Manufacturing method of power storage device

By arranging resin members beyond the metal foil ends and using transmitting pressure members, the method ensures complete welding and coverage of metal foils while preventing resin adhesion to pressure members, addressing the challenges of conventional laser joining methods.

JP7589719B2Active Publication Date: 2024-11-26TOYOTA JIDOSHA KK
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2022115470
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-20
Publication Date
2024-11-26
Estimated Expiration
2042-07-20

AI Technical Summary

Technical Problem

Conventional laser joining methods for bonding metal and resin can result in the resin being welded to the pressure member on the opposite side of the laser irradiation, making it difficult to remove the product, especially when thin metal foils are used, and may lead to incomplete welding due to uneven temperature distribution.

Method used

The method involves arranging thermoplastic resin members on both sides of a thin metal foil, with their ends extending beyond the foil ends, and using pressure members that transmit electromagnetic waves to weld the resin members to the foil while irradiating from one side, ensuring equal temperature distribution and preventing resin from welding to the pressure members.

Benefits of technology

This approach allows for successful welding of resin members to cover the metal foil ends without adhering to the pressure members, achieving complete coverage and strong bonding in a short processing time with energy efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589719000002
    Figure 0007589719000002
  • Figure 0007589719000003
    Figure 0007589719000003
  • Figure 0007589719000004
    Figure 0007589719000004
Patent Text Reader

Abstract

To provide a method for manufacturing a power storage device in which a step of covering the end of a metallic foil with a resin member welds the resin member to the metal member by irradiation with electromagnetic waves from one surface while suppressing welding of the resin member to the pressurization member.SOLUTION: A method for manufacturing a power storage device includes: an arrangement step of arranging a first resin member on a first surface of a metallic foil 1 having a thickness of 1 μm or more and 100 μm or less so that the end of the first resin member 2 becomes longer than the end of the metallic foil, and arranging a second resin member on a second surface of the metallic foil so that the end of the second resin member 3 becomes longer than the end of the metallic foil; and a welding step of arranging a first pressurization member 4 permeating electromagnetic waves on a surface opposite to the surface on the metallic foil side of the first resin member, arranging a second pressurization member 5 on a surface opposite to a surface on the metallic foil side of the second resin member, irradiating the end of the metallic foil with electromagnetic waves from the first pressurization member side while pressurizing the metallic foil with the first pressurization member and the second pressurization member, and thereby welding the first resin member and the second resin member to the metallic foil so as to cover the end of the metallic foil.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing an electricity storage device, the method including a step of welding a resin to a metal. [Background technology]

[0002] Conventionally, there are known methods for joining metal and resin with a laser. For example, Patent Document 1 discloses a method for joining metal and resin by applying pressure to a joint between the metal and resin with a pressure member and irradiating the joint with a laser. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-56308 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, as a measure to prevent corrosion and rust of metal members, it is known to cover the ends of the metal members with a resin member. When such a structure is produced using the above-mentioned laser joining method, if the metal member is a thin metal foil, the resin member may be welded to the pressure member on the opposite side to the laser irradiation side, making it impossible to remove the product.

[0005] The present disclosure has been made in consideration of the above-mentioned situation, and has a primary object to provide a manufacturing method for an energy storage device, which is capable of welding a resin member to a metal member so as to cover the end of the metal member by irradiating electromagnetic waves from one side of the metal member, while suppressing welding of the resin member to a pressure member in a process of covering the end of the metal foil with the resin member. [Means for solving the problem]

[0006] [1] a first resin member that contains a thermoplastic resin and is transparent to electromagnetic waves, on a first surface of a metal foil having a thickness of 1 μm or more and 100 μm or less, such that an end of the first resin member is longer than an end of the metal foil, and a second resin member that contains a thermoplastic resin and is transparent to electromagnetic waves, on a second surface of the metal foil, such that an end of the second resin member is longer than an end of the metal foil; and a welding step of: placing a first pressure member that is transparent to electromagnetic waves on a surface of the first resin member opposite to a surface of the metal foil side, placing a second pressure member that is transparent to electromagnetic waves on a surface of the second resin member opposite to a surface of the metal foil side, and welding the first resin member and the second resin member to the metal foil so as to cover the end of the metal foil by irradiating electromagnetic waves from the first pressure member side while applying pressure with the first pressure member and the second pressure member. [2] The method for manufacturing an energy storage device according to [1], wherein in the placing step, the distance between an end of the metal foil and an end of the first resin member, and the distance between the end of the metal foil and an end of the second resin member are each 0.5 mm or more. [3] The method for producing an electricity storage device according to [1] or [2], wherein the metal foil is a current collector of a battery. Effect of the Invention

[0007] In the present disclosure, while suppressing welding of the resin member to the pressure member, it is possible to weld the resin member to the metal member so as to cover the end of the metal member by irradiating one side of the metal member with electromagnetic waves. [Brief description of the drawings]

[0008] [Figure 1] 1A to 1C are schematic cross-sectional views illustrating an arrangement step and a welding step in the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view illustrating a welding process in the present disclosure. [Diagram 3] 1A and 1B are schematic plan views illustrating the arrangement steps in the examples and comparative examples, and optical microscope photographs of Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The manufacturing method of the electric storage device according to the present disclosure will be described in detail below with reference to the drawings. Each of the drawings shown below is a schematic illustration, and the size and shape of each part are appropriately exaggerated to facilitate understanding. In addition, in this specification, when expressing an aspect in which another member is arranged relative to a certain member, the term "above" or "below" simply refers to both a case in which another member is arranged directly above or below a certain member so as to be in contact with the certain member, and a case in which another member is arranged above or below a certain member via another member, unless otherwise specified.

[0010] FIG. 1 is a schematic cross-sectional view illustrating the arrangement step and the welding step in the present disclosure. First, as shown in FIG. 1(a), in the arrangement step, a first resin member 2 containing a thermoplastic resin and transmitting electromagnetic waves is arranged on a first surface S1 of a metal foil 1. At this time, the first resin member 2 is arranged so that an end E2 of the first resin member 2 is longer than an end E1 of the metal foil 1. In addition, a second resin member 3 containing a thermoplastic resin and transmitting electromagnetic waves is arranged on a second surface S2 of the metal foil 1. At this time, the second resin member 3 is arranged so that an end E3 of the second resin member 3 is longer than an end E1 of the metal foil 1. The thickness T of the metal foil 1 is within a predetermined range. Next, as shown in FIG. 1(b), in the welding step, a first pressure member 4 transmitting electromagnetic waves is arranged on a surface of the first resin member 2 opposite to the surface of the metal foil 1 side. In addition, a second pressure member 5 transmitting electromagnetic waves is arranged on a surface of the second resin member 3 opposite to the surface of the metal foil 1 side. While applying pressure with the first pressure member 4 and the second pressure member 5, the metal foil 1 is irradiated with electromagnetic waves from the first pressure member 4 side. In FIG. 1(b), laser light L is irradiated from a laser head 10 as the electromagnetic waves. At this time, the laser light L is irradiated to an area including the end E1 of the metal foil 1. The metal foil 1 absorbs the electromagnetic waves and generates heat. The first resin member 2 and the second resin member 3 are pressed by the first pressure member 4 and the second pressure member 5, respectively, and are in close contact with the metal foil 1. Therefore, the heat of the metal foil 1 is conducted to the first resin member 2 and the second resin member 3. The temperature of the interface between the metal foil 1 and the first resin member 2 and the second resin member 3 rises to near the melting point or softening point of the first resin member 2 and the second resin member 3, and the first resin member 2 and the second resin member 3 locally melt or soften at the interface with the metal foil 1. As a result, the first resin member 2 and the second resin member 3 are simultaneously welded to the first surface S1 and the second surface S2 of the metal foil 1, respectively. In addition, near the end E1 of the metal foil 1, the first resin member 2 and the second resin member 3 are also in close contact with each other because they are pressurized by the first pressing member 4 and the second pressing member 5, respectively. Also, near the end E1 of the metal foil 1, the heat of the metal foil 1 is conducted to the first resin member 2 and the second resin member 3, and the first resin member 2 and the second resin member 3 are locally melted or softened. As a result, the first resin member 2 and the second resin member 3 are welded to each other, as shown in FIG. 1(c).1(c), a region where the first resin member 2 and the second resin member 3 are welded to the metal foil 1 is a first welded portion 11, and a region where the first resin member 2 and the second resin member 3 are welded to the metal foil 1 near the end E1 of the metal foil 1 is a second welded portion 12.

[0011] Here, when a structure in which the end of a metal foil is covered with a resin member is produced using a laser joining method, it is possible to arrange the resin member on the metal foil so that the end of the resin member is longer than the end of the metal foil, as in the arrangement process in the present disclosure.

[0012] In the above case, for example, a resin member is placed on only one side of the metal foil, pressure members are placed on both sides, and the metal foil is irradiated with laser light from one side through the pressure members and the resin member while being pressed by the pressure members on both sides. In this case, if the thickness of the metal foil is thin, the resin member is easily attached to the pressure member located on the opposite side to the laser light irradiation side because the resin member is pressed by the pressure members on both sides near the end of the metal foil. In addition, the resin member tends to melt or soften and flow downward due to the laser light irradiation. Therefore, the resin member may also be welded to the pressure member located on the opposite side to the laser light irradiation side. In this case, the product cannot be removed from the pressure member on the opposite side to the laser light irradiation side.

[0013] In contrast, according to the present disclosure, by disposing a first resin member and a second resin member on the first and second surfaces, respectively, of the metal foil, it is possible to prevent the first resin member from welding to the second pressure member even if the thickness of the metal foil is thin.

[0014] In the above case, for example, consider a case where a resin member is placed on each side of the metal foil, a pressure member is placed on both sides, and the metal foil is irradiated with laser light from one side through the pressure member and the resin member while being pressed by the pressure members on both sides. In this case, if the pressure member located on the side opposite to the laser light irradiation side is a member that absorbs laser light, this pressure member absorbs the laser light and generates heat. Therefore, the resin member may be welded to the pressure member on the side opposite to the laser light irradiation side. In this case, too, the product cannot be removed from the pressure member on the side opposite to the laser light irradiation side.

[0015] In contrast, according to the present disclosure, the second pressure applying member on the side opposite to the electromagnetic wave application side also transmits electromagnetic waves, thereby making it possible to prevent the second resin member from welding to the second pressure applying member.

[0016] In the above case, for example, resin members are arranged on both sides of the metal foil, pressure members are arranged on both sides, and the metal foil is irradiated with laser light from one side through the pressure members and the resin members while being pressed by the pressure members on both sides, and the pressure members on both sides are members that transmit laser light. In this case, if the end of the metal foil is not irradiated with electromagnetic waves, the temperature of the end of the metal foil does not rise sufficiently. Therefore, the resin members near the end of the metal foil do not melt or soften, and the resin members do not weld to each other, so the end of the metal foil may remain exposed.

[0017] In contrast, according to the present disclosure, by irradiating the end of the metal foil with electromagnetic waves, the first resin member and the second resin member can be welded together near the end of the metal foil, and the end of the metal foil can be covered with the first resin member and the second resin member.

[0018] In addition, in the conventional laser joining method, it is difficult to weld the resin member to both sides of the metal member at the same time, and it is necessary to irradiate the laser light to each side at a time. When the laser light is irradiated from one side of the metal member, the metal member absorbs the laser light, generates heat, and the temperature rises on the side of the metal member irradiated with the laser light. On the other hand, when the thickness of the metal member is thick, the temperature on the side of the metal member opposite to the side irradiated with the laser light drops in the process of heat conduction from the side of the metal member irradiated with the laser light, so that the temperature becomes lower than the temperature of the side of the metal member irradiated with the laser light. In addition, since heat is conducted not only in the thickness direction but also in the in-plane direction within the metal member, a lot of heat energy transfer occurs in areas other than the area where the resin member is to be welded to the metal member. Therefore, in the area where the resin member is to be welded to the metal member, the temperature rise is insufficient on the side of the metal member opposite to the side irradiated with the laser light. Therefore, insufficient welding of the resin member may occur on the side of the metal member opposite to the side irradiated with the laser light.

[0019] In contrast, according to the present disclosure, the thickness of the metal foil is within a predetermined range, and the thinness of the metal foil allows the heat conduction distance in the thickness direction of the metal foil to be shortened. Therefore, in the welding process, the temperature rises on the first and second surfaces of the metal foil can be made almost equal. Therefore, by irradiating the metal foil with electromagnetic waves from the first pressure member side, the first resin member and the second resin member can be simultaneously welded to the first and second surfaces of the metal foil, respectively.

[0020] In this manner, in the present disclosure, the first resin member and the second resin member can be welded to the metal foil so as to cover the end portion of the metal foil by irradiating electromagnetic waves from the first surface of the metal foil while avoiding welding of the first resin member and the second resin member to the second pressure member. Furthermore, the first resin member and the second resin member can be simultaneously welded to both surfaces of the metal foil by irradiating electromagnetic waves from the first surface of the metal foil.

[0021] In addition, a hot plate welding method, typified by an impulse sealer, is also known as a method for joining metal and resin members. In the hot plate welding method, the resin member is welded to the metal member by utilizing the thermal conduction in the resin member. Therefore, it is necessary to increase the temperature of the entire resin member in order to raise the temperature of the interface with the metal member. Therefore, the resin member may melt and deform. In addition, since the thermal efficiency is poor, welding is possible when the resin member is thin, but when the resin member is thick, it is difficult for heat to be transmitted to the interface with the metal member, and the risk of deformation of the resin member increases. Therefore, it is necessary to ensure a cooling time, which increases the processing time.

[0022] In contrast, according to the present disclosure, the metal foil is heated by irradiating it with electromagnetic waves, thereby increasing the temperature of the interfaces between the metal foil and the first and second resin members. Since it is necessary to increase the temperature only at the interfaces between the metal foil and the first and second resin members, processing can be performed in a very short time with little energy.

[0023] 1.Placement process The placement process in the present disclosure is a process of placing a first resin member that contains a thermoplastic resin and is transparent to electromagnetic waves on a first surface of a metal foil having a thickness of 1 μm or more and 100 μm or less, so that an end of the first resin member is longer than an end of the metal foil, and placing a second resin member that contains a thermoplastic resin and is transparent to electromagnetic waves on a second surface of the metal foil, so that an end of the second resin member is longer than an end of the metal foil.

[0024] The metal foil is not particularly limited as long as it is a metal foil used in a member constituting an electric storage device, but among them, it is preferable that it is a metal foil used in a current collector of a battery. Examples of the metal foil include nickel foil, titanium foil, stainless steel foil, aluminum foil, and copper foil. In addition, as the metal foil, a metal foil that has been coated, and a metal foil that has been laminated by pressing a plurality of types of metal together under pressure or bonding with an adhesive can also be used. The thickness of the metal foil is 1 μm or more. In addition, the thickness of the metal foil is 100 μm or less, and may be 50 μm or less.

[0025] In addition, the first and second surfaces of the metal foil may be degreased with alcohol, etc. If foreign matter or the like is attached to the first and second surfaces of the metal foil, the foreign matter can be removed.

[0026] The first resin member and the second resin member transmit electromagnetic waves. The electromagnetic wave transmittance of the first resin member and the second resin member is, for example, 50% or more, or may be 60% or more, or may be 80% or more. The electromagnetic wave transmittance of the first resin member and the second resin member may be the same or different from each other.

[0027] The first resin member and the second resin member contain a thermoplastic resin. The thermoplastic resin contained in the first resin member and the second resin member is not particularly limited as long as it is a thermoplastic resin that transmits electromagnetic waves. The thermoplastic resin may be a crystalline resin or a non-crystalline resin. Examples of non-crystalline resins include polystyrene (PS), acrylonitrile styrene (AS), acrylonitrile butadiene styrene copolymer (ABS), polyetherimide (PEI), polycarbonate (PC), polyarylate (PAR), polymethyl methacrylate (PMMA), cycloolefin polymer (COP), cycloolefin copolymer (COC), polysulfone (PSF), polyethersulfone (PES), polyvinyl chloride (PVC), and polyvinyl chloride (PVDC). Examples of crystalline resins include polyethylene (PE), polypropylene (PP), polyoxymethylene (POM), polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyphenylene sulfide (PPS), nylon 6 (PA6), nylon 66 (PA66), nylon 6T (PA6T), liquid crystal polymer (LCP), and polytetrafluoroethylene (PTFE). The thermoplastic resins contained in the first resin member and the second resin member may be the same or different from each other. The thicknesses of the first resin member and the second resin member are, for example, 50 μm or more. The thicknesses of the first resin member and the second resin member are, for example, 1000 μm or less, and may be 300 μm or less. The thicknesses of the first resin member and the second resin member may be the same or different from each other.

[0028] It is preferable that the entire first resin member and the second resin member, or at least the surfaces in contact with the metal foil, are subjected to a modification treatment. This makes it possible to strengthen the bonding between the metal foil and the first resin member and the second resin member. The modification treatment can be, for example, an acid modification surface treatment.

[0029] In the welding process described later, the first resin member and the second resin member are simultaneously welded to the first and second surfaces of the metal foil, respectively, by irradiating electromagnetic waves from the first surface side. Therefore, the first resin member, the metal foil, and the second resin member are arranged so as to overlap each other in a plan view seen from the normal direction of the first surface of the metal foil. The first resin member and the second resin member may be the same in size and shape or may be different from each other.

[0030] The first resin member is disposed on the first surface of the metal foil such that the end of the first resin member is longer than the end of the metal foil. The distance between the end of the metal foil and the end of the first resin member, and the distance between the end of the metal foil and the end of the second resin member are, for example, 0.5 mm or more, and may be 10 mm or more. The upper limit of the distance is not particularly limited. The distance between the end of the metal foil and the end of the first resin member, and the distance between the end of the metal foil and the end of the second resin member may be the same or different from each other. The "end of the first resin member" refers to the end of the first resin member that is located outside the end of the metal foil. The "end of the second resin member" refers to the end of the second resin member that is located outside the end of the metal foil.

[0031] 2.Welding process The welding process in the present disclosure is a process of placing a first pressure member that is transparent to electromagnetic waves on the surface of the first resin member opposite to the surface facing the metal foil, placing a second pressure member that is transparent to electromagnetic waves on the surface of the second resin member opposite to the surface facing the metal foil, and welding the first resin member and the second resin member to the metal foil so as to cover the end of the metal foil by irradiating electromagnetic waves from the first pressure member side while applying pressure with the first pressure member and the second pressure member.

[0032] The first pressure member and the second pressure member are transparent to electromagnetic waves. The transmittance of the first pressure member and the second pressure member to electromagnetic waves is, for example, 50% or more, or may be 60% or more, or may be 80% or more. The transmittance of the first pressure member and the second pressure member to electromagnetic waves may be the same or different from each other.

[0033] The material of the first and second pressure members is not particularly limited as long as it transmits electromagnetic waves, but glass is preferred because of its high electromagnetic wave transmittance and thermal conductivity. When the first and second pressure members are made of glass, the thicknesses of the first and second pressure members are, for example, 1 mm or more and 40 mm or less. The thicknesses of the first and second pressure members may be the same or different from each other.

[0034] In a plan view seen from the normal direction of the first surface of the metal foil, the first pressure member and the second pressure member are arranged so as to overlap the first resin member, the metal foil, and the second resin member. The size of the first pressure member and the second pressure member is preferably larger than the combined size of an area where the first resin member and the second resin member are welded to the metal foil and an area where the first resin member and the second resin member are welded near the end of the metal foil. By applying pressure with the first pressure member and the second pressure member, the first resin member and the second resin member can be adhered to the metal foil, and the first resin member and the second resin member can be adhered to each other near the end of the metal foil.

[0035] Examples of the electromagnetic wave include laser light and infrared light. Among them, laser light is preferable. The processing time can be shortened. Examples of the laser light include semiconductor laser, YAG laser, and fiber laser. The laser light is preferably an infrared laser. The irradiation conditions of the electromagnetic wave (output, energy density, irradiation time, etc. of the electromagnetic wave) are not particularly limited as long as the first resin member and the second resin member can be welded to the metal foil and the first resin member and the second resin member can be welded near the end of the metal foil, and are appropriately set according to the transmittance of the electromagnetic wave of the first resin member, the second resin member, the first pressing member, and the second pressing member, and the thermal conductivity of the metal foil. By appropriately adjusting the irradiation conditions of the electromagnetic wave to control the temperature of the interface between the metal foil and the first resin member and the second resin member, it is possible to suppress insufficient welding of the first resin member and the second resin member. It is also possible to suppress welding of the first resin member to the first pressing member and welding of the second resin member to the second pressing member. Furthermore, the distance between the edge of the metal foil and the edge of the region where the first resin member and the second resin member are welded (the second welded portion) can be controlled. The energy density is, for example, 0.2 W / mm 2 Over 1.8W / mm 2 The irradiation time is, for example, 0.8 sec or more and 1.8 sec or less.

[0036] It is sufficient that the electromagnetic waves can be irradiated from the area where the metal foil and the first and second resin members overlap to the end of the metal foil. For example, as shown in FIG. 1(b), it is preferable to irradiate the electromagnetic waves from the area where the metal foil 1 and the first and second resin members 2 and 3 overlap to an area outside the end E1 of the metal foil 1. Specifically, it is preferable to irradiate the electromagnetic waves from the area where the metal foil and the first and second resin members overlap to an area 0.5 mm or more outside the end of the metal foil. In this case, the electromagnetic waves can be easily irradiated to the end of the metal foil. Moreover, regardless of the intensity distribution of the electromagnetic waves, the temperature of the end of the metal foil can be easily raised to near the melting point or softening point of the first and second resin members by irradiating the electromagnetic waves. The electromagnetic wave irradiation method may be, for example, a method of irradiating the area including the area where the first and second resin members are welded to the metal foil and the area near the end of the metal foil where the first and second resin members are welded, in one go, or a method of irradiating by scanning the beam. In the former method, a beam profile of the same size as the above-mentioned area is formed by a beam homogenizer, and irradiated in one go.

[0037] The pressure conditions (pressure, etc.) applied by the first and second pressure members are not particularly limited as long as they can adhere the first and second resin members to the metal foil and can adhere the first and second resin members to each other near the ends of the metal foil, and are appropriately set according to the strength, hardness, etc. of each member. The pressure is, for example, 0.01 MPa or more.

[0038] In the welding process, the first resin member and the second resin member are welded to cover the end of the metal foil. Therefore, for example, as shown in FIG. 1(c), the end E4 of the region (second welded portion 12) where the first resin member 2 and the second resin member 3 are welded is located outside the end E1 of the metal foil 1. The distance between the end of the metal foil and the end of the second welded portion is, for example, 0.5 mm or more, and may be 1 mm or more. In addition, the upper limit of the distance is not particularly limited and is equal to or less than the distance between the end of the metal foil and the end of the first resin member or the second resin member. Note that the "region where the first resin member and the second resin member are welded", that is, the "second welded portion", refers to the region where the first resin member and the second resin member are welded in the region outside the end of the metal foil. In addition, "the end of the area where the first resin member and the second resin member are welded" refers to the end of the area where the first resin member and the second resin member are welded, which is located on the opposite side to the end of the metal foil.

[0039] 3.Electricity storage device In the present disclosure, the power storage device is, for example, a power storage module. The power storage device may be, for example, a secondary battery such as a nickel-metal hydride secondary battery or a lithium-ion secondary battery, or a capacitor such as an electric double layer capacitor.

[0040] In the present disclosure, the metal foil is not particularly limited as long as it is a member constituting the electric storage device, but it is preferable that the metal foil is a current collector of the battery. In addition, the first resin member and the second resin member are not particularly limited as long as they are members constituting the electric storage device, but it is preferable that they are frame-shaped resin parts arranged on the periphery of the current collector and insulate adjacent current collectors. Specifically, in a manufacturing method of an electric storage device in which bipolar electrodes are stacked via separators, the above-mentioned arrangement step and welding step are preferably applied to a step of welding frame-shaped resin parts 31, 32 to the periphery of both sides of the current collector 21 so as to cover the end of the current collector 21 of the bipolar electrode 20 in which a positive electrode 22 and a negative electrode 23 are arranged on both sides of the current collector 21, as shown in FIG. According to the present disclosure, such a structure can be easily produced by irradiating electromagnetic waves from one side.

[0041] In the method for manufacturing an electricity storage device, general steps in the method for manufacturing an electricity storage device can be applied to steps other than the above-mentioned arrangement step and welding step.

[0042] Examples of applications of the power storage device include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicles (BEVs), gasoline-powered vehicles, and diesel-powered vehicles. In particular, it is preferable to use the power storage device as a driving power source for hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or electric vehicles (BEVs). The power storage device of the present disclosure may also be used as a power source for moving bodies other than vehicles (for example, railways, ships, and aircraft), and may also be used as a power source for electrical appliances such as information processing devices. EXAMPLES

[0043] The present disclosure will now be further described with reference to examples.

[0044] [Examples 1 to 8 and Comparative Example 1] A metal foil made mainly of aluminum, 66 μm thick and 50 mm x 30 mm rectangular, and a first resin member and a second resin member containing polypropylene and subjected to acid modification treatment, 200 μm thick and 50 mm x 10.5 mm rectangular, were prepared. As shown in FIG. 3(a), a first resin member 2 and a second resin member 3 were placed on both sides of the metal foil 1. In this case, the area where the metal foil 1 overlaps with the first resin member 2 and the second resin member 3 was 50 mm x 8 mm. The distance between the end of the metal foil 1 and the end of the first resin member 2, and the distance between the end of the metal foil 1 and the end of the second resin member 2 were both 2.5 mm.

[0045] In addition, a first pressure member and a second pressure member made of heat-resistant crystallized glass were prepared. The first pressure member was placed on the surface of the first resin member opposite the metal foil side, and the second pressure member was placed on the surface of the second resin member opposite the metal foil side. While applying pressure with the first pressure member and the second pressure member, laser light was irradiated from the first pressure member side using a semiconductor laser oscillator and a beam homogenizer. The laser light irradiation conditions and pressure conditions are shown in Table 1. The laser light was irradiated with a fixed head.

[0046] [evaluation] (Distance between the edge of the metal foil and the edge of the region where the first resin member and the second resin member are welded (second welded portion)) The obtained laminate was cut in the short direction (direction of line AA in FIG. 3) of the region (first welded portion) where the first resin member and the second resin member were welded to the metal foil. The distance between the end of the metal foil and the end of the second welded portion was measured on the cut surface by observation with an optical microscope. The number of measurements was 3, and the average value was calculated. The results are shown in Table 1. FIG. 3(b) shows an optical microscope photograph of Example 4. FIG. 3(b) corresponds to the cross section of line AA in FIG. 3(a). In FIG. 3(b), the distance between the end E1 of the metal foil 1 and the end E4 of the second welded portion 12 is indicated as d.

[0047] [Table 1]

[0048] (Joining strength) For Example 4, the obtained laminate was cut out in a width of 10 mm in the short direction of the region (first welded portion) where the first resin member and the second resin member were welded to the metal foil, and used as a measurement sample. A shear test was performed on the measurement sample in which the metal foil and the first resin member or the second resin member were pulled in opposite directions to each other, and the bonding strength (shear strength) was measured. The bonding strength between the metal foil and the first resin member (laser irradiated side) was 37.3 N / 10 mm, and the bonding strength between the metal foil and the second resin member (opposite side to the laser irradiated side) was 37.5 N / 10 mm. In the shear test, it was confirmed that the resin base material began to elongate, and that the resin members were bonded to both sides of the metal foil with a strength equal to or greater than the strength of the resin base material by laser irradiation from one side.

[0049] For the other examples, results similar to those of Example 4 were obtained.

[0050] In Examples 1 to 8, it was confirmed that by irradiating laser light from the first surface of the metal foil, it is possible to simultaneously weld the first resin member and the second resin member to the first surface and the second surface of the metal foil, respectively, while avoiding welding of the resin member to the pressure member and covering the ends of the metal foil with the first resin member and the second resin member.

[0051] On the other hand, in Comparative Example 1, the end of the metal foil could not be covered by the first resin member and the second resin member. Also, the welding of the first resin member and the second resin member to the metal foil was insufficient. This is believed to be due to the low laser output, short irradiation time, and small energy density, which resulted in insufficient temperature rise of the metal foil.

[0052] It was also confirmed that the distance between the edge of the metal foil and the edge of the second welded portion could be controlled by adjusting the conditions for irradiating the laser light.

[0053] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. [Explanation of symbols]

[0054] 1...Metal foil 2…First resin member 3…Second resin member 4...First pressure member 5...Second pressure member E1: Metal foil edge E2: End of the first resin member E3: End of the second resin member L: Laser light S1...Side 1 S2…Second side T: Metal foil thickness

Claims

1. a disposing step of disposing a first resin member containing a thermoplastic resin and transmitting electromagnetic waves on a first surface of a metal foil having a thickness of 1 μm or more and 70 μm or less such that an end of the first resin member is longer than an end of the metal foil, and disposing a second resin member containing a thermoplastic resin and transmitting electromagnetic waves on a second surface of the metal foil such that an end of the second resin member is longer than an end of the metal foil; a welding process in which a first pressure member that transmits electromagnetic waves is disposed on a surface of the first resin member opposite to the surface of the metal foil side, a second pressure member that transmits electromagnetic waves is disposed on a surface of the second resin member opposite to the surface of the metal foil side, and an electromagnetic wave is irradiated onto an end of the metal foil from the first pressure member side while applying pressure with the first pressure member and the second pressure member, thereby welding the first resin member and the second resin member to the metal foil so as to cover the end of the metal foil; having The metal foil has a solid structure and is a current collector of a battery; In the arranging step, a distance between an end of the metal foil and an end of the first resin member, and a distance between an end of the metal foil and an end of the second resin member are each 2.5 mm or more; In the welding step, a distance between the end of the metal foil and an end of the region where the first resin member and the second resin member are welded is set to 0.5 mm or more. A method for manufacturing an electricity storage device that is a lithium ion secondary battery.

2. A method for manufacturing an energy storage device as described in claim 1, wherein the first resin member and the second resin member each contain polypropylene and have been subjected to an acid modification treatment.

Citation Information

Patent Citations

  • Method for joining laser beam transmittable resin member and porous member together

    JP2005297288A

  • Method and apparatus for joining resin and metal together

    JP2010046831A

  • Laser bonding method

    JP2012056308A

  • Composite body and method for producing the same as well as shaped and coated metallic material and method for producing the same

    JP2015080884A

  • Nonaqueous electrolyte secondary battery, and method for manufacturing the same

    JP2015210892A