Polyamide yarn for thermal bonding and its manufacturing method
The aliphatic copolymer polyamide yarn, through controlled monomer composition and processing, stabilizes the crystal structure to maintain high-order processability and adhesive strength despite long-term storage, addressing the limitations of conventional yarns.
Patent Information
- Application Number
- JP2020180234
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Conventional polyamide yarns, such as highly oriented undrawn yarns and aliphatic copolymerized yarns, suffer from unstable crystal structures and significant decreases in strength and elongation after long-term storage, leading to inferior high-order processability and adhesive strength.
An aliphatic copolymer polyamide yarn formed by copolymerizing three or more monomers, with specific monomer compositions and processing conditions including stretching and heat setting, to stabilize the crystal structure and maintain high-order processability and adhesive strength.
The polyamide yarn achieves stable high-order processability and excellent adhesive strength even after long-term storage, with controlled crystal structure and low melting point for easy thermal bonding at low temperatures.
Smart Images

Figure 0007589501000001
Abstract
Description
[Technical field]
[0001] To provide a polyamide yarn for thermal bonding which is excellent for bonding mainly fiber materials by melting it through heat treatment, and which is particularly easy to melt at low temperatures and has excellent high-level processability even after long-term storage. [Background technology]
[0002] Polyamide yarns, such as polycaproamide and polyhexamethylene adipamide, have excellent mechanical properties and dimensional stability, and are therefore widely used not only for clothing applications but also for interior and vehicle interiors and industrial applications.
[0003] In addition to the above-mentioned applications, copolymer polyamide yarns having a specific melting point can be melted by heat treatment and suitably used as hot-melt adhesives for bonding mainly fibrous materials.
[0004] For example, a highly oriented undrawn yarn that is composed of a copolymer polyamide containing three or more copolymer components and has excellent processability and strength has been proposed (Patent Document 1).
[0005] In addition, an aliphatic copolyamide yarn containing three or more copolymer components that melts easily even at low temperature and has excellent adhesive strength has been proposed (Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-113730 A [Patent Document 2] JP 2010-189806 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the highly oriented undrawn yarn described in Patent Document 1 has not undergone a drawing process, and therefore although it is said to be highly oriented, the crystal structure of the yarn is unstable, and the strength and elongation of the yarn decrease significantly after long-term storage. As a result, the high-level processability after long-term storage is inferior.
[0008] Regarding the aliphatic copolyamide yarn described in Patent Document 2, an example of a drawn yarn is given, and the crystal structure of the yarn is more stable than that of the highly oriented undrawn yarn described in Patent Document 1. However, even in this example, the decrease in the strength and elongation of the yarn after long-term storage was not suppressed, and as a result, the high-order processability after long-term storage was inferior.
[0009] The present invention aims to provide a polyamide yarn for thermal bonding that has stable high-order processability even after long-term storage, which was difficult to achieve with conventional techniques, and also has excellent adhesive strength, and a method for producing the same. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention employs the following configuration. (1) A polyamide yarn for thermal bonding which is an aliphatic copolyamide obtained by copolymerizing three or more types of monomers and contains monomers constituting an aliphatic polyamide, and has an elongation of 50 to 90% and a heat of fusion of 10 to 50 J / g.
[0011] (2) The polyamide yarn for thermal bonding according to (1) above, which is a multifilament yarn having a single yarn fineness of 0.5 to 10 dtex.
[0012] (3) The polyamide yarn for thermal bonding according to (1) or (2) above, having a melting point of 80 to 140°C, a hot water shrinkage rate of 10 to 50%, and a strength of 2.5 to 4.0 cN / dtex.
[0013] (4) The polyamide yarn for thermal bonding according to any one of (1) to (3) above, wherein the aliphatic copolyamide contains a monomer (A) constituting polycaproamide and a monomer (B) constituting polyhexamethylene adipamide, and the total content of the monomer (A) and the monomer (B) is 40 to 70% by weight of the aliphatic copolyamide.
[0014] (5) The polyamide yarn for thermal bonding according to any one of (1) to (4) above, wherein the aliphatic copolyamide contains a monomer (C) constituting polydodecanamide, and the content of the monomer (C) is 5 to 40% by weight of the aliphatic copolyamide.
[0015] (6) A sewing thread having in a part thereof the polyamide thread for thermal bonding according to any one of (1) to (5) above.
[0016] (7) A mall yarn having, in a part thereof, the polyamide yarn for thermal bonding according to any one of (1) to (5) above.
[0017] (8) A thermal bonding tape having in a part thereof the thermal bonding polyamide yarn according to any one of (1) to (5) above.
[0018] (9) A method for producing a polyamide yarn for thermal bonding according to any one of the above (1) to (5), which is made of an aliphatic copolyamide obtained by copolymerizing three or more kinds of monomers including a monomer constituting an aliphatic polyamide, and which comprises drawing at a draw ratio of 1.5 to 3.5 times, and then heat setting at a temperature 10°C lower than the melting point of raw material pellets of the aliphatic copolyamide to below the melting point. Effect of the Invention
[0019] According to the present invention, it is possible to provide a polyamide yarn for thermal bonding having excellent high-order processability and adhesive strength. Furthermore, it is possible to provide a polyamide yarn for thermal bonding having stable high-order processability even after long-term storage by controlling the crystal structure of the polyamide yarn for thermal bonding through drawing and heat setting and stabilizing the fiber structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The polyamide thread for thermal bonding of the present invention is made of an aliphatic copolyamide. The aliphatic copolyamide used in the present invention is a resin made of a high molecular weight substance in which so-called hydrocarbons are linked to the main chain via amide bonds, and does not contain monomers having a cyclic structure such as aromatic or alicyclic as a copolymerization component. By making it have such a structure, the aliphatic copolyamide can have a low melting point, so that it melts completely even with relatively low temperature heat such as from an iron, and can exhibit excellent adhesive strength even when used, for example, as a tape for hemming trousers.
[0021] The polyamide thread for thermal bonding of the present invention is an aliphatic copolyamide thread containing a monomer constituting an aliphatic polyamide, which is an aliphatic copolyamide obtained by copolymerizing three or more kinds of monomers, preferably four or more kinds of monomers. By making it into such a structure, the aliphatic copolyamide can have a low melting point, so that it melts completely even with relatively low temperature heat such as with an iron, and can exhibit excellent adhesive strength even when used, for example, as a trouser hemming tape. When the number of monomers to be copolymerized is two or less, the melting point of the aliphatic copolyamide becomes high, and not only cannot maintain adhesive strength, but also it becomes difficult to perform thermal bonding with relatively low temperature heat such as with an iron.
[0022] Monomers constituting aliphatic copolyamides include aminocarboxylic acids and lactams (6-aminocaproic acid, ε-caprolactam, 11-aminoundecanoic acid, undecalactam, 12-aminododecanoic acid, dodecalactam, etc.) constituting polycaproamide, polyundecaneamide, polydodecaneamide, etc., and salts in which equimolar amounts of dicarboxylic acids and diamines are bonded to polytetramethylene adipamide, polypentamethylene adipamide, polypentamethylene sebacamide, polyhexamethylene adipamide, polyhexamethylene sebacamide, polyhexamethylene dodecaneamide, polyhexamethylene tridecanamide, etc.
[0023] The monomers constituting the aliphatic copolyamide preferably include a monomer (A) constituting polycaproamide and a monomer (B) constituting polyhexamethylene adipamide, and the total content of the monomers (A) and (B) is preferably 40 to 70% by weight of the aliphatic copolyamide. When the total content is 40% by weight or more, the combination of other monomers constituting the aliphatic copolyamide increases the strength and elongation of the thermal bonding polyamide yarn of the present invention, and when subjected to high-level processing, there is little occurrence of fluff or thread breakage, enabling stable high-level processability. When the total content is 70% by weight or less, the combination of other monomers constituting the aliphatic copolyamide makes the melting point of the thermal bonding polyamide yarn of the present invention 140°C or less, and the yarn is completely melted even by relatively low-temperature heat such as an iron, and can exhibit excellent adhesive strength even when used, for example, as a trouser hemming tape.
[0024] The monomers constituting the aliphatic copolyamide include a monomer (C) constituting polydodecanamide, and the content of the monomer (C) is preferably 5 to 40% by weight of the aliphatic copolyamide. When the content is 5% by weight or more, the melting point of the thermal bonding polyamide yarn of the present invention becomes 140°C or less depending on the combination of other monomers constituting the aliphatic copolyamide, and the yarn melts completely even at relatively low temperatures such as with an iron, and can exhibit excellent adhesive strength even when used as a trouser hemming tape, for example. When the content is 40% by weight or less, the melting point of the thermal bonding polyamide yarn of the present invention becomes 80°C or more depending on the combination of other monomers constituting the aliphatic copolyamide, and the yarn is particularly resistant to temperature changes such as high temperatures, and can be stably processed even after long-term storage.
[0025] The polyamide yarn for thermal bonding of the present invention may contain various additives within a range that does not impair the effects of the present invention. Examples of such additives include stabilizers such as manganese compounds, colorants such as titanium oxide, flame retardants, conductivity imparting agents, fibrous reinforcing agents, etc. However, when inorganic particles such as titanium oxide are added in large amounts, the adhesive strength tends to decrease, and the preferred range of the content of inorganic particles is 0 to 0.1% by weight.
[0026] The polyamide yarn for thermal bonding of the present invention has an elongation of 50 to 90%, preferably 60 to 80%. By setting the elongation within this range, the crystal structure of the polyamide yarn for thermal bonding is stabilized, so that stable high-order processing is possible even after long-term storage. In addition, the flexibility of the polyamide yarn for thermal bonding can be maintained, so that stable high-order processing is possible, particularly in applications that go through a twisting process such as sewing thread, in which twisting is easy to be introduced and there is no fuzz. If the elongation is less than 50%, the flexibility of the polyamide yarn for thermal bonding cannot be maintained, and particularly in applications that go through a twisting process such as sewing thread, twisting becomes extremely difficult, so fuzz is generated, making stable high-order processing difficult. If the elongation exceeds 90%, the crystal structure of the polyamide yarn for thermal bonding is not stable, so that the strength and elongation of the yarn decrease significantly after long-term storage, and as a result, stable high-order processing after long-term storage becomes difficult.
[0027] The heat of fusion of the polyamide yarn for thermal bonding of the present invention is 10 to 50 J / g. It is preferably 15 to 50 J / g. The heat of fusion is the amount of heat required when a substance undergoes a phase transition from solid to liquid. For crystalline polymers such as polyamides, the heat of fusion and the crystal structure are closely related, and the higher the heat of fusion, the more stable the crystal structure. It is generally known that various properties such as strength and elongation of polyamide yarns are affected by the crystal structure. However, for aliphatic (multi-element) copolymer polyamide yarns such as the polyamide yarn for thermal bonding of the present invention, the changes in various properties over time are greater than those of general polyamide yarns that are not copolymerized, and control of the crystal structure is extremely important. By setting the heat of fusion, which is closely related to the crystal structure, within this range, the crystal structure of the polyamide yarn for thermal bonding is stabilized, and stable high-order processing is possible even after long-term storage. If the heat of fusion is less than 10 J / g, the crystal structure of the polyamide yarn for thermal bonding is not stable, and the strength and elongation of the yarn after long-term storage is significantly reduced, which results in difficulty in stable high-level processing after long-term storage. Of course, the higher the heat of fusion, the better as long as the elongation of the polyamide yarn for thermal bonding is within the desired range and does not impair the effects of the present invention. However, if an attempt is made to obtain a heat of fusion of more than 50 J / g, the elongation of the polyamide yarn for thermal bonding of the present invention is likely to be less than 50%, which results in the inability to maintain the flexibility of the polyamide yarn for thermal bonding. In particular, in applications that go through a twisting process, such as sewing threads, the twisting becomes extremely difficult, which causes fluffing and makes stable high-level processing difficult.
[0028] The total fineness and the number of single filaments of the polyamide yarn for thermal bonding of the present invention are not particularly limited as long as the effects of the present invention are not impaired. However, it is preferable that the total fineness is 10 to 400 dtex and the number of filaments is 2 to 150.
[0029] The polyamide yarn for thermal bonding of the present invention is preferably a multifilament having a single yarn fineness of 0.5 to 10 dtex. More preferably, it is a multifilament having a single yarn fineness of 1 to 5 dtex. The polyamide yarn for thermal bonding of the present invention may be in the form of a monofilament, but when the total fineness of the polyamide yarn for thermal bonding is large, the single yarn fineness also becomes large, so that it does not melt completely with relatively low temperature heat such as an iron, and when used for, for example, hemming tape for trousers, the adhesive strength becomes poor. In this case, it is sufficient to make the single yarn fineness thin by making it in the form of a multifilament. When the single yarn fineness is 0.5 dtex or more, the strength of the single yarn is high, and when subjected to high-level processing, there is little occurrence of fluff or yarn breakage, and stable high-level processability is possible. When the single yarn fineness is 10 dtex or less, each single yarn comes into contact with each other in close contact and melts completely uniformly, so that excellent adhesive strength can be expressed.
[0030] The polyamide yarn for thermal bonding of the present invention preferably has a melting point of 80 to 140°C. More preferably, it is 90 to 120°C. When the melting point is 80°C or higher, it is particularly resistant to temperature changes such as high temperatures, and stable high-level processing is possible even after long-term storage. When the melting point is 140°C or lower, it is completely melted even by relatively low-temperature heat such as that of an iron, and excellent adhesive strength can be exhibited even when used, for example, as a tape for hemming trousers.
[0031] The hot water shrinkage of the polyamide yarn for thermal bonding of the present invention is preferably 10 to 50%, more preferably 15 to 45%. The hot water temperature is 35°C. If the hot water shrinkage is 50% or less, the crystal structure of the polyamide yarn for thermal bonding is stabilized, so that stable high-order processing is possible even after long-term storage. Of course, the lower the hot water shrinkage, the better as long as it does not impair the effects of the present invention. However, in consideration of the properties of aliphatic copolyamides and the manufacturing process of the polyamide yarn for thermal bonding, it is difficult to obtain one with a shrinkage of less than 10%.
[0032] The polyamide yarn for thermal bonding of the present invention preferably has a strength of 2.5 to 4.0 cN / dtex. More preferably, it is 3.0 to 4.0 cN / dtex. If the strength is 2.5 cN / dtex or more, there is little occurrence of fluff or yarn breakage when subjected to advanced processing, and stable advanced processability is possible. Of course, the higher the strength, the better as long as it does not impair the effects of the present invention. However, in consideration of the properties of the aliphatic copolyamide and the manufacturing process of the polyamide yarn for thermal bonding, if the strength exceeds 4.0 cN / dtex, it becomes difficult to keep the elongation in the desired range.
[0033] The cross-sectional shape of the polyamide yarn for thermal bonding of the present invention may be appropriately selected according to the required properties of the polyamide yarn for thermal bonding or its processed products, or in order to stably obtain them. Examples include a perfect circle, ellipse, trilobe, tetralobe, cross, hollow, flat, T-shaped, X-shaped, H-shaped cross section, etc., but in consideration of processing for thermal bonding, a perfect circle is preferable in terms of melt spinnability and ease of spinning. In addition, the fiber form can be various fiber product forms such as long fibers, short fibers, nonwoven fabrics, and thermoformed bodies.
[0034] The polyamide yarn for thermal bonding of the present invention is useful as a hot melt type adhesive, and is particularly useful when used for bonding textile products. Examples of textile products using the polyamide yarn for thermal bonding of the present invention include sewing threads, decorative twisted yarns (mould yarns) in which upright decorative yarns are arranged over the entire yarn and fixed by thermal bonding, so-called thermal bonding tapes such as hemming tapes for bonding fabrics together with an iron, and further yarns in which a part of a plurality of fibers is mixed and the shape is fixed by heat treatment (brush bristles used for mops, pile yarns used for carpets, etc.).
[0035] The method for producing the polyamide yarn for thermal bonding of the present invention will now be described. The aliphatic copolyamide used in the thermal bonding polyamide yarn of the present invention can be produced by any known polymerization method, but it is preferable to carry out an operation of extracting with hot water after polymerization to remove water-soluble components. The polymerization and extraction methods can be either batch or continuous, but when producing a variety of polymers with different melting points according to needs, the batch method is usually adopted. An example of a batch polymerization method is shown below.
[0036] First, the batch polymerization equipment will be described. When polymerizing an aliphatic copolyamide, it is necessary to apply pressure at the beginning of the polymerization, and so-called autoclaves are generally used as reactors. In order to promote uniform heating and reaction, it is also possible to equip the reactor with a heating coil or a stirring blade inside.
[0037] The maximum pressure in the polymerization apparatus during polymerization is adjusted according to the boiling point of the monomer used, but is usually 0.7 MPa or more. If it is less than 0.7 MPa, the amount of evaporation of the monomer components increases, the molar balance is lost, and the degree of polymerization of the resulting aliphatic copolyamide resin may be low. There is no particular upper limit, but taking into consideration the pressure resistance of the polymerization apparatus, it is preferably 3 MPa or less, more preferably 2 MPa or less. As a method for discharging the polymer after the completion of polymerization, a method is preferably used in which the polymerization apparatus is pressurized with an inert gas, the polymer extruded in the form of a strand is water-cooled, and then cut to obtain pellets.
[0038] The melting point of the raw material pellets of the aliphatic copolyamide used for the polyamide yarn for thermal bonding of the present invention is preferably 80 to 140° C., and more preferably 90 to 120° C. By setting it in this range, it is possible to set the melting point of the obtained polyamide yarn for thermal bonding in a desired range.
[0039] The polyamide yarn for thermal bonding of the present invention can be produced by a known melt spinning method if it is accompanied by a drawing-heat setting process, but from the viewpoint of controlling both the drawing-heat setting process, a direct spinning-drawing method is superior. An example of a production method using the direct spinning-drawing method is given below.
[0040] First, the melting section will be described. When melting the aliphatic copolyamide, a pressure melter method or an extruder method can be mentioned, but is not particularly limited. The melting temperature may be appropriately determined based on the melting point of the aliphatic copolyamide resin, but the preferred melting temperature range is 160 to 240°C. More preferably, it is 200 to 240°C from the viewpoint of maintaining the spinnability of the yarn discharged from the spinneret.
[0041] The spinning temperature is the same as the melting temperature. The spinning temperature here is the so-called heat retention temperature (spin block temperature) at which the polymer pipe, metering pump, spinneret, etc. are kept warm. The preferred spinning temperature range is 160°C to 240°C, and more preferably 200°C to 240°C from the viewpoint of maintaining the spinnability of the yarn discharged from the spinneret.
[0042] In addition, the polymer residence time from the tip of the polymer melting section, for example, from the melter section in the case of a pressure melter type melt spinning apparatus, to being discharged from the spinneret, is preferably within 20 minutes.
[0043] The yarn discharged from the spinneret is sucked to remove gaseous low polymer components coming out of the yarn (MO suction), and then cooled to room temperature by blowing cooling air onto the yarn using a yarn cooling device such as a chimney, and then oiled and bundled using an oiling device, entangled using a fluid treatment device, and if necessary, oiled and bundled again using an oiling device, and passes through a take-up roller and a stretching roller, during which the yarn is stretched according to the ratio of the peripheral speeds of the take-up roller and the stretching roller. The stretched yarn is heat-set and then wound up using a winding device. In order to set the parameters of the polyamide yarn for thermal bonding of the present invention, such as the elongation and heat of fusion, within the desired range, it is important to control both of the stretching and heat-setting steps. The stretching and heat-setting steps are exemplified below.
[0044] The stretch ratio is 1.5 to 3.5 times. It is preferably 2.0 to 3.0 times. The stretch ratio is a mechanical stretch ratio due to the speed difference between the take-up roller and the stretch roller. For example, when the take-up roller is 1200 m / min and the stretch roller is 3000 m / min, the stretch ratio is 2.5 times. By performing mechanical stretching and controlling the heat setting process described later, it is possible to set parameters such as the elongation and heat of fusion of the polyamide yarn for thermal bonding of the present invention within the desired range. When the stretch ratio is 1.5 times or more, active stretching is applied to the amorphous part where the polymer chains are not aligned and exist randomly, so that the polymer chains grow as crystalline parts where they are regularly aligned, and the heat of fusion can be set within the desired range. When the stretch ratio is 3.5 times or less, the flexibility of the polyamide yarn for thermal bonding can be maintained, so that the elongation can be set within the desired range.
[0045] As a method for setting the elongation and heat of fusion of polyamide yarn within the desired range, in addition to the mechanical drawing described above, for example, drawing by spinning draft in which the speed of the take-up roller is made as fast as possible and the speed of the take-up roller and the drawing roller is made as uniform as possible is generally known, and the method proposed in Patent Document 1 utilizes the latter spinning draft. However, with this method, in the polyamide yarn for thermal bonding of the present invention, although it is possible to set the elongation within the desired range, it is extremely difficult to set the heat of fusion within the desired range, and in order to set the heat of fusion within the desired range, it is important to control both the mechanical drawing and the heat setting process described above.
[0046] Heat setting is performed by contacting the yarn with a heater after drawing. As an example of the direct spinning drawing method, a method is preferably used in which a heater is provided inside a drawing roller and the yarn held (contacted) by the drawing roller is heat set. The heat setting temperature is 10°C lower than the melting point of the raw material pellets of the aliphatic copolyamide used in the thermal bonding polyamide yarn of the present invention to less than the melting point. Preferably, it is 10°C lower than the melting point of the raw material pellets of the aliphatic copolyamide used in the thermal bonding polyamide yarn of the present invention to 5°C lower than the melting point of the raw material pellets of the aliphatic copolyamide used in the thermal bonding polyamide yarn of the present invention. For example, when the melting point of the raw material pellets of the aliphatic copolyamide used in the thermal bonding polyamide yarn of the present invention is 110°C, 100≦heat setting temperature<110(°C). Preferably, 100≦heat setting temperature≦105(°C). By setting the heat setting temperature within this range and controlling the drawing step described above, it is possible to set the heat of fusion of the polyamide yarn for thermal bonding of the present invention within the desired range. If the heat setting temperature is less than a temperature 10°C lower than the melting point of the raw material pellets of the aliphatic copolyamide used in the polyamide yarn for thermal bonding of the present invention, it is difficult to set the heat of fusion within the desired range. If the heat setting temperature is equal to or higher than the melting point of the raw material pellets of the aliphatic copolyamide used in the polyamide yarn for thermal bonding of the present invention, fusion of the yarn strips occurs on the heater, and the polyamide yarn for thermal bonding cannot be obtained.
[0047] The winding speed may be appropriately set within a range in which parameters such as elongation and heat of fusion of the thermal bonding polyamide yarn of the present invention are within the desired range and stable production is possible, and is preferably 2500 to 4000 m / min. EXAMPLES
[0048] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. The methods for measuring the properties in the examples are as follows.
[0049] A. Melting point Thermal analysis was performed using a TA Instrument Q1000, and data processing was performed using Universal Analysis 2000. Thermal analysis was performed under nitrogen flow (50 mL / min), with a temperature range of -50 to 300°C, a heating rate of 10°C / min, and a sample weight of approximately 5 g (calorific data was normalized by the weight after measurement). The melting point was measured from the melting peak.
[0050] B. Hot water shrinkage rate The fiber sample was made into a 50 cm loop and an initial load of 1 / 30 (g) of the fineness was applied to measure length A. Next, with the initial load removed, the sample was immersed in warm water (35°C) for 20 minutes and then naturally dried. An initial load of 1 / 30 (g) of the fineness was again applied to measure length B, which was calculated using the following formula. Hot water shrinkage rate (%) = [(AB) / A] x 100.
[0051] C. Total size, single yarn size The fiber sample was wound 200 times at a tension of 1 / 30 (g) using a measuring machine with a frame circumference of 1.125 m to create a 225 m skein. The resulting skein was transferred to a desiccator (temperature 20°C, relative humidity 55% RH) and stored for 180 minutes. The weight of the skein was measured, and the weight per 10,000 m was calculated from the obtained value, and further multiplied by (1.045 / 1.025) to calculate the total fineness. The measurement was performed four times, and the average value was taken as the total fineness. The single yarn fineness was taken as the total fineness / number of filaments.
[0052] D. Heat of fusion The measurement was performed using a TA Instruments Q1000 as the measuring device. It is the heat of fusion (ΔH) (J / g) obtained from differential scanning calorimetry (DSC), and more specifically, it is the sum of each peak of the heat of fusion obtained from the DSC curve. The measurement was performed twice, and the average value was taken as the heat of fusion.
[0053] The DSC measurement conditions were as follows:
[0054] Measurement equipment: TA Instruments Q1000 Data processing: TA Instruments Universal Analysis 2000 Atmosphere: Nitrogen flow 50mL / min Sample size: Approx. 10 mg Sample container: Aluminum standard container Temperature and heat calibration: High purity indium (Tm=156.61℃, ΔHm=28.71 J / g) Temperature range: Approx. -50~300℃ Heating rate: 10℃ / min. First heating process (first run).
[0055] E. Strength and elongation Fiber samples were measured using Orientec's "TENSILON" (registered trademark), UCT-100, under the constant-speed elongation conditions specified in JIS L1013 (chemical fiber filament yarn test method, 2010). Elongation was determined from the elongation at the point showing the maximum strength in the tensile strength-elongation curve. Strength was determined as the value obtained by dividing the maximum strength by the fineness. Measurements were performed 10 times, and the average values were used as strength and elongation. The gripping distance was 500 mm, and the pulling speed was 500 mm / min.
[0056] F. Adhesive strength (1) The fabric to be bonded (Kurashiki Boseki broadcloth #KT4000) was cut to 12 cm vertically and 10 cm horizontally, and two pieces were prepared.
[0057] (2) The fiber samples were doubled to a yarn length of 50 cm and a yarn density of approximately 1650 dtex, and twisted at 50 T / m.
[0058] (3) A fiber sample with yarns doubled at approximately 1650 dT was placed on the adherend fabric. The fiber sample was placed 4 cm from the top (8 cm from the bottom) of the adherend fabric in the vertical direction, so that it was horizontal in the horizontal direction.
[0059] (4) Both ends of the adhesive fabric and the fiber sample were secured with Cellophane Tape (registered trademark) to prevent them from moving, and any excess fiber sample protruding from both ends was cut off.
[0060] (5) Another adhesive cloth was placed on top, and the fiber sample was sandwiched between the two adhesive cloths. Both ends of the adhesive cloths were secured with cellophane tape (registered trademark) to prevent the adhesive cloths from moving.
[0061] (6) The pieces were placed in a bonding press and pressed under conditions of 140°C x 17 kg x 5 seconds.
[0062] (7) Both ends of the bonded fabric were cut off by 1 cm. The bonded fabric was then cut into 2 cm widths. Four pieces were prepared for measuring adhesive strength.
[0063] (8) Using an autograph AGS-50D manufactured by Shimadzu Corporation, the maximum strength until peeling was measured and divided by the yarn fineness to determine the adhesive strength. The tensile conditions were a tensile speed of 5 cm / min and a peel angle of 180°C. The measurement was carried out four times, and the average value was determined as the adhesive strength.
[0064] (9) An adhesive strength of 3.0 cN / dtex or more was considered acceptable.
[0065] G. High-level processability Using a conventional ring twisting machine, a 210 dtex, 34 filament polyhexamethylene adipamide yarn was passed through each nip roller and through each slit hole of the twisting guide. Next, one fiber sample obtained in each Example and Comparative Example, which had been stored for 30 days under an environment of 30°C temperature and 60% humidity, was passed directly through the slit hole of the twisting guide without passing through the nip roller, and twisted together with the three 210 dtex, 34 filament polyhexamethylene adipamide yarns to obtain a sewing thread. The yield was measured based on the yield during fiber twisting processing, and was evaluated on the following four-point scale.
[0066] ◎: Yield 95% or more 〇: Yield is 90% or more, less than 95% △: Yield 85% or more, less than 90% ×: Yield less than 85%.
[0067] <Production of raw material pellets of aliphatic copolyamide> (Examples 1 to 7, Comparative Examples 1 to 3) ε-caprolactam (N6), equimolar salt of hexamethylenediamine and adipic acid (AH salt) (N66), equimolar salt of hexamethylenediamine and sebacic acid (SH salt) (N610), and ω-laurolactam (N12) were weighed out to a weight ratio of 31 / 18 / 32 / 19, respectively, and placed in a batch polymerization vessel with an internal volume of 80 L equipped with a stirrer with double helical ribbon blades and a heat medium jacket. After the inside of the polymerization vessel was sufficiently replaced with nitrogen, heating was started at 290°C while stirring at 30 rpm. When the pressure inside the vessel reached 1.7 MPa (gauge pressure), the heating temperature was changed to 270°C, and the pressure inside the vessel was maintained. When the internal temperature reached 220°C, the pressure was gradually released to atmospheric pressure over 90 minutes. When atmospheric pressure was reached, nitrogen gas was circulated at 5 L / min to blow the inside of the vessel for 30 minutes. Then, nitrogen pressure of 0.4 MPa (gauge pressure) was applied to the inside of the can, and the polymer discharged into a water bath was pelletized with a strand cutter. The obtained resin pellets were left at room temperature for 24 hours, then charged into a batch-type extraction tank, and ion-exchanged water (extraction water) adjusted to 60±1°C was added in an amount 20 times the weight of the resin pellets, and extraction treatment was performed for 24 hours. The pellets after the treatment were thoroughly rinsed with ion-exchanged water and dried under reduced pressure at 60°C for 24 hours to obtain raw material pellets of aliphatic copolyamide with a weight ratio of N6 / N66 / N610 / N12 of 31 / 18 / 32 / 19. The melting point of the obtained raw material pellets of aliphatic copolyamide was as shown in Table 1.
[0068] Example 8 Polymerization was carried out in the same manner as in Example 1, except that ε-caprolactam (N6), equimolar salt of hexamethylenediamine and adipic acid (AH salt) (N66), equimolar salt of hexamethylenediamine and sebacic acid (SH salt) (N610), and ω-laurolactam (N12) were weighed to have a weight ratio of 23 / 19 / 18 / 40, respectively, to obtain raw material pellets of aliphatic copolyamide having a weight ratio of N6 / N66 / N610 / N12 of 23 / 19 / 18 / 40. The melting point of the raw material pellets of the obtained aliphatic copolyamide was as shown in Table 1.
[0069] Example 9 Polymerization was carried out in the same manner as in Example 1, except that ε-caprolactam (N6), equimolar salt of hexamethylenediamine and adipic acid (AH salt) (N66), equimolar salt of hexamethylenediamine and sebacic acid (SH salt) (N610), and ω-laurolactam (N12) were weighed to have a weight ratio of 45 / 25 / 25 / 5, respectively, to obtain raw material pellets of aliphatic copolyamide with a weight ratio of N6 / N66 / N610 / N12 of 45 / 25 / 25 / 5. The melting point of the raw material pellets of the obtained aliphatic copolyamide was as shown in Table 1.
[0070] Comparative Example 4 Polymerization was carried out in the same manner as in Example 1, except that ε-caprolactam (N6) and an equimolar salt of hexamethylenediamine and adipic acid (AH salt) (N66) were weighed to give a weight ratio of 85 / 15, to obtain raw material pellets of an aliphatic copolyamide having a weight ratio of N6 / N66 of 85 / 15. The melting point of the obtained raw material pellets of the aliphatic copolyamide was as shown in Table 1.
[0071] <Production and evaluation of polyamide yarn for thermal bonding> (Examples 1 to 5, Comparative Examples 1 to 3) The obtained raw material pellets of the aliphatic copolyamide were melted in a pressure melter at a melting temperature of 220° C. and discharged from a spinneret. The spinning temperature was set to 220° C. After being discharged from the spinneret, the pellets were subjected to MO suction at a suction wind speed of 35 m / min, cooled with cold air at 18° C., and then oiled by an oiling device and entangled by an entanglement nozzle device. The yarn was subjected to a drawing-heat setting process at a draw ratio and heat setting temperature shown in Table 1, and then taken up at a take-up speed shown in Table 1 to obtain a 22 dtex, 10 filament polyamide yarn for thermal bonding.
[0072] The obtained polyamide yarn for thermal bonding was evaluated for melting point, hot water shrinkage, total fineness, single yarn fineness, heat of fusion, strength, elongation, adhesive strength, and advanced processability. The results are shown in Table 1.
[0073] Example 6 Except for changing the dtex and filament count to 22 dtex and 40 filaments, the yarn was subjected to the drawing-heat setting process at the draw ratio and heat setting temperature shown in Table 1 in the same manner as in Example 1, and then wound up at the winding speed shown in Table 1 to obtain a polyamide yarn for thermal bonding. The obtained polyamide yarn for thermal bonding was evaluated for melting point, hot water shrinkage, total fineness, single yarn fineness, heat of fusion, strength, elongation, adhesive strength, and advanced processability. The results are shown in Table 1.
[0074] Example 7 Except for changing the yarn to 44 dtex and 5 filaments, the yarn was subjected to the drawing-heat setting process at the draw ratio and heat setting temperature shown in Table 1 in the same manner as in Example 1, and then taken up at the winding speed shown in Table 1 to obtain a polyamide yarn for thermal bonding. The obtained polyamide yarn for thermal bonding was evaluated for melting point, hot water shrinkage, total fineness, single yarn fineness, heat of fusion, strength, elongation, adhesive strength, and advanced processability. The results are shown in Table 1.
[0075] Example 8 Except for melting the yarn in a pressure melter at a melting temperature of 180°C and setting the spinning temperature to 180°C, the yarn was subjected to a drawing-heat setting process at the draw ratio and heat setting temperature shown in Table 1 in the same manner as in Example 1, and then taken up at the winding speed shown in Table 1 to obtain a polyamide yarn for thermal bonding. The obtained polyamide yarn for thermal bonding was evaluated for melting point, hot water shrinkage, total fineness, single yarn fineness, heat of fusion, strength, elongation, adhesive strength, and advanced processability. The results are shown in Table 1.
[0076] Example 9 Except for melting the yarn in a pressure melter at a melting temperature of 230°C and setting the spinning temperature to 230°C, the yarn was subjected to a drawing-heat setting process at the draw ratio and heat setting temperature shown in Table 1 in the same manner as in Example 1, and then taken up at the winding speed shown in Table 1 to obtain a polyamide yarn for thermal bonding. The obtained polyamide yarn for thermal bonding was evaluated for melting point, hot water shrinkage, total fineness, single yarn fineness, heat of fusion, strength, elongation, adhesive strength, and advanced processability. The results are shown in Table 1.
[0077] Comparative Example 4 Except for melting the yarn in a pressure melter at a melting temperature of 260°C and setting the spinning temperature to 260°C, the yarn was subjected to a drawing-heat setting process at the draw ratio and heat setting temperature shown in Table 1 in the same manner as in Example 1, and then taken up at the winding speed shown in Table 1 to obtain a polyamide yarn for thermal bonding. The obtained polyamide yarn for thermal bonding was evaluated for melting point, hot water shrinkage, total fineness, single yarn fineness, heat of fusion, strength, elongation, adhesive strength, and advanced processability. The results are shown in Table 1. In the measurement of adhesive strength, the polyamide yarn for thermal bonding did not melt satisfactorily under the pressing conditions of 140°C x 17 kg x 5 seconds, and the adhesive strength value showed zero.
[0078] [Table 1]
[0079] As is clear from the results in Table 1, the polyamide yarn for thermal bonding of the present invention has extremely remarkable effects, compared to conventional polyamide yarns for thermal bonding, such as stable high-order processability even after storage for 30 days in an environment of 30°C and 60% humidity, which assumes use after long-term storage, and also excellent adhesive strength in low-temperature operations.
[0080] In Comparative Example 1, the stretch ratio was low, the elongation of the thermal bonding polyamide yarn was high, and the heat of fusion was low. Therefore, the crystal structure was not stable, and the processability in the advanced process after storage for 30 days in an environment of 30°C and 60% humidity was poor.
[0081] In Comparative Example 2, the draw ratio was high, the elongation of the thermal bonding polyamide yarn was low, and the heat of fusion was high. As a result, the flexibility of the drawn yarn was reduced, and in the higher-level process of the sewing yarn that passed through the twisting process, the twisting was extremely difficult to achieve, causing fluffing and poor higher-level processability.
[0082] In Comparative Example 3, the heat setting temperature was low and the heat of fusion of the thermal bonding polyamide yarn was low, so the crystal structure was not stable and the processability in the advanced process was poor after storage for 30 days in an environment of 30°C and 60% humidity.
Claims
1. The polyamide yarn for thermal bonding is an aliphatic copolyamide obtained by copolymerizing three or more types of monomers, the aliphatic copolyamide yarn containing monomers constituting an aliphatic polyamide, and has a melting point of 80 to 140°C, an elongation of 50 to 90%, and a heat of fusion of 10 to 50 J / g.
2. 2. The polyamide yarn for thermal bonding according to claim 1, which is a multifilament having a single yarn fineness of 0.5 to 10 dtex.
3. A polyamide yarn for thermal bonding as described in claim 1 or 2, having a hot water shrinkage rate of 10 to 50% and a strength of 2.5 to 4.0 cN / dtex.
4. The polyamide yarn for thermal bonding according to any one of claims 1 to 3, wherein the aliphatic copolyamide contains a monomer (A) constituting polycaproamide and a monomer (B) constituting polyhexamethylene adipamide, and the total content of the monomer (A) and the monomer (B) is 40 to 70% by weight of the aliphatic copolyamide.
5. The polyamide yarn for thermal bonding according to any one of claims 1 to 4, wherein the aliphatic copolyamide contains a monomer (C) constituting polydodecanamide, and the content of the monomer (C) is 5 to 40% by weight of the aliphatic copolyamide.
6. A sewing thread comprising, in a part thereof, the polyamide thread for thermal bonding according to any one of claims 1 to 5.
7. A mall yarn having, in a part thereof, the polyamide yarn for thermal bonding according to any one of claims 1 to 5.
8. A thermal bonding tape comprising, in a part thereof, the thermal bonding polyamide yarn according to any one of claims 1 to 5.
9. A method for producing a polyamide yarn for thermal bonding according to any one of claims 1 to 5, which is made of an aliphatic copolyamide obtained by copolymerizing three or more kinds of monomers including a monomer constituting an aliphatic polyamide, and which comprises drawing at a draw ratio of 1.5 to 3.5 times, and then heat setting at a heat setting temperature in the range of a temperature 10°C lower than the melting point of raw material pellets of the aliphatic copolyamide to less than the melting point.
Citation Information
Patent Citations
Low-melting point hot adhesion fiber and method for producing same
CN101555635A
Hot-melt type adhesive fiber with good unwinding performance and method for producing the same
JP2004204386A
Polyamide multi-filament for thermal adhesion
JP2010189806A
Copolyamide, and pellet and fiber comprising the same
JP2012177048A
Polyamide high orientation non-stretched yarn and manufacturing method therefor
JP2016113730A