Manufacturing method and apparatus for rubber-coated wire
By using a rubber viscosity index and temperature correlation to control the coating process, the method and apparatus stabilize the coating thickness of rubber-coated wires, addressing fluctuations and improving production quality and efficiency.
Patent Information
- Application Number
- JP2021011734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-28
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2041-01-28
AI Technical Summary
Existing methods for manufacturing rubber-coated wires fail to stably adjust the coating thickness of unvulcanized rubber to a target value due to the detection of outer diameter downstream of the heating position, leading to fluctuations and inconsistencies in the coating thickness.
A method and apparatus that utilize a rubber viscosity index and temperature correlation to adjust the coating thickness by controlling the temperature of the wire's outer peripheral surface during the coating process, ensuring stable adherence of unvulcanized rubber to the wire.
The method and apparatus enable the coating thickness to be accurately set to a target value, reducing fluctuations and improving the stability and quality of the rubber-coated wire production, enhancing productivity and reducing defects.
Smart Images

Figure 0007590649000001 
Figure 0007590649000002 
Figure 0007590649000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and apparatus for manufacturing a rubber-coated wire, and more particularly to a method and apparatus for manufacturing a rubber-coated wire that can more stably achieve a target coating thickness of unvulcanized rubber that coats the outer surface of the wire. [Background technology]
[0002] When manufacturing rubber products such as tires, rubber-coated wires, in which the outer surface of the wire is coated with unvulcanized rubber, are used. Rubber-coated wires are manufactured, for example, by passing a wire through unvulcanized rubber extruded from a rubber extruder. The thickness of the coating of unvulcanized rubber on this rubber-coated wire varies depending on various factors, such as manufacturing conditions, the type and lot of unvulcanized rubber, etc.
[0003] In order to stabilize the coating thickness of the unvulcanized rubber, it has been proposed to detect the outside diameter of the rubber-coated wire immediately after it passes through the unvulcanized rubber, and adjust the temperature of the wire immediately before it passes through the unvulcanized rubber based on the results of comparing the detected outside diameter data with a preset target outside diameter (see Patent Document 1). Since changing the wire temperature changes the amount of unvulcanized rubber adhering to the outer circumferential surface of the wire, it is possible to set the coating thickness to the target value by appropriately controlling the wire temperature.
[0004] However, in the wire movement path, the position where the outer diameter of the rubber-coated wire is detected (detection position) is downstream of the position where the wire is heated (heating position). Therefore, for the range of the rubber-coated wire extending between the detection position and the heating position at the time when the outer diameter of the rubber-coated wire is detected, it is not possible to pass the rubber-coated wire through the unvulcanized rubber in a state where the temperature is changed based on the detected outer diameter data. In this way, with the conventionally proposed method, there is a range of the rubber-coated wire where the coating thickness cannot be appropriately adjusted based on the detected outer diameter data, so there is room for improvement in order to more stably set the coating thickness to the target value. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-138467 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a method and apparatus for manufacturing a rubber-coated wire, which can more stably adjust the coating thickness of unvulcanized rubber that coats the outer peripheral surface of the wire to a target value. [Means for solving the problem]
[0007] In order to achieve the above object, the present invention provides a method for producing a rubber-coated wire, which comprises continuously passing a wire through unvulcanized rubber extruded from a rubber extruder to coat the outer circumferential surface of the wire with the unvulcanized rubber, and then adjusting the thickness of the unvulcanized rubber covering the wire to a target value. As a correlation, The correlation between the rubber viscosity index and the temperature of the outer surface of the wire at the time when the unvulcanized rubber is coated is grasped in advance and input into a control unit, and based on the correlation and the rubber viscosity index grasped before the outer surface of the wire is coated with the unvulcanized rubber, the control unit calculates an appropriate value for the temperature of the outer surface of the wire that will make the coating thickness the target value, and a heating mechanism adjusts the temperature of the outer surface of the wire at the time when the unvulcanized rubber is coated to the calculated appropriate value, and the wire is continuously passed through the unvulcanized rubber extruded from the rubber extruder.
[0008] The rubber-coated wire manufacturing apparatus of the present invention includes a rubber extruder and a wire moving mechanism for passing a wire through unvulcanized rubber extruded from the rubber extruder, and the unvulcanized rubber is coated on the outer peripheral surface of the wire after the wire has passed through the unvulcanized rubber. 、Set the coating thickness for the wire to a target value As a correlation, The wire extrusion machine is equipped with a control unit to which a previously determined correlation between a rubber viscosity index and the temperature of the outer surface of the wire at the time when the unvulcanized rubber is coated is input, a data acquisition unit to acquire the rubber viscosity index before coating the outer surface of the wire with the unvulcanized rubber, and a heating mechanism to adjust the temperature of the outer surface of the wire at the time when the unvulcanized rubber is coated, and based on the correlation and the rubber viscosity index acquired by the data acquisition unit, the control unit calculates an appropriate value for the temperature of the outer surface of the wire that will bring the coating thickness to the target value, and the control unit controls the heating mechanism to adjust the temperature of the outer surface of the wire at the time when the unvulcanized rubber is coated to the calculated appropriate value, and then passes the wire through the unvulcanized rubber extruded from the rubber extruder. Effect of the Invention
[0009] In the present invention, focusing on the fact that the viscosity of the unvulcanized rubber greatly affects the coating thickness, an index closely related to the change in viscosity is used as the rubber viscosity index (including viscosity). Then, using two items, the rubber viscosity index and the temperature of the outer peripheral surface of the wire at the time of coating the unvulcanized rubber, a correlation between the rubber viscosity index and the temperature that makes the coating thickness a target value is grasped in advance. Then, based on the correlation and the rubber viscosity index grasped before coating the outer peripheral surface of the wire with the unvulcanized rubber, an appropriate value of the temperature that makes the coating thickness the target value is calculated. The wire is adjusted by the heating mechanism so that the temperature becomes the appropriate value at the time of coating the unvulcanized rubber, and is continuously passed through the unvulcanized rubber extruded from the rubber extruder. Therefore, the coating thickness is appropriately adjusted to the target value over the entire length of the wire, and the coating thickness can be more stably set to the target value. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is an explanatory diagram illustrating a side view of a rubber-coated wire manufacturing apparatus according to the present invention. [Diagram 2] FIG. 2 is an explanatory diagram illustrating the manufacturing apparatus of FIG. 1 in a plan view. [Diagram 3] FIG. 2 is an explanatory diagram illustrating a cross-sectional view of a manufactured rubber-coated wire. [Figure 4] FIG. 2 is a graph illustrating the relationship between the outer diameter (coating thickness) of a rubber-coated wire and the temperature of the outer circumferential surface of the wire. [Diagram 5] FIG. 2 is a graph illustrating the correlation between the viscosity of unvulcanized rubber and the temperature of the outer circumferential surface of the wire in order to set the outer diameter (coating thickness) of the rubber-coated wire to a target value. [Figure 6] 4 is a graph illustrating the relationship between the viscosity of unvulcanized rubber and the internal pressure of the head. FIG. [Figure 7] FIG. 2 is a graph illustrating the correlation between the head pressure of a rubber extruder and the temperature of the outer peripheral surface of a wire in order to set the outer diameter (coating thickness) of a rubber-coated wire to a target value. [Figure 8] FIG. 2 is a graph illustrating the relationship between the viscosity and hardness of unvulcanized rubber. [Figure 9] FIG. 4 is a graph illustrating the relationship between the viscosity of unvulcanized rubber and the torque required to drive a screw. [Figure 10] FIG. 2 is an explanatory diagram illustrating the change over time in the outer diameter (coating thickness) of a rubber-coated wire manufactured by applying the present invention. [Figure 11] FIG. 1 is an explanatory diagram illustrating the change over time in the outer diameter (coating thickness) of a rubber-coated wire manufactured by a conventional technique. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a method and an apparatus for manufacturing a rubber-coated wire according to the present invention will be described with reference to the embodiments shown in the drawings.
[0012] A rubber-coated wire Wr shown in Fig. 3 is manufactured using a rubber-coated wire manufacturing apparatus 1 (hereinafter referred to as manufacturing apparatus 1) of the present invention shown in Fig. 1 and Fig. 2. The rubber-coated wire Wr is formed by coating the outer circumferential surface of a steel wire W with unvulcanized rubber R. Since the outer diameter d0 of the wire W is known, if the outer diameter d of the rubber-coated wire Wr is known, the coating thickness h of the unvulcanized rubber R in the rubber-coated wire Wr is also known. In other words, the coating thickness h = (outer diameter d - outer diameter d0) / 2. The rubber-coated wire Wr is formed, for example, into an annular shape and used as a bead core, which is a component of a tire.
[0013] As shown in Fig. 11, the outer diameter d (coating thickness h) of the manufactured rubber-coated wire Wr varies due to various factors such as differences in the lot of the unvulcanized rubber R, even if the wire is manufactured using the same manufacturing equipment under the same conditions. In Fig. 11, the target values of the outer diameter d and the coating thickness h are indicated as Gd and Gh, respectively, and the allowable range for the target values is indicated as AW. Note that this allowable range AW is a tolerance range in the manufacturing process that is stricter than the allowable range as a component of the rubber-coated wire Wr. The moving speed of the wire W is made substantially constant.
[0014] In particular, during the initial period TF from time T1, when the manufacturing process is started or when the lot of unvulcanized rubber R is changed, to time T2, when a predetermined time has elapsed, the fluctuations in the outer diameter d (coating thickness h) become large. In the stable period TS after the initial period TF has elapsed, the fluctuations in the outer diameter d (coating thickness h) become small and stable. When the rubber-coated wire Wr is manufactured by the conventional method, the fluctuations in the outer diameter d (coating thickness h) become large and the initial period TF becomes long, as shown in FIG. 11. Therefore, in the present invention, the fluctuations in the outer diameter d (coating thickness h) are reduced and the initial period TF is shortened so that the stable period TS is reached early.
[0015] This embodiment of the manufacturing apparatus 1 includes a reel 4 around which the wire W is wound and stored, a rubber extruder 2 that extrudes unvulcanized rubber R, a drum 5 that winds up the rubber-coated wire Wr, a rubber viscometer 7a and a pressure sensor 7b, a heating mechanism 8, a temperature sensor 9, and a control unit 11. The rotationally driven drum 5 functions as a wire moving mechanism that moves the wire W from the reel 4 toward the drum 5. In this embodiment, a flange portion 5a is protrudingly provided on the outer circumferential surface of the drum 5, the flange portion 5a being continuous around the entire circumference.
[0016] The rubber viscometer 7a and the pressure sensor 7b function as a data acquisition unit that acquires a rubber viscosity index PN, which will be described later. In this embodiment, the manufacturing apparatus 1 further includes a festoon unit 6 and an outer diameter sensor 10 that detects the outer diameter of the rubber-coated wire Wr.
[0017] The rubber extruder 2 has a cylinder body 2a, a screw 2b disposed inside the cylinder body 2a, and a head 3 attached to the tip of the cylinder body 2a. A wire inlet 3a, a wire outlet 3b, and an overflow outlet are formed in the head 3. The wire inlet 3a and the wire outlet 3b are disposed at positions facing each other.
[0018] The screw 2b, which is rotated by the drive motor 2c, moves the unvulcanized rubber R fed into the cylinder body 2a toward the head 3, heats it, and extrudes it into the head 3. This rubber extruder 2 is a so-called crosshead type. The inside of the head 3 is filled with unvulcanized rubber R, and excess unvulcanized rubber R is discharged from an overflow outlet.
[0019] The head 3 is disposed midway along the path of movement of the wire W from the reel 4 to the drum 5, and the wire W unwound from the reel 4 enters the inside of the head 3 through the wire inlet 3a and exits from the inside of the head 3 through the wire outlet 3b. The wire W unwound from the reel 4 thus penetrates the head 3 filled with unvulcanized rubber R, passing through the unvulcanized rubber R, and the unvulcanized rubber R adheres to the outer circumferential surface of the wire W. Therefore, by penetrating and moving through the head 3, the wire W becomes a rubber-coated wire Wr and moves from the wire outlet 3b toward the drum 5.
[0020] The manufacturing apparatus 1 of this embodiment has a festoon section 6 on the way from the head 3 to the drum 5. The festoon section 6 includes a driving roller 6a and a support roller 6b arranged opposite to each other. The support roller 6b is installed so that it can approach and move away from the driving roller 6a. The rubber-coated wire Wr manufactured by penetrating the head 3 moves toward the drum 5 after being wound around the driving roller 6a and the support roller 6b. The wire W (rubber-coated wire Wr) moves from the reel 4 toward the drum 5 by the driving roller 6a that is driven to rotate, so the driving roller 6a also functions as a wire moving mechanism. Note that the driving roller 6a is not limited to being installed in the festoon section 6, and can be installed in another position. For example, the festoon section 6 can be configured with a pair of support rollers 6b whose interval can be changed, and the driving roller 6a can be installed between the festoon section 6 and the rubber extruder 2 (head 3) and between the festoon section 6 and the drum 5.
[0021] The length of the movement path of the wire W from the reel 4 to the drum 5 is shortened when the support roller 6b moves toward the drive roller 6a, and is lengthened when the support roller 6b moves away from the drive roller 6a. Therefore, the movement path length is adjusted by the movement of the support roller 6b toward or away from the drive roller 6a. Therefore, even if the winding of the rubber-coated wire Wr by the drum 5 stops, the movement path length is lengthened, so that the rubber extruder 2 can continue to extrude the unvulcanized rubber R without interrupting production of the rubber-coated wire Wr.
[0022] The rubber viscometer 7a and the pressure sensor 7b functioning as data acquisition units acquire data on the rubber viscosity index PN. The rubber viscosity index PN is an index of rubber physical properties or equipment that is closely related to the viscosity fluctuation of the unvulcanized rubber R and is largely caused by the viscosity fluctuation, and includes the viscosity of the unvulcanized rubber R itself. As a specific rubber viscosity index PN, the viscosity PNa of the unvulcanized rubber R, the hardness PNb, the internal pressure PNc of the rubber extruder 2 when extruding the unvulcanized rubber R, or the drive torque PNd required to rotate the screw 2b can be used. As the rubber viscosity index PN, at least one of these four items (PNa, PNb, PNc, PNd) may be used, and in this embodiment, the viscosity PNa of the unvulcanized rubber R or the internal pressure PNc of the rubber extruder 2 is used.
[0023] The data acquisition units 7a and 7b grasp the rubber viscosity index PN of the unvulcanized rubber R before it is coated on the outer peripheral surface of the wire W. The rubber viscometer 7a acquires the viscosity PNa of the unvulcanized rubber R before it is fed into the rubber extruder 2. As the rubber viscometer 7a, for example, a known viscometer such as a Mooney viscometer can be used. Alternatively, the rubber extruder 2 can be equipped with a function for grasping the rubber viscosity, and a rubber viscometer that grasps the viscosity PNa of the unvulcanized rubber R in the rubber extruder 2 can be used. The data of the viscosity PNa grasped by the rubber viscometer 7a is input to the control unit 11.
[0024] This pressure sensor 7b is attached to the head 3 and acquires the internal pressure PNc of the head 3. Any known pressure sensor of various specifications can be used for the pressure sensor 7b. It is also possible to use a pressure sensor 7b that grasps the internal pressure PNc of the cylinder main body 2a. The data of the internal pressure PNc grasped by the pressure sensor 7b is input to the control unit 11.
[0025] When the hardness PNb of the unvulcanized rubber R is adopted as the rubber viscosity index PN, a known rubber hardness meter is used as the data acquisition unit. This rubber hardness meter acquires the hardness PNb of the unvulcanized rubber R before it is fed into the rubber extruder 2.
[0026] When the driving torque PNd required to rotate the screw 2b is used as the rubber viscosity index PN, a power meter or the like that detects the power consumption of the driving motor 2c when the screw 2b is rotated is used as the data acquisition unit. This power meter detects the power consumption of the driving motor 2c when the unvulcanized rubber R is moved inside the cylinder body 2a toward the head 3, and the driving torque PNd is grasped based on the detected power consumption. The data of the hardness PNb and the driving torque PNd acquired by the data acquisition unit are input to the control unit 11.
[0027] The heating mechanism 8 heats the outer peripheral surface of the wire W to an appropriate value Gt at the time when the wire W is coated with the unvulcanized rubber R. As the heating mechanism 8, it is preferable to use a non-contact type such as a known high-frequency heating device or an electric heater.
[0028] The temperature sensor 9 detects the temperature t of the outer circumferential surface of the wire W just before it is covered with the unvulcanized rubber R, that is, the temperature t at the time when it is substantially covered with the unvulcanized rubber R. It is preferable to use a known non-contact type as the temperature sensor 9. The data of the temperature t detected by the temperature sensor 9 is input to the control unit 11.
[0029] The outer diameter sensor 10 is disposed near the wire outlet 3b and detects the outer diameter d of the rubber-coated wire Wr immediately after it has passed through the head 3. A non-contact type displacement sensor or the like can be used as the outer diameter sensor 10. Data on the outer diameter d detected by the outer diameter sensor 10 is input to the control unit 11.
[0030] The control unit 11 controls the manufacturing apparatus 1. Therefore, the operation of the screw 2b (drive motor 2c), drum 5, festoon unit 6, and heating mechanism 8 are controlled by the control unit 11. A computer is used for the control unit 11. In addition to the various data described above, data such as the rotation speeds of the screw 2b, drive roller 6a, and drum 5, and the moving speed of the wire Wr penetrating the head 3 are input to the control unit 11.
[0031] Furthermore, the control unit 11 receives an input of a correlation CR between the rubber viscosity index PN of the unvulcanized rubber R that sets the coating thickness h (outer diameter d) to the target value Gh (Gd) and the temperature t of the outer circumferential surface of the wire W at the time of coating the unvulcanized rubber R. The control unit 11 performs various calculations using the input data.
[0032] The present invention was created by focusing on the fact that the viscosity PNa of the unvulcanized rubber R has a large effect on the coating thickness h. In general, when the viscosity PNa is small, the amount of unvulcanized rubber R adhering to the outer peripheral surface of the passing wire W increases, and the coating thickness h increases, whereas when the viscosity PNa is large, the amount of the unvulcanized rubber R adhering to the outer peripheral surface of the passing wire W decreases, and the coating thickness h tends to decrease. Also, the viscosity PNa tends to decrease at high temperatures and increase at low temperatures.
[0033] Therefore, multiple unvulcanized rubbers R with different viscosities are prepared and each is fed into the rubber extruder 2 to manufacture the rubber-coated wire Wr. In this case, only the temperature t of the outer surface of the wire W at the time of coating with the unvulcanized rubber R is substantially different, and the outer diameter d of the manufactured rubber-coated wire Wr is measured. This results in the data shown in Figure 4. Da, Db, and Dc are data on unvulcanized rubbers R with different viscosities P1, P2, and P3, respectively, and are shown as straight lines in Figure 4 for simplicity, but may be curved.
[0034] If the target values of the outer diameter d and the coating thickness h are Gd and Gh, respectively, the appropriate values of the temperature t to reach the target values are determined as ta, tb, and tc from the data Da, Db, and Dc in Figure 4. Note that the target value is set for at least one of the outer diameter d and the coating thickness h.
[0035] 4, it is possible to grasp the correlation CR between the viscosity PNa of the unvulcanized rubber R for making the outer diameter d (coating thickness h) a target value and the temperature t of the outer circumferential surface of the wire W at the time of coating with the unvulcanized rubber R, as shown in Fig. 5. This correlation CR is input and stored in the control unit 11, and is used when manufacturing the rubber-coated wire Wr.
[0036] The rubber viscosity index PN, which is the hardness PNb, the internal pressure PNc, and the driving torque PNd, are closely related to the variation of the viscosity PNa and have a high correlation, so they can be estimated from the viscosity PNa. Therefore, a preliminary test is performed to understand the correlation between the viscosity PNa and the internal pressure PNc, as shown in Fig. 6. The higher the viscosity PNa of the unvulcanized rubber R inside the rubber extruder 2, the higher the internal pressure PNc of the head 3 and the cylinder body 2a tends to be when extruding the unvulcanized rubber R.
[0037] Using the data in Figures 5 and 6, the data in Figure 7 can be obtained by converting the horizontal axis of the data in Figure 5 from viscosity PNa to internal pressure PNc. That is, it is possible to grasp the correlation CR between the internal pressure PNc that sets the outer diameter d (coating thickness h) to a target value and the temperature t of the outer circumferential surface of the wire W at the time of coating with unvulcanized rubber R. The correlation CR illustrated in Figure 7 can be input and stored in the control unit 11 and used when manufacturing the rubber-coated wire Wr.
[0038] Similarly, a preliminary test is performed for hardness PNb, and the correlation between viscosity PNa and hardness PNb is grasped as shown in FIG. 8. The higher the viscosity PNa of the unvulcanized rubber R, the higher the hardness PNb tends to be. Therefore, by using the data in FIG. 5 and FIG. 8 and converting the horizontal axis of the data in FIG. 5 from viscosity PNa to hardness PNb, data similar to that in FIG. 7 can be obtained. That is, the correlation CR between the hardness PNb for which the outer diameter d (coating thickness h) is the target value and the temperature t of the outer circumferential surface of the wire W at the time of coating the unvulcanized rubber R can be grasped. This correlation CR can be input and stored in the control unit 11 and used when manufacturing the rubber-coated wire Wr.
[0039] Similarly, a preliminary test is performed for the driving torque PNd, and the correlation between the viscosity PNa and the driving torque PNd is grasped as shown in FIG. 9. The higher the viscosity PNa of the unvulcanized rubber R inside the rubber extruder 2, the higher the driving torque PNd for extruding the unvulcanized rubber R tends to be. Therefore, by using the data in FIG. 5 and FIG. 9, the horizontal axis of the data in FIG. 5 is converted from the viscosity PNa to the driving torque PNd, and data similar to that in FIG. 7 can be obtained. That is, the correlation CR between the driving torque PNd for making the outer diameter d (coating thickness h) a target value and the temperature t of the outer circumferential surface of the wire W at the time of coating the unvulcanized rubber R can be grasped. This correlation CR can be input and stored in the control unit 11 and used when manufacturing the rubber-coated wire Wr.
[0040] Next, an example of a procedure for manufacturing the rubber-coated wire Wr using the manufacturing apparatus 1 will be described.
[0041] Unvulcanized rubber R is fed into the rubber extruder 2 shown in Fig. 1 and Fig. 2, and the screw 2b is rotated by the drive motor 2c to extrude the unvulcanized rubber R fed into the cylinder body 2a into the head 3. For the unvulcanized rubber R, a correlation CR between the rubber viscosity index PN that sets the coating thickness h for the wire W to the target value Gh (in other words, the outer diameter d of the rubber-coated wire Wr to the target value Gd) and the temperature t of the outer circumferential surface of the wire W at the time of coating with the unvulcanized rubber R is obtained in advance and inputted to the control unit 11. The tip portion of the wire W is passed through the head 3 via the wire inlet 3a and the wire outlet 3b, and is wound around the festoon section 6 and the drum 5.
[0042] By driving the drive roller 6a and the drum 5 to rotate, the wire W is unwound from the reel 4 and passes through the unvulcanized rubber R filled inside the head 3. When the wire W passes through the heating mechanism 8, the outer circumferential surface of the wire W is heated by the heating mechanism 8, and the wire W in the heated state enters the inside of the head 3. Since the unvulcanized rubber R adheres to the outer circumferential surface of the wire W when passing through the unvulcanized rubber R, the outer circumferential surface of the wire W that has passed through the head 3 is covered with the unvulcanized rubber R, and a rubber-coated wire Wr is produced. The produced rubber-coated wire Wr passes through the outer diameter sensor 10 and the festoon section 6 in this order, and is moved to the drum 5 and wound up. It is desirable to keep the moving speed of the wire W (rubber-coated wire Wr) substantially constant.
[0043] In this embodiment, the viscosity PNa of the unvulcanized rubber R is grasped by a rubber viscometer 7a before it is fed into the rubber extruder 2, and the data of the viscosity PNa is input to the control unit 11. Then, the control unit 11 calculates an optimum value Gt of the temperature t of the outer circumferential surface of the wire W that makes the coating thickness h a target value Gh, based on the correlation CR illustrated in Fig. 5 and the input data of the viscosity PNa. The optimum value Gt is, for example, about 50°C to 100°C.
[0044] Then, the control unit 11 controls the heating temperature by the heating mechanism 8 to adjust the temperature t of the outer peripheral surface of the wire Wr at the time of covering the unvulcanized rubber R to the calculated optimum value Gt. When the distance between the heating mechanism 8 and the head 3 is large, the temperature t of the outer peripheral surface of the wire W changes while moving from the heating mechanism 8 to the head 3. Therefore, the change in temperature t while moving from the heating mechanism 8 to the head 3 is anticipated in advance, and the heating mechanism 8 heats the wire W taking into account this change in temperature t. For example, under conditions in which the temperature t drops by 2°C while moving from the heating mechanism 8 to the head 3, the heating mechanism 8 heats the temperature t of the outer peripheral surface of the wire W to the optimum value Gt+2°C. This allows the temperature t of the outer peripheral surface when the wire W enters the head 3 to be the optimum value Gt.
[0045] Near the wire inlet 3a, a temperature sensor 9 detects the temperature t of the outer circumferential surface of the wire W immediately before it enters the head 3, and the temperature data is sequentially input to the control unit 11. Based on this input temperature data, the control unit 11 checks whether the temperature t of the outer circumferential surface of the wire W at the time when the wire W enters the head 3, i.e., when it coats the unvulcanized rubber R, is an appropriate value Gt. If the detected temperature data deviates from the appropriate value Gt beyond an allowable range, the control unit 11 adjusts the heating temperature by the heating mechanism 8 based on the difference between this temperature data and the appropriate value Gt, so that the temperature data detected by the temperature sensor 9 approaches the appropriate value Gt.
[0046] As a result, the wire W, with the temperature t of the outer circumferential surface adjusted to the appropriate value Gt, is continuously passed through the unvulcanized rubber R extruded from the rubber extruder 2. In this way, the rubber-coated wire Wr is continuously produced.
[0047] When the internal pressure PNc is used as the rubber viscosity index PN, the internal pressure PNc is grasped by the pressure sensor 7b while the wire W is passing through the head 3 from the reel 4 to produce the rubber-coated wire Wr. The grasped data of the internal pressure PNc is input to the control unit 11. The control unit 11 calculates an appropriate value Gt of the temperature t of the outer circumferential surface of the wire W that makes the coating thickness h a target value Gh, based on the correlation CR illustrated in Fig. 7 and the grasped data of the rubber internal pressure PNc. Thereafter, the heating temperature of the wire W is controlled by the heating mechanism 8, and the procedure for producing the rubber-coated wire Wr is as described above.
[0048] When hardness PNb and driving torque PNd are adopted as the rubber viscosity index PN, the data are obtained using the corresponding data acquisition units as described above. The control unit 11 calculates the appropriate value Gt of the temperature t of the outer circumferential surface of the wire W that makes the coating thickness h the target value Gh, based on the correlation CR illustrated in Fig. 7 and the data of the rubber internal pressure PNc obtained. Thereafter, the heating mechanism 8 controls the heating temperature for the wire W, and the procedure for manufacturing the rubber-coated wire Wr is as described above.
[0049] In this way, the present invention utilizes two items, the rubber viscosity index PN and the temperature t of the outer peripheral surface of the wire W at the time of coating the unvulcanized rubber R. In other words, by using the correlation CR between the two items that have a large influence on the coating thickness h, the temperature t of the outer peripheral surface of the wire W at the time of coating the unvulcanized rubber R can be accurately adjusted to the appropriate value Gt. Then, the outer peripheral surface of the wire W is heated to the appropriate value Gt and the wire W is continuously passed through the unvulcanized rubber R, so that it becomes possible to appropriately adjust the coating thickness h over the entire length of the wire W.
[0050] As a result, it becomes possible to more stably set the coating thickness h (outer diameter d of the rubber-coated wire Wr) to the target value Gh. That is, by adjusting only the temperature t of the outer peripheral surface of the wire W among the manufacturing conditions, the fluctuation of the outer diameter d (coating thickness h) in the manufacturing process of the rubber-coated wire Wr can be made smaller than that of the conventional method, as illustrated in FIG. 10. In addition, the initial period TF from time T1 when the manufacturing process of the rubber-coated wire Wr is started or when the lot of the unvulcanized rubber R is changed to time T2 when the fluctuation of the outer diameter d (coating thickness h) becomes small can be made shorter than that of the conventional method. Therefore, the stable period TS during which the outer diameter d (coating thickness h) is maintained within the allowable range AW of the target value Gd (Gh) arrives earlier, and a high-quality rubber-coated wire Wr can be stably manufactured. The occurrence of defective products such as defective coating of the unvulcanized rubber R is suppressed, which also contributes to improving productivity.
[0051] In this embodiment, the festoon unit 6 retains the rubber-coated wire Wr according to the winding speed of the rubber-coated wire W by the drum 5, so that the wire W unwound from the reel 4 can be kept moving and the production of the rubber-coated wire Wr can be continued without interruption. Therefore, the extrusion of the unvulcanized rubber R by the rubber extruder 2 is not interrupted, and the unvulcanized rubber R can be extruded into the head 3 under basically constant extrusion conditions. When the extrusion conditions change, the physical properties of the extruded unvulcanized rubber R vary, but in this embodiment, the unvulcanized rubber R can be continued to be extruded without changing the extrusion conditions, which is advantageous for producing a rubber-coated wire Wr of stable quality.
[0052] The above-mentioned procedure for manufacturing the rubber-coated wire Wr may be performed all the time, but may also be performed, for example, only during the initial period TF. That is, after a stable period TS during which the coating thickness h (outer diameter d) shown in Fig. 10 is maintained at the target value Gh (Gd) for a predetermined period of time has elapsed, the rubber-coated wire Wr may be manufactured by a different procedure. The stable period TS may be set to an appropriate time in advance by performing a preliminary test or the like.
[0053] This alternative procedure will be described. As illustrated in Fig. 10, from time T3 when a stable period TS during which the coating thickness h is maintained within the allowable range AW of the target value Gh for a predetermined period has elapsed, an outer diameter sensor 10 is used instead of the data acquisition unit. The outer diameter sensor 10 detects the outer diameter of the rubber-coated wire Wr immediately after the wire W passes through the unvulcanized rubber R filled inside the head 3. A target value Gd of the outer diameter d corresponding to the target value Gh of the coating thickness h is input to the control unit 11.
[0054] The outer diameter sensor 10 detects the outer diameter d of the passing rubber-coated wire Wr, and the detected data of the outer diameter d is sequentially input to the control unit 11. The control unit 11 compares the data of the outer diameter d detected by the outer diameter sensor 10 with a target value Gd. Based on the comparison result, the heating temperature of the wire W by the heating mechanism 8 is adjusted.
[0055] 4, the correlation between the temperature t of the outer peripheral surface of the wire W and the outer diameter d is grasped. Based on this correlation and the data of the outer diameter d detected by the outer diameter sensor 10, the heating mechanism 8 is controlled to adjust the temperature t of the outer peripheral surface of the wire W at the time of coating with the unvulcanized rubber R. In this manner, the heating temperature of the wire W by the heating mechanism 8 is controlled so that the data of the outer diameter d detected by the outer diameter sensor 10 approaches the target value Gd, thereby manufacturing the rubber-coated wire Wr. [Explanation of symbols]
[0056] 1. Rubber-coated wire manufacturing equipment 2. Rubber extruder 2a Cylinder body 2b Screw 2c Drive motor 3 Head 3a Wire inlet 3b Wire Exit 4 Reels 5 Drum (wire moving mechanism) 5a Flange part 6 Festoon Club 6a Drive roller (wire moving mechanism) 6b Support roller 7a Rubber viscometer (data acquisition section) 7b Pressure sensor (data acquisition part) 8 Warming mechanism 9 Temperature Sensor 10 Outer diameter sensor 11 Control section W Wire Wr Rubber-coated wire R Unvulcanized rubber
Claims
1. A method for producing a rubber-coated wire, comprising the steps of: continuously passing a wire through unvulcanized rubber extruded from a rubber extruder to coat an outer peripheral surface of the wire with the unvulcanized rubber, the method comprising the steps of: A method for manufacturing a rubber-coated wire, comprising: determining in advance the correlation between a rubber viscosity index and the temperature of the outer surface of the wire at the time the unvulcanized rubber is coated as a correlation for setting the coating thickness on the wire to a target value for the unvulcanized rubber; and inputting the correlation between the rubber viscosity index and the temperature of the outer surface of the wire at the time the unvulcanized rubber is coated into a control unit; calculating an appropriate value for the temperature of the outer surface of the wire that will set the coating thickness to the target value based on the correlation and the rubber viscosity index determined before the outer surface of the wire is coated with the unvulcanized rubber; and continuously passing the wire through the unvulcanized rubber extruded from the rubber extruder while adjusting the temperature of the outer surface of the wire at the time the unvulcanized rubber is coated to the calculated appropriate value using a heating mechanism.
2. 2. The method for manufacturing a rubber-coated wire according to claim 1, wherein at least one of the viscosity and hardness of the unvulcanized rubber, the internal pressure of the rubber extruder, and the torque required to drive a screw of the rubber extruder is used as the rubber viscosity index.
3. 3. A method for manufacturing a rubber-coated wire as described in claim 1 or 2, wherein after a stable period during which the coating thickness is maintained within an acceptable range of the target value for a predetermined time has elapsed, an outer diameter of the rubber-coated wire is detected by an outer diameter sensor immediately after passing through the unvulcanized rubber, a target value of the outer diameter of the rubber-coated wire corresponding to the target value is compared by the control unit with the outer diameter data detected by the outer diameter sensor, and based on the comparison result, the control unit controls the heating mechanism to adjust the temperature of the outer surface of the wire at the time of coating the unvulcanized rubber, thereby controlling the outer diameter data detected by the outer diameter sensor to approach the target value of the outer diameter.
4. A rubber-coated wire manufacturing apparatus includes a rubber extruder and a wire moving mechanism for passing a wire through unvulcanized rubber extruded from the rubber extruder, and the unvulcanized rubber is coated on an outer peripheral surface of the wire after the wire has passed through the unvulcanized rubber, a control unit to which a previously determined correlation between a rubber viscosity index and the temperature of the outer peripheral surface of the wire at the time of coating the unvulcanized rubber is input as a correlation for setting a coating thickness for the unvulcanized rubber to a target value; a data acquisition unit to acquire the rubber viscosity index before coating the outer peripheral surface of the wire with the unvulcanized rubber; and a heating mechanism to adjust the temperature of the outer peripheral surface of the wire at the time of coating the unvulcanized rubber, Based on the correlation and the rubber viscosity index acquired by the data acquisition unit, the control unit calculates an appropriate temperature value of the outer surface of the wire that will make the coating thickness the target value, and the control unit controls a heating mechanism to adjust the temperature of the outer surface of the wire to the calculated appropriate value at the time when the unvulcanized rubber is coated, and the wire is passed through the unvulcanized rubber extruded from the rubber extruder.
Citation Information
Patent Citations
Cable extruding covering device
JP1994231634A
Method of and device for forming bead using bead wire in one bundle
JP2004345312A
Method and apparatus for controlling rubber coating diameter of bead wire
JP2005138467A
Apparatus for coating cord with rubber and method for producing rubber-coated cord
JP2007152647A