Etching method and etching apparatus

By applying a protective film with controlled adsorption properties, the method selectively etches desired films on semiconductor wafers, preventing damage to adjacent films during the etching process.

JP7589578B2Active Publication Date: 2024-11-26TOKYO ELECTRON LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021022826
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-16
Publication Date
2024-11-26
Estimated Expiration
2041-02-16

AI Technical Summary

Technical Problem

Existing etching methods struggle to selectively etch specific films on semiconductor wafers without damaging adjacent films, particularly when etching silicon-containing films like polysilicon and SiGe.

Method used

Applying a protective film containing compounds with hydroxyl groups or water to the substrate, using gases like methanol to selectively protect one film while etching another by controlling the adsorption properties of the protective film on different films, preventing etching gases from reaching unintended films.

Benefits of technology

Enables selective etching of desired films by forming a protective film that seals pores and prevents etching gases from reaching adjacent films, ensuring precise etching without damaging the underlying structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589578000001
    Figure 0007589578000001
  • Figure 0007589578000002
    Figure 0007589578000002
  • Figure 0007589578000003
    Figure 0007589578000003
Patent Text Reader

Abstract

To selectively etch a desired film from among a plurality of types of films formed on the surface of a substrate.SOLUTION: An etching method includes the steps of: supplying a protective film forming gas including at least one of a compound including a hydroxyl group and water to a substrate having a surface on which a first film and a second film are formed, each of the first and second films having a property of being etched by an etching gas, and forming a protective film covering the first film such that the first film is selectively protected from among the first film and the second film when the etching gas is supplied; and selectively etching the second film by supplying the etching gas to the substrate in a state in which the protective film is formed.SELECTED DRAWING: Figure 3A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an etching method and an etching apparatus. [Background technology]

[0002] In constructing a semiconductor device, various films formed on a semiconductor wafer (hereinafter, referred to as a wafer) serving as a substrate are etched. For example, Patent Document 1 describes etching a wafer on which an interlayer insulating film called a low-k film is formed, and forming recesses in the interlayer insulating film for embedding wiring therein. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-63141 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a technique capable of selectively etching a desired film from among multiple types of films formed on a surface of a substrate. [Means for solving the problem]

[0005] The etching method of the present disclosure includes the steps of: supplying a protective film forming gas containing at least one of a compound having a hydroxyl group and water to a substrate having a first film and a second film, each of which is etchable by an etching gas, and forming a protective film that covers the first film so that the first film is selectively protected from the first film and the second film when the etching gas is supplied; supplying an etching gas to the substrate with the protective film formed thereon to selectively etch the second film; Equipped with picture, the first film and the second film are different types of silicon-containing films, The step of forming the protective film is a step of supplying the protective film forming gas to the substrate without turning the gas into plasma. Effect of the Invention

[0006] According to the present disclosure, it is possible to selectively etch a desired film from among a plurality of types of films formed on a surface of a substrate. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a cross-sectional side view of a surface of a wafer undergoing etching according to one embodiment of the present disclosure. [Figure 2A] FIG. 4 is a process diagram illustrating the etching. [Figure 2B] FIG. 4 is a process diagram illustrating the etching. [Figure 2C] FIG. 4 is a process diagram illustrating the etching. [Figure 3A] FIG. 4 is a process diagram illustrating the etching. [Figure 3B] FIG. 4 is a process diagram illustrating the etching. [Figure 4A] FIG. 4 is a process diagram illustrating the etching. [Figure 4B] FIG. 4 is a process diagram illustrating the etching. [Figure 5A] FIG. 4 is a process diagram illustrating the etching. [Figure 5B] FIG. 4 is a process diagram illustrating the etching. [Figure 6] FIG. 2 is a vertical cross-sectional side view of the surface of a wafer after etching processing. [Figure 7A] FIG. 4 is a chart showing an example of gas supply timing during etching. [Figure 7B] FIG. 4 is a chart showing an example of gas supply timing during etching. [Figure 8] FIG. 2 is a plan view of a substrate processing apparatus for performing etching. [Figure 9] 2 is a vertical sectional side view of an etching module provided in the substrate processing apparatus; FIG. [Figure 10A] FIG. 4 is a process diagram illustrating the etching. [Figure 10B] FIG. 4 is a process diagram illustrating the etching. [Figure 10C] FIG. 4 is a process diagram illustrating the etching. [Figure 11] FIG. 11 is a graph showing the results of an evaluation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] A process according to an embodiment of the etching method of the present disclosure will be described below. FIG. 1 shows a vertical cross-sectional side view of the surface of a wafer W on which the process is performed. FIG. 1 shows a vertical cross-sectional side view of the surface of a wafer W on which the process is performed. In the figure, 11 is a SiGe (silicon germanium) film, and a silicon oxide (SiOx) film 12 is laminated on the upper side of the SiGe film 11. A recess 13 is formed in the laminate of the silicon oxide film 12 and the SiGe film 11, and a polysilicon film 14 is embedded in the recess 13. In addition, between the side wall of the polysilicon film 14 and the side wall of the recess 13, a SiOCN film 15, that is, a film composed of silicon, oxygen, nitrogen, and carbon, is provided, which surrounds the side of the polysilicon film 14 and contacts the side wall of the polysilicon film 14 and the side wall of the recess 13, respectively. Therefore, when viewed in the lateral direction, the laminate of the silicon oxide film 12 and the SiGe film 11, the SiOCN film 15, and the polysilicon film 14 are formed so as to be adjacent to each other in this order. The polysilicon film 14 is a film to be etched, and the SiGe film 11 is a film not to be etched.

[0009] The SiOCN film 15 is an interlayer insulating film called a low-k film, and is a porous film. An outline of this embodiment will be described. In this embodiment, the purpose is to selectively etch the polysilicon film 14 out of the polysilicon film 14 and the SiGe film 11. To this end, a protective film forming gas made of alcohol or water (water vapor) and an etching gas such as ClF3 (chlorine trifluoride) gas are alternately and repeatedly supplied. The protective film forming gas is supplied because both the polysilicon film 14 and the SiGe film 11 are etchable by the etching gas. Suppose that the polysilicon film 14 is etched without supplying the protective film forming gas. In that case, during the etching of the polysilicon film 14, the etching gas passes through the holes in the SiOCN film 15 and is supplied to the sidewalls of the SiGe film 11, which results in etching of the sidewalls. The protective film forming gas is supplied to prevent the etching gas from passing through the holes in the SiOCN film 15 and to prevent such etching of the SiGe film 11.

[0010] To describe the protective film forming gas in detail, it exhibits a relatively high adsorptivity to the SiOCN film 15 as shown in the evaluation test described later. Therefore, the protective film forming gas is adsorbed relatively in large amounts to the surface of the SiOCN film 15. That is, the gas is adsorbed relatively in large amounts to the walls of the holes forming the SiOCN film 15, and the holes are sealed. This sealing prevents the etching gas from passing through the holes and being supplied to the SiGe film 11. On the other hand, the protective film forming gas has a low adsorptivity to the polysilicon film 14, so that the protective film is formed on the polysilicon film 14 with a relatively small thickness. Even if such a protective film with a small thickness is formed, it disappears during etching, so that the polysilicon film 14 can be etched.

[0011] The silicon oxide film 12 provided on the lower SiGe film 11 is a mask for preventing the etching of the SiGe film 11, and is a silicon-containing compound, so that it is etchable by the etching gas, like the polysilicon film 14. The protective film forming gas has high adsorption properties on the silicon oxide film 12, so that a protective film is also formed on the silicon oxide film 12. That is, the silicon oxide film 12 is also protected during etching, so that not only is the SiGe film 11 prevented from being etched from the side as described above, but also from being etched from above with high reliability. Regarding the polysilicon film 14 and the silicon oxide film 12, etching is performed in a state where the protective film on the silicon oxide film 12 remains even after the protective film on the polysilicon film 14 disappears during etching. That is, the polysilicon film 14 is selectively etched out of the silicon oxide film 12 and the polysilicon film 14 by utilizing the difference in thickness of the protective film formed.

[0012] As described above, the difference in the degree of hydrogen bond formation is considered to be involved in the cause of the difference in the adsorption of the protective film forming gas between the films. Specifically, the surface of each film is hydrogen-terminated. That is, in the case of the polysilicon film 14, the silicon atoms on the top surface of the film are bonded to hydrogen atoms. No hydrogen bond is formed between the hydrogen-terminated silicon atoms and the hydrogen atoms constituting the hydroxyl group or water. On the other hand, the silicon oxide film 12 and the SiOCN film 15 are also hydrogen-terminated, and the oxygen atoms and nitrogen atoms on the top surface of the film are bonded to hydrogen atoms, but hydrogen bonds can be formed between the oxygen atoms or nitrogen atoms in this state and the hydrogen atoms constituting the hydroxyl group or water. Such differences are considered to be the difference in adsorption described above. As described above, the protective film formed on each film of the wafer W may be liquid or solid.

[0013] Next, referring to FIG. 2 to FIG. 5, the processing performed on the wafer W will be described in order. These FIG. 2 to FIG. 5 are schematic diagrams showing how the surface of the wafer W described in FIG. 1 changes due to processing, and the processing shown in each of these figures is performed in a state in which the wafer W is carried into a processing vessel and the processing vessel is evacuated to a vacuum atmosphere of a predetermined pressure. In the figures, the hole formed in the SiOCN film 15 is indicated as 16. In this embodiment, methanol (CH3OH) is used as the above-mentioned protective film forming gas, and is indicated by the reference numeral 21 in the figures. The above-mentioned etching gas is indicated as 22. And the protective film formed on each surface of the SiOCN film 15 and the silicon oxide film 12 by the above-mentioned methanol 21 is indicated as 23. As described above, the protective film 23 is also formed on the polysilicon film 14, but this protective film 23 is not shown because it is thinner than the protective film 23 formed on each of the SiOCN film 15 and the silicon oxide film 12.

[0014] First, vaporized methanol 21 is supplied into the processing vessel (step S1, FIGS. 2A and 2B). As described above, methanol 21 is easily adsorbed to the SiOCN film 15 and silicon oxide film 12, and therefore, adsorption to the surfaces (upper surfaces) of these films progresses, forming a protective film 23. Also, methanol 21 is adsorbed to the pore walls of the SiOCN film 15 and remains in the pores 16, blocking the pores 16. Therefore, the protective film 23 is also formed in the pores 16, as described above.

[0015] Next, the supply of vaporized methanol 21 into the processing vessel is stopped, and the processing vessel is placed in a state in which exhaust and supply of purge gas, such as N2 (nitrogen) gas, are performed inside the processing vessel (step S2, FIG. 2C). As a result, the methanol 21 that is not adsorbed by each film and does not form the protective film 23 is removed by the air flow of the exhausted purge gas.

[0016] Then, the etching gas 22 is supplied into the processing vessel. The protective film 23 formed on each film is etched, but as described above, the protective film 23 on the polysilicon film 14 is thin and disappears during etching. Therefore, the protective film 23 is formed only on the SiOCN film 15 and the silicon oxide film 12, and the polysilicon film 14 is selectively etched to expose the sidewall on the upper side of the SiOCN film 15 (step S3, FIG. 3A). Since the hole 16 on the upper side of the SiOCN film 15 is blocked by the methanol 21, the etching gas 22 is prevented from passing through the hole 16 and being supplied to the sidewall of the SiGe film 11. That is, as described above, etching from the side of the SiGe film 11 through the hole 16 is prevented. Thereafter, the supply of etching gas 22 into the processing vessel is stopped, and the processing vessel is placed in a state in which exhaust and supply of purge gas are performed (step S4, FIG. 3B), and the etching gas 22 remaining in the processing vessel is removed by the air flow of purge gas exhausted from the processing vessel.

[0017] Subsequently, vaporized methanol 21 is supplied into the processing vessel. That is, step S1 is executed again. In the above step S3, the polysilicon film 14 is etched, and the sidewall on the upper side of the SiOCN film 15 is exposed. Therefore, the methanol 21 in the gas supplied in this second step S1 is supplied to the hole 16 in the SiOCN film 15 below the hole 16 to which the methanol 21 was supplied in the first step S1, and is adsorbed by the hole wall to close the hole 16 (FIG. 4A). In addition, a protective film 23 is formed on the sidewall of the exposed SiOCN film 15.

[0018] Then, exhaust and supply of purge gas into the processing vessel are performed again in step S2. Then, etching gas 22 is supplied into the processing vessel in step S3. At this time, as in the first etching, the protective film 23 formed on the polysilicon film 14 disappears quickly, while the protective film 23 remains on the SiOCN film 15 and the silicon oxide film 12, and the polysilicon film 14 is selectively etched further downward. As a result, the exposed area on the sidewall of the SiOCN film 15 expands downward.

[0019] Moreover, the second step S1 expands the area in the SiOCN film 15 to which the methanol 21 is supplied downward. Therefore, the methanol 21 remains in the holes 16 near the sidewalls of the SiOCN film 15 newly exposed by etching the polysilicon film 14. Therefore, even in the second step S3, the etching gas is prevented from passing through the holes 16 in the SiOCN film 15 and etching the silicon oxide film 12 (FIG. 4B). After this etching, exhaust and supply of purge gas are performed again in step S4.

[0020] If steps S1 to S4 performed in this order are regarded as one cycle, then even after step S4 is performed for the second time, the cycle is repeated and the polysilicon film 14 is etched downward. Then, when the polysilicon film 14 is completely etched and a predetermined number of cycles are completed (FIG. 5A), the wafer W is heated (step S5). By this heating, the methanol 21 forming the protective film 23 is vaporized and removed from the wafer W (FIG. 5B).

[0021] In the above series of processes, the methanol 21 has been described as remaining on the surface of the wafer W during etching, but it may remain on the surface of the wafer W as a reaction product by reacting with the etching gas 22. If such a reaction product is generated, heating is performed in step S5 so as to remove the reaction product. That is, the heating in step S5 is for removing the methanol 21 and / or the reaction product, and specifically, the wafer W is heated to, for example, 100°C to 400°C. FIG. 6 shows the surface of the wafer W after step S5 is performed, and in the recess 13 formed by removing the polysilicon film 14, a gate of a semiconductor device is formed in a later process, for example.

[0022] As described above, according to the process of the embodiment, the difference in the adsorptivity of the methanol 21 between the silicon oxide film 12, the polysilicon film 14, and the SiOCN film 15 is utilized to form the protective film 23 on the polysilicon film 14, which is thinner than the other films. As a result, the other films are covered with the protective film 23 during etching, while the polysilicon film 14 is not covered with the protective film 23, and the polysilicon film 14 can be selectively etched. When etching the polysilicon film 14 in this manner, the protective film 23 formed in the hole 16 of the SiOCN film 15 prevents the etching gas 22 from passing through the hole 16, and prevents the SiGe film 11 from being etched from the side. In addition, by sealing the hole of the SiOCN film 15, which is a porous film, the silicon oxide film 12 is also prevented from being etched from the side.

[0023] The exhaust flow rate of the processing vessel may be constant in the above steps S1 to S4, or the exhaust flow rate in steps S2 and S4 for removing unnecessary gases from the processing vessel may be set to be larger than the exhaust flow rate in steps S1 and S3 so as to more reliably remove the gases. Also, in steps S2 and S4, the unnecessary gases may be removed only by exhaust without supplying a purge gas.

[0024] 1 is an example, and the Si film to be etched is not limited to the polysilicon film 14, but may be, for example, an amorphous silicon (α-Si) film. The porous film is also not limited to the SiOCN film 15, and a porous film such as a SiCO film or a SiCOH film may be formed instead of the SiOCN film 15. Also, an example was shown in which methanol, an alcohol, was used as the protective film forming gas, but as described above, it is sufficient to use the difference in adsorptivity of each film due to the hydroxyl group to protect the underlying film (SiGe film 11) as described above while etching the polysilicon film 14. Therefore, alcohols other than methanol, such as ethanol and isopropyl alcohol, can also be used as the protective film forming gas, and phenols can also be used as the protective film forming gas. Furthermore, a gas in which a plurality of substances selected from various compounds having a hydroxyl group or water are mixed may be used as the protective film forming gas.

[0025] In the above embodiment, steps S1 to S4 are repeated three or more times, but the number of repetitions is not limited to the above example and may be, for example, two times. Also, steps S1 to S4 may be performed only once without repetition. Incidentally, the above steps S2 and S4 for removing unnecessary gases may be omitted. Specifically, as shown in FIG. 7A showing the timing of supplying a protective film forming gas and an etching gas into the processing vessel, one of the protective film forming gas and the etching gas may be supplied without an interval from the end of supplying the other gas. Also, even when steps S2 and S4 are omitted, steps S1 and S3 for supplying a protective film forming gas and an etching gas, respectively, are not limited to being repeated and may be performed only once.

[0026] In addition, the protective film forming gas and the etching gas 22 are not limited to being supplied in that order. In other words, the protective film forming gas and the etching gas 22 are not limited to being supplied after the supply of one of them is finished, and the protective film forming gas and the etching gas may be simultaneously supplied to the wafer W for processing, as shown in Fig. 7B. When the protective film forming gas and the etching gas 22 are simultaneously supplied in this manner, the formation of the protective film 23 and the etching of the polysilicon film 14 are performed in parallel.

[0027] As described above, the protective film is formed and the polysilicon film 14 is etched, but residues may adhere to the surface of the wafer W after etching (after step S3). The residues are considered to be CF-based compounds composed of C (carbon) constituting the protective film forming gas and F (fluorine) constituting the etching gas, that is, reaction products between the protective film forming gas and the etching gas. In order to remove the residues, a gas containing fluorine may be supplied as a purge gas in step S4 after etching. The residues are reacted with the purge gas to be changed into CF-based compounds different from the compounds constituting the residues, and are then sublimated and removed. By removing the residues in this way, when steps S1 to S4 are repeated as described above, the supply of the etching gas to the polysilicon film 14 is prevented from being hindered by the residues, and the amount of etching of the polysilicon film 14 is prevented from decreasing.

[0028] Note that the purging in step S4 is performed with an inert gas such as N2 gas, which will be described later, and steps S1 to S4 are repeated as described above. After this repetition, a fluorine-containing gas may be supplied as a purge gas before the heat treatment in step S5 is performed, and the residues accumulated on the surface of the wafer W may be sublimated and removed all at once. In this case, the residues are prevented from remaining attached to the wafer W after the treatment is completed, and a decrease in the yield of semiconductor devices is suppressed.

[0029] The fluorine-containing gas for sublimating the residue may be the same as the etching gas or may be different. Specific examples include ClF3 (chlorine trifluoride gas), IF5 (iodine pentafluoride) gas, BrF3 (bromine trifluoride) gas, and IF7 (iodine heptafluoride) gas. As described above, the residue is considered to be derived from the carbon atoms of the protective film forming gas. Therefore, it is considered that the amount of the residue generated can be relatively small or no residue can be generated by using, for example, a compound with a relatively small number of carbon atoms as the protective film forming gas. In other words, the sublimation process of the residue using the fluorine-containing gas is not essential. In addition, the evaluation test described below shows that methanol, ethanol, isopropyl alcohol, and water, that is, compounds with a very small carbon number of 0 to 3, can be used as the protective film forming gas. These compounds can be preferably used from the viewpoint of reducing the amount of the residue generated.

[0030] In the above embodiment, in step S5, the wafer W is heated so that the methanol 21 and / or the reaction products of the methanol 21 and the fluorine in the etching gas are removed from the SiOCN film 15. However, even if the methanol 21 and / or the reaction products are adsorbed on the surfaces (including the surfaces of the holes 16) of the silicon oxide film 12 and the SiOCN film 15, they may remain as such if there is no problem in the subsequent processing steps or in the practical use of the product. Therefore, the heat treatment in step S5 is not necessarily essential.

[0031] Next, a substrate processing apparatus 3 for performing the above-mentioned series of processes will be described with reference to the plan view of Fig. 8. The substrate processing apparatus 3 includes a load / unload section 31 for loading and unloading the wafer W, two load lock chambers 41 provided adjacent to the load lock chambers 31, two heat treatment modules 40 provided adjacent to the two load lock chambers 41, respectively, and two etching modules 5 provided adjacent to the two heat treatment modules 40, respectively.

[0032] The load / unload section 31 includes an atmospheric pressure transfer chamber 33 in which a first substrate transfer mechanism 32 is provided and which is kept under atmospheric pressure, and a carrier mounting table 35 provided on the side of the atmospheric pressure transfer chamber 33 and on which a carrier 34 storing a wafer W is mounted. In the drawing, reference numeral 36 denotes an orienter chamber adjacent to the atmospheric pressure transfer chamber 33, which is provided for rotating the wafer W to optically determine the amount of eccentricity and for aligning the wafer W with respect to the first substrate transfer mechanism 32. The first substrate transfer mechanism 32 transfers the wafer W between the carrier 34 on the carrier mounting table 35, the orienter chamber 36, and a load lock chamber 41.

[0033] A second substrate transfer mechanism 42 having, for example, a multi-joint arm structure is provided in each load lock chamber 41, and the second substrate transfer mechanism 42 transfers the wafer W between the load lock chamber 41, the heat treatment module 40, and the etching module 5. The inside of the processing vessel constituting the heat treatment module 40 and the inside of the processing vessel constituting the etching module 5 are in a vacuum atmosphere, and the inside of the load lock chamber 41 can be switched between a normal pressure atmosphere and a vacuum atmosphere so that the wafer W can be transferred between the inside of these vacuum atmosphere processing vessels and the normal pressure transfer chamber 33.

[0034] In the drawing, reference numeral 43 denotes a gate valve that can be opened and closed, and is provided between the normal pressure transfer chamber 33 and the load lock chamber 41, between the load lock chamber 41 and the heat treatment module 40, and between the heat treatment module 40 and the etching module 5. The heat treatment module 40 includes the above-mentioned processing vessel, an exhaust mechanism for exhausting the inside of the processing vessel to form a vacuum atmosphere, and a mounting table that is provided in the processing vessel and is capable of heating the wafer W placed thereon, and is configured to be able to perform the above-mentioned step S5.

[0035] Next, the etching module 5 will be described with reference to the vertical cross-sectional side view of FIG. 9. The etching module 5 is a module that performs the processes of steps S1 to S4 on the wafer W, and includes, for example, a circular processing vessel 51. That is, the processes of steps S1 to S4 are performed in the same processing vessel. The processing vessel 51 is an airtight vacuum vessel, and a circular mounting table (stage) 61 is provided at the lower side of the processing vessel 51, on whose horizontally formed surface (upper surface) the wafer W is mounted. In the figure, 62 is a stage heater embedded in the mounting table 61, and heats the wafer W to a predetermined temperature so that the processes of steps S1 to S4 can be performed. In the figure, 63 is a support that supports the mounting table 61, which is a mounting part, on the bottom surface of the processing vessel 51. In the figure, 64 is a vertical lift pin that is raised and lowered by a lift mechanism 65 to the surface of the mounting table 61, and transfers the wafer W between the above-mentioned second substrate transfer mechanism 42 and the mounting table 61. Three lift pins 64 are provided, but only two are shown.

[0036] In the figure, 66 denotes a sidewall heater provided on the sidewall of the processing vessel 51, which adjusts the temperature of the atmosphere inside the processing vessel 51. The sidewall of the processing vessel 51 is provided with an openable and closable transfer port for the wafer W (not shown). In the figure, 67 denotes an exhaust port opening in the bottom surface of the processing vessel 51, which is connected via an exhaust pipe to an exhaust mechanism 68 composed of a vacuum pump, a valve, etc. The pressure inside the processing vessel 51 is adjusted by adjusting the exhaust flow rate from the exhaust port 67 by the exhaust mechanism 68.

[0037] A gas shower head 7 constituting a protective film forming gas supply unit and an etching gas supply unit is provided on the ceiling of the processing vessel 51 above the mounting table 61 so as to face the mounting table 61. The gas shower head 7 includes a shower plate 71, a gas diffusion space 72, and a diffusion plate 73. The shower plate 71 is provided horizontally to form the lower surface of the gas shower head 7, and a large number of gas discharge holes 74 are formed in a distributed manner to discharge gas to the mounting table 61. The gas diffusion space 72 is a flat space formed such that the lower side is partitioned by the shower plate 71 in order to supply gas to each gas discharge hole 74. A diffusion plate 73 is provided horizontally to divide the gas diffusion space 72 into upper and lower parts. In the figure, 75 denotes through holes formed in the diffusion plate 73, and a large number of holes are formed in the diffusion plate 73 in a distributed manner. In the figure, 77 denotes a ceiling heater, which adjusts the temperature of the gas shower head 7.

[0038] The downstream ends of gas supply pipes 78 and 81 are connected to the upper side of the gas diffusion space 72. The upstream side of the gas supply pipe 78 is connected to a ClF3 gas supply source 70 via a flow rate adjustment unit 79. The flow rate adjustment unit 79 is composed of a valve and a mass flow controller, and adjusts the flow rate of gas supplied to the downstream side of the gas supply pipe 78. Each flow rate adjustment unit described later is also configured in the same way as the flow rate adjustment unit 79, and adjusts the flow rate of gas supplied to the downstream side of the pipe in which the flow rate adjustment unit is installed.

[0039] The upstream side of gas supply pipe 81 is connected to tank 83 in which methanol gas is stored via flow rate adjuster 82, and is configured to be able to supply the methanol gas to the downstream side of gas supply pipe 81. For example, gas supply pipe 81 branches upstream of flow rate adjuster 82 to form gas supply pipe 84. Gas supply pipe 84 is connected to N2 (nitrogen) supply source 86 via flow rate adjuster 85. Therefore, methanol gas and N2 gas can be supplied to gas showerhead 7 independently.

[0040] The correspondence between the above steps S1 to S4 performed in the etching module 5 and the gas supplied from the gas shower head 7 will be described. In step S1, methanol gas is supplied from the tank 83 to the gas shower head 7 and then supplied into the processing vessel 51. In steps S2 and S4, N2 gas is supplied from the N2 gas supply source 86 to the gas shower head 7 and then supplied as a purge gas into the processing vessel 51. In step S3, the supply of gas from the tank 83 and the N2 gas supply source 86 is stopped, and ClF3 gas is supplied from the supply source 70 to the gas shower head 7 and then supplied into the processing vessel 51.

[0041] As shown in FIG. 8 and FIG. 9, the substrate processing apparatus 3 includes a control unit 30, which is a computer, and the control unit 30 includes a program, a memory, and a CPU. The program includes commands (each step) for processing the wafer W and transporting the wafer W, and the program is stored in a computer storage medium, such as a compact disk, a hard disk, a magneto-optical disk, or a DVD, and is installed in the control unit 30. The control unit 30 outputs control signals to each part of the substrate processing apparatus 3 according to the program, and controls the operation of each part. Specifically, the operation of the etching module 5, the operation of the heat treatment module 40, the operation of the first substrate transport mechanism 32, the operation of the second substrate transport mechanism 42, and the operation of the orienter chamber 36 are controlled by the control signals. The operation of the etching module 5 includes the adjustment of the output of each heater, the supply and cut-off of each gas from the gas shower head 7, the adjustment of the exhaust flow rate by the exhaust mechanism 68, and the raising and lowering of the lift pins 64 by the lift mechanism 65. The control unit 30 and the etching module 5 constitute an etching apparatus.

[0042] The transfer path of the wafer W in the substrate processing apparatus 3 will be described. As described in FIG. 1, the carrier 34 storing the wafer W on which each film is formed is placed on the carrier mounting table 35. The wafer W is then transferred in the order of the normal pressure transfer chamber 33 → the orienter chamber 36 → the normal pressure transfer chamber 33 → the load lock chamber 41, and transferred to the etching module 5 via the heat treatment module 40. Then, as described above, the cycle consisting of steps S1 to S4 is repeated to process the wafer W. The wafer W is then transferred to the heat treatment module 40 and subjected to the process of step S5. Thereafter, the wafer W is transferred in the order of the load lock chamber 41 → the normal pressure transfer chamber 33, and returned to the carrier 34.

[0043] In addition, in the etching module 5, the above-mentioned fluorine-containing gas (purge gas) may be supplied to remove the residue after etching. When ClF3 gas, which is an etching gas, is used as the purge gas for removing the residue, the piping system of the etching module 5 may be configured as described above. When a gas other than ClF3 gas is used as the purge gas for removing the residue, a pipe for the purge gas equipped with a flow rate regulator may be added to the above-mentioned piping system so that the purge gas can be supplied to the gas shower head independently of the ClF3 gas, methanol gas, and N2 gas. Alternatively, the supply of methanol gas and the supply of etching gas may be performed in different processing vessels, and the wafer W may be transported between these processing vessels by a transport mechanism. However, by supplying these gases in the same processing vessel, the time required to transport the wafer W between modules can be saved when repeating the above cycle. Therefore, the configuration of the substrate processing apparatus 3 can improve the throughput.

[0044] 1 to 6 show an example in which a protective film is formed with a first thickness and a second thickness smaller than the first thickness due to the difference in the adsorptivity of the protective film forming gas for the silicon oxide film 12, which is a first film, and the polysilicon film 14, which is a second film, and the polysilicon film 14 is selectively etched. As shown in the evaluation test described later, the protective film forming gas shows different adsorptivity for various films, but if the first film (the film to be protected) and the second film (the film to be etched) have a higher adsorptivity for the protective film forming gas, selective etching can be performed for the second film. In other words, when selectively etching the second film of the first film and the second film, the first film and the second film formed on the surface of the wafer W are not limited to the silicon oxide film 12 and the polysilicon film 14, respectively, and may have different adsorptivity for the protective film forming gas.

[0045] Among silicon-containing compounds, compounds containing N or O as described above tend to form hydrogen bonds with compounds containing hydroxyl groups or with water. Therefore, in addition to the already-exemplified SiOCN and silicon oxide, for example, SiN can be used as the first film. For example, silicon-containing compounds not containing N or O, such as SiC (silicon carbide), can be used as the second film. Incidentally, the inclusion of N or O here means that they are included as constituent elements of the film, and does not mean that they are included as impurities.

[0046] To describe a specific processing example, assume that a SiC film 91 (second film) and a SiN film 92 (first film) are formed side by side on the surface of a wafer W as shown in Fig. 10A. A protective film forming gas is supplied, and a protective film 23 is formed thicker on the SiN film 92 than on the SiC film 81 (Fig. 10B). An etching gas 22 is supplied to etch the SiC film 91 while protecting the SiN film 92 (Fig. 10C).

[0047] Incidentally, it has been stated that a protective film is formed on the second film (film to be etched) by the protective film forming gas with a second thickness, but this second thickness may be zero. That is, the protective film forming gas may not have adsorptivity to the second film, and no protective film may be formed on the second film. The first film and the second film are not limited to silicon-containing compounds, and may be, for example, metal films.

[0048] As described above, the film to be etched is not limited to the polysilicon film shown in Figures 1 to 6. Therefore, the etching gas is also appropriately selected depending on the film to be etched. In order to etch silicon-containing compounds such as Si and SiC as described above, gases made of fluorine compounds such as F2 gas, IF5 gas, BrF3 gas, and IF7 gas can be used in addition to ClF3 gas.

[0049] In the above embodiment, the first film to be protected and the second film to be etched are shown aligned horizontally, but these films may be arranged vertically, for example, as long as they are exposed on the surface of the substrate. In other words, there is no limitation on the positional relationship of these films. Furthermore, the embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above embodiment may be omitted, substituted, modified, and / or combined in various forms without departing from the scope and spirit of the appended claims.

[0050] (Evaluation test) Evaluation tests carried out in relation to the technology of the present disclosure will be described. As an evaluation test, the adsorption energy of various molecules including Si was measured by simulation for methanol, ethanol, isopropyl alcohol, and water, which are compounds each having a hydroxyl group. Specifically, the adsorption energy of Si (silicon), SiC (silicon carbide), SiN (silicon nitride), SiO2CN (=SiOCN), and SiO (silicon oxide) was measured.

[0051] Figure 11 is a bar graph showing the results of the evaluation test. The vertical axis of the graph shows the adsorption energy (unit: eV), and the lower the adsorption energy, the easier the adsorption. As shown in this Figure 11, the adsorption energy of compounds with hydroxyl groups and water differs between Si, SiC, SiN, SiO2CN, and SiO. Among these, the adsorption energy of compounds with hydroxyl groups and water for SiN, SiO2CN, and SiO is significantly negative compared to Si and SiC. In this way, compounds with hydroxyl groups and water have a higher adsorption property to SiN, SiO2CN, and SiO compared to Si and SiC.

[0052] From the results of this evaluation test, it is found that the adsorption of various compounds having hydroxyl groups and water differs for each type of silicon-containing film. Therefore, it is presumed that, as described in the embodiment, by utilizing the difference in the adsorption of such compounds having hydroxyl groups and water, one of these silicon-containing films can be protected while etching the other film. Furthermore, the graph in FIG. 11 shows that the difference in adsorption energy between Si and SiO is particularly large. Furthermore, it is shown that the difference in adsorption energy between Si and SiOCN is also large. Therefore, it is found that selective etching of the Si film using the protective film 23 described in the embodiment can be performed. Furthermore, since the adsorption energy of compounds having hydroxyl groups and water is low for SiOCN, it is found that the hole 16 of the SiOCN film 15 described in the embodiment can be sufficiently sealed. [Explanation of symbols]

[0053] W wafer 12 Silicon oxide film 14 Polysilicon film 21 Methanol 22 Etching gas 23 Protective film

Claims

1. supplying a protective film forming gas containing at least one of a compound having a hydroxyl group and water to a substrate having a first film and a second film, each of which has an etching property with respect to an etching gas, and forming a protective film covering the first film so that the first film is selectively protected from the first film and the second film when the etching gas is supplied; supplying an etching gas to the substrate with the protective film formed thereon to selectively etch the second film; Equipped with the first film and the second film are different types of silicon-containing films, The etching method, wherein the step of forming the protective film is a step of supplying the protective film forming gas to the substrate without turning the protective film forming gas into plasma.

2. 2. The etching method according to claim 1, wherein the first film contains nitrogen or oxygen.

3. 3. The etching method according to claim 2, wherein the first film is any one of a SiOCN film, a silicon oxide film, and a silicon nitride film, and the second film is a Si film or a SiC film.

4. the first film, the porous film, and the second film are provided adjacent to each other in this order on the substrate; The step of forming the protective film includes a step of forming the protective film in a hole portion of the porous film to close the hole portion, 4. The etching method according to claim 1, wherein the step of selectively etching the second film includes the step of supplying an etching gas in a state where the pores of the porous film are blocked.

5. 5. The etching method according to claim 1, wherein the compound having a hydroxyl group is an alcohol.

6. 6. The etching method according to claim 1, further comprising a heating step of heating the substrate to remove the protective film or a reaction product generated by a reaction between the protective film and the etching gas after performing the steps of forming the protective film and selectively etching the second film.

7. 7. The etching method according to claim 1, further comprising a repeating step of repeating the step of forming the protective film and the step of selectively etching the second film in this order a plurality of times.

8. 7. The etching method according to claim 1, further comprising a step of simultaneously supplying the protective film forming gas and the etching gas to the substrate, and the step of selectively etching the second film is performed simultaneously with the step of forming the protective film.

9. 9. The etching method according to claim 1, further comprising a residue removing step of supplying a gas containing fluorine to remove residues generated in the step of selectively etching the second film.

10. A processing vessel; a stage provided in the processing vessel, the stage being configured to support a substrate having a first film and a second film formed on a surface thereof, the first film and the second film being different types of silicon-containing films and each of the first film and the second film being etchable by an etching gas supplied into the processing vessel; a protective film forming gas supply unit that supplies a protective film forming gas containing at least one of a compound having a hydroxyl group and water to the substrate in the processing vessel without plasma generation, and forms a protective film that covers the first film so that the first film is selectively protected from among the first film and the second film when the etching gas is supplied; an etching gas supply unit that supplies the etching gas into the processing vessel in order to selectively etch the second film in a state in which the protective film is formed; An etching apparatus comprising:

Citation Information

Patent Citations

  • Dry etching method and dry etching device

    JP2002313776A

  • Silicon etching method and apparatus with passivation using plasma-assisted oxidation

    JP2012507144A

  • Semiconductor device manufacturing method

    JP2015084404A

  • Method for manufacturing semiconductor device, and coat film formation method and device

    JP2016063141A

  • Etching method and etching device

    JP2020167285A