PERFORMANCE EVALUATION METHOD AND PERFORMANCE EVALUATION DEVICE

The method and device efficiently evaluate wear resistance by applying strain and X-ray imaging to detect low-density regions, providing accurate performance assessment of elastic materials.

JP7589534B2Active Publication Date: 2024-11-26SUMITOMO RUBBER INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020208704
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-16
Publication Date
2024-11-26
Estimated Expiration
2040-12-16

AI Technical Summary

Technical Problem

Conventional methods for evaluating the wear resistance of vulcanized rubber are inefficient and lack accuracy.

Method used

A performance evaluation method and device that applies strain to a test piece made of elastic material, uses X-ray imaging to detect low-density regions, and calculates the generation rate of these regions to evaluate wear resistance based on the volume ratio and strain applied.

Benefits of technology

Enables quick and accurate evaluation of wear resistance by detecting low-density regions generated due to strain, allowing for precise prediction of material performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589534000002
    Figure 0007589534000002
  • Figure 0007589534000003
    Figure 0007589534000003
  • Figure 0007589534000004
    Figure 0007589534000004
Patent Text Reader

Abstract

To provide a method for evaluating a performance that can obtain a high test result that is highly correlated to the performance when a vehicle is travelling.SOLUTION: A method for performance evaluation 100 includes: a strain provision step S2 of providing a strain to a test piece made of an elastic material; an imaging step S3 of irradiating the test piece with an X-ray and taking an image of a projected image; a measurement step S4 of measuring a density distribution of the elastic material from the projected image; a detection step S5 of detecting a low density region generated in the inside of the test piece in association with the provision of the strain; and an evaluation step S6 for evaluating the performance of the elastic material on the basis of the rate of generation of a low-density region.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a performance evaluation method for evaluating various performances such as the wear resistance of an elastic material, and a performance evaluation device used therein. [Background technology]

[0002] Conventionally, as a method for evaluating the abrasion resistance of vulcanized rubber, for example, a method for evaluating the abrasion resistance based on the density distribution of an elastic material to which a strain has been applied has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-83182 A Summary of the Invention [Problem to be solved by the invention]

[0004] The conventional method disclosed in the above Patent Document 1 is effective as a new evaluation technique to replace the Lambourn abrasion tester, and further improvements are expected.

[0005] The present invention has been devised in view of the above circumstances, and has as its main object to provide a performance evaluation method and a performance evaluation device that can evaluate the performance of elastic materials more quickly and accurately. [Means for solving the problem]

[0006] The performance evaluation device method according to the first aspect of the present invention is a method for evaluating the performance of an elastic material including rubber or an elastomer, and includes a strain imparting step of imparting strain to a test piece made of the elastic material, a photographing step of irradiating the test piece with X-rays and photographing a projection image, a measurement step of measuring the density distribution of the elastic material from the projection image, a detection step of detecting low-density regions generated inside the test piece as a result of the strain being imparted, and an evaluation step of evaluating the performance of the elastic material based on the generation speed of the low-density regions.

[0007] In the performance evaluation device method of the present invention, it is desirable that the low-density region is a region in which the ratio of the density of the elastic material after the application of the strain to the density of the elastic material before the application of the strain is 10 to 80%.

[0008] In the performance evaluation device method of the present invention, it is desirable that the measurement step includes a step of constructing a tomographic image of the test piece using the projection image, and a step of measuring the density distribution of the elastic material from the tomographic image.

[0009] In the performance evaluation apparatus and method according to the present invention, it is preferable that the distortion is an expansion distortion.

[0010] In the performance evaluation device method according to the present invention, it is desirable that the generation rate is calculated by the following formula (1). ν = V / ε (1) however ν: the generation rate V: Volume ratio (%) of the low density region in the test piece ε: Tensile strain (%) applied to the test piece Let us assume that.

[0011] In the performance evaluation device and method according to the present invention, it is desirable to evaluate the elastic material having the generation speed v of 50 or more as being excellent in wear resistance.

[0012] In the performance evaluation device and method according to the present invention, it is desirable that the tensile strain is 20% or more.

[0013] The elastic material is a rubber obtained by using one or more conjugated diene compounds. In the performance evaluation device and method according to the present invention, it is preferable that the rubber is rubber for tires.

[0014] In the performance evaluation method according to the present invention, the luminance (photons / s / mrad) of the X-rays is 2 / mm 2 / 0.1%bw) is 10 10 It is desirable that the above is the case.

[0015] In the performance evaluation method according to the present invention, the luminance is 10 12 It is desirable that the above is the case.

[0016] The performance evaluation device according to the second aspect of the present invention is a device for evaluating the performance of an elastic material including rubber or an elastomer, and includes a strain imparting unit that imparts strain to a test piece made of the elastic material, an imaging unit that irradiates the test piece with X-rays and captures a projection image, a measurement unit that measures the density distribution of the elastic material from the projection image, a detection unit that detects low-density regions generated inside the test piece as a result of the application of the strain, and an evaluation unit that evaluates the performance of the elastic material based on the generation speed of the low-density regions.

[0017] In the performance evaluation device according to the present invention, it is preferable that the imaging unit has a phosphor for converting X-rays into visible light, and the decay time of the phosphor is 100 ms or less. Effect of the Invention

[0018] In the performance evaluation device method of the first invention, the detection step detects the low-density region generated inside the test piece as the strain is applied. Then, the evaluation step evaluates the performance of the elastic material based on the generation speed of the low-density region. This makes it possible to quickly and accurately evaluate the performance of the elastic material.

[0019] In the second aspect of the present invention, the detection unit detects the low-density region generated inside the test piece as the strain is applied. The evaluation unit evaluates the performance of the elastic material based on the generation speed of the low-density region. This makes it possible to quickly and accurately evaluate the performance of the elastic material. [Brief description of the drawings]

[0020] [Figure 1] 1 is a perspective view showing a schematic configuration of an embodiment of a performance evaluation device of the present invention; [Diagram 2] 1 is a flowchart showing a processing procedure of a performance evaluation method according to the present invention. [Diagram 3] FIG. 2 is an exploded view showing the test piece and the jig in FIG. [Figure 4] FIG. 2 is a diagram showing a schematic example of a projected image captured by the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing low-density regions detected after a tensile strain is applied to a test piece made of elastic material A. [Figure 6] FIG. 2 is a schematic diagram showing low-density regions detected after a tensile strain is applied to a test piece made of elastic material A. [Figure 7] 1 is a graph showing the relationship between elongation strain and the volume fraction of low-density regions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view showing a schematic configuration of a performance evaluation device used in the performance evaluation method of this embodiment. The performance evaluation device 1 of the present invention is a device for evaluating various performances such as wear resistance, chipping resistance, and crack resistance of an elastic material. As shown in Fig. 1, the performance evaluation device 1 of this embodiment includes a distortion applying unit 2, an imaging unit 3, a measuring unit 4, a detecting unit 5, and an evaluating unit 6.

[0022] The strain applying unit 2 applies strain to a test piece 10 made of an elastic material including rubber or an elastomer.

[0023] The strain imparting unit 2 has a pair of jigs 21, 22 to which the test piece 10 is fixed, and a driving unit 23 that imparts strain to the test piece 10 by relatively moving the jigs 21 and 22. The driving unit 23 moves one jig 21, while fixing the other jig 22, in the axial direction of the test piece 10. As a result, the test piece 10 is stretched in the axial direction, and strain is imparted to the test piece 10.

[0024] The strain or load applied to the test piece 10 is detected by a load cell (not shown) or the like. The position and type of the load cell are arbitrary. A predetermined strain or load is applied to the test piece 10 by the strain application unit 2. The drive unit 23 is configured to be able to rotate the test piece 10 and the jigs 21, 22 around the axis of the test piece 10.

[0025] The photographing unit 3 irradiates the test piece 10 with X-rays and photographs a projection image. The photographing unit 3 has an X-ray tube 31 that irradiates X-rays and a detector 32 that detects the X-rays and converts them into an electrical signal. The photographing unit 3 photographs a plurality of projection images while rotating the test piece 10 and the jigs 21, 22 around the axis of the test piece 10, thereby making it possible to obtain projection images of the test piece 10 over the entire circumference.

[0026] The detector 32 has a phosphor 32a for converting X-rays into visible light. The decay time of the phosphor 32a is preferably 100 ms or less. If the decay time of the phosphor 32a exceeds 100 ms, when a plurality of projection images are successively captured while rotating the test piece 10 or the like around the axis of the test piece 10, there is a risk that an afterimage of a previously captured projection image may affect a projection image captured subsequently. From this viewpoint, the decay time of the phosphor 32a is more preferably 50 ms, and even more preferably 10 ms.

[0027] The measuring unit 4 measures the density distribution of the elastic material from the projected image. The detecting unit 5 detects low-density regions generated inside the test piece 10 as strain is applied. The evaluating unit 6 evaluates the performance of the elastic material based on the generation speed of the low-density regions.

[0028] For example, a computer 7 is applied to the measurement unit 4, the detection unit 5, and the evaluation unit 6. The computer 7 includes a main body 71, a keyboard 72, and a display device 73. This main body 71 is provided with a storage device, such as a central processing unit (CPU), a ROM, a working memory, and a hard disk. The storage device stores software for executing the performance evaluation method of this embodiment in advance. The measurement unit 4, the detection unit 5, and the evaluation unit 6 are realized by the central processing unit executing the software.

[0029] 2 shows the procedure of a performance evaluation method 100 for evaluating the performance of an elastic material including rubber or an elastomer using the performance evaluation device 1. The performance evaluation method 100 includes steps S1 to S8.

[0030] In step S1, the test piece 10 is fixed to jigs 21 and 22.

[0031] 3 shows the test piece 10 and jigs 21 and 22. In this embodiment, a cylindrical test piece 10 is used. Such a test piece 10 has symmetry and allows measurement results with high reproducibility to be easily obtained.

[0032] The test piece 10 desirably has a diameter of at least five times its axial length. With such a test piece 10, when strain is applied to the test piece 10, the deformation of the side surface of the test piece 10 is limited. As a result, the volume of the test piece 10 increases, and a very large stress is applied inside the test piece 10. Therefore, the density distribution inside the test piece 10 is easily biased, and the performance evaluation of the elastic material can be performed quickly and easily.

[0033] The test piece 10 is fixed in a state of being sandwiched between the jigs 21 and 22. The upper end surface 10a of the test piece 10 is fixed to the lower end surface 21a of the jig 21, and the lower end surface 10b of the test piece 10 is fixed to the upper end surface 22b of the jig 22. The fixing method can be appropriately selected according to the test environment, etc. For example, fixing by adhesive or fixing by vulcanization adhesion of the elastic material constituting the test piece 10 can be applied. In addition, the test piece 10 may be fixed to the jigs 21 and 22 by providing corresponding engaging parts on the upper end surface 10a, the lower end surface 21a, the lower end surface 10b, and the upper end surface 22b, respectively, and engaging the respective engaging parts.

[0034] An elastic material with a uniform density distribution is used for the test piece 10. An example of the elastic material constituting the test piece 10 is rubber obtained by using one or more conjugated diene compounds. Another example of the elastic material constituting the test piece 10 is rubber for tires.

[0035] In the strain imparting step S2, as shown in FIG. 1, the jig 21 and the jig 22 are moved relatively to each other by the driving unit 23, and strain is imparted to the test piece 10. In this embodiment, the jig 22 is moved in the axial direction of the cylindrical test piece 10, i.e., in the direction away from the jig 21, and the test piece 10 is stretched. The strain of the test piece 10 is not limited to stretching. For example, it may be compressive strain or shear strain. The application of strain in the strain imparting step S2 generates stress inside the elastic material, causing density bias. Then, a low-density region is generated inside the test piece 10.

[0036] The magnitude of the tensile strain is represented by the ratio (%) of the length of the test piece 10 after the strain is applied to the length (height) of the test piece 10 before the strain is applied.

[0037] In the imaging step S3, X-rays are irradiated onto the test piece 10 from the X-ray tube 31 while the test piece 10 is being rotated. The X-rays pass through the test piece 10 and are detected by the detector 32. The detector 32 converts the detected X-rays into an electrical signal and outputs it to the computer 7. The electrical signal output from the detector 32 is processed by the computer 60. As a result, a projection image of the test piece 10 is photographed and acquired.

[0038] When using a test piece 10 whose density is unknown, the photographing step S3 may be started prior to the strain imparting step S2, thereby obtaining projection images for measuring the density of the test piece 10 before and after the strain imparting step S2.

[0039] The strain applied to the test piece 10 may be increased stepwise. In this case, as shown in Fig. 5 described later, the strain applying step S2 and the photographing step S3 are repeated according to the number of steps.

[0040] 4 is a schematic diagram showing the projection images taken after the above steps S1 to S3. The projection images show low-density regions 15 generated inside the test piece 10. The low-density regions 15 can be defined as regions where the density of the elastic material is equal to or lower than a predetermined threshold value, for example. The density of the elastic material can be calculated from the projection images.

[0041] In the measuring step S4, the density distribution of the elastic material is measured from the projection image. The measuring step S4 is executed by the arithmetic processing device of the computer 7. The computer 7 obtains a three-dimensional tomographic image of the test piece 10 by reconstructing the projection image. This allows the three-dimensional density distribution of the elastic material to be measured. That is, the measuring step S4 includes a step of constructing a tomographic image of the test piece 10 using the projection image, and a step of measuring the density distribution of the elastic material from the tomographic image.

[0042] In the detection step S5, the three-dimensional shape of the low-density regions 15 in the test piece 10 is identified from the three-dimensional density distribution of the elastic material. Then, the computer 7 calculates the total volume of the low-density regions 15 generated inside the test piece 10 as a result of the application of strain from the tomographic image.

[0043] Furthermore, in the evaluation step S6, the performance of the elastic material is evaluated based on the generation rate of the low-density region 15. The generation rate is defined as the increase in the volume of the low-density region 15 relative to the increase in strain.

[0044] As a result of extensive research, the inventors of the present application have finally discovered the following regarding the relationship between the generation speed of the low-density regions 15 and the performance of the elastic material.

[0045] In other words, when an elastic material is subjected to strain, such as stretching, localized stress concentration occurs inside the elastic material, causing localized destruction of the molecular structure of the material. Such localized stress concentration points become the starting points of wear in microscopic areas, accelerating the progression of wear.

[0046] Meanwhile, inside the elastic material, the polymer moves so as to avoid the local stress concentration, resulting in the low-density region 15 shown in Fig. 4. Therefore, the faster the generation speed of the initial low-density region 15 when strain is applied, the fewer the points of local stress concentration in the rubber, improving various performances such as wear resistance.

[0047] Therefore, by calculating the generation rate of the low-density regions 15 when strain is applied to the elastic material, the wear performance of the elastic material can be accurately predicted. For example, in an elastic material in which the volume of the low-density regions 15 is generated at a high rate, there are fewer localized stress concentration points, and it can be predicted that various performances such as wear resistance will be improved. Moreover, by calculating the generation rate of the low-density regions 15, various performances can be quantified and evaluated objectively and accurately. Therefore, according to the performance evaluation method 100 using the performance evaluation device 1, the performance of an elastic material can be evaluated quickly and accurately.

[0048] The low-density region 15 is defined as a region in which the ratio of the density of the elastic material after the application of strain to the density of the elastic material before the application of strain is, for example, 10 to 80%. By defining the low-density region 15 in this way, it is possible to accurately estimate a region with little local stress concentration, which is effective in improving the performance of the elastic material.

[0049] 5 and 6 show low-density regions 15 detected after applying the same elongation strain (20%) to a test piece 10A made of elastic material A and a test piece 10B made of elastic material B. More low-density regions 15 were generated in the test piece 10A than in the test piece 10B. For this reason, it can be inferred that local stress concentration is alleviated in the elastic material A compared to the elastic material B.

[0050] The volume of the low-density region 15 can be calculated by adding up the tomographic images obtained by X-ray CT. The thickness of the tomographic image depends on the spatial resolution of the X-ray CT. In this measurement, the volume was calculated by adding up 200 tomographic images with a thickness of 10 μm.

[0051] The generation rate of the low density region 15 is preferably calculated by the following formula (1). ν = V / ε (1) however ν: Generation speed V: Volume ratio of low density region in the test piece (%) ε: Tensile strain applied to the test piece (%) Let us assume that.

[0052] Figure 7 shows the relationship between the elongation strain ε of elastic materials A and B and the volume fraction V of the low-density regions 15. The generation rate ν of the low-density regions 15 is shown by the slopes of lines A and B. Since the generation rate ν of the low-density regions 15 is higher in elastic material A than in elastic material B, local stress concentration is alleviated and destruction of the molecular structure is suppressed.

[0053] Moreover, an elastic material in which the generation rate v of the low-density region 15 is 50 or more may be evaluated as an elastic material with excellent wear resistance. This makes it possible to easily evaluate the wear resistance of the elastic material.

[0054] The tensile strain ε is desirably 20% or more. By setting the tensile strain ε to 20% or more, a low-density region 15 with a sufficient volume is generated inside the elastic material, and the evaluation accuracy of the performance of the elastic material can be easily improved.

[0055] If the tensile strain ε becomes large, adjacent low-density regions 15 may be connected to each other, making it difficult to accurately calculate the generation rate v of the initial low-density regions 15. Therefore, it is desirable for the tensile strain ε to be 100% or less.

[0056] In the photographing step S3, the brightness of the X-rays incident on the test piece 10 is closely related to the S / N ratio of the X-ray scattering data. When the brightness of the X-rays is low, the signal strength tends to be weaker than the statistical error of the X-rays, and it may be difficult to obtain data with a sufficiently good S / N ratio even if the measurement time is extended. From this viewpoint, the brightness of the X-rays (photons / s / mrad 2 / mm 2 / 0.1%bw) is 10 10 A brightness of 10 or more is desirable, and a more desirable brightness is 10 12 That's all.

[0057] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above specific embodiment and can be modified and carried out in various aspects. EXAMPLES

[0058] The elastic materials A to F were evaluated for wear resistance by the present invention, and the correlation with the evaluation of wear resistance by an actual vehicle running test was verified. As comparative examples, the elastic materials A to F were evaluated for wear resistance by using a Lambourn tester by the present invention, and the correlation with the evaluation of wear resistance by an actual vehicle running test was verified.

[0059] The reagents used are as follows: 1. Polymer (1): (1 modifying group) 2. Polymer (2): (2 modified groups; different amount of monomer from polymer (1)) 3. Polymer (3): (3 modified groups; different monomer amounts from polymer (1)) 4. SBR: Nipol NS522 manufactured by Zeon Corporation 5.BR: BR150B manufactured by Ube Industries, Ltd. 6. Modifier: AZMAX Corporation 3-(N,N-dimethylaminopropyl)trimethoxysilane 7. Anti-aging agent: Nocrac 6C (N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 8. Stearic acid: Stearin manufactured by Nippon Oil & Fats Co., Ltd. 9. Zinc oxide: Toho Zinc's Ginrei R 10. Aromatic oil: Diana Process AH-24 (Idemitsu Kosan) 11. Wax: Sunnock Wax manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 12. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Co., Ltd. 13. Vulcanization accelerator (1): Noccela CZ manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 14. Vulcanization accelerator (2): Noccelaer D manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 15. Silica: Degussa Ultrasil VN3 16. Silane coupling agent: Degussa Si69 17. Carbon black: Diablack LH (N326, N2SA: 84 m2 / g) manufactured by Mitsubishi Chemical Corporation

[0060] The monomers and polymers were synthesized by the following method. <Monomer (1)> 50 ml of cyclohexane, 4.1 ml of pyrrolidine, and 8.9 ml of divinylbenzene were added to a 100 ml container that had been thoroughly purged with nitrogen, and 0.7 ml of a 1.6 M n-butyllithium hexane solution was added at 0°C and stirred. After 1 hour, isopropanol was added to stop the reaction, and the monomer (1) was obtained by extraction and purification. <Polymer (1)> In a 1000 ml pressure vessel that had been thoroughly purged with nitrogen, 600 ml of cyclohexane, 12.6 ml of styrene, 71.0 ml of butadiene, 0.06 g of monomer (1), and 0.11 ml of tetramethylethylenediamine were added, and 0.2 ml of a 1.6 M n-butyllithium hexane solution was added at 40°C and stirred. After 3 hours, 0.5 ml of a modifier was added and stirred. After 1 hour, 3 ml of isopropanol was added to terminate the polymerization. After adding 1 g of 2,6-tert-butyl-p-cresol to the reaction solution, it was reprecipitated with methanol and dried by heating to obtain polymer (1). <Polymer (2)> Polymer (2) was obtained in the same manner as in the above-mentioned polymer (1) except that 0.17 g of monomer (1) was used. <Polymer (3)> Polymer (3) was obtained in the same manner as in the above-mentioned polymer (1) except that 0.29 g of monomer (1) was used.

[0061] The test method is as follows. <Generation speed evaluation> For elastic materials C to E, cylindrical test pieces with a diameter of 20 mm and an axial length of 1 mm were prepared, and the performance of the elastic materials was evaluated using the performance evaluation device shown in Fig. 1 and the performance evaluation method shown in Fig. 2. In the strain application step S2, a 20% elongation strain was applied to the test pieces. In step S6, the wear resistance was evaluated based on the generation speed ν of the low-density region 15. The results were expressed as an index, with a larger value indicating better wear resistance.

[0062] <Lambourn test> For elastic materials C to E, the amount of wear was measured using a Lambourn abrasion tester under the conditions of room temperature, a load of 1.0 kgf, and a slip ratio of 30%, and the reciprocal was calculated. The results are expressed as an index with elastic material C being 100, and the larger the value, the more excellent the abrasion resistance.

[0063] <Actual vehicle driving test> A pneumatic tire of size 195 / 65R15 with a tread made of elastic materials C to E was made and fitted to a domestically produced FF vehicle, and the groove depth of the tread after a distance of 8000 km was measured, and the distance traveled per mm of wear of the tread was calculated. The results are expressed as an index with elastic material C being 100, and the higher the value, the better the wear resistance.

[0064] [Table 1]

[0065] As is clear from Table 1, the performance evaluation method of the embodiment has a better correlation with the actual vehicle running test than the comparative example, and it was confirmed that the performance of the elastic material can be predicted with high accuracy. [Explanation of symbols]

[0066] 1. Performance evaluation device 2 Strain imparting section 3. Photography Department 4 Measuring part 5. Detection section 6 Evaluation section 10 Test Pieces 15 Low density area 32a Phosphor 100 Performance Evaluation Method S2 Strain imparting process S3 Shooting Process S4 Measurement process S5 Detection process S6 Evaluation process

Claims

1. 1. A method for evaluating the performance of a resilient material, including a rubber or elastomer, comprising: a strain imparting step of imparting strain to a test piece made of the elastic material; an imaging step of irradiating the test piece with X-rays and capturing a projection image; a measuring step of measuring a density distribution of the elastic material from the projected image; a detection step of detecting a low-density region generated inside the test piece as a result of the application of the strain; and evaluating the performance of the elastic material based on the generation rate of the low density region, the strain is tensile, The production rate is calculated by the following formula (1): The elastic material having the generation rate ν of 50 or more is evaluated as having excellent abrasion resistance. Performance evaluation method. v = V / ε (1) however ν: said generation rate V: Volume ratio (%) of the low density region in the test piece ε: Tensile strain (%) applied to the test piece

2. 2. The performance evaluation method according to claim 1, wherein the low density region is a region in which the ratio of the density of the elastic material after the application of the strain to the density of the elastic material before the application of the strain is 10 to 80%.

3. The measuring step includes: constructing a tomographic image of the test piece using the projection images; The performance evaluation method according to claim 1 or 2, further comprising the step of measuring a density distribution of the elastic material from the tomographic image.

4. A performance evaluation method described in any one of claims 1 to 3, wherein the extension strain is 20% or more.

5. A performance evaluation method described in any one of claims 1 to 4, wherein the elastic material is a rubber obtained using one or more types of conjugated diene compounds.

6. The performance evaluation method described in claim 5, wherein the rubber is rubber for tires.

7. The performance evaluation method according to claim 1, wherein the luminance (photons / s / mrad 2 / mm 2 / 0.1% bw) of the X-rays is 10 10 or more.

8. The performance evaluation method according to claim 7, wherein the luminance is 10 12 or more.

9. An apparatus for evaluating the performance of an elastic material, including rubber or an elastomer, comprising: A strain applying unit that applies a strain to the test piece made of the elastic material; an imaging unit that irradiates the test piece with X-rays and captures a projection image; a measurement unit for measuring a density distribution of the elastic material from the projected image; a detection unit that detects a low-density region generated inside the test piece as the strain is applied; and and an evaluation unit that evaluates the performance of the elastic material based on a generation rate of the low-density region, the strain is tensile, The production rate is calculated by the following formula (1): The elastic material having the generation rate ν of 50 or more is evaluated as having excellent abrasion resistance. Performance evaluation device. v = V / ε (1) however ν: said generation rate V: Volume ratio (%) of the low density region in the test piece ε: Tensile strain (%) applied to the test piece

10. The imaging unit has a phosphor for converting X-rays into visible light, 10. The performance evaluation device according to claim 9, wherein the decay time of the phosphor is 100 ms or less.

Citation Information

Patent Citations

  • Non-destructive testing methods for synthetic fiber ropes and ropes suitable for use in said methods

    JP2015532716A

  • Performance evaluation method and performance evaluation device

    JP2017083182A

  • Method for evaluating reinforcement agent hierarchical structure of high polymer material

    JP2019113488A

  • Method for evaluating performance of elastic material

    JP2020008282A

  • Method for non-destructive testing of synthetic ropes and rope suitable for use therein

    US20150225894A1