average particle size of the hydrophobic silica is greater than 100 nm, the surface area of the hydrophobic silica is reduced, so that the thickening effect and thixotropy imparting effect of the hydrophobic silica are weakened, and it may be difficult to apply a low-viscosity anticorrosive coating material thickly. This makes it more time-consuming to repair a deteriorated concrete structure. From this viewpoint, the average particle size of the hydrophobic silica is preferably 2 to 80 nm, more preferably 3 to 60 nm, and even more preferably 5 to 50 nm. The average particle size of hydrophobic silica can be determined, for example, by measuring the particle size distribution of hydrophobic silica using a laser diffraction scattering particle size distribution analyzer (LS-13 320) manufactured by Beckman Coulter, Inc., and determining the particle size at which the cumulative frequency is 50% by volume as the average particle size of hydrophobic silica, or by observing with a transmission electron microscope, directly counting the particle size and number of particles, and determining the particle size at which the cumulative frequency is 50% by number as the average particle size of hydrophobic silica.
[0012] The hydrophobic silica of the anticorrosive coating material of the present invention is preferably at least one of silica hydrophobized with an organosilane represented by the following general formula (1) and silica hydrophobized with an organosilane represented by the following general formula (2). This further strengthens the thickening effect and thixotropy imparting effect of the hydrophobic silica, making it easier to apply the anticorrosive coating material thicker. As a result, repair of concrete structures becomes easier. It is considered that the silanol groups present on the surface of the hydrophobic silica interact with the silanol groups present on the surface of other hydrophobic silica through hydrogen bonds, and the hydrophobic silica forms a three-dimensional network structure, which results in the thickening of the anticorrosive coating material and an increase in thixotropy. It is considered that the hydrophobic silica can be sufficiently dispersed in the anticorrosive coating material by hydrophobizing the silica with the organosilane represented by the following general formula (1) and the organosilane represented by the following general formula (2), and the sufficiently dispersed hydrophobic silica forms a three-dimensional network structure, which strengthens the thickening effect and thixotropy imparting effect of the hydrophobic silica.
[0013] R 1 x SiCl y H 4-x-y (1) In general formula (1), R 1 represents an alkyl group, x represents an integer of 1 to 3, y represents an integer of 0 to 3, and x+y≦4. (R 2 z H 3-z Si)2NR 3 (2) In general formula (2), R 2 represents hydrogen, an alkyl group, an alkenyl group, or a halogenated alkyl group; R 3 represents hydrogen, an alkyl group, or an alkali metal element; and z represents an integer of 1 to 3.
[0014] When the hydrophobic silica is silica hydrophobized with an organosilane represented by the above general formula (1), from the viewpoint of imparting viscosity and thixotropy to the anticorrosive coating material, which facilitates thick application of the anticorrosive coating material, R 1The number of carbon atoms in the alkyl group of R is preferably 1 to 12, more preferably 1 to 10, and further preferably 1 to 8. When the hydrophobic silica is silica hydrophobized with an organosilane represented by the above general formula (2), from the viewpoint of imparting to the anticorrosive coating material viscosity and thixotropy that facilitate thick application of the anticorrosive coating material, 2 R is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, an alkenyl group, or a halogenated alkyl group having 1 to 3 carbon atoms, more preferably a hydrogen atom, or an alkyl group having 1 to 3 carbon atoms, and further preferably a hydrogen atom or a methyl group. 3 is preferably hydrogen, an alkyl group having 1 to 3 carbon atoms, or an alkali metal element, more preferably hydrogen or an alkyl group having 1 to 3 carbon atoms, and even more preferably hydrogen.
[0015] Although the hydrophobic silica can be used alone, it is preferable to combine two or more kinds of hydrophobic silica to impart viscosity and thixotropy to the anticorrosion coating material, which facilitates thick application of the anticorrosion coating material having a low viscosity. In this case, it is preferable that the hydrophobic silica contains silica hydrophobized with a first organosilane represented by the above general formula (1) and silica hydrophobized with a second organosilane different from the first organosilane, which is represented by the above general formula (1). In the above general formula (1), R 1 is an alkyl group represented by the following general formula (3), and R of the second organosilane is 1 is an alkyl group represented by the following general formula (4). C s H 2s+1 (3) In the general formula (3), s represents an integer of 1 to 5. C t H 2t+1 (4) In the general formula (4), t represents an integer of 6 to 12.
[0016] From the viewpoint of imparting to the anticorrosion coating material viscosity and thixotropy that facilitate thick application of the anticorrosion coating material, preferably, in general formula (3), s is an integer of 1 to 3, and in general formula (4), t is an integer of 7 to 10, and more preferably, in general formula (3), s is an integer of 1 to 2, and in general formula (4), t is an integer of 8 to 9.
[0017] The mass ratio of the silica hydrophobized by the first organosilane and the silica hydrophobized by the second organosilane is not particularly limited as long as it can impart viscosity and thixotropy to the anticorrosive coating material, which facilitates thick application of the anticorrosive coating material. The mass ratio of the silica hydrophobized by the first organosilane and the silica hydrophobized by the second organosilane is, for example, 5:95 to 95:5, preferably 30:70 to 90:10, and more preferably 50:50 to 85:15.
[0018] From the viewpoint of imparting viscosity and thixotropy to the anticorrosion coating material that facilitates thick application of the anticorrosion coating material, the content of hydrophobic silica in the anticorrosion coating material is preferably 0.5 to 20 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 2 to 7 parts by mass, relative to 100 parts by mass of the (meth)acrylate monomer.
[0019] ((Meth)acrylate Monomer) The (meth)acrylate monomer of the corrosion-resistant coating material of the present invention is preferably a di(meth)acrylate having a bisphenol A skeleton. The di(meth)acrylate having a bisphenol A skeleton is preferably a di(meth)acrylate having a bisphenol A skeleton represented by the following general formula (5) (hereinafter, sometimes referred to as a (meth)acrylate monomer (A)). This can further improve the sulfuric acid resistance and durability of the corrosion-resistant coating material. [ka] In general formula (5), R 4 and R 4' represents a hydrogen atom or a methyl group, and R 5 and R 5 R′ represents an alkylene group which may have a substituent, and m and n represent integers of 1 to 20. 4 and R 4 ' may be the same or different. 5 and R 5 ' may be the same or different.
[0020] From the viewpoint of further improving the sulfuric acid resistance and durability of the corrosion protection coating material, 5 and R 5 is preferably an alkylene group having 1 to 12 carbon atoms which may have a substituent, more preferably an alkylene group having 2 to 4 carbon atoms which may have a substituent, even more preferably an n-propylene group having an ethylene group and a 2-hydroxyl group (-CHCH(OH)CH-), preferably m+n=2 to 10, more preferably m+n=2 to 4.
[0021] Examples of the (meth)acrylate monomer (A) include bisphenol A type EO2 modified di(meth)acrylate, bisphenol A type EO (ethylene oxide) 4 modified di(meth)acrylate, bisphenol A type EO10 modified di(meth)acrylate, bisphenol A type PO modified di(meth)acrylate, bisphenol A diglycidyl ether (meth)acrylic acid adduct, etc. These (meth)acrylate monomers (A) can be used alone or in combination of two or more.
[0022] Examples of commercially available (meth)acrylate monomers (A) include Miramer M-241 (manufactured by Miwon Specialty Chemical Co., Ltd.), Miramer M-2101 (manufactured by Miwon Specialty Chemical Co., Ltd.), Miramer PE210 (manufactured by Miwon Specialty Chemical Co., Ltd.), NK Ester BPE-100 (manufactured by Shin-Nakamura Chemical Co., Ltd.), NK Ester BPE-200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), NK Ester BPE-500 (manufactured by Shin-Nakamura Chemical Co., Ltd.), NK Ester BPE-1300 (manufactured by Shin-Nakamura Chemical Co., Ltd.), Light Ester BP-2EMBR-MA (Kyoeisha Chemical Co., Ltd.), Fancryl FA-321M (manufactured by Hitachi Chemical Co., Ltd.), and Fancryl FA-324A (manufactured by Hitachi Chemical Co., Ltd.).
[0023] The corrosion-resistant coating material of the present invention preferably contains, as the (meth)acrylate monomer, a (meth)acrylate having a dicyclopentenyl skeleton (hereinafter, sometimes referred to as (meth)acrylate monomer (B)) in addition to the (meth)acrylate monomer (A). The (meth)acrylate having a dicyclopentenyl skeleton is preferably a dicyclopentenyloxyalkylene (meth)acrylate represented by the following general formula (6). This can further improve the sulfuric acid resistance and durability of the corrosion-resistant coating material. In addition, the (meth)acrylate monomer (B) also has an effect as a reactive diluent. [ka] In general formula (6), R 6 represents hydrogen or a methyl group, R 7 represents an alkylene group, and p represents an integer of 1 to 20.
[0024] From the viewpoint of sulfuric acid resistance and durability of the corrosion protection coating material, R 6 is preferably a methyl group. 7is preferably an alkylene group having 1 to 12 carbon atoms, more preferably an alkylene group having 1 to 4 carbon atoms, and even more preferably an ethylene group; p is preferably an integer of 1 to 3, and more preferably 1.
[0025] Examples of the (meth)acrylate monomer (B) include dicyclopentenyloxyethyl (meth)acrylate, dicyclopentenyloxydiethylene glycol (meth)acrylate, dicyclopentenyloxytriethylene glycol (meth)acrylate, and dicyclopentenyloxypropylene glycol (meth)acrylate. These (meth)acrylate monomers (B) can be used alone or in combination of two or more. Among these, dicyclopentenyloxyethyl (meth)acrylate is preferred from the viewpoint of sulfuric acid resistance and durability of the anticorrosive coating material.
[0026] The corrosion-resistant coating material of the present invention preferably contains, as the (meth)acrylate monomer, a hydroxyalkyl (meth)acrylate (hereinafter, sometimes referred to as a (meth)acrylate monomer (C)) in addition to the (meth)acrylate monomer (A) and the (meth)acrylate monomer (B), which can further improve the sulfuric acid resistance and durability of the corrosion-resistant coating material.
[0027] Examples of the (meth)acrylate monomer (C) include 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and glycerol mono(meth)acrylate. These (meth)acrylate monomers (C) can be used alone or in combination of two or more. Among these, from the viewpoint of adhesion of the anticorrosive coating material, 2-hydroxyalkyl (meth)acrylate represented by the following general formula (7) is preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.
[0028] [ka] In general formula (7), R 8 represents hydrogen or a methyl group, R 9 represents hydrogen or an alkyl group.
[0029] From the viewpoint of adhesion of anticorrosive coating material, R 8 is preferably a methyl group, R 9 is preferably hydrogen or an alkyl group having 1 to 12 carbon atoms, more preferably hydrogen or an alkyl group having 1 to 5 carbon atoms, and even more preferably hydrogen.
[0030] From the viewpoint of sulfuric acid resistance and durability of the corrosion-resistant coating material, the content of the (meth)acrylate monomer (A) in the corrosion-resistant coating material is preferably 20 to 80 parts by mass, more preferably 40 to 70 parts by mass, based on 100 parts by mass of the total of the (meth)acrylate monomer (A), the (meth)acrylate monomer (B), and the (meth)acrylate monomer (C). On the other hand, from the viewpoint of sulfuric acid resistance and durability of the corrosion-resistant coating material, the content of the (meth)acrylate monomer (B) in the corrosion-resistant coating material is preferably 10 to 50 parts by mass, more preferably 20 to 40 parts by mass, based on 100 parts by mass of the total of the (meth)acrylate monomer (A), the (meth)acrylate monomer (B), and the (meth)acrylate monomer (C). In addition, from the viewpoint of the sulfuric acid resistance and durability of the corrosion-protective coating material, the content of the (meth)acrylate monomer (C) in the corrosion-protective coating material is preferably 5 to 35 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the total of the (meth)acrylate monomer (A), the (meth)acrylate monomer (B), and the (meth)acrylate monomer (C).
[0031] The (meth)acrylate monomer of the corrosion-protective coating material of the present invention may contain a (meth)acrylate monomer other than the (meth)acrylate monomer (A), the (meth)acrylate monomer (B), and the (meth)acrylate monomer (C) as long as the effects of the present invention are not impaired. From the viewpoint of sulfuric acid resistance and durability of the corrosion-protective coating material, the total content of the (meth)acrylate monomer (A), the (meth)acrylate monomer (B), and the (meth)acrylate monomer (C) in the (meth)acrylate monomer of the corrosion-protective coating material is preferably 80 to 100 mass%, more preferably 90 to 100 mass%, and even more preferably 95 to 100 mass%.
[0032] (Polymerization initiator) The anticorrosive coating material of the present invention preferably contains a polymerization initiator to promote the curing of the (meth)acrylate monomer. The polymerization initiator generates free radicals to initiate the polymerization of the (meth)acrylate monomer. Examples of the polymerization initiator include the following organic peroxides.
[0033] (1) Ketone peroxides: methyl ethyl ketone peroxide, cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, methylcyclohexanone peroxide, methylacetoacetate peroxide, acetylacetone peroxide, and the like. (2) Peroxyketals: 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)octane, n-butyl-4,4-bis(tert-butylperoxy)valerate, 2,2-bis(tert-butylperoxy)butane, and the like. (3) Hydroperoxides: tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and the like. (4) Dialkyl peroxides: di-tert-butyl peroxide, tert-butylcumyl peroxide, dicumyl peroxide, α,α'-bis(tert-butylperoxy-meta-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, and the like. (5) Diacyl peroxides: acetyl peroxide, isobutyl peroxide, octanoyl peroxide, decanoyl peroxide, laurinoyl peroxide, 3,3,5-trimethylhexanoyl peroxide, succinic acid peroxide, benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, meta-toluoyl peroxide, and the like. (6) Peroxydicarbonates: diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-normal propyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, di-2-ethoxyethyl peroxydicarbonate, dimethoxyisopropyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, diallyl peroxydicarbonate, and the like. (7) Peroxyesters: tert-butyl peroxyacetate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, tert-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,3,5-trimethylhexanoate, tert-butyl peroxylaurate, tert-butyl peroxybenzoate, di-tert-butyl peroxybenzoate, butyl peroxyisophthalate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxymaleic acid, tert-butyl peroxyisopropyl carbonate, cumyl peroxyoctoate, tert-hexyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxyneohexanoate, tert-hexyl peroxyneohexanoate, and cumyl peroxyneohexanoate. (8) Other organic peroxides: acetylcyclohexylsulfonyl peroxide, tertiary butyl peroxy allyl carbonate, and the like.
[0034] These polymerization initiators can be used alone or in combination of two or more. Among these polymerization initiators, organic peroxides are preferred in terms of adhesion and curability. Among organic peroxides, hydroperoxides are preferred. Among hydroperoxides, cumene hydroperoxide is preferred.
[0035] The content of the polymerization initiator in the corrosion-protective coating material is preferably 0.5 to 10 parts by mass, and more preferably 0.7 to 5 parts by mass, based on 100 parts by mass of the total content of the (meth)acrylate monomers.
[0036] (Decomposition accelerator) The anticorrosive coating material of the present invention preferably contains a decomposition accelerator in addition to the polymerization initiator. The decomposition accelerator plays a role in accelerating the decomposition of the polymerization initiator to promote the generation of free radicals and promote the curing reaction of the anticorrosive coating material. This makes it possible to more reliably cure the anticorrosive coating material at room temperature. Examples of the decomposition accelerator include the following. (1) Thiourea derivatives: diethylthiourea, dibutylthiourea, ethylenethiourea, tetramethylthiourea, mercaptobenzimidazole, benzoylthiourea, and the like. (2) Amines: N,N-diethyl-p-toluidine, N,N-dimethyl-p-toluidine, N,N-diisopropanol-p-toluidine, N,N-di(2-hydroxyethyl)-p-toluidine, triethylamine, tripropylamine, ethyldiethanolamine, N,N-dimethylaniline, ethylenediamine, triethanolamine, and the like. (3) Metal salts of organic acids: cobalt naphthenate, copper naphthenate, zinc naphthenate, cobalt octoate, iron octoate, and the like. (4) Organic metal chelate compounds: copper acetylacetonate, titanium acetylacetonate, manganese acetylacetonate, chromium acetylacetonate, iron acetylacetonate, vanadyl acetylacetonate, cobalt acetylacetonate, and the like. Other examples of the decomposition accelerator include condensation products of aldehydes and amines. These decomposition accelerators can be used alone or in combination of two or more. Among these, metal salts of organic acids are preferred from the viewpoint of curability. Among metal salts of organic acids, cobalt octylate is preferred. As the decomposition accelerator, it is more preferable to use an amine and a metal salt of an organic acid in combination. When an amine and a metal salt of an organic acid are used in combination, the ratio of the amine to the metal salt of an organic acid is preferably 1 to 45:55 to 99, more preferably 5 to 15:85 to 95, in terms of mass ratio, based on 100 parts by mass of the total of the amine and the metal salt of an organic acid.
[0037] The content of the decomposition accelerator in the corrosion-protective coating material is preferably 0.5 to 10 parts by mass, and more preferably 1.0 to 5 parts by mass, based on 100 parts by mass of the total content of the (meth)acrylate monomers.
[0038] (Silane coupling agent) The anticorrosive coating material of the present invention can contain a silane coupling agent for the purpose of improving adhesion. Examples of the silane coupling agent include γ-chloropropyltrimethoxysilane, vinyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tris(β-methoxyethoxy)silane, γ-(meth)acryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-ureidopropyltriethoxysilane. Among these, γ-(meth)acryloxypropyltrimethoxysilane is preferred in terms of adhesion. The amount of the silane coupling agent used is preferably 0.01 to 20 parts by mass, and more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the total content of the (meth)acrylate monomers.
[0039] (Other Ingredients) The corrosion-protective coating material of the present invention may contain components other than those mentioned above.
[0040] The content of the other components in the corrosion-protective coating material is preferably 50 parts by mass or less, and more preferably 30 parts by mass or less, per 100 parts by mass of the total content of the (meth)acrylate monomers.
[0041] (2-dose type) The anticorrosive coating material of the present invention may be a one-component type, but is preferably a two-component type consisting of a first anticorrosive coating material containing the polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica, and a second anticorrosive coating material containing the decomposition accelerator, the (meth)acrylate monomer, and the hydrophobic silica. However, the amine is preferably contained in the first anticorrosive coating material, and the thiourea derivative, the metal salt of the organic acid, and the organometallic chelate compound are preferably contained in the second anticorrosive coating material. By making the anticorrosive coating material of the present invention a two-component type, the workability of the anticorrosive coating material of the present invention is further improved. In addition, by making the first anticorrosive coating material and the second anticorrosive coating material have almost the same composition, the allowable range of the blending ratio is expanded, so that the anticorrosive coating material can be used even in a workplace where it is difficult to blend them at a strict blending ratio. Therefore, it is preferable that the compositions of the first anticorrosive coating material and the second anticorrosive coating material are almost the same, except for the polymerization initiator and the decomposition accelerator. Specifically, in the first and second anticorrosive coating materials, the hydrophobic silica, the (meth)acrylate monomer (A), the (meth)acrylate monomer (B) and the (meth)acrylate monomer (C) are the same, and the content of the hydrophobic silica relative to 100 parts by mass of the (meth)acrylate monomer, and the content of the (meth)acrylate monomer (A), the content of the (meth)acrylate monomer (B) and the content of the (meth)acrylate monomer (C) relative to 100 parts by mass of the total of the (meth)acrylate monomer (A), the (meth)acrylate monomer (B) and the (meth)acrylate monomer (C) are preferably the same. Furthermore, in the construction of anticorrosive coating for concrete structures, materials are usually delivered, then mixed and kneaded to prepare an anticorrosive coating material. Therefore, by making the corrosion-resistant coating material of the present invention a two-component type, the first corrosion-resistant coating material and the second corrosion-resistant coating material can be mixed easily, and the corrosion-resistant coating material can be produced efficiently.
[0042] (viscosity) The viscosity of the anticorrosion coating material of the present invention at 25°C is preferably 1700 to 15000 mPa·s. When the viscosity of the anticorrosion coating material at 25°C is 1700 mPa·s or more, the anticorrosion coating material can be easily applied thickly. When the viscosity of the anticorrosion coating material at 25°C is 15000 mPa·s or less, the anticorrosion coating material can be easily applied. From this viewpoint, the viscosity of the anticorrosion coating material at 25°C is more preferably 2000 to 15000 mPa·s, and further preferably 2500 to 10000 mPa·s. When the anticorrosion coating material of the present invention is a two-component type of a first anticorrosion coating material and a second anticorrosion coating material, the viscosity of the anticorrosion coating material of the present invention is the viscosity of the anticorrosion coating material obtained by mixing the first anticorrosion coating material and the second anticorrosion coating material. The viscosity of the anticorrosion coating material can be measured by the method described in the examples described later.
[0043] The viscosity of the anticorrosive coating material of the present invention in the range of 0 to 25°C is preferably 1700 to 15000 mPa·s. When the viscosity of the anticorrosive coating material in the range of 0 to 25°C is 1700 mPa·s or more, the anticorrosive coating material can be easily applied thickly even in low temperature periods. When the viscosity of the anticorrosive coating material in the range of 0 to 25°C is 15000 mPa·s or less, the anticorrosive coating material can be easily applied even in low temperature periods. From this viewpoint, the viscosity of the anticorrosive coating material in the range of 0 to 25°C is more preferably 2000 to 15000 mPa·s, and further preferably 2500 to 10000 mPa·s.
[0044] (thixotropy index) The thixotropy index of the anticorrosive coating material of the present invention at 25°C is preferably 3.0 or more. When the thixotropy index of the anticorrosive coating material at 25°C is 3.0 or more, the viscosity of the anticorrosive coating material is reduced during application, making it easier to apply the anticorrosive coating material, and the viscosity of the anticorrosive coating material after application is increased, making it possible to suppress sagging of the anticorrosive coating material. As a result, it becomes easier to apply the anticorrosive coating material thickly. From this viewpoint, the thixotropy index of the anticorrosive coating material at 25°C is more preferably 3.3 or more, and even more preferably 3.5 or more. The upper limit of the thixotropy index of the anticorrosive coating material at 25°C is not particularly limited, but is, for example, 10.0 or less. When the corrosion-protective coating material of the present invention is a two-component type consisting of a first corrosion-protective coating material and a second corrosion-protective coating material, the thixotropy index of the corrosion-protective coating material of the present invention is the thixotropy index of the corrosion-protective coating material obtained by mixing the first corrosion-protective coating material and the second corrosion-protective coating material. The thixotropy index of the corrosion-protective coating material can be measured by the method described in the examples below.
[0045] The thixotropy index of the anticorrosive coating material of the present invention in the range of 0 to 25°C is preferably 3.0 or more. When the thixotropy index of the anticorrosive coating material in the range of 0 to 25°C is 3.0 or more, even in low temperature periods, when the anticorrosive coating material is applied, the viscosity of the anticorrosive coating material is reduced, making it easier to apply the anticorrosive coating material, and the viscosity of the anticorrosive coating material after application is high, making it possible to suppress sagging of the anticorrosive coating material. As a result, it becomes easy to apply the anticorrosive coating material thickly even in low temperature periods. From this viewpoint, the thixotropy index of the anticorrosive coating material at 25°C is more preferably 4.0 or more, and even more preferably 5.0 or more. The upper limit of the thixotropy index of the anticorrosive coating material in the range of 0 to 25°C is not particularly limited, but is, for example, 10.0 or less.
[0046] (Pot life) From the viewpoint of workability of the corrosion-resistant coating material of the present invention, the pot life of the corrosion-resistant coating material of the present invention is preferably 15 to 75 minutes, and more preferably 30 to 50 minutes. The pot life of the corrosion-resistant coating material can be measured by the method described later in the Examples.
[0047] (Curing time) From the viewpoint of workability of the corrosion-protective coating material of the present invention, the curing time of the corrosion-protective coating material of the present invention is preferably 30 to 120 minutes, more preferably 50 to 80 minutes. The curing time of the corrosion-protective coating material can be measured by the method described later in the Examples.
[0048] (tensile shear adhesive strength) From the viewpoint of durability of the corrosion-protective coating material of the present invention, the tensile shear adhesive strength of the corrosion-protective coating material of the present invention is preferably 5 to 35 N / mm 2 and more preferably 10 to 30 N / mm 2 The tensile shear adhesive strength of the corrosion-protective coating material can be measured by the method described in the Examples below.
[0049] [Corrosion-resistant coating layer] The anticorrosive coating layer of the present invention includes a surface adjustment layer made of a hardened alumina cement composition containing alumina cement, a pozzolanic substance, and an aggregate, and an anticorrosive coating layer made of a hardened anticorrosive coating material of the present invention on the surface adjustment layer, which makes it easy to repair concrete structures deteriorated by sulfuric acid or the like, and provides an anticorrosive coating layer that is excellent in sulfuric acid resistance and durability.
[0050] (Tensile adhesive strength) From the viewpoint of durability of the anticorrosive coating layer of the present invention, the tensile adhesive strength of the anticorrosive coating layer of the present invention is preferably 1.0 to 4.0 N / mm 2 and more preferably 1.5 to 4.0 N / mm 2 The tensile adhesive strength of the corrosion-protective coating layer of the present invention can be measured by the method described in the Examples below.
[0051] (sulfuric acid penetration depth) From the viewpoint of sulfuric acid resistance of the corrosion-protective coating layer of the present invention, the sulfuric acid penetration depth of the corrosion-protective coating layer of the present invention is preferably less than 0.3 mm, more preferably less than 0.1 mm. The sulfuric acid penetration depth of the corrosion-protective coating layer of the present invention can be measured by the method described later in the Examples.
[0052] (Anti-corrosion coating layer) The anticorrosive coating layer in the anticorrosive coating layer of the present invention is made of a hardened product of the anticorrosive coating material of the present invention. Therefore, a thick anticorrosive coating layer can be easily formed. This makes it easy to repair concrete structures deteriorated by sulfuric acid or the like. In addition, the anticorrosive coating layer can have excellent sulfuric acid resistance and durability. This also makes the anticorrosive coating layer of the present invention excellent in sulfuric acid resistance and durability.
[0053] <Thickness> From the viewpoint of the sulfuric acid resistance and durability of the corrosion-resistant coating layer, the thickness of the corrosion-resistant coating layer in the corrosion-resistant coating layer of the present invention is preferably 0.4 mm or more, more preferably 0.5 mm or more, and even more preferably 0.8 mm or more. Moreover, by not making the corrosion-resistant coating layer thicker than necessary, the corrosion-resistant coating material is not wasted and the repair of the concrete structure is not laborious, so the thickness of the corrosion-resistant coating layer is preferably 2.0 mm or less, more preferably 1.5 mm or less, and even more preferably 1.0 mm or less.
[0054] (Base adjustment layer) The surface conditioning layer of the corrosion-resistant coating layer of the present invention is made of a hardened alumina cement composition. This further improves the sulfuric acid resistance and durability of the corrosion-resistant coating layer. The alumina cement composition contains alumina cement, a pozzolanic substance, and an aggregate.
[0055] <Alumina cement> The alumina cement in the alumina cement composition used in the surface adjustment layer of the corrosion-resistant coating layer of the present invention is different from Portland cement in that it forms a hardened body without producing slaked lime as a hydration product, and therefore has excellent sulfuric acid resistance. Alumina cement is obtained from ground clinker containing monocalcium aluminate as the main mineral, and for example, Alumina Cement No. 1, Alumina Cement No. 2, etc. can be used.
[0056] The fineness of alumina cement is 2000-8000 cm 2 / g is preferred in terms of hydration activity.
[0057] <Pozzolanic substances> The pozzolanic substance in the alumina cement composition used in the surface adjustment layer of the corrosion-resistant coating layer of the present invention is a substance that exhibits pozzolanic activity upon alkaline stimulation. By using the pozzolanic substance in combination with alumina cement, it is possible to suppress the decrease in strength due to the phase transition of hydrates and improve the sagging resistance of the alumina cement composition during application. Examples of the pozzolanic substance include granulated blast furnace slag, slowly cooled blast furnace slag, converter slag, silica fume, and fly ash. These pozzolanic substances can be used alone or in combination of two or more.
[0058] The fineness of the pozzolanic material is determined based on the hydration activity and the specific surface area of the Blaine powder of 3000 cm. 2 / g or more is preferable. The amount of the pozzolanic substance used is usually preferably 60 to 200 parts by mass, more preferably 80 to 150 parts by mass, per 100 parts by mass of alumina cement. The amount of silica fume used is preferably 1 to 20 parts by mass, per 100 parts by mass of alumina cement.
[0059] <Aggregate> The aggregate in the alumina cement composition used in the surface adjustment layer of the corrosion-resistant coating layer of the present invention is not particularly limited, and is a commonly available aggregate. Examples include silica sand aggregate, silica stone aggregate, limestone aggregate, heavy aggregate, and lightweight aggregate. These aggregates can be used alone or in combination of two or more. In terms of acid resistance, it is preferable to use aggregates other than limestone aggregate. Among aggregates other than limestone aggregate, silica sand is preferable. By including an aggregate in the alumina cement composition, the strength of the surface adjustment layer can be improved.
[0060] The amount of aggregate used is not particularly limited as long as it is used within a range that does not affect acid resistance or fluidity, but is preferably 100 to 400 parts by mass per 100 parts by mass of the total of the alumina cement and the pozzolanic substance.
[0061] <Portland cement> In order to further enhance the hardening property of the pozzolanic substance contained in the alumina cement composition, the alumina cement composition may further contain portland cement. This can improve the strength of the base adjustment layer. The amount of portland cement used is not particularly limited as long as it is used within a range that does not affect the acid resistance performance or fluidity, but is preferably 25 to 70 parts by mass relative to 100 parts by mass of alumina cement. In addition, when the alumina cement composition contains portland cement, the alumina cement composition may further contain gypsum in order to enhance the strength of the base adjustment layer. The amount of gypsum used is not particularly limited as long as it is used within a range that does not affect the acid resistance performance or fluidity, but is preferably 50 to 150 parts by mass relative to 100 parts by mass of portland cement. In addition, when the alumina cement composition contains portland cement, the alumina cement composition may further contain slaked lime in order to promote the hardening of the alumina cement composition. The amount of slaked lime used is not particularly limited as long as it is used within a range that does not affect acid resistance or fluidity, but is preferably 5 to 50 parts by mass relative to 100 parts by mass of Portland cement.
[0062] <Additives> The alumina cement composition used in the surface adjustment layer of the anticorrosive coating layer of the present invention can contain various additives to the extent that they do not adversely affect the quality of the surface adjustment layer. It is preferable not to use higher fatty acid-based admixtures for the purpose of waterproofing or crack prevention, etc., since they may deteriorate the adhesion between the concrete and the surface adjustment layer. It is also preferable not to use concrete curing agents in which wax, resin, chlorinated rubber, etc. are dissolved in a solvent, since they may deteriorate the adhesion between the concrete and the surface adjustment layer.
[0063] <Porosity> The porosity of the surface adjusting layer is preferably 5 to 40% by volume. When the porosity of the surface adjusting layer is 5% by volume or more, the anticorrosive coating material or the primer composition described later can be sufficiently permeated into the surface adjusting layer, and the anticorrosive coating layer or the primer can be further prevented from peeling off from the surface adjusting layer. As a result, the sulfuric acid resistance and durability of the anticorrosive coating layer are further improved. When the porosity of the surface adjusting layer is 40% by volume or less, the anticorrosive coating material or the primer composition described later can be prevented from excessively permeating into the surface adjusting layer. Note that, if the anticorrosive coating material or the primer composition described later excessively permeates into the surface adjusting layer, the amount of the anticorrosive coating material or the primer composition required to form the anticorrosive coating layer or the primer of the desired thickness becomes very large. From this viewpoint, the porosity of the surface adjusting layer is more preferably 5 to 30% by volume. In addition, when the surface adjustment layer has the above-mentioned porosity, the voids in the surface adjustment layer in the region near the anticorrosive coating layer or in the region near the primer are filled with the hardened body of the anticorrosive coating material or the hardened body of the primer composition. The region of the surface adjustment layer near the anticorrosive coating layer is within 0.5 mm from the interface between the surface adjustment layer and the anticorrosive coating layer. The region of the surface adjustment layer near the primer is within 2 mm from the interface between the surface adjustment layer and the primer.
[0064] <Thickness> From the viewpoint of sulfuric acid resistance and durability of the corrosion-protective coating layer, the thickness of the surface adjustment layer in the corrosion-protective coating layer of the present invention is preferably 10 mm or more, more preferably 15 mm or more, and even more preferably 20 mm or more. By not making the surface adjustment layer thicker than necessary, the alumina cement composition is not wasted and the repair of the concrete structure is not laborious, so the thickness of the surface adjustment layer is preferably 70 mm or less, more preferably 60 mm or less, and even more preferably 50 mm or less.
[0065] <Compressive strength> From the viewpoint of durability of the anticorrosive coating layer, the compressive strength of the alumina cement composition used in the base adjustment layer of the anticorrosive coating layer of the present invention is preferably 30 to 90 N / mm 2 and more preferably 40 to 80 N / mm 2 The compressive strength of the alumina cement composition can be measured by the method described in the Examples below.
[0066] (Primer) The anticorrosive coating layer of the present invention preferably includes a primer disposed between the surface adjustment layer and the anticorrosive coating layer. This makes it possible to prevent the anticorrosive coating layer from peeling off from the surface adjustment layer. As a result, the sulfuric acid resistance and durability of the anticorrosive coating layer are further improved. The primer is made of a cured product of a primer composition containing a (meth)acrylate monomer.
[0067] The (meth)acrylate monomer contained in the primer composition is preferably the same as the (meth)acrylate monomer used in the above-mentioned anticorrosive coating material. This can further strengthen the adhesion between the primer and the anticorrosive coating layer. As a result, the sulfuric acid resistance and durability of the anticorrosive coating layer are further improved. In addition, like the (meth)acrylate monomer used in the above-mentioned anticorrosive coating material, the primer composition also preferably contains a polymerization initiator and a decomposition accelerator. In addition, like the (meth)acrylate monomer used in the above-mentioned anticorrosive coating material, the primer composition may also contain the above-mentioned other components. In addition, like the (meth)acrylate monomer used in the above-mentioned anticorrosive coating material, the primer composition is preferably a two-part type consisting of a first primer composition containing the above-mentioned polymerization initiator and the above-mentioned (meth)acrylate monomer, and a second primer composition containing the above-mentioned decomposition accelerator and the above-mentioned (meth)acrylate monomer.
[0068] The (meth)acrylate monomer, polymerization initiator, and decomposition accelerator contained in the primer composition are the same as the (meth)acrylate monomer, polymerization initiator, and decomposition accelerator used in the above-mentioned anticorrosive coating material, so a description of the (meth)acrylate monomer, polymerization initiator, and decomposition accelerator contained in the primer composition will be omitted. The (meth)acrylate monomer, polymerization initiator, and decomposition accelerator contained in the primer composition are preferably the same as the (meth)acrylate monomer, polymerization initiator, and decomposition accelerator used in the anticorrosive coating material of the anticorrosive coating material layer provided adjacent to the primer.
[0069] <Thickness> From the viewpoint of preventing the corrosion-resistant coating layer from peeling off from the surface adjustment layer, the thickness of the primer is preferably 50 to 250 μm, more preferably 80 to 200 μm, and even more preferably 100 to 150 μm.
[0070] <Viscosity> From the viewpoint of workability of the primer composition, the viscosity of the primer composition at 25° C. is preferably 50 to 1000 mPa s, and more preferably 100 to 500 mPa s. The viscosity of the primer composition at 25° C. can be measured by the method described in the Examples below.
[0071] (Pot life) From the viewpoint of workability of the primer composition, the pot life of the primer composition is preferably 10 to 50 minutes, more preferably 20 to 30 minutes. The pot life of the primer composition can be measured by the method described in the examples below.
[0072] (Curing time) From the viewpoint of workability of the primer composition, the curing time of the primer composition is preferably 15 to 85 minutes, more preferably 30 to 50 minutes. The curing time of the primer composition can be measured by the method described in the examples below.
[0073] (Construction period) One of the factors that adversely affect the quality of a corrosion-resistant coating layer is the time of application, such as during rainy seasons, high temperatures, or low temperatures. Low temperatures are particularly unfavorable as an application time, since they adversely affect the hardening and performance of the resin. However, the corrosion-resistant coating layer of the present invention can maintain high quality even in low temperatures (for example, an application environment at a temperature of 0 to 15°C), and therefore the corrosion-resistant coating layer can be applied even in low temperatures.
[0074] [Corrosion prevention methods for concrete structures] The corrosion protection method for a concrete structure of the present invention includes the steps of assembling a formwork (A), casting the above-mentioned alumina cement composition into the formwork to form a surface adjustment layer (B), removing the formwork (C), and applying the corrosion protection coating material of the present invention to form a corrosion protection coating material layer on the surface adjustment layer (D). This makes it possible to easily form a corrosion protection coating layer that is excellent in sulfuric acid resistance and durability, and makes it easy to repair a concrete structure that has been deteriorated by sulfuric acid or the like.
[0075] (Process (A)) In step (A), a formwork is assembled. By using the formwork, anticorrosion work can be performed on a concrete structure in which the reinforcing steel is severely damaged and relatively large-scale repair is required. For example, when anticorrosion is performed on the inner wall surface of a manhole, a cylindrical formwork described in JP 2015-71939 A can be used.
[0076] (Process (B)) In step (B), the alumina cement composition is poured into the formwork to form a base adjustment layer. For example, when protecting the inner wall surface of a manhole from corrosion, the alumina cement composition is poured into the gap between the cylindrical formwork and the inner wall surface of the manhole, and hardened to form a base adjustment layer. The alumina cement composition must be poured in such a way that material separation is minimized and that defects in the base adjustment layer after pouring are not formed. After pouring the alumina cement composition, compaction may be performed using a vibrator. This allows the formation of a dense base adjustment layer with few air bubbles and voids. The alumina cement composition can also be sufficiently spread around the reinforcing bars and in every corner of the formwork.
[0077] (Process (C)) In step (C), the formwork is removed. The formwork must be removed after the surface adjustment layer has reached the strength required to support its own weight and the load applied during construction. In order to determine when the surface adjustment layer has reached the required strength, for example, the compressive strength of a standard specimen cured in the same condition as the surface adjustment layer may be measured. It is preferable to first remove the parts of the formwork that are relatively unloaded, and then remove the remaining important parts. For example, it is preferable to remove the horizontal parts of the formwork later than the vertical parts.
[0078] (Process (D)) In step (D), the anticorrosive coating material of the present invention is applied to form an anticorrosive coating layer on the surface adjustment layer. In order to ensure sulfuric acid resistance throughout the anticorrosive coating layer, it is important to ensure a uniform application thickness and to have no pinholes. For this reason, it is preferable to carefully apply the anticorrosive coating material using a roller, a metal trowel, a dedicated coating machine, or the like. The anticorrosive coating material of the present invention can be applied thickly even at a low viscosity, so that the coating thickness can be made uniform and the occurrence of pinholes can be suppressed. The applied anticorrosive coating material must have a required layer thickness. Since the anticorrosive coating material of the present invention can be easily applied thickly, it is easy to ensure the required layer thickness of the anticorrosive coating material. In order to ensure the durability of the anticorrosive coating layer, it is preferable to perform appropriate curing after the application of the anticorrosive coating material is completed so that the anticorrosive coating layer is not damaged until the anticorrosive coating layer is in a state that can withstand use. The curing period for the anticorrosive coating layer is, for example, 1 to 7 days.
[0079] (Process (E)) The method for preventing corrosion of a concrete structure of the present invention may further include a step (E) of applying a primer composition containing a (meth)acrylate monomer to a surface adjustment layer to form a primer. In this case, in step (D), a corrosion-resistant coating material is applied to the primer. This allows a primer to be formed between the surface adjustment layer and the corrosion-resistant coating material layer. The primer composition is applied to the surface adjustment layer using, for example, a brush or a roller. The primer composition is preferably applied to a dried surface adjustment layer. For example, the surface moisture content of the surface adjustment layer to which the primer composition is applied is preferably 7% or less.
[0080] (Steps inside a manhole) The steps (footrests) inside the manhole may be corroded by corrosive gases such as hydrogen sulfide. For this reason, it is preferable to replace the steps inside the manhole when carrying out corrosion protection on the inner wall surface of the manhole. From this perspective, the corrosion protection method for a concrete structure of the present invention may include a step of removing the old steps before step (A) and a step of attaching new steps after step (D). The old steps can be removed, for example, by cutting. Also, the new steps can be attached, for example, by the twin drill method recommended by the Twin Drill Method Association.
[0081] (Process to remove corroded parts) The method for preventing corrosion of a concrete structure of the present invention may include a step of removing the corroded portion of the concrete structure prior to step (A). For example, the corroded portion may be removed by ultra-high pressure water treatment until a sound concrete surface is exposed. The water pressure used in the ultra-high pressure water treatment is, for example, 150 to 200 MPa. Whether or not a sound concrete surface is exposed can be determined by, for example, the phenolphthalein method.
[0082] (Reinforcing bar processing) In the method for preventing corrosion of a concrete structure of the present invention, before the step (A), the corroded portion of the concrete structure may be removed, and then the reinforcing bar in the concrete structure may be treated. For example, in the treatment of the reinforcing bar, loose rust may be removed using sandblasting, power tools, or the like, and the reinforcing bar may be cleaned using air blasting or high-pressure water, and then a rust inhibitor may be applied to the reinforcing bar.
[0083] (Cross-section repair) If there are defects such as cracks in the cross section of the concrete that appears after removing the corroded parts of the concrete structure, the defects will cause defects in the anticorrosive coating layer. For this reason, it is preferable to repair the cross section of the concrete prior to step (A). For example, a V-cut is made along the crack in the concrete using a grinder or the like. Then, a primer may be applied to the V-cut area, and then a sealant may be filled in. Note that the sealant may be filled in after the construction of the anticorrosive coating layer.
[0084] [Application] The present invention is suitable for corrosion inhibition and corrosion prevention technologies for sewer concrete structures. The present invention can extend the service life of sewer concrete structures as long as possible. Sewer facilities are composed of, for example, sewer pipes, pumping stations, and treatment plants. Among these facilities, the present invention is more suitable for corrosion inhibition and corrosion prevention technologies for concrete structures of sewer pipes, which have a narrow working space, because the concrete structures can be easily repaired, and is even more suitable for corrosion inhibition and corrosion prevention technologies for manholes of sewer pipes. The corrosive environment in manholes of sewer pipes is generally a corrosive environment in which the annual average hydrogen sulfide gas concentration is 10 ppm or more and less than 50 ppm, and concrete corrosion is prominent (Classification of corrosive environments described on page 47 of Non-Patent Document 1: Class II). This corrosive environment is an environment in which, if left unattended, concrete will corrode in several years (annual average corrosion rate of approximately 4 mm / year), and the corrosion is thought to reach the reinforcing bars. However, the present invention can extend the service life of sewer concrete structures as long as possible even in such a severe corrosive environment. EXAMPLES
[0085] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0086] The anticorrosive coating materials of the Examples and Comparative Examples were evaluated as follows. (Viscosity / thixotropy index) The viscosity of the anticorrosive coating material was measured using a B-type viscometer (rotor No. 5) at a spindle speed of 20 rpm and in the temperature range of 0 to 35°C. In addition, the viscosity was measured at spindle rotation speeds of 2 rpm and 20 rpm, and then the thixotropy index was calculated based on the following formula. <Calculation formula for thixotropy index> Thixotropy index = Viscosity at 2 rpm ÷ Viscosity at 20 rpm The viscosity of the primer composition used as the primer for the corrosion-protective coating layer in the examples and comparative examples was also measured in the same manner.
[0087] (Curing time, pot life) 25g of agent A and 25g of agent B of the corrosion protection coating material were weighed and mixed to prepare a mixed solution, and the temperature of the mixed solution was measured using a thermocouple. The time when the temperature reached its highest was determined as the curing time. The pot life was calculated based on the following formula. <Pot life calculation formula> Pot life = curing time x 0.6 The curing time and pot life of the primer compositions used as the primer for the corrosion-protective coating layers in the Examples and Comparative Examples were also measured in the same manner.
[0088] (tensile shear adhesive strength) The tensile shear adhesive strength of the anticorrosive coating material was measured in accordance with JIS K6850. Specifically, two SS400 steel plates (100 mm × 25 mm × 1.6 mm thick) whose surfaces had been sandblasted and degreased with acetone were prepared. The anticorrosive coating material was applied to one of the SS400 steel plates within a range of 12.5 mm from the end in the longitudinal direction. The two SS400 steel plates were bonded together (adhesive area 3.125 cm) so that the portion of one SS400 steel plate to which the anticorrosive coating material was applied overlapped only with the portion of the other SS400 steel plate within a range of 12.5 mm from the end in the longitudinal direction. 2), and a tensile shear bond strength test piece was prepared. The anticorrosive coating material of the tensile shear bond strength test piece was then cured for one day at a temperature of 23°C and a humidity of 50%. The non-overlapping side of the two SS400 steel plates in the tensile shear bond strength test piece was the gripping part of the tensile tester. The tensile shear bond strength of the prepared test piece was measured using a tensile tester under conditions of a temperature of 23°C, humidity of 50%, and a tensile speed of 10 mm / min.
[0089] (Coatability) A mold formwork of 140 mm × 195 mm × 20 mm was attached to a concrete slab, and the alumina cement composition was poured into it to prepare a test specimen. After removing the formwork, the test specimen was immediately stood vertically and cured for one day at a temperature of 20°C and a humidity of 60%. After curing, a primer composition was applied to the surface of the test specimen in an amount of 150 g / m. 2 The primer was formed on the surface of the test specimen by applying a coating of 500 g / m2 to the surface of the primer. 2 The anticorrosion coating material was then cured for one day at a temperature of 20°C and a humidity of 60%. The appearance of the cured anticorrosion coating material was visually evaluated, and the thickness of the coating film was measured using a wet gauge. If a coating film of 0.4 mm or more was formed without dripping and there were no wrinkles, unevenness, or peeling in the appearance, it was judged as good. On the other hand, if there was dripping, if a coating film of 0.4 mm or more could not be formed, or if there was at least one defect of wrinkles, unevenness, or peeling in the appearance, it was judged as poor.
[0090] The alumina cement compositions used in the surface adjustment layers of the anticorrosive coating layers in the Examples and Comparative Examples were evaluated as follows. (Compressive strength, porosity) The compressive strength of the alumina cement composition was measured according to JIS R5201. Specifically, the alumina cement composition was poured into a mold formwork of 40 mm x 40 mm x 160 mm to prepare a test specimen. After demolding the next day, the test specimen was cured in water at 20°C for 27 days, and the compressive strength of the test specimen after 28 days was measured. In addition, the porosity of the test specimen was measured according to ASTM-C-642.
[0091] The corrosion-resistant coating layers of the examples and comparative examples were evaluated as follows. (Average particle size) The particle size distribution of the hydrophobic silica was measured using a laser diffraction scattering particle size distribution analyzer (LS-13 320) manufactured by Beckman Coulter, Inc., and the particle size at which the cumulative frequency was 50% by volume was determined as the average particle size of the hydrophobic silica. (Blaine specific surface area) Measurements were performed in accordance with JIS R5201. (Adhesiveness) The adhesion of the corrosion-resistant coating layer was measured according to JIS A7502-2:2015 "Concrete corrosion prevention technology for sewerage structures - Part 2: Corrosion prevention design standard, Annex L (regulations) Tensile test (sheet lining method and mortar lining method)". Specifically, a 280mm x 280mm x 20mm mold formwork was attached to a concrete slab (300mm x 300mm x 60mm), and an alumina cement composition was poured to form a base adjustment layer. After demolding the next day, the base adjustment layer was cured in water at 20°C for 27 days. A primer composition was applied to the surface of the cured base adjustment layer at an amount of 150g / m. 2 The primer was formed on the surface of the base adjustment layer by applying a coating of 500 g / m2 of anticorrosive coating material on the surface of the primer. 2 The coating was applied at 100°C, and cured for one day under an environment of 25°C and 50% humidity to form a corrosion-resistant coating layer on the surface of the concrete plate. A concrete cutter was used to cut the surface of the corrosion-resistant coating layer to a size of 40 mm x 40 mm until it reached the concrete plate to prepare a test piece for a tensile bond strength test. An upper tensile steel jig was attached to the surface of the corrosion-resistant coating layer using an adhesive (Denka Hardrock II acrylic resin mortar Dyna N, manufactured by Denka Co., Ltd.). Then, the maximum tensile load was measured under an environment of 23°C and 50% humidity using a Construction Research Institute type adhesion tester, and the tensile bond strength was calculated based on the following formula. The fracture surface of the test piece was also observed to identify the fracture location. <Tensile adhesive strength> σ t =T / 1600 σ t : Tensile adhesive strength (N / mm 2 ) T: Maximum tensile load (N)
[0092] (Sulfuric acid resistance test) A sulfuric acid resistance test was carried out according to JIS A7502 "Immersion test of anticorrosive coating layer c) In the case of mortar lining method". Specifically, the alumina cement composition was poured into a mold form of 75 mmφ×150 mm, and the form was removed the next day. The alumina cement hardened body was then cured in water at 20°C for 27 days. A primer composition was applied to the entire surface of the alumina cement hardened body at a rate of 100 g / m. 2 The primer was formed on the surface of the hardened alumina cement body by curing for 30 minutes. The anticorrosive coating material was applied to the surface of the primer at a rate of 500 g / m 2 The primer was applied at 100°C, and cured for one day in an environment with a temperature of 25°C and a humidity of 50%, forming a corrosion-resistant coating layer on the surface of the primer to prepare a test specimen for sulfuric acid resistance test. The prepared test specimen was immersed in a test liquid (5% sulfuric acid aqueous solution). The test liquid was replaced every 7 days for the first 4 weeks, and then every 4 weeks. The test specimen was removed after 112 days of immersion. The test specimen was then washed with water, and the appearance of the test piece was visually evaluated. If there were no wrinkles, unevenness, peeling, or cracks, it was judged to be good. On the other hand, if there was at least one defect of wrinkles, unevenness, peeling, or cracks, it was judged to be bad.
[0093] (sulfuric acid penetration depth) The sulfuric acid penetration depth was measured according to JIS A7502 "Method for measuring sulfuric acid penetration depth of corrosion protection coating layer (mortar lining method)". Specifically, the test specimen after the above-mentioned sulfuric acid resistance test was cut in half in a direction perpendicular to the axial direction of the cylinder. A 1% solution of phenolphthalein was sprayed on the circular cut surface. The length of the diameter of the part of the test specimen that turned red was measured at five points with a vernier caliper, and the average value was subtracted from the initial value (75 mm) to calculate half of the value, which was the sulfuric acid penetration depth. Note that the pH value of the test specimen decreases in the area where sulfuric acid penetrated, so the area where sulfuric acid penetrated does not turn color with phenolphthalein.
[0094] An anticorrosive coating material, an alumina cement composition and a primer composition were prepared as follows. (Anti-corrosion coating material) Anticorrosive coating materials were prepared using the materials shown in Tables 1 and 2, and their physical properties were measured. The results are shown in Tables 1 and 2.
[0095] (Alumina cement composition) An alumina cement composition was prepared using the materials shown in Table 3, and each physical property was measured. The results are shown in Table 3.
[0096] (Primer composition) A primer composition was prepared using the materials shown in Table 4, and each physical property was measured. The results are shown in Table 4.
[0097] (Anti-corrosion coating layer) The above-mentioned anticorrosive coating material, alumina cement composition and primer composition were used to form an anticorrosive coating layer, and the physical properties were measured. The results are shown in Table 5.
[0098] (Materials used) ((Meth)acrylate Monomer) M-241: Bisphenol A type EO4 modified dimethacrylate: In the general formula (5), R 4 and R 4 ' is a methyl group, and R 5 and R 5 ' is an ethylene group, and m+n is approximately 4. Manufactured by Miwon Specialty Chemical Co., Ltd. PE210: Bisphenol A glycidyl ether acrylic acid adduct: In the general formula (5), R 4 and R 4 ' is hydrogen and R 5 and R 5 ' is an n-propylene group having a 2-hydroxyl group, and m and n are 1. Fancryl FA512M: Dicyclopentenyloxyethyl methacrylate, in the general formula (6), R 6 is a methyl group, and R 7 is an ethylene group, and p is approximately 1. 2HEMA: 2-hydroxyethyl methacrylate, in general formula (7), R 8 is a methyl group, and R 9 is hydrogen. Manufactured by Mitsubishi Chemical Corporation (silica) Aerosil R-972: Dimethyldichlorosilane (R 1 is a methyl group, x is 2, and y is 2.) Hydrophobized silica: average particle size 16 nm, manufactured by Evonik Japan Co., Ltd. Aerosil R-805: Octylsilane (in general formula (1), R 1 is an octyl group (having 8 carbon atoms), x is 1, and y is 0.) Hydrophobized silica: average particle size 12 nm, manufactured by Evonik Japan Co., Ltd. Aerosil R-812: Hexamethyldisilazane (wherein R 2 is a methyl group, and R 3 is hydrogen, and z is 3.) Hydrophobized silica: average particle size 7 nm, manufactured by Evonik Japan Co., Ltd. Aerosil RX-50: Hexamethyldisilazane (R 2 is a methyl group, and R 3 is hydrogen, and z is 3.) Hydrophobized silica: average particle size 40 nm, manufactured by Evonik Japan Co., Ltd. FB-5D: Fused silica, average particle size 5 μm, manufactured by Denka Co., Ltd. Aerosil 380: Hydrophilic fumed silica, average particle size 7 nm, manufactured by Evonik Japan Co., Ltd. (Inorganic thixotropic agent) Esben WX: Organic bentonite with quaternary ammonium cations modified on the crystal surface of montmorillonite, manufactured by Hojun Co., Ltd. (Polymerization initiator) Kayakumen H: Cumene hydroperoxide, manufactured by Kayaku Nouryon Co., Ltd. (Decomposition accelerator) Co-12E: Cobalt octylate, manufactured by Tokyo Fine Chemical Co., Ltd. (Silane coupling agent) SILQUEST A-174: γ-Methacryloxypropyltrimethoxysilane, manufactured by Momentive Performance Materials Japan, LLC (Cure accelerator) PT-2HE: N,N-di(2-hydroxyethyl)-p-toluidine, manufactured by Morin Chemical Industry Co., Ltd. (Alumina cement) Alumina cement No. 1: Alumina cement, Blaine specific surface area 4800 cm 2 / g, manufactured by Denka Co., Ltd. (Portland cement) Ordinary cement: Portland cement, manufactured by Denka Co., Ltd. (Pozzolanic substances) Blast furnace slag: Granulated blast furnace slag, commercially available, Blaine specific surface area 6100cm 2 / g Silica fume, commercially available (others) Gypsum: Commercially available Slaked lime, commercially available Silica sand, commercially available
[0099] [Table 1]
[0100] [Table 2]
[0101] [Table 3]
[0102] [Table 4]
[0103] [Table 5]
[0104] The anticorrosive coating materials of Examples 1 to 5, which contain a (meth)acrylate monomer and hydrophobic silica with an average particle size of 1 to 100 nm, had good applicability. On the other hand, the anticorrosive coating material of Comparative Example 1, in which the silica was not hydrophobized and the average particle size of the silica was greater than 100 nm, could not be applied thickly. In addition, the anticorrosive coating material of Comparative Example 2, in which the silica was not hydrophobized, could not uniformly disperse the silica, resulting in unevenness. Furthermore, the anticorrosive coating material of Comparative Example 3, which does not contain hydrophobic silica, caused dripping and could not be applied thickly. In addition, the anticorrosive coating material of Comparative Example 4, in which organic bentonite, a type of inorganic thixotropic agent, was blended instead of hydrophobic silica, had little effect of thickening and imparting thixotropy, caused dripping, and could not be applied thickly. The primer compositions of Examples 6 to 11 could be applied to a thickness of 100 μm without dripping.
[0105] It was found that the anticorrosive coating layers of Examples 6 to 11, which include a surface adjustment layer made of a hardened product of an alumina cement composition containing alumina cement, a pozzolanic substance, and an aggregate, and an anticorrosive coating layer made of a hardened product of the anticorrosive coating material of the present invention on the surface adjustment layer, have excellent sulfuric acid resistance. In addition, since the tensile bond strength is high in addition to excellent sulfuric acid resistance, the anticorrosive coating layers of Examples 6 to 11 have excellent durability. Furthermore, by comparing the anticorrosive coating layer of Example 6 with the anticorrosive coating layer of Example 10, it is found that the provision of a primer improves sulfuric acid resistance, and therefore durability is further improved. Furthermore, it is found that the anticorrosive coating layer of the present invention can be applied as an excellent anticorrosive coating layer even in low temperature periods, as compared with the anticorrosive coating layer of Example 7. On the other hand, the anticorrosive coating layers of Comparative Examples 5 to 8, in which the anticorrosive coating layer is not made of a hardened product of the anticorrosive coating material of the present invention, had poor sulfuric acid resistance. Furthermore, the anticorrosive coating layers of Comparative Examples 9 and 10, which do not include an anticorrosive coating layer, had poor sulfuric acid resistance. Moreover, although the anticorrosive coating layers of Comparative Examples 5 to 8 have high tensile adhesive strength, they are inferior in sulfuric acid resistance, and therefore it is clear that the anticorrosive coating layers of Comparative Examples 5 to 8 have poor durability.
Claims
1. A coating composition comprising: a substrate adjustment layer made of a hardened alumina cement composition containing alumina cement, a pozzolanic substance, and an aggregate; a corrosion-resistant coating layer made of a hardened corrosion-resistant coating material; and a primer made of a hardened primer composition containing a (meth)acrylate monomer, the primer being disposed between the substrate adjustment layer and the corrosion-resistant coating layer; The corrosion-resistant coating material comprises a (meth)acrylate monomer and a hydrophobic silica, The anticorrosive coating layer has an average particle size of the hydrophobic silica of 1 to 100 nm.
2. 2. The corrosion-protective coating layer according to claim 1, wherein the hydrophobic silica is at least one of silica hydrophobized with an organosilane represented by the following general formula (1) and silica hydrophobized with an organosilane represented by the following general formula (2): R 1 x SiCl y H 4-x-y (1) In general formula (1), R 1 represents an alkyl group, x represents an integer of 1 to 3, y represents an integer of 0 to 3, and x+y≦4. (R 2 z H 3-z Si) 2 N.R. 3 (2) In general formula (2), R 2 represents hydrogen, an alkyl group, an alkenyl group, or a halogenated alkyl group; R 3 represents hydrogen, an alkyl group or an alkali metal element; z represents an integer of 1 to 3.
3. the hydrophobic silica includes silica hydrophobized with a first organosilane represented by the general formula (1) and silica hydrophobized with a second organosilane represented by the general formula (1) different from the first organosilane, In the general formula (1), R 1 is an alkyl group represented by the following general formula (3), and R 1The corrosion-resistant coating layer according to claim 2 , wherein: C s H 2s+1 (3) In formula (3), s represents an integer of 1 to 5. C t H 2t+1 (4) In the general formula (4), t represents an integer of 6 to 12.
4. The corrosion-resistant coating layer according to any one of claims 1 to 3, wherein the (meth)acrylate monomer comprises a di(meth)acrylate having a bisphenol A skeleton.
5. The corrosion-protective coating layer according to claim 4 , wherein the di(meth)acrylate monomer having a bisphenol A skeleton is a di(meth)acrylate having a bisphenol A skeleton represented by the following general formula (5): [Formula 1] In general formula (5), R 4 and R 4 ' represents hydrogen or a methyl group; R 5 and R 5 "M" represents an alkylene group which may have a substituent, and "m" and "n" each represent an integer of 1 to 20.
6. The viscosity of the corrosion-resistant coating material at 25°C is 1700 to 15000 mPa·s, The corrosion-protective coating layer according to any one of claims 1 to 5, wherein the corrosion-protective coating material has a thixotropy index at 25°C of 3.0 or more.
7. The viscosity of the corrosion-resistant coating material in the range of 0 to 25°C is 1700 to 15000 mPa·s, The corrosion-protective coating layer according to any one of claims 1 to 6, wherein the corrosion-protective coating material has a thixotropy index in the range of 0 to 25°C of 3.0 or more.
8. The corrosion-resistant coating layer described in any one of claims 1 to 7, wherein the corrosion-resistant coating material is a two-component type comprising a first corrosion-resistant coating material containing a polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica, and a second corrosion-resistant coating material containing a decomposition accelerator that accelerates decomposition of the polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica.
9. The corrosion-resistant coating layer according to any one of claims 1 to 8, wherein the (meth)acrylate monomer contained in the primer composition comprises a di(meth)acrylate having a bisphenol A skeleton.
10. The corrosion-resistant coating layer according to claim 9, wherein the di(meth)acrylate having a bisphenol A skeleton contained in the primer composition is a di(meth)acrylate having a bisphenol A skeleton represented by the following general formula (5): [chemical 2] In general formula (5), R 4 and R 4 ' represents hydrogen or a methyl group; R 5 and R 5 "M" represents an alkylene group which may have a substituent, and "m" and "n" each represent an integer of 1 to 20.
11. The porosity of the base material adjustment layer is 5 to 40 volume %, The corrosion-resistant coating layer according to any one of claims 1 to 10, wherein in a region of the surface adjustment layer adjacent to the primer, voids in the surface adjustment layer are filled with a cured product of the primer composition.
12. The process of assembling the formwork, A step of pouring an alumina cement composition containing an alumina cement, a pozzolanic substance, and an aggregate into the formwork to form a base adjustment layer; removing the formwork; A step of applying a primer composition containing a (meth)acrylate monomer to the surface adjustment layer to form a primer; applying a corrosion-resistant coating to form a corrosion-resistant coating layer on the primer; The corrosion-resistant coating material comprises a (meth)acrylate monomer and a hydrophobic silica, The method for preventing corrosion of a concrete structure, wherein the average particle size of the hydrophobic silica is 1 to 100 nm.
13. The corrosion prevention method for a concrete structure as described in claim 12, wherein the hydrophobic silica is at least one type of silica hydrophobized with an organosilane represented by the following general formula (1) and silica hydrophobized with an organosilane represented by the following general formula (2): R 1 x SiCl y H 4-x-y (1) In the general formula (1), R 1 represents an alkyl group, x represents an integer of 1 to 3, y represents an integer of 0 to 3, and x+y≦4. (R 2 z H 3-z Si) 2 N.R. 3 (2) In formula (2), R 2 represents hydrogen, an alkyl group, an alkenyl group or a halogenated alkyl group; R 3 represents hydrogen, an alkyl group or an alkali metal element; and z represents an integer of 1-3.
14. The hydrophobic silica comprises silica hydrophobized with a first organosilane represented by the general formula (1) and silica hydrophobized with a second organosilane represented by the general formula (1) different from the first organosilane, The corrosion prevention method for a concrete structure according to claim 13, wherein, in the general formula (1), R 1 of the first organosilane is an alkyl group represented by the following general formula (3), and R 1 of the second organosilane is an alkyl group represented by the following general formula (4). C s H 2s+1 (3) In formula (3), s represents an integer of 1 to 5. C t H 2t+1 (4) In the general formula (4), t represents an integer of 6 to 12.
15. The method for preventing corrosion of a concrete structure according to claim 12, wherein the (meth)acrylate monomer comprises a di(meth)acrylate having a bisphenol A skeleton.
16. A corrosion prevention method for a concrete structure as described in claim 15, wherein the di(meth)acrylate monomer having a bisphenol A skeleton is a di(meth)acrylate having a bisphenol A skeleton represented by the following general formula (5): [C3] In formula (5), R 4 and R 4 ′ each represent a hydrogen atom or a methyl group, R 5 and R 5 ′ each represent an alkylene group which may have a substituent, and m and n each represent an integer of 1-20.
17. The viscosity of the corrosion-resistant coating material at 25°C is 1700 to 15000 mPa·s, The method for preventing corrosion of a concrete structure according to any one of claims 12 to 16, wherein the anticorrosive coating material has a thixotropic index at 25°C of 3.0 or more.
18. The corrosion-resistant coating material has a viscosity in the range of 0 to 25°C of 1700 to 15000 mPa·s, The method for preventing corrosion of a concrete structure according to any one of claims 12 to 17, wherein the anticorrosive coating material has a thixotropic index in the range of 0 to 25°C of 3.0 or more.
19. The corrosion protection method for a concrete structure described in any one of claims 12 to 18, wherein the corrosion protection coating material is a two-component type consisting of a first corrosion protection coating material containing a polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica, and a second corrosion protection coating material containing a decomposition accelerator that accelerates decomposition of the polymerization initiator, the (meth)acrylate monomer, and the hydrophobic silica.
Citation Information
Patent Citations
Polymer cement composition
JP1991290348A
Corrosion-resistant mortar
JP2000128618A
Spraying material
JP2002293603A
Material for repairing acid resistant concrete cross section
JP2003089565A
Sulfuric acid-resistant cement composition
JP2003292362A