Method for manufacturing positive electrode for power storage device
By applying a carbon coating with an aqueous binder and controlling the pH of the slurry to 5 to 8, the method enhances adhesion between the positive electrode active material layer and the metal foil, addressing the alkalinity issue and improving the performance of power storage devices.
Patent Information
- Application Number
- JP2020192757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-19
AI Technical Summary
The alkalinity of the slurry for forming a positive electrode active material layer can adversely affect the adhesion between the positive electrode active material layer and the metal foil in the manufacturing process of power storage devices.
A method is employed that includes a carbon coating layer on the metal foil with an aqueous binder and a pH of 5 to 8, and a pH of 5.5 to 7.5 for the slurry, using a polyanionic compound like LiFePO4 with an olivine structure to enhance adhesion.
This approach improves the adhesion between the positive electrode active material layer and the metal foil, resulting in better performance and stability of the power storage device.
Smart Images

Figure 0007589517000002 
Figure 0007589517000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a positive electrode for an electricity storage device. [Background technology]
[0002] Patent Document 1 discloses a binder for a carbon-coated foil coating liquid. A carbon-coated foil coating liquid (slurry for forming a carbon coating layer) using this binder (binding agent) is applied to a metal foil used as a current collector in a power storage device such as a lithium-ion secondary battery or an electric double-layer capacitor to produce a carbon-coated foil. An electrode slurry containing an active material is applied to this carbon-coated foil to produce an electrode. The use of the carbon-coated foil improves the adhesion between the active material layer and the metal foil and reduces the resistance between the active material layer and the metal foil. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-229187 A Summary of the Invention [Problem to be solved by the invention]
[0004] In a method for producing a positive electrode for a power storage device, a slurry for forming a positive electrode active material layer containing a positive electrode active material tends to be alkaline. If the slurry for forming a positive electrode active material layer becomes alkaline, there is a risk that the improvement of adhesion between the positive electrode active material layer and a metal foil will be adversely affected. [Means for solving the problem]
[0005] A method for producing a positive electrode for a power storage device that achieves the above object includes a step of forming a positive electrode active material layer by applying a positive electrode active material layer-forming slurry containing an aqueous solvent and having a pH of 5 to 8 onto a carbon coating layer of a metal foil having the carbon coating layer containing carbon and an aqueous binder.
[0006] The manufacturing method of the positive electrode for a power storage device that achieves the above object is such that the pH of the slurry for forming the positive electrode active material layer is 5.5 to 7.5. The manufacturing method of the positive electrode for a power storage device that achieves the above object is such that the pH of the slurry for forming the positive electrode active material layer is 6 to 7.
[0007] The slurry for forming the positive electrode active material layer contains, as the positive electrode active material, a polyanion compound having an olivine-type structure represented by the general formula LiM h PO4 (M is at least one element selected from the group consisting of Mn, Fe, Co, Ni, Cu, Mg, Zn, V, Ca, Sr, Ba, Ti, Al, Si, B, Te, and Mo; h is a numerical value satisfying 0 < h < 2).
[0008] The polyanion compound is LiFePO4.
Advantages of the Invention
[0009] According to the present invention, the adhesion between the positive electrode active material layer and the metal foil is improved.
Brief Description of the Drawings
[0010] [Figure 1] Cross-sectional view of a power storage device.
Embodiments for Carrying Out the Invention
[0011] Hereinafter, an embodiment embodying the present invention will be described with reference to the drawings. The power storage device 10 shown in FIG. 1 is, for example, a power storage module used for batteries of various vehicles such as forklifts, hybrid vehicles, and electric vehicles. The power storage device 10 is, for example, a secondary battery such as a nickel-metal hydride secondary battery or a lithium-ion secondary battery. The power storage device 10 may be an electric double layer capacitor. In the present embodiment, the case where the power storage device 10 is a lithium-ion secondary battery will be exemplified.
[0012] As shown in Fig. 1, the energy storage device 10 includes a cell stack 30 (laminate) in which a plurality of energy storage cells 20 are stacked in a stacking direction. Hereinafter, the stacking direction of the plurality of energy storage cells 20 will be simply referred to as the stacking direction. Each energy storage cell 20 includes a positive electrode 21, a negative electrode 22, a separator 23, and a seal portion 24.
[0013] The positive electrode 21 includes a positive electrode collector 21a as a metal foil, a carbon coating layer 21b provided on a first surface 21a1 of the positive electrode collector 21a, and a positive electrode active material layer 21c provided on a first surface 21b1 of the carbon coating layer 21b, which is a surface of the carbon coating layer 21b opposite to the first surface 21a1 of the positive electrode collector 21a. The positive electrode collector 21a and the carbon coating layer 21b form a carbon-coated foil. In a plan view from the stacking direction (hereinafter simply referred to as a plan view), the positive electrode active material layer 21c is formed in the center of the carbon coating layer 21b. The peripheral portion of the carbon coating layer 21b in the plan view is a positive electrode uncoated portion 21d where the positive electrode active material layer 21c is not provided. The positive electrode uncoated portion 21d is arranged to surround the periphery of the positive electrode active material layer 21c in the plan view. Specific configurations of the positive electrode current collector 21a, the carbon coating layer 21b, and the positive electrode active material layer 21c will be described later.
[0014] The negative electrode 22 includes a negative electrode current collector 22a and a negative electrode active material layer 22b provided on a first surface 22a1 of the negative electrode current collector 22a. In a plan view, the negative electrode active material layer 22b is formed in the center of the first surface 22a1 of the negative electrode current collector 22a. In a plan view, the peripheral portion of the first surface 22a1 of the negative electrode current collector 22a is a negative electrode uncoated portion 22c where the negative electrode active material layer 22b is not provided. The negative electrode uncoated portion 22c is disposed so as to surround the periphery of the negative electrode active material layer 22b in a plan view.
[0015] The negative electrode current collector 22a is a chemically inactive electric conductor for continuously passing a current through the positive electrode active material layer 21c during discharging or charging of the lithium ion secondary battery. The negative electrode current collector 22a is, for example, a foil having a thickness of 1 to 100 μm. In this embodiment, the negative electrode current collector 22a is a copper foil. Examples of materials that can be used to form the negative electrode current collector 22a include metal materials, conductive resin materials, and conductive inorganic materials.
[0016] Examples of the conductive resin material include resins obtained by adding a conductive filler to a conductive polymer material or a non-conductive polymer material as necessary. The negative electrode current collector 22a may have a plurality of layers including one or more layers containing the above-mentioned metal material or conductive resin material. The surface of the negative electrode current collector 22a may be covered with a known protective layer. The surface of the negative electrode current collector 22a may be treated by a known method such as plating.
[0017] The negative electrode current collector 22a may be a metal foil such as an aluminum foil, a nickel foil, a titanium foil, or a stainless steel foil, other than a copper foil. From the viewpoint of ensuring mechanical strength, the negative electrode current collector 22a may be a stainless steel foil (e.g., SUS304, SUS316, SUS301, SUS304, etc., as specified in JIS G 4305:2015). The negative electrode current collector 22a may be an alloy foil of the above metals. The negative electrode current collector 22a may be a foil including a base material covered with a copper film.
[0018] The negative electrode active material layer 22b includes a negative electrode active material. The negative electrode active material is not particularly limited and may be any element, alloy, or compound capable of absorbing and releasing charge carriers such as lithium ions. For example, the negative electrode active material may be Li, carbon, a metal compound, an element capable of alloying with lithium, or a compound thereof. Examples of carbon include natural graphite, artificial graphite, hard carbon (hardly graphitizable carbon), or soft carbon (easily graphitizable carbon). Examples of artificial graphite include highly oriented graphite, mesocarbon microbeads, and the like. Examples of elements capable of alloying with lithium include silicon and tin.
[0019] The positive electrode 21 and the negative electrode 22 are arranged such that the positive electrode active material layer 21c and the negative electrode active material layer 22b face each other in the stacking direction. That is, the facing direction of the positive electrode 21 and the negative electrode 22 coincides with the stacking direction. The negative electrode active material layer 22b is formed to be slightly larger than the positive electrode active material layer 21c, and in a plan view seen from the stacking direction, the entire formation region of the positive electrode active material layer 21c is located within the formation region of the negative electrode active material layer 22b.
[0020] The positive electrode current collector 21a has a second surface 21a2 opposite to the first surface 21a1. The positive electrode 21 is an electrode having a monopolar structure in which neither the positive electrode active material layer 21c nor the negative electrode active material layer 22b is formed on the second surface 21a2 of the positive electrode current collector 21a. The negative electrode current collector 22a has a second surface 22a2 opposite to the first surface 22a1. The negative electrode 22 is an electrode having a monopolar structure in which neither the positive electrode active material layer 21c nor the negative electrode active material layer 22b is formed on the second surface 21a2 of the negative electrode current collector 22a.
[0021] The separator 23 is disposed between the positive electrode 21 and the negative electrode 22, and is a component that separates the positive electrode 21 and the negative electrode 22 to prevent a short circuit due to contact between the two electrodes, while allowing charge carriers such as lithium ions to pass through.
[0022] The separator 23 is, for example, a porous sheet or nonwoven fabric containing a polymer that absorbs and retains a liquid electrolyte. Examples of materials constituting the separator 23 include polypropylene, polyethylene, polyolefin, and polyester. The separator 23 may have a single-layer structure or a multi-layer structure. The multi-layer structure may include, for example, an adhesive layer, a ceramic layer as a heat-resistant layer, and the like.
[0023] The seal portion 24 is disposed between the first surface 21b1 of the carbon coating layer 21b of the positive electrode 21 and the first surface 22a1 of the negative electrode current collector 22a of the negative electrode 22, and is disposed on the outer circumferential side of the positive electrode current collector 21a and the negative electrode current collector 22a, and is bonded to both the positive electrode current collector 21a and the carbon coating layer 21b, and the negative electrode current collector 22a. The seal portion 24 prevents a short circuit between the current collectors by insulating between the positive electrode current collector 21a and the carbon coating layer 21b, and the negative electrode current collector 22a.
[0024] The sealing portion 24 extends along the periphery of the positive electrode current collector 21a, the carbon coating layer 21b, and the negative electrode current collector 22a in a plan view, and is formed in a frame shape surrounding the positive electrode current collector 21a, the carbon coating layer 21b, and the negative electrode current collector 22a. The sealing portion 24 is disposed between the first surface 21b1 of the carbon coating layer 21b and the negative electrode uncoated portion 22c of the first surface 22a1 of the negative electrode current collector 22a.
[0025] Examples of materials that can be used to form the seal portion 24 include various resin materials such as polyethylene (PE), polystyrene, ABS resin, modified polypropylene (modified PP), and acrylonitrile styrene (AS) resin.
[0026] An enclosed space S is formed inside the energy storage cell 20 and is surrounded by a frame-shaped seal portion 24, the positive electrode 21, and the negative electrode 22. A separator 23 and a liquid electrolyte are contained in the enclosed space S. The peripheral portion of the separator 23 is embedded in the seal portion 24.
[0027] The liquid electrolyte may, for example, include a liquid electrolyte containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. As the electrolyte salt, known lithium salts such as LiClO4, LiAsF6, LiPF6, LiBF4, LiCF3SO3, LiN(FSO2)2, and LiN(CF3SO2)2 may be used. As the non-aqueous solvent, known solvents such as cyclic carbonates, cyclic esters, chain carbonates, chain esters, and ethers may be used. Two or more of these known solvent materials may be used in combination.
[0028] The seal portion 24 can suppress permeation of the liquid electrolyte contained in the sealed space S to the outside by sealing the sealed space S between the positive electrode 21 and the negative electrode 22. The seal portion 24 can also suppress intrusion of moisture into the sealed space S from the outside of the electricity storage device 10. Furthermore, the seal portion 24 can suppress leakage of gas generated from the positive electrode 21 or the negative electrode 22 due to, for example, a charge / discharge reaction to the outside of the electricity storage device 10.
[0029] The cell stack 30 has a structure in which a plurality of storage cells 20 are stacked such that the second surface 21a2 of the positive electrode current collector 21a and the second surface 22a2 of the negative electrode current collector 22a are in contact with each other. As a result, the plurality of storage cells 20 constituting the cell stack 30 are connected in series.
[0030] Here, in the cell stack 30, two storage cells 20 adjacent to each other in the stacking direction form a pseudo bipolar electrode 25 in which the positive electrode current collector 21a and the negative electrode current collector 22a in contact with each other are regarded as one current collector. The pseudo bipolar electrode 25 includes a current collector having a structure in which the positive electrode current collector 21a and the negative electrode current collector 22a are stacked, a positive electrode active material layer 21c formed on one surface of the current collector, and a negative electrode active material layer 22b formed on the other surface.
[0031] The seal portion 24 of each storage cell 20 has an outer peripheral portion 24a that extends outward beyond the edges of the positive electrode current collector 21a and the negative electrode current collector 22a. When viewed from the stacking direction, the outer peripheral portion 24a protrudes in a direction perpendicular to the stacking direction beyond the edges of the positive electrode current collector 21a and the negative electrode current collector 22a. Adjacent storage cells 20 in the stacking direction are integrated by bonding the outer peripheral portions 24a of the seal portions 24 to each other. Examples of a method for bonding adjacent seal portions 24 to each other include known welding methods such as heat welding, ultrasonic welding, and infrared welding.
[0032] The energy storage device 10 includes a pair of current conductors, consisting of a positive electrode current conductor plate 40 and a negative electrode current conductor plate 50, disposed on either side of the cell stack 30 in the stacking direction of the cell stack 30. The positive electrode current conductor plate 40 and the negative electrode current conductor plate 50 are each made of a material having excellent electrical conductivity.
[0033] The positive electrode current-carrying plate 40 is electrically connected to the second surface 21a2 of the positive electrode current collector 21a of the positive electrode 21 arranged at the outermost side at one end in the stacking direction. The negative electrode current-carrying plate 50 is electrically connected to the second surface 22a2 of the negative electrode current collector 22a of the negative electrode 22 arranged at the outermost side at the other end in the stacking direction.
[0034] The electricity storage device 10 is charged and discharged through terminals provided on the positive electrode current-carrying plate 40 and the negative electrode current-carrying plate 50. The material constituting the positive electrode current-carrying plate 40 may be, for example, the same material as the material constituting the positive electrode current-collector 21a. The positive electrode current-carrying plate 40 may be made of a metal plate thicker than the positive electrode current-collector 21a used in the cell stack 30. The material constituting the negative electrode current-carrying plate 50 may be, for example, the same material as the material constituting the negative electrode current-collector 22a. The negative electrode current-carrying plate 50 may be made of a metal plate thicker than the negative electrode current-collector 22a used in the cell stack 30.
[0035] Next, a method for manufacturing the positive electrode 21 provided in the electricity storage device 10 will be described. The method for manufacturing the positive electrode 21 includes a slurry preparation step of preparing a carbon coat layer forming slurry that will become the carbon coat layer 21b when solidified, and a positive electrode composite preparation step of preparing a positive electrode active material layer forming slurry (hereinafter also referred to as a "positive electrode composite") having a pH of 5 to 8 that will become the positive electrode active material layer 21c when solidified. The method also includes a carbon coat layer forming step of applying the prepared carbon coat layer forming slurry onto the positive electrode current collector 21a to form the carbon coat layer 21b on the positive electrode current collector 21a. The method also includes a positive electrode active material layer forming step of applying the prepared positive electrode composite having a pH of 5 to 8 onto the carbon coat layer 21b to form the positive electrode active material layer 21c.
[0036] At least one of the carbon coat layer forming slurry and the positive electrode composite material may be a ready-made product such as a commercially available product. Therefore, at least one of the slurry preparation step and the positive electrode composite material preparation step may be omitted in the manufacturing method of the positive electrode 21. The manufacturing method of the positive electrode 21 may be composed of, for example, a carbon coat layer forming step and a positive electrode active material layer forming step.
[0037] Furthermore, a ready-made product in which the carbon coating layer 21b is formed in advance on the positive electrode current collector 21a may be used. Therefore, the method for producing the positive electrode 21 may omit the carbon coating layer forming step, and may be composed of only the positive electrode active material layer forming step.
[0038] Each step in the method for producing the positive electrode 21 will be described below. <Slurry preparation process> The slurry for forming the carbon coating layer is a slurry containing carbon as a conductive assistant, a water-based binder, and a water-based solvent.
[0039] The carbon as the conductive assistant is not particularly limited, and may be any known carbon used in a slurry for forming a carbon coating layer. Examples of carbon include carbon black, graphite, vapor grown carbon fiber, and carbon nanotubes. Examples of carbon black include acetylene black, Ketjen Black (registered trademark), furnace black, and channel black.
[0040] The conductive assistant may be used alone or in combination of two or more kinds. The aqueous binder is a binder that can be dissolved or dispersed in an aqueous solvent, and is used by mixing with a conductive assistant in a dispersed or dissolved state in the aqueous solvent. Examples of the aqueous binder include thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamideimide, alkoxysilyl group-containing resins, acrylic resins such as poly(meth)acrylic acid, styrene-butadiene rubber, alginates such as sodium alginate and ammonium alginate, water-soluble cellulose ester crosslinks, and starch-acrylic acid graft polymers.
[0041] The above aqueous binders may be used alone or in combination of two or more. In the present invention, for example, when polyvinylidene fluoride, which is a solvent-based binder, is used, there is a risk that the aqueous solvent contained in the positive electrode mixture reacts with polyvinylidene fluoride in the carbon coating layer, and corrosion of the carbon coating layer progresses. Therefore, in the present invention, an aqueous binder is used as the binder for the slurry for forming the carbon coating layer.
[0042] Examples of the aqueous solvent include water and mixed solvents mainly composed of water. Examples of other solvents include non-aqueous solvents such as N-methylpyrrolidone, dimethylsulfoxide, dimethylformamide, and acetonitrile. The volume ratio of water in the mixed solvent is 50% or more, and preferably 75% or more.
[0043] The slurry for forming the carbon coating layer may contain other components in addition to the conductive assistant. Examples of other components in addition to the conductive assistant include a dispersant. The dispersant is not particularly limited, and examples thereof include carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.
[0044] The above dispersants may be used alone or in combination of two or more. The content of the conductive assistant in the slurry for forming the carbon coating layer is, for example, preferably 30 to 90 parts by mass, and more preferably 40 to 60 parts by mass, when the total mass of the solid contents contained in the carbon coating layer, i.e., the mass of the carbon coating layer excluding the aqueous solvent (hereinafter referred to as the solid content mass), is taken as 100 parts by mass.
[0045] The content of the aqueous binder in the carbon coating layer forming slurry is, for example, preferably 10 to 60 parts by mass, and more preferably 30 to 50 parts by mass, when the solid content mass is taken as 100 parts by mass.
[0046] The content of the dispersant in the slurry for forming a carbon coating layer is, for example, preferably 1 to 20 parts by mass, and more preferably 3 to 10 parts by mass, when the solid content mass is taken as 100 parts by mass.
[0047] The content of the aqueous solvent in the slurry for forming a carbon coating layer is not particularly limited, but it is preferable that the content be such that the solid content ratio of the slurry for forming a carbon coating layer is 20 to 50 mass %, for example.
[0048] <Cathode composite material preparation process> The positive electrode mixture is a slurry containing a positive electrode active material, a pH adjuster, and an aqueous solvent, and has a pH of 5-8.
[0049] The positive electrode active material is not particularly limited, and any known positive electrode active material used in a positive electrode mixture for a power storage device can be used. The positive electrode active material is, for example, a compound represented by the general formula LiM h It is preferable to use a polyanion-based compound having an olivine structure represented by PO4 (hereinafter, referred to as an olivine structure positive electrode active material). h In PO4, M is at least one element selected from the group consisting of Mn, Fe, Co, Ni, Cu, Mg, Zn, V, Ca, Sr, Ba, Ti, Al, Si, B, Te, and Mo. The general formula is LiM hIn PO4, h is a numerical value satisfying 0 < h < 2. Also, h preferably satisfies 0.6 < h < 1.1, and more preferably is 1.
[0050] Examples of the olivine-type structure cathode active material include, for example, LiFePO4, and compounds represented by the general formula LiMn x Fe y PO4. In the general formula LiMn x Fe y PO4, x and y are numerical values satisfying x + y = 1, 0 < x < 1, and 0 < y < 1. Specific examples of the ranges of x and y include the cases where 0.5 ≤ x ≤ 0.9, 0.1 ≤ y ≤ 0.5, and 0.6 ≤ x ≤ 0.8, 0.2 ≤ y ≤ 0.4. The olivine-type structure cathode active material contained in the cathode active material layer 21c may be one type or two or more types.
[0051] The cathode composite material may contain other cathode active materials other than the olivine-type structure cathode active material, if necessary. Examples of other cathode active materials include those that can be used as cathode active materials for lithium-ion secondary batteries, such as lithium composite metal oxides having a layered rock salt structure and metal oxides having a spinel structure. The other cathode active materials contained in the cathode active material layer 21c may be used alone or in combination of two or more.
[0052] The pH adjuster is not particularly limited, and for example, organic acids or inorganic acids can be used. Examples of organic acids include carboxylic acids. Examples of inorganic acids include hydrochloric acid, nitric acid, sulfuric acid, acetic acid, and phosphoric acid.
[0053] The pH adjuster preferably shows weak acidity. Examples of pH adjusters showing weak acidity include carboxylic acids, acetic acid, and phosphoric acid. By the pH adjuster showing weak acidity, dissolution of the cathode active material can be suppressed.
[0054] The above pH adjuster may be used alone or in combination of two or more. The pH of the positive electrode mixture can be adjusted by adjusting the content of the pH adjuster contained in the positive electrode mixture. The pH of the positive electrode mixture is preferably 5.5 to 7.5, and more preferably 6 to 7.
[0055] Examples of the aqueous solvent include water and mixed solvents mainly composed of water. Examples of other solvents include non-aqueous solvents such as N-methylpyrrolidone, dimethylsulfoxide, dimethylformamide, and acetonitrile. The volume ratio of water in the mixed solvent is 50% or more, and preferably 75% or more.
[0056] The positive electrode mixture may contain other components in addition to the positive electrode active material and the pH adjuster, such as a water-based binder and a dispersant.
[0057] The aqueous binder and dispersant used may be the same as those used in the slurry for forming the carbon-coated foil. The positive electrode mixture may contain optional components such as a conductive assistant for increasing electrical conductivity, an electrolyte (polymer matrix, ion-conductive polymer, electrolyte solution, etc.), an electrolyte supporting salt for increasing ion conductivity (lithium salt), etc. Examples of the conductive assistant include acetylene black, carbon black, graphite, and carbon nanotubes.
[0058] The content of the positive electrode active material in the positive electrode mixture is, for example, preferably 70 to 99 parts by mass, and more preferably 90 to 98 parts by mass, when the solid content mass of the positive electrode mixture is 100 parts by mass. When other positive electrode active materials are contained, it is preferable that 50% by mass or more of the positive electrode active materials contained in the positive electrode mixture are olivine type structure positive electrode active materials, and more preferably 75% by mass or more of the positive electrode active materials are olivine type structure positive electrode active materials.
[0059] The content of the aqueous binder in the positive electrode mixture is, for example, preferably 1 to 30 parts by mass, and more preferably 1 to 5 parts by mass, when the solid content mass is taken as 100 parts by mass. The content of the dispersant in the positive electrode mixture is, for example, preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 1 part by mass, when the solid content mass is taken as 100 parts by mass.
[0060] The content of the aqueous solvent in the positive electrode mixture is not particularly limited, but is preferably such that the solid content ratio of the positive electrode mixture is 30 to 60 mass %, for example. <Carbon coat layer forming process> The carbon coating layer forming step is a step of forming the carbon coating layer 21b on the first surface 21a1 of the positive electrode current collector 21a using the above-mentioned carbon coating layer forming slurry.
[0061] The positive electrode collector 21a is a chemically inactive electrical conductor for continuously passing a current through the positive electrode active material layer 21c during discharging or charging of the lithium ion secondary battery. In this embodiment, the positive electrode collector 21a is an aluminum foil. Examples of materials that can be used to form the positive electrode collector 21a include metal materials, conductive resin materials, and conductive inorganic materials.
[0062] Examples of the conductive resin material include resins obtained by adding a conductive filler to a conductive polymer material or a non-conductive polymer material as necessary. The positive electrode collector 21a may have a plurality of layers including one or more layers containing the above-mentioned metal material or conductive resin material. The surface of the positive electrode collector 21a may be covered with a known protective layer. The surface of the positive electrode collector 21a may be treated by a known method such as plating.
[0063] The positive electrode current collector 21a may have a form such as a foil, a sheet, a film, a wire, a rod, a mesh, or a clad material. The positive electrode current collector 21a may be a metal foil such as a copper foil, a nickel foil, a titanium foil, or a stainless steel foil, other than an aluminum foil. From the viewpoint of ensuring mechanical strength, the current collector may be a stainless steel foil (for example, SUS304, SUS316, SUS301, SUS304, etc., as specified in JIS G 4305:2015).
[0064] The positive electrode current collector 21a may be an alloy foil of the above metals. The positive electrode current collector 21a may be a foil including a base material covered with an aluminum film. In the case of the foil-shaped positive electrode current collector 21a, the thickness of the positive electrode current collector 21a is, for example, 1 to 100 μm.
[0065] In the carbon coating layer forming step, the method of forming the carbon coating layer 21b on the first surface 21a1 of the positive electrode collector 21a using the carbon coating layer forming slurry is not particularly limited, and any known method applicable to the formation of a positive electrode 21 having a carbon coating layer 21b can be used.
[0066] For example, a carbon coating layer forming slurry is applied to the first surface 21a1 of the positive electrode current collector 21a to a predetermined thickness and adhered thereto. Thereafter, the adhered carbon coating layer forming slurry is dried and solidified to form a carbon coating layer 21b containing carbon and a water-based binder.
[0067] In the carbon coating layer 21b, the aqueous solvent may be completely removed, or a portion of it may remain in the carbon coating layer 21b. The carbon coating layer forming slurry can be applied by a conventionally known method such as roll coating, dip coating, doctor blade, spray coating, curtain coating, etc. Another method includes forming a sheet-like carbon coating layer 21b using the carbon coating layer forming slurry and bonding the sheet-like carbon coating layer 21b to the first surface 21a1 of the positive electrode current collector 21a.
[0068] The thickness and basis weight of the carbon coating layer 21b formed in the carbon coating layer forming step are not particularly limited, and conventionally known knowledge about lithium ion secondary batteries can be appropriately referred to.
[0069] The thickness of the carbon coating layer 21b is, for example, preferably 1 μm or more, and more preferably 3 μm or more. The thickness of the carbon coating layer 21b is, for example, 500 μm or less. The basis weight of the carbon coating layer 21b is, for example, 0.01 mg / cm 2 It is preferable that the concentration is 0.05 mg / cm or more. 2 The weight of the carbon coating layer 21b is preferably 10 mg / cm or more. 2 The following is the result.
[0070] As described above, the carbon coating layer 21b is formed on the first surface 21a1 of the positive electrode current collector 21a, thereby forming a carbon-coated foil. <Cathode active material layer formation process> The positive electrode active material layer forming process is a process of forming the positive electrode active material layer 21c on the first surface 21b1 of the carbon coating layer 21b opposite to the first surface 21a1 side of the positive electrode current collector 21a, using a positive electrode mixture containing the above-mentioned aqueous solvent and having a pH of 5 to 8.
[0071] In the positive electrode active material layer formation step, the method of forming the positive electrode active material layer 21c on the first surface 21b1 of the carbon coating layer 21b using a slurry-like positive electrode mixture containing an aqueous solvent and having a pH of 5 to 8 is not particularly limited, and any known method applicable to the formation of the positive electrode 21 of an electricity storage device can be used.
[0072] For example, a positive electrode mixture is applied to the first surface 21b1 of the carbon coating layer 21b to a predetermined thickness and then dried and solidified to form the positive electrode active material layer 21c.
[0073] In the positive electrode active material layer 21c, the aqueous solvent may be completely removed, or a portion of it may remain in the positive electrode active material layer 21c. The positive electrode composite material can be applied by a conventionally known method such as a roll coating method, a dip coating method, a doctor blade method, a spray coating method, a curtain coating method, etc. Another method includes a method in which a sheet-shaped positive electrode active material layer 21c is formed using the positive electrode composite material, and the sheet-shaped positive electrode active material layer 21c is bonded to the first surface 21b1 of the carbon coating layer 21b.
[0074] The thickness and basis weight of the positive electrode active material layer 21c formed in the active material layer forming step are not particularly limited, and conventionally known knowledge about lithium ion secondary batteries may be referred to as appropriate. However, from the viewpoint of increasing the energy density of the storage cell 20, it is preferable to increase the basis weight of the positive electrode active material layer 21c.
[0075] The thickness of the positive electrode active material layer 21c is, for example, preferably 100 μm or more, and more preferably 250 μm or more. The thickness of the positive electrode active material layer 21c is, for example, 800 μm or less. The basis weight of the positive electrode active material layer 21c is, for example, 20 mg / cm 2 It is preferable that the concentration is 50 mg / cm or more. 2 The weight per unit area of the positive electrode active material layer 21c is preferably 100 mg / cm or more. 2 The following is the result.
[0076] The positive electrode active material layer 21c of the positive electrode 21 formed in the active material layer forming step preferably contains a positive electrode active material including an olivine structure positive electrode active material, and a water-based binder. Next, a method for manufacturing the electricity storage device 10 will be described.
[0077] The electricity storage device 10 is manufactured by sequentially carrying out an electricity storage cell forming process and a cell stack forming process. <Storage cell formation process> In the storage cell formation process, first, a positive electrode 21 having a carbon coating layer 21b provided on a first surface 21a1 of a positive electrode collector 21a and a positive electrode active material layer 21c provided on a first surface 21b1 of the carbon coating layer 21b, and a negative electrode 22 having a negative electrode active material layer 22b provided on a first surface 22a1 of a negative electrode collector 22a are prepared. The negative electrode 22 can be manufactured using a known method. For example, the negative electrode 22 can be manufactured by performing the same operation as in the active material layer formation process using a negative electrode mixture that becomes the negative electrode active material layer 22b when solidified.
[0078] Next, the positive electrode 21 and the negative electrode 22 are arranged so that the positive electrode active material layer 21c and the negative electrode active material layer 22b face each other in the stacking direction with the separator 23 sandwiched therebetween, and a sealing material to become the sealing portion 24 is arranged between the positive electrode 21 and the negative electrode 22, and on the outer circumferential side of the positive electrode collector 21a, the carbon coating layer 21b, and the negative electrode collector 22a.
[0079] Thereafter, the positive electrode 21, the negative electrode 22, the separator 23, and the sealing material are bonded by welding to form an assembly in which the positive electrode 21, the negative electrode 22, the separator 23, and the sealing portion 24 are integrated together. Examples of a method for welding the sealing material include known welding methods such as heat welding, ultrasonic welding, and infrared welding.
[0080] Next, a liquid electrolyte is injected into the sealed space S inside the assembly through an injection port provided in a part of the seal portion 24, and then the injection port is sealed. In this way, the electricity storage cell 20 is formed. <Cell stack formation process> In the cell stack forming process, first, the multiple energy storage cells 20 are stacked so that the second surface 21a2 of the positive electrode current collector 21a and the second surface 22a2 of the negative electrode current collector 22a face each other. Then, the multiple energy storage cells 20 are integrated by bonding the outer circumferential portions 24a of the seal portions 24 of the energy storage cells 20 adjacent to each other in the stacking direction.
[0081] Next, the positive electrode current-carrying plate 40 is overlapped and fixed in an electrically connected state to the second surface 21a2 of the positive electrode current collector 21a of the positive electrode 21 arranged on the outermost side at one end in the stacking direction. Similarly, the negative electrode current-carrying plate 50 is overlapped and fixed in an electrically connected state to the second surface 22a2 of the negative electrode current collector 22a of the negative electrode 22 arranged on the outermost side at the other end in the stacking direction.
[0082] Next, the operation and effects of this embodiment will be described. (1) A method for producing a positive electrode for a power storage device includes a positive electrode active material layer forming step of applying a positive electrode active material layer forming slurry, which contains an aqueous solvent and has a pH of 5 to 8, to a first surface 21b1 of a carbon coating layer 21b containing carbon and an aqueous binder.
[0083] When the positive electrode active material layer forming slurry is applied to the first surface 21b1 of the carbon coating layer 21b, a chemical reaction of the carbon coating layer 21b caused by the alkaline positive electrode active material layer forming slurry, such as corrosion of the carbon coating layer 21b, can be suppressed, and therefore the adhesion between the positive electrode current collector 21a and the positive electrode active material layer can be improved.
[0084] (2) The positive electrode active material layer forming slurry contains an olivine-type structure positive electrode active material as a positive electrode active material. The olivine-type structure positive electrode active material has a more stable crystal structure, which can improve the adhesion between the positive electrode current collector 21a and the positive electrode active material layer.
[0085] (3) The polyanion compound is LiFePO4. When the polyanion compound is LiFePO4, the effect of (2) above is more pronounced. This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.
[0086] In the present embodiment, the positive electrode active material layer forming step is performed by applying the positive electrode composite material to the first surface 21b1 of the dried and solidified carbon coat layer 21b, but is not limited to this aspect. For example, in the carbon coat layer forming step, the positive electrode composite material may be applied to a predetermined thickness on the carbon coat layer forming slurry before drying and solidification. The carbon coat 21b layer and the positive electrode active material layer 21c may be formed simultaneously by performing a drying and solidification process on the applied positive electrode composite material.
[0087] In order to improve the thermal stability of the positive electrode 21, a heat-resistant layer may be provided on one or both of the first surface 21a1 and the second surface 21a2 of the positive electrode current collector 21a. The heat-resistant layer may be, for example, a layer containing inorganic particles and a binder, and may further contain additives such as a thickener. The same applies to the negative electrode 22.
[0088] The planar shapes of the positive electrode current collector 21a and the positive electrode active material layer 21c are not particularly limited. They may be polygonal, such as rectangular, or may be circular or elliptical. The same is true for the negative electrode current collector 22a and the negative electrode active material layer 22b.
[0089] The shape of the seal portion 24 in a plan view is not particularly limited, and may be a polygonal shape such as a rectangle, a circle, or an ellipse. Between the positive electrode current-carrying plate 40 and the positive electrode current-collector 21a, a conductive layer that adheres closely to the positive electrode current-collector 21a may be disposed in order to improve the conductive contact between the two members. Examples of the conductive layer include a layer containing carbon such as acetylene black or graphite, and a layer having a lower hardness than the positive electrode current-collector 21a, such as a plating layer containing Au or the like. A similar conductive layer may be disposed between the negative electrode current-carrying plate 50 and the negative electrode current-collector 22a.
[0090] The positive electrode active material layer 21c or the negative electrode active material layer 22b may be provided on the second surface 21a2 of the positive electrode current collector 21a. The positive electrode active material layer 21c or the negative electrode active material layer 22b may be provided on the second surface 22a2 of the negative electrode current collector 22a.
[0091] There is no particular limitation on the number of power storage cells 20 constituting the power storage device 10. The number of power storage cells 20 constituting the power storage device 10 may be one. EXAMPLES
[0092] Hereinafter, a more specific embodiment of the above embodiment will be described. Example 1 A slurry for forming a carbon coating layer with a solid content of 30 mass % was prepared by mixing acetylene black as a conductive additive, styrene-butadiene rubber (hereinafter also referred to as "SBR") as an aqueous binder, carboxymethyl cellulose (hereinafter also referred to as "CMC") as a dispersant, and water as an aqueous solvent.
[0093] LiFePO4 (hereinafter also referred to as "LFP") as a positive electrode active material, carbon nanotubes (hereinafter also referred to as "CNT") as a conductive additive, CMC as a dispersant, and SBR as a water-based binder were mixed in the proportions shown in Table 1, and acetic acid as a pH adjuster and water as a solvent were added to prepare a positive electrode mixture with a solid content ratio of 45 mass%. The proportion of acetic acid to LFP was 0.001, and the pH was 7.9.
[0094] The slurry for forming the carbon coating layer was applied in the form of a film by using a doctor blade method to one surface of an aluminum foil having a thickness of 15 μm as a positive electrode current collector. The applied slurry for forming the carbon coating layer was heat-treated at 50° C. to dry and solidify the slurry for forming the carbon coating layer, thereby forming a carbon coating layer having a thickness of 2 μm.
[0095] A film of the positive electrode mixture was applied onto the carbon coating layer by a doctor blade method. The applied positive electrode mixture was heat-treated at 50° C. to dry and solidify the positive electrode mixture, resulting in a coating weight of 50 mg / cm on the carbon coating layer. 2 A positive electrode sheet of Example 1 was produced, in which the positive electrode active material layer was formed.
[0096] Example 2 In Example 2, a positive electrode sheet was produced in the same manner as in Example 1, except that the mixing ratio of acetic acid to LFP was set to 0.01, and the pH of the positive electrode mixture was set to 6.8.
[0097] Example 3 In Example 3, a positive electrode sheet was produced in the same manner as in Example 1, except that the mixing ratio of acetic acid to LFP was set to 0.05, and the pH of the positive electrode mixture was set to 6.2.
[0098] Example 4 In Example 4, a positive electrode sheet was produced in the same manner as in Example 1, except that the mixing ratio of acetic acid to LFP was set to 0.08, and the pH of the positive electrode mixture was set to 5.6.
[0099] Example 5 In Example 5, a positive electrode sheet was produced in the same manner as in Example 1, except that the mixing ratio of acetic acid to LFP was set to 0.1 and the pH of the positive electrode mixture was set to 5.1.
[0100] Comparative Example 1 In Comparative Example 1, a positive electrode sheet was produced in the same manner as in Example 1, except that no acetic acid was added and the pH of the positive electrode mixture was 9.3.
[0101] Comparative Example 2 In Comparative Example 2, a positive electrode sheet was produced in the same manner as in Example 1, except that the mixing ratio of acetic acid to LFP was set to 0.5 and the pH of the positive electrode mixture was set to 4.2.
[0102] (Evaluation of peel strength) The peel strength of the positive electrode sheets of Examples 1 to 5 and Comparative Examples 1 and 2 was measured using a tensile tester. The test method was in accordance with JIS Z 0237. First, an adhesive tape was attached onto the positive electrode active material layer of the positive electrode sheet. The positive electrode sheet was attached onto a base via the adhesive tape with the positive electrode active material layer side facing downward. Next, the peel strength was measured by pulling the aluminum foil of the positive electrode sheet upward in a direction of 90 degrees. The results are shown in Table 1.
[0103] (Evaluation of output characteristics of power storage device) The positive electrode sheet of Example 1 thus prepared was cut into a rectangular shape measuring 30 mm in length and 25 mm in width, and the positive electrode was combined with a negative electrode and a separator to form an electrode body battery. The electrode body battery was housed in a battery case, and an electrolyte was poured into the battery case, which was then sealed to obtain a lithium ion secondary battery.
[0104] The negative electrode used was a negative electrode collector made of copper, and a negative electrode active material layer made of graphite as a negative electrode active material, SBR as a binder, and CMC as a dispersant. The separator used was a separator made of polyethylene. The electrolyte used was a mixed solvent of dimethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, and ethylene carbonate in a volume ratio of 40:35:5:20, in which lithium hexafluorophosphate was dissolved to a concentration of 1.2M.
[0105] The obtained lithium ion secondary battery was charged at a constant current (CC) of 10 mA DC until the voltage of the negative electrode relative to the positive electrode reached 3.75 V, and then discharged to a state of charge (SOC) of 80%. Thereafter, the battery was discharged at a current of 10 C rate at 25° C. for 10 seconds, and the resistance at the time of 10-second discharge (10s resistance) was measured. The results are shown in Table 1.
[0106] The obtained lithium ion secondary battery was charged at a constant current (CC) with a direct current of 10 mA until the voltage of the negative electrode relative to the positive electrode reached 3.75 V, and then discharged to a state of charge (SOC) of 95%. Thereafter, the battery was discharged at a constant current (CC) at 25°C and a current rate of 2.05 C until the voltage of the negative electrode relative to the positive electrode reached 3.00 V, and the ratio of the discharge capacity to the rated capacity was calculated. The results are shown in Table 1.
[0107] In addition, lithium ion secondary batteries were produced in the same manner as above using the positive electrode sheets of Examples 2, 3, and 5 and Comparative Examples 1 and 2, and the output characteristics of the obtained lithium ion secondary batteries were measured in the same manner as above. The results are shown in Table 1.
[0108] [Table 1] As shown in Table 1, in Comparative Example 1, the peel strength was 0.1 N / cm. In the positive electrode sheet after evaluation, the carbon coating layer peeled off from the aluminum foil base material. This is believed to be because the positive electrode mixture in Comparative Example 1 had a high pH of 9.3, and the SBR contained in the carbon coating layer had low alkali resistance, causing corrosion of the carbon coating layer. In Comparative Example 2, the peel strength was 0.11 N / cm. In the positive electrode sheet after evaluation, the positive electrode active material layer peeled off from the carbon coating layer. It is believed that the positive electrode mixture in Comparative Example 2 had a low pH of 4.2, which caused the dispersant in the positive electrode active material layer to condense, resulting in a decrease in dispersibility of the positive electrode mixture.
[0109] In contrast, in Examples 1 to 5, the peel strength was a high value of 0.16 N / cm or more, and it was confirmed that the adhesion was good. Furthermore, in Examples 1, 3, and 5, the 10s resistance value was reduced and the output characteristics were improved compared to Comparative Examples 1 and 2. In particular, it was found that Example 3 had the best 10s resistance and output characteristics. It is believed that the resistance was reduced due to the good adhesion, which resulted in the improved output characteristics. [Explanation of symbols]
[0110] S...sealed space, 10...energy storage device, 20...energy storage cell, 21...positive electrode, 21a...positive electrode current collector, 21b...carbon coating layer, 21c...positive electrode active material layer, 22...negative electrode, 22a...negative electrode current collector, 22b...negative electrode active material layer, 23...separator, 24...seal portion, 30...cell stack, 40...positive electrode current collector, 50...negative electrode current collector.
Claims
[Claim 1] The method includes a step of forming a positive electrode active material layer by applying a positive electrode active material layer-forming slurry containing an aqueous solvent and having a pH of 6 to 7 onto a carbon coating layer of a metal foil having the carbon coating layer containing carbon and an aqueous binder, The positive electrode active material layer forming slurry contains LiFePO having an olivine structure as a positive electrode active material. 4 Including, The LiFePO in the slurry for forming the positive electrode active material layer 4 is 90 to 98 parts by mass when the solid content mass of the positive electrode active material layer forming slurry is 100 parts by mass, The weight of the positive electrode active material layer on one side of the metal foil is 50 mg / cm 2 The method for producing a positive electrode for an electricity storage device is characterized by the above.
Citation Information
Patent Citations
Electrode for storage element, nonaqueous lithium type storage element, and method of manufacturing electrode for storage element
JP2010108703A
Binder for carbon coat foil coating solution, carbon coat foil coating solution, carbon coat foil, electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2013229187A
Electrode for lithium secondary battery and method for manufacturing the same, and lithium secondary battery and method for manufacturing the same
JP2014017199A
Conductive composition, electrode for power storage device, and power storage device
JP2016081704A
Conductive adhesive composition for electrochemical element electrode, collector with adhesive layer, and electrode for electrochemical element
WO2014051043A1