Methods for manufacturing objects from composite materials and objects formed therefrom - Patents.com

Incorporating 2D nanomaterial platelets in the matrix of fiber/fabric-reinforced composites forms labyrinthine paths to prevent liquid permeation, enhancing structural integrity and extending the service life of composite materials.

JP7589877B2Active Publication Date: 2024-11-26ユニヴァーサル マター ジービーアール リミテッド
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023208405
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-04-09
Filing Date
2023-12-11
Publication Date
2024-11-26
Estimated Expiration
2039-04-09

AI Technical Summary

Technical Problem

Fiber/fabric-reinforced composite materials are prone to degradation due to water and liquid permeation, leading to reversible and irreversible changes and damage, such as hydrolysis, delamination, and loss of structural integrity, necessitating thicker sections to compensate for environmental conditions.

Method used

Incorporation of a proof coating with 2D nanomaterial platelets, such as graphene/graphite nanoplates, dispersed in the matrix to create labyrinthine paths that significantly reduce liquid penetration, maintaining structural integrity and extending the service life of composite materials.

Benefits of technology

The proof coating reduces liquid penetration rates, minimizing damage and allowing for lighter, more efficient designs with extended service life and reduced material usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589877000002
    Figure 0007589877000002
  • Figure 0007589877000001
    Figure 0007589877000001
Patent Text Reader

Abstract

To provide a method for manufacturing an object from fiber / fabric-reinforced composite material, and an object.SOLUTION: In a method of manufacturing an object 4 from a first layer of a proof coating 10, a first matrix, and a composite material 12 reinforced with fibers and reinforcing material, manufacturing steps include the steps of: (a) creating the first layer of the proof coating 10; and (b) laying up a mixture of the fiber and / or the fabric reinforcing material and the composite matrix to form a composite element 12. Here, the first layer of the proof coating 10 is applied to a mold 2 or a support, followed by step (b), the lay-up is performed on the surface of the first layer of the proof coating 10 of step (a). The proof coating 10 is composed of a second matrix having 2D nanomaterial platelets dispersed therein.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to composite materials, and in particular to applications involving fiber / fabric reinforced composite materials having improved service life compared to known fiber / fabric reinforced composite materials. [Background technology]

[0002] Fiber / fabric reinforced composites are well known and consist of fibers and / or fabrics bonded in a matrix. The most well-known fibers and fabrics used in composites are glass fibers and fabrics or fabrics made from glass fibers, and carbon fibers and fabrics or fabrics made from carbon fibers. However, other types of fibers and fabrics made therefrom, both man-made and organic, are known to be used in fiber and / or fabric reinforced composites. Multiple types of fibers and / or fabrics can be used in composites. The choice of fiber(s) and / or fabric(s) used in a composite is often dictated by mechanical requirements or economics. Summary of the Invention [Problem to be solved by the invention]

[0003] The matrix of a fiber and / or fabric reinforced composite is typically a polyester resin, a vinyl ester resin, or an epoxy resin. The choice of the type of resin used will depend, at least in part, on the proposed use of the object to be made from the composite, the desired mechanical properties of the composite, and the differing costs of various resins. The matrix is ​​combined with the fiber and / or fabric reinforcement by known techniques, and when the matrix cures, the fiber and / or fabric reinforcement is bonded within the matrix.

[0004] Objects made from fiber and / or fabric reinforced composite materials also often include a coating of gelcoat covering at least one surface of the object. Typically, the gelcoat covers the surface or surfaces of the object that are expected to be exposed to the most adverse environmental conditions. Such adverse environmental conditions include, but are not limited to, exposure to liquids such as water, which may be constant (e.g., the hull of a boat) or intermittent (e.g., a bath or liquid storage tank).

[0005] Gelcoats are typically thermosetting polymers based on epoxy or unsaturated polyester resin chemistry and may contain pigments for aesthetic reasons. Gelcoats are designed to be durable and provide resistance to UV degradation and hydrolysis, but do not significantly affect the structural properties of the composite.

[0006] Fiber and / or fabric reinforced composite materials are the materials of choice for many applications because objects and structures made from such materials can be made with less weight and fewer components than traditional building materials such as metals. The mechanical properties of such composites are determined by the strength and stiffness of the fiber and / or fabric reinforcement, the strength and stiffness of the matrix, the strength of the interface between the fiber or fabric and the matrix, and environmental conditions such as temperature.

[0007] An object or structure made from fiber and / or fabric reinforced composite materials, during use or installation, is typically exposed to one or more environmental conditions that can degrade the mechanical integrity of the material immediately or over time. Such environmental conditions must be considered when designing the object or structure and the composite material from which the object or structure is manufactured. Typically, this results in a design that utilizes higher performance materials or thicker sections than necessary to allow for degradation of the mechanical performance of the composite material as a result of the environmental conditions.

[0008] A typical environmental condition that can affect the mechanical properties of fiber and / or fabric reinforced composites is exposure to water and / or other liquids, especially if such exposure is frequent or prolonged, since the materials that make up the matrix and gel coat are permeable and water and other liquids can migrate through the material over time.

[0009] Fiber- or fabric-reinforced composites often contain free volume or voids. These voids can be the result of manufacturing defects such as inter- and intra-molecular gaps in the matrix and / or gelcoat, trapped air bubbles, cracks, and / or dry fibers and / or fabrics (i.e., fibers and / or fabrics that are not saturated with the matrix material). When water or other liquids permeate the matrix or gelcoat, they accumulate in these voids.

[0010] The presence and accumulation of water and / or other liquids within a fiber and / or fabric reinforced composite structure is expected to result in reversible and irreversible changes and / or damage to the fibers and / or fabric, the matrix, and / or the interface between the fibers and / or fabric and the matrix.

[0011] In the case of matrices, the reversible changes that can occur are: Swelling of the matrix material; and the irreversible changes / damage that may occur are: · Chemical decomposition of the matrix through the process of hydrolysis; · Chemical destruction of the matrix due to swelling and stress-induced effects related to the applied stress; · Changes in chemical composition to the matrix material due to leaching; · Formation of surface cracks and fissures as a result of uneven shrinkage following water uptake and loss.

[0012] In the case of textiles and / or fabrics, irreversible changes / damage that may occur are: · Corrosion resulting in loss of strength; · Leaching leading to loss of strength.

[0013] In the case of the interface between the fibres and / or fabric and the matrix, the reversible changes that may occur are: · Plasticization / increased flexibility of the fiber surface and / or matrix adjacent to the fiber and / or fabric surface, resulting in loss of strength of the bond between the matrix and the fiber and / or fabric; and the irreversible changes / damage that may occur are: · Chemical breakdown of matrix / fiber and / or fabric bonds through the process of hydrolysis; Spalling due to internally generated stresses associated with expansion and contraction.

[0014] Hydrolysis is particularly damaging to fiber and / or fabric reinforced composites because when water and / or other liquids enter the voids of a composite, the water soluble materials in or adjacent to the voids go into solution with the water. This creates an osmotic pressure gradient between the solution in the voids and the water at the surface of the composite. As a result, more water is drawn into the voids as a result of infiltration. This can cause the solution to exert pressure on the composite, resulting in delamination and / or blistering of the composite.

[0015] The damaging effects of water and / or other liquids increase with increasing temperature.

[0016] The steps typically involved in the manufacture of objects from fiber and / or fabric reinforced composite materials are known and depend, at least in part, on the nature of the object being manufactured and the matrix and fiber and / or fabric reinforcement used. The object being manufactured may be a mould for use in the manufacture of other objects or products, a product, or a structure. Examples of such products may include, without limiting the fields in which the invention is useful, structural parts of boats, road vehicles, airplanes; liquid containment vessels such as storage tanks, baths, hot tubs, swimming pools, and the like; and turbine blades.

[0017] Some steps typically involved in the manufacture of objects from fiber and / or fabric reinforced composite materials are:

[0018] A mould is obtained that is suitable for use in moulding the composite material. The mould can be male or female. In a male mould, the composite material is formed around the outside of the mould. In a female mould, the composite material is formed inside the mould.

[0019] A release agent is applied to the surfaces of the mold in which the composite material is formed. Such release agents are known.

[0020] The surface of the mold on which the composite material is formed may optionally have one or more coatings of gelcoat applied thereto. Typically application is by brushing, rolling, or spraying. The desired thickness of the gelcoat is typically between 0.30 mm and 0.56 mm (0.012 inches to 0.022 inches), although other thicknesses may be suitable. The gelcoat is then allowed to cure. For clarity of expression, it should be understood that the outer surface or exterior of the gelcoat is adjacent the surface of the mold, and that the inner surface or interior of the gelcoat is remote from the surface of the mold.

[0021] If a gel coat is applied, once fully cured, a fiber layup and / or fabric reinforcement is applied on the inner surface of the gel coat using known techniques. If a gel coat is not used, a fiber layup and / or fabric reinforcement is applied on the surface of the mold using known techniques.

[0022] The fiber and / or fabric reinforcement may be in the form of a prepreg (a fiber and / or fabric reinforcement impregnated with a matrix ready for curing by application of suitable curing conditions, e.g., a sufficiently high temperature), or in the form of fibers and / or fabric to which a liquid matrix has been applied before being placed in place, or to which a liquid matrix has been applied after the fibers and / or fabric have been placed in place. Sufficient fibers and / or fabric are used to achieve the desired thickness of the composite.

[0023] Once all of the fibers and / or fabrics are in place, the matrix is ​​cured or exposed to curing conditions depending on the particular matrix used.

[0024] Once the matrix has hardened, the object is removed from the mold and may be ready for use or may require further processing. [Means for solving the problem]

[0025] According to a first aspect of the invention, there is provided a method for manufacturing an object from a fiber and / or fabric reinforced composite material comprising at least one first layer of a proof coating, a first or composite matrix, and one or more fiber and / or fabric reinforcing materials, the manufacturing steps comprising: a) forming a first layer of one of said proof coatings; and b) laying up a mixture of said fiber and / or fabric reinforcing material and said composite matrix forming a composite element; Where: (i) step (a) is first performed, in which the first layer of the proof coating is applied to a mould or support, followed by step (b), in which a lay-up is performed on the surface of the first layer of the proof coating of step (a); or (ii) step (b) is carried out first, in which a lay-up is carried out on a mould or support, followed by step (a), in which the first layer of the proof coating is applied to at least one surface of the composite element of step (b). The proof coating is characterized by comprising a second matrix having 2D nanomaterial platelets dispersed therein.

[0026] In some embodiments of the invention, the 2D nanomaterial platelets of the proof coating comprise one or a mixture of graphene nanoplates and graphite flakes, where the graphite flakes have a nanoscale dimension and 35 or fewer atomic layers (simply referred to as "layers"). In some embodiments, the graphene nanoplates comprise one or a mixture of two or more of graphene, graphene oxide, and / or reduced graphene oxide nanoplates, bilayer graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets, and few-layer graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets.

[0027] In some embodiments of the invention, the 2D nanomaterial platelets comprise one or a mixture of graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have one nanoscale dimension and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS2) nanoplates, tungsten diselenide (WSe2) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphyne (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, or 2D in-plane heterostructures of two or more of the foregoing materials.

[0028] In some embodiments of the invention, the 2D nanomaterial comprises a layered 2D material, which comprises graphite flakes, where the graphite flakes have dimensions of one nanoscale and 35 or fewer layers, one or a mixture of multi-layer graphene (C) nanoplates, multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS2) nanoplates, multi-layer tungsten diselenide (WSe2) nanoplates, multi-layer silicene (Si) nanoplates, multi-layer germanene (Ge) nanoplates, multi-layer graphene (C) nanoplates, multi-layer borophene (B) nanoplates, multi-layer phosphorene (P) nanoplates, or a 2D vertical heterostructure in-plane heterostructure of two or more of the aforementioned materials.

[0029] As noted above, epoxy resins and other materials suitable for use as composite matrices in the present invention will become saturated with water after a relatively short period of exposure to water or moisture. This can exacerbate the hydrolytic effects on the composite material. The mechanisms of hydrolysis are well known and need not be discussed here.

[0030] General studies on graphene have shown that graphene films can effectively isolate the metal substrate on which they are deposited from the environment. Single atom and defect-free films of graphene have been shown to be impermeable to gases, water, and the dissolved gases and ions in that water. However, the defect density is less than 1 um. -2 It has been estimated that water transport through graphene can occur at velocities greater than 1 m / s (>1 m / s) in the case of . Such mass transport rates could explain the observed corrosion effects on metals.

[0031] Graphene comes in many forms, and the growth of films by Chemical Vapor Deposition (CVD) is well understood and can produce graphene films of 1-3 atomic layers. Such films are used in most experiments related to graphene. Such techniques have limited commercial applicability as they allow only to create relatively small areas of film or to coat a substrate. In commercial applications, it is more common for graphene to be used in the form of graphene nanoplates (also called nanoplatelets). Graphene nanoplatelets can be produced either by exfoliation of graphite or by synthetic solvothermal processes. Such graphene nanoplatelets vary in number of atomic layers, surface area, functionality, and sp 2 The amount of carbon atoms in the graphite flakes may vary substantially. Such variations affect the physical properties of the graphene, such as the electrical conductivity of the graphene. Similarly, graphite flakes having nanoscale dimensions and 40 or fewer layers of carbon atoms, graphite flakes having nanoscale dimensions and 25-30 layers of carbon atoms, graphite flakes having nanoscale dimensions and 20-35 layers of carbon atoms, graphite flakes having nanoscale dimensions and 25-35 layers of carbon atoms, or graphite flakes having nanoscale dimensions and 20-40 layers of carbon atoms can be produced by either graphite exfoliation or synthetic solvothermal processes.

[0032] Epoxy resins and other materials suitable for use as the second matrix of the present invention become saturated with water and / or other liquids after a relatively short period of exposure to water, moisture, and / or other liquids.

[0033] The dispersion of 2D nanomaterial platelets in the second matrix to form the proof coating of the present invention will result in multiple layers of 2D nanomaterial platelets within the proof coating layer, depending on the applied dry film thickness of that layer. Each platelet is potentially several atomic layers thick. The presence of multiple layers of 2D nanomaterial platelets in the proof coating provides a complex and tortuous (maze-like) path for water and other liquids to penetrate. This maze-like path significantly reduces the diffusion rate of water and / or other liquids and substances dissolved in water through the second matrix and thus across the proof coating layer. This is evidenced by the results of testing the water vapor transmission rate of coatings including two commercially available graphene / graphite platelets (A-GNP35 with 6-14 layers of carbon atoms and A-GNP10 with 25-35 layers of carbon atoms, both available from Applied Graphene Materials Plc) and a control. The results are shown in Table 1 below. [Table 1]

[0034] Graphene / graphite platelets are typically 0.3 nm to 12 nm thick with lateral dimensions ranging from about 100 nm to 100 μm. As a result, and due to the large lateral aspect and surface area of ​​the graphene / graphite platelets, a coating layer comprised of graphene / graphite platelets dispersed in a second matrix can be relatively thin. As a result, the coating is unlikely to significantly affect the mechanical properties of the composite elements of the present invention.

[0035] In some embodiments of the present invention, the 2D nanomaterial platelets are graphene / graphite platelets and have a D50 particle size as measured by Mastersizer 3000 of less than 45 μm, less than 30 μm, or less than 15 μm.

[0036] An advantage of employing the manufacturing method according to the first aspect of the invention is that the rate of penetration of water or other liquids into the composite material or structural elements of the object to be manufactured, into the fibers and / or fabrics bonded to the composite material matrix, is significantly reduced. This has the effect that damage to the structural properties of the object by water and / or other liquids is also significantly reduced. This leads to an increased lifespan of the object manufactured using the manufacturing method according to the first aspect of the invention. This allows the designer of the object to include less material in the design, since he does not have to compensate for the expected damage from water and other liquids. The use of less material leads to less material used in the object with environmental and economic benefits that it brings. It also leads to a lighter object, which is also likely to lead to environmental and economic benefits.

[0037] In some embodiments of the first aspect of the present invention, the manufacturing step comprises: c) forming a layer of said gel coat; Further comprising: (iii) step (c) is performed first, in which the gel coat is applied to a mould or substrate, followed by step (a), in which the proof coating is formed on a surface of the gel coat, followed by step (b), in which a lay-up is performed on the free surface of the proof coating; or (iv) step (b) is performed first, in which a lay-up is performed on a mould or support, followed by step (a), in which the first layer of the proof coating is applied to at least one surface of the composite element of step (b), followed by step (c), in which the gel coat is applied to a free surface of the proof coating.

[0038] A free surface of a coating, layer, or composite element is one that is not covered by the coating, layer, or composite element.

[0039] Gel coats are known to be permeable, especially as the gel coat ages, but the use of the gel coat helps to physically protect the proof coating layer, so inclusion of the gel coat layer is beneficial in these embodiments. The use of the gel coat also provides aesthetic benefits in terms of color and surface finish. An additional benefit of the gel coat layer is that it becomes permeable, but where permeability limits the flow rate of water or other liquids.

[0040] It is known that there are several methods for manufacturing objects from composite materials. In general, however, all of these currently known techniques result in objects whose structural elements are fibers and / or fabrics bonded to a matrix. The structural elements tend to be weakened by the penetration of water and / or other liquids. The manufacturing method of the first aspect of the invention includes the incorporation of at least one proof coating layer that acts as a barrier against the penetration of water or other liquids into the fibers and / or fabrics bonded to the matrix.

[0041] In some embodiments of the first aspect of the invention, the manufacturing step includes creating at least two layers of a proof coating. In some of these embodiments, the manufacturing step includes creating a second, and optionally further, layer of the proof coating, where each layer of the proof coating overlays a different surface of the composite element.

[0042] These embodiments are particularly beneficial when more than one surface of the object being manufactured is expected to be exposed to water and / or other liquids. In some embodiments, the application methods of the first and second proof coating layers may be different to suit the nature of the fibers and / or fabrics bonded to the composite matrix and the exact manufacturing method.

[0043] In some embodiments of the first aspect of the invention, the manufacturing step further comprises overlaying at least one proof coating layer with at least one further proof coating layer. The proofing layers may be of different composition relative to each other. This approach provides greater resistance to penetration by water or other liquids than a single proof coating layer. The proof coating layers may be separated from each other by an intermediate layer. The intermediate layer may be of a material suitable for use in separating the proof coating layers.

[0044] In some embodiments of the first aspect of the invention, the or each layer of the proof coating is created by brushing, spraying, or printing. The proof coating may be applied to the surface of a mold, the surface of a gel coat layer, or the surface of fibers and / or fabrics bonded to a composite matrix, which may be in the form of a prepreg, tape, or tow, or fiber, and where the manufacturing methods include prepreg layup, hand layup automated tape layup, filament winding, resin transfer molding (RTM) including flexible RTM, continuous RTM, vacuum assisted RTM, high speed RTM, and pultrusion. Similarly, the proof coating may be applied to the surface of a mold, the surface of a gel coat layer of a composite product manufactured using short or discontinuous fibers, and where the manufacturing methods include chopped strand spray layup, sheet molding compound, and bulk molding compound.

[0045] In some embodiments of the first aspect of the present invention, the proof coating layer has a thickness in the range of 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 30 μm, 25 μm to 100 μm, or 40 μm to 60 μm.

[0046] In some embodiments of the first aspect of the present invention, the proof coating comprises 0.1% to 0.5% by weight of the 2D nanomaterial platelets.

[0047] In some embodiments of the first aspect of the present invention, the composite matrix is ​​comprised of one or more thermoset matrices, unsaturated polyester resins, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic polyester resins, vinyl ester resins, epoxy resins, cyanate esters, bismaleimides, urethane acrylates, phenolic, furan or poly(furfural alcohol), polyimides, benzoxazines, and mixtures and combinations thereof.

[0048] In some embodiments of the first aspect of the present invention, the second matrix is ​​comprised of suitable crosslinkable resins, epoxy resins, polyester resins, vinyl ester resins, acrylics, aminoplasts, urethanes, carbamates, alkyds, silicones, polyureas, silicates, polydimethylsiloxanes, vinyl esters, unsaturated polyesters, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic acid polyester resins, phenolics, furan or poly(furfuryl alcohol), polyimides, benzoxazines, and suitable non-crosslinkable resin mixtures and combinations thereof.

[0049] In some embodiments of the first aspect of the present invention, the proof coating further comprises a hardener. Such hardeners are known and ensure that the second matrix in the proof coating is properly hardened.

[0050] According to a second aspect of the invention, there is provided an object constructed from a fibre and / or fabric reinforced composite material, characterised in that the object is composed of a composite element and a proof coating layer, where the composite element is formed from a mixture of a fibre and / or fabric reinforcement material and a composite matrix, and the proof coating is composed of a second matrix having 2D nanomaterial platelets dispersed therein.

[0051] In some embodiments of the present invention, the 2D nanomaterial platelets of the proof coating comprise one or a mixture of graphene nanoplates and graphite flakes, where the graphite flakes have a nanoscale dimension and 35 or fewer atomic layers (simply referred to as "layers"). In some embodiments, the graphene nanoplates comprise one or a mixture of two or more of graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets, bilayer graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets, and few layer graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets.

[0052] In some embodiments of the invention, the 2D nanomaterial platelets comprise one or a mixture of graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have one nanoscale dimension and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS2) nanoplates, tungsten diselenide (WSe2) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphyne (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, or 2D in-plane heterostructures of two or more of the foregoing materials.

[0053] In some embodiments of the invention, the 2D nanomaterial comprises a layered 2D material, which comprises graphite flakes, where the graphite flakes have dimensions of one nanoscale and 35 or fewer layers, one or a mixture of multi-layer graphene (C) nanoplates, multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS2) nanoplates, multi-layer tungsten diselenide (WSe2) nanoplates, multi-layer silicene (Si) nanoplates, multi-layer germanene (Ge) nanoplates, multi-layer graphene (C) nanoplates, multi-layer borophene (B) nanoplates, multi-layer phosphorene (P) nanoplates, or a 2D vertical heterostructure in-plane heterostructure of two or more of the aforementioned materials.

[0054] An object according to the second aspect of the invention has the same advantages and benefits as an object made according to the method of the first aspect of the invention.

[0055] In some embodiments of the second aspect of the present invention, the article further comprises a layer of gel coat, and wherein the proof coating layer is between the gel coat layer and the composite element.

[0056] In some embodiments of the second aspect of the present invention, the article comprises at least two proof coating layers.

[0057] In some embodiments of the second aspect of the present invention, the article includes a second proof coating layer, where the first and second proof coating layers overlie the first and second surfaces of the composite element.

[0058] In some embodiments of the second aspect of the present invention, each proof coating layer is applied by brushing, spraying, or printing.

[0059] In some embodiments of the second aspect of the present invention, the proof coating layer has a thickness in the range of 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 30 μm, 25 μm to 100 μm, or 40 μm to 60 μm, 25 μm to 100 μm, or 40 μm to 60 μm.

[0060] In some embodiments of the second aspect of the present invention, the proof coating comprises between 0.1% and 0.5% by weight of the 2D nanomaterial platelets.

[0061] In some embodiments of the second aspect of the invention, the composite matrix is ​​comprised of one or more thermoset matrices, unsaturated polyester resins, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic polyester resins, vinyl ester resins, epoxy resins, cyanate esters, bismaleimides, urethane acrylates, phenolic, furan or poly(furfural alcohol), polyimides, benzoxazines, and mixtures and combinations thereof.

[0062] In some embodiments of the second aspect of the invention, the second matrix is ​​comprised of suitable crosslinkable resins, epoxy resins, polyester resins, vinyl ester resins, acrylics, aminoplasts, urethanes, carbamates, alkyds, silicones, polyureas, silicates, polydimethylsiloxanes, vinyl esters, unsaturated polyesters, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic polyester resins, phenolics, furans or poly(furfuryl alcohol), polyimides, benzoxazines, and suitable non-crosslinkable resins, mixtures thereof, and combinations thereof.

[0063] In some embodiments of the second aspect of the present invention, the proof coating further comprises a hardener.

[0064] In some embodiments of the second aspect of the invention, the object is a mould for use in making an object from a composite material.

[0065] According to a third aspect of the present invention there is provided a proof coating for use in a manufacturing method according to the first aspect of the present invention and an object according to the second aspect of the present invention characterised in that the proof coating comprises 0.1 wt% to 0.5 wt% of 2D nanomaterial platelets.

[0066] In some embodiments of the present invention, the 2D nanomaterial platelets of the proof coating comprise one or a mixture of graphene nanoplates and graphite flakes, where the graphite flakes have a nanoscale dimension and 35 or fewer atomic layers (simply referred to as "layers"). In some embodiments, the graphene nanoplates comprise one or a mixture of two or more of graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets, bilayer graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets, and few layer graphene, graphene oxide, and / or reduced graphene oxide nanoplatelets.

[0067] In some embodiments of the invention, the 2D nanomaterial platelets comprise one or a mixture of graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have one nanoscale dimension and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS2) nanoplates, tungsten diselenide (WSe2) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphyne (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, or 2D in-plane heterostructures of two or more of the foregoing materials.

[0068] In some embodiments of the invention, the 2D nanomaterial comprises a layered 2D material, which comprises graphite flakes, where the graphite flakes have dimensions of one nanoscale and 35 or fewer layers, one or a mixture of multi-layer graphene (C) nanoplates, multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS2) nanoplates, multi-layer tungsten diselenide (WSe2) nanoplates, multi-layer silicene (Si) nanoplates, multi-layer germanene (Ge) nanoplates, multi-layer graphene (C) nanoplates, multi-layer borophene (B) nanoplates, multi-layer phosphorene (P) nanoplates, or a 2D vertical heterostructure in-plane heterostructure of two or more of the aforementioned materials.

[0069] An object produced using a proof coating according to the third aspect of the invention has the same advantages and benefits as an object produced according to the method of the first aspect of the invention.

[0070] In some embodiments of the third aspect of the invention, the proof coating is composed of 0.1 wt% to 0.5 wt% graphene / graphite nanoplates consisting of 6-14 layers of carbon atoms, or graphite flakes with nanoscale dimensions and 25-35 layers of carbon atoms.

[0071] In some embodiments of the third aspect of the invention, the second matrix is ​​comprised of suitable crosslinkable resins, epoxy resins, polyester resins, vinyl ester resins, acrylics, aminoplasts, urethanes, carbamates, alkyds, silicones, polyureas, silicates, polydimethylsiloxanes, vinyl esters, unsaturated polyesters, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic polyester resins, phenolics, furans or poly(furfuryl alcohol), polyimides, benzoxazines, and suitable non-crosslinkable resins, mixtures thereof, and combinations thereof.

[0072] In some embodiments of the third aspect of the present invention, the proof coating further comprises a hardener.

[0073] According to a fourth aspect of the present invention there is provided the use of a proof coating according to the manufacturing method according to the first aspect of the present invention.

[0074] According to a fifth aspect of the invention there is provided a kit comprising a quantity of a proof coating according to the fourth aspect of the invention and instructions for use of the proof coating in a manufacturing method according to the first aspect of the invention. [Brief description of the drawings]

[0075] The invention will be further described and illustrated, by way of example, with reference to the accompanying drawings, in which: [Figure 1] FIG. 1 now shows a schematic partial cross-sectional view of an embodiment of a mould and an object according to the invention within said mould. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0076] With reference to the figure, there is shown a partial cross-section of a mould 2. Within the mould is an object 4 made from a composite material.

[0077] The object 4 is created or manufactured in the following way: A layer of release agent 6 is applied to the interior surface of mold 2 using a spray applicator. This allows for easy removal of the finished object 4 from mold 2. Release agent 6 is a commercially available release agent suitable for use in conjunction with gel coat 8 compositions.

[0078] A spray applicator is used to apply a layer of gel coat 8 to the surface or face of the layer of release agent 6, away from the form 2. The layer of gel coat 8 is allowed to at least partially cure. The gel coat layer 8 is any commercially available gel coat suitable for use in conjunction with the composition of the proof coating 10.

[0079] Once the layer of gel coat 8 is at least partially cured, a layer of proof coating 10 is applied using a brush to the side of gel coat layer 8 away from form 2. The proof coating layer 10 is allowed to at least partially cure. The proof coating 10 is comprised of a second matrix in the form of an epoxy resin in which 0.1 wt% to 0.5 wt% of graphene / graphite nanoplates or graphite flakes with nanoscale dimensions of 6-14 layers of carbon atoms and 25-35 layers of carbon atoms are dispersed. The dried / cured thickness of the proof coating layer 10 is between 5 μm and 50 μm.

[0080] Once the proof coating layer 10 is at least partially cured, reinforcing fibers mixed with a composite matrix to create a composite material 12 are placed against the face of the proof coating layer 10 away from the form 2 using known hand layup techniques. The composite layer 12 is allowed to at least partially cure. The reinforcing fibers are carbon fibers and the composite matrix is ​​a resin selected to impart the desired mechanical properties to the object 4. The materials of the first and second matrices can be the same, but are likely different given the different roles of each matrix.

[0081] Once the composite layer 12 is at least partially cured, a second proof coating layer 14 is applied to the surface of the composite layer 12 remote from the mold 2. The second proof coating layer 14 is applied by spraying and is of the same composition as the first proof coating layer 10. Again, the average thickness of the second proof coating layer 14 was between 5 μm and 50 μm.

[0082] Once all layers have hardened sufficiently so that the object 4 can be removed from the mould 2 without damage, it is removed from the mould 2 .

[0083] If the object 4 does not include a gel coat 8 , a first proof coating layer 10 is applied to the surface of the mold 2 .

[0084] It is understood that for other manufacturing methods, the proof coating may be applied to the surface of continuous fibers and / or fabrics bonded in a composite matrix, which may be in the form of prepregs, tapes, or tows or fibers, and where the manufacturing methods include prepreg layup, hand layup automated tape layup, filament winding, resin transfer molding (RTM) including flexible RTM, continuous RTM, vacuum assisted RTM, high speed RTM, and pultrusion.

[0085] It is expressly intended that within the scope of this application, the various aspects, embodiments, examples and alternatives described in the preceding paragraphs and / or claims, in particular their individual features, can be taken independently or in any combination. That is, all embodiments and / or features of any embodiment can be combined in any manner and / or combination, except where such features are incompatible. Applicant reserves the right to modify the originally filed claims or to file new claims accordingly, including the right to amend the originally filed claims to depend on and / or incorporate features of other claims.

[0086] Claim 1 1. A method of manufacturing an object from a fiber and / or fabric reinforced composite material comprising at least a first layer of a proof coating, a first or composite matrix, and one or more fiber and / or fabric reinforcement materials, the manufacturing step comprising: a) forming a first layer of one of said proof coatings; and b) laying up a mixture of said fiber and / or fabric reinforcing material and said composite matrix forming a composite element; Including, Where: (i) step (a) is performed first, in which the first layer of the proof coating is applied to a mold or substrate, followed by step (b), in which a lay-up is performed on the surface of the first layer of the proof coating of step (a); or (ii) step (b) is carried out first, in which a lay-up is carried out on a mould or support, followed by step (a), in which the first layer of the proof coating is applied to at least one surface of the composite element of step (b); It is characterized by: The method, wherein the proof coating comprises a second matrix having 2D nanomaterial platelets dispersed therein. Claim 2 2. The method of claim 1, wherein the 2D nanomaterial platelets of the proof coating comprise one or a mixture of graphene nanoplates and graphite flakes, the graphite flakes having dimensions on the nanoscale and 35 or fewer atomic layers. Claim 3 The 2D nanomaterial platelets may be graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have dimensions of 1 nanoscale and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS2) nanoplates, tungsten diselenide (WSe2) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphene (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, multi-layer graphene ( 3. The method of claim 1 or 2, wherein the nanoplates comprise one or a mixture of the following: multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS2) nanoplates, multi-layer tungsten diselenide (WSe2) nanoplates, multi-layer silicene (Si) nanoplates, multi-layer germanene (Ge) nanoplates, multi-layer graphene (C) nanoplates, multi-layer borophene (B) nanoplates, multi-layer phosphorene (P) nanoplates, or 2D in-plane or vertical heterostructures of two or more of the foregoing materials. Claim 4 The manufacturing steps are c) forming a layer of gel coat; 4. The method of claim 1, further comprising: Where: (iii) step (c) is performed first, in which the gel coat is applied to a mould or substrate, followed by step (a), in which the proof coating is formed on a surface of the gel coat, followed by step (b), in which a lay-up is performed on the free surface of the proof coating; or (iv) A method in which step (b) is first performed, in which a lay-up is performed on a mould or support, followed by step (a), in which the first layer of the proof coating is applied to at least one surface of the composite element of step (b), followed by step (c), in which the gel coat is applied to a free surface of the proof coating. Claim 5 The method of any of claims 1 to 4, wherein the manufacturing step further comprises forming at least two proof coating layers. Claim 6 The method of claim 5 , wherein the manufacturing step further comprises at least two proof coating layers covering different surfaces of the composite element. Claim 7 7. The method of claim 5 or 6, wherein the manufacturing step further comprises overlaying the at least one proof coating layer with a further proof coating layer. Claim 8 8. The method according to claim 1, wherein the layer of proof coating is applied by brushing, spraying or printing. Claim 9 9. The method of claim 1, wherein the proof coating layer has a dry thickness in the range of 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 30 μm, 25 μm to 100 μm, or 40 μm to 60 μm, 25 μm to 100 μm, 40 μm to 60 μm. Claim 10 10. The method of any of claims 1 to 9, wherein the proof coating is composed of 0.1% to 0.5% by weight of 2D nanomaterial platelets. Claim 11 11. The method of any of claims 1 to 10, wherein the composite matrix is ​​comprised of one or more thermoset matrices, unsaturated polyester resins, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic acid polyester resins, vinyl ester resins, epoxy resins, cyanate esters, bismaleimides, urethane acrylates, phenols, furans or poly(furfural alcohols), polyimides, benzoxazines, and mixtures and combinations thereof. Claim 12 12. The method of any of claims 1 to 11, wherein the second matrix is ​​comprised of one or more of crosslinkable resins, epoxy resins, polyester resins, vinyl ester resins, acrylics, aminoplasts, urethanes, carbamates, alkyds, silicones, polyureas, silicates, polydimethylsiloxanes, vinyl esters, unsaturated polyesters, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic acid polyester resins, phenols, furans or poly(furfuryl alcohol), polyimides, benzoxazines, and non-crosslinkable resins. Claim 13 The method of any one of claims 1 to 12, wherein the proof coating further comprises a hardener. Claim 14 An object constructed at least in part from a fiber and / or fabric reinforced composite material, the object being composed of at least one first proof coating layer, a first or composite matrix, and a fiber and / or fabric reinforcing material, wherein the fiber and / or fabric reinforcing material and the composite matrix form a composite element, and wherein the proof coating is composed of a second matrix having 2D nanomaterial platelets dispersed therein. Claim 15 15. The article of claim 14, wherein the 2D nanomaterial platelets of the proof coating comprise one or a mixture of graphene nanoplates and graphite flakes, the graphite flakes having a nanoscale dimension and 35 or fewer atomic layers. Claim 16 The 2D nanomaterial platelets can be graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have dimensions of 1 nanoscale and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS2) nanoplates, tungsten diselenide (WSe2) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphene (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, multi-layer graphene (C 16. The article of claim 14 or 15, comprising one or a mixture of the following: multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS2) nanoplates, multi-layer tungsten diselenide (WSe2) nanoplates, multi-layer silicene (Si) nanoplates, multi-layer germanene (Ge) nanoplates, multi-layer graphene (C) nanoplates, multi-layer borophene (B) nanoplates, multi-layer phosphorene (P) nanoplates, or a 2D in-plane or vertical heterostructure of two or more of the foregoing materials. Claim 17 17. The object of any of claims 14 to 16, wherein the object further comprises a layer of gel coat, and a proof coating layer is between the gel coat layer and the composite element. Claim 18 18. The object of claim 14, wherein the object comprises at least two proof coating layers. Claim 19 20. The object of claim 18, wherein at least two proof coating layers cover different surfaces of the composite element. Claim 20 20. An object according to claim 18 or 19, wherein at least one proof coating layer is covered with a further proof coating layer. Claim 21 21. The object of any of claims 14 to 20, wherein the proof coating layer has a dry thickness in the range of 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 30 μm, 25 μm to 100 μm, or 40 μm to 60 μm. Claim 22 22. The object of any one of claims 14 to 21, wherein the proof coating is composed of 0.1% to 0.5% by weight of 2D nanomaterial platelets. Claim 23 23. The article of any of claims 14 to 22, wherein the composite matrix is ​​comprised of one or more thermoset matrices, unsaturated polyester resins, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic acid polyester resins, vinyl ester resins, epoxy resins, cyanate esters, bismaleimides, urethane acrylates, phenols, furans or poly(furfural alcohols), polyimides, benzoxazines, and mixtures and combinations thereof. Claim 24 24. The article of any of claims 14 to 23, wherein the second matrix is ​​comprised of one or more of a crosslinkable resin, an epoxy resin, a polyester resin, a vinyl ester resin, an acrylic, an aminoplast, a urethane, a carbamate, an alkyd, a silicone, a polyurea, a silicate, a polydimethylsiloxane, a vinyl ester, an unsaturated polyester, an orthophthalic polyester resin, a terephthalic polyester resin, an isophthalic polyester resin, a dicyclopentadiene polyester resin, a chlorendic acid polyester resin, a phenol, a furan or a poly(furfuryl alcohol), a polyimide, a benzoxazine, and a non-crosslinkable resin. Claim 25 25. The object of any of claims 14 to 24, wherein the proof coating further comprises a hardener. Claim 26 26. An object according to any one of claims 14 to 25, wherein the object is a mould for use in making an object from a composite material. Claim 27 A proof coating for use in the method of manufacture according to claims 1 to 13 or the object according to claims 14 to 26, characterized in that the proof coating consists of 0.1 wt% to 0.5 wt% graphene / graphite nanoplates with 6 to 14 layers of carbon atoms or graphite flakes with 1 nanoscale dimensions and 25 to 35 layers of carbon atoms. Claim 28 28. The proof coating of claim 27, wherein the second matrix is ​​comprised of one or more of a crosslinkable resin, an epoxy resin, a polyester resin, a vinyl ester resin, an acrylic, an aminoplast, a urethane, a carbamate, an alkyd, a silicone, a polyurea, a silicate, a polydimethylsiloxane, a vinyl ester, an unsaturated polyester, an orthophthalic polyester resin, a terephthalic polyester resin, an isophthalic polyester resin, a dicyclopentadiene polyester resin, a chlorendic acid polyester resin, a phenol, a furan or a poly(furfuryl alcohol), a polyimide, a benzoxazine, and a non-crosslinkable resin. Claim 29 29. The proof coating of claim 27 or 28, wherein the proof coating further comprises a hardener. Claim 30 Use of a proof coating according to claims 27 to 29 in a manufacturing process according to claims 1 to 13. Claim 31 31. A kit comprising an amount of a proof coating according to claims 27 to 30 and instructions for using the proof coating in a method of manufacture according to claims 1 to 13.

Claims

1. 1. A method for producing an object from a fiber and / or fabric reinforced composite material, comprising the steps of: The fiber and / or fabric reinforced composite material has at least a first layer of a proof coating, a first or composite matrix, and one or more fiber and / or fabric reinforcing materials; The method comprises: a) forming a first layer of the proof coating; and b) laying up a mixture of said fiber and / or fabric reinforcing material and said composite matrix forming a composite element; Including, Where: (i) step (a) is performed first, where the first layer of the proof coating is applied to a mold or support, followed by step (b), where a lay-up is performed on the surface of the first layer of the proof coating of step (a); or (ii) step (b) is carried out first, a lay-up is carried out on a mould or support, followed by step (a), in which the first layer of the proof coating is applied to at least one surface of the composite element of step (b); the proof coating is comprised of a second matrix having 2D nanomaterial platelets dispersed therein, the 2D nanomaterial platelets being graphene / graphite platelets and having a D50 particle size of less than 45 μm, less than 30 μm, or less than 15 μm; the proof coating comprises multiple layers of 2D nanomaterial platelets to provide a tortuous path for penetration of water and / or other liquids; the proof coating is comprised of 0.1 wt % to 0.5 wt % 2D nanomaterial platelets; A method wherein the proof coating acts as a barrier to the penetration of water and / or other liquids into the fiber and / or fabric reinforcing material of the composite element.

2. 10. The method of claim 1 , wherein the 2D nanomaterial platelets of the proof coating comprise one or a mixture of graphene nanoplates and graphite flakes, the graphite flakes having dimensions on the nanoscale of 1 nanometer and 35 or fewer atomic layers.

3. The 2D nanomaterial platelets can be graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have dimensions of 1 nanoscale and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS 2 ) nanoplates, tungsten diselenide (WSe 2 ) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphene (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, multi-layer graphene (C) nanoplates, multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS 2 ) nanoplates, multi-layer tungsten diselenide (WSe 2 3. The method of claim 1 or 2, wherein the nanoplates comprise one or a mixture of the following: multi-layer silicon (Si) nanoplates, multi-layer germanene (Ge) nanoplates, multi-layer graphene (C) nanoplates, multi-layer borophene (B) nanoplates, multi-layer phosphorene (P) nanoplates, or 2D in-plane or vertical heterostructures of two or more of the foregoing materials.

4. The method comprises: c) forming a layer of gel coat; Further comprising: Where: (iii) step (c) is performed first, in which the gel coat is applied to a mould or substrate, followed by step (a), in which the proof coating is formed on a surface of the gel coat, followed by step (b), in which a lay-up is performed on the free surface of the proof coating; or (iv) A method according to any one of claims 1 to 3, in which step (b) is first carried out, in which a lay-up is carried out on a mould or support, followed by step (a), in which the first layer of the proof coating is applied to at least one surface of the composite element of step (b), followed by step (c), in which the gel coat is applied to a free surface of the proof coating.

5. A method according to any one of claims 1 to 4, further comprising forming at least two proof coating layers.

6. The method of claim 5, further comprising at least two proof coating layers covering different surfaces of the composite element.

7. The method of claim 5 or 6, further comprising overlaying at least one proof coating layer with a further proof coating layer.

8. The method according to any of claims 1 to 7, wherein the layer of proof coating is applied by brushing, spraying or printing.

9. 9. The method of claim 1, wherein the first layer of the proof coating has a dry thickness in the range of 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 30 μm, 25 μm to 100 μm, or 40 μm to 60 μm, 25 μm to 100 μm, 40 μm to 60 μm.

10. 10. The method of any of claims 1 to 9, wherein the composite matrix is ​​comprised of one or more thermoset matrices, unsaturated polyester resins, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic polyester resins, vinyl ester resins, epoxy resins, cyanate esters, bismaleimides, urethane acrylates, phenols, furans or poly(furfural alcohols), polyimides, benzoxazines, and mixtures and combinations thereof.

11. 11. The method of any of claims 1 to 10, wherein the second matrix is ​​comprised of one or more of a crosslinkable resin, an epoxy resin, a polyester resin, a vinyl ester resin, an acrylic, an aminoplast, a urethane, a carbamate, an alkyd, a silicone, a polyurea, a silicate, a polydimethylsiloxane, a vinyl ester, an unsaturated polyester, an orthophthalic polyester resin, a terephthalic polyester resin, an isophthalic polyester resin, a dicyclopentadiene polyester resin, a chlorendic acid polyester resin, a phenol, a furan or a poly(furfuryl alcohol), a polyimide, a benzoxazine, and a non-crosslinkable resin.

12. The method of claim 1 , wherein the proof coating further comprises a hardener.

13. 1. An object constructed at least in part from a fiber and / or fabric reinforced composite material, comprising: The article has at least one proof coating layer, a first or composite matrix, and one or more fiber and / or fabric reinforcing materials; the fiber and / or fabric reinforcing material and the composite matrix form a composite element; the proof coating layer is comprised of a second matrix having 2D nanomaterial platelets dispersed therein; the 2D nanomaterial platelets are graphene / graphite platelets and have a D50 particle size of less than 45 μm, less than 30 μm, or less than 15 μm; the proof coating layer comprises a plurality of layers of 2D nanomaterial platelets to provide a tortuous path for penetration of water and / or other liquids; the proof coating layer is comprised of 0.1 wt % to 0.5 wt % 2D nanomaterial platelets; The proof coating layer acts as a barrier to the penetration of water and / or other liquids into the fiber and / or fabric reinforcing material of the composite element.

14. 14. The article of claim 13, wherein the 2D nanomaterial platelets of the proof coating layer comprise one or a mixture of graphene nanoplates and graphite flakes, the graphite flakes having a nanoscale dimension and 35 or fewer atomic layers.

15. The 2D nanomaterial platelets can be graphene (C) nanoplates, graphene oxide nanoplates, reduced graphene oxide nanoplates, graphite flakes, where the graphite flakes have dimensions of 1 nanoscale and 35 or fewer layers, hexagonal boron nitride (hBN) nanoplates, molybdenum disulfide (MoS 2 ) nanoplates, tungsten diselenide (WSe 2 ) nanoplates, silicene (Si) nanoplates, germanene (Ge) nanoplates, graphene (C) nanoplates, borophene (B) nanoplates, phosphorene (P) nanoplates, multi-layer graphene (C) nanoplates, multi-layer graphene oxide nanoplates, multi-layer reduced graphene oxide nanoplates, multi-layer hexagonal boron nitride (hBN) nanoplates, multi-layer molybdenum disulfide (MoS 2 ) nanoplates, multi-layer tungsten diselenide (WSe 2 15. The article of claim 13 or 14, comprising one or a mixture of the following: multi-layered silicene (Si) nanoplates, multi-layered germanene (Ge) nanoplates, multi-layered graphene (C) nanoplates, multi-layered borophene (B) nanoplates, multi-layered phosphorene (P) nanoplates, or 2D in-plane or vertical heterostructures of two or more of the foregoing materials.

16. 16. An object according to any of claims 13 to 15, wherein the object further comprises a layer of gel coat, a proof coating layer being between said layer of gel coat and said composite element.

17. 17. An object according to any of claims 13 to 16, wherein the object comprises at least two proof coating layers.

18. 20. The article of claim 17, wherein at least two proof coating layers cover different surfaces of the composite element.

19. 19. An object according to claim 17 or 18, wherein at least one proof coating layer is covered with a further proof coating layer.

20. 20. The object of any of claims 13 to 19, wherein the proof coating layer has a dry thickness in the range of 5 μm to 100 μm, 5 μm to 50 μm, 10 μm to 30 μm, 25 μm to 100 μm, or 40 μm to 60 μm.

21. 21. The article of any of claims 13 to 20, wherein the composite matrix is ​​comprised of one or more thermoset matrices, unsaturated polyester resins, orthophthalic polyester resins, terephthalic polyester resins, isophthalic polyester resins, dicyclopentadiene polyester resins, chlorendic acid polyester resins, vinyl ester resins, epoxy resins, cyanate esters, bismaleimides, urethane acrylates, phenols, furans or poly(furfural alcohols), polyimides, benzoxazines, and mixtures and combinations thereof.

22. 22. The article of any of claims 13 to 21, wherein the second matrix is ​​comprised of one or more of a crosslinkable resin, an epoxy resin, a polyester resin, a vinyl ester resin, an acrylic, an aminoplast, a urethane, a carbamate, an alkyd, a silicone, a polyurea, a silicate, a polydimethylsiloxane, a vinyl ester, an unsaturated polyester, an orthophthalic polyester resin, a terephthalic polyester resin, an isophthalic polyester resin, a dicyclopentadiene polyester resin, a chlorendic acid polyester resin, a phenol, a furan or a poly(furfuryl alcohol), a polyimide, a benzoxazine, and a non-crosslinkable resin.

23. 23. The object of any of claims 13 to 22, wherein the proof coating layer further comprises a hardener.

24. 24. An object according to any one of claims 13 to 23, wherein the object is a mould for use in making an object from a composite material.

Citation Information

Patent Citations

  • Gas barrier coating agent, gas barrier film and method for producing the same

    JP2017210515A

  • Functionalized graphene barrier element

    WO2016149532A1

  • Composite article and method of manufacture

    WO2017014821A2