Laminated material
A laminated member with a glass member and Si-SiC structure, optimized for thermal and impact resistance, addresses the limitations of conventional materials by providing rapid temperature changes and improved durability.
Patent Information
- Application Number
- JP2022576695
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-20
- Filing Date
- 2022-01-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-01-18
AI Technical Summary
Conventional laminated members used for heating surfaces, such as cooking devices and electronic device inspection tables, lack sufficient thermal shock resistance, impact resistance, and temperature rise properties, necessitating a material with improved durability and thermal stability.
A laminated member comprising a glass member with specific compositional ranges of SiO2, Al2O3, B2O3, and P2O5, a bonding layer containing resin, and a Si-SiC member with controlled linear expansion coefficients, ensuring minimal stress and rapid temperature changes.
The laminated member achieves excellent temperature rise resistance, impact resistance, and thermal shock resistance, making it suitable for applications requiring rapid temperature adjustments and durability.
Smart Images

Figure 0007589757000008 
Figure 0007589757000001 
Figure 0007589757000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated member and a glass composition used in a glass member constituting the laminated member. [Background technology]
[0002] In a system kitchen, the worktop, heating cooker, etc. are connected by a worktop. Materials for the worktop include stainless steel, artificial marble, and ceramics.
[0003] In addition, in inspection equipment and testing equipment for conducting electrical tests on electronic devices, glass and the like are used as the material of the mounting tables on which the electronic devices are placed.
[0004] The cooking device is installed in an opening provided in the worktop. The cooking device includes a top plate on which a heated object (such as a pan) is placed. Examples of materials for the top plate include crystallized glass (see Patent Document 1), ceramics, etc.
[0005] Furthermore, Patent Documents 2 and 3 disclose inspection and testing equipment for inspecting electrical characteristics of electronic devices. For example, the mounting table in the inspection equipment of Patent Document 2 is equipped with a stage cover and a cooling unit made of ceramic, quartz, or glass. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2012-148958 [Patent Document 2] International Publication No. 2018 / 100881 [Patent Document 3] Japanese Patent Application Publication No. 9-298225 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, from the viewpoint of design, there has been a demand for the worktop and the top plate to be made of the same material. For this reason, the application of heating members used in the top plates of cooking appliances, inspection devices, etc. to the worktop has been considered.
[0008] Here, the heating member used in the top plate is required to have a structure capable of rapid heating in order to control the temperature within a predetermined temperature range with respect to the set temperature, and a cooling (heat absorbing) structure for protecting the temperature sensor part including the electronic device. Therefore, the heating member is required to have excellent temperature rise property and impact resistance.
[0009] The inventors evaluated a laminated member having a glass member, a resin bonding layer, and a Si-SiC member as a conventional heating member and found that although it had excellent temperature rise properties and impact resistance, there was room for improvement in terms of thermal shock resistance.
[0010] Therefore, an object of the present invention is to provide a laminated member excellent in temperature rise property, impact resistance and thermal shock resistance, and a glass composition used for a glass member constituting the laminated member. [Means for solving the problem]
[0011] As a result of intensive research into the above-mentioned problems, the inventors have discovered that a laminated member having a glass member with a predetermined linear transmittance, a bonding layer containing a resin, and a Si-SiC member, wherein the composition of the glass member is within a predetermined range, and the average linear expansion coefficient α of the Si-SiC member, the average linear expansion coefficient β of the glass member, and the absolute value of the difference between α and β (|α-β|) are within predetermined ranges, has excellent temperature rise properties, impact resistance, and thermal shock resistance, and have completed the present invention.
[0012] That is, the inventors discovered that the above problems can be solved by the following configuration. [1] A glass member having an in-line transmittance of 80% or more at a wavelength of 850 nm; a bonding layer including a resin on the glass member; A laminated member having a Si-SiC member on the bonding layer, The glass member has a SiO content of 55.0 to 85.0 mol % in terms of oxide-based mol percentage. 2 and 1.5 to 22.0 mol% Al 2 O 3 and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol% P 2 O 5 and The above SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O 5 The total content of is 70.0 to 97.0%, expressed as a mole percentage based on oxides; The Si-SiC member has an average linear expansion coefficient α of 2.85 to 4.00 ppm / °C at 20 to 200°C, The glass member has an average linear expansion coefficient β of 1.50 to 5.00 ppm / °C at 20 to 200°C, A laminate member, wherein the absolute value |α-β| obtained by subtracting the average linear expansion coefficient α of the Si-SiC member at 20 to 200° C. from the average linear expansion coefficient β of the glass member at 20 to 200° C. is 2.00 ppm / ° C. or less. [2] The glass member has a SiO content of 60.0 to 78.0 mol% in terms of oxide-based mole percentage. 2 and 8.0 to 18.0 mol% Al 2 O 3 and 2.0 to 11.0 mol% B 2 O 3 and 0 to 3.0 mol% P 2 O 5 and The above SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O 5The laminate member according to [1], wherein the total content of is 80.0 to 90.0%, expressed as a mole percentage based on the oxides. [3] The total content of RO and ZnO in the glass member is 2.0 to 25.0%, expressed in mole percentage based on oxides; R in the above glass material 2 The laminate member according to [1] or [2], wherein the total content of O is 0 to 15.0%, expressed in mole percentage on an oxide basis. [4] The laminate member according to any one of [1] to [3], wherein the glass member has an average linear expansion coefficient β of 2.00 to 3.50 ppm / °C, a Young's modulus of 40 to 120 GPa, and a melting temperature of 1000 to 2000°C. [5] The above B contained in the above glass material 2 O 3 The laminate member according to any one of [1] to [4], wherein the content of is 8.5 mol % or less. [6] The glass member contains, in terms of mole percentage based on oxide, 0 to 13.0 mole percent Na 2 The laminate member according to any one of [1] to [5], further comprising O. [7] The glass member contains, in terms of mole percentage based on oxide, 0.0001 to 0.0115 mole percent of Fe. 2 O 3 The laminated member according to any one of [1] to [6], [8] The laminate member according to any one of [1] to [7], wherein the glass member has an in-line transmittance of 90% or more at a wavelength of 850 nm. [9] The thickness of the glass member is 2 to 40 mm; The laminated member according to any one of [1] to [8], wherein the Si-SiC member has a thickness of 0.5 to 15 mm.
[10] The laminate member according to any one of [1] to [9], wherein the Si-SiC member has a thermal conductivity of 130 to 300 W / m·K at 20° C.
[11] The laminate member according to any one of [1] to
[10] , wherein the average linear expansion coefficient β of the glass member at 20 to 200° C. is smaller than the average linear expansion coefficient α of the Si—SiC member at 20 to 200° C.
[12] The laminate member according to any one of [1] to
[11] , wherein the Si-SiC member has a Young's modulus of 300 to 420 GPa.
[13] The laminate member according to any one of [1] to
[12] , wherein the Si-SiC member has a metal Si content of 8 to 60 mass %.
[14] The laminate member according to any one of [1] to
[13] , wherein the resin has a heat resistance temperature of 120 to 420°C.
[15] The laminate member according to any one of [1] to
[14] , wherein the bonding layer has an average linear expansion coefficient γ at 20 to 200° C. of 2 to 200 ppm / ° C.
[16] Density is 2.40 to 2.85 g / cm 3 The laminate member according to any one of [1] to
[15] , wherein
[17] The laminated member according to any one of [1] to
[16] , wherein the amount of warping is 0.25 mm or less.
[18] A second bonding layer provided on the Si-SiC member; The laminated member according to any one of [1] to
[17] , further comprising a second Si--SiC member joined to the Si--SiC member via the second bonding layer.
[19] A laminated member including a glass member, a bonding layer including a resin on the glass member, and a Si-SiC member on the bonding layer, comprising a glass composition used in the glass member, The glass composition has an in-line transmittance of 80% or more at a wavelength of 850 nm, The glass composition has a molar percentage of 55.0 to 85.0 mol% of SiO 2 and 1.5 to 22.0 mol% Al 2 O 3 and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol% P 2 O 5 and The glass composition is the SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O5 The total content of is 70.0 to 97.0%, expressed as a mole percentage based on oxides; The glass composition has an average linear expansion coefficient β of 1.50 to 5.00 ppm / °C at 20 to 200°C, The glass composition is used in a laminated member having a Si-SiC member having an average linear expansion coefficient α at 20 to 200°C of 2.85 to 4.00 ppm / °C, and is used so that the absolute value |α-β| obtained by subtracting the average linear expansion coefficient β at 20 to 200°C of the glass member from the average linear expansion coefficient α of the Si-SiC member at 20 to 200°C is 2.00 ppm / °C or less.
[20] SiO2 is 55.0 to 85.0 mol% in mole percent based on oxide. 2 and 1.5 to 22.0 mol% Al 2 O 3 and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol% P 2 O 5 and The above SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O 5 The total content of is 70.0 to 97.0%, expressed as a mole percentage based on oxides; The average linear expansion coefficient β at 20 to 200°C is 1.50 to 5.00 ppm / °C, A glass composition having an in-line transmittance of 80% or more at a wavelength of 850 nm. Effect of the Invention
[0013] According to the present invention, it is possible to provide a laminated member excellent in temperature rise property, impact resistance, and thermal shock resistance, and a glass composition used for a glass member constituting the laminated member. [Brief description of the drawings]
[0014] [Figure 1]FIG. 1 is a cross-sectional view that illustrates a laminated member according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The terms used in the present invention have the following meanings. A numerical range expressed using "~" means that the range includes the numerical values before and after "~" as the lower and upper limits.
[0016] [Laminated member] The laminated member of the present disclosure includes a glass member having an in-line transmittance of 80% or more at a wavelength of 850 nm, a bonding layer containing a resin on the glass member, and a Si-SiC member on the bonding layer, the glass member having an SiO content of 55.0 to 85.0 mol % in terms of oxide-based mole percentage. 2 and 1.5 to 22.0 mol% Al 2 O 3 and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol% P 2 O 5 and the SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O 5 the total content, expressed as a mole percentage based on oxides, of the Si-SiC member is 70.0 to 97.0%, the average linear expansion coefficient α of the Si-SiC member at 20 to 200°C is 2.85 to 4.00 ppm / °C, the average linear expansion coefficient β of the glass member at 20 to 200°C is 1.50 to 5.00 ppm / °C, and the absolute value |α-β| obtained by subtracting the average linear expansion coefficient β of the glass member at 20 to 200°C from the average linear expansion coefficient α of the Si-SiC member at 20 to 200°C is 2.00 ppm / °C or less.
[0017] The laminate member of the present disclosure has excellent temperature rise properties, impact resistance, and thermal shock resistance. Although the details of the reasons for this have not yet been clarified, it is generally assumed to be due to the following reasons.
[0018] In other words, it is presumed that by using a glass member with an in-line transmittance of 80% or more at a wavelength of 850 nm, sufficient infrared light for heating was transmitted, causing the temperature of the laminated members to rise rapidly.
[0019] It is also presumed that the inclusion of a resin-containing bonding layer allows the bonding layer to function as a buffer material, improving impact resistance.
[0020] In addition, since the average linear expansion coefficient α of the Si-SiC component, the average linear expansion coefficient β of the glass component, and the absolute value |α-β| are within the above ranges, the difference in expansion coefficient with the bonding layer containing resin is small, thereby reducing the generated stress and improving thermal shock resistance.
[0021] Hereinafter, a laminated member according to one embodiment of the present invention will be described with reference to the drawings.
[0022] 1 is a cross-sectional view showing a schematic diagram of a laminated member according to one embodiment of the present invention. The laminated member 100 includes a glass member 101, a bonding layer 103 disposed on the glass member 101, and a Si-SiC member 105 disposed on the bonding layer 103. The laminated member 100 has a layered structure in which the glass member 101, the bonding layer 103, and the Si-SiC member 105 are laminated in this order.
[0023] [Si-SiC components] In one embodiment of the present invention, the Si-SiC component means a sintered component made of a composite material containing silicon carbide (SiC) and silicon (Si) (metallic Si).
[0024] The Si-SiC member 105 is preferably a ceramic containing 40 to 92 mass% SiC and 8 to 60 mass% Si, more preferably 50 to 87 mass% SiC and 13 to 50 mass% Si, even more preferably 55 to 82 mass% SiC and 18 to 45 mass% Si, particularly preferably 60 to 77 mass% SiC and 23 to 40 mass% Si, and most preferably 65 to 72 mass% SiC and 28 to 35 mass% Si, based on the total mass of the Si-SiC member.
[0025] If the Si-SiC member 105 has Si and SiC contents within the above-mentioned ranges, the Si-SiC member 105 has an excellent balance between thermal properties and mechanical properties.
[0026] The composition of the Si-SiC member 105 is not particularly limited as long as it contains SiC and Si, and may contain components derived from sintering aids and trace amounts of impurities (Fe, etc.). The sintering aid is not particularly limited, but examples thereof include BeO, B 4 Examples include C, BN, Al, and AlN.
[0027] The thickness of Si-SiC member 105 is preferably 0.5 to 15 mm. The thickness of Si-SiC member 105 is more preferably 1.5 mm or more, further preferably 2.0 mm or more, and particularly preferably 2.5 mm or more.
[0028] The thickness of Si-SiC member 105 is more preferably 10.0 mm or less, further preferably 7.5 mm or less, and particularly preferably 5.5 mm or less.
[0029] The Si-SiC member 105 can be made thin by being supported by the glass member 101. Since the Si-SiC member 105 can be made thin, it is possible to quickly increase and decrease the temperature.
[0030] The thickness of the Si-SiC member 105 can be measured by, for example, a vernier caliper or a digital tape measure.
[0031] The average linear expansion coefficient α of the Si-SiC member 105 at 20 to 200° C. is 2.85 to 4.00 ppm / ° C. Hereinafter, the average linear expansion coefficient α of the Si-SiC member 105 at 20 to 200° C. will also be simply referred to as the average linear expansion coefficient α.
[0032] The average linear expansion coefficient α is preferably 2.90 ppm / ° C. or more, more preferably 2.95 ppm / ° C. or more, and particularly preferably 3.00 ppm / ° C. or more.
[0033] The average linear expansion coefficient α is preferably 3.40 ppm / ° C. or less, more preferably 3.20 ppm / ° C. or less, and particularly preferably 3.10 ppm / ° C. or less.
[0034] If the average linear expansion coefficient α of the Si-SiC member 105 is within the above-mentioned range, it is easy to make the average linear expansion coefficients of the Si-SiC member 105 and the glass member 101 match or approach each other. In addition, since the thermal conductivity and strength of the Si-SiC member 105 can be increased, the temperature rise rate can be increased and impact resistance can be improved.
[0035] In particular, if the average linear expansion coefficient α is 3.00 to 3.10 ppm / ° C., the balance between the thermal conductivity and strength of the Si-SiC member is more excellent.
[0036] The average linear expansion coefficient α can be measured by a dilatometer in a measurement temperature range of 20° C. to 200° C. or a thermomechanical analyzer (TMA).
[0037] The average linear expansion coefficient α of the Si—SiC member 105 can be adjusted to fall within the above range by adjusting the content of SiC and Si to fall within the above range.
[0038] The thermal conductivity of the Si-SiC member 105 at 20° C. is preferably 130 to 300 W / m·K.
[0039] The thermal conductivity of the Si-SiC member 105 at 20° C. is more preferably 190 W / m·K or more, further preferably 210 W / m·K or more, and particularly preferably 225 W / m·K or more.
[0040] The thermal conductivity of Si-SiC member 105 at 20° C. is more preferably 270 W / m·K or less, further preferably 260 W / m·K or less, and particularly preferably 250 W / m·K or less.
[0041] If the thermal conductivity of the Si-SiC member 105 at 20° C. is within the above range, the heating member has improved thermal uniformity. Furthermore, if the thermal conductivity of the Si-SiC member 105 is within the above range, a decrease in yield due to variations in thermal conductivity during the manufacture of the Si-SiC member 105 can be prevented, and the quality of the Si-SiC member 105 can be easily stabilized.
[0042] The thermal conductivity of the Si-SiC member 105 at 20° C. can be measured by, for example, a laser flash method.
[0043] One method for adjusting the thermal conductivity of Si-SiC member 105 at 20° C. to the above range is to adjust the content of SiC and Si to the above range.
[0044] The Young's modulus of the Si-SiC member 105 is preferably 300 to 420 GPa, more preferably 320 GPa or more, further preferably 350 GPa or more, and particularly preferably 370 GPa or more.
[0045] The Young's modulus of the Si-SiC member 105 is more preferably 410 GPa or less, further preferably 400 GPa or less, and particularly preferably 390 GPa or less.
[0046] The lower the Young's modulus, the higher the thermal shock resistance. The Si-SiC member 105 is preferable because the thermal shock resistance is improved by having a Young's modulus that satisfies the above range. In addition, the Si-SiC member 105 has a lower Young's modulus than other silicon carbide ceramics, and is therefore preferable because it has high thermal shock resistance.
[0047] The Young's modulus of the Si-SiC member 105 can be measured at 20° C. by the elastic modulus test method (ultrasonic pulse method: dynamic elastic modulus) described in the Japanese Industrial Standards (JIS R1602:1995).
[0048] One method for adjusting the Young's modulus of the Si-SiC member 105 to fall within the above range is to adjust the content of SiC and Si to fall within the above range.
[0049] The bending strength of the Si-SiC member 105 is preferably 130 to 300 MPa, more preferably 200 MPa or more, further preferably 220 MPa or more, and particularly preferably 230 MPa or more.
[0050] The bending strength of Si-SiC member 105 is more preferably 260 MPa or less, further preferably 250 MPa or less, and particularly preferably 240 MPa or less.
[0051] When the bending strength of Si-SiC member 105 satisfies the above range, cracking of Si-SiC member 105 and therefore laminated member 100 due to a falling object can be prevented, and impact resistance can be improved.
[0052] The bending strength of the Si-SiC member 105 can be measured at 20° C. by the bending strength test method (four-point bending strength) described in the Japanese Industrial Standards (JIS R1601:2008).
[0053] The Vickers hardness (Hv) of the Si-SiC member 105 is preferably 20 to 27 GPa.
[0054] The Vickers hardness is more preferably 21 GPa or more, further preferably 22 GPa or more, and particularly preferably 23 GPa or more.
[0055] The Vickers hardness is more preferably 26 GPa or less, further preferably 25 GPa or less, and particularly preferably 24 GPa or less.
[0056] When the Vickers hardness of the Si-SiC member 105 satisfies the above range, the scratch resistance of the Si-SiC member 105 and therefore of the laminate member 100 is improved.
[0057] The Vickers hardness of the Si-SiC member 105 can be measured at 20° C. using a Vickers hardness tester system.
[0058] [Glass Members] Examples of the glass member 101 include soda-lime glass, borosilicate glass, aluminosilicate glass, and alkali-free glass. The glass member 101 may be chemically strengthened glass (chemically strengthened glass), physically strengthened glass by air cooling or the like (physically strengthened glass), or glass that has been subjected to a crystallization process (crystallized glass).
[0059] The following describes the glass composition of the glass member 101. In this specification, the glass composition (content of target components in the glass member) is expressed in terms of oxide-based mole percentage (mol%).
[0060] The glass member 101 is made of SiO 2 Contains SiO 2 is the main component of glass.
[0061] SiO 2 From the viewpoint of enhancing the weather resistance of the glass, the content is 55.0 mol % or more, preferably 57.0 mol % or more, more preferably 60.0 mol % or more, and particularly preferably 62.0 mol % or more.
[0062] SiO 2 From the viewpoint of lowering the melting temperature of the glass and improving manufacturability, the content is 85.0 mol % or less, preferably 83.0 mol % or less, more preferably 80.0 mol % or less, and particularly preferably 78.0 mol % or less.
[0063] The glass member 101 is made of Al 2 O 3 Contains Al. 2 O 3By containing this, the weather resistance of the glass can be improved and the linear expansion coefficient can be reduced.
[0064] Al 2 O 3 The content is 1.5 mol % or more, preferably 3.0 mol % or more, more preferably 5.0 mol % or more, and particularly preferably 8.0 mol % or more, in order to increase the Young's modulus of the glass.
[0065] Al 2 O 3 The content of is 22.0 mol% or less from the viewpoint of increasing the acid resistance of the glass. Also, from the viewpoints of suppressing devitrification of the glass (capable of lowering the devitrification temperature), suppressing the generation of unmelted materials in the raw materials, and suppressing an increase in the melting temperature of the glass to improve clarification, the content is preferably 18.0 mol% or less, more preferably 17.0 mol% or less, and particularly preferably 16.0 mol% or less.
[0066] The glass member 101 is B 2 O 3 Contains. B 2 O 3 By containing this, the linear expansion coefficient of the glass can be adjusted.
[0067] B 2 O 3 The content is at least 2.0 mol %, preferably at least 3.5 mol %, and particularly preferably at least 5.0 mol %, from the viewpoint of suppressing the linear expansion coefficient of the glass.
[0068] B 2 O 3 The content of is 14.0 mol % or less from the viewpoint of improving the weather resistance of the glass. Also, from the viewpoint of increasing the Young's modulus of the glass, it is preferably 11.0 mol % or less, more preferably 10.0 mol % or less, further preferably 8.5 mol % or less, and particularly preferably 7.5 mol % or less.
[0069] The glass member 101 may or may not contain RO. RO means at least one of MgO, CaO, SrO, and BaO. The content of RO represents the total amount of MgO, CaO, SrO, and BaO.
[0070] The total content of RO and ZnO is preferably 2.0 mol % or more, more preferably 3.0 mol % or more, even more preferably 4.0 mol % or more, and particularly preferably 5.0 mol % or more, from the viewpoints of lowering the melting temperature of the glass to enhance the solubility and controlling the linear expansion coefficient.
[0071] From the viewpoints of lowering the devitrification temperature of the glass to improve manufacturability and controlling the linear expansion coefficient, the total content of RO and ZnO is preferably 25.0 mol% or less, more preferably 20.0 mol% or less, even more preferably 16.0 mol% or less, and particularly preferably 15.0 mol% or less.
[0072] MgO may be contained in order to lower the melting temperature of the glass to increase the meltability and to control the linear expansion coefficient.
[0073] The MgO content is preferably 1.0 mol % or more, more preferably 2.0 mol % or more, further preferably 2.5 mol % or more, and particularly preferably 3.0 mol % or more.
[0074] The MgO content is preferably 15.0 mol % or less, more preferably 12.0 mol % or less, even more preferably 10.0 mol % or less, and particularly preferably 9.0 mol % or less, from the viewpoints of lowering the devitrification temperature of the glass to increase productivity and controlling the linear expansion coefficient.
[0075] CaO may be contained in order to lower the melting temperature of the glass to increase the meltability and to control the linear expansion coefficient.
[0076] The CaO content is preferably 0.5 mol % or more, and more preferably 1.0 mol % or more.
[0077] The CaO content is preferably 10.0 mol % or less, and more preferably 8.0 mol % or less.
[0078] SrO may be contained in order to lower the melting temperature of the glass to increase the meltability and to control the linear expansion coefficient.
[0079] The SrO content is preferably 0 mol % or more, more preferably 0.01 mol % or more, and further preferably 0.1 mol % or more.
[0080] The SrO content is preferably 5.0 mol % or less, more preferably 3.0 mol % or less, and further preferably 2.0 mol % or less.
[0081] BaO may be contained in order to lower the melting temperature of the glass to increase productivity and to control the linear expansion coefficient.
[0082] The BaO content is preferably 0 mol % or more, and more preferably 0.01 mol % or more.
[0083] The BaO content is preferably 3.0 mol % or less, and more preferably 2.0 mol % or less.
[0084] Even if BaO is not intentionally added, it can be mixed in as an impurity from raw materials such as limestone, dolomite, and strontium carbonate, or from the manufacturing process.
[0085] The glass member 101 is R 2 It may or may not contain O. 2 O is Li 2 O, Na 2 O and K 2 O. 2 The O content is Li 2 O, Na 2 O and K 2 represents the total amount of O.
[0086] R 2O is a component that promotes the melting of glass raw materials and is useful for adjusting the linear expansion coefficient, melting temperature, and the like.
[0087] R 2 In order to satisfactorily exert the above effects, the O content is preferably 0 mol % or more, and more preferably 0.01 mol % or more.
[0088] R 2 The O content is preferably 15.0 mol % or less, more preferably 10.0 mol % or less, further preferably 6.0 mol % or less, and particularly preferably 5.0 mol % or less, from the viewpoint of reducing the linear expansion coefficient of the glass and reducing the stress generated during temperature changes.
[0089] In addition, Li 2 R without O 2 O, i.e. Na 2 O and K 2 The total amount of O is preferably 0 mol % or more, and more preferably 0.01 mol % or more.
[0090] Li 2 R without O 2 O, i.e. Na 2 O and K 2 The total amount of O is preferably 13.0 mol % or less, more preferably 10.0 mol % or less, further preferably 5.0 mol % or less, and particularly preferably 3.0 mol % or less, in order to reduce the linear expansion coefficient.
[0091] Li 2 O is a component that promotes the melting of glass raw materials and is useful for adjusting the linear expansion coefficient, melting temperature, and the like.
[0092] Li 2 The O content is preferably 0 mol % or more, and more preferably 0.01 mol % or more.
[0093] Li 2From the viewpoint of reducing the linear expansion coefficient of the glass and reducing the stress generated during temperature changes, the O content is preferably 10.0 mol % or less, more preferably 7.0 mol % or less, further preferably 5.0 mol % or less, and particularly preferably 4.0 mol % or less.
[0094] Na 2 O is a component that promotes the melting of glass raw materials and is useful for adjusting the linear expansion coefficient, melting temperature, and the like.
[0095] Na 2 The O content is preferably 0 to 13.0 mol %. Na 2 The O content is more preferably 0.01 mol % or more. Na 2 The O content is more preferably 10.0 mol % or less, further preferably 5.0 mol % or less, and particularly preferably 3.0 mol % or less. Na 2 If the O content is 13.0 mol % or less, the linear expansion coefficient of the glass can be made small, and the stress generated during temperature changes can be reduced.
[0096] K 2 O is a component that promotes the melting of glass raw materials and is useful for adjusting the linear expansion coefficient, melting temperature, and the like.
[0097] K 2 The O content is preferably 0 mol % or more, and more preferably 0.01 mol % or more.
[0098] K 2 The O content is preferably 3.0 mol % or less, more preferably 1.0 mol % or less, and even more preferably 0.1 mol % or less, from the viewpoint of reducing the linear expansion coefficient of the glass and reducing the stress generated when exposed to high temperatures.
[0099] The glass member 101 is ZrO 2 It may or may not contain ZrO 2 When it contains, the chemical resistance of the glass can be improved.
[0100] ZrO 2 The content of is preferably 0 mol % or more, more preferably 0.01 mol % or more, and even more preferably 0.1 mol % or more, in order to satisfactorily exert the above-mentioned effects.
[0101] ZrO 2 From the viewpoint of lowering the devitrification temperature of the glass and increasing the productivity, the content is preferably 5.0 mol % or less, more preferably 3.0 mol % or less, and even more preferably 2.0 mol % or less.
[0102] The glass member 101 is made of TiO 2 It may or may not contain TiO 2 When it contains, the chemical resistance of the glass can be improved.
[0103] TiO 2 The content of is preferably 0 mol % or more, more preferably 0.01 mol % or more, and even more preferably 0.1 mol % or more, in order to satisfactorily exert the above-mentioned effects.
[0104] TiO 2 The content is preferably 5.0 mol % or less, more preferably 3.0 mol % or less, and even more preferably 2.0 mol % or less, from the viewpoints of lowering the devitrification temperature of the glass to increase productivity and suppressing unnecessary coloring.
[0105] The glass member 101 is made of P 2 O 5 It may or may not contain P 2 O 5 When it contains, crystallization of the glass can be suppressed and the glass can be stabilized.
[0106] P 2 O 5 The content of is 0 mol % or more. In order to satisfactorily exert the above-mentioned effects, the content is preferably 0.05 mol % or more, and more preferably 0.1 mol % or more.
[0107] P 2 O 5The content of is 5.0 mol % or less, preferably 4.0 mol % or less, more preferably 3.5 mol % or less, and particularly preferably 3.0 mol % or less, from the viewpoints of being able to stabilize the glass without making the melting temperature of the glass too high and of being able to suppress phase separation of the glass and improve transparency.
[0108] The glass member 101 is made of Fe 2 O 3 It may or may not contain Fe. 2 O 3 When the glass contains , the clarity of the glass is improved without impairing the color of the glass, and the temperature of the bottom base of the melting furnace can be controlled. In addition, it becomes easy to adjust the linear transmittance of the glass member 101 at a wavelength of 850 nm to the range described below, and a stable product can be obtained.
[0109] Fe 2 O 3 The content of is preferably 0.0001 mol % or more, more preferably 0.0005 mol % or more, and even more preferably 0.0010 mol % or more, in order to satisfactorily exert the above-mentioned effects.
[0110] Fe 2 O 3 From the viewpoint of maintaining the color of the glass, the content is preferably 0.0115 mol % or less, more preferably 0.0100 mol % or less, even more preferably 0.0080 mol % or less, and particularly preferably 0.0050 mol % or less.
[0111] Glass member 101 may or may not contain ZnO. The ZnO content is preferably 0 mol % or more, more preferably 0.01 mol % or more, further preferably 0.1 mol % or more, and particularly preferably 0.5 mol % or more.
[0112] From the viewpoint of lowering the devitrification temperature of the glass and increasing productivity, the ZnO content is preferably 15.0 mol % or less, more preferably 12.0 mol % or less, further preferably 10.0 mol % or less, and particularly preferably 8.0 mol % or less.
[0113] The glass member 101 may contain other components (e.g., TiO 2 , Y 2 O 3 , Gd 2 O 3 etc.) may also be contained. The total content of other components is preferably 10.0 mol % or less.
[0114] The glass member 101 contains sulfates, chlorides, fluorides, halides, hydroxides, SnO as a fining agent when melting the glass. 2 , Sb 2 O 3 , As 2 O 3 etc. may be appropriately contained.
[0115] Furthermore, in order to adjust the color, coloring components such as Ni, Co, Cr, Mn, V, Se, Au, Ag, and Cd may be contained.
[0116] Furthermore, when coloring is desired, a coloring component such as Fe, Ni, Co, Cr, Mn, V, Se, Au, Ag, or Cd may be contained in an amount of 0.0001 mol % or more.
[0117] Among the other components listed above, sulfates, chlorides, fluorides, halides, hydroxides, SnO 2 , Sb 2 O 3 , and As 2 O 3 When at least one selected from the group consisting of is contained, the total content of these groups is preferably 0.01 mol % or more, more preferably 0.02 mol % or more, and even more preferably 0.05 mol % or more, from the viewpoint of clarity.
[0118] The total content of these elements is preferably 5.0 mol % or less, more preferably 2.0 mol % or less, and even more preferably 1.0 mol % or less, in order not to affect the glass properties.
[0119] SiO 2 , Al2 O 3 , B 2 O 3 and P 2 O 5 is a glass network former.
[0120] SiO in the glass member 101 2 , Al 2 O 3 , B 2 O 3 and P 2 O 5 From the viewpoint of enhancing the stability and chemical durability of the glass structure, the total content of is 70.0 mol % or more, preferably 75.0 mol % or more, more preferably 78.0 mol % or more, and particularly preferably 80.0 mol % or more.
[0121] SiO 2 , Al 2 O 3 , B 2 O 3 and P 2 O 5 From the viewpoint of suppressing an increase in the melting temperature of the glass and improving the clarity, the total content of is 97.0 mol % or less, preferably 95.0 mol % or less, more preferably 93.0 mol % or less, and particularly preferably 90.0 mol % or less.
[0122] A preferred embodiment of the glass composition of the glass member 101 is 55.0 to 85.0 mol % SiO 2 and 1.5 to 14.5 mol% Al 2 O 3 and 3.0 to 14.0 mol% B 2 O 3 and 0 to 3.5 mol% P 2 O 5 and SiO in the glass member 101. 2 , Al 2 O 3 , B 2 O 3 and P 2 O 5The total content of these elements, expressed as a mole percentage based on oxides, may be 70.0 to 97.0%, which provides more excellent glass properties.
[0123] There is no particular limitation on the thickness of glass member 101, as long as it is thick enough to support Si-SiC member 105. Specifically, the thickness of glass member 101 is preferably 2 to 40 mm.
[0124] The thickness of glass member 101 is more preferably 3 mm or more, further preferably 5 mm or more, particularly preferably 10 mm or more, and most preferably 15 mm or more.
[0125] The thickness of glass member 101 is more preferably 35 mm or less, further preferably 30 mm or less, and particularly preferably 25 mm or less.
[0126] If the thickness of glass member 101 is within the above range, it can maintain sufficient strength as a supporting member.
[0127] The thickness of the glass member 101 can be measured, for example, by using a vernier caliper or a digital tape measure.
[0128] The average linear expansion coefficient β of the glass member 101 at 20 to 200° C. is 1.50 to 5.00 ppm / ° C. Hereinafter, the average linear expansion coefficient β of the glass member 101 at 20 to 200° C. will also be simply referred to as the average linear expansion coefficient β.
[0129] The average linear expansion coefficient β is preferably 2.00 ppm / ° C. or more, more preferably 2.50 ppm / ° C. or more, and particularly preferably 2.60 ppm / ° C. or more.
[0130] The average linear expansion coefficient β is preferably 3.50 ppm / °C or less, more preferably 3.25 ppm / °C or less, further preferably 3.10 ppm / °C or less, and particularly preferably 3.00 ppm / °C or less.
[0131] If the average linear expansion coefficient β of the glass member 101 is within the above-mentioned range, it is easier to match the average linear expansion coefficients of the glass member 101 and the Si-SiC member 105, and the smaller β is, the smaller the distortion that occurs inside the glass when a temperature difference occurs inside the glass member.
[0132] The average linear expansion coefficient β can be measured by a dilatometer in the measurement temperature range of 20° C. to 200° C. or a thermomechanical analyzer (TMA).
[0133] The absolute value |α-β| of the average linear expansion coefficient α of the Si-SiC member 105 minus the average linear expansion coefficient β of the glass member 101 is 2.00 ppm / ° C. or less. The absolute value |α-β| is preferably 1.00 ppm / ° C. or less, more preferably 0.50 ppm / ° C. or less, and particularly preferably 0.30 ppm / ° C. or less.
[0134] By setting the absolute value |α-β| to the above value or less, warping of the resulting laminate member 100 can be prevented.
[0135] Since Si-SiC has a higher thermal conductivity than glass, a temperature difference may occur during use between the Si-SiC member 105 and the glass member 101. In particular, when cooling, tensile stress is applied to the surface of the glass opposite the bonding layer, making the glass more likely to break. Therefore, it is preferable that the average linear expansion coefficient β of the glass member 101 is smaller than the average linear expansion coefficient α of the Si-SiC member 105.
[0136] The linear transmittance of glass member 101 at a wavelength of 850 nm is 80% or more, preferably 85% or more, more preferably 88% or more, and even more preferably 90% or more. If the linear transmittance of glass member 101 at a wavelength of 850 nm is 80% or more, a sufficient amount of infrared light can be transmitted for heating. The upper limit of the in-line transmittance of the glass member 101 is 100%.
[0137] The linear transmittance is the transmittance of light that is linearly transmitted through the glass member 101 in its thickness direction with the incident angle of the incident light being 0°, and can be measured at 20° C. using a spectrophotometer.
[0138] As a method for adjusting the in-line transmittance of the glass member 101 to the above range, Fe 2 O 3 The content of the antireflection coating may be adjusted to fall within the above-mentioned range, or an antireflection coating may be formed to suppress the surface reflection of the glass member 101. As a method for forming the antireflection coating, a commonly known method may be used, such as wet coating by spray coating, spin coating, flow coating, or the like, or dry coating by sputtering, vapor deposition, or the like.
[0139] The Young's modulus of the glass member 101 is preferably 40 to 120 GPa.
[0140] The Young's modulus of the glass member 101 is more preferably 60 GPa or more, further preferably 65 GPa or more, and particularly preferably 70 GPa or more.
[0141] The Young's modulus of the glass member 101 is more preferably 100 GPa or less, further preferably 95 GPa or less, and particularly preferably 90 GPa or less.
[0142] If the Young's modulus of glass member 101 falls within the above range, it will maintain sufficient strength as a supporting member and the amount of warping can be reduced.
[0143] The Young's modulus of the glass member 101 can be measured at 20° C. by the ultrasonic pulse method described in the Japanese Industrial Standards (JIS R1602:1995).
[0144] The melting temperature of the glass member 101 is preferably 1000 to 2000°C.
[0145] The melting temperature of the glass member 101 is more preferably 1300° C. or higher, further preferably 1400° C. or higher, and particularly preferably 1500° C. or higher.
[0146] The melting temperature of the glass member 101 is more preferably 1900° C. or lower, further preferably 1800° C. or lower, and particularly preferably 1700° C. or lower.
[0147] If the melting temperature of glass member 101 is within the above-mentioned range, the clarity of the glass and the solubility of the raw materials are excellent, and defects in the glass can be suppressed.
[0148] The melting temperature of the glass member 101 was measured by measuring the viscosity using a rotational viscometer. 2 The temperature T2 (℃) at which the viscosity becomes dPa·s is indicated.
[0149] The devitrification temperature of the glass member 101 is preferably 800 to 1600°C.
[0150] The devitrification temperature of the glass member 101 is more preferably 900° C. or higher, further preferably 1000° C. or higher, and particularly preferably 1100° C. or higher.
[0151] The devitrification temperature of the glass member 101 is more preferably 1500° C. or lower, further preferably 1450° C. or lower, and particularly preferably 1400° C. or lower.
[0152] If the devitrification temperature of glass member 101 falls within the above range, defects occurring during glass production are reduced.
[0153] The devitrification temperature of glass member 101 is the maximum temperature at which no crystals precipitate on the surface or inside of the glass when crushed glass particles are placed in a platinum dish and heat-treated for 17 hours in an electric furnace controlled at a constant temperature, and observed with an optical microscope after the heat treatment.
[0154] [Joining layer] The bonding layer 103 is a member that bonds the glass member 101 and the Si—SiC member 105 together.
[0155] Examples of the resin contained in the bonding layer 103 include epoxy resin, silicone resin, fluororesin, and polyimide resin. Epoxy resin, silicone resin, and fluororesin are preferred because they have superior heat resistance. The resins may be used alone or in combination of two or more kinds.
[0156] The resin content is preferably 40 to 100% by mass, more preferably 50 to 90% by mass, and further preferably 60 to 80% by mass, based on the total mass of the bonding layer 103.
[0157] If the resin content is within the above range, the adhesion between glass member 101 and Si--SiC member 105 via bonding layer 103 is superior, and the difference in the expansion coefficient with the Si--SiC member can be reduced.
[0158] The bonding layer 103 may or may not contain components other than resin (hereinafter, also referred to as “other components”). Specific examples of other components include, for example, a plasticizer, a filler, and the like.
[0159] When bonding layer 103 contains other components, the content of the other components is preferably 10 to 50 mass %, more preferably 20 to 40 mass %, and even more preferably 25 to 35 mass %, relative to the total mass of bonding layer 103. If the content of the other components is 50 mass % or less, the adhesion between glass member 101 and Si-SiC member 105 via bonding layer 103 is better.
[0160] The bonding layer 103 may be made of a resin film, a coating type adhesive, or the like.
[0161] When the bonding layer 103 is made of a resin film, it can be produced using, for example, a heating press device. The resin film that constitutes the bonding layer 103 is sandwiched between the glass member 101 and the Si-SiC member 105 (this configuration is called a temporary laminate). The temporary laminate is heated to a temperature equal to or higher than the softening point of the resin film, and pressure is applied to press the temporary laminate to bond the glass member 101 and the Si-SiC member 105. In order to prevent bubbles from being trapped during bonding, it is preferable to press the temporary laminate in a vacuum atmosphere.
[0162] Furthermore, when bonding layer 103 is made of a coating type adhesive, it is applied onto glass member 101 by any conventionally known method, and Si-SiC member 105 is laminated thereon.
[0163] In order to enhance the anchor effect, the contact surface of glass member 101 with bonding layer 103 and the contact surface of Si--SiC member 105 with bonding layer 103 may be appropriately roughened by blasting or the like.
[0164] The thickness of the bonding layer 103 is preferably 0.001 to 0.300 mm.
[0165] The thickness of the bonding layer 103 may be 0.005 mm or more, 0.008 mm or more, or 0.010 mm or more.
[0166] The thickness of the bonding layer 103 may be 0.150 mm or less, 0.050 mm or less, or 0.030 mm or less.
[0167] The thickness of the bonding layer 103 can be calculated using digital data captured by SEM cross-sectional observation and image processing software.
[0168] The linear transmittance of the bonding layer 103 at a wavelength of 850 nm is preferably 88% or more, more preferably 91% or more, even more preferably 93% or more, and particularly preferably 95% or more. If the linear transmittance of the bonding layer 103 is 88% or more, a sufficient amount of infrared light can be transmitted for heating. The upper limit of the in-line transmittance of the bonding layer 103 is 100%.
[0169] The linear transmittance is the transmittance of light that is linearly transmitted through the bonding layer 103 in its thickness direction with the incident angle of the incident light being 0°, and can be measured at 20° C. with a spectrophotometer.
[0170] The heat resistance temperature of the resin contained in the bonding layer 103 is preferably 120 to 420° C., and more preferably 120 to 300° C. from the viewpoint of stress relaxation during use at high temperatures.
[0171] The heat resistance temperature of the resin contained in the bonding layer 103 is more preferably 140° C. or higher, particularly preferably 160° C. or higher, and most preferably 180° C. or higher.
[0172] The heat resistance temperature of the resin contained in the bonding layer 103 may be 280° C. or lower, 260° C. or lower, or 240° C. or lower.
[0173] The heat-resistant temperature of the resin contained in the bonding layer 103 is determined as the temperature at which the mass of a measurement object decreases by 1% by mass when thermogravimetry (TGA) is performed in the air.
[0174] The average linear expansion coefficient γ of the bonding layer 103 at 20 to 200° C. is preferably 2 to 200 ppm / ° C. Hereinafter, the average linear expansion coefficient γ of the bonding layer 103 at 20 to 200° C. will also be simply referred to as the average linear expansion coefficient γ.
[0175] The average linear expansion coefficient γ is more preferably 4 ppm / ° C. or more, further preferably 7 ppm / ° C. or more, and particularly preferably 10 ppm / ° C. or more.
[0176] The average linear expansion coefficient γ is more preferably 100 ppm / ° C. or less, further preferably 50 ppm / ° C. or less, particularly preferably 30 ppm / ° C. or less, and most preferably 20 ppm / ° C. or less.
[0177] If the average linear expansion coefficient γ of the bonding layer 103 is within the above range, the bonding layer 103 has excellent adhesion, and the difference in expansion coefficient with the Si--SiC member can be reduced, so that the laminate member 100 has excellent thermal shock resistance.
[0178] The average linear expansion coefficient γ can be measured by a dilatometer in the measurement temperature range of 20° C. to 200° C. or a thermomechanical analyzer (TMA).
[0179] As a method for setting the average linear expansion coefficient γ of the bonding layer 103 within the above range, there is a method in which the above-mentioned types of resin are used and a filler such as carbon or silica is blended therein.
[0180] When a resin film is used to prepare the bonding layer 103, the Young's modulus of the resin film is preferably 0.05 GPa or more, more preferably 0.10 GPa or more, and even more preferably 0.15 GPa or more, in order to increase the adhesion between the Si-SiC member 105 and the glass member 101 and maintain the shape of the entire member.
[0181] When a resin film is used to prepare the bonding layer 103, the Young's modulus of the resin film is preferably 3.5 GPa or less, more preferably 3.0 GPa or less, even more preferably 2.0 GPa or less, particularly preferably 1.0 GPa or less, and most preferably 0.5 GPa or less, in order to reduce stress arising from the difference in expansion coefficient with the Si-SiC component.
[0182] The stress generated by the difference in expansion coefficient with the Si-SiC member increases as the Young's modulus of the resin layer increases, and decreases as the Young's modulus decreases.
[0183] The Young's modulus of the resin layer can be measured at 25° C. by the elastic modulus test method described in the Japanese Industrial Standards (JIS K7171).
[0184] [Physical properties of laminated materials] The amount of warping of the laminate member 100 is preferably 0.25 mm or less, more preferably 0.20 mm or less, even more preferably 0.10 mm or less, and particularly preferably 0.05 mm or less.
[0185] If the amount of warping of the laminated member 100 is equal to or less than the above value, stress concentration at a specific location can be prevented when stress is generated, and impact resistance can be further improved. In addition, when the laminated member 100 is used for kitchen applications, it is possible to prevent the surroundings from being distorted due to the warping of the laminated member 100, which is reflected in the laminated member 100 and reduces the design quality. In addition, when a heated object is placed on the laminated member 100, the heated object can be prevented from wobbling.
[0186] The lower limit of the warpage of the laminated member 100 is 0 mm.
[0187] The amount of warping of the laminated member 100 can be measured by a non-contact three-dimensional shape measuring device.
[0188] Methods for keeping the amount of warping of the laminated member 100 within the above range include adjusting the thicknesses of the glass member 101, bonding layer 103, and Si-SiC member 105, and the types and contents of the components constituting each member (layer) as described above.
[0189] The density of the laminated member 100 is 2.40 to 2.85 g / cm 3 is preferred.
[0190] The density of the laminated member 100 is 2.45 g / cm 3 More preferably, 2.50 g / cm 3 More preferably, 2.55 g / cm 3 The above is particularly preferred.
[0191] The density of the laminated member 100 is 2.80 g / cm 3 Less than 2.75 g / cm is more preferable. 3 More preferably, 2.70 g / cm 3 The following are particularly preferred:
[0192] If the density is within the above range, workability is improved when the laminate member is incorporated into a housing as a heating member.
[0193] The density is a value obtained by dividing the total mass of the lamination member 100 by the total volume of the lamination member 100. The total mass of the lamination member 100 can be measured by a mass measuring device. The total volume of the lamination member 100 can be measured by a digital measure.
[0194] Methods for setting the density of the laminated member 100 within the above range include adjusting the thicknesses of the glass member 101, bonding layer 103, and Si-SiC member 105, and the types and contents of the components constituting each member (layer) as described above.
[0195] The area of the top surface of the laminated member 100 on the Si-SiC member 105 side (the main surface of the laminated member 100 on the Si-SiC member 105 side) is 0.01 to 10 m 2 is preferred.
[0196] The area of the top surface of the laminated member 100 is 0.07 m 2 More preferably, 0.15m or more 2 More preferably, 0.30m or more 2 More than 0.60m is particularly preferable. 2 The above is most preferable.
[0197] The area of the top surface of the laminated member 100 is 8 m 2 Less than 4m is preferable. 2 Less than 2m is more preferable. 2 The following is particularly preferred: 1m 2 The following are most preferred:
[0198] If the area of the top surface of the laminated member 100 is within the above-mentioned range, workability is improved when the laminated member 100 is incorporated into a housing as a heating member.
[0199] The area of the uppermost surface is calculated by measuring the dimensions of the laminated member 100 with a digital tape measure.
[0200] [Method for manufacturing laminated member] One example of a method for manufacturing the laminated member 100 is to place a bonding layer 103 between the glass member 101 and the Si-SiC member 105, and bond the glass member 101 and the Si-SiC member 105 together with the bonding layer 103 interposed therebetween.
[0201] As a more detailed example of a method for producing the laminated member 100, there is a method in which the glass member 101, the bonding layer 103, and the Si-SiC member 105 are laminated in this order, and then bonded together at a temperature of 150 to 380°C.
[0202] Other Aspects A laminated member of another embodiment (hereinafter also referred to as "a laminated member of another embodiment") which is an example of the laminated member of the present invention and differs from the laminated member 100 described above will be described.
[0203] The laminated member of another embodiment further includes a second bonding layer provided on the Si-SiC member 105, and a second Si-SiC member bonded to the Si-SiC member 105 via the second bonding layer. The second Si--SiC member is configured similarly to the above-mentioned Si--SiC member 105, and therefore a description thereof will be omitted.
[0204] By stacking the Si-SiC member 105 and the second Si-SiC member, it becomes easy to fabricate a laminated member with a complex shape. For example, when providing a space for inserting a temperature measuring sensor in the laminated member, a groove is formed in advance in one of the Si-SiC member 105 and the second Si-SiC member, and the other is bonded together, making it easy to provide a space in the laminated member.
[0205] The method for bonding the Si-SiC member 105 and the second Si-SiC member by the second bonding layer is not particularly limited, but examples thereof include bonding using a resin such as epoxy resin or fluororesin, bonding using a molten metal such as tin or indium, and bonding using glass frit. Assuming that the laminated member is used as a heating member, bonding using a metal is preferable in terms of heat resistance and thermal conductivity.
[0206] From the viewpoints of heat resistance and thermal conductivity, glass frit has high heat resistance but low thermal conductivity, while resin has low heat resistance and low thermal conductivity, so that bonding using a metal is preferable. Specific examples of metals include indium, tin, tin-based alloys, and lead-based alloys. Among them, tin metal and tin-based alloys are preferable from the viewpoints of thermal conductivity, heat resistance, and environmental load.
[0207] An example of bonding using molten metal will be described. The Si-SiC member 105 and the second Si-SiC member are heated to a desired temperature, for example, 250°C to 270°C. While applying ultrasonic waves to the bonding surfaces of the heated Si-SiC member and the second Si-SiC member, metal that has been melted at a temperature close to the desired temperature (for example, 250°C to 270°C) is applied, and then the bonding surfaces are overlapped.
[0208] The laminated member of another embodiment may further include a third bonding layer provided on the second Si-SiC member, and a third Si-SiC member bonded to the second Si-SiC member via the third bonding layer. The third bonding layer is configured similarly to the second bonding layer. The third Si-SiC member is configured similarly to the Si-SiC member 105. However, in terms of thickness, the laminated member of another embodiment preferably does not include the third bonding layer and the third ceramic member.
[0209] The laminated member of the present invention may have a configuration that allows the laminated member to be rapidly cooled.
[0210] For example, the laminated member 100 may have a flow path at least between the glass member 101 and the bonding layer 103 and between the Si-SiC member 105 and the bonding layer 103. Alternatively, the laminated member 100 may be processed so that at least one of the glass member 101 and the Si-SiC member 105 forms a flow path.
[0211] Furthermore, the stacked member of another embodiment may have a flow path in at least one of between the glass member 101 and the bonding layer 103, between the Si-SiC member 105 and the bonding layer 103, between the Si-SiC member 105 and the second bonding layer, and between the second Si-SiC member and the second bonding layer. Alternatively, the stacked member of another embodiment may be processed so that at least one of the glass member 101, the Si-SiC member 105, and the second Si-SiC member becomes a flow path. The laminated members can be cooled by passing water through the channels.
[0212] The laminate member of the present invention may be provided with an anti-reflection coating that enhances transmittance and irradiation efficiency.
[0213] For example, the laminated member 100 may be provided with an anti-reflection film on the main surface of the glass member 101 opposite the bonding layer 103 side and / or on the main surface of the glass member 101 on the bonding layer 103 side.
[0214] Furthermore, in another embodiment of the laminated member, an anti-reflection film may be provided on the main surface of the Si-SiC member 105 on the bonding layer 103 side or on the main surface of the second Si-SiC member on the second bonding layer side.
[0215] By providing an anti-reflection film on a surface that transmits infrared rays, the irradiation efficiency (heating efficiency) can be improved.
[0216] The laminated member of the present invention may be equipped with a temperature sensor.
[0217] For example, the laminated member 100 may include a temperature sensor inside the Si-SiC member 105. Also, in another embodiment of the laminated member, the temperature sensor may be included inside the Si-SiC member 105 or inside the second Si-SiC member.
[0218] A specific example of a configuration having a temperature sensor is a configuration in which a temperature sensor is inserted into a hole opened in a side surface of the Si-SiC member 105 or the second Si-SiC member. In this case, the temperature sensor is disposed directly under the main surface of the Si-SiC member 105 opposite the bonding layer 103 side, or directly under the main surface of the second Si-SiC member opposite the second bonding layer. The temperature sensor is disposed so as not to contact the bonding layer 103 or the second bonding layer, and so as not to be exposed. The temperature sensor can measure the main surface temperature of the Si-SiC member 105 opposite the bonding layer 103 side, or the main surface temperature of the second Si-SiC member opposite the second bonding layer.
[0219] The laminated member of the present invention can be suitably used as a heating member. The laminated member of the present invention can be suitably used as a heating member of, for example, a cooking device.
[0220] The laminate member of the present invention may also be used as a kitchen worktop (top plate).
[0221] The laminate member of the present invention may also be used as a material for a mounting table on which an electronic device is placed in an inspection apparatus or test apparatus for conducting electrical tests on electronic devices.
[0222] Furthermore, the laminated member of the present invention may also function as a top plate for an inspection or testing apparatus for conducting electrical tests on cooking appliances or electronic devices, and as a kitchen worktop.
[0223] [Glass composition] One aspect of the glass composition of the present disclosure is a glass composition used in a laminated member including a glass member, a bonding layer containing a resin on the glass member, and a Si-SiC member on the bonding layer, the glass composition having a linear transmittance of 80% or more at a wavelength of 850 nm, and a SiO content of 55.0 to 85.0 mol % expressed in terms of oxide-based mole percentage. 2 and 1.5 to 22.0 mol% Al 2 O 3and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol% P 2 O 5 and the glass composition comprises the SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O 5 and the total content, expressed as a mole percentage based on oxides, of the glass composition is 70.0 to 97.0%, the glass composition has an average linear expansion coefficient β at 20 to 200°C of 1.50 to 5.00 ppm / °C, and the glass composition is used in a laminate member having a Si-SiC member having an average linear expansion coefficient α at 20 to 200°C of 2.85 to 4.00 ppm / °C, and is used so that the absolute value |α-β| of the value obtained by subtracting the average linear expansion coefficient β of the glass member at 20 to 200°C from the average linear expansion coefficient α of the Si-SiC member at 20 to 200°C is 2.00 ppm / °C or less.
[0224] Another embodiment of the glass composition of the present disclosure is a glass composition having, in terms of mole percentage based on oxides, 55.0 to 85.0 mol% of SiO 2 and 1.5 to 22.0 mol% Al 2 O 3 and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol% P 2 O 5 and the SiO 2 , the above Al 2 O 3 , above B 2 O 3 and the above P 2 O 5 The total content, expressed as a mole percentage based on oxides, is 70.0 to 97.0%, the average linear expansion coefficient β at 20 to 200°C is 1.50 to 5.00 ppm / °C, and the linear transmittance at a wavelength of 850 nm is 80% or more.
[0225] The glass composition is preferably used as a glass member constituting the above-mentioned laminated member. By using the glass composition as the glass member constituting the above-mentioned laminated member, the laminated member has excellent temperature rise properties, impact resistance, and thermal shock resistance.
[0226] The glass composition and each physical property value of the glass composition are the same as those of the glass member of the laminated member of the present disclosure. The linear transmittance of the glass composition at a wavelength of 850 nm means a value measured when the glass composition is used as a glass member. In addition, in a laminated member having a glass member obtained using the above glass composition, the above description regarding the glass member of the laminated member also applies to the bonding layer and Si-SiC member that constitute the laminated member. EXAMPLES
[0227] Hereinafter, one embodiment of the present invention will be described with reference to examples, but the embodiment of the present invention is not limited to these.
[0228] [Glass components] The glasses prepared are shown in Tables 1 and 2.
[0229] [Table 1]
[0230] [Table 2]
[0231] [Glass preparation procedure] The glasses (iA) to (v) and (vii) to (xxix) in Tables 1 and 2 were prepared as follows so as to have the glass compositions shown in Tables 1 and 2 in terms of oxide-based mole percentages. Note that blanks in Tables 1 and 2 mean that the corresponding component was not contained. First, commonly used glass raw materials such as oxides, hydroxides, carbonates, sulfates, halides, or nitrates were appropriately selected and weighed to make 10,000 g of glass. Next, the mixed raw materials were placed in a platinum crucible and put into a resistance heating electric furnace at 1500 to 1700 ° C., where they were melted for about 12 hours, degassed, and homogenized. The resulting molten glass was poured into a mold material and held at a temperature of glass transition point + 50 ° C. for 1 hour, and then cooled to room temperature at a rate of 0.5 ° C. / min to obtain a glass block.
[0232] The glass (vi) in Table 1 was synthetic quartz glass (product name: AQ) manufactured by AGC Inc.
[0233] Each of the obtained glass blocks was cut, ground and polished to obtain a glass member (length 300 mm, width 300 mm).
[0234] [Physical properties of glass components] The following measurements were carried out on the obtained glass member. The measurement results are shown in Tables 1 and 2.
[0235] The thickness was measured at 20° C. using a digital tape measure.
[0236] The average linear expansion coefficient β was measured using a high-precision thermal dilatometer "DIL402 Expedis" manufactured by Netzsch in the temperature range of 20° C. to 200° C. Note that the glass of (xi) in Table 1 was cloudy due to phase separation and was obviously unable to be used as a glass member, so the average linear expansion coefficient β was not measured.
[0237] The in-line transmittance was measured using a spectrophotometer at 20° C. and a wavelength of 850 nm. The glass of (xi) in Table 1 was cloudy due to phase separation, and it was clear that the linear transmittance was less than 80%, so the linear transmittance was not measured.
[0238] The Young's modulus was measured at 20° C. by the ultrasonic pulse method described in the Japanese Industrial Standards (JIS R1602:1995). Since the glass of (xi) in Table 1 was cloudy due to phase separation and was obviously not usable as a glass member, the Young's modulus was not measured.
[0239] The dissolution temperature (T2) was measured using a rotational viscometer and 2 The temperature T2 (℃) at which the viscosity becomes dPa·s is indicated. The melting temperatures (T2) of glasses (iv) and (v) in Table 1 could not be measured, so were calculated by extrapolation. Glass (vi) could not be measured with a rotational viscometer because its viscosity was too high.
[0240] The devitrification temperature is the maximum temperature (℃) at which no crystals precipitate on the surface or inside of the glass when observed under an optical microscope after heat treatment for 17 hours in an electric furnace controlled at a constant temperature. Note that the glass (xi) in Table 1 was cloudy due to phase separation and was obviously unusable as a glass component, so the devitrification temperature was not measured.
[0241] The density was measured by the Archimedes method.
[0242] Phase separation was evaluated by observing the glass members with a SEM (scanning electron microscope). When no phase separation was observed, it was marked as "◯", and when phase separation was observed, it was marked as "×".
[0243] [Si-SiC components] The fabricated Si-SiC components are shown in Table 3.
[0244] [Table 3]
[0245] [Si-SiC component manufacturing procedure] The Si-SiC members (a-1) to (a-3) were fabricated as follows. The α-SiC powder A1 was classified using a 325 mesh sieve to obtain α-SiC powder A2 (maximum particle size 44 μm, average particle size 8 μm). The α-SiC powder A2 was washed with mixed acid (hydrofluoric acid:nitric acid = 2:1 (mass ratio)) and pure water to obtain α-SiC powder A3 (iron content 2.1 mass ppm). The α-SiC powder A3, pure water, and acrylic resin emulsion (binder) were mixed to obtain a slurry (solid concentration about 75 mass%).
[0246] Next, the slurry was poured into a plaster mold to obtain a green body (size: 320 mm × 320 mm × 16 mm). The obtained green body was dried at 50 ° C for 14 days, and then fired at 1900 ° C in an electric furnace with an inert argon atmosphere to obtain a sintered body. The porosity of the sintered body was 18.2%. Next, the sintered body A1 was transferred to another electric furnace, and high-purity silicon was molten and infiltrated into the sintered body A1 under the condition of 1500°C in a vacuum to obtain a Si-SiC member in which all pores were filled with high-purity silicon. The iron content in the Si-SiC member was 2.2 ppm.
[0247] Next, the Si-SiC members were machined to have a length of 30 cm, a width of 30 cm, and a thickness shown in Table 3, to obtain Si-SiC members (a-1) to (a-3).
[0248] The Si-SiC member (b) was produced in the same manner as the Si-SiC member (a-1), except that the solids concentration of the slurry was changed to about 79 mass %.
[0249] The Si-SiC member (c) was produced in the same manner as the Si-SiC member (a-1), except that the solid content of the slurry was changed to about 61 mass %.
[0250] The Si-SiC member (d) was fabricated as follows. A kneader (manufactured by Miyazaki Iron Works Co., Ltd., model number: MP100) was charged with 48.2 mass% SiC powder (manufactured by Pacific Random Co., Ltd., model number: GMF-12S (average particle size 0.7 μm)), 25.0 mass% silicon powder (manufactured by Yamaishi Metals Co., Ltd., model number: No. 700 (average particle size 2.5 μm)), 5.5 mass% Metolose (manufactured by Shin-Etsu Chemical Co., Ltd., model number SM8000) as a binder, and 21.5 mass% pure water, and the mixture was kneaded for 6 hours to obtain a clay body.
[0251] The obtained clay was put into an extrusion molding machine (manufactured by Miyazaki Iron Works Co., Ltd., model number: FM100) and extrusion molded under conditions of head pressure of 1.0 MPa and discharge rate of 1200 g / min to obtain a molded body. The obtained molded body was dried at 50°C for 14 days, and then heated in an air atmosphere at 450°C for 3 hours to be degreased, thereby obtaining a degreased body. The obtained degreased body was heated in a carbon sintering furnace for 10 -3 The mixture was sintered at 1700°C for 2 hours in a vacuum atmosphere of 100 Pa to obtain a sintered body. The obtained sintered body was impregnated with Si at 1500°C in an argon atmosphere to obtain a Si-SiC member. The obtained Si-SiC member was processed to have a length of 30 cm, a width of 30 cm, and a thickness shown in Table 3 to obtain a Si-SiC member (d).
[0252] The Si-SiC member (e) was produced in the same manner as the Si-SiC member (a-1), except that the solid content of the slurry was changed to about 77 mass %.
[0253] The Si-SiC member (f) was produced in the same manner as the Si-SiC member (a-1), except that the solid content of the slurry was changed to about 58 mass %.
[0254] [Physical properties of Si-SiC components] The following measurements were carried out on the obtained Si-SiC members (a-1) to (f). The measurement results are shown in Table 3.
[0255] The amount (composition) of each component of the Si-SiC member was measured by an inductively coupled plasma mass spectrometer ICP-MS (manufactured by Shimadzu Corporation).
[0256] The thickness was measured at 20°C using a vernier caliper (AD-5764A) manufactured by A&D Co., Ltd.
[0257] The average linear expansion coefficient α was measured in the temperature range of 20°C to 200°C using a Bruker AXS differential thermal expansion meter (TMA) "TMA4000SA."
[0258] The thermal conductivity was measured at a temperature of 20°C using a laser flash method thermal property measuring device "MODEL LFA-502" manufactured by Kyoto Electronics Manufacturing Co., Ltd.
[0259] The Young's modulus was measured at 20°C using an Autocom universal testing machine "AC-300KN" manufactured by TSE Corporation, according to the elastic modulus test method (dynamic elastic modulus method) described in the Japanese Industrial Standards (JIS R1602:1995).
[0260] The bending strength was measured at 20°C using an Autocom universal testing machine "AC-300KN" manufactured by TSE Corporation, according to the bending strength test method (four-point bending strength) described in the Japanese Industrial Standards (JIS R1601:2008).
[0261] The Vickers hardness was measured at 20° C. using a Vickers hardness tester system (manufactured by Nippon Steel & Sumikin Technology Co., Ltd.) by pressing with a pressing load of 10 kgf for 15 seconds.
[0262] [Joining layer] The following measurements were carried out for each resin (resin film, coating-type adhesive) shown in Table 4. The measurement results are shown in Table 4. In Table 4, the fluororesin used was manufactured by AGC Inc. and had the product name EA-2000 (resin film), the epoxy resin used was manufactured by ThreeBond Co., Ltd. and had the product name TB2237J (spray-on adhesive), and the polyimide resin used was manufactured by Kawamura Sangyo Co., Ltd. and had the product name KPI-MX300F (resin film). Since epoxy resin is a coating type adhesive, the following measurements were carried out after it was molded into a sheet.
[0263] [Table 4]
[0264] The thickness was measured with a digital tape measure.
[0265] The in-line transmittance was measured using a spectrophotometer at 20° C. and a wavelength of 850 nm.
[0266] The heat resistance temperature was determined by thermogravimetry (TGA) in an air atmosphere, and was defined as the temperature at which the mass of the resin film or coating-type adhesive decreased by 1% by mass.
[0267] The average linear expansion coefficient γ was measured in the temperature range of 20°C to 200°C using a Bruker AXS differential thermal expansion meter (TMA) "TMA4000SA." The average linear expansion coefficient γ of the resin film or coating type adhesive and the average linear expansion coefficient γ of a bonding layer (described below) obtained using the resin film or coating type adhesive were the same value.
[0268] The Young's modulus was measured at 25° C. using a universal testing machine (model 5966) manufactured by Instron Corporation according to the elastic modulus test method described in the Japanese Industrial Standards (JIS K7171).
[0269] [Laminated member] The produced laminated members are shown in Tables 5 to 7.
[0270] [Table 5]
[0271] [Table 6]
[0272] [Table 7]
[0273] [Preparation procedure] Samples (laminate members) of Examples 1 to 14 and 18 to 43 were produced as follows so that the respective members were combined as shown in Tables 5 to 7. Samples of Examples 15 to 17 were also prepared. Examples 1 to 5, 7, 9 to 13, 20 to 24, and 26 to 43 are working examples, and Examples 6, 8, 14 to 19, and 25 are comparative examples.
[0274] First, the surfaces of the glass members shown in Tables 1 and 2 that come into contact with the resin (bonding layer) were processed to a surface roughness of Ra = 0.2 μm using SiC abrasive paper. Similarly, the surfaces of the Si-SiC members shown in Table 3 that come into contact with the resin (bonding layer) were processed to a surface roughness of Ra = 0.2 μm using SiC abrasive paper. Next, the resin film shown in Table 4 was sandwiched between the glass member and the Si-SiC member, heated to a temperature of the softening point of the resin film +20 degrees, and pressed for 5 minutes with a pressure of 2 MPa to bond the glass member and the Si-SiC member via a bonding layer. Alternatively, the adhesive of the coating type shown in Table 4 was applied to the glass member with a thickness of 0.080 mm using a dispenser ND type made by Hyojinja, and the Si-SiC member was laminated on top of it, and the glass member and the Si-SiC member were bonded via a bonding layer by pressing with a pressure of 1.0 MPa and heating and curing at 120 ° C for 4 hours. In this way, samples (laminate members) of Examples 1 to 14 and 18 to 43 were obtained.
[0275] [Evaluation of laminated members] The samples of each example were evaluated as follows, and the evaluation results are shown in Tables 5 to 7 above.
[0276] (Temperature rise evaluation) The samples of each example were irradiated with infrared rays (850 nm) for 2 minutes using nine 2 kW infrared lamps, and the temperature rise was evaluated. The evaluation criteria were as follows: ◯ when the temperature of the outermost surface of the sample exceeded 200°C; × when the temperature of the outermost surface of the sample did not exceed 200°C. The laminated member samples of Examples 1 to 14 and 18 to 43 were irradiated with infrared rays from the glass member side and evaluated based on the outermost surface temperature of the Si-SiC member side. The laminated member samples of Examples 15 to 17 were evaluated based on the outermost surface temperature of the side opposite to the infrared ray irradiated side.
[0277] (Impact resistance evaluation) A 533g steel ball was dropped onto each sample to evaluate impact resistance. Impact resistance evaluation was performed on three samples (n=3) for each example. A support frame made of rubber plate with a thickness of 3 mm, width of 15 mm, and hardness of A50 was provided on the outer periphery of the sample, and the sample was clamped and fixed from above and below. The steel ball was dropped so that it was within a distance of 25 mm from the center of the sample. The evaluation criteria were as follows: if two or more of the three samples broke, it was marked as "X", if one of the three samples broke, it was marked as "△", and if none of the three samples broke, it was marked as "O", with any score of "△" or above being considered a pass. The steel ball was dropped from the Si-SiC member side of the laminated member samples of Examples 1 to 14 and 18 to 43. Note that the impact resistance of Samples 17 and 25 was not evaluated.
[0278] (Heat resistance evaluation) The samples of each example were heated at a temperature of 230°C for 24 hours, and visually evaluated for changes in appearance. The evaluation criteria were ◯ if there was no change in appearance (discoloration, bubbles, generation of foreign matter, bleeding of the bonding layer, etc.), and × if there was a change in appearance. The sample of Example 25 was not evaluated for heat resistance.
[0279] (Warpage) The amount of warping of the samples in each example was measured by measuring the three-dimensional characteristics of the sample surface in accordance with ISO25178-605 using a non-contact three-dimensional shape measuring device "NH-5Ns" manufactured by Mitaka Koki Co., Ltd., and determining the maximum inclined flatness of the sample surface. Specifically, the sample was placed on a precision surface plate, and the height of each point on the top surface of the sample was measured using a laser autofocus microscope. The amount of warping was calculated as the value of the gap created when the top surface of the sample was sandwiched between two parallel flat surfaces, i.e., the maximum inclined flatness.
[0280] (density) The mass of each sample was calculated by dividing it by the volume measured using a digital measure manufactured by Digi-Tech Corporation.
[0281] (area) The area of the top surface of each sample (the exposed main surface of the Si-SiC component in the case of a laminated component, or one of the main surfaces in the case of a single component) was determined from the dimensions measured using a digital tape measure manufactured by DigiTech Corporation.
[0282] (Bonding layer thickness) The thickness of the bonding layer (resin) of each of the samples of Examples 1 to 14 and 18 to 43 was calculated by observing the cross section with an SEM.
[0283] (Thermal shock resistance evaluation) A laminated member with a width of 15 mm and a length of 100 mm was prepared using the same combination as the samples of Examples 1 to 14 and 18 to 43, and the Si-SiC member side was heated using a hot plate to create a temperature difference between the glass and the laminated member, and the thermal shock resistance was evaluated. Specifically, the surface of the Si-SiC member was heated using a hot plate set at 220°C, and the glass member side was cooled using a cooling plate cooled to 10°C by running cooling water through it, and the temperature difference was maintained for 1 hour. The evaluation criteria were as follows: when cracks or cloudiness were found in the adhesive layer by visual inspection, it was marked X, and when no change was found, it was marked O. Note that the samples of Examples 15 to 17 and Example 25 were not evaluated for thermal shock resistance.
[0284] The results in Tables 5 to 7 show that the laminated members of the present invention have a fast temperature rise rate, high impact resistance and high thermal shock resistance, and are suitable as heating members (Examples 1 to 5, 7, 9 to 13, 20 to 24, and 26 to 43).
[0285] On the other hand, the laminate member of Example 6 had a low average linear expansion coefficient α of less than 2.85 ppm / °C at 20 to 200°C for the Si-SiC member, and thus had low thermal shock resistance. In the laminate member of Example 8, the average linear expansion coefficient α of the Si-SiC member at 20 to 200° C. was low at less than 2.85 ppm / ° C., and the impact resistance and thermal shock resistance were low. The laminated member of Example 14 had a fast temperature rise rate and high impact resistance and thermal shock resistance, but the amount of warping was large. The samples of Examples 15 to 17 had low temperature rise rates or low impact resistance. In the laminate members of Examples 18 and 19, the average linear expansion coefficient α of the Si-SiC members at 20 to 200° C. was low at less than 2.85 ppm / ° C., and the thermal shock resistance was low. The laminated member of Example 23 had low impact resistance and a large amount of warping. The laminate of Example 25 had a slow temperature rise rate.
[0286] Although various embodiments have been described above with reference to the drawings, it goes without saying that the present invention is not limited to such examples. It is clear that a person skilled in the art can come up with various modified or revised examples within the scope of the claims, and it is understood that these also naturally belong to the technical scope of the present invention. Furthermore, the components in the above-mentioned embodiments may be arbitrarily combined within the scope of the invention.
[0287] This application is based on a Japanese patent application (Patent Application No. 2021-007287) filed on January 20, 2021, the contents of which are incorporated by reference into this application. [Explanation of symbols]
[0288] 100 Laminated material 101 Glass materials 103 Bonding layer 105 Si-SiC components
Claims
1. A glass member having an in-line transmittance of 80% or more at a wavelength of 850 nm; a bonding layer including a resin on the glass member; A laminated member having a Si-SiC member on the bonding layer, The glass member has a SiO content of 55.0 to 85.0 mol % in terms of oxide-based mole percentage. 2 and 1.5 to 22.0 mol% Al 2 O 3 and 2.0 to 14.0 mol% B 2 O 3 and 0 to 5.0 mol % P 2 O 5 and The SiO 2 , the Al 2 O 3 , the B 2 O 3 and the P 2 O 5 The total content of is 70.0 to 97.0%, expressed as a mole percentage based on oxides, The Si-SiC member has an average linear expansion coefficient α of 2.85 to 4.00 ppm / °C at 20 to 200°C, The average linear expansion coefficient β of the glass member at 20 to 200° C. is 1.50 to 5.00 ppm / ° C.; The laminated member has an absolute value |α-β| obtained by subtracting the average linear expansion coefficient β of the glass member at 20 to 200° C. from the average linear expansion coefficient α of the Si-SiC member at 20 to 200° C., which is 2.00 ppm / ° C. or less.
2. The glass member has a SiO content of 60.0 to 78.0 mol % in terms of oxide-based mole percentage. 2 and 8.0 to 18.0 mol % Al 2 O 3 and 2.0 to 11.0 mol% B 2 O 3 and 0 to 3.0 mol % P 2 O 5 and The SiO 2 , the Al 2 O 3 , the B 2 O 3 and the P 2 O 5 The laminate member according to claim 1, wherein the total content of is 80.0 to 90.0% in terms of mole percentage based on oxides.
3. the total content of RO and ZnO in the glass member is 2.0 to 25.0%, expressed in mole percentage on an oxide basis; R in the glass member 2 The laminated member according to claim 1 or 2, wherein the total content of O is 0 to 15.0%, expressed as a mole percentage based on oxides.
4. The laminated member according to any one of claims 1 to 3, wherein the glass member has an average linear expansion coefficient β of 2.00 to 3.50 ppm / °C, a Young's modulus of 40 to 120 GPa, and a melting temperature of 1000 to 2000°C.
5. The B contained in the glass member 2 O 3 The laminate member according to any one of claims 1 to 4, wherein the content of is 8.5 mol% or less.
6. The glass member contains 0 to 13.0 mol % Na, expressed in terms of mole percentage based on oxide. 2 The laminated member according to any one of claims 1 to 5, comprising O.
7. The glass member has an oxide-based mole percentage of 0.0001 to 0.0115 mol % of Fe. 2 O 3 The laminated member according to any one of claims 1 to 6, comprising:
8. The laminate member according to any one of claims 1 to 7, wherein the glass member has an in-line transmittance of 90% or more at a wavelength of 850 nm.
9. The glass member has a thickness of 2 to 40 mm; The laminated member according to any one of claims 1 to 8, wherein the Si-SiC member has a thickness of 0.5 to 15 mm.
10. The laminated member according to any one of claims 1 to 9, wherein the Si-SiC member has a thermal conductivity of 130 to 300 W / m · K at 20 ° C.
11. A laminated member described in any one of claims 1 to 10, wherein the average linear expansion coefficient β of the glass member at 20 to 200°C is smaller than the average linear expansion coefficient α of the Si-SiC member at 20 to 200°C.
12. The laminated member according to any one of claims 1 to 11, wherein the Si-SiC member has a Young's modulus of 300 to 420 GPa.
13. The laminated member according to any one of claims 1 to 12, wherein the Si-SiC member has a metal Si content of 8 to 60 mass%.
14. The laminated member according to any one of claims 1 to 13, wherein the resin has a heat resistance temperature of 120 to 420°C.
15. The laminated member according to any one of claims 1 to 14, wherein the bonding layer has an average linear expansion coefficient γ at 20 to 200 ° C. of 2 to 200 ppm / ° C.
16. Density: 2.40 to 2.85 g / cm 3 The laminated member according to any one of claims 1 to 15.
17. The laminated member according to any one of claims 1 to 16, wherein the amount of warping is 0.25 mm or less.
18. a second bonding layer provided on the Si-SiC member; The laminated member according to any one of claims 1 to 17, further comprising a second Si-SiC member joined to the Si-SiC member via the second bonding layer.
Citation Information
Patent Citations
Metal-ceramic structure having pyrogenetic reaction filter layer in the middle
JP1991088783A
Component made of quartz glass with coating film
JP1996083835A
Low temperature test device
JP1997298225A
Wafer chuck and method of forming wafer chuck
JP2008199006A
Crystallized glass
JP2012148958A