Resin film, laminate, and method for producing laminate

A single-layer resin film with controlled elastic properties and urethane bonds addresses the flexibility and anchoring issues of conventional films, providing durable adhesion in flexible devices.

JP7589479B2Active Publication Date: 2024-11-26TORAY INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020163366
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-11-26
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Conventional resin films used in flexible devices lack sufficient flexibility, resilience, and anchoring properties, leading to issues with peeling and inadequate performance during repeated bending and stretching operations.

Method used

A resin film with a single-layer structure and specific elastic modulus and loss tangent values, incorporating urethane bonds and controlled crosslinking to minimize internal stress differences, ensuring high flexibility and restorability while maintaining strong anchoring forces.

Benefits of technology

The resin film achieves high flexibility, resilience, and anchoring properties, preventing peeling and ensuring reliable adhesion even under repeated expansion and contraction, thereby enhancing the durability of flexible devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589479000020
    Figure 0007589479000020
  • Figure 0007589479000021
    Figure 0007589479000021
  • Figure 0007589479000022
    Figure 0007589479000022
Patent Text Reader

Abstract

To provide a resin film or a laminate having anchoring properties with an adhesive layer while maintaining high flexibility and restoring property.SOLUTION: There is provided a resin film which comprises a specific structure and a urethane bond and satisfies the following conditions 1 to 3. Condition 1: the resin film has a storage modulus at a temperature of 25°C and a frequency of 1 Hz of 0.5 mPa or more and 50 MPa or less, Condition 2: the resin film has a loss tangent at 25°C of 0.5 or less. Condition 3: the resin film is composed of a single layer in which an elastic modulus F1 (MPa) of at least one surface of the resin film and an elastic modulus F2 (MPa) of a thickness direction central portion by an atomic force microscope satisfy the expression 1: F1 / F2≤0.9 (1)SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film, a laminate, and a method for producing a laminate, which maintain high flexibility and restorability while having anchoring properties with an adhesive layer. [Background technology]

[0002] In recent years, flexible devices that can freely change shape have been actively developed. For example, displays that can be folded or rolled up have been put to practical use, and wearable sensors that can respond with high sensitivity to minute changes in pressure and strain are being developed in various fields including industry and medicine. These devices can now be attached to various objects in daily life, and are expected to fundamentally change our lives by collecting huge amounts of data and using that data to provide alarms and advice.

[0003] Various resin films have been used as the support substrate for these devices. However, conventional materials are films with rigid chemical bonds and strong crystallinity, such as polyimide, which can be bent freely but cannot be stretched. Therefore, a material that can be easily stretched and instantly restored is required as the support substrate. Furthermore, when the support substrate is modularized, it may be attached to other members. In this case, an adhesive layer is often provided between the support substrate and the other member, and the support substrate and the adhesive layer are required to have sufficient adhesion to prevent peeling, that is, the so-called "anchoring property."

[0004] As a representative example of a resin film having such high flexibility and recovery, a "resin film that maintains flexibility and high recovery while achieving both moist heat resistance and suitability for post-processing" has been proposed in Patent Document 1.

[0005] As an example of an improved flexibility, Patent Document 2 proposes a "stretch release tape with improved anchoring of the adhesive to the substrate."

[0006] Furthermore, as an example of laminating a flexible layer, Patent Document 3 proposes a "novel multi-layer laminated film which hardly scatters chemicals or additives, has improved compliance when bending or stretching, ensures stable medicinal efficacy, and leaves no adhesive residue on the adhesive layer when peeled off." [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2019-151815 A [Patent Document 2] JP 2010-189660 A [Patent Document 3] JP 2017-13306 A [Non-patent literature]

[0008] [Non-Patent Document 1] Katsuhiko Nakamae: Interfacial chemistry of the mechanism of adhesion and bonding between resin and metal, Surface Technology, Vol. 66, No. 8 (2015) Summary of the Invention [Problem to be solved by the invention]

[0009] It is important that the resin film used in the displays and sensors mentioned above does not peel off from the adhesive layer when it is "flexibly bent and stretched." Here, "flexibly bent and stretched" refers to the ability to stretch a large amount with a small force and then restore almost complete elasticity at a temperature below 0°C and at a fast cycle of more than once per second. The resin film and adhesive layer must have a strong anchoring force that is strong enough to withstand repeated stretching and contracting movements. In other words, the resin film must meet high standards in all three characteristics: flexibility, resilience, and anchoring.

[0010] In response to the above demands, the present inventors have confirmed the above-mentioned viewpoints, and have found that the material proposed in Patent Document 1 is indeed excellent in flexibility and recovery, but there is room for improvement in anchoring performance.

[0011] Furthermore, the material proposed in Patent Document 2 has excellent flexibility and anchoring properties, but its restoring properties are insufficient.

[0012] In addition, the material proposed in Patent Document 3 has excellent anchoring properties but insufficient flexibility and recovery. In addition, in comparison with the material proposed in Patent Document 1, the multilayer laminate coated with a flexible layer proposed in Patent Document 3 has excellent flexibility and recovery properties but has room for improvement in anchoring properties.

[0013] In view of the above, an object of the present invention is to provide a resin film and a laminate that maintain high flexibility and recovery while having anchoring properties with an adhesive layer. [Means for solving the problem]

[0014] As a result of intensive research conducted by the present inventors in order to solve the above problems, the present invention has been completed. That is, a preferred embodiment of the resin film, laminate, and method for producing the laminate of the present invention is as follows. (1) A resin film that meets all of the following conditions 1 to 3.

[0015] Condition 1: The storage modulus of the resin film at a temperature of 25°C and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less.

[0016] Condition 2: The loss tangent of the resin film at 25°C is 0.5 or less.

[0017] Condition 3: The resin film is composed of a single layer, and the elastic modulus F1 (MPa) of at least one surface of the resin film and the elastic modulus F2 (MPa) of the central portion in the thickness direction, measured with an atomic force microscope, satisfy formula 1.

[0018] Formula 1: F1 / F2≦0.9 (2) The resin film according to (1), which satisfies the following conditions:

[0019] Condition 4: The dissipation amount Q1 (eV) on at least one surface of the resin film and the dissipation amount Q2 (eV) at the center in the thickness direction, as measured by an atomic force microscope, satisfy formula 2.

[0020] Formula 2: Q1 / Q2≧1.2 (3) The resin film according to (1) or (2), comprising a structure of Chemical Formula 1 and a urethane bond.

[0021] [ka]

[0022] In addition, R in Chemical Formula 1 1 refers to a hydrogen or a methyl group. (4) The resin film according to (3), which satisfies the following conditions:

[0023] Condition 5: 1620 cm on at least one surface of the resin film -1 over 1640cm -1 The maximum absorbance A1 and the 1620 cm -1 over 1640cm -1 The following maximum absorbance value A2 satisfies Equation 3:

[0024] Formula 3: 1.2≦A1 / A2≦2.0 (5) A resin film according to any one of (1) to (4), which satisfies the following conditions:

[0025] Condition 6: Regarding the elastic modulus of the resin film, when the elastic moduli measured with an atomic force microscope at depths of 0% to 5%, 5% to 10%, 95% to 100%, and 90% to 95% in the thickness direction from one surface are F3, F4, F5, and F6, respectively, Equations 4 and 5, and / or Equations 6 and 7 are satisfied.

[0026] Formula 4: F4 / F2≦0.9 Formula 5: F3 / F4≦0.8 Formula 6: F6 / F2≦0.9 Formula 7: F5 / F6≦0.8 (6) A laminate having a resin film satisfying all of conditions 7 to 9 and at least another layer.

[0027] Condition 7: After removing other layers, the resin film has a storage modulus of 0.5 MPa or more and 50 MPa or less at a temperature of 25° C. and a frequency of 1 Hz.

[0028] Condition 8: The loss tangent of the resin film at 25°C after removing other layers is 0.5 or less.

[0029] Condition 9: The resin film after removing another layer is a single layer, and the elastic modulus F7 (MPa) of at least one surface of the resin film after removing another layer and the elastic modulus F8 (MPa) of the central portion in the thickness direction satisfy formula 8.

[0030] Formula 8: F7 / F8≦0.9 (7) The laminate according to (6), wherein the other layer comprises a supporting substrate. (8) The laminate according to (7), wherein the supporting substrate has a multi-layer structure and has a layer containing a polymerization inhibitor on the resin film side. (9) The laminate according to any one of (6) to (8), wherein the another layer includes an adhesive layer. (10) The method for producing a laminate according to (7), comprising carrying out steps 1, 2, and 3 in this order and satisfying condition 10. Step 1: A step of applying a coating composition containing a resin precursor containing a segment of Chemical Formula 2 and a solvent onto a supporting substrate to form a coating layer.

[0031] [ka]

[0032] Step 2: Removing the solvent from the coating layer. Step 3: A step of crosslinking the resin precursor by irradiating with active energy rays. Condition 10: In step 3, the oxygen concentration in the atmosphere during irradiation with active energy rays is 5% by volume or more. (11) The method for producing a laminate according to (10), wherein step 4 is carried out after step 3. Step 4: forming an adhesive layer. Effect of the Invention

[0033] It is possible to provide a resin film or laminate that maintains high flexibility and recovery while having anchoring properties with an adhesive layer, and a method for producing the laminate. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 3] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 4] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 5] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 6] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 7] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 8] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 9] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 10] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 11] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 12] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 13] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 14] FIG. 1 is a cross-sectional view illustrating the concept of the present invention. [Figure 15] FIG. 1 is a cross-sectional view illustrating the concept of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Before describing the modes for carrying out the present invention, the present inventors consider the reason why it is difficult to solve the problems of the present invention using conventional techniques as follows.

[0036] First, let us consider the anchoring force when bonding general dissimilar materials from the perspective of the factors involved. The factors involved in anchoring can be divided into three categories: interfacial interaction between dissimilar materials, contact surface area (anchor effect), and internal stress difference. According to Non-Patent Document 1, "apparent adhesive force = true adhesive force - residual stress". The actual adhesive force is the value obtained by subtracting the "residual stress" derived from the difference in internal stress generated to restore elastic deformation in dissimilar materials from the "true adhesive force" derived from the interfacial interaction and anchor effect. In other words, in order to strongly bond dissimilar materials, it is necessary to minimize the difference in internal stress generated in each material due to elastic deformation when bonding dissimilar materials.

[0037] Next, the adhesion between the resin film and the adhesive layer of the present invention will be considered from the above-mentioned difference in internal stress. The adhesive layer in this application is preferably at least one selected from acrylic adhesives, urethane adhesives, rubber adhesives, and silicone adhesives, and more preferably at least one selected from acrylic adhesives and urethane adhesives. These adhesive layers are flexible compared to the resin film, and are materials with small internal stress for restoring elastic deformation. On the other hand, the resin film required in this application is highly flexible, so that elastic deformation is likely to occur, and further, is highly restorable, so that the internal stress is high. Therefore, it is considered that a resin film with high flexibility and restorability is a material that is difficult to increase anchoring force, because the difference in internal stress between the resin film and the adhesive layer is large and the loss of anchoring force due to residual stress is large.

[0038] The material described in Patent Document 1 uses urethane acrylate, and is a material with high flexibility and high recovery by forming strong chemical crosslinks by acrylate crosslinks at low density within the film, rather than relying on physical crosslinks by aggregation between hard segments. Therefore, it is presumed that the reason why there is room for improvement in the anchoring properties of this material is because of the large difference in internal stress between the resin film and the adhesive layer, as discussed above.

[0039] Moreover, the material described in Patent Document 2 is a mixed composition of EVA (ethylene vinyl acetate copolymer resin) and SEBS (styrene-ethylene-butylene-styrene block copolymer). The cohesive strength depends on the π-π interaction of styrene, and since a flexible olefin is used, the material is more flexible but has lower recovery compared to the material described in Patent Document 1. Therefore, it is presumed that the reason why this material had high anchoring ability is because the difference in internal stress with the adhesive layer was reduced due to the low recovery of the resin film.

[0040] Furthermore, the material described in Patent Document 3 is a multilayer laminate in which a thin, flexible EVOH (ethylene-vinyl alcohol copolymer) layer is coated on a rigid PET substrate. Because the substrate is rigid, the flexibility and recovery of the entire resin film is low, but it is assumed that the anchoring force was high because elastic deformation is unlikely to occur when the adhesive layer is attached, and the adhesive interface with the adhesive layer is a thin layer that is flexible and has a low recovery rate.

[0041] In addition, when the flexible thin film layer described in Patent Document 3 is coated on a main material with high flexibility and resilience as in Patent Document 1, the resilience and anchoring properties change depending on the thickness of the flexible thin film layer, but there is a trade-off, and the anchoring properties are not at the level required for this application and are insufficient. The reason for this is presumed to be that the interface between the surface layer and the center layer causes a difference in internal stress within the laminate, preventing the flexible surface layer from demonstrating its potential.

[0042] In response to this, the present inventors came up with the idea of ​​solving the above-mentioned problems by gradually lowering the modulus of elasticity toward the surface side in the thickness direction of a single layer without creating an interface inside a resin film having high flexibility and resilience, thereby reducing the difference in internal stress at the resin film / adhesive layer interface without reducing the anchoring force at the interface. It was then revealed that this method can provide anchoring to the adhesive layer while maintaining high flexibility and resilience, which is the problem, and thus the present invention was arrived at. The details of the present invention are described below.

[0043] It is important that the resin film of the present invention satisfies all of the following conditions 1 to 3.

[0044] Condition 1: The storage modulus of the resin film at a temperature of 25°C and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less.

[0045] Condition 2: The loss tangent of the resin film at 25°C is 0.5 or less.

[0046] Condition 3: The resin film is composed of a single layer, and the elastic modulus F1 (MPa) of at least one surface of the resin film and the elastic modulus F2 (MPa) of the central portion in the thickness direction, measured with an atomic force microscope, satisfy formula 1.

[0047] Formula 1: F1 / F2≦0.9 (Condition 1, 2) It is important that the resin film of the present invention has a storage modulus of 0.5 MPa or more and 50 MPa or less under conditions of a temperature of 25° C. and a frequency of 1 Hz. By having a storage modulus of 0.5 MPa or more, it is possible to prevent the resin film from being too tacky and difficult to handle, and by having a storage modulus of 50 MPa or less, it is possible to make the resin film easily deformable. From the same viewpoint, it is preferably 1.0 MPa or more and 25 MPa or less, and more preferably 3.0 MPa or more and 10 MPa or less.

[0048] It is important that the resin film of the present invention has a loss tangent of 0.5 or less at 25° C. By making the loss tangent 0.5 or less, sufficient restorability can be obtained when used as a resin film. From the same viewpoint, the loss tangent of the resin film at 25° C. is preferably 0.2 or less, more preferably 0.05 or less.

[0049] The storage modulus and loss tangent refer to values ​​measured by DMA (dynamic mechanical analysis) method, and the measurement method will be described later.

[0050] The method for making the storage modulus and loss tangent of the resin film fall within the above ranges is to mix one or more polymer polyols selected from polyester polyols, polyether polyols, and polycarbonate polyols with TDI (tolylene diisocyanate), MDI (4,4'-diphenylmethane diisocyanate), NDI (1,5-naphthalene diisocyanate), TODI (tolidine diisocyanate), XDI (xylylene diisocyanate), PPDI (paraphenylene diisocyanate), TMXDI (tetramethylxylylene diisocyanate), A method of reacting one or more bifunctional isocyanates selected from HMDI (hexamethylene diisocyanate), IPDI (isophorone diisocyanate), H6XDI (hydrogenated xylylene diisocyanate), and H12MDI (dicyclohexylmethane diisocyanate) with one or more acrylic raw materials selected from HEA (hydroxyethyl acrylate) and 4HBA (4-hydroxybutyl acrylate) at a molar ratio of 1: (1-2): (0.4-1.0) and polymerizing with heat or active energy rays can be preferably used. Here, when the amount of high molecular weight polyol charged is 1 with respect to the charged molar ratio, the amount of low molecular weight polyols with a molecular weight of 500 g / mol or less, such as 1,6-hexanediol, triethylene glycol, and 3-methyl-1,5-pentanediol, is preferably 0.1 or less. Regarding the molar ratio of the charges, when the charge amount of the bifunctional isocyanate is taken as 1, the charge amount of the trifunctional or higher isocyanate is preferably 0.1 or less. In addition, the ash content in 100% by mass of the resin film is preferably 1% by mass or less. Here, the ash content refers to the components when heated at 500°C under nitrogen for 1 hour. When using a method of polymerization using active energy rays, it is preferable that the oxygen concentration of the atmosphere during polymerization is less than 5% by volume, or that the content of the polymerization initiator is 1 part by mass or more per 100 parts by mass of the entire resin.

[0051] In order to obtain a resin film having a desired storage modulus and loss tangent, it is preferable that, when the content of the monomer unit derived from the polymer polyol is taken as 1 mole, the content of the monomer unit derived from the bifunctional isocyanate is 1 to 2 moles, the content of the monomer unit derived from the acrylic raw material is 0.4 to 1.0 moles, the content of the monomer unit derived from the low molecular weight polyol is 0.1 mole or less, and the content of the monomer unit derived from the trifunctional or higher isocyanate is 0.2 moles or less. The qualitative and quantitative analysis of each monomer unit can be performed by subjecting the resin film to alkaline hydrolysis, followed by a combination of nuclear magnetic resonance spectroscopy, GC-MS, size exclusion chromatography, and time-of-flight mass spectrometry.

[0052] (Condition 3) It is important that the resin film of the present invention is composed of a single layer, and the ratio (F1 / F2) of the elastic modulus F1 (MPa) of at least one surface of the resin film to the elastic modulus F2 (MPa) of the central part in the thickness direction by atomic force microscope is 0.9 or less. Here, "composed of a single layer" means that no discontinuous boundary surface is observed when the cross section is observed by scanning electron microscope (SEM). As a specific observation method, the method described in the examples can be preferably adopted.

[0053] F1 / F2 is a parameter that represents the ratio of the elastic modulus of the inside of the resin film to that of the surface, and the smaller this value, the softer the surface of the resin film is relative to the inside of the resin film. That is, by making F1 / F2 0.9 or less, only the surface of the resin film is made soft, and the wetting and spreading of the resin film surface to the adhesive layer can be maintained, thereby improving the anchoring force. From the same viewpoint, F1 / F2 is preferably 0.8 or less, and more preferably 0.7 or less.

[0054] The resin film required for this application is one that maintains flexibility and resilience while having high anchoring power with the adhesive layer. Conditions 1 and 2 are conditions related to flexibility and resilience, respectively, and by satisfying these conditions, flexibility and resilience can be maintained at a high level. On the other hand, as mentioned above, a resin film with high flexibility and resilience has a large internal stress generated when recovering from elastic deformation, and the internal stress difference with the adhesive layer is large. In this case, the wetting and spreading at the interface between the resin film and the adhesive layer is insufficient, causing a loss of anchoring power, and the original adhesive power based on the interfacial interaction between the materials and the anchor effect cannot be exerted.

[0055] As a countermeasure, a material has been proposed in which a flexible thin film layer with low internal stress is provided on the surface of the resin film in order to reduce the difference in internal stress between the resin film and the adhesive layer. However, this creates an interface between the resin film and the thin film layer, and a loss of anchoring force occurs at this interface.

[0056] In the present invention, by satisfying condition 3 in addition to conditions 1 and 2, the resin film has flexibility and restorability, and has a structure in which the resin film is gradually flexible toward the surface side in the thickness direction in a single layer. This structure, unlike the conventional multilayer structure with a flexible thin film layer, does not have an interface inside the resin film, and loss of anchoring force can be suppressed. Furthermore, since only the surface of the resin film is flexible and has small internal stress, loss of anchoring force due to the difference in internal stress at the interface between the adhesive layer and the resin film can be suppressed as much as possible, and the anchoring force with the adhesive layer can be exhibited as it should be while maintaining flexibility and restorability.

[0057] In other words, when a conventional highly resilient film and an object to be attached are attached by applying pressure with a roll or the like as shown in Figure 14, a stretching force is applied to the highly resilient film as shown in Figure 14, and as a result, after the attachment, the highly resilient film is subjected to internal stress to restore as shown in Figure 15, which may result in peeling as shown in Figure 15.Therefore, by satisfying condition 3 in addition to conditions 1 and 2, the resin film of the present invention can alleviate the internal stress that causes the film to peel off from the object to be attached, which is caused by the high resilience of the stretch film as described above, and therefore can have excellent anchoring properties with the object to be attached.

[0058] In addition, F1 / F2 is preferably 0.01 or more. By having F1 / F2 be 0.01 or more, material destruction due to the difference in elastic modulus between the surface and the center can be prevented. From the same viewpoint, F1 / F2 is more preferably 0.1 or more, and further preferably 0.5 or more.

[0059] The ratio (F1 / F2) of the elastic modulus F1 (MPa) of the surface of a resin film to the elastic modulus F2 (MPa) of the central part in the thickness direction of the resin film using an atomic force microscope is measured using an AFM (DimensionIcon made by Burker Corporation) in PeakForceQNM mode, and the obtained force curve is analyzed based on the JKR contact theory using the attached analysis software "NanoScopeAnalysis V1.40", and the ratio can be calculated from the average value of the obtained DMT Modulus data.

[0060] Specifically, it can be determined by the following method.

[0061] A cross section is cut out of the resin film by a freezing microtome method, and the cross section is set in an AFM (DimensionIcon, manufactured by Burker Corporation) so that it becomes the measurement surface.

[0062] Following the PeakForceQNM mode manual, calibrate the cantilever's warp sensitivity, spring constant, and tip curvature, then perform measurements under the following conditions. Cantilever: Bruker AXS SCANASYST-AIR (Material: Si, spring constant K: 0.4 (N / m), tip curvature radius R: 2 (nm)) Measurement atmosphere: 23℃ in air Measurement range: 2 (μm) square Resolution: 512×512 Cantilever movement speed: 1Hz Push-in load: 4(nN).

[0063] Measurements are taken at any 30 locations from at least one surface portion of the resin film (the portion 0% deep in the thickness direction from one surface) to a depth of 5% of the entire thickness direction (however, the measurement range should be as even as possible from 0 to 5% deep in the thickness direction).

[0064] For the measurement results of each measurement range, the obtained DMT Modulus channel data was analyzed using the analysis software "NanoScope Analysis V1.40", and the Image Raw Mean value in the Results tab obtained by processing with Roughness was adopted as the elastic modulus of that measurement range, and the average value of the elastic modulus at 30 points was taken as the elastic modulus of one surface (f1a).

[0065] Using the same method as above, the elastic modulus is measured from the other surface (the portion 100% deep in the thickness direction from the one surface) to a depth of 95% in the entire thickness direction, and this is regarded as the elastic modulus of the other surface (f1b).

[0066] Furthermore, the elastic modulus is measured in the same manner as above from the portion at 45% depth to the portion at 55% depth in the thickness direction, and this is designated as the elastic modulus (F2) at the center portion in the thickness direction.

[0067] After mounting the measurement sample, a series of measurements f1a, f1b, and F2 are performed using the same sample-cantilever, without removing the sample or exchanging the cantilever midway.

[0068] For example, if either the value of f1a / F2 or the value of f1b / F2 is 0.9 or less, the ratio (F1 / F2) of the elastic modulus F1 (MPa) of at least one surface of the resin film to the elastic modulus F2 (MPa) of the central portion in the thickness direction is deemed to be 0.9 or less.

[0069] Specific preferred methods for satisfying condition 3 include a method in which the oxygen concentration is intentionally increased during crosslinking with active energy rays, thereby causing crosslinking inhibition, and a method in which the coating composition is applied to a supporting substrate containing a polymerization inhibitor, and drying and crosslinking are performed in a state in which the polymerization inhibitor has been transferred to the surface of the coating composition facing the supporting substrate. Details of these methods will be described later.

[0070] (Condition 4) The resin film of the present invention preferably satisfies condition 4.

[0071] Condition 4: The dissipation amount Q1 (eV) on at least one surface of the resin film and the dissipation amount Q2 (eV) at the center in the thickness direction, as measured by an atomic force microscope, satisfy formula 2.

[0072] Formula 2: Q1 / Q2≧1.2 Here, Q1 / Q2 is a parameter that represents the ratio of the viscosity terms inside and on the surface of the resin film. In other words, by increasing this value, only the surface of the resin film is made viscous, the difference in internal stress at the resin film / adhesive layer interface is reduced, and the anchoring force can be improved. From the same viewpoint, Q1 / Q2 is preferably 1.5 or more, and more preferably 2.0 or more.

[0073] Specifically, the surface dissipation amount of the resin film by atomic force microscope is measured in PeakForceQNM mode using AFM (DimensionIcon made by Burker Corporation) in the same manner as the above-mentioned method for measuring the elastic modulus and the ratio of the elastic modulus at the center in the thickness direction, and the obtained force curve is analyzed based on the JKR contact theory using the attached analysis software "NanoScopeAnalysis V1.40", and the average value of the obtained dispilation data can be obtained. If the dissipation amount of one surface is q1a and the dissipation amount of the other surface is q1b, and either the value of q1a / Q2 or the value of q1b / Q2 is 1.2 or more, the ratio (Q1 / Q2) of the dissipation amount Q1 (eV) of at least one surface of the resin film to the dissipation amount Q2 (eV) at the center in the thickness direction is 1.2 or more.

[0074] Specific preferred methods for satisfying condition 4 include a method in which the oxygen concentration is intentionally increased during crosslinking with active energy rays, thereby causing crosslinking inhibition, and a method in which the coating composition is applied to a supporting substrate containing a polymerization inhibitor, and drying and crosslinking are performed in a state in which the polymerization inhibitor has been transferred to the surface of the coating composition facing the supporting substrate. Details of these methods will be described later. The condition 3 focuses on the fact that the elastic modulus of the surface of the resin film is low, and the elastic restoration behavior of the surface can be suppressed. On the other hand, the condition 4 focuses on the fact that only the surface becomes viscous, and the internal stress generated by adhering the adhesive layer to the resin film is relaxed and reduced. Therefore, by satisfying the condition 4 in addition to the conditions 1 to 3, the internal stress difference at the interface between the adhesive layer and the resin film can be reduced, and the loss of anchoring property can be further suppressed.

[0075] (Material / Structure / Bond) The resin film of the present invention preferably contains one or more resins selected from acrylic resins, methacrylic resins, silicone resins, urethane resins, acrylic urethane resins, epoxy resins, and styrene resins, from the viewpoint of obtaining appropriate elasticity.

[0076] In particular, the resin film of the present invention preferably contains the structure of Chemical Formula 1 and a urethane bond.

[0077] [ka]

[0078] In addition, R in Chemical Formula 1 1 refers to a hydrogen or a methyl group.

[0079] Whether the resin film contains the above-mentioned structure or bond can be determined by various analytical methods, but the most convenient methods are FT-ATR-IR (Fourier transform attenuated total reflection infrared spectroscopy) and pyrolysis GC-MS (gas chromatography mass spectrometry). It can also be determined from the raw materials that form the resin film.

[0080] The resin film having the above structure forms a strong chemical cross-linked structure and can impart strong restoring properties. In addition, the resin film containing urethane bonds forms weak physical cross-links due to hydrogen bonds, which can impart restoring properties while maintaining flexibility.

[0081] More preferably, the structure of Chemical Formula 1 includes the structure of Chemical Formula 3.

[0082] [ka]

[0083] In addition, R in Chemical Formula 3 1 refers to a hydrogen or a methyl group.

[0084] R in Chemical Formula 3 2 refers to any of the following: - a substituted or unsubstituted alkylene group, - a substituted or unsubstituted arylene group, An alkylene group having an internal ether group, ester group, or amide group, Arylene groups having an internal ether group, ester group, or amide group, - Unsubstituted alkylene groups having an internal ether group, ester group, or amide group; An unsubstituted arylene group having an internal ether group, ester group, or amide group.

[0085] The segment formed by the urethane bond preferably includes a structure represented by Chemical Formula 4.

[0086] [ka]

[0087] In addition, R in Chemical Formula 4 3 refers to any of the following: - a substituted or unsubstituted alkylene group, Substituted or unsubstituted arylene groups.

[0088] In addition, it is preferable for the resin film of the present invention to contain 30% by mass or more of an acrylic urethane resin based on 100% by mass, from the viewpoint of obtaining a high level of flexibility and restorability.

[0089] (Condition 5) The resin film of the present invention preferably satisfies condition 5.

[0090] Condition 5: 1620 cm on at least one surface of the resin film -1 over 1640cm -1 The maximum absorbance A1 and the 1620 cm -1 More than 1420cm -1 The following maximum absorbance value A2 satisfies Equation 3:

[0091] Formula 3: 1.2≦A1 / A2≦2.0 Here, A1 / A2 is a parameter indicating the amount of acrylic residue on the surface relative to the entire resin film, and this value is preferably 1.2 or more and 2.0 or less, and more preferably 1.4 or more and 1.8 or less.

[0092] By setting A1 / A2 to 1.2 or more, UV curing originating from the acrylic group on the surface alone can be suppressed, improving anchoring power. Also, by setting A1 / A2 to 2.0 or less, high recovery can be achieved.

[0093] The absorbance at the surface is the absorbance obtained by cutting a cross section by a freezing microtome method and measuring the FT-IR spectrum by the KBr method for a region from one surface to a depth of 0% to 5% or 95% to 100% in the thickness direction, and the absorbance at the center in the thickness direction is the absorbance obtained by measuring the FT-IR spectrum by the KBr method for a region from a depth of 45% to 55% in the thickness direction. Specifically, it can be measured by the method in the Examples.

[0094] The maximum absorbance on one surface is a1a and the maximum absorbance on the other surface is a1b. If either the value of a1a / A2 or the value of a1b / A2 is 1.2 or more and 2.0 or less, then the ratio (A1 / A2) of the maximum absorbance A1 on at least one surface of the resin film to the maximum absorbance A2 at the center in the thickness direction is 11.2 or more and 2.0 or less.

[0095] Specific preferred methods for satisfying condition 5 include a method in which the oxygen concentration is intentionally increased during crosslinking with active energy rays, thereby causing crosslinking inhibition, and a method in which the coating composition is applied to a supporting substrate containing a polymerization inhibitor, and drying and crosslinking are performed in a state in which the polymerization inhibitor has been transferred to the surface of the coating composition on the supporting substrate side. Details of these methods will be described later.

[0096] (Condition 6) The resin film of the present invention preferably satisfies condition 6.

[0097] Condition 6: Regarding the elastic modulus of the resin film, when the elastic moduli measured with an atomic force microscope at depths of 0% to 5%, 5% to 10%, 95% to 100%, and 90% to 95% in the thickness direction from one surface are F3, F4, F5, and F6, respectively, Equations 4 and 5, and / or Equations 6 and 7 are satisfied.

[0098] Formula 4: F4 / F2≦0.9 Formula 5: F3 / F4≦0.8 Formula 6: F6 / F2≦0.9 Formula 7: F5 / F6≦0.8 Here, F3, F4, F5, and F6 are parameters that further subdivide the elastic modulus of the resin film surface, and F3 is a parameter that represents the elastic modulus of the portion closer to the surface than F4, and F6 is a parameter that represents the elastic modulus of the portion closer to the surface than F5. That is, satisfying formula 4 and formula 5, and / or formula 6 and formula 7 indicates that the elastic modulus changes continuously toward the surface side in the thickness direction, and the structure becomes gradually more flexible. As an effect of this, there is no boundary surface where the elastic modulus changes suddenly in the thickness direction, and the anchoring force with the adhesive layer can be exerted as it should be without generating "residual stress" derived from the difference in internal stress. From the same viewpoint, it is preferable that F4 / F2 is 0.8 or less and F3 / F4 is 0.75 or less, and more preferably that F4 / F2 is 0.75 or less and F3 / F4 is 0.70 or less. Moreover, it is preferable that F5 / F2 is 0.8 or less, and F6 / F5 is 0.75 or less, and more preferably, F5 / F2 is 0.75 or less, and F6 / F5 is 0.70 or less. Each measurement can be performed in the same manner as the measurement of F1 / F2.

[0099] (Example 1 of a specific method for satisfying conditions 3 to 6: oxygen concentration) As a specific method for satisfying condition 3, a method of intentionally increasing the oxygen concentration during crosslinking by active energy rays to cause crosslinking inhibition can be preferably adopted. Specifically, a method of crosslinking a formulation containing a crosslinking component by active energy rays with active energy rays at an oxygen concentration in the range of 5% by volume to 20% by volume can be mentioned. From the viewpoint of reaction efficiency, the formulation preferably has a structure as shown in Chemical Formula 1, and more preferably has an acrylic group. From the viewpoint of versatility, the active energy rays are preferably electron beams (EB) and / or ultraviolet rays (UV), and more preferably ultraviolet rays. Examples of the type of ultraviolet lamp used for irradiating ultraviolet rays include discharge lamp type, flash type, laser type, and electrodeless lamp type. When ultraviolet curing is performed using a high-pressure mercury lamp of the discharge lamp type, the illuminance of the ultraviolet rays is 100 to 3,000 (mW / cm 2 ), and more preferably 200 to 2,000 (mW / cm 2 ), and more preferably 300 to 1,500 (mW / cm 2 ), and the integrated amount of ultraviolet light is 100 to 3,000 (mJ / cm 2 ), and more preferably 200 to 2,000 (mJ / cm 2 ), and more preferably 300 to 1,500 (mJ / cm 2 ) is the condition where the ultraviolet irradiance is the irradiation intensity per unit area, which varies depending on the lamp output, emission spectrum efficiency, diameter of the light-emitting bulb, design of the reflector, and the distance between the irradiated object and the light source. However, the irradiance does not vary depending on the conveying speed. The integrated ultraviolet light amount is the irradiation energy per unit area, which is the total amount of photons that reach the surface. The integrated light amount is inversely proportional to the irradiation speed passing under the light source, and proportional to the number of irradiations and the number of lamps. The oxygen partial pressure during active energy ray irradiation is measured using a zirconia oxygen concentration meter. The oxygen partial pressure is adjusted by adjusting the partial pressure of the inert gas in the active energy ray irradiation environment.

[0100] (Example 2 of a specific method for satisfying conditions 3 to 6: Polymerization inhibitor) As a specific method for satisfying condition 3, a method can be preferably adopted in which a coating composition is applied to a support substrate containing a polymerization inhibitor, and the polymerization inhibitor is transferred to the support substrate side surface of the coating composition, and then drying and crosslinking are performed in that state. Specific examples of the polymerization inhibitor include 4-methoxyphenol, 4-dimethyl-6-t-butylphenol, 2-hydroxy-1,4-naphthoquinone, 4-methoxy-1-naphthol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, 2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl acrylate, and 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diylbis[3-(dodecylthio)propionate. Those having a hydroxy group are preferred, and 2-hydroxy-1,4-naphthoquinone is more preferred. These may be used alone or in combination of two or more. Polymerization inhibitors having a hydroxyl group are likely to form hydrogen bonds with the urethane groups of the resin film, and therefore have high migration properties to the surface of the resin film, and can efficiently inhibit the UV curing reaction of the acrylic groups.

[0101] The polymerization inhibitor is preferably added to the resin layer of the supporting substrate in order to improve migration to the resin film surface, and more preferably to the release layer, which is a resin layer containing silicone. The amount of the polymerization inhibitor added is preferably 20 to 40 parts by mass relative to 100 parts by mass of the resin in the resin layer of the supporting substrate.

[0102] (Another layer) The laminate of the present invention is preferably a laminate having a resin film that satisfies all of conditions 7 to 9 and at least another layer. Condition 7: After removing other layers, the resin film has a storage modulus of 0.5 MPa or more and 50 MPa or less at a temperature of 25° C. and a frequency of 1 Hz. Condition 8: The loss tangent of the resin film at 25°C after removing other layers is 0.5 or less. Condition 9: The resin film after removing another layer is a single layer, and the elastic modulus F7 (MPa) of at least one surface of the resin film after removing another layer and the elastic modulus F8 (MPa) of the central portion in the thickness direction satisfy formula 8.

[0103] Formula 8: F7 / F8≦0.9 Here, the other layer is any layer, and the other layer may satisfy conditions 7 to 9.

[0104] The other layers include a supporting substrate for ensuring processability and transportability in subsequent processes, an adhesive layer or bonding layer for bonding to different materials, a particle layer, a colored layer or a design layer for changing the surface characteristics or optical characteristics of the resin film, an electronic circuit layer for processing the resin film, a printed layer, and the like.

[0105] Methods for removing the other layer include chemical etching, freeze microtome, and freeze polishing, with the freeze polishing method being preferred from the viewpoint of simplicity. In addition, whether the other layer has been removed can be confirmed by observing whether a discontinuous boundary surface is observed when observing the cross section with a scanning electron microscope (SEM).

[0106] (Supporting base material) The laminate of the present invention is preferably a laminate including a resin film and a supporting substrate, an example of which is shown in FIG.

[0107] The supporting substrate herein refers to an article that is flat in the in-plane direction and on whose surface the resin film-forming coating composition described below can be spread.

[0108] The reason why it is preferable to provide a supporting substrate in the laminate of the present invention is that in the method of producing a resin film described below, a liquid coating composition is applied onto the supporting substrate and crosslinked to form a resin film, and this ensures processability and transportability in subsequent processes in which the resin film is processed.

[0109] When the resin film is peeled off from the supporting substrate and post-processed as a single unit, it is preferable that the laminate 4 has a supporting substrate 7 including a release layer 6 between the resin film 5 as shown in FIG.

[0110] When the laminate is wound into a roll to produce an intermediate product, the laminate 8 may have a support substrate 11 including a release layer 10 on the side opposite to the resin film 9, as shown in Fig. 3, in order to stabilize the rolled appearance. Of course, the laminate 12 may have a release layer 14 between the resin film 13 and a support substrate 16 including a release layer 15 on the opposite side, as shown in Fig. 4. In this case, the release layers 14 and 15 may be the same, but it is preferable that they are different because it is necessary to adjust the peeling force between the resin film 9 and the release layer 15 when the laminate is unwound from the roll, and the peeling force between the resin film 13 and the release layer 14 in a later process.

[0111] In order to improve the transportability of the resin film in the process and prevent scratches, the laminate 17 may have a peelable support substrate 19 on one side of the resin film 18 and a peelable protective material 20 on the other side as shown in FIG. 5. The protective material and the support substrate may be the same, but the laminate 21 may have a support substrate 24 including a release layer 23 between the resin film 22 and a protective material 25 as shown in FIG. 6, the laminate 26 may have a support substrate 29 including a release layer 28 between the resin film 27 and a protective material 31 including a release layer 30 as shown in FIG. 7, and the laminate 32 may have a support substrate 35 including a release layer 34 between the resin film 33 and a protective material 37 including an adhesive layer 36 as shown in FIG. 8. Whether the laminate has a protective material having an adhesive layer or a protective material using a release layer is appropriately selected based on the suitability of the subsequent process and the physical properties of the resin film.

[0112] In addition, when the resin film is not peeled off from the supporting substrate and the laminate of the supporting substrate and the resin film is subjected to post-processing, it is preferable that the laminate 38 has a supporting substrate 41 including an adhesive layer 40 described later between the supporting substrate 41 and the resin film 39 as shown in FIG. 9.

[0113] When the laminate is wound into a roll to produce an intermediate product, in order to stabilize the rolled shape, the laminate 42 may have an adhesive layer 44 between the resin film 43 and the supporting substrate, as shown in Figure 10, and may have a supporting substrate 46 including a release layer 45 on the side of the supporting substrate opposite the resin film.

[0114] In order to improve the transportability of the resin film in the process and prevent scratches, as shown in FIG. 11, a laminate 47 may have a support substrate 50 having an adhesive layer 49 on one side of a resin film 48 and a peelable protective material 51 on the other side. The protective material and the support substrate may be the same, but as shown in FIG. 12, a laminate 52 may have a support substrate 55 including an adhesive layer 54 between the resin film 53 and a protective material 57 including a release layer 56, and as shown in FIG. 13, a laminate 58 may have a support substrate 61 including an adhesive layer 60 between the resin film 59 and a protective material 63 including an adhesive layer 62. Whether the laminate has a protective material having an adhesive layer or a protective material using a release layer is appropriately selected based on the suitability of the subsequent process and the physical properties of the resin film.

[0115] (Support substrate containing polymerization inhibitor) In the laminate of the present invention, the supporting substrate has a multi-layer structure, and preferably has a layer containing a polymerization inhibitor on the resin film side. By adopting this embodiment, the anchoring property of the surface of the resin film on the supporting substrate side can be increased.

[0116] Specific examples of the polymerization inhibitor used in the present invention include 4-methoxyphenol, 4-dimethyl-6-t-butylphenol, 2-hydroxy-1,4-naphthoquinone, 4-methoxy-1-naphthol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, 2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl acrylate, and 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diylbis[3-(dodecylthio)propionate. Those having a hydroxy group are preferred, and 2-hydroxy-1,4-naphthoquinone is more preferred. These may be used alone or in combination of two or more. Polymerization inhibitors having a hydroxyl group are likely to form hydrogen bonds with the urethane groups of the resin film, and therefore have high migration properties to the surface of the resin film, and can efficiently inhibit the UV curing reaction of the acrylic groups. The polymerization inhibitor is preferably added to the resin layer in order to improve migration to the resin film surface, and more preferably to the release layer, which is a resin layer containing silicone. The amount of the polymerization inhibitor added is preferably 20 parts by mass to 40 parts by mass relative to 100 parts by mass of the resin. In particular, the amount of the polymerization inhibitor added is preferably 20 parts by mass to 30 parts by mass so as not to excessively inhibit polymerization.

[0117] (Adhesive layer) The laminate of the present invention preferably includes a resin film and an adhesive layer. Here, the adhesive layer refers to a layer having an adhesive strength of 3N / 20mm or more to a SUS304 plate at 23°C, a peel speed of 300mm / min, and a peel angle of 180°. From the viewpoint of suppressing peeling during high expansion and contraction or during processing, the adhesive layer is preferably at least one selected from acrylic adhesives, urethane adhesives, rubber adhesives, and silicone adhesives, and more preferably at least one selected from acrylic adhesives and urethane adhesives.

[0118] In addition, in the method for producing a resin film of the present invention, it is preferable that steps 1, 2, and 3 are carried out in this order and condition 10 is satisfied. Step 1: A step of applying a coating composition containing a resin precursor containing a segment of Chemical Formula 2 onto a supporting substrate to form a coating layer.

[0119] [ka]

[0120] R 4 refers to a hydrogen or a methyl group. R 5 is preferably any one of the following, and n is preferably an integer of 3 or more. Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group. R 6 is preferably one of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. Step 2: Removing the solvent from the coating layer. Step 3: A step of crosslinking the resin precursor by irradiating with active energy rays. Condition 10: In step 3, the oxygen concentration in the atmosphere during irradiation with active energy rays is 5% by volume or more.

[0121] By using the resin precursor with the above structure and setting the oxygen concentration in the atmosphere at the time of irradiation with active energy rays to 5% by volume or more, oxygen inhibition of the crosslinking reaction can be intentionally induced only on the surface, thereby reducing the elastic modulus of the surface and improving the anchoring property.

[0122] The support substrate is a substrate for improving transportability and preventing scratches, and may be a multi-layer laminate including a release layer and an adhesive layer. By including a release layer, it becomes possible to peel off from the support substrate, and the resin film alone can be post-processed. In addition, by including an adhesive layer, it is strongly adhered to the support substrate, and the laminate of the support substrate and the resin film can be post-processed.

[0123] In condition 10, the oxygen concentration in the atmosphere during irradiation with active energy rays is more preferably 10% by volume or more, and even more preferably 20% by volume or more. By making the oxygen concentration 10% by volume or more, the curing reaction caused by active energy rays can be intentionally inhibited, and the anchoring ability of the resin film on the side opposite to the support substrate can be increased.

[0124] [Mode of the present invention] Hereinafter, the embodiment of the present invention will be described in detail.

[0125] [Resin film] The resin film of the present invention has a film-like structure formed by a single layer. Here, the layer refers to a portion having a boundary surface distinguishable from adjacent portions in the thickness direction and having a finite thickness. More specifically, when the cross section of the resin film is observed with an electron microscope (transmission type, scanning type) or an optical microscope, it refers to a portion that is distinguished by the presence or absence of a discontinuous boundary surface. Even if the composition changes in the thickness direction of the resin film, if there is no boundary surface between them, it is treated as a single layer.

[0126] The resin film of the present invention may have other functions such as concealment, gloss, fingerprint resistance, moldability, design, scratch resistance, antifouling, solvent resistance, antireflection, antistatic, electrical conductivity, heat ray reflection, near infrared absorption, electromagnetic wave shielding, easy adhesion, etc., in addition to the intended flexibility, recovery, and anchoring properties, and may further have one or more layers formed thereon to form a laminate. For example, a functional layer, an adhesive layer, an electronic circuit layer, a printing layer, an optical adjustment layer, or other functional layers may be provided.

[0127] The thickness of the resin film is not particularly limited and is appropriately selected depending on the application. The lower limit of the thickness of the resin film is not generally determined because it is affected by the elastic modulus, breaking elongation, peeling force and peeling angle between the support substrate and the resin film, etc., but when the same physical properties as those of a general flexible material are realized using the manufacturing method of the laminate described later, the lower limit is about several μm.

[0128] [Laminate] Preferred embodiments of the laminate of the present invention are as described above, but it is preferable that the laminate has a supporting substrate on at least one side of a resin film exhibiting the above-mentioned physical properties, and the laminate may be in a planar state or may have a three-dimensional shape after molding.

[0129] [Supporting base material] The supporting substrate used in the laminate of the present invention may be either a thermoplastic resin or a thermosetting resin, and may be a homogeneous resin, a copolymer, or a blend of two or more kinds. The resin constituting the supporting substrate is preferably one having good moldability, and from this point of view, a thermoplastic resin is more preferable.

[0130] Examples of thermoplastic resins that can be suitably used for the supporting substrate include polyolefin resins such as polyethylene, polypropylene, polystyrene, and polymethylpentene, alicyclic polyolefin resins, polyamide resins such as nylon 6 and nylon 66, aramid resins, polyimide resins, polyester resins, polycarbonate resins, polyarylate resins, polyacetal resins, polyphenylene sulfide resins, fluororesins such as tetrafluoroethylene resin, trifluoroethylene resin, trifluorochloroethylene resin, tetrafluoroethylene-hexafluoropropylene copolymer, and vinylidene fluoride resin, acrylic resins, methacrylic resins, polyacetal resins, polyglycolic acid resins, and polylactic acid resins.

[0131] Examples of thermosetting resins suitable for use in the support substrate include phenol resin, epoxy resin, urea resin, melamine resin, unsaturated polyester resin, polyurethane resin, polyimide resin, silicone resin, etc. The thermoplastic resin is preferably a resin having sufficient stretchability and conformability. From the viewpoints of strength, heat resistance, and transparency, the thermoplastic resin is more preferably a polyester resin, a polycarbonate resin, an acrylic resin, or a methacrylic resin.

[0132] The polyester resin preferably used for the support substrate is a general term for polymers having an ester bond as the main bond in the main chain, and is obtained by polycondensation of an acid component and its ester with a diol component. Specific examples include polyethylene terephthalate, polypropylene terephthalate, polyethylene-2,6-naphthalate, and polybutylene terephthalate. These may also be copolymerized with other dicarboxylic acids and their esters or diol components as the acid component or diol component. Among these, polyethylene terephthalate and polyethylene-2,6-naphthalate are particularly preferred in terms of transparency, dimensional stability, heat resistance, and the like.

[0133] In addition, the supporting substrate may contain various additives, such as an antioxidant, an antistatic agent, a crystal nucleating agent, inorganic particles, organic particles, a viscosity reducer, a heat stabilizer, a lubricant, an infrared absorber, an ultraviolet absorber, and a dopant for adjusting the refractive index.

[0134] Furthermore, the supporting substrate may have either a single layer structure or a laminate structure.

[0135] In addition, a functional layer such as an easy-adhesion layer, an antistatic layer, an undercoat layer, an ultraviolet absorbing layer, or a release layer may be provided in advance on the surface of the supporting substrate in addition to the resin film of the present invention, and the laminate of the present invention preferably has a release layer in order to reduce the peeling force between the supporting substrate and the resin film. The details of the release layer will be described later.

[0136] Examples of supporting substrates provided with a release layer include "Therapeel" (registered trademark) manufactured by Toray Advanced Film Co., Ltd., "Unipeel" (registered trademark) manufactured by Unitika Ltd., "Panapeel" (registered trademark) manufactured by Panac Corporation, "Toyobo Ester" (registered trademark) manufactured by Toyobo Co., Ltd., and "Purex" (registered trademark) manufactured by Teijin Limited, and these products can also be used.

[0137] The surface of the supporting substrate may be subjected to various surface treatments before forming the resin film. Examples of the surface treatments include chemical treatment, mechanical treatment, corona discharge treatment, flame treatment, ultraviolet irradiation treatment, high frequency treatment, glow discharge treatment, active plasma treatment, laser treatment, mixed acid treatment, and ozone oxidation treatment. Among these, glow discharge treatment, ultraviolet irradiation treatment, corona discharge treatment, and flame treatment are preferred, and glow discharge treatment and ultraviolet treatment are more preferred.

[0138] [Release layer] In the laminate of the present invention, when the resin film alone is post-processed, it is preferable that the support substrate has a release layer as described above. A support substrate having a release layer is also called a release film. The release layer may be composed of multiple layers from the viewpoint of imparting adhesion, antistatic properties, solvent resistance, etc., and may be present on both sides of the support substrate.

[0139] The composition and thickness of the release layer are preferably from 10 to 500 nm, more preferably from 20 to 300 nm, in terms of the in-plane uniformity of the release layer, the appearance quality, and the peeling force.

[0140] [Protective material] The laminate of the present invention may have a protective material on the surface of the resin film opposite to the supporting substrate as shown in FIG. 5. The protective material and the supporting substrate are distinguished in that, in the manufacturing method of the laminate, the one to which the coating composition is applied is the supporting substrate, and the one to which the resin film is laminated after formation is the protective material. The protective material may be the same as or different from the supporting substrate described above, but it is preferable that the protective material has a different peeling force from the supporting substrate described above when used in a later process. The magnitude relationship between the peeling force of the protective material and the supporting substrate from the resin film is appropriately selected depending on the method of use in the later process. Therefore, the protective material may have a release layer as shown in FIGS. 7 and 12, may have an adhesive layer as shown in FIGS. 8 and 13, or may not have a layer as shown in FIGS. 6 and 11.

[0141] [Manufacturing method of resin film] In the method for producing the resin film of the present invention, a coating composition containing a resin precursor having a segment of chemical formula 2 is applied onto a supporting substrate to form a coating layer (step 1), the solvent is then removed from the coating layer and the coating layer is dried (step 2), and the resin precursor is crosslinked by irradiating with active energy rays to produce a laminate (step 3).

[0142] The method of applying the coating composition onto the supporting substrate in step 1 is not particularly limited as long as the coating composition can be applied onto the supporting substrate to form a uniform coating layer in the plane. The coating method onto the film can be appropriately selected from a dip coating method, a roller coating method, a wire bar coating method, a gravure coating method, a die coating method (US Pat. No. 2,681,294), and the like. Here, the coating layer refers to a "liquid layer" formed by the coating step.

[0143] The method for removing the solvent in step 2, i.e., the drying method, is not particularly limited as long as it can remove the solvent from the coating layer formed on the support substrate. Drying methods include heat transfer drying (contact with a high-heat object), convection heat transfer (hot air), radiation heat transfer (infrared rays), and others (microwaves, induction heating), and among these, in the manufacturing method of the present invention, a method using convection heat transfer or radiation heat transfer is preferred because it is necessary to precisely make the drying speed uniform even in the width direction.

[0144] The crosslinking method in step 3 involves irradiating the coating layer from which the solvent has been removed after drying with active energy rays to cause a reaction and crosslink the coating film.

[0145] Crosslinking by active energy rays is preferably performed using electron beams (EB) and / or ultraviolet rays (UV) from the viewpoint of versatility. Examples of the type of ultraviolet lamp used for irradiating ultraviolet rays include discharge lamp type, flash type, laser type, and electrodeless lamp type. When ultraviolet curing is performed using a high-pressure mercury lamp, which is a discharge lamp type, the illuminance of the ultraviolet rays is 100 to 3,000 (mW / cm 2 ), and more preferably 200 to 2,000 (mW / cm 2 ), and more preferably 300 to 1,500 (mW / cm 2 ), and the integrated amount of ultraviolet light is 100 to 3,000 (mJ / cm 2 ), and more preferably 200 to 2,000 (mJ / cm 2 ), and more preferably 300 to 1,500 (mJ / cm 2 ) where UV illuminance is the radiation intensity received per unit area, and varies with lamp output, emission spectral efficiency, diameter of the light-emitting bulb, design of the reflector, and the distance between the irradiated object and the light source. However, illuminance does not vary with transport speed. Additionally, the integrated UV light quantity is the radiation energy received per unit area, and is the total amount of photons that reach the surface. The integrated light quantity is inversely proportional to the radiation speed passing under the light source, and proportional to the number of irradiations and the number of lamps. The oxygen partial pressure during irradiation with active energy rays is measured using a zirconia oxygen concentration meter. The oxygen partial pressure is adjusted by adjusting the irradiation partial pressure of the inert gas in the active energy ray irradiation environment.

[0146] [Resin precursor] The resin precursor is not particularly limited as long as it is a compound having a site that can be crosslinked, but A resin precursor containing the structure of Chemical Formula 2 is preferred, and a resin precursor containing the structure of Chemical Formula 5 is more preferred.

[0147] [ka]

[0148] [ka]

[0149] R 4 and R 7 refers to a hydrogen or a methyl group. R 5 , R 8 , and R 10 is preferably any one of the following, and n is preferably an integer of 3 or more. Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group. R 6 , R 9 is preferably one of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups.

[0150] As described above, the structures of Chemical Formulae 2 and 5 have a (meth)acrylic group, indicated by X in the diagram, at the end, and this (meth)acrylic group (X) at the end corresponds to a site that can be crosslinked. Furthermore, the (meth)acrylic group (X) is adjacent to a polyisocyanate residue, indicated by Y in the diagram. Furthermore, the segment of Chemical Formula 2 means that the other end of the polyisocyanate residue, indicated by Y, is adjacent to a polyol residue, indicated by Z in Chemical Formula 5, indicated by Z.

[0151] The polyisocyanate residue (Y) of Chemical Formulas 2 and 5 is preferably a residue of a polyisocyanate such as TDI (tolylene diisocyanate), MDI (4,4'-diphenylmethane diisocyanate), NDI (1,5-naphthalene diisocyanate), TODI (tolidine diisocyanate), XDI (xylylene diisocyanate), PPDI (paraphenylene diisocyanate), TMXDI (tetramethylxylylene diisocyanate), HMDI (hexamethylene diisocyanate), IPDI (isophorone diisocyanate), H6XDI (hydrogenated xylylene diisocyanate), or H12MDI (dicyclohexylmethane diisocyanate).

[0152] The polyol residue of Chemical Formula 5 is preferably a polyester polyol, a polyether polyol, or a polycarbonate polyol.

[0153] [Paint composition] The "coating composition" used in the method for producing the laminate of the present invention is not particularly limited as long as it can be uniformly applied on the surface of the supporting substrate and can form a resin film exhibiting the characteristics of the present invention, but it is preferable that the coating composition is suitable for the method for producing the laminate described above. Specifically, it is preferable to prepare the coating composition by adding the resin precursor described above to the solvent and other components described below.

[0154] [solvent] The coating composition used in the method for producing the laminate of the present invention may contain a solvent, and it is preferable to contain a solvent in order to form a coating layer uniformly in the plane. The number of types of solvents is preferably 1 to 20, more preferably 1 to 10, even more preferably 1 to 6, and particularly preferably 1 to 4. Here, the term "solvent" refers to a substance that is liquid at room temperature and normal pressure and can be evaporated almost entirely in the drying process described above.

[0155] Here, the type of solvent is determined by the molecular structure that constitutes the solvent. In other words, solvents that have the same elemental composition and the same type and number of functional groups but different bond relationships (structural isomers), and solvents that are not structural isomers but do not overlap exactly in any conformation in three-dimensional space (stereoisomers) are treated as different types of solvents. For example, 2-propanol and n-propanol are treated as different solvents.

[0156] [Other components in the coating composition] The coating composition used in the method for producing the laminate of the present invention preferably contains an antioxidant, a polymerization initiator, a curing agent, and a catalyst. The polymerization initiator and catalyst are used to promote crosslinking of the resin film. The polymerization initiator is preferably one that can initiate or promote polymerization, condensation, or crosslinking reaction of the components contained in the coating composition by anionic, cationic, or radical polymerization reaction, etc.

[0157] Antioxidants are roughly classified into radical chain initiation inhibitors, radical scavengers, and peroxide decomposers based on their mechanism of action. Any of these can provide the effects of the present invention in terms of inhibiting deterioration under high temperature conditions, but radical scavengers or peroxide decomposers are more preferred, and hindered phenol-based and semi-hindered phenol-based radical scavengers, or phosphite-based and thioether-based peroxide decomposers are more preferred.

[0158] Various polymerization initiators, curing agents, and catalysts can be used. The polymerization initiators, curing agents, and catalysts may be used alone, or multiple polymerization initiators, curing agents, and catalysts may be used simultaneously. Furthermore, an acid catalyst or a thermal polymerization initiator may be used in combination. Examples of acid catalysts include hydrochloric acid aqueous solution, formic acid, and acetic acid. Examples of thermal polymerization initiators include peroxides and azo compounds. Examples of photopolymerization initiators include alkylphenone compounds, sulfur-containing compounds, acylphosphine oxide compounds, and amine compounds. Examples of crosslinking catalysts that promote the reaction of forming urethane bonds include dibutyltin dilaurate and dibutyltin diethylhexoate.

[0159] As the photopolymerization initiator, it is preferable to use an alkylphenone compound or an acylphosphine oxide compound from the viewpoint of curability. Furthermore, it is more preferable to use an alkylphenone compound having a hydroxyethoxy group introduced therein from the viewpoint of wet heat resistance. Specific examples of alkylphenone compounds include 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-phenyl)-1-butane, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-(4-phenyl)-1-butane, 2-benzyl-2-dimethylamino-1-(4- morpholinophenyl)-1-butane, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butane, 1-cyclohexyl-phenyl ketone, 2-methyl-1-phenylpropan-1-one, 1-[4-(2-ethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, bis(2-phenyl-2-oxoacetate)oxybisethylene, and materials that have been made into high molecular weights. Specific examples of acylphosphine oxide compounds include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and materials that have been made into high molecular weights. These may be used alone or in combination of two or more.

[0160] In addition, a leveling agent, a lubricant, an antistatic agent, etc. may be added to the coating composition used to form the resin film as long as the effects of the present invention are not impaired. As a result, the resin film can contain the leveling agent, the lubricant, the antistatic agent, etc.

[0161] Examples of the leveling agent include acrylic copolymers, silicone-based, and fluorine-based leveling agents. Examples of the antistatic agent include metal salts such as lithium salts, sodium salts, potassium salts, rubidium salts, cesium salts, magnesium salts, and calcium salts.

[0162] [Application example] The resin film of the present invention has advantages such as excellent optical properties, flexibility, stretchability, transportability, and appearance quality, and can be suitably used in applications where particularly high flexibility and stretchability are required.

[0163] For example, the resin film can be suitably used for the surface, internal, structural, and manufacturing process materials of plastic molded products such as glasses / sunglasses, cosmetic cases, and food containers, aquariums, showcases for exhibitions, smartphone housings, touch panels, color filters, flat panel displays, flexible displays, flexible devices, wearable devices, sensors, circuit materials, electrical and electronic applications, home appliances such as keyboards, television and air conditioner remote controls, mirrors, window glass, buildings, dashboards, car navigation touch panels, vehicle parts such as room mirrors and windows, and various printed matter, medical films, sanitary material films, medical films, agricultural films, building material films, etc. The quality of these materials can be improved by using the resin film of the present invention. EXAMPLES

[0164] Next, the present invention will be described based on examples, but the present invention is not necessarily limited to these.

[0165] "Synthesis of resin precursors" In the synthesis of the resin precursor, the raw materials used are as follows:

[0166] "Diisocyanate" IPDI: Isophorone diisocyanate "Polyol" PBAA-1: Polybutylene adipate, Tosoh Corporation, Nipponran 3027 (weight average molecular weight 2500) "Hydroxy acrylate (HEA)" 4HBA: 4-Hydroxybutyl acrylate [Resin precursor A] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, IPDI as a diisocyanate, PBAA-1 as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.43:0.29, and the solid content concentration was set to 60% by mass. The reaction was carried out at 90°C, and when the remaining isocyanate groups in the unreacted state were taken as 100% by mass, the temperature was lowered to 70°C when the remaining isocyanate groups became 1.4% by mass due to the reaction, and hydroxyacrylate (HEA) was added. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate in the unreacted state was set to 0.43:0.29:0.29. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of Resin Precursor A.

[0167] [Resin precursor B] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, IPDI as a diisocyanate, PBAA-1 as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.48:0.32, and the solid content concentration was set to 60% by mass. The reaction was carried out at 90°C, and when the remaining isocyanate groups in the unreacted state were taken as 100% by mass, the temperature was lowered to 70°C when the remaining isocyanate groups became 1.4% by mass due to the reaction, and hydroxyacrylate (HEA) was added. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate in the unreacted state was set to 0.48:0.32:0.20. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of resin precursor B.

[0168] [Resin precursor C] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, IPDI as a diisocyanate, PBAA-1 as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.38:0.27, and the solid content concentration was set to 60% by mass. The reaction was carried out at 90°C, and when the remaining isocyanate groups in the unreacted state were taken as 100% by mass, the temperature was lowered to 70°C when the remaining isocyanate groups became 1.4% by mass due to the reaction, and hydroxyacrylate (HEA) was added. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate in the unreacted state was set to 0.38:0.27:0.35. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of resin precursor C.

[0169] [Paint composition formulation] [Paint composition 1] The following materials were diluted with methyl ethyl ketone to obtain a resin film-forming coating composition 1 having a solid content concentration of 40 mass %. Resin precursor A: 100 parts by weight Photopolymerization initiator “IRGACURE” (registered trademark) 184 (manufactured by BASF Japan Ltd.): 3 parts by mass. Fluorine-based leveling agent “Ftergent” (registered trademark) 650AC (manufactured by NEOS Corporation): 0.03 parts by mass.

[0170] [Preparation of coating compositions 2 to 6] Coating compositions 2 to 6 were prepared by changing the resin precursor type, the amount of photopolymerization initiator, and the solids concentration in the formulation of coating composition 1 to the combinations shown in Table 1.

[0171] [Table 1]

[0172] [7. Preparation of coating composition] Hydrogenated styrene-based thermoplastic elastomer ("SOE" (registered trademark) S1606 manufactured by Asahi Kasei Corporation) was dissolved in toluene to obtain coating composition 7 having a solids concentration of 40 mass %.

[0173] [8. Preparation of coating composition] An EVOH resin (EVAL (registered trademark) EP-E105 manufactured by Kuraray Co., Ltd.) was dissolved in a 35% water-containing normal propanol solution to obtain a coating composition 8 having a solids concentration of 10 mass %.

[0174] [Release layer coating composition] The following materials were mixed and diluted with a mixed solvent of methyl ethyl ketone / isopropyl alcohol (mixture ratio by mass: 50 / 50) to obtain a coating composition for a release layer having a solids concentration of 5% by mass. Side-chain carbinol modified reactive silicone oil (X-22-4015 Shin-Etsu Chemical Co., Ltd. Solid content: 100% by mass): 5 parts by mass ·Both-end polyether modified reactive silicone oil (X-22-4952 Shin-Etsu Chemical Co., Ltd. Solid content: 100% by mass): 5 parts by mass Acrylic modified alkyd resin solution (Hariftar KV-905, Harima Chemicals Co., Ltd., solid content concentration 53% by mass): 100 parts by mass Isobutyl alcohol modified melamine resin solution “Melan” (registered trademark) 2650L Hitachi Chemical Co., Ltd. Solid content concentration 60% by mass: 20 parts by mass · Paratoluenesulfonic acid: 5 parts by weight.

[0175] The above materials were used as the basic materials for the coating composition for the release layer, and 30 parts by mass of the additives described below were added in some cases. "Additives" Polymerization inhibitor A: Quinone-based polymerization inhibitor "Kinopower" (registered trademark) QS-20 (manufactured by Kawasaki Chemical Industries, Ltd.) (2-hydroxy-1,4-naphthoquinone) Polymerization inhibitor B: Acrylate group-containing phenolic polymerization inhibitor "SUMILIZER" (registered trademark) GM (manufactured by Sumitomo Chemical Co., Ltd.) (2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl acrylate) [Method of manufacturing laminate and resin film] [Formation of Support Substrate with Release Layer] Using a coating device with a small-diameter gravure coater, the coating composition for the release layer was applied to a polyester film (manufactured by Toray Industries, Inc., trade name "Lumilar" (registered trademark) R75X) having a thickness of 50 μm by adjusting the line number of the gravure roll, the peripheral speed of the gravure roll, and the solid content concentration of the coating composition for the release layer so that the thickness of the release layer would be about 200 nm, and then the film was held at a hot air temperature of 140° C. for 30 seconds to dry and crosslink, thereby obtaining support substrates 1 to 4 with release layers. The combination of additives was as shown in Table 2.

[0176] [Table 2]

[0177] [Method of forming laminate] (Process 1) The support substrate with the release layer described above was used as the support substrate, and the coating composition described above was applied onto the release layer of the support substrate using a continuous coating device with a slot die coater, with the discharge flow rate adjusted so that the thickness of the resin film after crosslinking would be the specified film thickness, to form a coating layer.

[0178] (Process 2) The coating layer formed in step 1 was dried under the following conditions to remove the solvent.

[0179] Air blowing temperature: Temperature: 50℃, Wind speed: Coating side: 5m / sec, non-coating side: 5m / sec Air flow direction: Coating side: Parallel to the surface of the substrate, Non-coating side: Perpendicular to the surface of the substrate Dwell time: 2 minutes (Step 3) In step 2, the coating layer (uncrosslinked resin film) obtained by removing the solvent was crosslinked by irradiating it with active energy rays under the conditions described below to obtain a laminate consisting of a supporting substrate, a release layer and a resin film.

[0180] Irradiation light source: High pressure mercury lamp Irradiation power: 400W / cm 2 Accumulated light output: 120mJ / cm 2 Oxygen concentration: 0.1% by volume, 2% by volume, 5% by volume, or 21% by volume When the resin film was to have a multi-layer structure, the above-mentioned coating composition was applied again onto the laminate consisting of the supporting substrate, release layer and resin film prepared in step 3 using a continuous coating device, and steps 1 to 3 were repeated to obtain a multi-layer resin film laminate.

[0181] In addition, in Comparative Examples 11 and 12, various coating compositions were applied to a polyester film having a thickness of 50 μm (manufactured by Toray Industries, Inc., under the trade name "Lumirror" (registered trademark) R75X), and the laminate obtained by carrying out steps 1 to 3 was regarded as a multilayer resin film and evaluated.

[0182] By the above-mentioned method, laminates and resin films were prepared in Examples 1 to 13 and Comparative Examples 1 to 10. Table 3 shows the coating composition for forming a resin film, the type of support substrate with a release layer, the method for forming the laminate, and the thickness of each resin film corresponding to each Example and Comparative Example.

[0183] [Table 3]

[0184] [Evaluation of resin film] The resin film was subjected to the following performance evaluations, and the results are shown in Table 4. When the laminate was made of a resin film and a supporting substrate, and the supporting substrate could be easily peeled off from the resin film, the substrate was peeled off to obtain a measurement sample. When the laminate was made of a resin film and another layer, and the other layer could not be easily peeled off, the laminate was frozen with liquid nitrogen, and the other layer was polished to prepare several samples. The sample with a single layer of resin film was used as the measurement sample according to the method described in the section on observation of the thickness and number of layers of the resin film below. Unless otherwise specified, measurements were performed three times for one sample in each Example and Comparative Example at different locations, and the average value was used.

[0185] [Measurement of storage modulus and loss tangent of resin film] The measurement sample was cut into a rectangular shape with a width of 10 mm to prepare a test piece.

[0186] Based on the tensile vibration-non-resonance method of JIS K7244-4 (1999) (this is called the dynamic viscoelasticity method), the storage modulus and loss tangent of the resin film were determined using a dynamic viscoelasticity measuring device DMS6100 manufactured by Seiko Instruments Inc. Measurement mode: Tensile Chuck distance: 20mm Test piece width: 10mm Frequency: 1Hz Distortion amplitude: 10μm Minimum tension: 20mN Initial force amplitude: 40mN Measurement temperature: -100℃ to 200℃ Heating rate: 5℃ / min [Measurement of elastic modulus and dissipation amount of resin film] A cross section was cut out of the measurement sample by a freezing microtome method, and the cross section was set in an AFM (DimensionIcon, manufactured by Burker Corporation) so that it became the measurement surface.

[0187] Following the PeakForceQNM mode manual, the cantilever's warping sensitivity, spring constant, and tip curvature were calibrated, and measurements were then performed under the following conditions. Cantilever: Bruker AXS SCANASYST-AIR (Material: Si, spring constant K: 0.4 (N / m), tip curvature radius R: 2 (nm)) Measurement atmosphere: 23℃ in air Measurement range: 2 (μm) square Resolution: 512×512 Cantilever movement speed: 1Hz Push-in load: 4(nN).

[0188] Measurements were taken at 30 random locations from at least one surface portion of the resin film (the portion 0% deep in the thickness direction from one surface) to a depth of 5% of the entire thickness direction (however, measurements were taken as evenly as possible from 0 to 5% deep in the thickness direction).

[0189] For the measurement results of each measurement range, the obtained DMT Modulus channel data was analyzed using the analysis software "NanoScope Analysis V1.40", and the Image Raw Mean value in the Results tab obtained by processing with Roughness was adopted as the elastic modulus of that measurement range, and the average value of the elastic modulus at 30 points was taken as the elastic modulus of one surface (f1a).

[0190] Using the same method as above, the elastic modulus was measured from the other surface (the portion 100% deep in the thickness direction from the one surface) to a depth of 95% in the entire thickness direction, and this was designated as the elastic modulus of the other surface (f1b).

[0191] Furthermore, the elastic modulus was measured in the same manner as above from the 45% to 55% depth in the thickness direction, and this was taken as the elastic modulus (F2) of the central portion in the thickness direction.

[0192] In addition, using a similar method, each dissipation amount was calculated using the data from the Dispilation channel. [Measurement of infrared absorption spectrum of resin film] The FT-IR spectrum of the resin film was measured by the KBr method on the surface and at the center in the thickness direction.

[0193] A portion of the resin film was sliced ​​from one surface to a depth of 0% to 5% in the thickness direction, then freeze-pulverized, mixed with KBr powder, and molded into tablets to obtain a measurement sample.

[0194] The measuring device and conditions are as follows.

[0195] Measurement equipment: Varian FT-IR Varian-670 Measurement conditions: Light source: Special ceramics Detector DTGS Resolution 4cm -1 Accumulation count: 128 Measurement wave number range: 4,000~680cm -1 .

[0196] Similarly, measurements were taken at a portion from 45% to 55% of the thickness in the thickness direction, and in addition, measurements were taken at a portion from 95% to 100% of the thickness in the thickness direction.

[0197] From the spectrum obtained, 1620 cm -1 over 1640cm -1The following minimum values ​​of transmittance (resin film surface: A1, resin film thickness direction central portion: A2) were determined.

[0198] [Observation of resin film thickness and number of layers] The thickness and number of layers of the resin film were observed by cross-sectional SEM observation of the film using a SEM JSM-6700F manufactured by JEOL Ltd. The procedure for preparing test pieces for cross-sectional SEM observation was as follows.

[0199] 1. The resin film was embedded in UV-curable resin.

[0200] 2. The resin film was cut together with the embedded resin using a rotary microtome RMS manufactured by Nippon Microtome Co., Ltd. to obtain a cross section through the thickness of the resin film.

[0201] 3. Using an Auto Fine Coater JFC-1600 manufactured by JEOL Ltd., platinum was deposited to a thickness of approximately 10 μm on the cut cross section of the sample (conditions: 30 mA x 20 seconds x 2 times) to prepare a test piece.

[0202] The cross-sectional SEM observation was performed under the following conditions. Measurement mode: LEI mode ·Magnification: 5000x Acceleration voltage: 3kV WD (sample distance): 8.0mm The thickness of the resin film was calculated from the vertical distance between the embedded resins in the cross-sectional SEM images, and the arithmetic mean value was used. The number of layers of the resin film was calculated from the number of discontinuous interfaces between the embedded resins in the vertical direction in the cross-sectional SEM images.

[0203] [Evaluation of resin film flexibility] The resin film was cut into a rectangle measuring 10 mm wide x 150 mm long to prepare a test piece. The direction of the 150 mm long was aligned with the longitudinal direction of the resin film. Using a tensile tester (Orientec Tensilon UCT-100), the initial tensile chuck distance was set to 50 mm, the tensile speed was set to 300 mm / min, and the measurement temperature was set to 23°C.

[0204] Read the load b (N) applied to the sample when the chuck distance is a (mm), and use the following formula to calculate the strain x (%) and stress y (N / mm 2 ) was calculated, where k (mm) is the sample thickness before the test. Strain amount: x = ((a-50) / 50) x 100 Stress: y=b / (k×10).

[0205] Of the data obtained above, the stress at a strain of 5% was defined as the 5% strain stress, and a value of 5 MPa or less was deemed acceptable.

[0206] When the longitudinal direction was unknown, samples were taken in any direction, and then rotated 60 degrees and 120 degrees to take samples again. Evaluation was based on the average value of the measurement results for a total of three samples.

[0207] [Evaluation of Resin Film Restoration] The resin film was cut into a rectangle of 10 mm width x 150 mm length to prepare a test piece. The direction of the 150 mm length was aligned with the longitudinal direction of the resin film. Using a tensile tester (Orientec "Tensilon" (registered trademark) UCT-100), evaluation was performed at a measurement temperature of 23°C under two conditions with different deformation speeds to determine the superiority or inferiority of the restoring property.

[0208] Condition A: Initial chuck distance 50 mm, tensile speed 50 mm / min. After stretching the sample to 100% strain, the tensile load on the sample was released, and the distance marked as the initial test length before the measurement was measured and taken as L mm. The elastic recovery rate z was calculated using the following formula: 1 (%) and shear rate s 1 (s -1 ) was calculated.

[0209] Elastic recovery rate z 1 =(1-(L-50) / 100)×100 (%).

[0210] Shear rate s 1 =(50 / 60) / 10=0.08(s -1 ) Condition B: Initial chuck distance 50 mm, tensile speed 300 mm / min. After stretching the sample to 100% strain, the tensile load on the sample was released, and the distance marked as the initial test length before the measurement was measured and defined as L mm. The elastic recovery rate z was calculated from the following formula. 1 The percentage was calculated.

[0211] Elastic recovery rate z 2 =(1-(L-50) / 100)×100 (%).

[0212] Shear rate s 1 =(50 / 60) / 10=0.08(s -1 ) In the above evaluation, condition A was considered to be 90% or more and condition B was 70% or more, respectively, to be a pass.

[0213] [Evaluation of anchoring properties of resin film] The anchoring property was evaluated by the resistance value (N) when the adhesive film was peeled off from the elastic film at 180 degrees using a tensile tester "Tensilon" (registered trademark) UCT-100 manufactured by Orientec Co., Ltd. After cutting the resin film into a strip (25 mm x 120 mm), the adhesive layer side of an adhesive film ("PanaProtect" (registered trademark) manufactured by Panac Corporation (product number: HUCB Type2, size: 20 mm x 100 mm)) was attached to the surface of the resin film to be evaluated. Next, Nitto double-sided tape (product number: 5000NS) was attached to the other surface of the resin film, the support substrate of the double-sided tape was peeled off, and the adhesive film was attached to a stainless steel plate. Finally, a part of the adhesive layer / resin film interface of the adhesive film was peeled off, fixed to a load cell with tape, and measured under the following conditions. 6N or more was considered to be a pass.

[0214] Measurement distance: 50mm or more Test piece width: 20mm Peel speed: 300 mm / min (Pulling speed: 600 mm / min) Peel angle: 180° Tables 4 and 5 show the structure and urethane bond of the resin film of chemical formula 1, the presence / absence of chemical formula 2, and the evaluation results under the above-mentioned conditions 1 to 6, while Table 6 shows the results of the flexibility, recovery, and anchoring property of the resin film.

[0215] [Table 4]

[0216] [Table 5]

[0217] [Table 6]

[0218] In Table 4, "includes" in the column for the structure of Chemical Formula 1 means that each Example contains the structure of Chemical Formula 1, and "does not include" means that each Example does not contain the structure of Chemical Formula 1. The same applies to the urethane bond. [Explanation of symbols]

[0219] 1, 4, 8, 12, 17, 21, 26, 32, 38, 42, 47, 52, 58, 64, 71: Laminate 2, 5, 9, 13, 18, 22, 27, 33, 39, 43, 48, 53, 59, 65, 72: Resin film 6, 10, 14, 15, 23, 28, 30, 34, 45, 56: Release layer 3, 7, 11, 16, 19, 24, 29, 35, 41, 46, 50, 55, 61, 66, 73: Supporting base material 20, 25, 31, 37, 51, 57, 63, 68, 75: Protective material 36, 40, 44, 49, 54, 60, 62, 67, 74: Adhesive layer 69: Lamination roll 70, 76: Internal stress [Industrial Applicability]

[0220] The resin film of the present invention has advantages such as excellent optical properties, flexibility, stretchability, transportability, and appearance quality, and can be suitably used in applications where particularly high flexibility and stretchability are required.

[0221] To name a few examples, it can be suitably used for the surface materials, internal materials, constituent materials, and manufacturing process materials of plastic molded products such as glasses / sunglasses, cosmetic cases, and food containers, aquariums, showcases for exhibitions, smartphone housings, touch panels, color filters, flat panel displays, flexible displays, flexible devices, wearable devices, sensors, circuit materials, electrical and electronic applications, home appliances such as keyboards, remote controls for televisions and air conditioners, mirrors, window glass, buildings, dashboards, car navigation touch panels, vehicle parts such as rearview mirrors and windows, and various printed matter, medical films, films for sanitary materials, medical films, agricultural films, and building materials.

Claims

1. A resin film that satisfies all of the following conditions 1 to 3 and condition P, and includes a structure shown in Chemical Formula 1 and a structure shown in Chemical Formula 4. Condition 1: The storage modulus of the resin film at a temperature of 25° C. and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less. Condition 2: The loss tangent of the resin film at 25° C. is 0.5 or less. Condition 3: The resin film is composed of a single layer, and the elastic modulus F1 (MPa) of at least one surface of the resin film and the elastic modulus F2 (MPa) of the central portion in the thickness direction, as measured by an atomic force microscope, satisfy Formula 1. Formula 1: F1 / F2≦0.9 【Chemistry 1】 In addition, R 1 in Chemical Formula 1 represents hydrogen or a methyl group. 【Chemistry 2】 In addition, R 3 in Chemical Formula 4 represents any one of the following. - a substituted or unsubstituted alkylene group, A substituted or unsubstituted arylene group. Condition P: The resistance value when the pressure-sensitive adhesive film is peeled off from the resin film at an angle of 180 degrees is 6 N or more, as determined by the anchoring property evaluation method for resin films described below. (Method for evaluating anchoring properties of resin film) The adhesive film is peeled off from the resin film at an angle of 180 degrees using a tensile tester "Tensilon" (registered trademark) UCT-100 manufactured by Orientec Co., Ltd., and the resistance value (N) is evaluated. After cutting the resin film into a rectangular shape (25 mm x 120 mm), the adhesive layer side of an adhesive film (PANAC Corporation's "PanaProtect" (registered trademark) (product number: HUCB Type 2, size: 20 mm x 100 mm)) is attached to the resin film. Next, Nitto's double-sided tape (product number: 5000NS) is attached to the other side of the resin film, the support substrate of the double-sided tape is peeled off, and the adhesive film is attached to a stainless steel plate. Finally, a part of the adhesive layer / resin film interface of the adhesive film is peeled off and fixed to a load cell with tape, and measurements are performed under the following conditions. Measurement distance: 50mm or more Test piece width: 20 mm Peel speed: 300 mm / min (pulling speed: 600 mm / min) Peel angle: 180°

2. The resin film according to claim 1 , which satisfies the following conditions: Condition 4: The amount of dissipation Q1 (eV) on at least one surface of the resin film and the amount of dissipation Q2 (eV) at the center in the thickness direction, as measured by an atomic force microscope, satisfy Expression 2. Formula 2: Q1 / Q2≧1.2

3. The resin film according to claim 1 or 2, which satisfies the following conditions: Condition 5: 1620 cm on at least one surface of the resin film -1 1640cm or more -1 The maximum absorbance A1 below and 1620 cm -1 1640cm or more -1 The following maximum absorbance value A2 satisfies Equation 3: Formula 3: 1.2≦A1 / A2≦2.0

4. The resin film according to claim 1 , which satisfies the following conditions: Condition 6: Regarding the elastic modulus of the resin film, when the elastic moduli measured with an atomic force microscope at depths of 0% to 5%, 5% to 10%, 95% to 100%, and 90% to 95% in the thickness direction from one surface are designated as F3, F4, F5, and F6, respectively, Equations 4 and 5, and / or Equations 6 and 7 are satisfied. Formula 4: F4 / F2≦0.9 Formula 5: F3 / F4≦0.8 Formula 6: F6 / F2≦0.9 Formula 7: F5 / F6≦0.8

5. A laminate having a resin film that satisfies all of Conditions 7 to 9 and Condition P and contains a structure of Chemical Formula 1 and a structure shown in Chemical Formula 4, and at least another layer, wherein the another layer includes a supporting substrate, the supporting substrate has a multi-layer structure, and the supporting substrate has a layer containing a polymerization inhibitor on the resin film side. Condition 7: The storage modulus of the resin film after removing other layers at a temperature of 25° C. and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less. Condition 8: The loss tangent of the resin film at 25° C. after removing other layers is 0.5 or less. Condition 9: The resin film after removing another layer is a single layer, and the elastic modulus F7 (MPa) of at least one surface of the resin film after removing another layer and the elastic modulus F8 (MPa) of the central portion in the thickness direction satisfy formula 8. Formula 8: F7 / F8≦0.9 【Chemistry 3】 In addition, R 1 in Chemical Formula 1 represents hydrogen or a methyl group. 【Chemistry 4】 In addition, R 3 in Chemical Formula 4 represents any one of the following. - a substituted or unsubstituted alkylene group, A substituted or unsubstituted arylene group. Condition P: The resistance value when the pressure-sensitive adhesive film is peeled off from the resin film at an angle of 180 degrees is 6 N or more, as determined by the anchoring property evaluation method for resin films described below. (Method for evaluating anchoring properties of resin film) The adhesive film is peeled off from the resin film at an angle of 180 degrees using a tensile tester "Tensilon" (registered trademark) UCT-100 manufactured by Orientec Co., Ltd., and the resistance value (N) is evaluated. After cutting the resin film into a rectangular shape (25 mm x 120 mm), the adhesive layer side of an adhesive film (PANAC Corporation's "PanaProtect" (registered trademark) (product number: HUCB Type 2, size: 20 mm x 100 mm)) is attached to the resin film. Next, Nitto's double-sided tape (product number: 5000NS) is attached to the other side of the resin film, the support substrate of the double-sided tape is peeled off, and the adhesive film is attached to a stainless steel plate. Finally, a part of the adhesive layer / resin film interface of the adhesive film is peeled off and fixed to a load cell with tape, and measurements are performed under the following conditions. Measurement distance: 50mm or more Test piece width: 20 mm Peel speed: 300 mm / min (pulling speed: 600 mm / min) Peel angle: 180°

6. The laminate of claim 5 , wherein the additional layer comprises an adhesive layer.

7. The method for producing a laminate according to claim 5 , wherein steps 1, 2, and 3 are carried out in this order and condition 10 is satisfied. Step 1: A step of applying a coating composition containing a resin precursor containing a segment of Chemical Formula 2 and a solvent onto a supporting substrate to form a coating layer. 【Chemistry 5】 Step 2: Removing the solvent from the coating layer. Step 3: A step of crosslinking the resin precursor by irradiating with active energy rays. Condition 10: In step 3, the oxygen concentration in the atmosphere during irradiation with active energy rays is 5% by volume or more.

8. The method for producing a laminate according to claim 7 , wherein step 4 is carried out after step 3 . Step 4: forming an adhesive layer.

Citation Information

Patent Citations

  • Manufacture of decorative material

    JP1984199249A

  • Method for manufacturing color filter and semi-transmissive liquid crystal display device using color filter manufactured by the method

    JP2008197494A

  • Sulfur-containing multi-branched compound and unsaturated group-containing multi-branched compound

    JP2008208324A

  • Oriented release tape

    JP2010189660A

  • Multilayer laminate film and manufacturing method therefor

    JP2017013306A