Ni-based alloy powder for additive manufacturing, additive manufactured products, and manufacturing method for additive manufactured products

A tailored Ni-based alloy powder composition addresses weld cracking and oxidation resistance issues in additive manufacturing, producing high-temperature-resistant components with reduced defects for semiconductor and electronic components.

JP7589859B2Active Publication Date: 2024-11-26PROTERIAL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024504719
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-04
Filing Date
2023-03-01
Publication Date
2024-11-26
Estimated Expiration
2043-03-01

AI Technical Summary

Technical Problem

Existing Ni-based alloys used in additive manufacturing for semiconductor and electronic components face high weld cracking susceptibility and poor high-temperature oxidation resistance, especially when forming complex shapes with gas flow channels, leading to defects and cracks.

Method used

A Ni-based alloy powder composition with specific ranges of Al, Cr, C, Si, Mn, O, and limited Zr content, along with controlled particle size and hardness, is developed to enhance high-temperature oxidation resistance and reduce weld cracking, suitable for additive manufacturing processes.

Benefits of technology

The alloy powder results in additively manufactured products with fewer cracks, defects, and excellent high-temperature oxidation resistance, suitable for semiconductor and electronic component manufacturing equipment, maintaining structural integrity and preventing contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589859000004
    Figure 0007589859000004
  • Figure 0007589859000001
    Figure 0007589859000001
  • Figure 0007589859000002
    Figure 0007589859000002
Patent Text Reader

Abstract

Provided are: Ni-based alloy powder which is free from cracks and defects, excellent in high-temperature oxidation resistance, and suitable for lamination molding; a lamination molded article using the Ni-based alloy powder; and a manufacturing method thereof. A solution therefor is Ni-based alloy powder for lamination molding, containing Al: 3.5-5.5%, Cr: 0.8-4.0%, C: 0.02-0.06%, Si: 1.0-3.0%, Mn: 1.5% or less, and O: 0.001-0.050% in terms of mass%, the balance being Ni and inevitable impurities, the Ni-based alloy powder being characterized in that Zr included in the inevitable impurities is limited to 0.01% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Ni-based alloy powder for additive manufacturing (hereinafter sometimes referred to as Ni-based alloy powder) suitable for additive manufacturing, an additive manufactured product, and a method for manufacturing an additive manufactured product, and relates to members and parts used in, for example, oxidation furnaces used in semiconductor manufacturing and sintering furnaces for electronic components. [Background technology]

[0002] In general, Ni-based alloys with excellent high-temperature oxidation resistance are used for components and parts installed in furnaces used in oxidation furnaces used in semiconductor manufacturing and firing furnaces for electronic parts to prevent oxide scale generated from the components and parts from being mixed into the product. As an example of such Ni-based alloys with excellent high-temperature oxidation resistance, as shown in Patent Document 1, a Ni-based alloy with excellent high-temperature oxidation resistance has been proposed, which contains Al: 3.6 to 4.4% by mass (hereinafter, % refers to mass%), and further contains one or more of Si: 0.1 to 2.5%, Cr: 0.8 to 4.0%, and Mn: 0.1 to 1.5% as necessary, with the balance being Ni and unavoidable impurities, and is used as fins and tubes for high-temperature heat exchangers.

[0003] Furthermore, Patent Document 2 proposes a Ni-based alloy that has excellent hot forgeability and high-temperature oxidation resistance, containing 2.0-5.0% Al, 0.1-2.5% Si, 0.8-4.0% Cr, 0.1-1.5% Mn, 0.001-0.01% B, 0.001-0.1% Zr, and the remainder being Ni and unavoidable impurities. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-262491 A [Patent Document 2] JP 2014-080675 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in recent years, in applications such as semiconductor product and electronic component manufacturing furnace members and parts, it is required to realize not only excellent high-temperature oxidation resistance but also complex shapes such as gas flow paths inside the members and parts. It is known that additive manufacturing using alloy powder (hereinafter referred to as additive manufacturing in the present invention) is suitable as a means for realizing this complex shape. Here, although the Ni-based alloys described in Patent Documents 1 and 2 above have excellent high-temperature oxidation resistance, they have a problem of high weld crack susceptibility (hereinafter sometimes referred to as crack susceptibility) due to their high Al content. The additive manufacturing method involves a process of repeatedly melting and solidifying individual powders, and this process corresponds to welding at a micro level, so it can be easily inferred that cracks will occur even if the Ni-based alloys described in Patent Documents 1 and 2 above, which have high weld crack susceptibility, are applied to the additive manufacturing method. In addition, if the high-temperature oxidation resistance is poor, defects caused by oxides will become apparent. Based on the above, the present invention aims to provide a Ni-based alloy powder that is suitable for producing additively manufactured products that have few cracks and defects and have excellent resistance to high-temperature oxidation, an additively manufactured product using this Ni-based alloy powder, and a method for manufacturing the additively manufactured product. [Means for solving the problem]

[0006] The present invention provides a Ni-based alloy powder for additive manufacturing, characterized in that it contains, by mass%, 3.5-5.5% Al, 0.8-4.0% Cr, 0.02-0.06%, 1.0-1.8% Si, 1.5% or less Mn, 0.001-0.050% O, with the balance being Ni and unavoidable impurities, with the Zr contained in the unavoidable impurities being limited to 0.01% or less.

[0007] The Ni-based alloy powder for additive manufacturing preferably contains 3.6 to 5.0% Al, 1.5 to 3.0% Cr, 0.03 to 0.05% C, 1.2 to 1.5% Si, 0.2 to 1.0% Mn, and 0.008 to 0.030% O.

[0008] The Ni-based alloy powder for additive manufacturing preferably has a Vickers hardness in the range of 160 to 220 HV.

[0009] In addition, in an cumulative distribution curve showing the relationship between particle diameter and volume accumulation from the small particle diameter side, obtained by a laser diffraction method, the Ni-based alloy powder for additive manufacturing preferably has a particle diameter d10 corresponding to a cumulative frequency of 10 volume% of the powder of 10 μm or more and 25 μm or less, a particle diameter d50 corresponding to a cumulative frequency of 50 volume% of the powder of 25 μm or more and 40 μm or less, and a particle diameter d90 corresponding to a cumulative frequency of 90 volume% of the powder of 45 μm or more and 60 μm or less.

[0010] Moreover, it is preferable that the uniformity represented by (d90-d10) / d50 is in the range of 0.8 to 1.2.

[0011] In addition, in the Ni-based alloy powder for additive manufacturing, it is preferable that the angle of repose measured in accordance with JIS R9301-2-2 is 40 degrees or less.

[0012] The present invention also relates to a method for producing an additive manufacturing product, characterized in that it comprises an additive manufacturing process for forming an additive manufacturing body using Ni-based alloy powder containing, by mass%, 3.5-5.5% Al, 0.8-4.0% Cr, 0.02-0.06% C, 1.0-1.8% Si, 1.5% or less Mn, 0.001-0.050% O, with the remainder being Ni and unavoidable impurities, wherein Zr among the unavoidable impurities is limited to 0.01% or less.

[0013] The present invention also relates to a steel sheet containing, by mass%, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 1.8% Si, 1.5% or less Mn, 0.001 to 0.050% O, with the balance being Ni and unavoidable impurities, in which Zr contained in the unavoidable impurities is limited to 0.01% or less, the defect rate is 0.1% or less, and the unit area oxidation amount, which is obtained by an oxidation test performed in an atmospheric furnace at 800°C for 950 hours and is expressed as [mass loss before and after oxidation test] / [surface area before oxidation test], is 0.005 mg / mm 2The present invention relates to an additive manufacturing product characterized in that:

[0014] The hardness of the layered product is preferably in the range of 210 to 300 HV. Effect of the Invention

[0015] The Ni-based alloy powder of the present invention is an alloy powder for additive manufacturing that has excellent high-temperature oxidation resistance and low weld crack susceptibility, and is also suitable for suppressing defects. When this Ni-based alloy powder is used to manufacture members and parts for semiconductor and electronic component manufacturing equipment by additive manufacturing, it is possible to obtain additive manufactured products with few cracks and defects and excellent high-temperature oxidation resistance, and members and parts made of this additive manufactured product. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a diagram showing oxidation test results of additive manufacturing products according to an embodiment of the present invention and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Ni-based alloy powder] The present inventors conducted extensive research into alloy compositions and additive manufacturing methods in order to develop Ni-based alloy powders for additive manufacturing that have excellent high-temperature oxidation resistance and additive manufacturing properties. As a result, it was found that Ni-based alloy powders containing, by mass%, 3.5-5.5% Al, 0.8-4.0% Cr, 0.02-0.06% C, 1.0-3.0% Si, 1.5% or less Mn, 0.001-0.050% O, with the balance being Ni and unavoidable impurities, in which the Zr contained in the unavoidable impurities is limited to 0.01% or less, have excellent properties in terms of high-temperature oxidation resistance and additive manufacturing properties that allow molding with fewer cracks and defects.

[0018] The reasons for the numerical limitations of each component element in the alloy composition of the Ni-based alloy powder of the present invention will be described in detail below. After that, the manufacturing method of the alloy powder and the layered manufacturing product will be described. In this specification, a numerical range expressed using "~" includes the numerical values ​​written before and after "~" as the lower and upper limits. The upper and lower limits written in stages can be arbitrarily combined. In addition, "%" is to be read as "mass%".

[0019] (Al: 3.5-5.5%) Al forms an alumina coating on the surface of the additive manufacturing product, improves high-temperature oxidation resistance, and reduces the occurrence of oxide scale. In addition, Al is added to Ni-based alloy powder because it forms a passivation coating of oxide on the surface layer to prevent further oxidation of the Ni-based alloy powder. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the Al content is 3.5%. On the other hand, if the Al content is too high, microcracks are likely to occur during additive manufacturing, which involves repeated local melting and solidification, so the upper limit of the Al content is 5.5%. In addition, the preferred Al content is 3.6 to 5.0%, and more preferably 3.7 to 4.1%.

[0020] (Cr: 0.8~4.0%) Cr is an effective element for improving high-temperature oxidation resistance by stabilizing the alumina coating. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the Cr content is 0.8%. On the other hand, if the Cr content is too high, the formation of the alumina coating is inhibited, so the upper limit of the Cr content is 4.0%. The preferred Cr content is 1.5 to 3.0%, and more preferably 1.9 to 2.1%.

[0021] (C: 0.02~0.06%) C is effective in reducing crack sensitivity, preventing shrinkage cavities during solidification, and improving tensile strength. In order to sufficiently reduce crack sensitivity, the lower limit of the C content is 0.02%. On the other hand, if the C content is too high, Cr carbides are formed and corrosion resistance decreases, so the upper limit of the C content is 0.06%. The C content is preferably 0.03 to 0.05%, and more preferably 0.035 to 0.04%.

[0022] (O:0.001~0.050%) O has the effect of instantly bonding with Al during the gas atomization process in the production of Ni-based alloy powder, forming a very thin and strong oxide film on the powder surface, thereby suppressing the further progression of oxidation. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the O content is 0.001%. On the other hand, if the O content is too high, the oxide film formed on the powder surface becomes apparent as defects during additive manufacturing, so the upper limit of the O content is 0.050%. In addition, the preferred O content is 0.008 to 0.030%, and more preferably 0.010 to 0.015%.

[0023] The C and O contents can be controlled, for example, by melting in a vacuum and controlling the atmosphere by argon gas atomization.

[0024] (Zr:0.01% or less) Zr is an impurity that is inevitably mixed in when manufacturing Ni-based alloy powder. If the Zr content is high, it forms oxides and inhibits the formation of an alumina coating. Furthermore, its segregation at the grain boundaries makes it easier for microcracks to occur from the grain boundaries. In order to avoid these problems, Zr is particularly limited. The Zr content is aimed for 0%, with the upper limit set at 0.01%. It is preferably 0.001% or less, and more preferably 0.0001% or less.

[0025] (Si: 1.0-1.8%) Like Cr, Si has the effect of improving high-temperature oxidation resistance by stabilizing the alumina coating formed on the additive manufacturing product. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the Si content is 1.0%. On the other hand, if the Si content is too high, shrinkage cavities are likely to occur during solidification in the process in which each Ni-based alloy powder repeatedly melts and solidifies, so the upper limit of the Si content is 1.8%. In addition, the preferred Si content is 1.2 to 1.6%, and more preferably 1.3 to 1.5%.

[0026] (Mn:1.5% or less) Mn has the effect of suppressing solidification cracking that is increased by the inclusion of Al. In addition, for example, when the additive manufacturing speed is increased, the heat input increases and solidification cracking is likely to occur, so it is preferable to adjust the amount added according to the additive manufacturing speed. The above-mentioned effect can be exhibited by making the Mn content more than 0%. Furthermore, in order to effectively exhibit the effect, it is preferable that the Mn content is 0.1% or more. On the other hand, if the Mn content exceeds 1.5%, the high-temperature oxidation resistance decreases. Therefore, the Mn content is set to 1.5% or less. Furthermore, the preferable Mn content is 0.2 to 1.0%, and more preferably 0.4 to 0.6%.

[0027] (The balance is Ni and unavoidable impurities) For example, the total of the unavoidable impurities is preferably 1.0% or less. Each of the unavoidable impurities is preferably 0.5% or less, more preferably 0.1% or less. More specifically, the P, S, and N contents are preferably 0.01% or less, and the Fe, B, Ti, Cu, Nb, Mo, and Co contents are preferably 0.5% or less.

[0028] The composition of the Ni-based alloy powder of this embodiment can be determined by the following measurement method. As described in the examples below, the powder for additive manufacturing after classification was dissolved in an appropriate aqueous solution, and the aqueous solution was analyzed by high-frequency inductively coupled plasma (ICP) to measure the content of the predetermined components. The content of C, N, and O can be determined by performing gas analysis by a combustion method.

[0029] (Hardness of Ni-based alloy powder: 160~220HV) The hardness of the Ni-based alloy powder can be set to 160HV or more so that the particles are not crushed when the powder is spread. On the other hand, if the hardness of the powder is too high, the manufactured additive manufacturing product is likely to crack, so the upper limit of the hardness can be set to 220HV. Also, it is preferably 170 to 200HV, more preferably 180 to 190HV.

[0030] (Particle size of Ni-based alloy powder: 1 to 200 μm) Additive manufacturing is a manufacturing method in which individual powders are repeatedly melted and solidified to create a shape. Since the requirements for the particle size of the alloy powder vary depending on the additive manufacturing device, the particle size range of the Ni-based alloy powder can be set to 1 to 200 μm in order to be compatible with various manufacturing devices. For example, in the case of powder bed fusion (PBF), if the particle size of the Ni-based alloy powder is less than 1 μm, the flowability is reduced, making it difficult to obtain a sound additive manufacturing product. On the other hand, if the particle size of the Ni-based alloy powder exceeds 80 μm, the layer pitch must be set large, and the dimensional accuracy is reduced. Therefore, the particle size range of the Ni-based alloy powder for the powder bed fusion method can be 1 to 80 μm. Also, it is preferably 10 to 60 μm. In the case of Directed Energy Deposition (DED), if the particle size of the Ni-based alloy powder is less than 1 μm, the supply amount cannot be increased, and the modeling speed becomes slow. On the other hand, if the particle size of the Ni-based alloy powder exceeds 200 μm, the volume required for one melting and solidification is too large, and unmelted powder is likely to remain. Therefore, the particle size range of the Ni-based alloy powder for the Directed Energy Deposition method can be 20 to 200 μm. Also, it is preferably 40 to 120 μm. In addition, powder obtained by gas atomization, which can obtain a spherical shape, is preferable. Regarding the particle size of the powder, the particle size distribution can be measured by using a laser diffraction method (a laser diffraction type particle size distribution measuring device).

[0031] (Particle size distribution of Ni-based alloy powder) In additive manufacturing, if the powder particle size is too small, the powder layer will be worn off or biased, resulting in poor coating properties. On the other hand, if the powder particle size is too large, the laser output may be insufficient, resulting in residual melting, which tends to increase defects during stacking and reduce surface roughness. For this reason, in the cumulative distribution curve showing the relationship between the particle size determined by the laser diffraction method and the volume cumulative from the small particle size side, it is preferable that the particle diameter d10 corresponding to a cumulative frequency of 10 volume% is in the range of 10 μm to 25 μm, the particle diameter d50 corresponding to a cumulative frequency of 50 volume% is in the range of 25 μm to 40 μm, and the particle diameter d90 corresponding to a cumulative frequency of 90 volume% is in the range of 45 μm to 60 μm. Also, preferably, d10 is 15 μm or more and 20 μm or less, d50 is 30 μm or more and 35 μm or less, and d90 is 50 μm or more and 55 μm or less, and more preferably, d10 is 18 μm or more and 20 μm or less, d50 is 32 μm or more and 34 μm or less, and d90 is 53 μm or more and 55 μm or less.

[0032] (Uniformity of Ni-based alloy powder: 0.8~1.2) Regarding the particle size of the Ni-based alloy powder of the present invention, the numerical value expressed by (d90-d10) / d50 is defined as the uniformity. The larger the uniformity is than 1, the lower the spreading property is, and the smaller the uniformity is than 1, the lower the yield tends to be, and the lower the productivity is. For this reason, it is preferable that the lower limit of the uniformity is 0.8 and the upper limit is 1.2. Also, it is preferably 0.90 to 1.15, and more preferably 0.95 to 1.10.

[0033] (Angle of repose of Ni-based alloy powder: 40 degrees or less) In additive manufacturing, the powder as the raw material has better fluidity because it has better spreadability. The fluidity of the Ni-based alloy powder of the present invention is evaluated by the angle of repose according to JIS R9301-2-2. If the angle of repose exceeds 40 degrees, the fluidity is poor and the spreadability is reduced, so the angle of repose is preferably 40 degrees or less. There is no particular limit. The angle of repose is more preferably 35 degrees or less, and even more preferably 31 degrees or less. Moreover, the flowability of the Ni-based alloy powder having the above-mentioned angle of repose is preferably 15 sec / 50 g or more, more preferably 18 sec / 50 g or more, and further preferably 19 sec / 50 g or more.

[0034] [Method of manufacturing alloy powder] For example, a gas atomization method can be used as a method for producing Ni-based alloy powder (alloy powder). After raw material powders mixed to obtain a specified composition are melted in a crucible, the molten metal is discharged from the bottom of the crucible while high-pressure gas is sprayed onto the discharged molten metal. The kinetic energy of the high-pressure sprayed medium causes the molten metal to fly as droplets, which are then solidified to produce spherical Ni-based alloy powder. The crucible used in this process is preferably made of Al2O3 to prevent the inclusion of Zr impurities.

[0035] [Manufacturing method for additive manufacturing] The method for producing an additive manufacturing product of the present invention includes an additive manufacturing step of forming an additive manufacturing product using Ni-based alloy powder which contains, by mass%, 3.5-5.5% Al, 0.8-4.0% Cr, 0.02-0.06%, 1.0-1.8% Si, 1.5% or less Mn, 0.001-0.050% O, and the remainder Ni and unavoidable impurities, with Zr among the unavoidable impurities limited to 0.01% or less.

[0036] (Additive manufacturing process) The additive manufacturing method in the additive manufacturing process is not particularly limited. For example, the Ni-based alloy powder of the present invention is supplied to an additive manufacturing device of the powder bed fusion method (PBF), and the area where the powder is spread is irradiated with high energy such as a laser beam or an electron beam to selectively melt and bond the alloy powder, thereby additively manufacturing a molded product of a desired shape. The additive manufacturing device can be classified into a powder bed fusion method (PBF) and a directed energy deposition method (DED) according to the shape of the additive manufacturing product, but the additive manufacturing product of this embodiment can be manufactured by either method, and the type of the additive manufacturing device is not particularly limited.

[0037] (Heat treatment of additive manufacturing products) In the method for manufacturing an additive manufacturing product of the present invention, the molded product manufactured by the additive manufacturing method may be subjected to a solution heat treatment for the purpose of removing residual stress and reducing microsegregation. The temperature for the solution heat treatment is preferably 1000°C or higher to dissolve the microsegregation, and 1200°C or lower because it is necessary to be lower than the solidus temperature. More preferably, the temperature is 1050°C or higher and 1180°C or lower, and even more preferably, the temperature is 1100°C or higher and 1160°C or lower.

[0038] [Additive manufacturing products] The additive manufacturing product of the present invention contains, by mass%, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 1.8% Si, 1.5% or less Mn, 0.001 to 0.050% O, with the remainder being Ni and unavoidable impurities, the Zr contained in the unavoidable impurities being limited to 0.01% or less, the defect rate being 0.1% or less, and the unit area oxidation amount, which is obtained by an oxidation test performed in an atmospheric furnace at 800°C for 950 hours and is expressed as [mass loss before and after oxidation test] / [surface area before oxidation test], is 0.005 mg / mm 2The additive manufacturing product is characterized by having excellent high-temperature oxidation resistance due to the alumina coating formed on the surface layer. The application of the additive manufacturing product is not particularly limited, but for example, it is possible to provide a semiconductor manufacturing equipment member made of the additive manufacturing product. The additive manufacturing product has excellent high-temperature oxidation resistance, particularly at 700°C or higher, and an oxide coating on the surface is unlikely to grow even when used in a high-temperature environment. Therefore, when the additive manufacturing product is applied to a member or part to be installed inside an oxidation furnace for semiconductor manufacturing or a baking furnace for electronic component manufacturing, it is effective because it makes it difficult for oxides to peel off from the surface of the member or part, and it is possible to suppress the inclusion of foreign matter in products such as semiconductors and electronic components. In addition to semiconductor manufacturing equipment members, additive manufacturing products with good high-temperature oxidation resistance and complex shapes can be provided in a wide range of fields such as parts in the aviation industry, space industry, and automobile industry, chemical plants, pharmaceutical manufacturing equipment, and energy fields such as oil and gas.

[0039] (Amount of oxidation per unit area of ​​the AM product: 0.5mg / cm 2 below) The additive manufacturing product of the present invention has excellent resistance to high-temperature oxidation. Here, high-temperature oxidation resistance can be evaluated by the amount of oxidation per unit area expressed by (Equation 1). In a high-temperature oxidation test carried out in an atmospheric furnace at 800°C for 950 hours, the amount of oxidation per unit area was 0.5 mg / cm 2 If the amount of oxidation is less than 0.4 mg / cm2, the growth of the oxide film can be significantly suppressed. 2 The more preferable unit area oxidation amount is 0.3 mg / cm or less. 2 The following is the result.

[0040] [Unit area oxidation amount (mg / cm 2 )] = [Mass loss before and after oxidation test (mg)] / [Surface area before oxidation test (cm 2 )]...(Formula 1)

[0041] (Defect rate of additively manufactured products: 0.1% or less) Since internal defects in an AM product can be the starting point of cracks, it is desirable for the defect rate to be low. The defect rate can be measured as the area ratio of defective parts such as voids and unmelted powder. Details of the measurement conditions will be described later. If the defect rate is 0.1% or less, there are very few internal defects that can be the starting point of cracks, so the defect rate is set to 0.1% or less. In addition, a preferable defect rate is 0.05% or less, and a more preferable defect rate is 0.025% or less.

[0042] (Hardness of additively manufactured products: 210~300HV) In the layered product of the present invention, it is desirable that the tensile strength is high. Therefore, the hardness, which is proportional to the tensile strength, is set to 210HV or more. On the other hand, from the viewpoint of maintaining machinability and preventing cracking, the upper limit of the hardness is set to 300HV. In addition, the preferred range of hardness is 240 to 290HV, more preferably 260 to 280HV. Details of the measurement conditions, etc. will be described later. EXAMPLES

[0043] Examples of the present invention will be described below. First, as an example, alloy powder (hereinafter, simply referred to as powder) a with the composition shown in Table 1 was produced. In addition, alloy powders b to e with the composition shown in Table 1 were produced as comparative examples. A vacuum gas atomization method was used to produce the alloy powder. Raw material powders mixed to obtain the specified composition were melted in a high-frequency vacuum melting furnace, with alloy powders a, c, and e in an Al2O3 crucible, and alloy powders b and d in a ZrO2 crucible. Then, argon gas was sprayed onto the molten metal discharged from the bottom of the crucible to make it finer, and the molten metal was solidified in a cooling tower to obtain a spherical powder. The obtained powder was then classified to obtain alloy powders a to e with a particle size range of 10 to 60 μm.

[0044] [Table 1]

[0045] The chemical compositions of these alloy powders shown in Table 1 were analyzed, for example, by inductively coupled plasma (ICP) optical emission spectrometry. Comparing the component compositions of the example powders and the comparative example powders shown in Table 1, it can be seen that, compared to the example powder a, powder b has a decreased C content and an increased Zr content, powder c has decreased C and Si contents, powder d has an increased Zr content, and powder e has an increased Al content.

[0046] [Characteristics evaluation of Ni-based alloy powder] The fluidity, angle of repose, and hardness of the alloy powders a to e were measured, and the results are shown in Table 2. The measurement methods and conditions are described below.

[0047] (Particle size and flowability evaluation) The particle sizes d10, d50, and d90 were measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical: Master Sizer 3000). The measured d10, d50, and d90 were used to calculate the uniformity expressed as (d90-d10) / d50. Furthermore, the flowability of each powder was measured using a flowability measuring device (manufactured by Tsutsui Rikagaku Co., Ltd.) in accordance with JIS-Z2502.

[0048] (Angle of repose evaluation) The angle of repose was measured using a multi-function powder property measuring instrument (Seishin Co., Ltd.: Multitester MT-02). The measurement was performed in accordance with JIS R9301-2-2, specifically, the alloy powder was fed into a tray in the measuring instrument, and the angle of the formed peak was measured. At this time, a 355 μm sieve was used to feed the alloy powder.

[0049] (Hardness evaluation) After filling a hole with 2 mm in diameter with 1 g of alloy powder, the alloy powder was embedded in resin using a vacuum device for cold resin embedding (Struers: CitoVac). The alloy powder embedded in resin was polished to #1500 with waterproof emery paper, and then polished with diamond paste in the order of grain size 1 μm and 0.3 μm to a mirror finish to obtain a test piece for hardness evaluation. The Vickers hardness of the mirror-finished surface was measured using a micro Vickers hardness tester (FM-110 manufactured by Featuretec Co., Ltd.). Specifically, a square pyramid diamond indenter was pressed into a total of 10 points on powder particles with a particle size of 30 to 40 μm, and held for 15 seconds with a test load of 25 gf. The diagonal length of the depressions remaining on the surface was then measured to calculate the hardness, and the average value and standard deviation of the hardness at the 10 points of each test piece powder were obtained.

[0050] [Table 2]

[0051] The evaluation results of the fluidity, angle of repose, and hardness of powders a to e are shown in Table 2. Comparing the measurement results of the Examples and Comparative Examples, it was found that for the fluidity, which is also related to the spreading property, powder a satisfied the above-mentioned preferable ranges, and even more preferable ranges, for both the particle size distribution and the uniformity.

[0052] On the other hand, when comparing the hardness of each powder shown in Table 2, it can be seen that powder c has a lower hardness and powder e has a higher hardness than powders a, b, and d. It is presumed that the decrease in Si content of powder c has acted to reduce the powder hardness. Also, it is presumed that the increase in Al content of powder e has acted to improve the powder hardness. Also, although there is no clear significant difference in hardness between powders a, b, and d, the hardness of powders b and d has a high standard deviation and a large variance in the measured values, so it can be said that powder a, which is an example, can obtain a more stable hardness.

[0053] [Characteristic evaluation of additive manufacturing products] Additive manufacturing products (hereinafter also simply referred to as molded products) A to E were produced for each of the alloy powders a to e using an additive manufacturing device (M290 manufactured by EOS) for selective laser melting (SLM) using a laser as a heat source. The conditions for additive manufacturing are energy density of 20 to 200 J / mm 3In this embodiment, the parameters are set to 300 W laser power, 1000 mm / s scanning speed, 0.1 mm scanning pitch, and 0.04 mm layer thickness, and the energy density is 75 J / mm 3 It was.

[0054] [Energy density (J / mm 3 )] = [Laser power (W)] / ([Scanning speed (mm / s)] × [Scanning pitch (mm)] × [Layer thickness (mm)]) (Equation 2)

[0055] Additive manufacturing products A to E were produced as plate materials (25mm x 25mm x 5mm) and block materials (10mm x 10mm x 10mm). Additive manufacturing products A to E were evaluated for defect rate and hardness, and additive manufacturing products A to C were evaluated for high-temperature oxidation resistance. The results are shown in Table 3 and Figure 1. The measurement methods and conditions are described below.

[0056] (Defect Rate Evaluation) The cross sections of the block material (10mm x 10mm x 10mm) of the additively manufactured products A to E were cut and embedded in resin using a vacuum device for hot resin embedding (Struers: CitoPress-30). The additively manufactured products embedded in resin were polished to #1500 with waterproof emery paper, and then polished with diamond paste with grain sizes of 1μm and 0.3μm in that order to give them a mirror finish, obtaining test pieces for measuring the defect rate. The mirror-finished surface was checked for crack occurrence and the defect rate was measured using a digital microscope (Keyence Corp.: VHX-6000). If fine cracks were confirmed, the defect rate was not evaluated. The defect rate was measured at one location in the center of the mirror-finished surface and at four locations approximately 1 mm away from the center toward the four corners. For each measurement area, a surface image of 1.58 mm x 1.25 mm was obtained, and each acquired image was binarized to determine the area of ​​blackened voids and unmelted powder within 0.18 μm 2 The above-mentioned parts were identified as defective parts. The area ratio of the defective parts (defect rate) was then calculated, and the average value and standard deviation of the defect rate at five points in each test piece were obtained.

[0057] (Hardness evaluation) The Vickers hardness of the mirror-finished surface was measured using a micro Vickers hardness tester (FM-110 manufactured by Featuretec Co., Ltd.). The measurement area was one location at the center of the mirror-finished surface and four locations approximately 1 mm away from the center toward the four corners. Specifically, the specimen was pressed with a square pyramid diamond indenter and held for 15 seconds under a test load of 25 gf. The hardness was then calculated by measuring the diagonal length of the depression remaining on the surface, and the average value and standard deviation of the hardness at five points in each test piece were obtained.

[0058] [Table 3]

[0059] Table 3 shows the hardness (HV) and defect rate (area%) of the additively manufactured products. The measurement results show that the hardness of manufactured products A, D, and E is higher than that of manufactured products B and C. This is thought to be because manufactured products A, D, and E have a higher carbon content than manufactured products B and C.

[0060] The measurement results also showed that there were no fine cracks in the molded products A and C. Furthermore, the defect rate of the molded product A was 0.016%, and the defect rate of the molded product C was 0.026%, both of which were less than 0.1%, which was an extremely excellent result for a composition system with high weld crack susceptibility. This is because many of the defects in the composition system of Ni-based corrosion-resistant alloys containing Zr are originally cracks, and it is thought that the occurrence of cracks was prevented by limiting the Zr content of both alloy powders a and c to a low value of 0.01% or less. On the other hand, a large number of cracks occurred in the molded products B, D, and E. This is thought to be because the molded products B and D contain a large amount of Zr, and the molded product E contains an excessive amount of Al. It was also confirmed that the molded products A and C actually have a high internal density as additive molded products and have excellent additive moldability. However, the hardness of the molded product C is low, and there is a concern that the tensile strength of the molded product will also be low. In addition, for molded products B, D, and E, the defect rate could not be calculated due to the large number of cracks that occurred.

[0061] (Evaluation of high-temperature oxidation resistance) In order to evaluate the high-temperature oxidation resistance of molded products A and C, which did not develop cracks in the defect evaluation described above, as-formed materials were prepared for the plate-shaped molded products A and C. For comparison, as-formed materials were also prepared for molded product B as an example of a sample in which cracks developed. The surfaces of these plate materials were polished with waterproof emery paper up to #400, and then electrolytically polished. After electrolytic polishing, each plate material was degreased by applying ultrasonic vibration to acetone and holding it for 5 minutes to obtain high-temperature oxidation resistance test pieces. After measuring the mass of each test piece, it was held at 800°C in a small atmospheric furnace and the oxidation time was set to four stages of 250 hours, 500 hours, 750 hours, and 950 hours. The test piece was cooled to room temperature and the mass change amount was measured at each stage. The amount of oxidation per unit area (mg / cm2) for each test piece was calculated using the above (Equation 1). 2 The measurement results are shown in Figure 1.

[0062] From the high-temperature oxidation resistance test results shown in Figure 1, the unit area oxidation amount of the molded product A was 0.23 mg / cm even after 950 hours.2 On the other hand, the density of model B was maintained at 3.14 mg / cm 2 , and model C is 1.34 mg / cm 2 The amount of oxidation is significantly greater. It was confirmed that molded product A has extremely excellent high-temperature oxidation resistance, as the amount of oxidation per unit area was suppressed over a long period of time. This is believed to be because alloy powder a contains more Si than alloy powder c, which stabilizes the alumina coating that forms on the surface of molded product A and suppresses further oxidation. On the other hand, molded product B has a deteriorated high-temperature oxidation resistance because alloy powder b contains more Zr than alloy powders a and c, which causes Zr oxide to form and inhibits the formation of an alumina coating on the surface.

[0063] From the above test results, it was confirmed that alloy powder a, which is an embodiment of the Ni-based alloy powder for additive manufacturing of the present invention, has a composition that is superior in high-temperature oxidation resistance and has low cracking sensitivity compared to alloy powders b to e, which are comparative examples, and also has fluidity and hardness that are suitable for suppressing defects and for spreading during additive manufacturing. Furthermore, for the additively manufactured products produced using alloy powder a, it was confirmed that the manufactured product A of the embodiment was superior in hardness, defect rate, and high-temperature oxidation resistance compared to the manufactured products B to E of the comparative examples.

Claims

1. In mass percent, Al: 3.5-5.5%, Cr: 0.8-4.0%, C: 0.02-0.06%, Si: 1.0 to 1.8%, Mn: 1.5% or less, O: 0.001 to 0.050%, and the balance being Ni and unavoidable impurities, wherein Zr in the unavoidable impurities is limited to 0.01% or less.

2. In mass percent, Al: 3.6-5.0%, Cr: 1.5-3.0%, C: 0.03-0.05%, Si: 1.2-1.5%, Mn: 0.2-1.0%, O: 0.008-0.030% The Ni-based alloy powder for additive manufacturing according to claim 1 ,

3. The Ni-based alloy powder for additive manufacturing according to claim 1 or 2, characterized in that the Vickers hardness is in the range of 160 to 220 HV.

4. 3. The Ni-based alloy powder for additive manufacturing according to claim 1 or 2, characterized in that in an cumulative distribution curve showing the relationship between particle diameter and volume accumulation from the small particle diameter side, obtained by a laser diffraction method, the particle diameter d10 corresponding to a cumulative frequency of 10 volume % is 10 μm or more and 25 μm or less, the particle diameter d50 corresponding to a cumulative frequency of 50 volume % is 25 μm or more and 40 μm or less, and the particle diameter d90 corresponding to a cumulative frequency of 90 volume % is 45 μm or more and 60 μm or less.

5. The Ni-based alloy powder for additive manufacturing according to claim 4, characterized in that the uniformity represented by (d90-d10) / d50 is in the range of 0.8 to 1.

2.

6. The Ni-based alloy powder for additive manufacturing according to claim 1 or 2, characterized in that the angle of repose measured in accordance with JIS R9301-2-2 is 40 degrees or less.

7. In mass percent, Al: 3.5-5.5%, Cr: 0.8-4.0%, C: 0.02-0.06%, Si: 1.0 to 1.8%, Mn: 1.5% or less, O: 0.001-0.050% and the balance being Ni and unavoidable impurities, wherein Zr among the unavoidable impurities is limited to 0.01% or less.

8. In mass percent, Al: 3.5-5.5%, Cr: 0.8-4.0%, C: 0.02-0.06%, Si: 1.0 to 1.8%, Mn: 1.5% or less, O: 0.001 to 0.050%, The balance is Ni and unavoidable impurities, The Zr contained in the inevitable impurities is limited to 0.01% or less, The defect rate is 0.1% or less, and the amount of oxidation per unit area, calculated by performing an oxidation test for 950 hours in an atmospheric furnace at 800°C, expressed as [mass loss before and after oxidation test] / [surface area before oxidation test], is 0.005 mg / mm 2 That is: An additively manufactured product characterized by:

9. The additive manufacturing product according to claim 8, characterized in that the Vickers hardness is in the range of 210 to 300 HV.

Citation Information

Patent Citations

  • Fin and tube for high temperature heat exchanger

    JP2003262491A

  • Ni-BASED ALLOY EXCELLENT IN HOT FORGING PROPERTY, HIGH TEMPERATURE OXIDATION RESISTANCE AND HIGH TEMPERATURE HALOGEN GAS CORROSION PROPERTY AND MEMBER USING Ni-BASED ALLOY

    JP2014080675A

  • Ni-BASED SUPERALLOY POWDER FOR LAMINATE MOLDING

    JP2017036485A

  • Gamma-prime precipitation-strengthened nickel-base superalloys used in powder-based additive manufacturing processes

    JP2017508877A

  • Alloy powder for laminate molding, laminated molding, and laminate molding method

    JP2020152978A