Unit stack cell structure and all-solid-state secondary battery including the same

The unit stack cell structure with an elastic layer addresses the efficiency and stability issues in all-solid-state secondary batteries by uniformly pressurizing the solid electrolyte and absorbing volume changes, enhancing discharge efficiency and preventing short circuits.

JP7590471B2Active Publication Date: 2024-11-26SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023007480
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-20
Filing Date
2023-01-20
Publication Date
2024-11-26
Estimated Expiration
2043-01-20

AI Technical Summary

Technical Problem

All-solid-state secondary batteries face issues with low Coulombic efficiency due to changes in the thickness of the negative electrode during charging and discharging, leading to stress on the solid electrolyte and potential short circuits.

Method used

A unit stack cell structure is designed with a laminate configuration of positive electrode, solid electrolyte, negative electrode, and an elastic layer with a compressive strength of 0.28 MPa to 0.6 MPa, dispersing stress and maintaining uniform pressure, thereby improving the contact between the negative electrode and solid electrolyte.

Benefits of technology

The structure enhances discharge efficiency and maintains high Coulombic efficiency by uniformly pressurizing the solid electrolyte and absorbing volume changes in the negative electrode, reducing the risk of short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590471000002
    Figure 0007590471000002
  • Figure 0007590471000003
    Figure 0007590471000003
  • Figure 0007590471000004
    Figure 0007590471000004
Patent Text Reader

Abstract

To provide a unit stack cell structure and an all-solid secondary battery including the same.SOLUTION: A unit stack cell structure includes a plurality of stacked unit cells, and the unit cell includes a laminate in which a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and an elastic layer are sequentially arranged, the compressive strength of the elastic layer is 0.28 MPa or more and less than 0.6 MPa. This makes it possible to provide an all-solid secondary battery with high coulombic efficiency even when the thickness of the negative electrode active material layer changes due to charging and discharging.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a unit stack cell structure and an all-solid-state secondary battery including the same. [Background technology]

[0002] Recently, in response to industrial demand, there has been active development of batteries with high energy density and stability. For example, lithium-ion batteries are being used not only in the fields of information-related devices and communication devices, but also in the field of automobiles. In particular, in the field of automobiles, safety is considered important because life is at stake.

[0003] Currently available lithium ion batteries use electrolytes that contain flammable organic solvents, and therefore there is a risk of overheating and fire if a short circuit occurs. In response to this, all-solid-state secondary batteries that use solid electrolytes instead of electrolytes have been proposed. All-solid-state secondary batteries do not use flammable organic solvents, and can greatly reduce the possibility of fire or explosion even if a short circuit occurs. Therefore, such all-solid-state secondary batteries can be significantly safer than lithium ion batteries that use electrolytes.

[0004] All-solid-state secondary batteries using a solid electrolyte, for example, a sulfide-based solid electrolyte, cannot be used in a state exposed to the atmosphere due to the nature of the solid electrolyte, and must be isolated from the atmosphere. For this reason, the all-solid-state secondary battery can be manufactured by injecting it into an exterior body using a laminate film or a material with rigidity, thereby isolating the all-solid-state secondary battery from the atmosphere.

[0005] However, when the lamination agent of the all-solid-state secondary battery is injected into the exterior body or compressed using a laminate film after lamination, or when the all-solid-state secondary battery is pressurized, stress is transmitted to the solid electrolyte, causing cracks and resulting in a short circuit. In addition, after pressurization, the thickness of the negative electrode changes in a state where stress is accumulated or in a charge / discharge environment, and at this time, cracks in the solid electrolyte may occur, resulting in a short circuit.

[0006] In particular, if pressure is not applied uniformly from the outside during discharging of an all-solid-state secondary battery, the lithium ion migration speed decreases and the discharge efficiency decreases, and if pressure is applied locally, lithium ions move to the pressurized area, resulting in low discharge efficiency. Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a unit stack cell structure having high Coulomb efficiency even when the thickness of the negative electrode varies due to charging and discharging.

[0008] Another object of the present invention is to provide an all-solid-state secondary battery including the unit stack cell structure. [Means for solving the problem]

[0009] According to one aspect, there is provided a unit stack cell structure including a plurality of stacked unit cells, the unit cells including a laminate in which a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and an elastic layer are sequentially arranged, and the elastic layer has a compressive strength of 0.28 MPa or more and less than 0.6 MPa.

[0010] In another aspect, there is provided an all-solid-state secondary battery including a plurality of stacked unit stack cell structures, the stacked unit stack cell structures being connected in a bipolar manner. Effect of the Invention

[0011] According to one aspect, the unit stack cell structure distributes stress applied to the solid electrolyte when an all-solid-state secondary battery including the unit stack cell structure is pressurized, thereby uniformly applying pressure, and has excellent restoring force under charge and discharge conditions, thereby uniformly applying pressure to the contact surface between the negative electrode and the solid electrolyte during discharge, thereby improving discharge efficiency. In addition, even if the thickness of the negative electrode active material layer changes due to charge and discharge, an all-solid-state secondary battery with high Coulombic efficiency can be provided. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic cross-sectional view of a unit cell included in a unit stack cell structure according to an embodiment. [Diagram 2] FIG. 13 is a schematic cross-sectional view of a unit cell included in a unit stack cell structure according to another embodiment. [Diagram 3] FIG. 13 is a schematic cross-sectional view of a unit cell included in a unit stack cell structure according to still another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventive concept described below can be modified in various ways and can have various embodiments, and specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the present inventive concept to a specific embodiment, and it should be understood that the present inventive concept includes any modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.

[0014] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In the following, terms such as "include" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the situation.

[0015] In the drawings, thicknesses are exaggerated or reduced to clearly depict multiple layers and regions. Similar parts are designated by the same reference numerals throughout the specification. When a part, such as a layer, film, region, plate, etc., is described as being "on" or "above" another part throughout the specification, this does not only include the case where it is directly on top of the other part, but also the case where there is another part in between. Throughout the specification, terms such as first, second, etc. may be used to describe various components, but the components should not be limited by the terms. Terms are used only to distinguish one component from another.

[0016] In the case of an all-solid-state secondary battery, the Coulombic efficiency is also reduced due to the thickness fluctuation of the negative electrode active material layer caused by charging and discharging. When the thickness of the negative electrode active material layer increases during charging, stress is applied to the solid electrolyte layer and the negative electrode current collector, and an electrode reaction occurs in this state. In the stressed state, even if the solid electrolyte layer and the negative electrode current collector, i.e., the solid-state contact, are not good, the ion conduction path and the electron conduction path are likely to be secured. Conversely, when the thickness of the negative electrode active material layer decreases during discharging, the stress is relieved, and the contact state between the solids becomes poor. As a result, the ion conduction path and the electron conduction path are easily interrupted in the all-solid-state secondary battery, and the Coulombic efficiency is reduced.

[0017] In order to solve the above problem, the inventors have focused on the conformability of the negative electrode current collector. Specifically, even when the thickness of the negative electrode active material layer changes due to charging and discharging, the inventors have studied how to suppress deterioration of the contact state between solids by improving the conformability of the negative electrode current collector to the change, and have arrived at the present invention.

[0018] Hereinafter, a unit stack cell structure and an all-solid-state secondary battery including the same according to an illustrative embodiment will be described in more detail.

[0019] [Unit stack cell structure] According to an embodiment, the unit stack cell structure includes: The unit cell includes a plurality of stacked unit cells. The unit cell includes a laminate in which a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and an elastic layer are sequentially arranged, The elastic layer has a compressive strength of 0.28 MPa or more and less than 0.6 MPa.

[0020] FIG. 1 is a schematic diagram showing a structure of a unit cell included in a unit stack cell structure according to an embodiment.

[0021] 1, a unit cell 1 includes a laminate in which a positive electrode layer 10, a solid electrolyte layer 30, a negative electrode layer 20, and an elastic layer 40 are sequentially arranged. The positive electrode layer 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12 arranged on the positive electrode current collector 11, and the negative electrode layer 20 includes a negative electrode current collector 21 and a negative electrode active material layer 22 arranged on the negative electrode current collector 21.

[0022] In this way, the unit cell 1 included in the unit stack cell structure can increase the Coulomb efficiency of the all-solid-state secondary battery by disposing the elastic layer 40 having a compressive strength of 0.28 MPa or more and less than 0.6 MPa on the anode layer 20. The unit cell 1 including the elastic layer 40 can improve the conformity to the anode current collector 21 even when the thickness of the anode active material layer 22 changes due to charging and discharging, and can suppress the contact state between the solid electrolyte layer 30, which is a solid, and the anode current collector 21 from being deteriorated, thereby providing an all-solid-state secondary battery with high Coulomb efficiency. In addition, since the elastic layer 40 is disposed on the opposite side of the solid electrolyte layer 30 with respect to the anode current collector 21, there is an advantage that the elastic layer 40 can be prevented from reacting with the lithium of the anode layer 20 and being deteriorated. This aspect can also increase the Coulomb efficiency.

[0023] According to one embodiment, the unit stack cell structure has a structure in which a plurality of bi-cells, each of which has a pair of unit cells symmetrically arranged on both sides of a positive electrode current collector, are stacked. The bi-cells may be bipolarly connected. When a plurality of such bi-cells are stacked, an elastic layer is disposed between adjacent bi-cells to absorb a volume change of the negative electrode layer in the unit stack cell structure. The unit stack cell structure has an advantage in that it includes an elastic layer that absorbs a volume change of the negative electrode, thereby suppressing a volume change of the entire cell and obtaining a stable lifespan, and that it has both a stack and bipolar structure, allowing the capacity and voltage to be freely designed.

[0024] Each component will be described below. [Elastic layer] On the negative electrode layer 20 of the unit cell 1, an elastic layer 40 having a compressive strength of 0.28 MPa or more and less than 0.6 MPa, 0.28 MPa or more and less than 0.5 MPa, 0.28 MPa or more and less than 0.4 MPa, or 0.28 MPa or more and less than 0.35 MPa is disposed.

[0025] The compressive strength of the elastic layer 40 is 0.28 MPa or more and less than 0.6 MPa in the compression ratio range of 40 to 70%. For example, the compressive strength is 0.28 MPa or more and 0.5 MPa or less at a compression ratio of 40%, specifically, the compressive strength is 0.28 MPa or more and 0.4 MPa or less, and more specifically, the compressive strength is 0.28 MPa or more and 0.35 MPa or less. If the compressive strength of the elastic layer 40 is less than 0.28 MPa, the elastic sheet is compressed by 40% or more due to insufficient rigidity against pressure in the compression direction when the all-solid-state battery structure is assembled and pressurized, and a uniform surface pressure cannot be obtained, resulting in overcompression, and a high pressure is transmitted in the charge / discharge environment of the all-solid-state battery, causing a short circuit or the like. On the other hand, if the compressive strength of the elastic layer 40 is greater than 0.6 MPa in the compression ratio range of 70%, the interface resistance at the interface between solids cannot be reduced due to the non-uniform surface pressure when the all-solid-state battery structure is assembled and pressurized, causing a short circuit or other adverse effects on the lifespan. When the compressive strength of the elastic layer 40 is in the range of 0.28 MPa or more and less than 0.6 MPa, an all-solid-state secondary battery exhibiting high coulombic efficiency can be provided.

[0026] According to one embodiment, the stress relaxation rate of the elastic layer 40 is 5% to 20%, and the recovery rate is 60% or more, and the sum of the stress relaxation rate and the recovery rate is 78% to 95%. Within this range, the stress applied to the solid electrolyte when the cell stack is pressurized is distributed and pressurized uniformly, and a highly stress-relieving elastic layer can be provided that has excellent recovery force under charge and discharge conditions, that uniformly pressurizes the contact surface between the negative electrode and the solid electrolyte during discharge to increase discharge efficiency, and that is compressed due to an increase in the thickness of the negative electrode in a charging environment.

[0027] The stress relaxation rate of the elastic layer 40 is 5% to 20%, for example, 6.5% to 15%. Within this range, stress is dispersed even when the thickness of the all-solid-state secondary battery varies due to compression and charging / discharging, making it easier to apply uniform compression. The recovery rate of the elastic layer 40 is 60% or more, for example, 70% or more, or 80% or more. Within this range, excellent recovery force can be provided in the compression direction.

[0028] However, the sum of the stress relaxation rate and the recovery rate is 78% to 95%. If the sum of the stress relaxation rate and the recovery rate is less than 78% or exceeds 95%, short circuits are likely to occur during charging and discharging, the discharge efficiency is poor, and the cycle characteristics may be significantly reduced.

[0029] The modulus of the elastic layer 40 is preferably 0.01 MPa to 5 MPa at 45° C. and 1 rad / s, and the elastic layer 40 may be a single layer or a multi-layer structure. In the case of a multi-layer structure, it may have different materials with different moduli.

[0030] The material constituting the elastic layer is not particularly limited as long as it satisfies the above-mentioned conditions for compressive strength and has stress relaxation properties.

[0031] According to one embodiment, the elastic layer 40 is also a compression pad made of elastic material. Examples of the elastic material include at least one selected from the group consisting of polyurethane, natural rubber, spandex, butyl rubber (Isobutylene Isoprene Rubber, IIR), fluoroelastomer, elastomer, ethylene propylene rubber (EPR), styrene butadiene rubber (SBR), chloroprene, elastin, rubber epichlorohydrin, nylon, terpene, isoprene rubber, polybutadiene, nitrile rubber, thermoplastic elastomer, silicone rubber, ethylene propylene diene rubber (EPDM), ethylene vinyl acetate (EVA), halogenated butyl rubber, neoprene, and copolymers thereof, but are not limited thereto. Any material having elasticity may be used without limitation.

[0032] For example, the elastic material of the elastic layer 40 may be silicone rubber, cellulose fiber, polyolefin resin, polyurethane resin, acrylic resin, or the like.

[0033] The elastic layer 40 is also compressed so that the thickness when installed is 40 to 90% of the initial thickness before pressure. As a specific example, the thickness when installed is 50 to 85%, more specifically, 60 to 80%, or 65 to 75% of the initial thickness before pressure. Within the above range, the volume change of the negative electrode can be effectively absorbed, enabling smooth charging and discharging of the all-solid-state battery.

[0034] The thickness of the elastic layer 40 can be determined in the range of 200 to 1000% of the thickness of the lithium deposit layer of the negative electrode formed during charging of the all-solid-state secondary battery. The thickness of the lithium deposit layer of the negative electrode in the all-solid-state secondary battery is determined in proportion to the current density of the positive electrode, that is, the thickness of the lithium deposit layer of the negative electrode is determined by the amount of lithium moving from the positive electrode to the negative electrode, and this causes a volume change of the negative electrode. Therefore, the thickness of the elastic layer can be determined so as to absorb such a volume change of the negative electrode. Therefore, by setting the thickness of the elastic layer 40 in the range of 200 to 1000% of the thickness of the lithium deposit layer of the negative electrode formed during charging of the all-solid-state battery, the volume change of the negative electrode can be effectively absorbed. For example, the thickness of the elastic layer 40 is in the range of 250 to 800%, specifically, for example, in the range of 300 to 600%, of the thickness of the lithium deposit layer of the negative electrode formed during charging of the all-solid-state battery.

[0035] The thickness of the elastic layer 40 is set in the range of, for example, 50 μm to 300 μm, and can be selectively set depending on the situation, for example, to 100 μm to 150 μm, 200 μm to 300 μm, or 50 μm to 100 μm.

[0036] By providing the elastic layer 40 on the negative electrode layer 20 in this manner, the volume change due to the lithium deposition reaction in the negative electrode can be absorbed, and the volume change of the entire cell can be suppressed, thereby achieving a stable lifespan.

[0037] [Positive electrode layer] The positive electrode layer 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12 disposed on the positive electrode current collector 11 .

[0038] [Positive electrode layer: positive electrode current collector] The positive electrode current collector 11 is, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector 11 is optional.

[0039] [Cathode layer: Cathode active material] The positive electrode active material layer 12 includes, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the positive electrode layer 10 may be similar to or different from the solid electrolyte included in the solid electrolyte layer 30. For details about the solid electrolyte, please refer to the solid electrolyte layer 30 section.

[0040] The positive electrode active material is a positive electrode active material that can reversibly absorb and desorb lithium ions. Examples of the positive electrode active material include lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium manganate, and lithium iron phosphate, nickel sulfide, copper sulfide, lithium sulfide, iron oxide, and vanadium oxide, but are not limited thereto, and any positive electrode active material used in the art can be used. The positive electrode active material is used alone or in a mixture of two or more kinds.

[0041] The positive electrode active material is, for example, Li a A 1-b B b D2 (wherein, 0.90≦a≦1, and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05); LiE 2-b B b O 4-c D c (wherein, 0≦b≦0.5, 0≦c≦0.05); Li a Ni 1-b-c Cob B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B c O 2-α F α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0.001≦d≦0.1); Li a Ni b CoCMn d GeO2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, 0.001≦e≦0.1); Li a NiG b O2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Lia CoG b O2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein 0.90≦a≦1, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f)A compound represented by any one of the chemical formulas Fe2(PO4)3(0≦f≦2);LiFePO4. In such a compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. A compound having a coating layer added to the surface of such a compound can also be used, and a mixture of the above-mentioned compound and a compound having a coating layer added can also be used. The coating layer added to the surface of such a compound includes, for example, a coating element compound such as an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of a coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. A detailed description of the specific coating method is omitted since it is well understood by those skilled in the art.

[0042] The positive electrode active material includes, for example, a lithium salt of a transition metal oxide having a layered rock salt type structure among the above-described lithium transition metal oxides. The "layered rock salt type structure" is, for example, a structure in which oxygen atom layers and metal atom layers are alternately and regularly arranged in the <111> direction of a cubic rock salt type structure, whereby each atom layer forms a two-dimensional plane. The "cubic rock salt type structure" indicates a sodium chloride type (NaCl type) structure which is a kind of crystal structure. Specifically, it shows a structure in which face centered cubic lattices (fcc) formed by cations and anions are displaced from each other by about 1 / 2 of the ridge of the unit lattice. Such a lithium transition metal oxide having a layered rock salt type structure is, for example, LiNi x Co y Al z O2 (NCA) or LiNi x Co y Mn z O2 (NCM) (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), etc., which are ternary lithium transition metal oxides. When the positive electrode active material includes a ternary lithium transition metal oxide having a layered rock salt type structure, the energy density and thermal stability of the all-solid-state secondary battery 1 are further improved.

[0043] The positive electrode active material is also covered by a coating layer as described above. Any coating layer can be used as long as it is known as a coating layer for the positive electrode active material of an all-solid-state secondary battery. The coating layer is, for example, Li2O-ZrO2 (LZO), etc.

[0044] When the positive electrode active material is a ternary lithium transition metal oxide such as NCA or NCM and contains nickel (Ni), the capacity density of the all-solid-state secondary battery 1 can be increased, and the elution of the metal from the positive electrode active material in the charged state can be reduced. As a result, the cycle characteristics of the all-solid-state secondary battery 1 in the charged state are improved.

[0045] The shape of the positive electrode active material is, for example, a particle shape such as a perfect sphere or an oval sphere. The particle size of the positive electrode active material is not particularly limited, and is within a range applicable to the positive electrode active material of a conventional all-solid-state secondary battery. The content of the positive electrode active material of the positive electrode 10 is also not particularly limited, and is within a range applicable to the positive electrode of a conventional all-solid-state secondary battery.

[0046] [Positive electrode layer: solid electrolyte] The positive electrode active material layer 12 includes, for example, a solid electrolyte. The solid electrolyte included in the positive electrode layer 10 may be the same as or different from the solid electrolyte included in the solid electrolyte layer 30. For details about the solid electrolyte, see the solid electrolyte layer 30 section.

[0047] The solid electrolyte contained in the positive electrode active material layer 12 has a smaller D50 average particle size than the solid electrolyte contained in the solid electrolyte layer 30. For example, the D50 average particle size of the solid electrolyte contained in the positive electrode active material layer 12 is 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or even 20% or less of the D50 average particle size of the solid electrolyte contained in the solid electrolyte layer 30.

[0048] [Positive electrode layer: binder] The positive electrode active material layer 12 contains a binder. The binder is, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or the like.

[0049] [Positive electrode layer: conductive material] The positive electrode active material layer 12 contains a conductive material, such as graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or metal powder.

[0050] [Positive electrode layer: Other additives] The positive electrode layer 10 further contains additives such as a filler, a coating agent, a dispersant, and an ion-conductive assistant in addition to the above-mentioned positive electrode active material, solid electrolyte, binder, and conductive material.

[0051] The filler, coating agent, dispersant, and ion-conductive assistant contained in the positive electrode layer 10 may be any known material generally used in electrodes of all-solid-state secondary batteries.

[0052] [Solid electrolyte layer] As shown in FIG. 1, a solid electrolyte layer 30 is disposed between the positive electrode layer 10 and the negative electrode layer 20, and the solid electrolyte layer 30 may include a sulfide-based solid electrolyte.

[0053] [Solid electrolyte layer: sulfide solid electrolyte] Examples of sulfide-based solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiX (X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z. m S n (m and n are positive numbers, Z is one of Ge, Zn, and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p, q are positive numbers, M is one of P, Si, Ge, B, Al, GaIn), Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2) and Li 7-x P.S. 6-xIx (0≦x≦2). The sulfide-based solid electrolyte is prepared by processing starting materials such as Li2S and P2S5 by melt quenching or mechanical milling. After such processing, heat treatment can be performed. The solid electrolyte may be amorphous, crystalline, or a mixture of these. The solid electrolyte may be, for example, the above-mentioned sulfide-based solid electrolyte material, and may contain at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements. For example, the solid electrolyte may be a material containing Li2S-P2S5. When a sulfide-based solid electrolyte material containing Li2S-P2S5 is used to form the solid electrolyte, the mixture molar ratio of Li2S and P2S5 is, for example, in the range of about Li2S:P2S5=50:50 to 90:10.

[0054] The sulfide-based solid electrolyte is, for example, Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2), and Li 7-x P.S. 6-x I x (0≦x≦2). In particular, the sulfide-based solid electrolyte is an argyrodite-type compound containing one or more selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.

[0055] The density of the argyrodite-type solid electrolyte is 1.5 to 2.0 g / cc. When the argyrodite-type solid electrolyte has a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery is reduced, and the penetration of the solid electrolyte by Li can be effectively suppressed. The elastic modulus of the solid electrolyte is, for example, 15 to 35 GPa.

[0056] [Solid electrolyte layer: binder] The solid electrolyte layer 30 includes, for example, a binder. The binder included in the solid electrolyte layer 30 is, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc., but is not limited thereto, and any binder used as a binder in the relevant technical field can be used. The binder of the solid electrolyte layer 30 may be the same as or different from the binder included in the positive electrode active material layer 12 and the negative electrode active material layer 22.

[0057] [Negative electrode layer] [Negative electrode layer: negative electrode active material] The negative electrode active material layer 22 contains, for example, a negative electrode active material and a binder. The negative electrode active material contained in the negative electrode active material layer 22 has, for example, a particulate shape. The average particle size of the particulate negative electrode active material is, for example, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, or 900 nm or less. The average particle size of the particulate negative electrode active material is, for example, 10 nm to 4 μm or less, 10 nm to 3 μm or less, 10 nm to 2 μm or less, 10 nm to 1 μm or less, or 10 nm to 900 nm or less. When the negative electrode active material has an average particle size in such a range, reversible absorbing and / or desorbing of lithium during charging and discharging is further facilitated. The average particle size of the negative electrode active material is, for example, a median diameter (D50) measured using a laser type particle size distribution meter.

[0058] The negative electrode active material contained in the negative electrode active material layer 22 includes, for example, one or more selected from a carbon-based negative electrode active material and a metal or semi-metal negative electrode active material.

[0059] The carbon-based negative electrode active material is, in particular, amorphous carbon. Examples of amorphous carbon include, but are not limited to, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, etc., and any material that is classified as amorphous carbon in the art can be used. Amorphous carbon is carbon that has no crystallinity or has very low crystallinity, and is classified as crystalline carbon or graphite-based carbon.

[0060] The metal or metalloid negative electrode active material includes, but is not necessarily limited to, one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), and any metal or metalloid negative electrode active material that forms an alloy or compound with lithium in the art can be used. For example, nickel (Ni) is not a metal negative electrode active material because it does not form an alloy with lithium.

[0061] The negative electrode active material layer 22 includes one type of negative electrode active material among such negative electrode active materials, or includes a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer 22 includes only amorphous carbon, or includes one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Differently, the negative electrode active material layer 22 includes a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture of amorphous carbon and gold, etc., in terms of weight ratio, is, for example, 10:1 to 1:2, 5:1 to 1:1, or 4:1 to 2:1, but is not necessarily limited to such ranges and is selected depending on the required characteristics of the all-solid-state secondary battery 1. When the negative electrode active material has such a composition, the cycle characteristics of the all-solid-state secondary battery 1 are further improved.

[0062] The negative electrode active material contained in the negative electrode active material layer 22 includes, for example, a mixture of first particles made of amorphous carbon and second particles made of a metal or a metalloid. The metal or metalloid includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). In other words, the metalloid is a semiconductor. The content of the second particles is 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt%, based on the total weight of the mixture. When the second particles have a content in such a range, for example, the cycle characteristics of the all-solid-state secondary battery 1 are further improved.

[0063] [Negative electrode layer: binder] The binder contained in the negative electrode active material layer 22 may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited to these, and any binder used in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders.

[0064] The negative electrode active material layer 22 contains a binder, so that the negative electrode active material layer 22 is stabilized on the negative electrode current collector 21. In addition, cracks in the negative electrode active material layer 22 are suppressed despite changes in volume and / or relative position of the negative electrode active material layer 22 during charging and discharging. For example, if the negative electrode active material layer 22 does not contain a binder, the negative electrode active material layer 22 may be easily separated from the negative electrode current collector 21. When the negative electrode active material layer 22 is detached from the negative electrode current collector 21, the negative electrode current collector 21 comes into contact with the solid electrolyte layer 30 at the exposed portion of the negative electrode current collector 21, increasing the possibility of short circuit occurrence. The negative electrode active material layer 22 is prepared, for example, by applying a slurry in which materials constituting the negative electrode active material layer 22 are dispersed onto the negative electrode current collector 21 and drying it. By including a binder in the negative electrode active material layer 22, the negative electrode active material can be stably dispersed in the slurry. For example, when the slurry is applied onto the negative electrode current collector 21 by a screen printing method, clogging of the screen (for example, clogging due to aggregates of the negative electrode active material) can be suppressed.

[0065] [Negative electrode layer: Other additives] The negative electrode active material layer 22 may further include additives used in conventional all-solid-state secondary batteries, such as a filler, a coating agent, a dispersant, and an ion-conducting assistant.

[0066] [Negative electrode layer structure] The thickness of the negative electrode active material layer 22 is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer. The thickness of the first negative electrode active material layer is, for example, 1 μm to 20 μm, 2 μm to 10 μm, or 3 μm to 7 μm. If the thickness of the first negative electrode active material layer is excessively thin, lithium dendrites formed between the negative electrode active material layer 22 and the negative electrode current collector 21 collapse the negative electrode active material layer, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery. If the thickness of the negative electrode active material layer is excessively increased, the energy density of the all-solid-state secondary battery decreases, and the internal resistance of the all-solid-state secondary battery due to the negative electrode active material layer increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery.

[0067] If the thickness of the negative electrode active material layer is reduced, the charge capacity of the first negative electrode active material layer is also reduced, for example. The charge capacity of the negative electrode active material layer 22 is, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 2% or less compared to the charge capacity of the positive electrode active material layer 12. The charge capacity of the negative electrode active material layer 22 is, for example, 0.1% to 50%, 0.1% to 40%, 0.1% to 30%, 0.1% to 20%, 0.1% to 10%, 0.1% to 5%, or 0.1% to 2% compared to the charge capacity of the positive electrode active material layer 12. If the charge capacity of the negative electrode active material layer 22 is excessively small, the thickness of the negative electrode active material layer 22 becomes very thin, and thus lithium dendrites formed between the negative electrode active material layer 22 and the negative electrode current collector 21 during repeated charge and discharge processes collapse the negative electrode active material layer 22, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery. If the charge capacity of the negative electrode active material layer 22 is excessively increased, the energy density of the all-solid-state secondary battery decreases, and the internal resistance of the all-solid-state secondary battery due to the negative electrode active material layer 22 increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery.

[0068] The charge capacity of the positive electrode active material layer 12 is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer 12. When multiple types of positive electrode active materials are used, the charge capacity density x mass value is calculated for each positive electrode active material, and the total of these values ​​is the charge capacity of the positive electrode active material layer 12. The charge capacity of the negative electrode active material layer 22 is also calculated in a similar manner. That is, the charge capacity of the negative electrode active material layer 22 is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the negative electrode active material layer 22. When multiple types of negative electrode active materials are used, the charge capacity density x mass value is calculated for each negative electrode active material, and the total of these values ​​is the capacity of the negative electrode active material layer 22. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is a capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer 12 and the negative electrode active material layer 22 is directly measured by measuring the charge capacity using an all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. In addition, the charge capacity of the positive electrode active material layer 12 and the negative electrode active material layer 22 is also the initial charge capacity measured during the first cycle of charging.

[0069] [Negative electrode layer: negative electrode current collector] The negative electrode current collector 21 is made of, for example, a material that does not react with lithium, i.e., does not form any alloy or compound. The material constituting the negative electrode current collector 21 is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), etc., but is not necessarily limited thereto, and any material used as an electrode current collector in the technical field can be used. The thickness of the negative electrode current collector is 1 to 20 μm, for example, 5 to 15 μm, for example, 7 to 10 μm.

[0070] The negative electrode current collector 21 may be made of one of the above-mentioned metals, or may be made of an alloy or a coating material of two or more of the above-mentioned metals. The negative electrode current collector 21 may be, for example, in the form of a plate or foil.

[0071] Referring to FIG. 2, the unit cell 1 of the unit stack cell structure further includes, for example, a thin film 24 on the negative electrode current collector 21, the thin film 24 including an element that forms an alloy with lithium. The thin film 24 is disposed between the negative electrode current collector 21 and the negative electrode active material layer 22. The thin film 24 includes, for example, an element that forms an alloy with lithium. The element that forms an alloy with lithium is, for example, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., but is not limited thereto, and any element that forms an alloy with lithium in the art can be used. The thin film 24 is composed of one of these metals or a metal alloy of multiple kinds. By disposing the thin film 24 on the negative electrode current collector 21, for example, the deposition form of a second negative electrode active material layer (not shown) deposited between the thin film 24 and the negative electrode active material layer 22 can be further flattened, and the cycle characteristics of the all-solid-state secondary battery can be further improved.

[0072] The thickness of the thin film 24 is, for example, 1 nm to 800 nm, 10 nm to 700 nm, 50 nm to 600 nm, or 100 nm to 500 nm. If the thickness of the thin film 24 is less than 1 nm, it is difficult for the thin film 24 to exert its function. If the thin film 24 is excessively thick, the thin film 24 itself absorbs lithium, reducing the amount of lithium precipitated in the negative electrode layer, thereby reducing the energy density of the all-solid-state battery, and the cycle characteristics of the all-solid-state secondary battery may be reduced. The thin film 24 may be disposed on the negative electrode current collector 21 by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to such a method, and any method capable of forming the thin film 24 in the art may be used.

[0073] [Negative electrode layer: second negative electrode active material layer] Referring to FIG. 3, the all-solid-state secondary battery including the unit cell 1a of the unit stack cell structure further includes a second negative electrode active material layer 23 disposed between the negative electrode current collector 21 and the negative electrode active material layer 22. The second negative electrode active material layer 23 is a metal layer including lithium or a lithium alloy. Since the second negative electrode active material layer 23 is a metal layer including lithium or a lithium alloy, it acts as a lithium reservoir, for example. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., but is not limited thereto, and any alloy used as a lithium alloy in the art may be used. The second negative electrode active material layer 23 may be made of one of such alloys or lithium, or may be made of a plurality of alloys.

[0074] The thickness of the second negative electrode active material layer 23 is not particularly limited, and may be, for example, 1 μm to 1000 μm, 1 μm to 500 μm, 1 μm to 200 μm, 1 μm to 150 μm, 1 μm to 100 μm, or 1 μm to 50 μm. If the thickness of the second negative electrode active material layer 23 is too thin, it is difficult for the second negative electrode active material layer 23 to perform the role of a lithium reservoir. If the thickness of the second negative electrode active material layer 23 is too thick, the mass and volume of the all-solid-state secondary battery may increase, and the cycle characteristics may rather deteriorate. The second negative electrode active material layer 23 may be, for example, a metal foil having a thickness in this range.

[0075] In the unit stack cell structure, the second negative electrode active material layer 23 may be disposed between the negative electrode current collector 21 and the negative electrode active material layer 22 before assembling the unit stack cell structure, or may be deposited between the negative electrode current collector 21 and the negative electrode active material layer 22 by charging the all-solid-state secondary battery after assembling the unit stack cell structure.

[0076] When the second negative electrode active material layer 23 is disposed between the negative electrode current collector 21 and the negative electrode active material layer 22 before the unit stack cell structure is assembled, the second negative electrode active material layer 23 acts as a lithium reservoir since it is a metal layer containing lithium. The cycle characteristics of the all-solid-state secondary battery including the second negative electrode active material layer 23 are further improved. For example, lithium foil is disposed between the negative electrode current collector 21 and the negative electrode active material layer 22 before the unit stack cell structure is assembled.

[0077] When the second negative electrode active material layer 23 is disposed by charging after assembling the unit stack cell structure, the energy density of the all-solid-state secondary battery is increased since the second negative electrode active material layer 23 is not included when assembling the unit stack cell structure. For example, when charging the all-solid-state secondary battery, the negative electrode active material layer 22 is charged beyond its charge capacity. That is, the negative electrode active material layer 22 is overcharged. At the beginning of charging, lithium is absorbed in the negative electrode active material layer 22. That is, the negative electrode active material contained in the negative electrode active material layer 22 forms an alloy or compound with the lithium ions transferred from the positive electrode layer 10. If the negative electrode active material layer 22 is charged beyond its capacity, for example, lithium is precipitated on the back side of the negative electrode active material layer 22, i.e., between the negative electrode current collector 21 and the negative electrode active material layer 22, and a metal layer corresponding to the second negative electrode active material layer 23 is formed by the precipitated lithium. The second negative electrode active material layer 23 is a metal layer mainly composed of lithium (i.e., metallic lithium). Such a result can be obtained, for example, by the negative electrode active material contained in the negative electrode active material layer 22 being composed of a material that forms an alloy or compound with lithium. During discharge, lithium in the negative electrode active material layer 22 and the second negative electrode active material layer 23, i.e., the metal layer, is ionized and moves to the positive electrode layer 10 side. Therefore, lithium can be used as the negative electrode active material in the all-solid-state secondary battery. In addition, the negative electrode active material layer 22 covers the second negative electrode active material layer 23, and therefore serves as a protective layer for the second negative electrode active material layer 23, i.e., the metal layer, and also serves to suppress the precipitation growth of lithium dendrites. Therefore, the short circuit and capacity reduction of the all-solid-state secondary battery are suppressed, and as a result, the cycle characteristics of the all-solid-state secondary battery are improved. In addition, when the second negative electrode active material layer 23 is disposed by charging the all-solid-state secondary battery after assembling the unit stack cell structure, the negative electrode current collector 21, the negative electrode active material layer 22, and the region therebetween are, for example, Li-free regions that do not contain lithium (Li) in the initial state or after discharge of the all-solid-state secondary battery.

[0078] [All-solid-state secondary battery] According to an embodiment, the all-solid-state secondary battery includes a plurality of stacked unit stack cell structures, and the stacked unit stack cell structures may be bipolar-connected. The all-solid-state secondary battery can be designed to have a desired voltage by connecting the unit stack cell structures bipolarly, and the introduction of an elastic layer 40 in the unit cell can suppress a change in the volume of the entire cell.

[0079] The all-solid-state secondary battery can be applied to medium- to large-sized batteries or energy storage systems (ESS).

[0080] The present invention will be described in more detail through the following examples and comparative examples, however, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0081] (All-solid-state secondary battery manufacturing) Example 1 (Elastic layer manufacturing) A resin mixture was prepared by mixing 70 parts by weight of n-butyl acrylate (hereinafter also referred to as "BA") as resin components, 10 parts by weight of 2-hydroxyethyl acrylate (2-HEA), and 20 parts by weight of isobornyl acrylate in a reactor. 0.1 parts by weight of azobisisobutyronitrile as a polymerization initiator and 150 parts by weight of ethyl acetate as a solvent were mixed with the resin mixture, and the temperature was raised to 75°C while stirring to carry out a polymerization reaction. Further, a polymerization catalyst solution in which 0.1 parts by weight of azobisisobutyronitrile was dissolved in 10 parts by weight of ethyl acetate was added in sequence, and the polymerization was completed at the same temperature for 8 hours. After the polymerization was completed, a dilution solvent (ethyl acetate) was added to produce a solution containing a carboxyl group-free acrylic copolymer with a weight average molecular weight of 1 million and a solid content of 35% by weight.

[0082] Based on 100 parts by weight of the prepared acrylate copolymer solution having a weight average molecular weight of 1 million, 7 parts by weight of Expancel 551 DU 40 (Akzo Nobel Chemicals) as a foaming agent and 0.2 parts by weight of an isocyanate crosslinking agent (XDI (Xylylene Diisocyanate), trade name "Takenate D110N", Mitsui Chemicals Polyurethanes, molecular weight 698, trifunctionality, solid content concentration 75% by weight) were mixed into the acrylate copolymer solution, and the mixture was coated on a PET release film and dried at 150°C for 5 minutes to prepare a sheet-shaped elastic layer having a thickness of 300 μm.

[0083] (Negative electrode layer manufacturing) A 10 μm thick Ni foil was prepared as a negative electrode current collector, and carbon black (CB) with a primary particle size of about 30 nm and silver (Ag) particles with an average particle diameter of about 60 nm were prepared as a negative electrode active material.

[0084] 4 g of mixed powder, which is a mixture of carbon black (CB) and silver (Ag) particles at a weight ratio of 3:1, was placed in a container, and 4 g of NMP solution containing 7 wt% of PVDF binder (Kureha #9300) was added thereto to prepare a mixed solution. Next, the mixed solution was stirred while adding NMP little by little to prepare a slurry. The prepared slurry was applied to a SUS sheet using a bar coater and dried in air at 80°C for 10 minutes. The laminate obtained in this way was vacuum dried at 40°C for 10 hours. The dried laminate was roll pressed at a pressure of 300 MPa for 10 ms to flatten the surface of the negative electrode active material layer of the laminate. The negative electrode layer was produced by the above process. The thickness of the negative electrode active material layer included in the negative electrode layer was about 7 μm.

[0085] (Positive electrode layer manufacturing) Li2O-ZrO2 (LZO) coated LiNi as the positive electrode active material 0.8 Co 0.15 Mn 0.05O2 (NCM) was prepared. The LZO-coated positive active material was prepared according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Argyrodite-type crystal Li6PS5Cl (D50=0.5μm, crystalline) was prepared as a solid electrolyte. Polytetrafluoroethylene (PTFE) binder (DuPont's Teflon (registered trademark) binder) was prepared as a binder. Carbon nanofiber (CNF) was prepared as a conductive agent. These materials were mixed with xylene solvent in a weight ratio of positive active material: solid electrolyte: conductive agent: binder = 84: 11.5: 3: 1.5, and the mixture was formed into a sheet and vacuum dried at 40 ° C for 8 hours to prepare a positive active material layer. The positive active material layer was pressed onto a positive current collector made of carbon-coated aluminum foil with a thickness of 18 μm to prepare a positive electrode layer. The thickness of the positive electrode layer was about 105 μm.

[0086] (Manufacturing of solid electrolyte layer) A mixture was prepared by adding 1.5 parts by weight of an acrylic binder to 98.5 parts by weight of the solid electrolyte, Li6PS5Cl, an argyrodite-type crystal (D50=3.0μm, crystalline). Octyl acetate was added to the prepared mixture and stirred to prepare a slurry. The prepared slurry was applied to a nonwoven fabric using a bar coater and dried in air at 80°C for 10 minutes to obtain a laminate. The obtained laminate was vacuum-dried at 80°C for 6 hours. A solid electrolyte layer was manufactured by the above process.

[0087] (Manufacturing of unit stack cell structures) First, a solid electrolyte layer was placed on the positive electrode active material layer of the positive electrode layer, and a negative electrode layer was placed on the solid electrolyte layer so that the solid electrolyte layer was in contact with the positive electrode layer. Two laminates were prepared as the basis of a unit cell by applying pressure. An elastic layer was placed on the negative electrode layer of one of the laminates and laminated. Next, another laminate was placed on the elastic layer so that the negative electrode layer of the other laminate was in contact with the elastic layer, to prepare a laminate structure.

[0088] The laminated structure was placed in a laminate film and plate pressed at 85° C. with a torque wrench pressure of 0.5 N for 30 minutes to prepare a unit stack cell structure, which was used as an all-solid-state secondary battery.

[0089] The all-solid-state secondary battery was placed in a test module and fixed with a force of 5000 kgf, and a charge / discharge evaluation was carried out.

[0090] Example 2 To manufacture the elastic layer, a solvent-free acrylate mixed resin with a weight average molecular weight of 1.2 million was first prepared. 4-Hydroxybutyl acrylate (4-HBA) (Osaka Organic Chemical) and 2-ethylhexyl acrylate (2-EHA) (LG Chem) were mixed in a 30 / 70 weight ratio, 0.01 parts by weight of a photoinitiator (Irgacure 651) was added, and the mixture was irradiated with UV light to produce a solvent-free acrylate mixed resin with a weight average molecular weight of 1.2 million.

[0091] Based on 100 parts by weight of the solvent-free acrylate mixed resin, 0.5 parts by weight of a photoinitiator (Irgacure 651), 0.3 parts by weight of a crosslinker (1,6-hexanediol diacrylate (HDDA), Sigma-Aldrich), and 6 parts by weight of Expancel 551 DU 40 (Akzo Nobel Chemicals) were mixed with the solvent-free acrylate mixed resin, and the mixture was coated between general-purpose PET films treated with silicone release, and UV was applied at 2000 mj / cm. 2 The sheet was left at 150° C. for 5 minutes to expand the 551 DU 40, producing a sheet-like elastic layer having a thickness of 300 μm.

[0092] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the elastic layer thus manufactured was used.

[0093] Example 3 To manufacture the elastic layer, a mixture containing 30 parts by weight of a propylene-based polyol with a weight average molecular weight of 4000, 70 parts by weight of a polyether-based polyol (manufactured by Sanyo Chemical Industries, Ltd., product name "GP-3000", viscosity (25°C) 500 mPa·s, number of functional groups 3, number average molecular weight 3000), and 11 parts by weight of an isocyanate-based crosslinking agent (BASF, Lupranate T80) was stirred with 100 cc / min of nitrogen added for 5 minutes, and then the mixture was coated on a PET film and the elastic sheet was heated to 120-200°C to manufacture a sheet-shaped elastic layer with a coating thickness of 300 μm.

[0094] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the elastic layer thus manufactured was used.

[0095] Example 4 An acrylic elastic sheet (Youngwoo, BHF) of 125 μm was placed on both sides and a urethane sheet (Ventwin, Grade 2085) of 50 μm was bonded to prepare an elastic layer of 300 μm in thickness.

[0096] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the elastic layer thus manufactured was used.

[0097] Example 5 An elastic layer was placed under the negative electrode layer of one laminate and laminated, and then another laminate was placed on the elastic layer so that the positive electrode layer of the other laminate was in contact with the elastic layer, and an elastic layer made of the same material was placed on the negative electrode layer of the other laminate and laminated to prepare a laminate structure.

[0098] The thus prepared laminated structure was pressed at a pressure of 15 N to manufacture a unit stack cell structure, and the same process as in Example 1 was carried out to manufacture an all-solid-state secondary battery.

[0099] Example 6 An all-solid-state secondary battery was manufactured by performing the same process as in Example 5, except that the elastic layer used in Example 2 was used as the elastic layer.

[0100] Example 7 An all-solid-state secondary battery was manufactured by performing the same process as in Example 5, except that the elastic layer used in Example 3 was used as the elastic layer.

[0101] Example 8 An all-solid-state secondary battery was manufactured by performing the same process as in Example 5, except that the elastic layer used in Example 4 was used as the elastic layer.

[0102] Comparative Example 1 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 1, except that a 300 μm-thick silicone pad (AS ONE, T3) was used as the elastic layer.

[0103] Comparative Example 2 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 1, except that a PTFE sheet (GORE, SG05X-J) having a thickness of 300 μm was used as the elastic layer.

[0104] Comparative Example 3 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 1, except that a urethane pad (Main Elecom, M3) having a thickness of 300 μm was used as the elastic layer.

[0105] Comparative Example 4 An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that an acrylic adhesive sheet (3M, VHB) having a thickness of 300 μm was used as the elastic layer.

[0106] Comparative Example 5 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 5, except that a 300 μm-thick silicone pad (AS ONE, T3) was used as the elastic layer.

[0107] Comparative Example 2 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 5, except that a PTFE sheet (GORE, SG05X-J) having a thickness of 300 μm was used as the elastic layer.

[0108] Comparative Example 3 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 5, except that a urethane pad (Main Elecom, M3) having a thickness of 300 μm was used as the elastic layer.

[0109] Comparative Example 4 An all-solid-state secondary battery was manufactured by carrying out the same process as in Example 5, except that an acrylic adhesive sheet (3M, VHB) having a thickness of 300 μm was used as the elastic layer.

[0110] Evaluation example 1: Measurement of physical properties of elastic layer The physical properties of the elastic layers used in Examples 1 to 4 and Comparative Examples 1 to 4 were measured as follows, and the results are shown in Table 1 below.

[0111] (1) Compressive strength This is the value at 40% CFD (Compression Force Deflection), and indicates the compressive strength when the elastic layer is physically compressed by 40%. After compressing the specimen by 40% at a compression ratio of 0.6 mm / min (10 μm / sec) using a compression tester with a spherical jig with a diameter of 10 mm, the load was calculated when the thickness became 60% of the original thickness, and the calculation was performed using the following formula 1. <Number 1> Compressive strength (MPa) = [Load at 40% compression (kgf)] / [Specimen area (m 2 )] × 0.1

[0112] (2) Stress relaxation rate and recovery rate The stress relaxation rate indicates the change in stress over 60 seconds after the elastic layer is initially compressed to 2.5 kgf at a compression speed of 0.6 mm / min (10 μm / sec) using a compression tester having a spherical jig with a diameter of 10 mm, and then further compressed by 40 μm from that point (initial point), and was calculated using the following formula 2. The recovery rate indicates the change in stress when the elastic layer is compressed to 40 μm under the same conditions and then restored to the initial point immediately before compression by 40 μm, and was calculated using the following formula 3.

[0113] 1. Apply pressure at a speed of 10 μm / sec until it reaches 2.5 kgf, then apply pressure at the same speed to 40 μm. The change in stress at the 2.40 μm pressure point is measured for 60 seconds, and the rate of change is defined as the stress relaxation rate. 3. After steps 1 and 2 have been advanced, the pressurized distance (40 μm) is restored again, and the stress is measured at the 0 μm point. The difference in stress from the initial 2.5 kgf is defined as the restoration rate.

[0114] <Number 2> Stress relaxation rate (%) = (stress after 60 seconds after compression of 40 μm) / (initial stress when compressed to 40 μm) × 100

[0115] <Number 3> Recovery rate (%) = (stress when restored to the initial position after 40 μm compression) / (initial stress when compressed by 40 μm) × 100

[0116] [Table 1]

[0117] As shown in Table 1, the properties of the elastic layers used in Examples 1 to 4 were measured, and it was confirmed that the elastic layers had excellent strength in the compression direction and stress relaxation properties and recovery rates suitable for use as a buffer material for an all-solid-state secondary battery, as compared with the elastic layers used in Comparative Examples 1 to 4.

[0118] Evaluation example 2: Charge / discharge test The charge / discharge characteristics of the all-solid-state secondary batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 8 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a thermostatic chamber at 45°C.

[0119] First, the all-solid-state secondary batteries of Examples 1 to 8 and Comparative Examples 1 to 8 were charged at a constant current of 0.1 C until the voltage reached 4.25 V, and then charged at a constant voltage of 0.05 C. The charged cells were rested for about 10 minutes, and then discharged at a constant current of 0.1 C until the voltage reached 2.5 V.

[0120] The charge / discharge cycle was repeated a total of 300 times, and the charge / discharge efficiency and the occurrence of short circuits were evaluated. The charge / discharge efficiency was evaluated as a capacity retention rate expressed by the following Equation 4 after 300 cycles.

[0121] <Number 4> Capacity retention rate (%) = (discharge capacity after each cycle / discharge capacity after the first cycle) x 100

[0122] Examples 1 to 8 achieved a charge / discharge efficiency of 90% or more during 300 cycles. In Comparative Example 1, a short circuit occurred less than 50 cycles. Comparative Example 2 achieved 300 cycles, but the charge / discharge efficiency was 88%. In Comparative Example 3, a short circuit occurred less than 50 cycles. In Comparative Example 4, a short circuit occurred less than 50 cycles. In Comparative Example 5, a short circuit occurred in less than 30 cycles. Comparative Example 6 achieved 300 cycles, but the charge / discharge efficiency was 88%. In Comparative Example 7, a short circuit occurred less than 50 cycles. In Comparative Example 8, a short circuit occurred less than 50 cycles.

[0123] Through the charge / discharge test, it can be seen that the all-solid-state secondary batteries of Examples 1 to 8 have an elastic sheet having excellent compressive strength and stress relaxation properties, and thus have improved coulombic efficiency without short circuit even when the volume of the cell changes due to charge / discharge.

[0124] Although one embodiment has been described above with reference to the drawings and examples, this is merely an example, and a person skilled in the art will understand that various modifications and equivalent embodiments are possible. Therefore, the scope of protection of the present invention should be determined by the claims. [Explanation of symbols]

[0125] 1,1a unit cell 10 Positive electrode layer 11 Positive electrode current collector 12 Cathode active material layer 20 Negative electrode layer 21 Negative electrode current collector 22 Negative electrode active material layer 23 Second negative electrode active material layer 24 Thin Film 30 Solid electrolyte layer 40 Elastic layer

Claims

1. The unit cell includes a plurality of stacked unit cells. The unit cell includes a laminate in which a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and an elastic layer are sequentially arranged, The compressive strength of the elastic layer is 0.28 MPa or more and less than 0.6 MPa in a compression ratio range of 40 to 70%, The compressive strength was measured by compressing the elastic layer by 40% at a compression speed of 0.6 mm / min using a compression tester having a spherical jig with a diameter of 10 mm, and then determining the load at which the thickness became 60% of the original thickness. The load was calculated using the following formula 1: <Formula 1> Compressive strength (MPa) = [load at 40% compression (kgf)] / [specimen area (m 2 )] × 0.1 The unit stack cell structure was calculated using the following formula:

2. 2. The unit stack cell structure according to claim 1, wherein the elastic layer has a compressive strength of 0.28 MPa or more and 0.35 MPa or less at a 40% compression rate.

3. The elastic layer has a stress relaxation rate of 5% to 20% and a recovery rate of 60% or more, and the sum of the stress relaxation rate and the recovery rate is 78% to 95%, The stress relaxation rate and the recovery rate were measured by using the compression tester to pressurize the elastic layer to 2.5 kgf at a compression speed of 0.6 mm / min, setting the initial point as the point, and measuring the change in stress for 60 seconds at the point where the elastic layer was compressed by an additional 40 μm from the initial point. Thereafter, the stress at the initial point where the elastic layer was restored by 40 μm was measured, and the stress relaxation rate and the recovery rate were measured by using the following formulas 2 and 3: <Formula 2> Stress relaxation rate (%)=(stress after 60 seconds after compression of 40 μm) / (initial stress when compressed to 40 μm)×100 <Formula 3> Recovery rate (%)=(stress when restored to the initial point after compression of 40 μm) / (initial stress when compressed by 40 μm)×100 The unit stack cell structure according to claim 1 , wherein the calculated value is calculated using the formula:

4. 4. The unit stack cell structure according to claim 3, wherein the stress relaxation rate of the elastic layer is 6.5% to 15%.

5. The unit stack cell structure according to claim 3 , wherein the elastic layer has a recovery rate of 70% or more.

6. 2. The unit stack cell structure according to claim 1, wherein the elastic layer is a compression pad made of an elastic material.

7. The unit stack cell structure according to claim 6 , wherein the elastic material comprises at least one material selected from the group consisting of a polyolefin resin, a polyurethane resin, and an acrylic resin.

8. 2. The unit stack cell structure according to claim 1, wherein the elastic layer is a compression pad that is compressed to have a thickness of 40 to 90% of an initial thickness before compression.

9. 2. The unit stack cell structure according to claim 1, wherein the thickness of the elastic layer is set to be in the range of 200 to 500% of the thickness of a lithium deposition layer of the negative electrode formed during charging of the all-solid-state secondary battery.

10. The unit stack cell structure according to claim 1 , wherein the solid electrolyte layer includes a sulfide-based solid electrolyte.

11. The sulfide-based solid electrolyte is Li 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -LiX (X is a halogen element), Li 2 S-P 2 S 5 -Li 2 O. Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 - LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S-B 2 S 3 , Li 2 S-P 2 S 5 -Z m S n (m and n are positive numbers, and Z is one of Ge, Zn, and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li p M.O. q (p, q are positive numbers, M is one of P, Si, Ge, B, Al, and GaIn), Li 7-x P.S. 6-x C x (0≦x≦2), Li 7-x P.S. 6-x B x (0≦x≦2), and Li 7-x P.S. 6-x I x The unit stack cell structure according to claim 10 , wherein x is one or more selected from (0≦x≦2).

12. The sulfide-based solid electrolyte is Li 6 P.S. 5 Cl, Li 6 P.S. 5 Br and Li 6 P.S. 5 The unit stack cell structure according to claim 10, wherein the solid electrolyte is an argyrodite-type sulfide-based electrolyte containing one or more selected from the group consisting of I.

13. 2 . The unit stack cell structure according to claim 1 , wherein the negative electrode layer includes a negative electrode active material layer containing a negative electrode active material and a binder, the negative electrode active material having a particulate shape, and an average particle size of the negative electrode active material being 4 μm or less.

14. 14. The unit stack cell structure of claim 13, wherein the negative electrode active material comprises one or more selected from the group consisting of a carbon-based negative electrode active material and a metal or semi-metal negative electrode active material, the carbon-based negative electrode active material comprises amorphous carbon, and the metal or semi-metal negative electrode active material comprises one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn).

15. 14. The unit stack cell structure of claim 13, wherein the negative active material comprises a mixture of first particles made of amorphous carbon and second particles made of a metal or semi-metal, and a content of the second particles is 8 to 60 wt % based on a total weight of the mixture.

16. The unit stack cell structure according to claim 1, wherein the unit stack cell structure has a structure in which a plurality of bi-cells are stacked, each bi-cell having a pair of unit cells symmetrically arranged on both sides of a positive electrode current collector.

17. 17. An all-solid-state secondary battery comprising a plurality of stacked unit stack cell structures according to claim 1, the stacked unit stack cell structures being connected in a bipolar manner.

Citation Information

Patent Citations

  • Rigid polyurethane foam and production thereof

    JP1996193118A

  • Power storage body, power storage device, and method for determining usability of power storage body

    JP2018125215A

  • All-solid battery and all-solid battery system

    JP2021002495A

  • Battery and battery module

    WO2018025557A1

  • Solid-state battery

    WO2019189007A1