Double-sided antistatic silicone release film

The double-sided antistatic silicone release film addresses static-related contamination and peeling issues by integrating a conductive polymer resin with a binder mixture, ensuring stable antistatic properties and high adhesion, thus reducing manufacturing costs and improving processing stability.

JP7590596B2Active Publication Date: 2024-11-26TORAY ADVANCED MATERIALS KOREA INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023557813
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-16
Filing Date
2021-10-14
Publication Date
2024-11-26
Estimated Expiration
2041-10-14

AI Technical Summary

Technical Problem

Conventional release films with antistatic functions on both sides face issues such as contamination due to static electricity, poor peeling, and instability over time, leading to high manufacturing costs and quality problems like blocking and scratches during processing.

Method used

A double-sided antistatic silicone release film is developed by integrating a conductive polymer resin with a binder mixture into a silicone release coating composition, allowing for simultaneous coating of both sides in a single process, ensuring stable antistatic properties and high adhesion without interfering with curing.

Benefits of technology

The film effectively reduces contamination and peeling issues, maintains consistent performance over time, and prevents blocking, while maintaining the functionality of the adhesive layer, with excellent solvent resistance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590596000006
    Figure 0007590596000006
  • Figure 0007590596000001
    Figure 0007590596000001
  • Figure 0007590596000002
    Figure 0007590596000002
Patent Text Reader

Abstract

The present invention provides a double-sided antistatic silicone release film that has excellent antistatic properties so that problems caused by static electricity do not occur when peeling off from an adhesive, has excellent adhesion between the cured layer and a substrate, has a high degree of crosslinking in the cured layer so that there is no change in physical properties over time or in response to temperature and humidity, and has stable release properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a double-sided antistatic silicone release film, and more specifically, to a double-sided antistatic silicone release film that has excellent antistatic function so that problems due to static electricity do not occur when peeling off from an adhesive, has excellent adhesion between the cured layer and the substrate, has a high degree of crosslinking in the cured layer so that there is no change in physical properties over time or in response to temperature and humidity, and has stable release properties. [Background technology]

[0002] Currently, with the rapid development of industrialization in the fields of semiconductors, electric and electronic equipment, and displays, the use of synthetic resins and synthetic fibers in these technical fields is increasing rapidly, which has resulted in the emergence of static electricity problems during processing.

[0003] In general, the demand for antistatic function is gradually increasing in the field of release films used to protect adhesive layers. Conventionally, antistatic function has been imparted to adhesives to solve problems such as contamination and peeling failure caused by static electricity generated when separating a release film from an adhesive layer, but it has been difficult to realize sufficient antistatic performance due to incompatibility between antistatic components and adhesive components. Therefore, recently, antistatic function has been often imparted to release layers other than adhesives.

[0004] Meanwhile, the release properties required for release films for precision material applications include peel strength in an appropriate range according to the type and application of the adhesive, a high residual adhesion rate so that the release layer is not transferred to the adhesive layer and the function of the adhesive layer is not reduced, solvent resistance so that the release layer is not damaged by the organic solvent used in the adhesive, and high adhesion between the release layer and the substrate so that the release layer does not fall off due to friction during processing, etc. In addition, as release films are also used as adhesive carrier films due to the thinning of the adhesive layer, stable release properties that do not change much with temperature and time must be ensured.

[0005] In addition, in the OLED process, the secondary materials used can cause the inflow of foreign matter and static electricity during the process, resulting in a decrease in yield. Therefore, secondary materials for protective films in the OLED process must have antistatic properties on both sides, not only for the adhesive base film but also for the release film.

[0006] Conventional technologies for such release films with antistatic properties on both sides are mainly manufactured through an offline manufacturing process in which the antistatic layer and the release layer are separately coated, which causes many quality problems due to foreign matter and scratches during the coating process in each process, and also causes problems in that the manufacturing cost is high.

[0007] In addition, the antistatic composition on the release surface and the opposite surface of the release surface interferes with hardening during silicone release coating, and the coating layer changes over time due to insufficient hardening, resulting in problems with reduced physical properties. Furthermore, after being laminated with the adhesive film, when wound into a roll or laminated into a sheet, there are many quality issues, such as the phenomenon of the sheets not being separated one by one due to contact between the adhesive film and the release film and blocking problems over time.

[0008] For the above reasons, the inventors have confirmed that by mixing a conductive polymer resin with excellent compatibility and a binder mixture with excellent reactivity into a silicone release coating composition for producing a release film, a silicone release film having antistatic properties on both sides can be produced in a single coating process, and have completed the present invention. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent Publication No. 10-2015-0104477 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been devised to solve the above problems and meet the conventional requirements, and an object of the present invention is to provide a double-sided antistatic silicone release film which has excellent antistatic properties and thereby can reduce problems such as product contamination and poor release caused by static electricity when peeled off from an adhesive when used as a release film for semiconductors, electric and electronic devices, and displays.

[0011] Yet another object of the present invention is to provide a double-sided antistatic silicone release film which has excellent peel strength and a high level of residual adhesion rate, thereby allowing it to be used appropriately according to the application without reducing the performance of the pressure-sensitive adhesive layer, has excellent durability of the cured layer by forming a dense cured layer, has resistance to organic solvents, has high adhesion between the cured layer and the substrate, and has stable release properties due to little change in physical properties over time and temperature.

[0012] It is yet another object of the present invention to provide a double-sided antistatic silicone release film that can reduce problems such as a decrease in the degree of hardening of the silicone release layer caused by forming antistatic layers on both sides to realize excellent antistatic properties, and a phenomenon in which the release film and adhesive film cannot be separated one by one after lamination.

[0013] The above and other objects and advantages of the present invention will become more apparent from the following detailed description of the preferred embodiment. [Means for solving the problem]

[0014] The above object can be achieved by a double-sided antistatic silicone release film comprising a base film, an antistatic silicone release layer which is a cured layer of an antistatic silicone release composition located on one side of the base film, and an antistatic layer which is a cured layer of the antistatic composition located on the other side of the base film.

[0015] Preferably, the antistatic composition may include a polyester binder, antistatic particles, a crosslinking agent, and a surfactant.

[0016] Preferably, the antistatic particles can be a conductive polymer resin.

[0017] Preferably, the conductive polymer resin has an average particle size of 10 to 90 nm and may be an aqueous dispersion containing a polyanion and a polythiophene or an aqueous dispersion containing a polyanion and a polythiophene derivative.

[0018] Preferably, the antistatic composition may contain 10 to 50 parts by weight of antistatic particles per 100 parts by weight of polyester binder.

[0019] Preferably, the antistatic composition may contain from 0.5 to 3% by weight solids.

[0020] Preferably, the dry thickness of the antistatic layer may be between 5 and 30 nm.

[0021] Preferably, the antistatic silicone release composition can include an alkenylpolysiloxane, a hydrogenpolysiloxane, a conductive polymer resin, a binder compound, and a platinum chelate catalyst.

[0022] Preferably, the antistatic silicone release composition contains 1 to 10 parts by weight of hydrogen polysiloxane, 1 to 5 parts by weight of conductive polymer resin, 10 to 20 parts by weight of epoxy binder compound, and 10 ppm to 1,000 ppm of platinum chelate catalyst, per 100 parts by weight of alkenyl polysiloxane.

[0023] Preferably, the antistatic silicone release composition may contain from 2.5 to 15% by weight solids.

[0024] Preferably, the antistatic silicone release layer may have a dry thickness of 0.01 to 10 μm.

[0025] Preferably, the antistatic silicone release layer has an intensity ratio of silicon ions exhibiting silicone release properties to sulfur ions exhibiting antistatic properties (Si - / S - ) is less than 1 and silicone release areas are greater than 10.

[0026] Preferably, the intensity ratio (Si - / S - ) may be 10 to 10,000 at the top, which is the furthest from the boundary with the base film, and 0.001 to 1 at the bottom, which is the boundary with the base film.

[0027] Preferably, the thickness ratio of the antistatic area and the silicone release area satisfies the following formula 1, (Formula 1) 1 / 10 <AV / RV<1 / 3で、 where AV can be the thickness of the antistatic area and RV can be the thickness of the silicone release area.

[0028] Preferably, the coefficient of friction value of the antistatic layer may be between 0.05 and 0.3.

[0029] Preferably, the water contact angle of the antistatic layer may be between 70 and 80 degrees.

[0030] Preferably, the double-sided antistatic silicone release film is a laminate of an adhesive film made of an adhesive and an adhesive base film on an antistatic silicone release layer, and two or more of the same interleaving films are laminated together. After aging at a temperature of 80° C. for six months, the shear strength of the interface between the adhesive base film and the antistatic silicone release layer when the interleaving films are separated is 5 N / m 2 It could be the following:

[0031] Preferably, the surface resistivity of the antistatic silicone release layer may be from 1x10^4 to 1x10^9 Ω / sq.

[0032] Preferably, the surface resistance of the antistatic layer may be 1x10^4 to 1x10^10 Ω / sq.

[0033] Preferably, the antistatic silicone release layer satisfies the following formulas 2 to 3 simultaneously: (Formula 2) 5≦RF≦30 (Formula 3) 80≦SA≦100 In the formula, RF (g / inch) can be the peel force of the antistatic silicone release layer, and SA (%) can be the residual adhesion rate of the antistatic silicone release layer. Effect of the Invention

[0034] According to the double-sided antistatic silicone release film of the present invention, since it has antistatic properties on both sides, it has the effect of solving problems such as contamination caused by static electricity and poor peeling that occur when the release film is separated from the adhesive layer.

[0035] Furthermore, since there is no factor interfering with the curing of the antistatic layer and the antistatic silicone release layer, the adhesive layer has excellent peel strength and a high level of residual adhesion, and thus has the effect of not deteriorating the functionality of the adhesive layer.

[0036] In addition, since the antistatic layer and the antistatic silicone release layer have excellent hardness and durability, they have excellent resistance to organic solvents and have high adhesion to the substrate, so that the antistatic layer and the antistatic silicone release layer are less likely to fall off due to friction.

[0037] In addition, since the surface of the antistatic layer has a water contact angle and a friction coefficient value within a specific range, it has the effect of suppressing blocking or the phenomenon of the sheets not being separated one by one even after being laminated with an adhesive film, wound into a roll or laminated in a sheet state, and then aged for a long period of time.

[0038] However, the effects of the present invention are not limited to those mentioned above, and other effects not mentioned will be clearly understood by those skilled in the art from the following description. [Brief description of the drawings]

[0039] [Figure 1] 1 is a schematic cross-sectional view of a double-sided antistatic silicone release film according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in order to enable those skilled in the art to easily carry out the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0041] In the drawings, the thickness of the layers and regions is exaggerated to clearly show them. Similar parts are designated by the same reference numerals throughout the specification. When a part, such as a layer, film, region, or plate, is described as being "on" another part, this includes not only the case where the part is "directly on" the other part, but also the case where there is another part between them. In contrast, when a part is described as being "directly on" another part, it means that there is no other part between them.

[0042] As used herein, the terms "comprise," "comprising," "include," "including," "containing," "characterized by," "has," "having," or any other variation thereof, are intended to cover an exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of elements is not necessarily limited to only those elements, but may include other elements that are not expressly recited or that are inherent to such process, method, article, or apparatus. Also, unless expressly stated to the contrary, "or" means an inclusive "or" and not an exclusive "or."

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one skilled in the art to which this invention belongs. In case of conflict, the present specification, including definitions, shall control. In addition, although methods and materials similar or equivalent to those described herein may be used in the practice or testing of the present invention, suitable methods and materials are described herein.

[0044] The present invention will now be described in detail with reference to the accompanying drawings.

[0045] 1 is a schematic cross-sectional view of a double-sided antistatic silicone release film according to an embodiment of the present invention. Referring to FIG 1, a double-sided antistatic silicone release film 100 according to an embodiment of the present invention includes a base film 120, an antistatic silicone release layer 110 which is a cured layer of an antistatic silicone release composition located on one side, and an antistatic layer 130 which is a cured layer of an antistatic composition located on the other side of the base film.

[0046] Here, the antistatic silicone release layer 110 has both antistatic properties and silicone release properties, and the antistatic layer 130 has antistatic properties. The antistatic properties and silicone release properties are realized simultaneously by coating the antistatic silicone release composition and the antistatic composition on both sides of the substrate film in-line once during the production of the release film.

[0047] In one embodiment, the antistatic composition forming the antistatic layer 130 may include a polyester binder, antistatic particles, a crosslinking agent, and a surfactant.

[0048] In one embodiment, the antistatic particles may be a conductive polymer resin, and preferably, for example, an aqueous dispersion containing polyanion and polythiophene or an aqueous dispersion containing polyanion and polythiophene derivative. The polyanion is an acidic polymer, such as a polymeric carboxylic acid or polymeric sulfonic acid, polyvinyl sulfonic acid, etc. Examples of polymeric carboxylic acids include polyacrylic acid, polymethacrylic acid, polymaleic acid, etc., and examples of polymeric sulfonic acids include, but are not limited to, polystyrene sulfonic acid, etc. It is preferable that the solid weight ratio of polyanion is excessive with respect to polythiophene or polythiophene derivative in terms of imparting conductivity. Therefore, in the embodiment of the present invention, an aqueous dispersion containing 0.5 wt % poly(3,4-ethylenedioxythiophene) and 0.8 wt % polystyrene sulfonic acid is used, but is not limited to this.

[0049] Preferably, the weight ratio of polyanion to polythiophene or polythiophene derivative is in the range of more than 1 and less than 5, more preferably more than 1 and less than 3.

[0050] In addition, it is preferable to use an aqueous dispersion of conductive polymer resin with an average particle size of 10 to 90 nm to achieve stable antistatic performance. In this case, when the average particle size of the conductive polymer resin is less than 10 nm, the molecular weight becomes smaller and the distance between the molecules becomes greater than a certain distance, making it impossible to realize antistatic performance, and when stretched in-line, the smaller the average particle size, the lower the antistatic performance. In addition, when the average particle size of the conductive polymer resin exceeds 90 nm, it is not uniformly distributed inside the cured layer, so the deviation in surface resistance becomes very large and it becomes impossible to properly realize antistatic performance.

[0051] In one embodiment, the antistatic composition preferably contains 10 to 50 parts by weight of antistatic particles per 100 parts by weight of polyester binder. If the antistatic particles are contained less than 10 parts by weight, they cannot be uniformly distributed on the substrate film, making it difficult to obtain excellent surface resistance properties, and if the antistatic particles are contained more than 50 parts by weight, the viscosity increases and a large amount of coating unevenness such as ribbing, rainbows, or clouds occurs, resulting in poor appearance.

[0052] In one embodiment, the binder of the antistatic composition is preferably a polyester-based binder. When a melamine-based, acrylic-based, oxazoline-based, or urethane-based binder is used, it is difficult to realize excellent surface resistance properties, and it acts as a curing interference factor of the silicone release layer, thereby reducing the silicone release properties. In addition, after the antistatic layer and the antistatic silicone release layer located on the other side are wound in a roll state, they are vulnerable to blocking during long-term aging, and there is a problem that the residual adhesion rate is reduced due to the post-cure interference factor of the antistatic silicone release layer.

[0053] In one embodiment, the crosslinking agent of the antistatic composition may be any one or more resins selected from the group consisting of isocyanate, carbonyl imide, oxazoline, and epoxy. The amount of the crosslinking agent resin added is preferably 200 to 600 parts by weight per 100 parts by weight of the conductive polymer resin. If the content of the crosslinking agent is less than 200 parts by weight, it is difficult to maintain the antistatic performance before and after rubbing or before and after cleaning with an organic solvent, so that durability is reduced and whitening may occur. On the other hand, if the content exceeds 600 parts by weight, the insulating effect of the crosslinking agent becomes large, so that the antistatic performance is rather reduced, and the durability against the antistatic performance is also reduced.

[0054] In one embodiment, the antistatic composition is preferably diluted to a solid content of 0.5 to 3 wt % and then coated on a polyester substrate film. If the solid content of the antistatic composition is less than 0.5 wt %, the thickness of the cured layer becomes too thin, resulting in poor coating coverage and poor appearance and physical properties. If the solid content exceeds 3 wt %, the viscosity of the antistatic composition becomes high, resulting in a large amount of coating unevenness.

[0055] In one embodiment, the dry thickness of the antistatic layer 130 is preferably 5 to 30 nm. At this time, if the dry thickness is less than 5 nm, the coverage of the antistatic layer is poor, which may result in poor appearance due to non-coating and reduced surface resistance properties, and if the dry thickness exceeds 30 nm, blocking may occur due to contact with the antistatic silicone release layer 110 on the other side during winding and long-term aging.

[0056] In one embodiment, the friction coefficient value of the antistatic layer 130 is preferably 0.05 to 0.3. At this time, if the friction coefficient value is less than 0.05, the slipperiness becomes strong and the winding section may become loose and the appearance may become poor due to scratches, and if it exceeds 0.3, the slipperiness may be insufficient, and after laminating with the adhesive film and laminating the laminated sheet, the laminated sheets may not be separated one by one when they are separated.

[0057] In one embodiment, the water contact angle of the antistatic layer 130 is preferably 70 to 80 degrees. At this time, if the water contact angle is less than 70 degrees, the surface can be easily contaminated due to high surface energy, and as the contact force with the antistatic silicone release layer on the other side increases, it becomes vulnerable to blocking. On the other hand, if the water contact angle exceeds 80 degrees, the slippage becomes strong after winding into a roll or laminating with an adhesive film, and thus, the winding cut surface and scratches may cause poor appearance.

[0058] In one embodiment, an adhesive film consisting of an adhesive and an adhesive base film is laminated on the antistatic silicone release layer 110, and two or more of the same interleaving films are laminated together. After aging at a temperature of 80° C. for six months, when the interleaving films are separated, the shear strength (tension) of the interface between the adhesive base film and the antistatic silicone release layer is 5 N / m 2 At this time, it is preferable that the shear strength (tensile strength) of the interface between the adhesive substrate film and the antistatic silicone release layer is 5 N / m or less. 2 If the number of sheets exceeds this, a problem occurs in that the sheets cannot be separated one by one.

[0059] Furthermore, the solvent for the antistatic silicone release composition is not limited to a particular type as long as it can disperse the solid content of the present invention and coat it onto the polyester substrate film. However, it is preferable to coat the composition in the form of an aqueous coating liquid containing water as the main medium.

[0060] The antistatic silicone release layer 110 according to one embodiment of the present invention can be formed by applying the above-mentioned antistatic silicone release composition to the base film 120 at least once using a known method such as a bar coating method, a reverse roll coating method, or a gravure roll coating method.

[0061] In one embodiment, the antistatic silicone release composition forming the antistatic silicone release layer 110 can include alkenyl polysiloxane, hydrogen polysiloxane, conductive polymer resin, binder compound, and platinum chelate catalyst. In one embodiment, the antistatic silicone release composition can further include an ionic surfactant having both cations and anions.

[0062] The alkenyl polysiloxane of the antistatic silicone release composition can have the structure of Formula 1 below: [ka] In the formula, m and n are each independently an integer of 10 to 500. In this case, m and n do not mean a block bond, but merely mean that the sum of the units is m and n, respectively.

[0063] Therefore, each unit in Chemical Formula 1 is randomly or block-bonded. Furthermore, R1, R2, and R3 are each an alkyl or alkenyl group selected from -CH3, -CH=CH2, -CH2CH=CH2, and -CH2CH2CH2CH2CH=CH2, and the alkenyl group may be present anywhere in the molecule, but it is preferable that at least two or more alkenyl groups are present.

[0064] Additionally, the hydrogen polysiloxane of the antistatic silicone release composition can have the structure of Formula 2 below. [ka] In the formula, a is an integer of 1 to 200, and b is an integer of 1 to 400. In this case, a and b do not mean block bonds, but merely mean that the sum of each unit is a and b. Therefore, in chemical formula 2, each unit is randomly bonded or block-bonded.

[0065] The alkenylpolysiloxane represented by Chemical Formula 1 and the hydrogenpolysiloxane represented by Chemical Formula 2 may be linear, branched, radial, or cyclic, or may be a mixture of these. In addition, the mixing ratio of the alkenylpolysiloxane and the hydrogenpolysiloxane is preferably 1 to 10 parts by weight of the hydrogenpolysiloxane per 100 parts by weight of the alkenylpolysiloxane. If the amount of the hydrogenpolysiloxane is less than 1 part by weight, the amount of unreacted alkenylpolysiloxane increases, making it impossible to obtain sufficient curing properties, and stable release properties cannot be realized, and if the amount of unreacted hydrogenpolysiloxane exceeds 10 parts by weight, the amount of unreacted hydrogenpolysiloxane increases, making it impossible to obtain sufficient curing properties, making it impossible to realize stable release properties.

[0066] In addition, the antistatic silicone release composition uses a conductive polymer resin to impart antistatic properties, and the conductive polymer resin is preferably an aqueous dispersion containing polyanion and polythiophene or an aqueous dispersion containing polyanion and polythiophene derivative. The polyanion is an acidic polymer, such as a polymeric carboxylic acid, polymeric sulfonic acid, or polyvinyl sulfonic acid. Examples of polymeric carboxylic acids include polyacrylic acid, polymethacrylic acid, and polymaleic acid, and examples of polymeric sulfonic acids include polystyrene sulfonic acid, but are not limited thereto.

[0067] In addition, it is preferable that the solid weight ratio of polyanion is excessive with respect to polythiophene or polythiophene derivative in terms of imparting electrical conductivity. In the embodiment of the present invention, an aqueous dispersion containing 0.5% by weight of poly(3,4-ethylenedioxythiophene) and 0.8% by weight of polystyrene sulfonic acid is used, but the present invention is not limited thereto. It is preferable that the weight ratio of polyanion to polythiophene or polythiophene derivative is in the range of more than 1 and less than 5, more preferably more than 1 and less than 3.

[0068] In addition, it is preferable to use an aqueous dispersion of conductive polymer resin particles with an average particle size of 10 to 90 nm to achieve stable antistatic performance. If the average particle size of the conductive polymer resin exceeds 90 nm, it is not uniformly distributed inside the cured layer, resulting in a large deviation in surface resistance and making it impossible to properly realize antistatic performance. If the average particle size of the conductive polymer resin is less than 10 nm, the molecular weight becomes smaller and the distance between the molecules becomes greater than a certain distance, making it impossible to realize antistatic performance. When stretched in-line, the smaller the average particle size, the lower the antistatic performance.

[0069] In one embodiment, the conductive polymer resin is preferably contained in an amount of 1 to 5 parts by weight based on 100 parts by weight of the alkenyl polysiloxane. If the content of the conductive polymer resin is less than 1 part by weight based on 100 parts by weight of the alkenyl polysiloxane, the antistatic properties are insufficient and the surface resistance properties are reduced, and if the content exceeds 5 parts by weight, the release properties are reduced due to the prevention of silicone curing.

[0070] In addition, the antistatic silicone release composition has stable release properties and antistatic properties by controlling the crosslink density, realizes uniform antistatic properties by increasing the compatibility of the conductive polymer resin, improves the solvent resistance and durability of the antistatic silicone release layer, and may contain a binder compound to increase the adhesion between the antistatic silicone release layer and the substrate film.

[0071] The binder compound may include a silane-based compound and a non-silane-based multifunctional compound. More specifically, the binder compound preferably has a weight ratio of the non-silane-based multifunctional compound to the silane-based compound of 2 to 20. The silane-based compound may be at least one of epoxy silane-based, amino silane-based, vinyl silane-based, methacryloxy silane-based, and isocyanate silane-based compounds, and the non-silane-based multifunctional compound may be an epoxy-based multifunctional compound having an epoxy functional group.

[0072] Epoxy-based polyfunctional compounds are preferred because epoxy-based compounds have excellent compatibility with conductive polymers and extensibility. That is, the compatibility differs depending on the N, C, and O content, and the conductive polymer resin has an alkenyl group as a functional group, which improves extensibility due to the swell effect. Such epoxy-based polyfunctional compounds have at least one functional group selected from the group consisting of amino-based, hydroxy-based, aldehyde-based, ester-based, vinyl-based, acrylic-based, imide-based, cyano-based, and isocyanate-based, and preferably have three or more functional groups in one molecule.

[0073] In one embodiment, the binder compound is an epoxy-based binder compound, and is preferably contained in an amount of 10 to 20 parts by weight based on 100 parts by weight of the alkenylpolysiloxane. If the content of the binder compound is less than 10 parts by weight, there are problems in that the adhesion of the cured layer to the substrate is low, leading to peeling of the cured layer, or the compatibility of the conductive polymer resin is reduced, leading to non-uniform antistatic performance, and if the content of the binder compound exceeds 20 parts by weight, there are problems in that the peel strength and residual adhesion rate are affected, leading to poor release properties.

[0074] In one embodiment, the antistatic silicone release composition contains a platinum chelate catalyst to facilitate the addition reaction of the alkenylpolysiloxane and the hydrogenpolysiloxane, and the platinum chelate catalyst is preferably present in the antistatic silicone release composition in an amount of 10 ppm to 1,000 ppm.

[0075] In one embodiment, the antistatic silicone release composition is preferably diluted to a solid content of 2.5 to 15% by weight and then coated onto a polyester substrate film. If the solid content of the antistatic silicone release composition is less than 2.5% by weight, a uniform cured layer cannot be obtained, and stable release and antistatic properties cannot be obtained. If the solid content exceeds 15% by weight, blocking occurs between the films, the adhesion of the coating composition to the substrate becomes poor, causing silicone transfer problems and poor coating appearance.

[0076] Furthermore, there is no limitation on the type of solvent for the antistatic silicone release composition, so long as it allows the solid content of the present invention to be dispersed and applied onto the polyester substrate film, but it is preferable to coat the composition in the form of an aqueous coating liquid containing water as the main medium.

[0077] The antistatic silicone release layer 110 of the double-sided antistatic silicone release film according to one embodiment of the present invention can be formed by applying the above-mentioned antistatic silicone release composition to the base film 120 at least once by a known method such as a bar coating method, a reverse roll coating method, or a gravure roll coating method.

[0078] In addition, the base film 120 according to an embodiment of the present invention is preferably a polyester base film, and has a thickness of 15 to 300 μm. If the thickness of the base film is less than 15 μm, the degree of deformation due to an external force becomes large, and the use as a carrier film cannot be fulfilled, and if the thickness of the film exceeds 300 μm, there is a problem that it is less economical.

[0079] In one embodiment, the dry thickness of the antistatic silicone release layer 110 is preferably 0.01 to 10 μm. If the dry thickness of the antistatic silicone release layer is less than 0.01 μm, a uniform antistatic silicone release layer may not be formed, and if it exceeds 10 μm, blocking may occur between the surface of the antistatic layer 130 located on one side of the polyester base film 120 and the surface of the antistatic silicone release layer 110 located on the other side.

[0080] In one embodiment, the antistatic silicone release layer 110 is formed by dissolving silicon ions (Si - ) and sulfur ions (S - ) Intensity (or counts) ratio (Si - / S - ) is less than 1 and silicone release areas are greater than 10. Such intensity ratios can be measured by TOF-SIMS and are the relative percentages of silicon ions and sulfur ions within a single cured layer.

[0081] In one embodiment, the intensity ratio (Si - / S - ) is preferably 10 to 10,000 at the top farthest from the boundary with the substrate film 120, and 0.001 to 1 at the bottom which is the boundary with the substrate film. This allows a single cured layer to simultaneously realize excellent antistatic properties and silicone release properties. Preferably, the intensity ratio at the top may be 100 to 5,000. This is because, like a phase separation structure, silicon ions that exhibit silicone release properties and sulfur ions that exhibit antistatic properties are embodied in a laminated form, allowing both properties to be realized simultaneously.

[0082] In one embodiment, the thickness ratio of the antistatic area to the silicone release area of ​​the antistatic silicone release layer 110 preferably satisfies the following formula 1. In this case, if the value of formula 1 is 1 / 10 or less, the surface resistance property of the antistatic silicone release layer decreases, and if it is 1 / 3 or more, the release property of the antistatic silicone release layer decreases. (Formula 1) 1 / 10 <AV / RV<1 / 3 で、 where AV is the thickness of the antistatic area and RV is the thickness of the silicone release area.

[0083] In one embodiment, the surface resistivity (Ω / sq) of the antistatic silicone release layer 110 is preferably 1×10^4 to 1×10^9.

[0084] In one embodiment, the surface resistance of the antistatic layer 130 is preferably 1×10^4 to 1×10^10 Ω / sq.

[0085] In one embodiment, the antistatic silicone release layer 110 preferably satisfies the following formulas 2 to 3 simultaneously. (Formula 2) 5≦RF≦30 (Formula 3) 80≦SA≦100 In the formula, RF (g / inch) is the peel force of the antistatic silicone release layer, and SA (%) is the residual adhesion rate of the antistatic silicone release layer.

[0086] If the peel strength of the antistatic silicone release layer is less than 5g / inch, there is a problem of pre-peeling occurring, where the adhesive peels off first before the peeling operation (process) or during storage or transportation, and if it exceeds 30g / inch, there is a problem of poor peeling occurring, where the adhesive falls off when peeled off due to the high peel strength. Also, if the residual adhesion rate of the antistatic silicone release layer is less than 80%, there is a problem of reduced performance of the adhesive layer. EXAMPLES

[0087] Hereinafter, the present invention will be described in more detail with reference to examples and comparative examples. However, these examples are provided to further explain the present invention, and the scope of the present invention is not limited to these examples.

[0088] Example 1 In order to form an antistatic silicone release layer on one side of a corona-treated polyester substrate film (Toray Advanced Materials Co., Ltd., Excell-50 μm), 100 parts by weight of alkenyl polysiloxane (Dow Corning Corporation), 3 parts by weight of hydrogen polysiloxane (Dow Corning Corporation), 2.5 parts by weight of conductive polymer resin (water dispersion containing 0.5% by weight of poly 3,4-ethylenedioxythiophene and 0.8% by weight of polystyrene sulfonic acid (molecular weight Mn = 150,000), average particle size 50 nm), 10 parts by weight of epoxy binder compound (Esprix Technologies Corporation), 50 ppm of platinum chelate catalyst (Dow Corning Corporation), and 0.2 parts by weight of ionic surfactant (dioctyl sulfosuccinate sodium salt) were diluted in water to produce an antistatic silicone release composition so that the solid content was 5% by weight.

[0089] On the other side of the substrate film, an antistatic layer was formed by mixing 1.5 parts by weight of a conductive polymer resin (aqueous dispersion containing 0.5% by weight of poly3,4-ethylenedioxythiophene and 0.8% by weight of polystyrenesulfonic acid (molecular weight Mn=150,000), average particle size 50 nm) as solid contents, 6 parts by weight of an epoxy-based crosslinking agent (manufactured by Esprix Technologies), 10 parts by weight of a polyester-based binder compound (manufactured by Base Korea), and 0.3 parts by weight of a diol-based surfactant (manufactured by Evonik) in water, and diluting the mixture with water to a solid content of 1.5% by weight.

[0090] The prepared antistatic silicone release composition and the antistatic composition were simultaneously coated on both sides of a polyester substrate film, and then dried at 180° C. for 50 seconds to prepare a double-sided antistatic silicone release film.

[0091] Example 2 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 10 parts by weight of hydrogenpolysiloxane was mixed with 100 parts by weight of alkenylpolysiloxane in the antistatic silicone release composition.

[0092] Example 3 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 1 part by weight of hydrogenpolysiloxane was mixed with 100 parts by weight of alkenylpolysiloxane in the antistatic silicone release composition.

[0093] Example 4 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 1 part by weight of conductive polymer resin was mixed with 100 parts by weight of alkenyl polysiloxane in the antistatic silicone release composition.

[0094] Example 5 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 5 parts by weight of the conductive polymer resin was mixed with 100 parts by weight of the alkenyl polysiloxane in the antistatic silicone release composition.

[0095] Example 6 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 15 parts by weight of an epoxy-based binder compound was mixed into the antistatic silicone release composition.

[0096] Example 7 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 20 parts by weight of an epoxy-based binder compound was mixed into the antistatic silicone release composition.

[0097] Example 8 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic silicone release composition was diluted with water to a solids content of 2.5% by weight.

[0098] Example 9 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition was diluted with water to a solids content of 1.0% by weight.

[0099] Example 10 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition was diluted with water to a solids content of 2.0% by weight.

[0100] Example 11 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition contained 1 part by weight of a conductive polymer resin.

[0101] Example 12 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition contained 3 parts by weight of a conductive polymer resin.

[0102] (Example 13) A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition contained 5 parts by weight of a polyester-based binder.

[0103] Example 14 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition contained 20 parts by weight of a polyester binder.

[0104] Example 15 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition contained 3 parts by weight of an epoxy-based crosslinking agent.

[0105] Example 16 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition contained 10 parts by weight of an epoxy-based crosslinking agent.

[0106] (Example 17) A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition was diluted with water to a solids content of 0.5% by weight.

[0107] (Example 18) A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition was diluted with water to a solids content of 3% by weight.

[0108] Comparative Example 1 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 0.5 parts by weight of hydrogenpolysiloxane was mixed with 100 parts by weight of alkenylpolysiloxane in the antistatic silicone release composition.

[0109] Comparative Example 2 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 11 parts by weight of hydrogenpolysiloxane was mixed with 100 parts by weight of alkenylpolysiloxane in the antistatic silicone release composition.

[0110] Comparative Example 3 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 0.5 parts by weight of a conductive polymer resin was mixed with 100 parts by weight of an alkenyl polysiloxane in the antistatic silicone release composition.

[0111] Comparative Example 4 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 7 parts by weight of the conductive polymer resin was mixed with 100 parts by weight of the alkenyl polysiloxane in the antistatic silicone release composition.

[0112] Comparative Example 5 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 21 parts by weight of an epoxy-based binder compound was mixed into the antistatic silicone release composition.

[0113] Comparative Example 6 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 5 parts by weight of an epoxy-based binder compound was mixed into the antistatic silicone release composition.

[0114] Comparative Example 7 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic silicone release composition was diluted with water to a solids content of 2% by weight.

[0115] Comparative Example 8 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic silicone release composition was diluted with water to a solids content of 20% by weight.

[0116] Comparative Example 9 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that no binder mixture was mixed into the antistatic silicone release composition.

[0117] Comparative Example 10 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that no conductive polymer resin was mixed into the antistatic silicone release composition.

[0118] Comparative Example 11 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the polyester-based binder compound was omitted from the antistatic composition.

[0119] Comparative Example 12 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the epoxy-based crosslinking agent was omitted from the antistatic composition.

[0120] Comparative Example 13 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 10 parts by weight of a melamine-based binder compound was mixed in place of 10 parts by weight of the polyester-based binder compound in the antistatic composition.

[0121] (Comparative Example 14) A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 10 parts by weight of an acrylic binder compound was mixed in place of 10 parts by weight of the polyester binder compound in the antistatic composition.

[0122] Comparative Example 15 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 10 parts by weight of an oxazoline-based binder compound was mixed in place of 10 parts by weight of a polyester-based binder compound in the antistatic composition.

[0123] Comparative Example 16 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that 10 parts by weight of a urethane-based binder compound was mixed in place of 10 parts by weight of the polyester-based binder compound in the antistatic composition.

[0124] Comparative Example 17 A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition was diluted with water to a solids content of 3.5% by weight.

[0125] (Comparative Example 18) A double-sided antistatic silicone release film was produced in the same manner as in Example 1, except that the antistatic composition was diluted with water to a solids content of 0.3% by weight.

[0126] Using the double-sided antistatic silicone release films according to Examples 1 to 18 and Comparative Examples 1 to 18, physical properties were measured through the following experiments, and the results are shown in Tables 1 and 2 below.

[0127] (Experimental Example) 1. Antistatic properties Using a surface resistance measuring instrument (Mitsubishi, MCP-T600), the sample was placed in an environment of 23° C. and 50% RH, and the surface resistance of the antistatic layer and the antistatic silicone release layer were measured according to JIS K7194.

[0128] 2. Peel force measurement A release film was attached to a cold-rolled stainless steel plate with double-sided adhesive tape so that the antistatic silicone release layer was on top, and then an adhesive tape (TESA 7475) was placed on the antistatic silicone release layer and pressed with a 2 kg pressure roller, and the sample was left at room temperature for 1 to 7 days, after which the peel force was measured. The peel force was measured using an AR-1000 (Chem-Instrument) at a peel angle of 180° and a peel speed of 0.3 mpm, and the average value (g / inch) was calculated from 5 measurements and rounded off to the nearest decimal place.

[0129] 3.Residual adhesion rate measurement An adhesive tape (Nitto 31B) was placed on the antistatic silicone release layer, pressed with a 2 kg pressure roller, and left at room temperature for 30 minutes. The adhesive tape was then peeled off from the cured layer and attached to a cold-rolled stainless steel plate, after which the peel force was measured.

[0130] For comparison, an adhesive tape (Nitto 31B) that had not been used was attached to a cold-rolled stainless steel plate and the peel strength was measured.

[0131] The peel strength was measured using AR-1000 (Chem-Instrument) at a peel angle of 180° and a peel speed of 0.3 mpm, and the average value was calculated from five measurements. The residual adhesion rate was calculated according to the following equation 1.

number

[0132] 4.Water contact angle measurement The water contact angle of the antistatic layer surface of a 5cm x 5cm double-sided antistatic silicone release film sample was measured. The water contact angle was measured using a DROPMASTER 300 (KYOWA INTERFACE SCIENCE), and the average value was calculated from three measurements.

[0133] 5. Dry thickness measurement The dry thickness of the antistatic layer of a 5 cm x 5 cm double-sided antistatic silicone release film sample was measured. The thickness was measured using an ellipsometer, Elli-SE (manufactured by Elipso Technology), and the average value was calculated from three measurements.

[0134] 6. Shear Strength Measurement The antistatic silicone release layer of a 5cm x 5cm double-sided antistatic silicone release film and the adhesive film (3M acrylic adhesive - 30μm + Toray Advanced Materials XD500 - 50μm) are laminated with two or more sheets of the same laminated paper, and after aging in an 80 degree environment for six months, the shear strength (N / m 2 The shear strength was measured using a TAXplus50 (manufactured by SMS, UK), and the average value was calculated from three measurements.

[0135] 7. Friction coefficient measurement The friction coefficient of a 5cm x 5cm double-sided antistatic silicone release film was measured. The friction coefficient was measured by preparing two double-sided antistatic silicone release films and measuring the surface of the antistatic layer. The friction coefficient was measured using a 14FW (manufactured by HEIDON), and the average value was calculated from three measurements.

[0136] 8. Coating appearance (defect area measurement) The area of ​​bubble defects was measured for the area of ​​the antistatic layer of a 5cm x 5cm double-sided antistatic silicone release film sample. The longest length of the bubble defect in the 5cm x 5cm release film sample was measured, the area was calculated with a circle, and the total area was calculated as the bubble defect area (cm 2 The degree of bubble defects (coating appearance) was calculated by calculating the bubble defect area ratio according to the following formula 2, and evaluated according to the following criteria. (Formula 2) Air bubble defect area ratio (%) = Air bubble defect area / 25cm 2 X100(%) ◎: 0% or more but less than 1% ○: 1% or more but less than 2% △: 2% or more but less than 5% X: 5% or more

[0137] 9. Solvent resistance measurement The resistance to solvents of the surface of the antistatic silicone release layer of the double-sided antistatic silicone release film sample was measured. The solvent resistance was measured by dipping a cotton swab in methyl ethyl ketone, and then moving the cotton swab back and forth 10 times at a 45 degree angle over the antistatic silicone release layer with a 100g load, and then evaluating the solvent resistance of the coating surface according to the following criteria: ◎:Even number ○: Good △:Normal X: Unpaid

[0138] 10. Slippage measurement The surface of the antistatic silicone release layer of the double-sided antistatic silicone release film sample was stroked back and forth five times with the thumb, and then the surface was inspected with the naked eye and evaluated according to the following criteria. ◎: No change after evaluation (No smear) ○: Slightly slippery, but no problem in use (Slightly smeared) △: The hardened layer is white and hazy, like oil sliding. X: The hardened layer hardens and can be removed (Rub-off)

[0139] 11. Measuring the separation of each piece An adhesive film and a double-sided antistatic silicone release film were laminated together, and when the laminated products were separated, measurements were made to see whether or not there was a phenomenon of two or more sheets of laminated products sticking together and not being separated. If there was no phenomenon such as blocking, where the sheets could not be separated one by one, it was displayed as "O", and if there was a phenomenon such as blocking, where the sheets could not be separated one by one, it was displayed as "X".

[0140] [Table 1]

[0141] [Table 2]

[0142] As can be seen from Table 1 above, the double-sided antistatic silicone release films according to Examples 1 to 18 of the present invention have excellent coating appearance, excellent slippage of the antistatic silicone release layer, and both sides have surface resistance and peel strength within appropriate ranges, and the residual adhesion rate is also excellent. In addition, the crosslinking degree of the cured layer coated on both sides of the substrate film is excellent, and there is no post-cure obstruction between the antistatic layer and the antistatic silicone release layer, so that even after processing with the adhesive and laminating, and aging at high temperature for a long time, a phenomenon in which the films cannot be separated one by one, such as blocking, does not occur.

[0143] More specifically, as can be seen from the double-sided antistatic silicone release films of Examples 2 and 3 of the present invention and Comparative Examples 1 and 2, it can be seen that the physical properties of peel force and residual adhesion rate change in a correlated manner depending on the degree of crosslinking of the antistatic silicone release layer.

[0144] In addition, it can be confirmed that the antistatic properties of the antistatic silicone release layer made of the epoxy-based binder compound and conductive polymer resin in the double-sided antistatic silicone release film of Examples 4 to 7 of the present invention are excellent in terms of surface resistance as the content of the conductive polymer and epoxy-based binder compound increases based on the same composition.

[0145] In addition, it was confirmed that the thicker the dry thickness of the antistatic silicone release layer in the double-sided antistatic silicone release films of Examples 9, 10, 17, and 18 of the present invention, the better the release properties are. It was confirmed that the thickness of the antistatic layer does not affect the antistatic silicone release layer, but the shear strength value changes in a correlated manner depending on the dry thickness value.

[0146] It can also be seen that the higher the content of conductive polymer resin in the antistatic layer of the double-sided antistatic silicone release films according to Examples 11 and 12 of the present invention, the more excellent the surface resistance.

[0147] In addition, it can be seen that the content of the polyester binder in the antistatic layer in the double-sided antistatic silicone release film of Examples 13 and 14 of the present invention does not affect the antistatic silicone release layer, but does change the shear strength value in a correlated manner depending on the dry thickness.

[0148] In addition, it can be seen that the surface resistance property changes in correlation with the content of the epoxy-based crosslinking agent in the antistatic layer of the double-sided antistatic silicone release film according to Examples 15 and 16 of the present invention.

[0149] In contrast, as can be seen from Table 2 above, it can be seen that depending on the degree of hardening of the antistatic silicone release layer in the double-sided antistatic silicone release films of Comparative Examples 1 and 2, the residual adhesion rate is insufficient or the peel force increases excessively.

[0150] In addition, when the amount of conductive polymer resin or epoxy-based binder compound in the antistatic silicone release layer in the double-sided antistatic silicone release films according to Comparative Examples 3 to 6 is too little or too much, it can be confirmed that the surface resistance properties are reduced or the degree of hardening of the antistatic silicone release layer is reduced.

[0151] In addition, in the antistatic silicone release composition of the double-sided antistatic silicone release film of Comparative Examples 7 and 8, when the solid content is low or high, it can be seen that the surface resistance decreases or the peel force increases, and as the shear strength value increases, the film cannot be separated one by one.

[0152] In addition, in the antistatic silicone release composition of the double-sided antistatic silicone release films according to Comparative Examples 9 to 16, if the binder mixture or conductive polymer resin is not mixed, or if the binder compound composition of the antistatic composition interferes with the post-cure of the antistatic silicone release layer, the residual adhesion rate decreases, the water contact angle of the antistatic layer falls outside the range of the present invention, or the shear strength value increases and the films cannot be separated one by one.

[0153] In addition, in the double-sided antistatic silicone release films of Comparative Examples 17 and 18, when the dry thickness of the antistatic layer is excessively thick, the shear strength value increases, causing a problem in which the layers cannot be separated one by one, and when the dry thickness of the antistatic layer is excessively thin, the surface resistance properties decrease.

[0154] As described above, the double-sided antistatic silicone release film according to the present invention can be appropriately applied to a desired application, but is not limited thereto. In addition, the present invention can provide a double-sided antistatic silicone release film of excellent quality for use in applications in the field of precision materials, which has an appropriate range of peel strength and a high level of residual adhesion rate, and can be appropriately used to suit the application without deteriorating the function of the adhesive layer.

[0155] Furthermore, the double-sided antistatic silicone release film according to the present invention has excellent durability of the cured layer, excellent resistance to organic solvents, high adhesion to the substrate, and the cured layer is less likely to fall off due to friction. In addition, it has excellent antistatic properties, which can solve problems such as contamination caused by static electricity and poor peeling.

[0156] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also belong to the scope of the present invention. [Explanation of symbols]

[0157] 100 Double-sided antistatic silicone release film 110 Antistatic silicone release layer 120 Base film 130 Antistatic layer.

Claims

1. A base film; an antistatic silicone release layer which is a cured layer of an antistatic silicone release composition located on one side of the base film; and an antistatic layer which is a cured layer of an antistatic composition located on the other side of the base film, The antistatic silicone release composition comprises an alkenyl polysiloxane, a hydrogen polysiloxane, a conductive polymer resin, a binder compound, and a platinum chelate catalyst; The double-sided antistatic silicone release film, wherein the antistatic composition comprises a polyester binder, antistatic particles, a crosslinking agent and a surfactant.

2. 2. The double-sided antistatic silicone release film of claim 1, wherein the antistatic particles are a conductive polymer resin.

3. 3. The double-sided antistatic silicone release film according to claim 2, wherein the conductive polymer resin has an average particle size of 10 to 90 nm and is an aqueous dispersion containing polyanion and polythiophene or an aqueous dispersion containing polyanion and polythiophene derivative.

4. 2. The double-sided antistatic silicone release film according to claim 1, wherein the antistatic composition comprises 10 to 50 parts by weight of antistatic particles per 100 parts by weight of a polyester binder.

5. 2. The double-sided antistatic silicone release film of claim 1, wherein the antistatic composition comprises 0.5 to 3 weight percent solids.

6. 2. The double-sided antistatic silicone release film of claim 1, wherein the antistatic layer has a dry thickness of 5 to 30 nm.

7. 2. The double-sided antistatic silicone release film according to claim 1, wherein the antistatic silicone release composition comprises, relative to 100 parts by weight of the alkenylpolysiloxane, 1 to 10 parts by weight of a hydrogenpolysiloxane, 1 to 5 parts by weight of a conductive polymer resin, 10 to 20 parts by weight of an epoxy binder compound, and 10 ppm to 1,000 ppm of a platinum chelate catalyst.

8. 2. The double-sided antistatic silicone release film of claim 1, wherein the antistatic silicone release composition comprises 2.5 to 15 weight percent solids.

9. 2. The double-sided antistatic silicone release film of claim 1, wherein the antistatic silicone release layer has a dry thickness of 0.01 to 10 [mu]m.

10. The antistatic silicone release layer has an intensity ratio of silicon ions that exhibit silicone release properties and sulfur ions that exhibit antistatic properties (Si - / S - 2. The double sided antistatic silicone release film of claim 1 , comprising antistatic areas having a R(N) of less than 1 and silicone release areas having a R(N) of greater than 10.

11. The intensity ratio of the antistatic silicone release layer (Si - / S - 10. The double-sided antistatic silicone release film according to claim 9, wherein the surface roughness (T) is 10 to 10,000 at the top farthest from the boundary with the base film, and 0.001 to 1 at the bottom which is the boundary with the base film.

12. The thickness ratio of the antistatic area and the silicone release area satisfies the following formula 1, (Formula 1) 1 / 10<AV / RV<1 / 3, 11. The double sided antistatic silicone release film of claim 10, wherein AV is the thickness of the antistatic region and RV is the thickness of the silicone release region.

13. 13. The double-sided antistatic silicone release film according to claim 1, wherein the antistatic layer has a coefficient of friction of 0.05 to 0.

3.

14. 13. The double-sided antistatic silicone release film according to claim 1, wherein the antistatic layer has a water contact angle of 70 to 80 degrees.

15. The double-sided antistatic silicone release film is laminated with an adhesive film consisting of an adhesive and an adhesive base film on the antistatic silicone release layer, and two or more of the same interleaving films are laminated together. After aging at a temperature of 80° C. for six months, the shear strength of the interface between the adhesive base film and the antistatic silicone release layer when the interleaving films are separated is 5 N / m 2 13. The double-sided antistatic silicone release film according to claim 1, wherein:

16. 13. The double-sided antistatic silicone release film according to claim 1, wherein the surface resistance of the antistatic silicone release layer is 1x10^4 to 1x10^9 Ω / sq.

17. 13. The double-sided antistatic silicone release film according to claim 1, wherein the surface resistance of the antistatic layer is 1x10^4 to 1x10^10 Ω / sq.

18. The antistatic silicone release layer satisfies the following formulas 2 to 3 simultaneously, (Formula 2) 5≦RF≦30 (Formula 3) 80≦SA≦100 13. The double-sided antistatic silicone release film according to claim 1, wherein RF (g / inch) is the peel strength of the antistatic silicone release layer, and SA (%) is the residual adhesion rate of the antistatic silicone release layer.

Citation Information

Patent Citations

  • Antistatic film, and coating for forming antistatic layer

    JP2007321014A

  • Tight-release coating polyester film

    KR1020150104477A

  • Antistatic film and liquid crystal display device

    WO2016063793A1

  • Mold release film

    WO2016133092A1

  • Antistatic silicone release film

    WO2020189882A1