Glass interleaving paper

The nonwoven glass interleaving paper with controlled thickness and core-sheath fibers addresses the low bending strength issue, ensuring clean and efficient vertical handling of large glass plates by reducing particle generation and overlapping.

JP7589957B1Active Publication Date: 2024-11-26K PLUS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024083169
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-11-26
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Conventional nonwoven fabrics used as glass interleaving paper have low bending strength, making them difficult to handle and prone to particle generation, especially when used in vertically stacked laminates of large glass plates, which can lead to improper feeding and contamination.

Method used

A nonwoven fabric with a thickness of 60 μm to 160 μm, core-sheath structured fibers with a diameter of 20 μm or more, and controlled particle generation, ensuring a bending strength of 70 mm or less, measured using specific methods to maintain cleanliness and facilitate vertical handling.

Benefits of technology

The solution provides nonwoven glass interleaving paper with enhanced bending strength and reduced particle generation, allowing for clean handling and vertical stacking of glass laminates without overlapping issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589957000003
    Figure 0007589957000003
  • Figure 0007589957000004
    Figure 0007589957000004
  • Figure 0007589957000005
    Figure 0007589957000005
Patent Text Reader

Abstract

To provide a glass interleaving paper which is a nonwoven fabric having a predetermined bending strength. [Solution] The glass interleaving paper is a nonwoven fabric having a thickness of 60 μm or more and 160 μm or less. A first test piece cut out from this nonwoven fabric is 20 mm x 150 mm, and the drooping length measured by the bending resistance measurement method specified in JIS-L1096-2010, Method B, when the overhang length is 100 mm is 70 mm or less. With this configuration, it is possible to provide glass interleaving paper made of a nonwoven fabric having a predetermined bending strength while suppressing the thickness when glass is laminated. This makes it possible to suppress particle generation during lamination of the glass interleaving paper, to keep the glass using the glass interleaving paper clean, and to handle the laminate laminated in a vertical position.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass interleaving paper. More specifically, the present invention relates to a glass interleaving paper that is a nonwoven fabric. [Background technology]

[0002] Glass interleaving paper is used by being sandwiched between glass sheets when conveying plate-like glass such as architectural glass sheets, automotive glass sheets, and glass sheets for liquid crystal displays. Among these plate-like glass sheets, particularly in the case of flat panel display glass sheets used in liquid crystal displays, elements such as fine electrical wiring, electrodes, electrical circuits, and partition walls are formed on the surface, so that even slight scratches or contamination on the surface can cause defects such as disconnection. Therefore, in order to prevent scratches or contamination, high quality is required for the glass interleaving paper in terms of the generation of particles, etc. In addition, recently, the glass interleaving paper used in automotive glass sheets may be required to have the same quality as the glass interleaving paper used in flat panel display glass sheets.

[0003] In order to solve the above problems, Patent Documents 1 and 2 disclose glass interleaving paper, which is a nonwoven fabric having a specific structure.

[0004] Patent Document 3 discloses a laminate in which glass plates and glass interleaving paper are alternately stacked in a vertical position on a pallet. Flat glass for flat panel displays has become larger as the size of the flat panel displays increases, and in recent years, even when the laminate is transported, the glass plates are transported in a vertical position. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-2777991 A [Patent Document 2] JP 2009-173510 A [Patent Document 3] JP 2022-143331 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, when the thickness of a nonwoven fabric is the same, the bending strength, generally expressed as bending resistance, is lower than that of paper made from pulp. FIG. 3 shows an explanatory diagram of a laminate 51 in which glass plates 52 and glass interleaving papers 53 are alternately stacked in a vertical position. An enlarged schematic diagram of a protruding portion of the glass interleaving paper 53 is also shown. When the glass plates 52 become larger, that is, when the area of ​​the glass plates 52 becomes larger, it becomes easier to handle the glass plates 52 by stacking them in a vertical position rather than stacking them in a horizontal position. Here, when the glass plates 52 are stacked in a vertical position on the conveyor 50, the glass interleaving paper 53 sandwiched between the glass plates 52 protrudes above the laminate 51 by about 100 mm. When the glass plates 52 are taken up one by one from the stack 51, the glass interleaving papers 53 are also taken up one by one, but if the bending strength of the glass interleaving paper 53 is low, the protruding parts of the glass interleaving paper 53 will overlap with the protruding parts of adjacent glass interleaving papers 53, making it impossible to properly feed the gripping parts of the glass interleaving paper 53 between the glass interleaving papers 53, and making it impossible to remove the glass interleaving papers 53 one by one from the stack 51. For this reason, there is a problem that glass interleaving paper 53 with a low bending strength is difficult to use for vertical transport.

[0007] In view of the above circumstances, an object of the present invention is to provide a glass interleaving paper that is a nonwoven fabric having a predetermined bending strength. [Means for solving the problem]

[0008] The glass interleaving paper of the first invention is a nonwoven fabric having a thickness of 60 μm or more and 160 μm or less, and a first test piece of the nonwoven fabric cut into a size of 20 mm x 150 mm has a drooping length of 70 mm or less when measured by the bending resistance measurement method specified in the B method of JIS-L1096-2010 when the overhanging length is 100 mm. The diameter of the fibers constituting the nonwoven fabric is 20 μm or more, and the fibers have a core-sheath structure. It is characterized by the above. No.2 The glass interleaving paper of the invention is the first Clearly In the nonwoven fabric, a second test piece having a size of 295 mm x 208 mm is cut out and not washed. In a measurement using the tumbling method of JIS-B9923-1997, the number of separable particles per second is 10 or less, the number of particles having a size of 0.3 μm or more and smaller than 0.5 μm is 20 or less, and the number of particles having a size of 1.0 μm or more and smaller than 5.0 μm is 20 or less. Effect of the Invention

[0009] According to the first invention, since the bending strength value when the thickness is equal to or less than a predetermined thickness is 70 mm or less, it is possible to provide glass interleaving paper made of a nonwoven fabric with a predetermined bending strength while suppressing the thickness when the glass is laminated. This makes it possible to suppress particle generation during lamination of the glass interleaving paper, to keep the glass to which the glass interleaving paper is used clean, and to enable handling of the laminate laminated in a vertical position. Also, By making the fibers constituting the nonwoven fabric have a diameter of 20 μm or more, it is possible to increase the bending strength while maintaining the thickness of the nonwoven fabric in a thin state. No. 2 According to the invention, by controlling the number of particles in the nonwoven fabric to a predetermined number or less, when the nonwoven fabric is used as glass interleaving paper, the glass can be kept cleaner. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is an explanatory diagram of a method for measuring the bending strength of a nonwoven fabric. [Diagram 2] FIG. 4 is an explanatory diagram of measurement points when measuring the thickness of a nonwoven fabric. [Diagram 3] 1 is an explanatory diagram of a laminate in which glass plates and glass interleaving paper are alternately stacked in a vertical position, and an enlarged schematic diagram of a protruding portion of the glass interleaving paper. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Next, an embodiment of the present invention will be described with reference to the drawings. However, the embodiment shown below is an example of a glass interleaving paper for embodying the technical idea of ​​the present invention, and the present invention does not specify the glass interleaving paper as described below. Note that the dimensions, materials, shapes, etc. of the components described in the embodiment are merely illustrative examples, and are not intended to limit the scope of the present invention, unless otherwise specified. Furthermore, the size or positional relationship of the components shown in each drawing may be exaggerated to clarify the explanation.

[0012] The glass interleaving paper of the present invention is a nonwoven fabric having a thickness of 60 μm or more and 160 μm or less, and a first test piece 20 cut out of the nonwoven fabric and measuring 20 mm x 150 mm has a drooping length of 70 mm or less when measured using the bending resistance measurement method specified in Method B of JIS-L1096-2010 when the overhang length is 100 mm.

[0013] By making the hanging length 70 mm or less when the thickness of the glass interleaving paper is within a predetermined thickness range, it is possible to provide glass interleaving paper made of nonwoven fabric with a predetermined bending strength while suppressing the thickness when the glass is laminated. This makes it possible to suppress particle generation during lamination of the glass interleaving paper, keep the glass to which the glass interleaving paper is used clean, and makes it possible to handle the laminate stacked in a vertical position.

[0014] In addition, the diameter of the fibers constituting the nonwoven fabric is preferably 20 μm or more. By making the diameter of the fibers constituting the nonwoven fabric 20 μm or more, the bending strength can be further increased while the thickness of the nonwoven fabric is maintained at a thin state.

[0015] Furthermore, for a second test piece of the nonwoven fabric cut to a size of 295 mm x 208 mm and not subjected to a washing treatment, the number of separable particles per second measured using the tumbling method of JIS-B9923-1997 is preferably 10 or less particles that are 0.3 μm or more and smaller than 0.5 μm, 20 or less particles that are 0.5 μm or more and smaller than 1.0 μm, and 20 or less particles that are 1.0 μm or more and smaller than 5.0 μm. By keeping the number of particles in the nonwoven fabric to a predetermined number or less, when the nonwoven fabric is used as glass interleaving paper, the glass can be kept cleaner.

[0016] <Embodiment> (Thickness of nonwoven fabric) Most conventional glass interleaving papers are made from paper made from pulp, and their thickness is required to be between 60 μm and 160 μm. If the glass interleaving paper is thinner than 60 μm, there is a high possibility that the pieces of glass will come into contact with each other when they are stacked. Also, if the glass interleaving paper is thicker than 160 μm, when several dozen sheets of glass are stacked, the height in the stacking direction becomes too high. Therefore, the thickness required for the nonwoven fabric that becomes the glass interleaving paper is between 60 μm and 160 μm.

[0017] The thickness of the nonwoven fabric according to this embodiment is in accordance with the test method for "thickness" according to Method A of JIS-L1913-2010. FIG. 2 shows an explanatory diagram of the measurement points when measuring the thickness of the nonwoven fabric. FIG. 2 shows a rectangular test piece 30 of 150 mm x 100 mm. For example, the test piece 30 is measured at five points as shown in the figure, and the measured thickness is obtained at each point, and the average of the measured values ​​can be used as the thickness of the test piece 30, i.e., the thickness of the nonwoven fabric. This is because the thickness of the nonwoven fabric varies depending on the measurement point.

[0018] (Flexural strength of nonwoven fabric) FIG. 1 is an explanatory diagram of a method for measuring the bending strength of a nonwoven fabric as a glass interleaving paper. FIG. 1 shows a front view of a tester 10. This tester 10 is an example of a tester specified in the B method of JIS-L1096-2010. The thickness of the nonwoven fabric was measured according to the "General nonwoven fabric test method" of JIS-L1913-2010, while the bending strength of the nonwoven fabric as a glass interleaving paper was measured according to the B method of JIS-L1096-2010 "Test method for woven and knitted fabrics". The glass interleaving paper may be sandwiched between the glass interleaving paper and the glass by using static electricity. In this case, a material that is easily charged with static electricity is used as the material for the glass interleaving paper. In this case, the first test piece 20 easily becomes charged with static electricity, and the bending strength cannot be measured accurately by the method specified in the "General nonwoven fabric test method" of JIS-L1913-2010.

[0019] The testing machine 10 has a configuration in which a pillar-shaped column 12 is erected on a flat base 11. A movable stage 13 that moves up and down along the side of the column 12 is provided for the column 12. The base 11 is adjusted so that the top surface of the movable stage 13 is horizontal. The movable stage 13 is fixed to the column 12 by a knob 15 provided on the column 12. The knob 15 is located opposite the side of the column 12 on which the movable stage 13 is provided. The column 12 is provided with a scale 14 that indicates the distance of the movable stage 13 from the top of the column 12.

[0020] The user of the tester 10 cuts the nonwoven fabric to be measured to 20 mm x 150 mm to prepare the first test piece 20 to be measured. The longitudinal direction of the first test piece 20 preferably coincides with the longitudinal direction of the entire nonwoven fabric, i.e., coincides with the direction perpendicular to the width direction of the entire nonwoven fabric. When forming the laminate 50 as shown in FIG. 3, the laminate 50 is often fed from above, and it is therefore preferable that the vertical direction of the protruding portion of the glass interleaving paper 53 coincides with the longitudinal direction of the first test piece 20.

[0021] The user of the test machine 10 loosens the knob 15, moves the top surface of the movable stage 13 to a position where it coincides with the top surface of the column 12, and in this state, tightens the knob 15 to fix the movable stage 13. Next, the user places the first test piece 20 on the top surface of the column 12. At this time, the user places the first test piece 20 so that it overhangs by a predetermined length, for example, so that the overhang length l of the first test piece 20, i.e., the length overhanging the movable stage 13 side, is 100 mm, and then places the weight 16 on the end of the column 12 to fix the first test piece 20. It is preferable to place the weight 16 so that it overhangs slightly toward the movable stage 13 side. Then, the user loosens the knob 15 and moves the movable stage 13 downward. Then, the user fixes the movable stage 13 to the column 12 with the knob 15 at a height where the free end side of the first test piece 20 is separated from the movable stage 13, and measures the hanging length b.

[0022] In the glass interleaving paper according to the present embodiment, the first test piece 20 cut out of the nonwoven fabric to a size of 20 mm x 150 mm has a drooping length of 70 mm or less measured by the bending resistance measurement method specified in the B method of JIS-L1096-2010 when the overhanging length is 100 mm. A small drooping length means a large bending strength value, and a large drooping length means a small bending strength value. The drooping length is preferably 0 mm, but it is almost never 0 mm as long as the nonwoven fabric has weight. However, if the drooping length is 30 mm or more, the gripping parts for gripping the glass interleaving paper can be accurately positioned between the glass interleaving papers, which is preferable. If the drooping length is greater than 70 mm, when a laminate of glass is formed in a vertical position, the glass interleaving papers overlap each other, which is a problem in that it becomes difficult to feed the gripping parts for removing the glass interleaving paper between the glass interleaving papers.

[0023] By making the hanging length of the glass interleaving paper 70 mm or less when the thickness is equal to or less than a predetermined value, it is possible to provide glass interleaving paper made of nonwoven fabric with a predetermined bending strength while suppressing the thickness when the glass is laminated. This makes it possible to suppress particle generation during lamination of the glass interleaving paper, to keep the glass to which the glass interleaving paper is used clean, and to enable handling of the laminate laminated in a vertical position.

[0024] (Nonwoven fabric material) The material of the nonwoven fabric that is the glass interleaving paper according to this embodiment is not particularly limited. For example, aramid fiber, glass fiber, cellulose fiber, nylon fiber, vinylon fiber, polyester fiber, polyethylene fiber, polypropylene fiber, polyolefin fiber, rayon fiber, etc. can be appropriately used. In addition, a plurality of these fibers may be used. Among them, the glass interleaving paper according to this embodiment is preferably made of polyester fiber that is deposited. The deposited continuous fibers are preferably thermally bonded to each other. Since the thermoplastic synthetic fiber called polyester is used as a component of the continuous fibers, the glass interleaving paper can be produced inexpensively and well. In addition, polyester fiber has the advantage of being excellent in strength and has the advantage of being moderately hydrophilic, so that it is difficult to be charged in the air and is difficult to attract dust in the air.

[0025] The polyester used as the material of the nonwoven fabric, which is the glass interleaving paper according to this embodiment, is a polycondensate of a polyvalent carboxylic acid (dicarboxylic acid) and a polyalcohol (diol), and is not particularly limited as long as it is obtained by dehydration condensation of a polyalcohol (a compound having a plurality of alcoholic functional groups -OH) and a polyvalent carboxylic acid (a compound having a plurality of carboxylic acid functional groups -COOH). For example, polyethylene terephthalate or polybutylene terephthalate obtained from terephthalic acid as the polyvalent carboxylic acid (acid component) and ethylene glycol and butanediol as the polyalcohol (glycol component) are preferably used. The acid component may be a copolymer using terephthalic acid and another acid component. The glycol component may be a copolymer using ethylene glycol and another glycol component. Examples of other acid components include aromatic dicarboxylic acids such as isophthalic acid, diphenyl ether-4,4'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, and naphthalene-2,6-dicarboxylic acid, aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, and undecadicarboxylic acid, and alicyclic dicarboxylic acids such as hexahydroterephthalic acid. Examples of other glycol components include aliphatic glycols such as propylene glycol and neopentyl glycol, alicyclic glycols such as cyclohexane dimethanol, and aromatic dihydroxy compounds such as bisphenol A. As the polyester, only one type of polyester may be used, or a blend of homopolymers or a blend of a homopolymer and a copolymer may be used.

[0026] In the nonwoven fabric that is the glass interleaving paper according to the present embodiment, the polyester that is preferably used is a polyester whose acid component is an aromatic dicarboxylic acid and whose glycol component is a straight-chain diol, for example, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate, because the polyester has excellent mechanical strength, heat resistance, and flexibility.

[0027] The polyester may be appropriately blended with additives as necessary. Additives to be blended include antistatic agents, colorants, softening agents, antioxidants, heat stabilizers, weathering agents, metal deactivators, light stabilizers, antibacterial and antifungal agents, dispersants, softeners, plasticizers, crystal nucleating agents, flame retardants, foaming agents, foaming assistants, etc. However, additives that bleed out from the polyester or that generate powder or dust and fall off should not be blended.

[0028] The fibers constituting the nonwoven fabric that is the glass interleaving paper according to the present embodiment may be single-phase fibers made of one type of polyester, or composite fibers made of the same or different types of polyesters. In addition, it does not matter if the fibers are a mixture of single-phase fibers made of different polyesters, composite fibers made of a combination of different polyesters, or a mixture of single-phase fibers and composite fibers.

[0029] (Nonwoven fiber manufacturing method and fiber diameter) The fibers used in the nonwoven fabric, which is the glass interleaving paper according to this embodiment, are preferably continuous fibers. This is because no fallen fibers are generated. Examples of nonwoven fabrics formed by accumulating continuous fibers include spunbond nonwoven fabrics, meltblown nonwoven fabrics, and flash spun nonwoven fabrics. It is preferable to use spunbond nonwoven fabrics because of their excellent single fiber strength, good dimensional stability of the sheet, the fact that the contact area with the glass plate can be reduced because the single fiber fineness is not too small, and the fact that no solvent is used during production. In addition, it is preferable that the diameter of the fibers constituting the nonwoven fabric is 20 μm or more. For example, when producing continuous fibers used in nonwoven fabrics by the spunbond method, the diameter of the fibers can be made the same as the diameter of the mold for injecting the fibers, 20 μm or more. In addition, the structure of the fibers of the nonwoven fabric can be a so-called core-sheath structure. When the fiber structure is a core-sheath structure, the diameter of the fibers can be easily made thicker. There is no particular upper limit on the diameter of the fibers constituting the nonwoven fabric, but in consideration of handling after production, the diameter of the fibers constituting the nonwoven fabric is preferably 40 μm or less.

[0030] By making the diameter of the fibers constituting the nonwoven fabric that is the glass interleaving paper according to this embodiment 20 μm or more, it is possible to further increase the bending strength while maintaining the thickness of the nonwoven fabric in a thin state.

[0031] (Amount of dust generated by nonwoven fabric) The nonwoven fabric, which is the glass interleaving paper according to this embodiment, is cut into a size of 295 mm x 208 mm, and when a second test piece that has not been washed is prepared, the number of separable particles per second measured using the tumbling method of JIS-B9923-1997 is preferably 10 or less particles smaller than 0.3 μm and 0.5 μm, 20 or less particles smaller than 0.5 μm and 1.0 μm, and 20 or less particles smaller than 1.0 μm and 5.0 μm. The "General Nonwoven Fabric Test Method" of JIS-L1913-2010 does not specify a measurement method for the dust generation of nonwoven fabric. Therefore, the measurement specified in JIS-B9923-1997 "Method for measuring contaminant particles in cleanroom clothing" is applied mutatis mutandis, and the amount of dust generation of the nonwoven fabric is specified using the measurement method.

[0032] By keeping the number of particles in the nonwoven fabric to a predetermined number or less, when the nonwoven fabric is used as glass interleaving paper, the glass can be kept cleaner. EXAMPLES

[0033] Specific examples of the glass interleaving paper according to the present invention will be described below, but the present invention is not limited to these examples.

[0034] (Examples of thickness, basis weight, sag length, and fiber thickness) Example 1 A nonwoven fabric was manufactured using polyethylene terephthalate with a core-sheath structure of continuous fibers. The thickness of this nonwoven fabric was measured using the "thickness" test method A specified in JIS-L1913-2010. A rectangular test piece 30 of 150 mm x 100 mm was used for the measurement, and the thickness was measured at five points as shown in Figure 2, and the average value was used as the measured value. The measured thickness was 109.2 μm. The basis weight of the nonwoven fabric, that is, the weight per square meter of this nonwoven fabric, was 20 g. The values ​​are shown in Table 1.

[0035] Next, the nonwoven fabric was cut into a 20 mm x 150 mm strip shape so that the longitudinal direction was the longitudinal direction of the entire nonwoven fabric to prepare the first test pieces 20. The hanging length of each of the first test pieces 20 was measured twice on the front and back sides when the overhang length was 100 mm using the bending resistance measurement method specified in JIS-L1096-2010, Method B, and the average value was taken as the measured value. The measured hanging length was 52.9 mm, and it was confirmed that the nonwoven fabric had sufficient bending strength. The values ​​are shown in Table 1.

[0036] Finally, the fiber thickness of this nonwoven fabric was measured using a digital microscope. Five first test pieces 20 measuring 20 mm x 150 mm were prepared, and each first test piece 20 was measured twice at a magnification of 200 times. The average value of the total of 10 measurements was taken as the measured fiber thickness. The measured fiber thickness was 25.28 μm, and it was confirmed that the fiber had a sufficient thickness. The values ​​are shown in Table 1.

[0037] Example 2 The differences between Example 1 and Example 2 are the thickness, basis weight, and fiber thickness after production. The other production conditions are the same as in Example 1. The methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness in Example 2 was 120.8 μm. The basis weight was 25 g. The values ​​are shown in Table 1.

[0038] In Example 2, the measured hanging length was 48.5 mm, which confirmed that the fiber had sufficient bending strength. In addition, the measured fiber thickness was 29.70 μm, which confirmed that the fiber had sufficient thickness. The values ​​are shown in Table 1.

[0039] Comparative Example 1 The differences between Example 1 and Comparative Example 1 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 1 was 168.9 μm. The basis weight was 35 g. The values ​​are shown in Table 1.

[0040] In Comparative Example 1, the measured value of the hanging length was 73.8 mm, and it was confirmed that the bending strength was small. The measured value of the fiber thickness in this case was 14.75 μm, which was not thick enough. Furthermore, in Comparative Example 1, the thickness was more than the standard value of 160 μm, and it was found that in the case of this glass interleaving paper, the stacking height reaches more than the specified value when stacked. The values ​​are shown in Table 1.

[0041] Comparative Example 2 The differences between Example 1 and Comparative Example 2 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 2 was 169.4 μm. The basis weight was 30 g. The values ​​are shown in Table 1.

[0042] In Comparative Example 2, the measured value of the hanging length was 73.4 mm, and it was confirmed that the bending strength was small. The measured value of the fiber thickness in this case was 18.41 μm, which was not thick enough. Furthermore, in Comparative Example 2, the thickness was more than the standard value of 160 μm, and it was found that in the case of this glass interleaving paper, the stacking height reaches more than the specified value when stacked. The values ​​are shown in Table 1.

[0043] Comparative Example 3 The differences between Example 1 and Comparative Example 3 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 3 was 181.0 μm. The basis weight was 35 g. The values ​​are shown in Table 1.

[0044] In Comparative Example 3, the measured hanging length was 69.1 mm, and it was confirmed that the bending strength was sufficient. However, the measured fiber thickness was 17.91 μm, which was not thick enough. Furthermore, in Comparative Example 3, the thickness was more than the standard value of 160 μm, and it was found that in the case of this glass interleaving paper, the stacking height reaches more than the specified value when stacked. The values ​​are shown in Table 1.

[0045] Comparative Example 4 The differences between Example 1 and Comparative Example 4 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 4 was 186.6 μm. The basis weight was 40 g. The values ​​are shown in Table 1.

[0046] In Comparative Example 4, the measured hanging length was 63.6 mm, and it was confirmed that the bending strength was sufficient. However, the measured fiber thickness was 13.53 μm, which was not thick enough. Furthermore, in Comparative Example 4, the thickness was more than the standard value of 160 μm, and it was found that in the case of this glass interleaving paper, the stacking height reaches more than the specified height when stacked. The values ​​are shown in Table 1.

[0047] Comparative Example 5 The differences between Example 1 and Comparative Example 5 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 5 was 192.5 μm. The basis weight was 45 g. The values ​​are shown in Table 1.

[0048] In Comparative Example 5, the measured hanging length was 61.0 mm, and it was confirmed that the bending strength was sufficient. However, the measured fiber thickness was 12.82 μm, which was not thick enough. Furthermore, in Comparative Example 5, the thickness was more than the standard value of 160 μm, and it was found that in the case of this glass interleaving paper, the stacking height reaches more than the specified height when stacked. The values ​​are shown in Table 1.

[0049] Comparative Example 6 The differences between Example 1 and Comparative Example 6 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 6 was 197.1 μm. The basis weight was 45 g. The values ​​are shown in Table 1.

[0050] In Comparative Example 6, the measured hanging length was 45.4 mm, and it was confirmed that the bending strength was sufficient. However, the measured fiber thickness was 16.37 μm, which was not thick enough. Furthermore, in Comparative Example 6, the thickness was more than the standard value of 160 μm, and it was found that in the case of this glass interleaving paper, the stacking height reaches more than the specified height when stacked. The values ​​are shown in Table 1.

[0051] Comparative Example 7 The differences between Example 1 and Comparative Example 7 are the thickness and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 7 was 117.7 μm. The basis weight was 20 g. The values ​​are shown in Table 1.

[0052] In Comparative Example 7, the thickness was found to be sufficiently thin, being less than the standard value of 160 μm. However, the measured hanging length was 100.9 mm, and it was confirmed that the bending strength was small. And the measured fiber thickness was 14.34 μm, which was not sufficient. The values ​​are shown in Table 1.

[0053] Comparative Example 8 The differences between Example 1 and Comparative Example 8 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 8 was 129.8 μm. The basis weight was 25 g. The values ​​are shown in Table 1.

[0054] In Comparative Example 8, the thickness was found to be sufficiently thin, being less than the standard value of 160 μm. However, the measured hanging length was 91.2 mm, and it was confirmed that the bending strength was small. And the measured fiber thickness was 15.60 μm, which was not sufficient. The values ​​are shown in Table 1.

[0055] Comparative Example 9 The differences between Example 1 and Comparative Example 9 are the thickness, basis weight, and fiber thickness after production. Also, the fiber structure is a single fiber structure, not a core-sheath structure. The other production conditions are the same as in Example 1. Also, the methods for measuring the thickness, hanging length, and fiber thickness are the same as in Example 1. The measured thickness value in Comparative Example 9 was 156.3 μm. The basis weight was 30 g. The values ​​are shown in Table 1.

[0056] In Comparative Example 9, the thickness was found to be sufficiently thin, being less than the standard value of 160 μm. However, the measured hanging length was 86.2 mm, and it was confirmed that the bending strength was small. And the measured fiber thickness was 13.09 μm, which was not sufficient. The values ​​are shown in Table 1.

[0057] (Reference example 1) The difference between Example 1 and Reference Example 1 is that Example 1 is a nonwoven fabric, while Reference Example 1 is a paper made from pulp. That is, the concept of fiber thickness does not exist in Reference Example 1. In addition, the difference between Example 1 and Reference Example 1 is the thickness and basis weight after production. Moreover, the methods for measuring the thickness, hanging length, and fiber thickness are the same as those of Example 1. The measured thickness value in Reference Example 1 was 83.2 μm. The basis weight was 50 g. The values ​​are shown in Table 1.

[0058] In Reference Example 1, the measured hanging length was 41.3 mm, which confirmed that the sample had sufficient bending strength. The values ​​are shown in Table 1.

[0059] [Table 1]

[0060] Glass interleaving papers were prepared for each of the examples and comparative examples, and the positions of adjacent glass interleaving papers after stacking were visually checked. As a result, for the glass interleaving papers of Examples 1 and 2, sufficient space was provided between adjacent glass interleaving papers, and the gripping parts of the glass interleaving paper could be easily fed between the glass interleaving papers. In contrast, for the glass interleaving papers of Comparative Examples 1 to 6, the glass interleaving paper was thick, and the thickness of the laminate was large. Furthermore, in Comparative Examples 7 to 9, the glass interleaving papers stuck together, and there were cases where the gripping parts of the glass interleaving paper could not be fed between adjacent glass interleaving papers.

[0061] (Example regarding the amount of dust generated by nonwoven fabric) For Example 1 and Comparative Example 1, a second test piece was prepared and measured for the amount of dust generated by the nonwoven fabric. The amount of dust generated by the nonwoven fabric was determined by measurement using the tumbling method specified in JIS-B9923-1997 "Method for measuring contaminant particles in cleanroom clothing."

[0062] Example 1 A second test piece of nonwoven fabric measuring 295 mm x 208 mm was prepared. This sample was not washed. The amount of dust generated from this second sample was determined using a tumbling dust generation tester CW-HDT-102 manufactured by Akado Seisakusho Co., Ltd. The drum rotation speed of the test device was 30 RPM, and the flow rate was 0.0102 m 3 The flow rate was 1 ft3 / s, the suction volume was 1 ft3 / m, and the particle counter used was a Hach Ultra Analytics Met One A2400B. The results showed that the number of separable particles per second was 1.3 for particles between 0.3 and 0.5 μm, 3.7 for particles between 0.5 and 1.0 μm, and 2.0 for particles between 1.0 and 5.0 μm, all of which were lower than the standard values ​​for pulp-based paper, which are 10 for particles between 0.3 and 0.5 μm, 20 for particles between 0.5 and 1.0 μm, and 20 for particles between 1.0 and 5.0 μm. The values ​​are shown in Table 2.

[0063] Comparative Example 1 The differences between Example 1 and Comparative Example 1 are the thickness, basis weight, and fiber thickness after production. The fiber structure is a single fiber structure, not a core-sheath structure. Other production conditions are the same as in Example 1. The method for measuring the amount of dust is the same as in Example 1. The measurement results show that the number of particles that can be separated per second is 13.8 for particles between 0.3 μm and 0.5 μm, 22.3 for particles between 0.5 μm and 1.0 μm, and 28.5 for particles between 1.0 μm and 5.0 μm, all of which exceed the standard value for paper made from pulp. The values ​​are shown in Table 2.

[0064] [Table 2] [Explanation of symbols]

[0065] 10 Testing Machine 11. Base 12 Column 13 Mobile stand 14 Scale 15 Knob 16 Weight 20 Test Pieces b Hanging length l Overhang length

Claims

1. The nonwoven fabric has a thickness of 60 μm or more and 160 μm or less, A first test piece cut out from the nonwoven fabric measuring 20 mm x 150 mm has a droop length of 70 mm or less when measured by a bending resistance measurement method specified in Method B of JIS-L1096-2010, when the overhang length is 100 mm; The diameter of the fibers constituting the nonwoven fabric is 20 μm or more, The fiber has a core-sheath structure. A glass interleaving paper characterized by:

2. a second test piece cut into a size of 295 mm x 208 mm from the nonwoven fabric and not subjected to a washing treatment, the number of separable particles per second measured using the tumbling method of JIS-B9923-1997 is 10 or less, the number of particles of 0.3 μm or more and less than 0.5 μm or less is 20 or less, and the number of particles of 1.0 μm or more and less than 5.0 μm or less is 20 or less; The glass interleaving paper according to claim 1 .

Citation Information

Patent Citations

  • JP2004-2777991A

  • Interleaving paper for glassy plate material

    JP2004277991A

  • Cushioning sheet between glass sheets

    JP2009173510A

  • Laminate of glass sheet

    JP2011126724A

  • Sheet feeder and laminate manufacturing method