Method for producing fiber-reinforced resin foam

The method enhances fiber-reinforced resin foam by extruding foamed matrix resin around reinforcing fibers, addressing adhesion issues to improve mechanical strength and heat insulation.

JP7590362B2Active Publication Date: 2024-11-26FUKUBI KAGAKU IND
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022008014
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-21
Publication Date
2024-11-26
Estimated Expiration
2042-01-21

AI Technical Summary

Technical Problem

Existing fiber-reinforced resin foams face issues with insufficient adhesion between the core material layer and reinforcing fibers, leading to inadequate mechanical strength and reduced porosity, which affects heat insulation performance.

Method used

A manufacturing method involving an extruder and mold configuration that extrudes foamed matrix resin around reinforcing fibers, allowing the resin to expand on both sides of the fibers, ensuring close contact and high porosity, thereby enhancing mechanical strength and heat insulation.

Benefits of technology

The method produces a fiber-reinforced resin foam with improved mechanical strength and heat insulation performance by ensuring the matrix resin fully encapsulates the fibers, allowing for high porosity and effective bubble formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590362000001
    Figure 0007590362000001
  • Figure 0007590362000002
    Figure 0007590362000002
  • Figure 0007590362000003
    Figure 0007590362000003
Patent Text Reader

Abstract

To provide a fiber-reinforced resin foam which secures thermal insulation performance and has high mechanical strength.SOLUTION: A manufacturing method of a fiber-reinforced resin form executes: a feeding step (S2) of feeding a reinforcement fiber (1) so as to pass through an inside of a mold (30); a kneading step (S3) of kneading a matrix resin (2) and a foaming agent (3) in an extruder (20); and an extrusion step (S4) of pumping the matrix resin (2) having been mixed with the foaming agent (3) to the mold (30), and expanding the matrix resin (2) by foaming the foaming agent (3) while extruding the matrix resin (2) having been introduced to the mold (30) to an outside of the mold (30). In the extrusion step (S4), the matrix resin (2) is extruded from the mold (30) at a position alienated from the reinforcement fiber (1) on both sides in a second direction to expand the matrix resin (2) on both sides of the reinforcement fiber (1) in the second direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a fiber-reinforced resin foam containing a resin foam and reinforcing fibers. [Background technology]

[0002] A fiber-reinforced resin foam is known, as disclosed in Patent Document 1. This fiber-reinforced resin foam has a core layer made of a thermoplastic resin foam and a skin layer made of a fiber-reinforced thermoplastic resin fused to the surface of the core layer so as to cover the outer peripheral surface of the core layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 8-300537 Summary of the Invention [Problem to be solved by the invention]

[0004] In the fiber-reinforced resin foam described in Patent Document 1, reinforcing fibers are arranged in the skin layer (the outer peripheral surface of the molded product). Therefore, the core layer may not be sufficiently adhered to the reinforcing fibers, resulting in an insufficient reinforcing effect of the reinforcing fibers, or the foaming of the core layer may be inhibited by the reinforcing fibers, resulting in a small porosity of the core layer and insufficient heat insulating performance. Thus, Patent Document 1 has room for improvement in terms of achieving both heat insulating performance and mechanical strength.

[0005] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a method for producing a fiber-reinforced resin foam that can improve both the heat insulating performance and the mechanical strength. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention provides a method for producing a fiber-reinforced resin foam containing a foaming resin and reinforcing fibers, using an extruder and a mold connected to the extruder, the method including: a feeding step of feeding the reinforcing fibers along a predetermined first direction so that the reinforcing fibers pass through the inside of the mold; a kneading step of feeding a matrix resin and a foaming agent into the extruder and kneading the matrix resin and the foaming agent in the extruder; and an extrusion step of pressurizing the matrix resin mixed with the foaming agent by the extruder to the mold and extruding the matrix resin introduced into the mold to the outside of the mold while foaming the foaming agent to expand the matrix resin, wherein when a direction perpendicular to the first direction is defined as a second direction, in the extrusion step, the matrix resin is extruded from the mold at positions spaced apart from the reinforcing fibers on both sides of the second direction, and the matrix resin is expanded on both sides of the reinforcing fibers in the second direction (Claim 1).

[0007] In the present invention, a foaming agent is mixed into the matrix resin, and when the matrix resin is extruded from the die, the matrix resin expands due to foaming of the foaming agent. Specifically, the matrix resin mixed with the foaming agent is pumped into the die by the extruder and then extruded to the outside, so that the pressure applied to the matrix resin decreases. This pressure reduction causes the foaming agent contained in the matrix resin to foam and generate bubbles, or bubbles already generated inside the die grow, and the matrix resin is pushed by the bubbles and expands. In the present invention, the matrix resin is extruded from the die on both sides of the second direction of the reinforcing fibers passing through the inside of the die, and the matrix resin expands on both sides of the second direction of the reinforcing fibers. Thus, according to the present invention, the matrix resin can be expanded so as to cover the reinforcing fibers, and the matrix resin and the reinforcing fibers can be reliably adhered to each other. Moreover, since the matrix resin containing the foaming agent is extruded from the die at a position separated from the reinforcing fibers, the inhibition of the expansion of the matrix resin by the reinforcing fibers can be suppressed, and the matrix resin can be expanded at a high magnification. Therefore, it is possible to produce a fiber-reinforced resin foam having high mechanical strength and high porosity, i.e., high heat insulating performance.

[0008] In the above configuration, preferably, when a direction perpendicular to the first direction and the second direction is defined as a third direction, in the extrusion process, the matrix resin is extruded from the mold at multiple positions spaced apart from each other in the third direction (Claim 2).

[0009] In this configuration, the matrix resins extruded from different positions of the mold in the third direction can be expanded to fill the gaps between the matrix resins, thereby expanding the matrix resin at a sufficient rate to increase the porosity of the fiber-reinforced resin foam.

[0010] In the above configuration, preferably, the method further includes a preparation step of preparing a plurality of rod-shaped reinforcing fiber bundles which are bundles of the reinforcing fibers, and when a direction perpendicular to the first direction and the second direction is defined as a third direction, the feeding step feeds out the reinforcing fiber bundles so that the plurality of reinforcing fiber bundles pass through the die while being spaced apart from each other in the third direction (Claim 3).

[0011] In this configuration, a fiber-reinforced resin foam having high mechanical strength and heat insulating performance can be easily manufactured using the reinforcing fiber bundles before they are spread. In addition, the matrix resin can be expanded so as to fill the gaps between the reinforcing fiber bundles, and a fiber-reinforced resin foam having a reliably increased porosity, i.e., improved heat insulating performance, can be manufactured.

[0012] In the above configuration, preferably, in the feeding process, the reinforcing fiber bundles are fed out so that the multiple reinforcing fiber bundles pass through the die while being spaced apart from each other in the second direction, and in the extrusion process, the matrix resin is extruded from the die at a position between adjacent reinforcing fiber bundles in the second direction (Claim 4).

[0013] According to this configuration, the matrix resin can be expanded so as to fill the gaps between the reinforcing fiber bundles in the second direction as well, and therefore a fiber-reinforced resin foam having a sufficient amount of reinforcing fibers disposed therein and a high porosity can be continuously produced.

[0014] In the above configuration, it is preferable that the method further includes a preparation step of preparing a reinforcing fiber sheet in which the reinforcing fibers are gathered in a sheet-like form, and in the feeding step, the reinforcing fiber sheet is fed so as to pass through the mold in an orientation in which its thickness direction coincides with the second direction (Claim 5).

[0015] According to this configuration, a fiber-reinforced resin foam in which sheet-like reinforcing fibers are contained in a matrix resin can be continuously produced.

[0016] In the above configuration, preferably, in the preparation step, a plurality of the reinforcing fiber sheets are prepared, in the feeding step, the reinforcing fiber sheets are fed out so that the plurality of the reinforcing fiber sheets pass through the die while being spaced apart from one another in the second direction, and in the extrusion step, the matrix resin is extruded from the die at a position between adjacent reinforcing fiber sheets (Claim 6).

[0017] According to this configuration, it is possible to continuously produce a fiber-reinforced resin foam having increased mechanical strength by incorporating a plurality of sheet-like reinforcing fibers in a matrix resin. In addition, since the matrix resin can be expanded so as to fill the gaps between the reinforcing fiber sheets, the porosity of the fiber-reinforced resin foam can also be increased. Effect of the Invention

[0018] As described above, according to the manufacturing method of the present invention, a fiber-reinforced resin foam having both improved heat insulating performance and mechanical strength can be manufactured. [Brief description of the drawings]

[0019] [Figure 1] 1 is a schematic side view, partially in cross section, showing an apparatus for producing a composite molded product (fiber-reinforced resin foam) according to a first embodiment of the present invention. [Diagram 2] 1 is a schematic plan view, partially in cross section, showing an apparatus for producing a composite molded product according to a first embodiment of the present invention. [Diagram 3] 2 is a schematic side view of the mold shown in FIG. 1 as viewed from the downstream side in the conveying direction. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. [Diagram 5] 1 is a flowchart showing an outline of the procedure of a manufacturing method according to a first embodiment of the present invention. [Figure 6] FIG. 2 is a diagram showing a state in which a foaming agent-containing matrix resin is extruded from the mold shown in FIG. [Figure 7] 1 is a diagram showing a cross-sectional structure of a composite molded product according to a first embodiment of the present invention. [Figure 8]FIG. 11 is a diagram for explaining a manufacturing method of a composite molded product in accordance with a second embodiment of the present invention, in which (a) is a schematic side view of a mold seen from the downstream side in the conveying direction, and (b) is a diagram showing the cross-sectional structure of the composite molded product. [Figure 9] FIG. 11 is a diagram for explaining a manufacturing method of a composite molded product in accordance with a third embodiment of the present invention, in which (a) is a schematic side view of a mold seen from the downstream side in the conveying direction, and (b) is a diagram showing the cross-sectional structure of the composite molded product. [Figure 10] FIG. 11 is a diagram for explaining a manufacturing method of a composite molded product in accordance with a fourth embodiment of the present invention, in which (a) is a schematic side view of a mold seen from the downstream side in the conveying direction, and (b) is a diagram showing the cross-sectional structure of the composite molded product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] FIG. 1 is a schematic side view of an apparatus used in a manufacturing method of a composite molded product (fiber-reinforced resin foam) according to a first embodiment of the present invention, that is, an apparatus for manufacturing a composite molded product. FIG. 2 is a schematic plan view of the apparatus for manufacturing a composite molded product. Hereinafter, this apparatus will be simply referred to as a manufacturing apparatus. A composite molded product 10 manufactured in the first embodiment is a composite molded product 10 including a base material 11 made of a foamed resin and reinforcing fibers 12 arranged in the base material 11, as shown in FIG. 7 described later. In the first embodiment, the composite molded product 10 includes, as the reinforcing fibers 12, four rod-shaped reinforcing fiber bundles 1 that are bundles of reinforcing fibers.

[0021] As shown in FIGS. 1 and 2, the manufacturing apparatus 100 includes an extruder 20, a die 30 communicating with the extruder 20, a cooler 40, a take-up machine 50, and a cutter 60. The take-up machine 50 is a take-up machine.

[0022] In the first embodiment, the reinforcing fibers 12 (reinforcing fiber bundles 1) are transported (sent out) approximately horizontally, and hereinafter, the transport direction of the reinforcing fibers 12 along the horizontal plane, which is the left-right direction in Figs. 2 and 3, will be simply referred to as the transport direction. Also, the direction perpendicular to the transport direction and the up-down direction and perpendicular to the paper surface of Fig. 2 will be referred to as the width direction. Here, the above transport direction is the "first direction" in the claims, and in the first embodiment, the up-down direction corresponds to the "second direction" in the claims, and the width direction corresponds to the "third direction."

[0023] (Configuration of manufacturing equipment) The extruder 20 has a cylinder 21 with a storage chamber 22 formed therein capable of storing a fluid, and a screw 26 housed in the storage chamber 22. The screw 26 has a shaft body 27 extending along the central axis of the cylinder 21, and screw blades 28 arranged in a spiral shape on the outer circumferential surface of the shaft body 27. The screw 26 pumps the fluid in the storage chamber 22 along the central axis of the shaft body 27 by the shaft body 27 being driven to rotate about its central axis by a drive device 29. Hereinafter, the direction along the central axis of the shaft body 27 of the screw 26 and the central axis of the cylinder 21 will be referred to as the cylinder axial direction, and the downstream side of the direction of transport of the fluid by the screw 26 will be referred to as the tip side, and the opposite side will be referred to as the base side.

[0024] The cylinder 21 has a first input section 24 into which the matrix resin 2 is input, and a second input section 25 into which the foaming agent 3 is input. In the cylinder axial direction, the first input section 24 is located closer to the base end than the second input section 25. An introduction section 23 that communicates with the storage chamber 22 and opens to the outside of the cylinder 21 is provided at the tip of the cylinder 21 (the end on the tip side in the cylinder axial direction).

[0025] Fig. 3 is a schematic side view of the mold 30 as viewed from the downstream side in the conveying direction. Fig. 4 is a cross-sectional view taken along line IV-IV in Fig. 3.

[0026] The mold 30 has an outer shape of a substantially rectangular parallelepiped. The mold 30 has a through-hole 36 penetrating it in the conveying direction. In the first embodiment, four through-holes 36 are arranged side by side in a state spaced apart from each other in the width direction. Each through-hole 36 has the same configuration. Specifically, each through-hole 36 has a substantially cylindrical shape extending in the conveying direction. As described later, one reinforcing fiber bundle 1 is inserted into each of these through-holes 36. Thus, the hole diameter of each through-hole 36 is set to a dimension equal to or larger than the outer diameter of the reinforcing fiber bundle 1.

[0027] The mold 30 is formed with a cavity 30c that communicates with the introduction portion 23 of the cylinder 21 and opens to a surface (hereinafter, appropriately referred to as the opening surface 30a) on the downstream side in the conveying direction of the mold 30. The cavity 30c opens to portions of the opening surface 30a that are spaced apart on both sides in the up-down direction from the opening ends 36a of each of the through portions 36.

[0028] Specifically, the cavity 30c has an inlet portion 31, two main passages 32 that branch out vertically from the inlet portion 31 and extend in the width direction, and a plurality of branch passages 34 that extend downstream in the conveying direction from different positions in the width direction of each main passage 32 and open to the opening surface 30a. Five branch passages 34 extend from each main passage 32. The inlet portion 31 opens on one side surface in the width direction of the mold 30 and communicates with the introduction portion 23 of the cylinder 21 through this opening portion. The upper main passage 32 passes above the four through-holes 36, and the lower main passage 32 passes below the four through-holes 36.

[0029] The ten branch passages 34 have the same configuration. These branch passages 34 have a generally cylindrical shape extending in the conveying direction. The five branch passages 34 extending from the same main passage 32 are arranged parallel to each other in the width direction and open to the opening surface 30a with gaps between them in the width direction. The five branch passages 34 extending from the upper main passage 32 open to the opening surface 30a at positions spaced upward from the opening ends 36a of the respective through-portions 36, and the five branch passages 34 extending from the lower main passage 32 open to the opening surface 30a at positions spaced downward from the opening ends 36a of the respective through-portions 36. The vertical separation distance between the opening end 34a of the upper branch passage 34 and the opening end 36a of the through portion 36 is set to be the same as the vertical separation distance between the opening end 34a of the lower branch passage 34 and the opening end 36a of the through portion 36, and the through portion 36 is located approximately in the vertical center of the upper branch passage 34 and the lower branch passage 34. The opening ends 34a of the branch passages 34 on both sides in the width direction are located on both sides in the width direction outside the opening ends 36a of the through portions 36 on both sides in the width direction. The diameter of the opening end 34a of each branch passage 34 is larger than the diameter of the opening end 36a of the through portion 36, and the opening area of ​​each branch passage 34 is set to be larger than the opening area of ​​the through portion 36.

[0030] As described later, the foaming agent-containing matrix resin 4 is extruded from the opening end 34a of each branch passage 34, and the foaming agent-containing matrix resin 4 envelops the reinforcing fiber bundles 1 that have passed through the opening end 36a of the through-hole 36, thereby forming the composite molded product 10.

[0031] The cooling machine 40 is provided downstream of the mold 30 in the conveying direction. The cooling machine 40 cools and shapes the composite molded article 10 sent out from the mold 30. The cooling machine 40 has a cavity (hereinafter, appropriately referred to as a molding cavity 41) that penetrates the cooling machine 40 in the conveying direction. The molding cavity 41 has a cross section that is approximately the same as the cross section of the composite molded article 10 (finished product). The cooling machine 40 cools and shapes the composite molded article 10 as it passes through the molding cavity 41.

[0032] The take-off machine 50 is provided downstream of the cooling machine 40 in the conveying direction. The take-off machine 50 has a plurality of pairs of rollers 51 and a pair of endless belts 52 that are arranged in the vertical direction and are wound around the rollers 51. The take-off machine 50 sends out the composite molded product 10 downstream in the conveying direction by rotating the rollers 51 in a state in which the composite molded product 10 after molding sent out from the cooling machine 40 is sandwiched from above and below by the endless belts 52. Here, as described later, the composite molded product 10 includes a reinforcing fiber bundle 1, and the take-off machine 50 sends out the composite molded product 10 and simultaneously sends out the reinforcing fiber bundle 1 downstream in the conveying direction.

[0033] The cutting machine 60 is disposed downstream in the conveying direction of the take-off machine 50. The cutting machine 60 has a conveying section 62 that receives the composite molded article 10 sent out from the take-off machine 50, and a cutter 61 disposed on the conveying section 62. The cutting machine 60 cuts the composite molded article 10 on the conveying section 62 with the cutter 61.

[0034] (Method of manufacturing composite molded products) 5 is a flowchart showing an outline of the steps of a method for producing a composite molded article 10 (fiber-reinforced resin foam) using the manufacturing apparatus 100. The method for producing the composite molded article 10 includes a preparation step S1, a feeding step S2, a kneading step S3, an extrusion step S4, a cooling / molding step S5, and a cutting step S6.

[0035] [Preparation process] In the preparation step S1, the reinforcing fibers 12 to be contained in the composite molded product 10 are prepared. In the first embodiment, four reinforcing fiber bundles 1 are prepared in the preparation step S1. Specifically, four reinforcing fiber bundle rolls 1R around which the reinforcing fiber bundles 1 are wound are prepared.

[0036] [Feed process] In the feeding step S2, the reinforcing fiber bundle 1 is fed downstream in the conveying direction. In the first embodiment, four reinforcing fiber bundles 1 are fed out in a state in which they are spaced apart from each other in the width direction and pass through each of the through-holes 36 of the mold 30. Specifically, the reinforcing fiber bundle rolls 1R are supported by the guide rollers 55. Each reinforcing fiber bundle 1 is pulled out from the guide rollers 55, passes through each of the through-holes 36, and is introduced between the endless belts 52 of the take-off machine 50. Each reinforcing fiber bundle 1 is fed out from the guide rollers 55 toward the mold 30 and from the mold 30 toward the take-off machine 50 together with the composite molded product 10 by the take-off machine 50 feeding the composite molded product 10 including the reinforcing fiber bundle 1 downstream in the conveying direction.

[0037] [Kneading process] In the kneading step S3, the foaming agent 3 and the matrix resin 2 are charged into the extruder 20, and the foaming agent 3 and the matrix resin 2 are kneaded in the extruder 20.

[0038] In the first embodiment, the foaming agent 3 and the matrix resin 2 are separately fed into the extruder 20, and are kneaded in the extruder 20. Specifically, the matrix resin 2 is fed into the accommodation chamber 22 of the extruder 20 from the first feeding portion 24 of the cylinder 21, the foaming agent 3 is fed into the accommodation chamber 22 from the second feeding portion 25, and the matrix resin 2 and the foaming agent 3 are kneaded in the accommodation chamber 22 by the rotation of the screw 26 of the extruder 20. Hereinafter, the matrix resin 2 into which the foaming agent 3 is mixed and in which the foaming agent 3 is not yet foamed is referred to as a foaming-agent-containing matrix resin 4. The screw 26 of the extruder 20 is continuously rotated at least during the period from the start to the end of the production of the composite molded product 10.

[0039] In the first embodiment, a thermoplastic resin is used as the matrix resin 2. The first input section 24 is in communication with a hopper 81 that stores the matrix resin 2, and the matrix resin 2 is introduced from the hopper 81 into the storage chamber 22 through the first input section 24. For example, any of polyamide (particularly PA6, PA9T, PA12), polyethylene, polypropylene, polyphenylene sulfide, polyester, polyacetal, polycarbonate, acrylic resin, acrylonitrile-butadiene-styrene copolymer (ABS), polyamideimide, polysulfone, polyphenylsulfone, polyetherimide, polyethersulfone, polyetheretherketone, polyetherketoneketone, polyimide, polyarylate, fluororesin, liquid crystal polymer, and thermoplastic epoxy resin can be used as the matrix resin 2. Alternatively, a polymer alloy in which two or more of these thermoplastic resins are mixed may be used as the matrix resin 2.

[0040] In the first embodiment, liquefied carbon dioxide is used as the foaming agent 3. The second input part 25 is connected to a cylinder 82 that stores liquefied carbon dioxide, and carbon dioxide as the foaming agent 3 is introduced into the storage chamber 22 from the cylinder 82 via the second input part 25.

[0041] [Extrusion process] In the extrusion step S4, the extruder 20 pressure-feeds the foaming agent-containing matrix resin 4 into the mold 30, and extrudes the foaming agent-containing matrix resin 4 out of the mold 30 while foaming the foaming agent 3 to expand the matrix resin 2.

[0042] Specifically, the foaming agent-containing matrix resin 4 is introduced into the inlet 31 of the mold 30 through the introduction section 23 while being pressurized by the rotation of the screw 26. The foaming agent-containing matrix resin 4 branches from the inlet 31 into each of the main passages 32, and is then forced into each of the branch passages 34 and extruded out of the mold 30 from the open ends 34a of each of the branch passages 34.

[0043] The pressure in the cavity 30c of the mold 30 including the branch passage 34 is increased by the action of the screw 26. Therefore, when the matrix resin 4 containing the foaming agent is extruded to the outside from the mold 30, the pressure applied thereto is reduced. As a result, the foaming agent 3 in the matrix resin 4 containing the foaming agent is foamed by being extruded to the outside of the mold 30. In the first embodiment, carbon dioxide is used as the foaming agent 3 as described above, and the carbon dioxide foams. When the foaming agent (carbon dioxide) 3 foams, bubbles 3a are generated in the matrix resin 2, and the bubbles 3a grow in the matrix resin 2. This causes the matrix resin 2 to expand. Note that the pressure on the downstream side (opening surface 30a side) of the cavity 30c of the mold 30 is lower than the pressure on the upstream side (screw 26 side), so the pressure applied to the matrix resin 4 containing the foaming agent is also reduced during the passage through the mold 30. Therefore, although some of the foaming agent may foam during the passage through the mold 30, the generated bubbles 3a mainly grow outside the mold 30.

[0044] Fig. 6 corresponds to Fig. 4 and is a schematic diagram showing how the foaming agent-containing matrix resin 4 is extruded from the die 30. In Fig. 6 and Fig. 2, the gradual increase in the width dimension of the matrix resin 2 from the opening surface 30a of the die 30 toward the downstream side in the conveying direction represents the expansion of the matrix resin 2. Similarly, in Fig. 1, the gradual increase in the vertical dimension of the matrix resin 2 from the opening surface 30a of the die 30 toward the downstream side in the conveying direction represents the expansion of the matrix resin 2.

[0045] As shown in Figures 1 and 6, the matrix resin 2 extruded from the mold 30 expands until the matrix resin 2 extruded from the open ends 34a of adjacent branch passages 34 in the width direction and up and down direction come into contact with each other and become integrated.

[0046] Here, as described above, the open end 34a of each branch passage 34 is open above and below the open end 36a of the through portion 36. As a result, the matrix resins 2 extruded from the open ends 34a of the branch passages 34 adjacent to each other in the vertical direction expand until they are integrated with each other, and as shown in FIG. 1, the reinforcing fiber bundles 1 that have passed through the through portions 36 are taken into the inside of these matrix resins 2, and a composite molded product 10 containing the reinforcing fiber bundles 1 is molded. In the first embodiment, as described above, the open end 36a of each through portion 36 is located at approximately the center in the vertical direction of the open ends 34a of the upper and lower branch passages 34. In addition, the open ends 36a of each through portion 36 are arranged at approximately equal intervals in the width direction. As a result, a composite molded product 10 in which the reinforcing fiber bundles 1 are arranged at equal intervals in the width direction at the center in the vertical direction of the matrix resin 2 is molded as the composite molded product 10.

[0047] [Cooling / forming process] In the cooling and molding step S5, the composite molded article 10 is cooled and molded by the cooler 40. Specifically, the composite molded article 10 is sent into the molding cavity 41 of the cooler 40 by the take-up machine 50, and is cooled by passing through it. The cooler 40 cools the composite molded article 10 until the temperature of the matrix resin 2 after expansion is completed drops below the softening temperature of the material (thermoplastic resin). This hardens the matrix resin 2. In addition, by passing through the molding cavity 41, the cross section of the composite molded article 10 is molded into a shape corresponding to the cross section of the molding cavity 41.

[0048] [Cutting process] In the cutting process S6, the composite molded article 10 is cut to a predetermined length by the cutting machine 60. Specifically, the composite molded article 10 is sent to the conveying section 62 of the cutting machine 60 by the take-up machine 50, and is cut to the predetermined length by the cutter 61 of the cutting machine 60 during the conveying. This completes the composite molded article 10 having the predetermined length. The cut composite molded article 10 is then conveyed further downstream in the conveying direction by the conveying section 62.

[0049] Fig. 7 is a diagram showing a cross section of a composite molded product 10 after molding. As shown in Fig. 7, the composite molded product 10 has a substantially rectangular cross section, and includes a base material 11 made of a matrix resin 2, and a plurality of reinforcing fiber bundles 1 contained in the base material 11. A large number of air bubbles (cavities) 3a generated by foaming of a foaming agent 3 are formed in the base material 11. The reinforcing fiber bundles 1 are contained in the base material 11 in a state in which they are continuous in the longitudinal direction and dispersed in the width direction inside the base material 11. In the first embodiment, as described above, four reinforcing fibers 12 are arranged at equal intervals in the width direction at substantially the center in the vertical direction of the base material 11.

[0050] (effect, etc.) As described above, in the first embodiment of the present invention, the reinforced fiber bundle 1 is sent out so as to pass through the through-hole 36 provided inside the mold 30. Then, the foaming agent-containing matrix resin 4 is pressure-fed into the mold 30 and pushed out of the mold 30 at both positions in the vertical direction of the through-hole 36, so that the foaming agent 3 foams and the matrix resin 2 expands outside the mold 30. Therefore, the matrix resin 2 can be expanded so as to cover the reinforced fiber bundle 1, so that the reinforced fiber bundle 1 can be encapsulated in the matrix resin 2, and the matrix resin 2 and the reinforced fiber bundle 1 can be sufficiently adhered to each other. Therefore, a composite molded product 10 (fiber-reinforced resin foam) having increased mechanical strength and having heat insulating performance secured by including air bubbles 3a can be continuously manufactured.

[0051] Moreover, the open end 34a of the branch passage 34 through which the foaming agent-containing matrix resin 4 is extruded is provided at a position spaced apart in the vertical direction from the open end 36a of the through-hole 36, so that the foaming agent-containing matrix resin 4 is extruded from the mold 30 at a position spaced apart in the vertical direction from the position through which the reinforced fiber bundle 1 passes. This makes it possible to prevent the reinforced fiber bundle 1 from hindering the vertical expansion of the matrix resin 2, and allows the matrix resin 2 to expand at a high rate. This makes it possible to increase the porosity of the composite molded product 10 (fiber reinforced resin foam), and to produce a fiber reinforced resin foam with high thermal insulation performance.

[0052] Furthermore, in the first embodiment, the opening ends 34a of the branch passages 34 are spaced apart from each other in the width direction above and below the opening ends 36a of the through-holes 36, and the foaming agent-containing matrix resin 4 is extruded from the mold 30 in a state of being spaced apart from each other in the width direction as well. Therefore, the matrix resins 2 extruded from the opening ends 34a of the branch passages 34 adjacent to each other in the width direction can be expanded so as to fill the gaps between them, and the matrix resin 2 can be expanded at a sufficient magnification in the width direction as well. This makes it possible to further increase the porosity and heat insulating performance of the composite molded product 10 (fiber reinforced resin foam).

[0053] Second embodiment Next, a method for producing a composite molded product (reinforced fiber resin foam) according to the second embodiment will be described with reference to Fig. 8(a) and (b). Fig. 8(a) corresponds to Fig. 3 and is a schematic side view of a mold 230 as viewed from the downstream side in the conveying direction. Fig. 8(b) is a diagram showing the cross-sectional structure of a composite molded product 210. Note that Fig. 8(a) also shows a reinforcing fiber bundle 1.

[0054] In the second embodiment, a plurality of reinforcing fiber bundles 1 are encapsulated in a matrix resin 2 (substrate 11) as in the first embodiment. On the other hand, in the second embodiment, a plurality of reinforcing fiber bundles 1 are encapsulated in the matrix resin 2 so as to be aligned in the vertical and width directions.

[0055] Specifically, in the second embodiment, as shown in FIG. 8(a), a die 230 is used in which a plurality of through-holes 236 are arranged in a row spaced apart from each other in the width direction, and the rows are arranged at positions spaced apart from each other in the vertical direction. In addition, a die 230 is used in which a plurality of branch passages 234 are provided between the rows of the through-holes 236 and at positions spaced apart above and below the region in which the through-holes 236 are provided, and are spaced apart from each other in the width direction. Then, in the preparation step, the same number of reinforced fiber bundles 1 as the number of the through-holes 236 are prepared, and in the feeding step, these reinforced fiber bundles 1 are fed so as to pass through each of the through-holes 236. As described above, the through-holes 236 are arranged in a lattice pattern in the width direction and the vertical direction. Therefore, the reinforced fiber bundles 1 are fed so as to pass through the die 230 in a state spaced apart from each other in the width direction and the vertical direction by being fed so as to pass through the through-holes 236.

[0056] Similarly to the first embodiment, the matrix resin 2 and the foaming agent 3 are mixed in the extruder 20, and the foaming agent-containing matrix resin 4 is extruded from each branch passage 234, and the matrix resin 2 is expanded by foaming of the foaming agent 3. However, in the second embodiment, as described above, the branch passages 234 are provided between the rows of the through-holes 236 aligned in the width direction, that is, between the through-holes 236 adjacent in the up-down direction. As a result, the foaming agent-containing matrix resin 4 is extruded from the die 230 at positions between the reinforcing fiber bundles 1 adjacent in the up-down direction.

[0057] In the second embodiment, the matrix resin 4 containing the foaming agent is extruded to the outside of the mold 230 at positions spaced above and below the through-hole 236, so that the matrix resin 2 expands at a high rate. Therefore, in the second embodiment, a composite molded product 210 can be manufactured in which the substrate 11 made of a foamed resin and having a high porosity and the reinforcing fiber bundles 1 are contained in the substrate 11, that is, a fiber-reinforced resin foam with ensured heat insulating performance and enhanced mechanical strength. In particular, in the second embodiment, as shown in FIG. 8(b), a plurality of reinforcing fiber bundles 1 are arranged in different positions in the vertical direction in addition to the width direction inside the substrate 11. Therefore, a fiber-reinforced resin foam with enhanced mechanical strength can be manufactured.

[0058] Third embodiment Next, a manufacturing method of a composite molded product (reinforced fiber resin foam) according to the third embodiment will be described with reference to Fig. 9(a) and (b). Fig. 9(a) corresponds to Fig. 3 and is a schematic side view of a mold 330 as seen from the downstream side in the conveying direction. Fig. 9(b) is a diagram showing the cross-sectional structure of a composite molded product 310. Fig. 9(a) also shows a reinforcing fiber sheet 301, which will be described later.

[0059] In the third embodiment, unlike the first and second embodiments, the reinforcing fibers 12 are in the form of a sheet and are embedded in the matrix resin 2 (substrate 11).

[0060] Specifically, in the third embodiment, as shown in FIG. 9(a), a die 330 having a through-hole 336 extending in the width direction and a plurality of branch passages 334 arranged in the width direction at positions spaced apart above and below the through-hole 336 is used. In the third embodiment, in the preparation step, a reinforcing fiber sheet 301 in which reinforcing fibers are gathered in a sheet shape is prepared as the reinforcing fibers 12. For example, the reinforcing fibers are opened and formed into a sheet shape and prepared as the reinforcing fiber sheet 301. Then, in the feeding step, the reinforcing fiber sheet 301 is fed so as to pass through the above-mentioned through-hole 336. As described above, the through-hole 336 extends in the width direction. Therefore, the reinforcing fiber sheet 301 is fed so as to pass through the die 330 in a posture extending in the width direction, that is, in a posture in which the thickness direction of the reinforcing fiber sheet 301 coincides with the up-down direction, by being fed so as to pass through the through-hole 336.

[0061] The other configurations are the same as those of the first embodiment. The matrix resin 2 and the foaming agent 3 are mixed in the extruder 20, and the foaming agent-containing matrix resin 4 is extruded from each branch passage 334, and the matrix resin 2 is expanded by the foaming of the foaming agent 3.

[0062] As a result, in the third embodiment, as shown in FIG. 9(b), a composite molded product 310 is formed in which the base material 11 made of foamed resin and the reinforcing fiber sheet 301 are embedded in the base material 11.

[0063] Also in the third embodiment, the matrix resin 4 containing a foaming agent is extruded out of the mold 330 at positions spaced above and below the through-hole 336, so that the matrix resin 2 expands at a high expansion ratio. Therefore, also in the third embodiment, it is possible to produce a composite molded product 310 in which the substrate 11 made of a foamed resin and having a high porosity and the substrate 11 contains reinforcing fibers 12, that is, a fiber-reinforced resin foam in which heat insulating performance is ensured and mechanical strength is increased.

[0064] (Fourth embodiment) Next, a manufacturing method of a composite molded product (reinforced fiber resin foam) according to the fourth embodiment will be described with reference to Fig. 10(a) and (b). Fig. 10(a) corresponds to Fig. 3 and is a schematic side view of a mold 430 as seen from the downstream side in the conveying direction. Fig. 10(b) is a diagram showing the cross-sectional structure of a composite molded product 410. Note that Fig. 10(a) also shows a reinforcing fiber sheet 301.

[0065] In the fourth embodiment, unlike the third embodiment, a plurality of reinforcing fiber sheets 301 are embedded in a matrix resin 2 (substrate 11) in a state where they are spaced apart from one another in the vertical direction.

[0066] Specifically, in the fourth embodiment, as shown in FIG. 10(a), a mold 430 is used in which a plurality of through-holes 436 each extending in the width direction are provided at positions spaced apart from each other in the vertical direction. In the example of FIG. 10(a), the through-holes 436 are arranged at equal intervals in the vertical direction. In addition, a mold 430 is used in which a plurality of branch passages 434 are provided between the through-holes 436 and at positions spaced apart from each other in the width direction at positions spaced apart above and below the region in which the through-holes 436 are provided. Then, in the preparation step, the same number of reinforcing fiber sheets 301 as the number of the through-holes 436 are prepared, and in the feeding step, these reinforcing fiber sheets 301 are fed so as to pass through the through-holes 436. As described above, the through-holes 436 are arranged at positions spaced apart from each other in the vertical direction. Therefore, the reinforcing fiber sheets 301 are fed so as to pass through the mold 430 in a state spaced apart from each other in the vertical direction.

[0067] Similarly to the first embodiment, the matrix resin 2 and the foaming agent 3 are mixed in the extruder 20, and the foaming agent-containing matrix resin 4 is extruded from each branch passage 434, and the matrix resin 2 is expanded by foaming of the foaming agent 3. However, in the fourth embodiment, as described above, the branch passages 434 are provided between the through-holes 436. As a result, the foaming agent-containing matrix resin 4 is extruded from the die 430 at a position between the reinforcing fiber sheets 301.

[0068] In the fourth embodiment, the matrix resin 4 containing the foaming agent is extruded to the outside of the mold 430 at positions spaced above and below the through-hole 436, so that the matrix resin 2 expands at a high rate. Therefore, in the fourth embodiment, a composite molded product 410 can be manufactured in which the substrate 11 made of a foamed resin and having a high porosity and the substrate 11 contains reinforcing fibers 12, that is, a fiber-reinforced resin foam with good heat insulating properties and improved mechanical strength can be manufactured. In particular, in the fourth embodiment, as shown in FIG. 10(b), a plurality of reinforcing fiber sheets 301 are disposed at different positions in the vertical direction inside the substrate 11. Therefore, a fiber-reinforced resin foam with improved mechanical strength can be manufactured.

[0069] (Other variations) In the above embodiment, the case where liquefied carbon dioxide is used as the foaming agent has been described, but the type of foaming agent is not limited to this. For example, water may be used as the foaming agent. In addition, other physical foaming agents, chemical foaming agents, or supercritical fluids may be used as the foaming agent. When using a chemical foaming agent that starts foaming when heated, the mold may be heated by a heater or the like.

[0070] In the above embodiment, the foaming agent and the matrix resin are separately charged into the extruder 20. However, a mixture of these may be introduced into the extruder 20. For example, when a chemical foaming agent is used as the foaming agent, the chemical foaming agent and the matrix resin may be mixed in advance, and the mixture of the chemical foaming agent and the matrix resin may be introduced into the extruder 20.

[0071] In the above embodiment, the case where a thermoplastic resin is used as the matrix resin has been described, but the matrix resin is not limited to this. For example, a thermosetting resin may be used as the matrix resin. [Explanation of symbols]

[0072] 1 Reinforced fiber bundle 2. Matrix resin 3. Foaming Agent 10 Composite molded product (fiber reinforced resin foam, first embodiment) 12 Reinforced Fiber 20 Extruder 30 Mold 210 Composite molded product (fiber reinforced resin foam, second embodiment) 310 Composite molded product (fiber reinforced resin foam, third embodiment) 410 Composite molded product (fiber reinforced resin foam, fourth embodiment) S1 Preparation process S2 Feeding process S3 kneading process S4 Extrusion process

Claims

1. A method for producing a fiber-reinforced resin foam containing a foamed resin and reinforcing fibers, using an extruder and a die communicating with the extruder, A feeding step of feeding reinforcing fibers along a predetermined first direction so as to pass through an interior of the mold; a kneading step of feeding a matrix resin and a foaming agent into the extruder and kneading the matrix resin and the foaming agent in the extruder; an extrusion step of feeding the matrix resin mixed with the foaming agent into the mold by the extruder, and extruding the matrix resin introduced into the mold to the outside of the mold while foaming the foaming agent to expand the matrix resin, A method for producing a fiber-reinforced resin foam, characterized in that, when a direction perpendicular to the first direction is defined as a second direction, in the extrusion process, the matrix resin is extruded from the mold at positions spaced apart on both sides of the reinforcing fibers in the second direction, and the matrix resin is expanded on both sides of the reinforcing fibers in the second direction.

2. The method for producing a fiber-reinforced resin foam according to claim 1, A method for producing a fiber-reinforced resin foam, characterized in that, when a direction perpendicular to the first direction and the second direction is defined as a third direction, in the extrusion process, the matrix resin is extruded from the mold at multiple positions spaced apart from each other in the third direction.

3. The method for producing a fiber-reinforced resin foam according to claim 1 or 2, The method further includes a preparation step of preparing a plurality of rod-shaped reinforcing fiber bundles which are bundles of the reinforcing fibers, A method for producing a fiber-reinforced resin foam, characterized in that, when a direction perpendicular to the first direction and the second direction is defined as a third direction, in the feeding process, the reinforcing fiber bundles are fed out so that the reinforcing fiber bundles pass through the mold while being spaced apart from each other in the third direction.

4. The method for producing a fiber-reinforced resin foam according to claim 3, In the feeding step, the reinforcing fiber bundles are fed so that the reinforcing fiber bundles pass through the die while being spaced apart from each other in the second direction, A method for producing a fiber-reinforced resin foam, characterized in that in the extrusion step, the matrix resin is extruded from the mold at a position between the reinforcing fiber bundles adjacent to each other in the second direction.

5. The method for producing a fiber-reinforced resin foam according to claim 1 or 2, The method further includes a preparation step of preparing a reinforcing fiber sheet in which the reinforcing fibers are assembled in a sheet shape, A method for producing a fiber-reinforced resin foam, characterized in that in the feeding process, the reinforcing fiber sheet is fed so as to pass through the mold in an orientation in which its thickness direction coincides with the second direction.

6. The method for producing a fiber-reinforced resin foam according to claim 5, In the preparation step, a plurality of the reinforcing fiber sheets are prepared, In the feeding step, the reinforcing fiber sheets are fed so that the reinforcing fiber sheets pass through the mold while being spaced apart from each other in the second direction, The method for producing a fiber-reinforced resin foam, wherein in the extrusion step, the matrix resin is extruded from the mold at a position between adjacent reinforcing fiber sheets.

Citation Information

Patent Citations

  • JP1975054663A

  • Method of producing reinforced thermoplastic resin foam

    JP1976144466A

  • Fiber-reinforced thermoplastic resin foam

    JP1996300537A

  • Ply material manufacturing method and pneumatic tire using the ply material