Curable composition, cured product and laminated body
A curable composition with specific particle sizes and organic polymers forms a hard coat layer that addresses transparency and refractive index control issues, providing stable and scratch-resistant laminates for thermoplastic resin films.
Patent Information
- Application Number
- JP2023070667
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-11-09
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2036-02-12
AI Technical Summary
Existing hard coating technologies for thermoplastic resin films face issues with transparency, stability, and control of refractive index due to particle size and shape variations, leading to inadequate anti-blocking properties and limited freedom in coating conditions.
A curable composition containing ethylenically unsaturated compounds and particles with specific particle sizes and distributions, along with organic polymer compounds, to form a hard coat layer that provides excellent anti-blocking, transparency, and controlled refractive index.
The composition achieves stable, transparent, and scratch-resistant laminates with adjustable refractive index, suitable for various coating conditions and applications.
Smart Images

Figure 0007589764000001 
Figure 0007589764000002 
Figure 0007589764000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition, and a cured product and a laminate obtained by using the curable composition. More specifically, the present invention relates to a curable composition that has excellent storage stability, has a high degree of freedom in coating conditions, can obtain a cured product under various coating conditions, can obtain a laminate excellent in antiblocking property, transparency, recoatability, scratch resistance, curl resistance, etc., and can easily control the refractive index of the obtained cured product, a cured product and a laminate of the curable composition, and a hard coat film. [Background technology]
[0002] A hard coating having excellent hardness and slipperiness may be applied to the surface of a thermoplastic resin film, such as a polyethylene terephthalate (PET) film. Films with such hard coating may be wound into a roll during storage for the purpose of securing storage space, ease of handling during molding, prevention of dirt, etc. Thus, when a hard-coated film is wound into a roll, it is required to prevent blocking between the films.
[0003] As a method for preventing blocking of a film, a method is disclosed in which a hard coat layer is formed on the film surface, and organic fine particles having a specific particle size and a dispersant are blended into the hard coat layer to form irregularities on the surface of the hard coat layer (Patent Document 1). Also, a method is disclosed in which a hard coat layer is formed on the film surface, and a large amount of reactive fine particles are blended into the hard coat layer to form irregularities on the surface of the hard coat layer to prevent blocking (Patent Document 2). Also, a method is disclosed in which a resin composition for forming a hard coat layer is applied to a substrate, and then precipitated by phase separation in a drying process and an ultraviolet (UV) irradiation process to form irregularities on the surface of the hard coat layer to prevent blocking (Patent Document 3). Furthermore, a method is disclosed in which large irregularities are formed on the surface of the hard coat layer by using a material consisting of a polyfunctional polymerizable unsaturated compound, a radical polymerization initiator, monodispersed inorganic particles, a particle flocculant, etc. as a hard coat layer to be applied to the surface of the film (Patent Document 4). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 2013-75955 [Patent Document 2] Japanese Patent Application Publication No. 2014-16608 [Patent Document 3] Japanese Patent Application Publication No. 2013-209516 [Patent Document 4] Japanese Patent Publication No. 2011-29175 Summary of the Invention [Problem to be solved by the invention]
[0005] Through detailed studies by the present inventors, it has been found that the techniques disclosed in the above Patent Documents 1 to 4 have the following problems. In the technique disclosed in Patent Document 1, the particles mixed have an average primary particle diameter of 0.5 to 1.5 μm, which is large, and the internal haze increases, resulting in insufficient transparency. In the technique disclosed in Patent Document 2, the particles mixed are small, resulting in good transparency, but the technique contains a large amount of two types of particles with different shapes and reactive groups, resulting in poor storage stability. In the technique disclosed in Patent Document 3, particles such as inorganic particles are not essential, but the shape of the unevenness on the hard coat layer surface changes depending on the drying conditions and UV irradiation conditions, resulting in low freedom in coating conditions. In the technique disclosed in Patent Document 4, the particle diameter of the aggregated particles is large, resulting in low transparency of the coating film.
[0006] Furthermore, various materials are usually laminated before and after the hard coat layer that requires anti-blocking properties. In this case, it is important for various optical applications to adjust the refractive index between each layer. For this reason, it is required to control the refractive index of the hard coat layer over a wide range without impairing the anti-blocking properties and transparency.
[0007] The present invention aims to solve such problems of the conventional techniques. That is, the present invention aims to provide a curable composition which has excellent storage stability, has a high degree of freedom in coating conditions, is capable of obtaining a cured product under various coating conditions, gives a laminate excellent in anti-blocking properties, transparency, recoating properties, scratch resistance, curl resistance, etc., and allows easy control of the refractive index of the obtained cured product. [Means for solving the problem]
[0008] As a result of intensive research by the present inventors in consideration of the above problems, it has been found that the above problems can be solved by a curable composition containing an ethylenically unsaturated compound and particles having a specific particle size, and the blending amounts of these are within a specific range. That is, the gist of the present invention is as follows: [1] to
[17] .
[0009] [1] A curable composition comprising the following components (A) and (B), in which the amount of component (B) is 0.01 to 150 parts by weight per 100 parts by weight of component (A): Component (A): A compound having an ethylenically unsaturated bond Component (B): A group of particles having an average primary particle size of 1 to 100 nm and a d90 of 100 to 2,000 nm as measured by a laser diffraction particle size distribution analyzer.
[0010] [2] The curable composition according to [1], wherein the value of [average primary particle size] / [d90] of component (B) is 0.01 to 0.40. [3] The curable composition according to [1] or [2], wherein component (B) has a d10 of 10 to 500 nm and a d50 of 30 to 1,000 nm, as measured by a laser diffraction particle size distribution analyzer. [4] The curable composition according to any one of [1] to [3], wherein the weight-average molecular weight of component (A) is less than 2,100, and the composition contains the following component (C) in an amount of 0.01 to 20 parts by weight per 100 parts by weight of component (A): Component (C): An organic polymer compound having a weight average molecular weight (Mw) of 2,100 to 200,000 [5] The curable composition according to [4], wherein the solubility parameter (SP value) of component (C) is 9.3 to 12.6.
[0011] [6] The curable composition according to [4] or [5], comprising a (meth)acrylic resin as component (C). [7] The curable composition according to any one of [1] to [6], comprising a polyfunctional (meth)acrylate as component (A). [8] The curable composition according to [7], wherein the polyfunctional (meth)acrylate comprises at least one selected from the group consisting of polyfunctional (meth)acrylates having a nitrogen atom-containing heterocyclic structure, polyfunctional (meth)acrylates having a dendrimer structure, and polyfunctional (meth)acrylates having a hyperbranched polymer structure, and the total content of the polyfunctional (meth)acrylates is 1 to 65% by weight based on the total weight of component (A).
[0012] [9] The curable composition according to any one of [1] to [8], which contains an organic solvent and has a solid content concentration of 5 to 95% by weight.
[10] The curable composition according to [9], wherein the organic solvent is at least one selected from the group consisting of saturated hydrocarbon solvents, ester solvents, ether solvents, alcohol solvents and ketone solvents.
[11] The curable composition according to any one of [1] to
[10] , which contains a polymerization initiator and has a content of 0.01 to 20 parts by weight relative to 100 parts by weight of component (A).
[0013]
[12] A cured product obtained by irradiating the curable composition according to any one of [1] to
[11] with active energy rays.
[13] A laminate having a substrate and a hard coat layer, the hard coat layer being a layer formed by applying a curable composition according to any one of claims [1] to
[10] onto the substrate and irradiating the applied composition with active energy rays.
[14] The laminate according to
[13] , wherein the substrate is a plastic substrate.
[0014]
[15] The laminate according to
[14] , wherein the plastic substrate is at least one selected from the group consisting of polycarbonate resin, polyethylene terephthalate resin, and polymethyl methacrylate resin.
[16] A laminate having a substrate layer and a hard coat layer, the hard coat layer containing the following component (B) and having a haze value measured in accordance with JIS K7136 (2000) of less than 0.6%: Component (B): A group of particles having an average primary particle size of 1 to 100 nm and a d90 of 100 to 2,000 nm as measured by a laser diffraction particle size distribution analyzer.
[17] A hard coat film comprising the following component (B), the content of which is 0.01 to 55% by weight based on the entire hard coat film: Component (B): A group of particles having an average primary particle size of 1 to 100 nm and a d90 of 100 to 2,000 nm as measured by a laser diffraction particle size distribution analyzer. Effect of the Invention
[0015] According to the present invention, there is provided a curable composition which has excellent storage stability, has a high degree of freedom in coating conditions, can produce a cured product under various coating conditions, can produce a laminate excellent in antiblocking property, transparency, recoatability, scratch resistance, curl resistance, etc., and can easily control the refractive index of the obtained cured product. Furthermore, according to the present invention, there are provided a cured product and a laminate, as well as a hard coat film, obtained by using this curable composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The following description is an example of an embodiment of the present invention, and the present invention is not limited to the following description as long as it does not deviate from the gist of the present invention. In this specification, when the expression "~" is used, it is used as an expression including the numerical value or physical property value before and after it. In this invention, when the expression "(meth)acrylate" is used, it means one or both of "acrylate" and "methacrylate", and the same applies to the use of expressions such as "(meth)acryloyl" and "(meth)acrylic".
[0017] The curable composition of the present invention contains the following components (A) and (B), and contains 0.01 to 150 parts by weight of component (B) per 100 parts by weight of component (A). Component (A): A compound having an ethylenically unsaturated bond Component (B): A group of particles having an average primary particle size of 1 to 100 nm and a d90 of 100 to 2,000 nm as measured by a laser diffraction particle size distribution analyzer.
[0018] [Component (A)] The component (A) used in the present invention is a compound having an ethylenically unsaturated bond. The curable composition of the present invention is provided with curability and scratch resistance by containing the component (A).
[0019] The type of ethylenically unsaturated bond contained in the compound of component (A) is not particularly limited, and examples thereof include a (meth)acryloyl group, a (meth)acrylamide group, a styryl group, and an allyl group. Of these, it is preferable that component (A) contains a compound having a (meth)acryloyl group. In component (A), the number of ethylenically unsaturated bonds in one molecule is not particularly limited, and is usually 1 to 15. Two or more compounds having different numbers of ethylenically unsaturated bonds may be mixed and used as the compound of component (A).
[0020] Among the components (A), the compound having a (meth)acryloyl group includes a monofunctional (meth)acrylate having one (meth)acryloyl group and a polyfunctional (meth)acrylate having two or more (meth)acryloyl groups. These may be used alone or in combination of two or more, but it is preferable to include a polyfunctional (meth)acrylate.
[0021] Examples of monofunctional (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, (meth)acryloylmorpholine, tetrahydrofurfuryl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, isodeoxy (meth)acrylate, and the like. Sil (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide modified phenoxy (meth)acrylate, propylene oxide modified phenoxy (Meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl chiral hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate,Examples of the mono(meth)acrylate include adamantane derivative mono(meth)acrylates such as adamantyl(meth)acrylate having a monovalent mono(meth)acrylate derived from 2-adamantane and adamantanediol. These may be used alone or in combination of two or more.
[0022] Examples of the polyfunctional (meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, poly ... Bifunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate; trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate; acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate , ditrimethylolpropane hexa(meth)acrylate, and other polyfunctional (meth)acrylates having three or more functional groups; modified products of polyfunctional (meth)acrylate compounds in which part of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone; polyfunctional (meth)acrylates having a nitrogen atom-containing heterocyclic structure, such as polyfunctional (meth)acrylates having an isocyanurate structure; polyfunctional (meth)acrylates having a dendrimer structure, polyfunctional (meth)acrylates having a hyperbranched dendritic structure, such as polyfunctional (meth)acrylates having a hyperbranched polymer structure;Examples of such urethane (meth)acrylates include urethane (meth)acrylates in which a (meth)acrylate having a hydroxyl group is added to a diisocyanate or triisocyanate, and urethane (meth)acrylates in which a (meth)acrylate having a hydroxyl group is added to a reaction product having an isocyanate group at the end obtained by reacting an isocyanate compound with a diol compound. These may be used alone or in combination of two or more.
[0023] Among the polyfunctional (meth)acrylates that can be used as component (A), it is preferable to include at least one of a polyfunctional (meth)acrylate having a nitrogen atom-containing heterocyclic structure and a polyfunctional (meth)acrylate having a multi-branched dendritic structure. From the viewpoint of hardness, the polyfunctional (meth)acrylate having a nitrogen atom-containing heterocyclic structure and the polyfunctional (meth)acrylate having a multi-branched dendritic structure are preferably contained in a total amount of 65% by weight or less, more preferably 50% by weight or less, even more preferably 35% by weight or less, particularly preferably 20% by weight or less, and most preferably 10% by weight or less, based on the entire component (A). On the other hand, from the viewpoint of improving curl resistance, the total amount of these is preferably contained in a total amount of 1% by weight or more, more preferably 3% by weight or more, and even more preferably 5% by weight or more, based on the entire component (A).
[0024] The polyfunctional (meth)acrylate having a nitrogen atom-containing heterocyclic structure is preferably one in which a (meth)acryloyl group is linked to the nitrogen atom-containing heterocyclic structure directly or via a hydrocarbon group having 1 to 10 carbon atoms or an alkylene oxide structure having 1 to 10 carbon atoms, and specifically includes polyfunctional (meth)acrylates having an isocyanurate structure. Examples of such polyfunctional (meth)acrylates include isocyanuric acid ethylene oxide (EO) modified diacrylate (e.g., Aronix M-215, manufactured by Toagosei Co., Ltd.), ε-caprolactone modified tris(acryloxyethyl)isocyanurate (e.g., Aronix M-327, A-9300-1CL, manufactured by Toagosei Co., Ltd.), isocyanuric acid EO modified di- and triacrylate (e.g., Aronix M-313, Aronix M-315, A-9300, manufactured by Toagosei Co., Ltd.), and the like.
[0025] Examples of the polyfunctional (meth)acrylate having a multi-branched dendritic structure include polyfunctional (meth)acrylate having a dendrimer structure and polyfunctional (meth)acrylate having a hyperbranched polymer structure. The polyfunctional (meth)acrylate having a dendrimer structure is a compound having a structure branched with high regularity, and the polyfunctional (meth)acrylate having a hyperbranched polymer structure is a compound having a structure branched with low regularity, and has a low viscosity and excellent solvent solubility compared to linear polymers. Examples of the polyfunctional (meth)acrylate having a dendrimer structure include Viscoat #1000 manufactured by Osaka Organic Chemical Industry Co., Ltd. Examples of the polyfunctional (meth)acrylate having a hyperbranched polymer structure include STAR-501, SIRIUS-501, SUBARU-501, and the like manufactured by Osaka Organic Chemical Industry Co., Ltd.
[0026] From the viewpoint of improving the handling and coating properties of the curable composition, the component (A) preferably has a weight average molecular weight (Mw) of less than 2,100. From the viewpoint of improving this effect, the component (A) preferably has an Mw of 1,600 or less, more preferably 1,100 or less. On the other hand, a low molecular weight compound in a range where the molecular weight is not usually measured as a weight average molecular weight can also be used as the component (A) used in the present invention. In the component (A), the weight average molecular weight (molecular weight) of such a low molecular weight compound is usually 50 or more. The Mw of the component (A) can be measured by gel permeation chromatography (GPC) as shown in the examples below.
[0027] [Component (B)] The component (B) used in the present invention is a particle group having an average primary particle size of 1 to 100 nm and a d90 (particle size value at which the cumulative value is 90% in the results measured by a laser diffraction type particle size distribution analyzer) of 100 to 2,000 nm, measured by a laser diffraction type particle size distribution analyzer. Here, the fact that d90 is in a predetermined range different from the value of the average primary particle size indicates that the component (B) is in the form of an aggregate. That is, the component (B) is a particle having an average primary particle size in a specific range, which exists in a specific aggregated state. In the curable composition of the present invention, the component (B) mainly contributes to anti-blocking properties. It is presumed that the reason why the cured product and laminate obtained by using the curable composition of the present invention are particularly excellent in anti-blocking properties and transparency is that the component (B) has an average primary particle size in the above range but is in the form of a specific aggregate, and thus when the curable composition is cured, the component (B) forms unevenness on the surface to express anti-blocking properties, while allowing sufficient light transmission.
[0028] The content of component (B) is 0.01 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, even more preferably 2 parts by weight or more, and particularly preferably 3 parts by weight or more, relative to 100 parts by weight of component (A), from the viewpoint of antiblocking properties of the coating film. On the other hand, the content of component (B) is 150 parts by weight or less, preferably 130 parts by weight or less, more preferably 110 parts by weight or less, even more preferably 90 parts by weight or less, particularly preferably 70 parts by weight or less, and most preferably 45 parts by weight or less, relative to 100 parts by weight of component (A), from the viewpoint of transparency.
[0029] Component (B) has an average primary particle size of 1 to 100 nm, and a d90 measured by a laser analysis type particle size distribution analyzer of 100 to 2,000 nm, so that the antiblocking property and transparency are good. The average primary particle size of component (B) is 1 nm or more, preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and most preferably 30 nm or more, from the viewpoint of antiblocking property, while it is 100 nm or less, more preferably 75 nm or less, and even more preferably 50 nm or less, from the viewpoint of transparency. Moreover, d90 of component (B) is 100 nm or more, preferably 150 nm or more, more preferably 200 nm or more, even more preferably 250 nm or more, and particularly preferably 300 nm or more, from the viewpoint of antiblocking property, while it is 2,000 nm or less, preferably 1,500 nm or less, and more preferably 1,000 nm or less, from the viewpoint of transparency. In particular, from the viewpoint of controlling the refractive index when the curable composition is cured, d90 of component (B) is preferably 575 nm or less, more preferably 550 nm or less, even more preferably 525 nm or less, particularly preferably 500 nm or less, and most preferably 475 nm or less.
[0030] In addition, from the viewpoint of obtaining good antiblocking properties and transparency, it is preferable that the value of [average primary particle size] / [d90] of component (B) is 0.01 to 0.40. From this viewpoint, the value of [average primary particle size] / [d90] is more preferably 0.02 or more, more preferably 0.35 or less, even more preferably 0.30 or less, particularly preferably 0.25 or less, and most preferably 0.20 or less.
[0031] In addition, in the results measured by the laser analysis type particle size distribution meter, the particle size value (d10) at which the cumulative value becomes 10% and the particle size value (d50) at which the cumulative value becomes 50% are preferably in the following ranges from the viewpoint of achieving both antiblocking properties and transparency. That is, the d10 of component (B) is preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, particularly preferably 40 nm or more, and most preferably 50 nm or more, while it is preferably 500 nm or less, more preferably 300 nm or less, even more preferably 200 nm or less, and particularly preferably 150 nm or less. In addition, the d50 of component (B) is preferably 30 nm or more, more preferably 50 nm or more, even more preferably 70 nm or more, and particularly preferably 90 nm or more, while it is preferably 1,000 nm or less, more preferably 750 nm or less, and even more preferably 500 nm or less.
[0032] The average primary particle size of component (B) is a value measured using a scanning electron microscope or a transmission electron microscope, and when the primary particles of component (B) have a shape other than spherical, the average primary particle size is calculated as the average of the major axis diameter and the minor axis diameter. The particle size measured by a laser diffraction particle size distribution analyzer is specifically a value calculated using a Microtrack UPA (manufactured by Nikkiso Co., Ltd.).
[0033] The average primary particle size and d90 of component (B) may be within the above-mentioned ranges, and the particle size may be adjusted by crushing aggregated particles, by producing aggregated particles using a sol-gel method or the like, or by aggregating dispersed particles using an aggregating agent.
[0034] The type of component (B) is not particularly limited as long as the average primary particle size and d90 satisfy the above ranges, and it may be any of inorganic particles, organic particles, and organic-inorganic composite particles. Only one of these may be used, or two or more types may be used in combination. When the particles of component (B) are inorganic particles, the heat resistance and hardness tend to be high when made into a hard coat, and anti-blocking properties tend to be better, which is preferable.
[0035] Examples of inorganic particles include oxide particles such as silica, alumina, titania, zirconia, zeolite, mica, synthetic mica, calcium oxide, zirconium oxide, zinc oxide, magnesium fluoride, smectite, synthetic smectite, vermiculite, ITO (indium oxide / tin oxide), ATO (antimony oxide / tin oxide), tin oxide, indium oxide, antimony oxide, etc. Among these, at least one oxide particle selected from the group consisting of silica, alumina, titania, zirconia, zinc oxide, magnesium fluoride, ITO, tin oxide, and antimony oxide is preferred, and oxide particles containing at least silica are more preferred.
[0036] The oxide particles containing silica can be obtained as a commercial product. Examples of the commercial products include SIRMIBK15WT%-H58, SIRMIBK15WT%-M18, SIRMIBK15WT%-E83, SIRMIBK15WT%-M05, SIRMIBK15WT%-H84, SIRMIBK15WT%-H94, SIRMIBK15WT%-M36, SIRMIBK15WT%-M06, SIRMIBK15WT%-M44, SIRMIBK15WT%-M46, SIRMIBK15WT%-M42, SIRMIBK15WT%-M47, SIRMIBK15WT%-M61, and SIRMIBK15WT%-M62 from CIK Nanotech.
[0037] Specific examples of the organic particles include organic crosslinked polymer particles, such as (meth)acrylic crosslinked polymer particles, styrene crosslinked polymer particles, urethane crosslinked polymer particles, polyester crosslinked polymer particles, silicone crosslinked polymer particles, polyimide crosslinked polymer particles, and fluorine crosslinked polymer particles. In particular, acrylic crosslinked polymer particles are preferred, and specific examples thereof include (meth)acrylic crosslinked polymer particles obtained by polymerization methods such as suspension polymerization, emulsion polymerization, soap-free emulsion polymerization, mini-emulsion polymerization, dispersion polymerization, seed polymerization, etc., of (meth)acrylic monofunctional monomers such as methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate (herein, "(meth)acrylic monofunctional monomer" is a general term for (meth)acrylic acid monomers, (meth)acrylate monomers having one unsaturated double bond, and (meth)acrylamide monomers having one unsaturated double bond), and (meth)acrylic polyfunctional monomers such as trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, and ethylene glycol di(meth)acrylate (herein, "(meth)acrylic polyfunctional monomer" is a general term for (meth)acrylate monomers having two or more unsaturated double bonds, and (meth)acrylamide monomers having two or more unsaturated double bonds). The (meth)acrylic crosslinked particles may be styrene-(meth)acrylic crosslinked polymer particles obtained by further copolymerizing a styrene-based monofunctional monomer such as styrene or α-methylstyrene, or a styrene-based polyfunctional monomer such as divinylbenzene during polymerization.
[0038] Examples of organic-inorganic composite particles include particles having an organic polymer skeleton and a polysiloxane skeleton having an organosilicon in which a silicon atom is directly chemically bonded to at least one carbon atom in the skeleton, and particles in which a vinyl polymer is contained in the structure of polysiloxane particles having (meth)acryloxy groups.
[0039] As long as the average primary particle size and d90 of component (B) satisfy the above ranges, the shape of the aggregated state is not particularly limited, and may be any shape such as spherical, chain-like, needle-like, plate-like, scaly, crushed, bale-like, cocoon-like, or confetti-like. The shape of component (B) is preferably spherical or chain-like, and is particularly preferably spherical. When the shape of component (B) is spherical or chain-like, the uniformity of the antiblocking property of the obtained cured product surface is higher, and better antiblocking property tends to be obtained.
[0040] The curable composition of the present invention may contain, as component (B), only one type of the particles as described above, or may contain two or more types.
[0041] [Component (C)] From the viewpoint of further improving antiblocking properties and coating film appearance, the curable composition of the present invention preferably contains the following component (C). Component (C): An organic polymer compound having a weight average molecular weight (Mw) of 2,100 to 200,000
[0042] By having Mw of component (C) of 2,100 or more, it is possible to suppress bleeding out of component (C) from the surface of the cured product after curing the curable composition, and antiblocking properties also tend to be improved. From these viewpoints, Mw of component (C) is preferably 2,200 or more, more preferably 2,300 or more, and even more preferably 2,400 or more. On the other hand, by having Mw of component (C) of 200,000 or less, component (C) tends to segregate easily on the surface of the cured product when cured, and antiblocking properties tend to be better. From this viewpoint, Mw of component (C) is preferably 150,000 or less, more preferably 100,000 or less, even more preferably 70,000 or less, and particularly preferably 40,000 or less. The Mw of the organic polymer compound of component (C) can be measured by gel permeation chromatography (GPC) as shown in the examples below.
[0043] In the present invention, the component (C) preferably has a solubility parameter (SP value) of 9.3 to 12.6. When the SP value is 9.3 or more, the compatibility with other components tends to be good, and when the SP value is 12.6 or less, the slipperiness of the cured surface when the curable composition is cured tends to be good, and the antiblocking property tends to be better. From these viewpoints, the SP value is more preferably 9.4 or more, and even more preferably 9.5 or more, while it is more preferably 12.6 or less, even more preferably 12.0 or less, and particularly preferably 11.5 or less. The solubility parameter (SP value) is a solubility parameter. This SP value is a measure of solubility, and the larger the value, the higher the polarity, and conversely, the smaller the value, the lower the polarity. The solubility parameter (SP value) of the component (C) is a value calculated by the method proposed by Fedors et al. Specifically, the above can be determined by referring to "POLYMER ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol. 14, No. 2, ROBERT F. FEDORS. (pp. 147-154)".
[0044] In the present invention, it is preferable that the glass transition temperature (Tg) of component (C) is 35°C or less from the viewpoint of handleability because it can be handled in a liquid state. From this viewpoint, the glass transition temperature (Tg) is more preferably 25°C or less, further preferably 15°C or less, and particularly preferably 0°C or less. On the other hand, the lower limit of the glass transition temperature is not particularly limited, but is usually -125°C. The glass transition temperature of component (C) can be measured according to JIS K7121 "Method of measuring transition temperature of plastics", but as in the examples shown later, when it is in a liquid state at room temperature (23 to 25°C), it can also be visually confirmed that the glass transition temperature is below room temperature.
[0045] The component (C) may be a natural polymer compound or a synthetic polymer compound, as long as its Mw satisfies the above range. Examples of natural polymer compounds include regenerated cellulose polymer compounds such as cellophane and triacetyl cellulose. Examples of synthetic polymer compounds include addition polymerization polymer compounds such as polyolefin resins, vinyl chloride resins, vinyl acetate resins, (meth)acrylic resins, epoxy resins, and polyurethane resins; polycondensation polymer compounds such as amide resins, polycarbonate resins, polyester resins, alkyd resins, and polyimide resins; and addition condensation polymer compounds such as phenol resins, urea resins, and melamine resins. Among these, the component (C) is preferably a synthetic polymer compound, more preferably an addition polymerization polymer compound, and even more preferably a polyolefin resin or a (meth)acrylic resin. In particular, the (meth)acrylic resin is most preferable because it is easy to control the chemical structure due to the large number of options for the constituent monomers, and the SP value is easy to control within the above range. The organic polymer compounds listed above may be used alone or in combination of two or more.
[0046] In component (C), the (meth)acrylic resin is an organic polymeric compound obtained by polymerizing a (meth)acrylic monomer having a radically polymerizable double bond. The (meth)acrylic resin preferably has a hydrocarbon group in the side chain, and the number of carbon atoms in this hydrocarbon group is usually 1 to 24, but is preferably 2 or more, more preferably 4 or more, and is preferably 22 or less, more preferably 18 or less, even more preferably 12 or less, and particularly preferably 8 or less. Within the above range, the longer the carbon number of the alkyl group in the side chain of component (C), the more likely it is to segregate on the coating film surface when cured, and the more likely the antiblocking property is to be improved, and the shorter the chain, the more likely the surface hardness is to be improved. The hydrocarbon group in the side chain of the (meth)acrylic resin may be a straight-chain hydrocarbon group, a chain-chain hydrocarbon group, or a cyclic hydrocarbon group, but a chain-chain hydrocarbon group is preferable, and a straight-chain hydrocarbon group is particularly preferable. In the present invention, the hydrocarbon group in the side chain of the (meth)acrylic resin means a group bonded to the carbon atom of the main chain via at least an atom other than carbon.
[0047] Although the radical polymerizable monomer used as the raw material of the (meth)acrylic resin is not particularly limited, it is preferable to use a compound represented by the following formula (1) from the viewpoint of antiblocking properties. That is, the (meth)acrylic resin preferably contains a structural unit derived from the compound represented by the following formula (1). By using the compound represented by formula (1), it is possible to easily obtain a (meth)acrylic resin having a hydrocarbon group in the side chain, and it is also preferable because the polymerization of the (meth)acrylic resin is easy. CH2=C(R 1 )-C(O)-XR 2 (1) (R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R 2 represents an alkyl group having 1 to 24 carbon atoms which may have a hydroxyl group as a substituent, and X is -O- or -NH-. )
[0048] In the above formula (1), R 1 More preferably, R is a hydrogen atom or a methyl group. 2 R is more preferably a hydrocarbon group having 2 or more carbon atoms, and even more preferably a hydrocarbon group having 4 or more carbon atoms, while it is more preferably a hydrocarbon group having 22 or less carbon atoms, even more preferably a hydrocarbon group having 18 or less carbon atoms, particularly preferably a hydrocarbon group having 12 or less carbon atoms, and most preferably a hydrocarbon group having 8 or less carbon atoms. 2 Within the above range, the longer the carbon number of the hydrocarbon group, the easier it is to segregate on the coating surface, and the more anti-blocking properties tend to be improved, while the shorter the chain, the more the surface hardness tends to be improved. 2 The hydrocarbon group in formula (1) may be a straight-chain hydrocarbon group, a chain hydrocarbon group, or a cyclic hydrocarbon group, but a chain hydrocarbon group is preferable, and a straight-chain hydrocarbon group is particularly preferable. 2 When X has a hydroxyl group, this hydroxyl group can impart hydrophilicity to component (C), and therefore the solubility parameter (SP) of component (C) can be controlled. Furthermore, in formula (1), X is preferably -O-.
[0049] The compound represented by the above formula (1) may be present in a plurality of types during the production of the organic polymer compound of component (C). 1 , R 2 A plurality of monomers having different structures corresponding to X may be used.
[0050] Examples of the compound represented by formula (1) include (meth)acrylate monomers in which X in formula (1) is -O-, such as alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glycerin (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, and benzyl (meth)acrylate. Examples of the compound represented by formula (1) include (meth)acrylamide monomers in which X in formula (1) is -NH-, such as alkyl (meth)acrylamides such as ethyl (meth)acrylamide, n-butyl (meth)acrylamide, i-butyl (meth)acrylamide, and t-butyl (meth)acrylamide; and N-hydroxyalkyl (meth)acrylamides such as N-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, and N,N-dihydroxyethyl (meth)acrylamide.
[0051] The organic polymer compound of component (C) may be copolymerized with a radical polymerizable monomer other than the compound represented by formula (1). Examples of such monomers include glycol (meth)acrylic monomers having an alkyl group at the end such as methoxy (poly) ethylene glycol (meth) acrylate, methoxy (poly) propylene glycol (meth) acrylate, methoxy (poly) ethylene glycol (poly) propylene glycol (meth) acrylate, methoxy tetramethylene glycol (meth) acrylate, octoxy (poly) ethylene glycol (meth) acrylate, octoxy (poly) propylene glycol (meth) acrylate, octoxy (poly) ethylene glycol (poly) propylene glycol (meth) acrylate, octoxy tetramethylene glycol (meth) acrylate, lauroxy (poly) ethylene glycol (meth) acrylate, and stearoxy (poly) ethylene glycol (meth) acrylate; (meth)acrylic monomers having a carboxyl group such as (meth) acrylic acid; (poly) ethylene glycol (meth) acrylate; (Poly)alkylene glycol (meth)acrylates such as acrylates, (poly)propylene glycol (meth)acrylates, (poly)ethylene glycol / (poly)propylene glycol (meth)acrylates, and tetramethylene glycol (meth)acrylates; (meth)acrylic monomers having a phosphate ester group in the molecule such as 2-(meth)acryloyloxyethyl phosphate; (meth)acrylic monomers having an epoxy group such as glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate; (meth)acrylic monomers having an oxolane group such as tetrahydrofurfuryl (meth)acrylate and (meth)acryloyloxypropyl-1,3-dioxolane; (meth)acrylic monomers having an ethylene urea group such as N-(2-(meth)acryloyloxyethyl)ethylene urea; (meth)acrylic monomers having a dicyclopentyl group such as dicyclopentenyloxyethyl (meth)acrylate;(Meth)acrylic monomers having an amino group such as tetramethylpiperidinyl (meth)acrylate, pentamethylpiperidinyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, (meth)acryloyloxyethyl trimethyl ammonium chloride, (meth)acryloyloxyethyl dimethyl benzyl ammonium chloride; (meth)acrylic monomers having an alkoxy group such as 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane; styrene-based monomers such as styrene, p-chlorostyrene, and p-bromostyrene. In the organic polymer compound of component (C) used in the present invention, the above raw material monomers may be used alone or in combination of two or more kinds.;
[0052] Furthermore, the (meth)acrylic resin that can be used in component (C) is (meth)acryloy The (meth)acrylic resin may have an unsaturated double bond such as an aryl group. Examples of the method for introducing a (meth)acryloyl group into a (meth)acrylic resin include a method for reacting a compound having a (meth)acryloyl group and a carboxyl group with a (meth)acrylic resin having an epoxy group, a method for reacting a compound having a (meth)acryloyl group and an epoxy group with a (meth)acrylic resin having a carboxyl group, a method for reacting a compound having a (meth)acryloyl group and a carboxyl group with a (meth)acrylic resin having a hydroxyl group, a method for reacting a compound having a (meth)acryloyl group and a hydroxyl group with a (meth)acrylic resin having a carboxyl group, a method for reacting a compound having a (meth)acryloyl group and a hydroxyl group with a (meth)acrylic resin having an isocyanate group, and a method for reacting a compound having a (meth)acryloyl group and an isocyanate group with a (meth)acrylic resin having a hydroxyl group.
[0053] In the (meth)acrylic resin usable as component (C), the amount of (meth)acryloyl groups is preferably less than 2.0 mmol / g, more preferably 1.0 mmol / g or less, and even more preferably 0.5 mmol / g or less, from the viewpoint of antiblocking properties. On the other hand, the lower limit of the amount of (meth)acryloyl groups is not limited, and is usually 0, that is, there is no methacryloyl group.
[0054] The reaction time of the radical polymerization reaction in producing the (meth)acrylic resin is usually 1 to 20 hours, and preferably 3 to 12 hours, and the reaction temperature is usually 40 to 120°C, and preferably 50 to 100°C.
[0055] Examples of organic solvents that can be used in the radical polymerization reaction when producing a (meth)acrylic resin include ketone-based solvents such as acetone, methyl ethyl ketone (MEK), and methyl isobutyl ketone (MIBK); alcohol-based solvents such as ethanol, methanol, isopropyl alcohol (IPA), and isobutanol; ether-based solvents such as ethylene glycol dimethyl ether and propylene glycol monomethyl ether (PGM); ester-based solvents such as ethyl acetate, propylene glycol monomethyl ether acetate, and 2-ethoxyethyl acetate; and aromatic hydrocarbon solvents such as toluene. These organic solvents may be used alone or in combination of two or more. Note that such organic solvents may be left as they are after the synthesis of the (meth)acrylic resin and used as the organic solvent in the curable composition.
[0056] As the radical polymerization initiator that can be used when producing the (meth)acrylic resin, known radical polymerization initiators can be used, for example, organic peroxides such as benzoyl peroxide and di-t-butyl peroxide; and azo compounds such as 2,2'-azobisbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). These radical polymerization initiators may be used alone or in combination of two or more. The radical polymerization initiator is usually used in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the total of the radical polymerizable monomers as the raw material.
[0057] The (meth)acrylic resin usable for component (C) can be produced by using the above-mentioned radical polymerizable monomers and a known radical polymerization reaction. The radical polymerization reaction can usually be carried out in an organic solvent in the presence of a radical polymerization initiator. In order to make the weight average molecular weight (Mw) of the (meth)acrylic resin fall within the above range, for example, a method of controlling the polymerization conditions such as the polymerization temperature, the amount of the polymerization initiator, the amount of the chain transfer agent, the solid content concentration, and the method of adding the monomer can be adopted.
[0058] When obtaining a (meth)acrylic resin, it is preferable to use a chain transfer agent because it is easy to control the weight average molecular weight (Mw). The amount of the chain transfer agent used is preferably 0.1 to 25 parts by weight, more preferably 0.5 to 20 parts by weight, and even more preferably 1.0 to 15 parts by weight, based on 100 parts by weight of the total of the radical polymerizable monomers used as raw materials.
[0059] Known chain transfer agents can be used when obtaining the (meth)acrylic resin. For example, butanethiol, octanethiol, decanethiol, dodecanethiol, hexadecanethiol, octadecanethiol, cyclohexyl mercaptan, thiophenol, octyl thioglycolate, octyl 2-mercaptopropionate, octyl 3-mercaptopropionate, 2-ethylhexyl mercaptopropionate, 2-ethylhexyl thioglycolate, butyl-3-mercaptopropionate, methyl-3-mercaptopropionate, 2,2-(ethylenedioxy)diethanethiol, ethanethiol, 4-methylbenzenethiol, octyl mercaptopropion ...ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mercaptopropionate, ethyl mer Examples of thiol-based compounds include 2-mercaptoethyl tanoate, 1,8-dimercapto-3,6-dioxaoctane, decane trithiol, dodecyl mercaptan, diphenyl sulfoxide, dibenzyl sulfide, 2,3-dimethylcapto-1-propanol, mercaptoethanol, thiosalicylic acid, thioglycerol, thioglycolic acid, 3-mercaptopropionic acid, thiomalic acid, mercaptoacetic acid, mercaptosuccinic acid, 2-mercaptoethanesulfonic acid, 3-mercaptopropyltrimethoxysilane, and 3-mercaptopropylmethyldimethoxysilane.
[0060] The (meth)acrylic resin usable as component (C) can be produced by the above-mentioned method, but a commercially available product can also be used as it is. Examples of commercially available products include "Polyflow No. 75", "Polyflow No. 77", "Polyflow No. 90", "Polyflow No. 50EHF", "Polyflow No. 85HF", "Polyflow No. 95", "Polyflow No. 99C", "Polyflow No. 7", "Polyflow No. 54N", "Polyflow KL-800" (all manufactured by Kyoeisha Chemical Co., Ltd.), "LF1984", "LF1983", "LHP90", "LHP95", "UV Examples of such polymers include "UVX-271", "UVX-272", "UVX-190", "UVX-36", "UVX-35", "UVX-3750", and "UVX-189" (all manufactured by Kusumoto Chemicals), "BYK-350", "BYK-352", "BYK-354", "BYK-356", "BYK-361N", "BYK-381", "BYK-392", "BYK-394", "BYK-3441", and "BYK-3440" (all manufactured by BYK).
[0061] The content of component (C) in the curable composition of the present invention is, relative to 100 parts by weight of component (A), 0.01 parts by weight or more, and preferably 0.1 parts by weight or more, from the viewpoint of improving antiblocking properties, and on the other hand, 20 parts by weight or less, preferably 10 parts by weight or less, and more preferably 5 parts by weight or less, from the viewpoint of suppressing a decrease in surface hardness.
[0062] [Organic solvents] The curable composition of the present invention preferably contains an organic solvent. When the curable composition of the present invention contains an organic solvent, the solid content concentration is preferably 5 to 95% by weight. A solid content concentration of 5% by weight or more is preferable from the viewpoint of transparency, which makes the dispersibility of the component (B) good, and is also preferable for preventing an unintended curing reaction (gelation, etc.) of the curable composition. A solid content concentration of 95% by weight or less is preferable from the viewpoint of coatability and storage stability. From these viewpoints, the solid content concentration is more preferably 10% by weight or more, even more preferably 15% by weight or more, more preferably 90% by weight or less, even more preferably 85% by weight or less, and particularly preferably 80% by weight or less. In the present invention, the term "solid content" means a component excluding the solvent, and includes not only solid components but also semi-solid and viscous liquid components.
[0063] The organic solvent is not particularly limited, and can be appropriately selected in consideration of the types of components (A), (B), and (C), the type of substrate used when forming the hard coat layer, the method of application to the substrate, etc. Specific examples of the organic solvent include saturated hydrocarbon solvents such as n-hexane, n-heptane, n-octane, n-decane, n-dodecane, 2,3-dimethylhexane, 2-methylheptane, 2-methylhexane, 3-methylhexane, and cyclohexane; aromatic solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone (MEK), acetone, methyl isobutyl ketone (MIBK), and cyclohexanone; diethyl ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ... Examples of suitable solvents include ether-based solvents such as ethylene glycol diethyl ether, propylene glycol monomethyl ether, anisole, and phenetole; ester-based solvents such as ethyl acetate, butyl acetate, isopropyl acetate, ethylene glycol diacetate, and propylene glycol monomethyl ether acetate; amide-based solvents such as dimethylformamide, diethylformamide, and N-methylpyrrolidone; cellosolve-based solvents such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; alcohol-based solvents such as methanol, ethanol, propanol, isopropanol, and butanol; and halogen-based solvents such as dichloromethane and chloroform.
[0064] These organic solvents may be used alone or in combination of two or more. Among these, it is preferable to use at least one selected from saturated hydrocarbon solvents, ester solvents, ether solvents, alcohol solvents, and ketone solvents.
[0065] [Polymerization initiator] The curable composition of the present invention preferably contains a polymerization initiator in order to improve the curability. The polymerization initiator is preferably a photopolymerization initiator, and examples thereof include 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. These polymerization initiators may be used alone or in combination of two or more.
[0066] The content of the polymerization initiator is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and even more preferably 0.1 parts by weight or more, relative to 100 parts by weight of component (A) from the viewpoint of enhancing curability. Also, the content of the polymerization initiator is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and particularly preferably 3 parts by weight or less, relative to 100 parts by weight of component (A) from the viewpoint of stability of the curable composition.
[0067] [Other ingredients] The curable composition of the present invention may contain other components other than the components (A), (B), (C), organic solvent, and polymerization initiator, as long as the effects of the present invention are not impaired. Examples of other components include ultraviolet absorbers, hindered amine light stabilizers, fillers (excluding those corresponding to component (B)), silane coupling agents (excluding those corresponding to component (B)), reactive diluents (excluding those corresponding to component (A)), antistatic agents, organic pigments, slip agents, dispersants, thixotropic agents (thickeners), defoamers, antioxidants, and thermoplastic resins (excluding those corresponding to component (C)).
[0068] [Method of producing curable composition] The method for producing the curable composition of the present invention is not particularly limited, but for example, the composition can be obtained by mixing components (A), (B), (C), and, if necessary, an organic solvent, a polymerization initiator, other components, etc. When mixing the components, it is preferable to mix them uniformly using a disperser, a stirrer, etc.
[0069] [Cured product, laminate and hard-coated film] A cured product (sometimes referred to as "cured product of the present invention") can be obtained by curing the curable composition of the present invention by irradiating it with active energy rays or the like. A laminate can also be obtained by applying the curable composition onto a substrate and irradiating it with active energy rays to form a hard coat layer. In particular, a hard coat film can be obtained by applying the curable composition onto a substrate or the like and curing it into a film. In the present invention, the term "application" is used as a concept that also includes what is generally called "coating". In the present invention, the term "hard coat" refers to a product obtained by applying and curing a curable composition.
[0070] Examples of the substrate used in the laminate include organic materials such as plastic substrates; and inorganic materials such as metal substrates and glass substrates. Examples of the plastic substrates include various synthetic resins, such as acrylonitrile-butadiene-styrene copolymer (ABS) resin, polycarbonate (PC) resin, polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polymethyl methacrylate (PMMA) resin, polystyrene (PS) resin, polyimide (PI) resin, and polyolefin (PO) resin. Examples of the metal substrates are not particularly limited, and include, for example, hot-rolled steel sheets, cold-rolled steel sheets, hot-dip galvanized steel sheets, electrogalvanized steel sheets, tinplate, tin-free steel, and other various plated or alloy-plated steel sheets, stainless steel sheets, and aluminum sheets. Furthermore, these may be subjected to various surface treatments such as phosphate treatment, chromate treatment, organic phosphate treatment, organic chromate treatment, and heavy metal replacement treatment such as nickel. As the glass substrate, in addition to ordinary glass, glass that has been subjected to various chemical treatments (for example, Gorilla Glass (registered trademark) from Corning Incorporated and Dragontrail (registered trademark) from Asahi Glass Co., Ltd., etc.) and multi-component glass may be used. The curable composition of the present invention is suitable for plastic substrates and glass substrates, and is particularly suitable for plastic substrates, and among plastic substrates, is particularly suitable for polycarbonate resins, polyethylene terephthalate resins, and polymethyl methacrylate resins. The substrates listed above may be used alone or in combination of two or more.
[0071] Examples of the method for applying (coating) the curable composition of the present invention onto a substrate include a reverse coating method, a gravure coating method, a rod coating method, a bar coating method, a Mayer bar coating method, a die coating method, a spray coating method, etc. The form of the cured product is not particularly limited, but in the case of a cured product obtained by curing by irradiating an active energy ray onto a substrate, it can usually be obtained in the form of a cured coating (cured film) on at least a part of one side of the substrate.
[0072] The humidity when the curable composition is applied (coated) onto a substrate is not particularly limited, and is usually 1 to 100%, preferably 5 to 95%. When obtaining a cured product, it is preferable to dry the composition before irradiating it with active energy rays, and the drying temperature is usually 40 to 160°C, preferably 45 to 150°C.
[0073] The active energy rays that can be used to cure the curable composition include ultraviolet rays, electron beams, X-rays, infrared rays, and visible light. Among these active energy rays, ultraviolet rays and electron beams are preferred from the viewpoints of curability and prevention of resin deterioration.
[0074] When the curable composition is cured by ultraviolet irradiation, various ultraviolet irradiation devices can be used, and as the light source, a xenon lamp, a high-pressure mercury lamp, a metal halide lamp, an LED-UV lamp, etc. can be used. The ultraviolet irradiation dose is usually 10 to 10,000 mJ / cm. 2 From the viewpoints of the curability of the curable composition, the flexibility of the cured product (cured film), etc., it is preferably 30 to 5,000 mJ / cm 2 and more preferably 50 to 3,000 mJ / cm 2 The UV irradiance is usually 50 to 1,000 mW / cm 2 and preferably 70 to 800 mW / cm 2 It is.
[0075] When the curable composition is cured by electron beam irradiation, various electron beam irradiation devices can be used. The dose (Mrad) of the electron beam is usually 0.5 to 20 Mrad, and preferably 1 to 15 Mrad from the viewpoints of the curability of the curable composition, the flexibility of the cured product, and prevention of damage to the substrate.
[0076] The curable composition of the present invention has a high degree of freedom in coating conditions, and as shown in the examples below, various conditions during coating such as humidity, drying temperature, UV irradiation amount, UV illuminance, etc. can be selected from a wide range of conditions. Even if these conditions are changed, the cured product and laminate have the advantage of being easily able to obtain good physical properties such as antiblocking property and transparency.
[0077] In addition, the laminate according to another embodiment of the present invention has a substrate layer and a hard coat layer, the hard coat layer contains the component (B), and has a haze value measured according to JIS K7136 (2000) of less than 0.6%. The lower the haze value, the better the transparency, which is preferable. This laminate can be obtained by curing the curable composition of the present invention on a substrate. The substrate and curing conditions that can be used are as described above.
[0078] Furthermore, the hard coat film of the present invention contains the component (B), and the content thereof is 0.01 to 55% by weight based on the entire hard coat film. When the hard coat film contains the component (B) in an amount equal to or more than the lower limit, the antiblocking property is good, and when the amount is equal to or less than the upper limit, the transparency is good. From these viewpoints, the content of the component (B) in the hard coat film is preferably 0.5% by weight or more, more preferably 1% by weight or more, even more preferably 2% by weight or more, and particularly preferably 3% by weight or more, while it is preferably 48% by weight or less, more preferably 41% by weight or less, even more preferably 34% by weight or less, particularly preferably 27% by weight or less, and most preferably 20% by weight or less. The content of the component (B) is based on the entire hard coat film. This hard coat film can be obtained by curing the curable composition of the present invention. The curing conditions are as described above.
[0079] The thickness of the hard coat film is preferably 0.5 μm or more, more preferably 1 μm or more, while the thickness of the hard coat film is preferably 100 μm or less, more preferably 75 μm or less, even more preferably 50 μm or less, particularly preferably 25 μm or less, and most preferably 15 μm or less.
[0080] [Application] The curable composition of the present invention has excellent storage stability and a high degree of freedom in coating conditions, and the cured products and laminates obtained under various coating conditions have excellent antiblocking properties, transparency, recoatability, scratch resistance, curl resistance, etc. Therefore, it can be suitably used in any application where these properties are required, and is suitable as optical adjustment films such as retardation films and brightness enhancement films; protective films used in polarizing plates; and optical films such as ITO films used in touch panels and electromagnetic wave prevention films. Furthermore, these optical films are suitable for use in display devices (liquid crystal displays, light-emitting diode displays, electroluminescence displays, etc.) installed in bank ATMs, vending machines, personal digital assistants (PDAs), copiers, facsimiles, game machines, guide display devices installed in facilities such as museums and department stores, car navigation systems, multimedia stations (multifunctional terminals installed in convenience stores), mobile phones, monitor devices for railway vehicles, smartphones, tablets, etc. The present invention can be used in a variety of applications, including display, fluorescent display, and plasma display panels. EXAMPLES
[0081] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples. Note that the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples.
[0082] [Evaluation method] The curable compositions and cured films (hard coat films) produced in the following Examples and Comparative Examples were evaluated as follows.
[0083] <Anti-blocking property (AB property)> Two sheets of hard-coated film were prepared and hard-coated in an atmosphere of 23°C and 60% relative humidity. The curable compositions produced in each film example were overlapped with each other with their cured surfaces (the sides opposite to the surface coated with the clear hard-coat material) and a load of approximately 1 kg was applied with finger pressure. Then, it was confirmed whether the cured film surfaces had slipperiness or not, and the anti-blocking properties were evaluated according to the following criteria. ◎: Easy to slide ○: Can be slid and does not make noise △: It is possible to slide it, but it makes noise ×: The cured film surfaces are in close contact with each other and cannot be slid over each other.
[0084] <Transparency> The hard coat film was left in a thermostatic chamber at 23° C. and a relative humidity of 60% for 12 hours, after which the transparency was evaluated in terms of haze value (H%) according to JIS K7136 (2000), and the evaluation was performed according to the following criteria. ○: Haze value of the cured film is less than 0.6% △: Haze value of the cured film is 0.6% or more and less than 1.0% ×: Haze value of the cured film is 1.0% or more
[0085] <Recoatability> A line was drawn with an oil-based magic marker (Zebra's Maki Care Extra Fine (black) fine marker) on the surface of the hard coat film where the curable composition produced in each example had been cured (the side opposite to the surface coated with the clear hard coat material), and 30 seconds after drawing the line, the line was evaluated based on whether or not it repelled as follows. From the viewpoint of recoatability, it is preferable that the line does not repel. ○: Lines are not repelled ×: Repel lines
[0086] <Scratch resistance> Using #0000 steel wool, weighted at 176g / cm 2 The surface of the hard coat film on which the curable composition produced in each Example had been cured (the side opposite to the surface coated with the clear hard coat material) was rubbed back and forth 10 times with a rubbing cloth, and the degree of damage to the cured film caused by this was evaluated as follows. The fewer the scratches, the better. ○: 0 to 10 scratches △: 11 to 100 scratches ×: 101 or more scratches
[0087] <Storage stability> The curable composition was allowed to stand at 50° C., the time until gelation was measured, and the composition was evaluated according to the following criteria. ◎: No gelation after 90 days ○: No gelation after 30 days, but gelation within 90 days ×: Gel formed within 30 days
[0088] <Curl resistance> A curable composition (coating liquid) was applied using a bar coater onto a 100 μm-thick PET film whose four corners were fixed to glass plates so that the coating thickness after drying would be 3 to 5 μm, and the film was dried by heating at 80°C for 1 minute with an accumulated light dose of 500 mJ / cm 2 The pieces were cured by irradiating them with ultraviolet light using an ultraviolet light irradiation device manufactured by iGraphics, model number: UB0452-0752 [a mercury lamp (with a main wavelength of 365 nm, emitting ultraviolet light with wavelengths of 254 nm, 303 nm, and 313 nm)] so that the curl value was as follows: After that, the pieces were cut into 10 cm x 10 cm pieces. Immediately after cutting, the curl value of the four corners was measured as the height from the desk. The average value of the four measured points was regarded as the curl value, and it was evaluated according to the following criteria. ○: Curl value is less than 11 mm △: Curl value is 11mm or more and less than 25mm ×: Curl value is 25mm or more
[0089] <Refractive index> The refractive index of the cured film on the substrate (PET) was measured using a digital Abbe refractometer DR-A1 manufactured by ATAGO.
[0090] [Raw materials] The components (A) to (C) used as raw materials for the curable composition are as follows:
[0091] [Component (A)] A-1: Kayarad DPHA manufactured by Nippon Kayaku Co., Ltd. Mixture of dipentaerythritol tetraacrylate and dipentaerythritol hexaacrylate, weight average molecular weight (Mw): 700
[0092] A-2: Aronix M313 manufactured by Toagosei A mixture of ethylene oxide isocyanurate (EO) modified diacrylate (molecular weight: 369) and ethylene oxide isocyanurate (EO) modified triacrylate (molecular weight: 423)
[0093] A-3: Viscoat #1000 manufactured by Osaka Organic Chemical Industry Co., Ltd. Dendrimer acrylate (branched polyester polyol terminated acrylate), Mw): 1,900 The method for measuring Mw of A-1 and A-3 above is the same as that for component (C) described below.
[0094] [Component (B)] The particles used as component (B) are shown in Table 1. In Table 1, the "shape" and "dispersion state" were confirmed by a scanning electron microscope.
[0095] [Table 1]
[0096] In Table 1, the particle size distribution values of b-2, b-3, and b-4 are smaller than the average primary particle diameter. The reason for this is presumably due to the difference in the methods used, that is, the average primary particle diameter was confirmed by a scanning electron microscope, while the particle size distribution was measured by an optical method using a laser diffraction particle size distribution meter. In particular, it is presumed that for b-2, an accurate value for the particle size distribution could not be measured because the particles in the form of long chains were aggregated to a certain extent. Also, it is presumed that for b-3 and b-4, this is due to the fact that they are in a dispersed state, not in an aggregated state.
[0097] [Component (C)] Commercially available products were used for C-1 to C-5, and those synthesized by the method described below were used for C-6 to C-11. The abbreviations used below are as follows.
[0098] MEK: Methyl ethyl ketone ·DT: Dodecanethiol EA: ethyl acrylate (R 1 is a hydrogen atom, R 2 is an ethyl group) BMA: butyl methacrylate (R 1 is a methyl group, R 2 is a butyl group) HEA: Hydroxyethyl acrylate (R 1 is a hydrogen atom, R 2 is a hydroxyethyl group) BA: butyl acrylate (in the above formula (1), R 1 is a hydrogen atom, R 2 is a butyl group) LMA: lauryl methacrylate (R 1 is a methyl group, R 2 is a dodecyl group) HEMA: hydroxyethyl methacrylate (R 1 is a methyl group, R 2 is a hydroxyethyl group) EHA: 2-ethylhexyl acrylate (R 1 is a hydrogen atom, R 2 is a 2-ethylhexyl group)
[0099] C-1: Polyflow No. 36 manufactured by Kyoeisha Chemical Co., Ltd. Acrylic polymer (liquid at room temperature), Mw: 10,000, SP value: 9.6
[0100] C-2: Kyoeisha Chemical Co., Ltd. Polyflow No. 50EHF Acrylic polymer (liquid at room temperature), Mw: 10,000, SP value: 9.7
[0101] C-3: Polyflow No. 75 manufactured by Kyoeisha Chemical Co., Ltd. Acrylic polymer (liquid at room temperature), Mw: 2,400, SP value: 9.9
[0102] C-4: Polyflow No. 77 manufactured by Kyoeisha Chemical Co., Ltd. Acrylic polymer (liquid at room temperature), Mw: 2,200, SP value: 10.3
[0103] C-5: Polyflow No. 90 manufactured by Kyoeisha Chemical Co., Ltd. Acrylic polymer (liquid at room temperature), Mw: 12,000, SP value: 9.6
[0104] C-6: In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 250.33g of MEK, 15.00g of DT, 25.00g of EA, 25.00g of BMA, and 1.20g of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed, and a mixture of 25.00g of EA, 25.00g of BMA, and 10.40g of MEK was added dropwise over 1.5 hours, while reacting for 3 hours at 65°C. After that, 0.60g of 2,2'-azobis(2,4-dimethylvaleronitrile) was added and reacted for 3 hours, and then 10.80g of MEK and 0.50g of p-methoxyphenol were added and heated to 100°C to obtain a (meth)acrylic resin (liquid at room temperature). Mw: 2,600, SP value: 10.2
[0105] C-7: In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 243.33g of MEK, 15.00g of DT, 9.00g of HEA, 20.00g of BA, 21.00g of EHA, and 1.20g of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed, and a mixture of 9.00g of HEA, 20.00g of BA, 21.00g of EHA, and 21.40g of MEK was added dropwise over 1.5 hours, while reacting for 3 hours at 65°C. After that, 0.60g of 2,2'-azobis(2,4-dimethylvaleronitrile) was added and reacted for 3 hours, and then 8.97g of MEK and 0.50g of p-methoxyphenol were added and heated to 100°C to obtain an acrylic resin (liquid at room temperature). Mw: 3,400, SP value: 10.8
[0106] C-8: In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 131.67g of MEK, 5.00g of DT, 20.00g of EA, 20.00g of BMA, 10.00g of HEMA, and 1.20g of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed, and a mixture of 20.00g of EA, 20.00g of BMA, 10.00g of HEMA, and 21.40g of MEK was added dropwise over 1.5 hours, while reacting for 3 hours at 65°C. After that, 0.60g of 2,2'-azobis(2,4-dimethylvaleronitrile) was added and reacted for 3 hours, and then 8.90g of MEK and 0.50g of p-methoxyphenol were added and heated to 100°C to obtain a (meth)acrylic resin (liquid at room temperature). Mw: 6,100, SP value: 11.0
[0107] C-9: In a flask equipped with a thermometer, a stirrer and a reflux condenser, 131.67g of MEK, 5.00g of DT, 20.00g of EA, 20.00g of BMA, 10.00g of LMA and 1.20g of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed, and a mixture of 20.00g of EA, 20.00g of BMA, 10.00g of LMA and 21.40g of MEK was added dropwise over 1.5 hours, while reacting for 3 hours at 65°C. After that, 0.60g of 2,2'-azobis(2,4-dimethylvaleronitrile) was added and reacted for 3 hours, and then 8.90g of MEK and 0.50g of p-methoxyphenol were added and heated to 100°C to obtain a (meth)acrylic resin (liquid at room temperature). Mw: 6,400, SP value: 10.2
[0108] C-10: In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 131.67g of MEK, 9.00g of HEA, 21.00g of EHA, 20.00g of BA, and 1.20g of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed, and a mixture of 9.00g of HEA, 21.00g of EHA, 20.00g of BA, and 21.40g of MEK was added dropwise over 1.5 hours, while reacting for 3 hours at 65°C. After that, 0.60g of 2,2'-azobis(2,4-dimethylvaleronitrile) was added and reacted for 3 hours, and then 8.90g of MEK and 0.50g of p-methoxyphenol were added and heated to 100°C to obtain an acrylic resin (liquid at room temperature). Mw: 21,600, SP value: 11.1
[0109] C-11: In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 131.67g of MEK, 25.00g of BMA, 25.00g of EA, and 1.20g of 2,2'-azobis(2,4-dimethylvaleronitrile) were placed, and a mixture of 25.00g of BMA, 25.00g of EA, and 21.40g of MEK was added dropwise over 1.5 hours while reacting for 3 hours at 65°C. After that, 0.60g of 2,2'-azobis(2,4-dimethylvaleronitrile) was added and reacted for 3 hours, and then 8.90g of MEK and 0.50g of p-methoxyphenol were added and heated to 100°C to obtain a (meth)acrylic resin (liquid at room temperature). Mw: 19,900, SP value: 10.4
[0110] (Method of measuring weight average molecular weight (Mw)) Measurement was performed by GPC under the following conditions. Equipment: Tosoh Corporation "HLC-8120GPC" Column: Tosoh Corporation "TSKgel Super H1000+H2000+H3000" Detector: Differential refractive index detector (RI detector / built-in) Solvent: Tetrahydrofuran Temperature: 40℃ Flow rate: 0.5mL / min Injection volume: 10μL Concentration: 0.2% by weight Calibration sample: monodisperse polystyrene Calibration method: Polystyrene equivalent
[0111] [Polymerization initiator] Irgacure 184: BASF, Irgacure (trademark) 184, 1-hydroxy-cyclohexyl-phenyl-ketone
[0112] Example 1-1 [Substrate with clear hard coat] In a four-neck flask, 100 parts by weight of a mixture of dipentaerythritol tetraacrylate and dipentaerythritol hexaacrylate (Kayarad DPHA, manufactured by Nippon Kayaku Co., Ltd.) and 0.5 parts by weight of an acrylic polymer (Polyflow No. 75, manufactured by Kyoeisha Chemical Co., Ltd.) were mixed, and then 5 parts by weight of 1-hydroxy-cyclohexyl-phenyl-ketone (Irgacure (trademark) 184, manufactured by BASF) was added as a polymerization initiator, and 105.5 parts by weight of methyl ethyl ketone was further added to obtain a clear hard coat material. The above clear hard coat material was applied to a transparent biaxially oriented polyethylene terephthalate (PET) film (Diafoil (trademark) O321E125, manufactured by Mitsubishi Plastics Co., Ltd.) having a thickness of 125 μm using a bar coater so that the coating thickness after drying was 1 to 2 μm, and the film was dried by heating at 80 ° C for 1 minute, and the accumulated light amount was 300 mJ / cm. 2 The above clear hard coat material was applied to compensate for haze caused by the unevenness of the substrate itself.
[0113] [Production of Curable Composition] In a four-neck flask, components (A), (B), and (C) were mixed in the amounts shown in Table 2, and then the mixture was diluted with methyl ethyl ketone to a solid content of 50% by weight to obtain a curable composition.
[0114] [Coating process] The curable composition was applied to the surface of the PET film opposite to the surface coated with the clear hard coat material using a bar coater so that the coating thickness after drying would be 1 to 2 μm (5 to 10 μm for the film used for refractive index evaluation), and then heated and dried at 80° C. for 1 minute.
[0115] [Curing process] The PET film on which the coating of the curable composition was formed was exposed to light at a cumulative light intensity of 300 mJ / cm using an EYE UV METER UVPF-A1, PD365 manufactured by EYE GRAPHICS, Inc., at a position 15 cm below the light source, using a high-pressure mercury lamp with an output density of 120 W / cm. 2 (500mJ / cm for the curl resistance evaluation) 2) to obtain a cured film.
[0116] [evaluation] The prepared curable compositions and the formed cured films (hard coat films) were evaluated for anti-blocking property (AB property), transparency, refractive index, recoatability, scratch resistance, storage stability and curl resistance, and the results are shown in Table 2.
[0117] In Table 2, the weight parts of each component indicate the amount excluding the solvent, "-" for each raw material indicates that the raw material is not used, and "-" for "storage stability" and "curl resistance" indicates that the evaluation was not performed. These items in Table 2 have the same meanings in Tables 3 to 9.
[0118] <Examples 1-2 to 1-51 and Comparative Examples 1-1 to 1-17> Curable compositions were obtained in the same manner as in Example 1-1, except that the blending composition of the curable composition was changed as shown in Tables 2 to 9. The obtained curable compositions were subjected to the coating step and the curing step in the same manner as in Example 1-1 to obtain cured films (hard coat films). The obtained curable compositions and hard coat films were used to evaluate anti-blocking property (AB property), transparency, recoating property, and scratch resistance, and the results are shown in Tables 2 to 9. For Examples 1-2 to 1-4, storage stability and curl resistance were evaluated, and the results are shown in Table 2.
[0119] [Table 2]
[0120] [Table 3]
[0121] [Table 4]
[0122] [Table 5]
[0123] [Table 6]
[0124] [Table 7]
[0125] [Table 8]
[0126] [Table 9]
[0127] [Evaluation result (1)] As shown in Table 2, all of Examples 1-1 to 1-8, which correspond to the curable composition of the present invention and further contain component (C), were good in antiblocking property (AB property), transparency, recoatability, and scratch resistance. In addition, Examples 1-1 to 1-3 used "A-2" corresponding to a polyfunctional (meth)acrylate having a nitrogen atom-containing heterocyclic structure and "A-3" corresponding to a polyfunctional (meth)acrylate having a dendrimer structure as component (A), and therefore had better curl resistance than Example 1-4, which did not use these. Example 1-9 corresponds to the curable composition of the present invention, and was good in all of AB property, transparency, recoatability, and scratch resistance, but was slightly inferior to Examples 1-1 to 1-8 because particles with a relatively small d10 value were used as component (B). Moreover, Example 1-10 corresponds to the curable composition of the present invention, and was good in all of the AB property, transparency, recoatability, and scratch resistance, but since component (C) was not used, the AB property was slightly inferior to Examples 1-1 to 1-8.
[0128] Examples 1-11 to 1-21 shown in Table 3 are examples in which the type of component (C) was changed from that of Example 1-2, and all of them had good AB properties, transparency, recoatability, and scratch resistance. Examples 1-22 to 1-26 shown in Table 4 are examples in which the type of component (B) was changed from that of Example 1-4, and all of them had good AB properties, transparency, recoatability, and scratch resistance. As shown in Tables 6 and 7, the type and amount of each of the components (A), (B) and (C) were changed, and all of them had good AB properties, transparency, Ricoh properties and scratch resistance. In particular, the refractive index can be easily controlled by changing the type and amount of the component (B) as shown in Table 7.
[0129] In Table-8, Comparative Example 1-1 is an example in which component (B) was not used compared to Example 1-4, but the antiblocking property (AB property) was poor. Comparative Example 1-2 is an example in which "B-5" corresponding to component (B) was used and its blending amount was increased, but the transparency was poor. Furthermore, Comparative Examples 1-3 to 1-7 are examples in which particles other than component (B) were used instead of component (B) used in the present invention compared to Example 1-4, but all of them had inferior AB property to Example 1-4. Comparative Example 1-8 is an example in which particles having a large average primary particle size and d90 were used as particles other than component (B) instead of component (B) used in the present invention compared to Example 1-4, but the transparency was poor. Furthermore, Comparative Example 1-9 is an example in which particles having a larger d90 value than component (B) were used instead of component (B) used in the present invention compared to Example 1-4, but the transparency was poor.
[0130] On the other hand, in Table 8, when Example 1-10 is compared with Comparative Examples 1-10 to 1-12, which do not use the component (B) used in the present invention and instead use "b-1", "b-3", and "b-5" that do not correspond to component (B), it is found that Example 1-10 has good AB properties. That is, even if component (C) is not essential, by blending components (A) and (B) in predetermined amounts, the AB properties are improved and the transparency, recoatability, and scratch resistance are also good.
[0131] Comparative Examples 1-13 to 1-15 in Table 9 are examples in which the component (B) used in the present invention was not used in Example 1-30, and instead "b-1", "b-4", and "b-5" which do not correspond to the component (B) were used, respectively, but either the transparency or the AB property was poor. In addition, Comparative Examples 1-16 and 1-17, which did not use the component (B) used in the present invention, both had poor AB property.
[0132] [Examples 2-1 to 2-28] As shown in Tables 10 to 13, the curable compositions of the same formulation as in Examples 1-1 to 1-3 and Example 1-27 were used, and the opposite side of the clear hard-coated substrate to the side coated with the clear hard-coat material was coated with a bar coater so that the coating thickness after drying would be 1 to 2 μm, and then dried. Then, a cured film was obtained by irradiating with ultraviolet light. In the above operations, the humidity during coating, the drying temperature, the ultraviolet (UV) irradiation amount, and the ultraviolet (UV) illuminance were set under the conditions shown in Tables 10 to 13, respectively. The obtained cured films were evaluated for anti-blocking property (AB property) and transparency, and the results are shown in Tables 10 to 13.
[0133] [Table 10]
[0134] [Table 11]
[0135] [Table 12]
[0136] [Table 13]
[0137] [Evaluation result (2)] Examples 2-1 to 2-7, 2-8 to 2-14, 2-15 to 2-21, and 2-22 to 2-28 are examples in which the coating conditions were changed with the same formulation as the curable compositions of Examples 1-1, 1-2, 1-3, and 1-27, respectively. As shown in Tables 10 to 13, it can be seen that the anti-blocking properties and transparency were excellent under all coating conditions. [Industrial Applicability]
[0138] The curable composition of the present invention has excellent storage stability and a high degree of freedom in coating conditions, and the cured product and laminate obtained under various coating conditions have excellent antiblocking properties, transparency, recoatability, scratch resistance, curl resistance, etc. Therefore, it can be suitably used in any application where these properties are required, and is suitable as an optical film such as an optical adjustment film such as a retardation film and a brightness improvement film; a protective film used in a polarizing plate; and an ITO film used in a touch panel and an electromagnetic wave prevention film. Furthermore, these optical films can be used in display devices (liquid crystal displays, light-emitting diode displays, electroluminescence displays, fluorescent displays, plasma display panels, etc.) installed in facilities such as bank ATMs, vending machines, personal digital assistants (PDAs), copiers, facsimiles, game machines, museums, and department stores, car navigation systems, multimedia stations (multifunctional terminals installed in convenience stores), mobile phones, monitor devices for railway vehicles, smartphones, tablets, etc.
Claims
1. A curable composition comprising the following components (A), (B) and (C), and containing 0.01 to 110 parts by weight of component (B) per 100 parts by weight of component (A). Component (A): A compound containing at least one polyfunctional (meth)acrylate selected from the group consisting of polyfunctional (meth)acrylates having a nitrogen atom-containing heterocyclic structure, polyfunctional (meth)acrylates having a dendrimer structure, and polyfunctional (meth)acrylates having a hyperbranched polymer structure. Component (B): Silica particles having an average primary particle size of 10 to 50 nm, and having a d90 of 250 to 1,000 nm, a d10 of 20 to 150 nm, and a d50 of 30 to 500 nm as measured by a laser diffraction particle size distribution meter, and a value of [average primary particle size] / [d90] of 0.02 to 0.
20. Component (C): a (meth)acrylic resin having a weight average molecular weight (Mw) of 2,100 to 200,000 and a solubility parameter (SP value) of 9.3 to 12.6
2. The curable composition according to claim 1, wherein the weight average molecular weight of component (A) is less than 2,100, and the content of component (C) is 0.01 to 20 parts by weight per 100 parts by weight of component (A).
3. The curable composition according to claim 1 or 2, wherein the total content of the polyfunctional (meth)acrylate is 1 to 65% by weight based on the total content of component (A).
4. The curable composition according to any one of claims 1 to 3, which contains an organic solvent and has a solid content concentration of 5 to 95% by weight.
5. The curable composition according to claim 4, wherein the organic solvent is at least one selected from the group consisting of saturated hydrocarbon solvents, ester solvents, ether solvents, alcohol solvents, and ketone solvents.
6. The curable composition according to any one of claims 1 to 5, which contains a polymerization initiator and has a content of 0.01 to 20 parts by weight based on 100 parts by weight of the component (A).
7. A cured product obtained by irradiating the curable composition according to any one of claims 1 to 6 with active energy rays.
8. A laminate having a substrate and a hard coat layer, the hard coat layer being a layer formed by applying the curable composition according to any one of claims 1 to 6 onto the substrate and irradiating the applied composition with active energy rays.
9. The laminate of claim 8 , wherein the substrate is a plastic substrate.
10. The laminate according to claim 9, wherein the plastic substrate is at least one selected from the group consisting of a polycarbonate resin, a polyethylene terephthalate resin, and a polymethyl methacrylate resin.
Citation Information
Patent Citations
Film having cured coat of radiation-cured type resin composition
JP2009196375A
Curable composition, conductive laminate, method of manufacturing the same, and touch panel
JP2011029175A
Colored photosensitive resin composition