Manufacturing method of wound magnetic core
By simultaneously winding soft magnetic alloy ribbons with and without insulating layers, the method addresses insulation challenges in wound magnetic cores, reducing eddy current loss and core size while simplifying the manufacturing process.
Patent Information
- Application Number
- JP2022138962
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2038-07-25
AI Technical Summary
Existing methods for manufacturing wound magnetic cores using soft magnetic alloy ribbons face challenges in ensuring insulation between layers, leading to increased eddy current loss and larger core sizes due to the use of insulating tapes, which complicate the manufacturing process and reduce the space factor.
A method involving the simultaneous winding of soft magnetic alloy ribbons with insulating layers on one side and without insulating layers on the other side, ensuring insulation by laminating the former on both sides of the latter, thereby reducing the need for additional insulating layers and simplifying the manufacturing process.
This approach effectively maintains insulation between layers, reduces eddy current loss, and minimizes core size, enhancing the manufacturing efficiency and cost-effectiveness of wound magnetic cores.
Smart Images

Figure 0007589721000001 
Figure 0007589721000002 
Figure 0007589721000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a wound magnetic core using a soft magnetic alloy ribbon, and a wound magnetic core obtained thereby. [Background technology]
[0002] The magnetic cores used in electromagnetic devices such as intermediate frequency transformers and reactors generate iron loss during operation. Because these electromagnetic devices are widely used in power converters, the overall loss due to iron loss is enormous. In today's world, where there is a strong demand for energy conservation and reduction in CO2 emissions, there is a strong demand for reducing iron loss.
[0003] Conventionally, magnetic steel sheets have been mainly used as the material for magnetic cores, but in order to reduce iron loss, they are increasingly being replaced with soft magnetic alloy ribbons (hereinafter also referred to as alloy ribbons), such as amorphous alloy ribbons and nanocrystalline alloy ribbons. These soft magnetic alloy ribbons have iron loss that is approximately 1 / 10 to 1 / 50 lower than that of standard electromagnetic steel sheets, making them suitable for improving the efficiency of converters when used in intermediate frequency transformers and the like, and contributing to reducing losses.
[0004] Iron loss is broadly divided into hysteresis loss and eddy current loss, and eddy current loss is further divided into classical eddy current loss and anomalous eddy current loss. The reason why the iron loss of soft magnetic alloy ribbon is lower than that of electromagnetic steel sheet is that the coercive force is smaller than that of electromagnetic steel sheet, so hysteresis loss can be reduced, and the sheet thickness is also about 1 / 10 that of electromagnetic steel sheet, so classical eddy current loss can be reduced.
[0005] For this reason, when a small magnetic core weighing about 1 kg is made using a soft magnetic alloy ribbon, a magnetic core with low loss can be easily obtained, but when a large magnetic core weighing more than 10 kg is made, iron loss several times greater than the inherent iron loss of the soft magnetic alloy ribbon may occur. The reason for this is that the increase in width of the soft magnetic alloy ribbon and the increase in the weight of the magnetic core make it easier for current to flow between the layers of the soft magnetic alloy ribbon, and the generation of this current generates eddy currents, which increase loss.
[0006] The magnetic core made of the soft magnetic alloy ribbon may be a laminated core obtained by cutting the ribbon to a predetermined length and laminating the ribbon, but it is often used as a wound core wound in a spiral shape. In a wound core, in order to suppress the occurrence of eddy current loss and reduce iron loss in the wound core, the insulation between layers of the alloy ribbon may be improved. For example, Patent Document 1 discloses a method of manufacturing a wound magnetic core with interlayer insulation by overlapping and winding an alloy ribbon and an insulating tape, and also discloses a method of forming an oxide layer on the alloy surface to form an insulating layer on the alloy surface. Furthermore, Patent Document 2 discloses that an insulating tape is used in addition to the soft magnetic alloy ribbon, and the two are wound at the same time. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 63-302504 [Patent Document 2] Japanese Utility Model Application Publication No. 1-58914 Summary of the Invention [Problem to be solved by the invention]
[0008] Since a wound core can be made into a magnetic core simply by winding a long alloy ribbon, it does not require the steps required in the manufacturing process of a laminated magnetic core, such as cutting the alloy ribbon to a predetermined length, laminating it, and fixing the alloy ribbons together after lamination, etc. Therefore, it is desired to establish a means for increasing the insulation between layers of an alloy ribbon by a simple device in the manufacturing method of a wound core.
[0009] However, the methods of using insulating tape for interlayer insulation described in Patent Documents 1 and 2 have the following problems. Because the soft magnetic alloy ribbon is very thin, having a thickness of about 5 μm to 50 μm, even if a thin insulating tape is used, the insulating tape takes up a large proportion of the magnetic core. As a result, the space factor of the soft magnetic alloy ribbon is small, and the wound magnetic core becomes larger accordingly.
[0010] As mentioned above, Patent Document 1 discloses that an oxide layer is formed on the surface of the alloy to form an insulating layer on the surface of the alloy. Methods of forming this oxide layer include, for example, immersion in powder of SiO2, MgO, Al2O3, etc., attachment by spraying or electrophoresis, and deposition of a film of SiO2, etc. by sputtering or vapor deposition. However, when an insulating layer is formed on the surface of the soft magnetic alloy ribbon, a separate manufacturing process is required, which complicates the manufacturing process.
[0011] An object of the present invention is to provide a manufacturing method for a wound magnetic core that can easily ensure insulation between layers of a soft magnetic alloy ribbon. Another object of the present invention is to provide a wound magnetic core obtained by the simple manufacturing method, in which insulation between layers of a soft magnetic alloy ribbon is ensured. [Means for solving the problem]
[0012] One aspect of the present invention is A method for manufacturing a wound magnetic core in which a soft magnetic alloy ribbon is wound, comprising the steps of: forming insulating layers on both sides of the soft magnetic alloy ribbon to obtain a first soft magnetic alloy ribbon; a step of simultaneously winding a plurality of soft magnetic alloy ribbons each including a combination of the first soft magnetic alloy ribbon and a second soft magnetic alloy ribbon having no insulating layer formed thereon, so that the first soft magnetic alloy ribbons are laminated on both sides of the second soft magnetic alloy ribbon; The present invention relates to a method for manufacturing a wound magnetic core having the above structure.
[0013] Another aspect of the present invention is A wound magnetic core in which a soft magnetic alloy ribbon is wound, The wound core is configured such that a plurality of soft magnetic alloy ribbons, each of which is a combination of a first soft magnetic alloy ribbon having insulating layers formed on both sides thereof and a second soft magnetic alloy ribbon having no insulating layer formed thereon, are wound around the core, and the first soft magnetic alloy ribbon is laminated on both sides of the second soft magnetic alloy ribbon. Effect of the Invention
[0014] The present invention makes it possible to provide a manufacturing method for a wound core that can easily ensure insulation between layers of a soft magnetic alloy ribbon, and thereby to provide a wound core in which insulation between layers of a soft magnetic alloy ribbon is ensured at low cost. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a schematic diagram of a lamination surface in a wound magnetic core of the present invention. [Diagram 2] 4 is a schematic diagram showing a state in which the first and second soft magnetic alloy ribbons are wound simultaneously. FIG. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus for adhering insulating particles to a soft magnetic alloy ribbon. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will now be described in detail with reference to the following embodiments, but the present invention is not limited to these embodiments. One aspect of the present invention is A method for manufacturing a wound magnetic core in which a soft magnetic alloy ribbon is wound, comprising the steps of: forming insulating layers on both sides of the soft magnetic alloy ribbon to obtain a first soft magnetic alloy ribbon; a step of simultaneously winding a plurality of soft magnetic alloy ribbons each including a combination of the first soft magnetic alloy ribbon and a second soft magnetic alloy ribbon having no insulating layer formed thereon, so that the first soft magnetic alloy ribbons are laminated on both sides of the second soft magnetic alloy ribbon; The present invention relates to a method for manufacturing a wound magnetic core having the above structure. According to this manufacturing method, even if multiple soft magnetic alloy ribbons are wound simultaneously, the generation of eddy currents between the layers of the soft magnetic alloy ribbons can be suppressed. Therefore, compared to the case of winding a single soft magnetic alloy ribbon, the number of windings can be reduced, and the manufacturing time can be shortened. In addition, in the manufacturing method of the present invention, a first soft magnetic alloy ribbon having insulating layers formed on both sides and a second soft magnetic alloy ribbon having no insulating layer are used in combination as the soft magnetic alloy ribbon to be wound. Therefore, it is only necessary to form insulating layers on some of the soft magnetic alloy ribbons used in the wound magnetic core, thereby reducing the work of forming insulating layers on the soft magnetic alloy ribbons. Furthermore, in the manufacturing method of the present invention, insulating layers are formed on both sides of the first soft magnetic alloy ribbon, and the first soft magnetic alloy ribbon is laminated on both sides of the second soft magnetic alloy ribbon, so that the second soft magnetic alloy ribbon always maintains its insulation due to the insulating layers formed on both sides of the first soft magnetic alloy ribbon. The insulating layer may be, for example, formed by adhering insulating particles to the surface of a soft magnetic alloy ribbon.
[0017] Another aspect of the present invention obtained by the above-mentioned production method is A wound magnetic core in which a soft magnetic alloy ribbon is wound, The wound core is configured such that a plurality of soft magnetic alloy ribbons, each of which is a combination of a first soft magnetic alloy ribbon having insulating layers formed on both sides and a second soft magnetic alloy ribbon having no insulating layer, are wound around the core, and the first soft magnetic alloy ribbon is laminated on both sides of the second soft magnetic alloy ribbon.
[0018] The present invention will be described in further detail below, but the present invention is not limited thereto. The soft magnetic alloy ribbon may be, for example, a strip-shaped alloy ribbon obtained by cooling a molten alloy with a roll. Specifically, the soft magnetic alloy ribbon can be formed by preparing a molten alloy, ejecting the molten alloy onto the surface of a rotating chill roll to form a film of the molten alloy on the surface of the chill roll, and peeling off the amorphous alloy ribbon formed on the surface of the chill roll from the surface of the chill roll. The peeled alloy ribbon can be wound into a roll by a winding roll.
[0019] For the soft magnetic alloy ribbon, for example, an amorphous alloy or an amorphous alloy that can be nano-crystallized can be used. It is preferable that the first and second soft magnetic alloy ribbons used in the present invention are made of the same alloy. In particular, when heat treatment is performed, the use of the same alloy allows both soft magnetic alloy ribbons to be heat treated under optimal conditions.
[0020] The composition of the amorphous alloy can be, for example, such that, when the total amount of Fe, Si, and B is 100 atomic %, Si is 0 atomic % or more and 10 atomic % or less, B is 10 atomic % or more and 20 atomic % or less, and the remainder is Fe. If the Si content and B content are outside this range, it becomes difficult to produce an amorphous alloy by roll cooling, and mass productivity tends to decrease. As additives or unavoidable impurities, elements other than Fe, Si, and B, such as Mn, S, C, and Al, may be contained. When additives or unavoidable impurities are contained, the total proportion of Fe, Si, and B is preferably 95 mass% or more, and more preferably 98 mass% or more. Amorphous alloys have no anisotropy due to their crystal structure, and no grain boundaries that impede magnetic wall movement, so they have excellent soft magnetic properties, including high magnetic permeability and low loss, while still having high magnetic flux density. The soft magnetic alloy ribbon made of the amorphous alloy with the above composition has a magnetic flux density B of 1.48 T or more by itself. 80 The present invention can be implemented as follows:
[0021] Amorphous alloys that can be nanocrystallized are, for example, alloys having a general formula: (Fe1-aMa)100-xyz-α-β-γCuxSiyBzM'αM″βXγ (atomic %), where M is Co and / or Ni, M' is at least one element selected from the group consisting of Nb, Mo, Ta, Ti, Zr, Hf, V, Cr, Mn, and W, and M″ is an element selected from the group consisting of Al, platinum group elements, Sc, rare earth elements, Zn, Sn, and Re. X is at least one element selected from the group consisting of C, Ge, P, Ga, Sb, In, Be, and As, and a, x, y, z, α, β, and γ satisfy 0≦a≦0.5, 0.1≦x≦3, 0≦y≦30, 0≦z≦25, 5≦y+z≦30, 0≦α≦20, 0≦β≦20, and 0≦γ≦20, respectively. Preferably, in the above general formula, a, x, y, z, α, β, and γ satisfy 0≦a≦0.1, 0.7≦x≦1.3, 12≦y≦17, 5≦z≦10, 1.5≦α≦5, 0≦β≦1, and 0≦γ≦1, respectively.
[0022] This amorphous alloy capable of nanocrystallization can be transformed into a nanocrystalline alloy with a nanocrystalline structure in which bcc-Fe solid solution crystals with an average grain size of 100 nm or less account for 50% or more of the structure by undergoing heat treatment for nanocrystallization. In the manufacture of wound magnetic cores, the heat treatment for nanocrystallization is usually performed on a laminate formed by winding soft magnetic alloy ribbons. In the case of a soft magnetic alloy ribbon having the above composition, a heat treatment for nanocrystallization is usually performed in the range of 450° C. to 650° C. If the heat treatment temperature is less than 450° C., crystallization is unlikely to occur and the heat treatment takes too much time, while if the heat treatment temperature exceeds 650° C., coarse crystal grains may be generated non-uniformly, making it difficult to obtain uniform nanocrystal grains. The nanocrystallization heat treatment can also be carried out in a magnetic field.
[0023] The thickness of the soft magnetic alloy ribbon is preferably 5 μm or more and 50 μm or less. If the thickness is less than 5 μm, the mechanical strength of the soft magnetic alloy ribbon tends to be insufficient. The thickness is more preferably 10 μm or more, and more preferably 15 μm or more. On the other hand, if the thickness of the soft magnetic alloy ribbon exceeds 50 μm, it tends to be difficult to stably obtain an amorphous phase when produced by roll cooling. The thickness is more preferably 35 μm or less, and more preferably 30 μm or less.
[0024] The insulating layer will now be described. The insulating layer may be any known insulating layer used for soft magnetic alloy ribbons, for example, an insulating layer having insulating particles attached to the surface of a soft magnetic alloy ribbon may be used. The insulating particles may be, for example, metal oxides such as SiO2, Al2O3, MgO, etc. In this case, a known method may be appropriately adopted, such as a method of applying an alcohol solution containing a metal alkoxide to an alloy ribbon and drying the applied metal alkoxide, a method of attaching the metal alkoxide by a powder immersion method, a spray method, or an electrophoretic method, a method of forming a film by a sputtering method or a vapor deposition method, or a method of forming the metal alkoxide on the surface of the alloy ribbon by a heat treatment. Hereinafter, an embodiment in which insulating particles are attached to the surface of a soft magnetic alloy ribbon as the insulating layer will be described.
[0025] In one embodiment of the present invention, the insulating particles are attached to both sides of the first soft magnetic alloy ribbon. FIG. 3 is a schematic diagram showing an apparatus for adhering insulating particles to both sides of the first soft magnetic alloy ribbon. The apparatus 100 has a structure capable of continuously immersing a soft magnetic alloy ribbon 2' unwound from a winding reel 20' in a coating solution 3 stored in a liquid tank. The unwinding reel 20' is wound with the soft magnetic alloy ribbon 2' obtained by cooling the roll. The soft magnetic alloy ribbon 2' unwound from the unwinding reel 20' is conveyed into the coating solution 3 while being bent by a plurality of bars. The coating solution 3 may be, for example, an organic solvent in which insulating particles are stirred. The soft magnetic alloy ribbon 2' passing through the coating solution 3 has insulating particles attached to both sides thereof together with the organic solvent. After being unwound from the coating solution 3, the soft magnetic alloy ribbon is carried into a drying furnace. The organic solvent remaining on the surface of the soft magnetic alloy ribbon is removed by the drying furnace, and the first soft magnetic alloy ribbon 1 having insulating particles attached to both sides thereof is obtained. The first soft magnetic alloy ribbon 1 obtained in this way is wound around a winding reel to become the unwinding reel 10 used in manufacturing a wound magnetic core. In this embodiment, IPA (isopropyl alcohol) was used as the coating solution 3, and oxide powder (MgO) was used as the insulating particles. The oxide powder was added to IPA at 5 wt %. When the soft magnetic alloy ribbon was transported in the coating solution, the oxide powder was stirred by ultrasonic waves. The soft magnetic alloy ribbon was immersed in the coating solution 3 for approximately 0.2 seconds, so that 0.2 to 1% of MgO particles based on the ribbon mass were adhered to the surface of the soft magnetic alloy ribbon.
[0026] For the second soft magnetic alloy ribbon to which no insulating particles are attached, the soft magnetic alloy ribbon obtained by roll cooling can be used as it is. For example, the same unwinding reel 20' as shown in Fig. 3 can be used as the unwinding reel for the second soft magnetic alloy ribbon. The soft magnetic alloy ribbon used was an Fe-based amorphous alloy ribbon with a width of 50 mm and a thickness of 14 μm, which was obtained by quenching a molten alloy consisting of, in atomic percent, Cu: 1%, Nb: 3%, Si: 15.5%, B: 6.5%, with the balance being Fe and unavoidable impurities, by a single roll method.
[0027] FIG. 2(a) is a schematic diagram showing a process of simultaneously winding a first soft magnetic alloy ribbon 1 having insulating particles attached to both sides and a second soft magnetic alloy ribbon 2 having no insulating particles attached thereto to form a wound magnetic core. The first soft magnetic alloy ribbon 1 is unwound from the unwinding reel 10, and the second soft magnetic alloy ribbon 2 is unwound from the unwinding reel 20. The unwound first and second soft magnetic alloy ribbons have their leading ends fixed to a bobbin 60. The bobbin 60 has an axial cross section of a substantially rectangular shape. The bobbin 60 rotates about its axis, whereby the first soft magnetic alloy ribbon 1 and the second soft magnetic alloy ribbon 2 are unwound and then wound around the bobbin 60 at the same time. In this way, the wound magnetic core 50 is obtained. When an amorphous alloy ribbon capable of being nano-crystallized is used as the soft magnetic alloy ribbon, it is wound around the bobbin 60, and then heat-treated for nano-crystallization. 2(b) is different from FIG. 2(a) in that the position of the unwinding reel 20 from which the second soft magnetic alloy ribbon is unwound is changed. Specifically, the positions of the unwinding reel 10 and the unwinding reel 20 are arranged so as to be point-symmetrical with respect to the rotation axis of the bobbin 60.
[0028] 1 is a schematic diagram of the lamination surface of a wound magnetic core 50 obtained in the present invention viewed in the axial direction. In the wound magnetic core 50, first soft magnetic alloy ribbons are laminated on both sides of a second soft magnetic alloy ribbon. In other words, first soft magnetic alloy ribbons 1 to which insulating particles 1a are attached and second soft magnetic alloy ribbons 2 to which no insulating particles are attached are alternately laminated in the lamination direction (radial direction).
[0029] As an embodiment of the present invention other than the wound magnetic core of Fig. 1, two first soft magnetic alloy ribbons and one second soft magnetic alloy ribbon may be used, and three soft magnetic alloy ribbons consisting of one first soft magnetic alloy ribbon, the other first soft magnetic alloy ribbon, and the second soft magnetic alloy ribbon are wound simultaneously in the stacking direction, and the soft magnetic alloy ribbons consisting of the combination of these three ribbons may be repeatedly stacked. Also, two each of the first soft magnetic alloy ribbon 1 and the second soft magnetic alloy ribbon 2 may be used, and four soft magnetic alloy ribbons consisting of one first soft magnetic alloy ribbon, one second soft magnetic alloy ribbon, the other first soft magnetic alloy ribbon, and the other second soft magnetic alloy ribbon are wound simultaneously in the stacking direction, and the soft magnetic alloy ribbons consisting of the combination of these four ribbons may be repeatedly stacked. Even in such a combination, the first soft magnetic alloy ribbons are laminated on both sides of the second soft magnetic alloy ribbons, and the insulation between the layers of the soft magnetic alloy ribbons can be maintained. In this manner, in the present invention, the combination of the first soft magnetic alloy thin ribbon and the second soft magnetic alloy thin ribbon that are wound simultaneously can be changed as appropriate.
[0030] In this embodiment, a wound body in which the first soft magnetic alloy ribbon is laminated on both sides of the second soft magnetic alloy ribbon is obtained, and then this wound body is placed in a heat treatment furnace and heat treated for nanocrystallization by holding it at 550°C for 60 minutes in no magnetic field. In the wound magnetic core of the present invention obtained in this way, the first and second soft magnetic alloy ribbons have a nanocrystalline structure in which bcc-Fe solid solution crystals with an average grain size of 100 nm or less account for 50% or more of the structure. [Explanation of symbols]
[0031] 1: first soft magnetic alloy ribbon, 1a: insulating particles, 2: second soft magnetic alloy ribbon, 3: coating solution, 4: drying furnace, 10, 20: unwinding reel, 50: wound magnetic core, 60: bobbin
Claims
[Claim 1] A method for manufacturing a wound magnetic core in which a soft magnetic alloy ribbon having a thickness of 5 to 35 μm is wound, comprising the steps of: The soft magnetic alloy ribbon has the general formula: (Fe 1-a M a ) 100-x-y-z-α-β-γ Cu x S y B z M' α M” β X γ (atomic %), wherein M is Co and / or Ni, M' is at least one element selected from the group consisting of Nb, Mo, Ta, Ti, Zr, Hf, V, Cr, Mn, and W, M" is at least one element selected from the group consisting of Al, platinum group elements, Sc, rare earth elements, Zn, Sn, and Re, X is at least one element selected from the group consisting of C, Ge, P, Ga, Sb, In, Be, and As, and a, x, y, z, α, β, and γ satisfy 0≦a≦0.5, 0.1≦x≦3, 0≦y≦30, 0≦z≦25, 5≦y+z≦30, 0≦α≦20, 0≦β≦20, and 0≦γ≦20, respectively. forming insulating layers by adhering insulating particles to both sides of the soft magnetic alloy ribbon to obtain a first soft magnetic alloy ribbon; a step of simultaneously winding a plurality of soft magnetic alloy ribbons each including a combination of the first soft magnetic alloy ribbon and a second soft magnetic alloy ribbon having no insulating layer formed thereon, so that the first soft magnetic alloy ribbon is laminated on both sides of one second soft magnetic alloy ribbon, thereby maintaining insulation between the first soft magnetic alloy ribbon and the second soft magnetic alloy ribbon; a step of subjecting the wound magnetic core to a heat treatment for nanocrystallization at a temperature in the range of 450° C. to 650° C.; having The step of producing the first soft magnetic alloy ribbon includes: the soft magnetic alloy ribbon is unwound from a winding reel, conveyed into a coating solution in which MgO particles are stirred in IPA (isopropyl alcohol), the soft magnetic alloy ribbon is passed through the coating solution, the IPA and the MgO particles are attached to both sides of the soft magnetic alloy ribbon, the soft magnetic alloy ribbon is conveyed out of the coating solution, and the IPA remaining on the surface of the soft magnetic alloy ribbon is removed, a mass of the MgO particles attached to the surface of the soft magnetic alloy ribbon is 0.2 to 1% of a mass of the soft magnetic alloy ribbon; Manufacturing method of wound magnetic core.
Citation Information
Patent Citations
Wound iron core
JP1981118306A
Magnetic core and manufacture thereof
JP1988302504A
JP1989058914U
Manufacture of amorphous core
JP1990016706A