Method for Producing Nanofiber Filter Laminates

A novel spinning method for nanofiber laminates using a polymeric material with carbon black particles, supported by nonwoven fabric, addresses the challenges of high voltage risks and cost in electrospinning, achieving efficient and safe filtration with low air resistance.

JP7590718B2Active Publication Date: 2024-11-27TAMARU SEISAKUSHO +3
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021006012
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-18
Publication Date
2024-11-27
Estimated Expiration
2041-01-18

AI Technical Summary

Technical Problem

Conventional nanofiber production methods, particularly electrospinning, require high voltages, are dangerous, difficult to handle, and increase production costs, and the use of carbon black fine particles in spinning solutions leads to conductive nanofibers, reducing ventilation efficiency and increasing costs.

Method used

A spinning method using a polymeric material with a long molecular arrangement, mixed with carbon black fine particles, is spun from a nozzle with a ring-shaped high-speed outlet to vaporize the solvent, and the nanofiber laminate is washed with water or alcohol to remove excess particles, supported by nonwoven fabric or mesh, and integrated into masks or filters.

Benefits of technology

The method produces nanofiber laminates with high collection efficiency, low air pressure loss, and sufficient air permeability, suitable for masks and filters, maintaining breathability and safety while being cost-effective and durable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590718000001
    Figure 0007590718000001
  • Figure 0007590718000002
    Figure 0007590718000002
  • Figure 0007590718000003
    Figure 0007590718000003
Patent Text Reader

Abstract

To provide a nanofiber filter laminate having excellent collection efficiency of floating fine particles, viruses and the like, being safe, having excellent air permeability and being no stifling and to provide a mask using the same.SOLUTION: In a nanofiber filter laminate and a mask using the same,: a polymer material having a long molecular arrangement is dissolved in dissolving liquid; nanofiber spinning liquid is made by mixing carbon black fine particles in the dissolving liquid; spinning from a spinning nozzle is performed by pressing the spinning liquid; a ring-shaped high speed blowing port coaxial with a center discharge port is disposed so as to surround the center discharge port of the spinning nozzle; the polymer material is stretched from the spinning nozzle by an air flow from the high speed blowing port; and the produced nanofiber laminate is washed with water, methanol or isopropyl alcohol for determined time.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention provides a nanofiber filter laminate, a mask using the laminate that is capable of collecting airborne pollen, dust such as fine particulate matter PM2.5, and viruses, and a mask using the same. More specifically, the present invention relates to a mask using the nanofiber filter laminate, which is produced by dissolving a polymer material having a long molecular arrangement in a solvent, mixing carbon black particles or manganese oxide particles into the solvent to produce a nanofiber spinning solution, and using the spinning solution to produce a nanofiber filter laminate. [Background technology]

[0002] Recently, nanofibers, generally defined as fibers with a diameter of 1 micron (=1,000 nm) or less, have been developed, and the technique known as ESD (Electro-Spray Deposition) or electrospinning has attracted the most attention as a method for producing nanofibers, and this technique has been developed (see, for example, Patent Document 1). However, the electrospinning method requires a high voltage of 10 kV, and therefore the use of conductive polymer materials such as polyvinyl alcohol (PVA) is dangerous and difficult to handle. In addition, the carbon particles used are effective in adsorbing and removing airborne particles and electrostatically adding them to the polymer melt, but when mixing the carbon particles into the melt and spinning it, it is difficult to spin nanofibers using the ESD method, which requires high voltage, because the carbon black particles are electrically conductive.

[0003] Incidentally, as a method for producing conventional synthetic fibers of the micro order that do not use high-voltage electrodes, in addition to the electrospinning method mentioned above, non-patent document 1 discloses that currently, in addition to the electrospinning method mentioned above, the sea-island composite spinning method, the melt-blow spinning method in which a low-viscosity dissolved polymer is blown away, and the flash spinning method in which a polymer solution is suddenly expanded and solidified and turned into fiber while blowing away the polymer, have been developed. As a method for producing ultrafine fibers using only dissolution, non-patent document 1 discloses a polymer blend spinning method in which two types of polymers are blended, which is turned into fiber, and then the sea polymer is dissolved out, but the limit of the fiber thickness is said to be on the order of μm. Therefore, the inventors have succeeded in producing nanofibers by dissolving a polymer in a solvent to reduce viscosity, and then blowing it out of a very fine nozzle together with jet air to stretch it, as shown in Patent Documents 2 and 3. Using this, they are producing thin-film deodorizing and shielding members that capture fine particulate matter PM2.5 suspended in the air, which deposits in the respiratory system and has an adverse effect on health. It has been found that the material in Patent Document 2 can capture droplets of viruses and the like in addition to capturing fine particulate matter PM2.5.

[0004] Incidentally, Patent Document 4 provides a nonwoven fabric substrate for air filters or masks that uses a nanofiber laminate that captures fine dust while maintaining breathability with low pressure loss. However, the nonwoven fabric substrate for air filters or masks in Patent Document 3 has the above-mentioned inconvenient problems because a nanofiber spinning device using an electrospinning method is used for conventional nanofiber production. Furthermore, since the nonwoven fabric is laminated by spraying a fibrous or powdery adhesive on the nonwoven fabric surface, these adhesives fill the gaps formed by the nanofibers for ventilation, thereby reducing the efficiency of ventilation. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-127234 A [Patent Document 2] JP 2014-144579 A [Patent Document 3] JP 2019-37963 A [Patent Document 4] JP 2014-114521 A

[0006] [Non-Patent Document 1] SEN'I GAKKAISHI (Textiles and Industry) Vol.63, No.12 (2007) 423-425P [Development of melt-spun nanofibers] Takashi Ochi Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, Patent Documents 1 and 4 disclose nanofibers produced by the conventional electrospinning method, which requires high voltage and is therefore dangerous. In particular, when producing a nanofiber laminate from a spinning solution in which carbon black fine particles are mixed with a water-soluble polymer material as in the present invention, there are problems in that the handling is difficult and the production costs are high, and there are problems with using conductive carbon black fine powder in the spinning solution. The present invention has been made in view of the above problems, and provides a nanofiber filter laminate for collecting fine particles suspended in the air. How to produce and a mask using the same. Furthermore, nanofiber filters Method for producing a laminate The nanofiber filter laminate is used as a filter for a general mask, a medical mask, an industrial dust mask, etc., and has a high collection efficiency, is safe, has good air permeability, and is not stuffy. How to produce , and masks using it How to produce It is what we intend to provide. [Means for solving the problem]

[0008] In order to solve the above problems, a polymer material having a long molecular arrangement is dissolved in a solvent, Add carbon black particles with a diameter of 24 nm or less to the solution. The spinning solution is pressurized and spun from a spinning nozzle, and a ring-shaped high-speed blowing outlet is provided coaxially with a central outlet of the spinning nozzle so as to surround the central outlet of the spinning nozzle, and the polymer material from the spinning nozzle is stretched by an airflow from the high-speed blowing outlet while the solvent is vaporized to form a nanofiber laminate, The nanofiber laminate is washed with water, methanol, or isopropyl alcohol to remove excess carbon black particles. Nanofiber filter laminate It is a method of producing . The polymer material having the long molecular sequence is a nanofiber filter laminate made of polyvinylidene fluoride (PVDF) and a solvent selected from N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), dimethylacetamide (DMAC), and dimethylsulfoxide (DMSO). It is a method of production. Furthermore, a deodorant attachment step is provided for attaching a deodorant to an appropriate portion of the nanofiber laminate formed. It is a method of production. In addition, the nanofiber filter laminate How to produce masks for daily use, medical use, and industrial dust masks How to produce A nanofiber filter laminate in which both sides of the nanofiber laminate are supported by a nonwoven fabric, a cloth, or a plain weave mesh net. It is a method for producing The method for producing a nanofiber filter laminate of the present invention and a mask using the same comprise dissolving a polymeric material having a long molecular arrangement in a solvent, pressurizing a spinning solution in which carbon black fine particles are mixed into the solvent to spin the solution from a spinning nozzle, providing a ring-shaped high-speed blowing outlet coaxially with the central outlet of the spinning nozzle so as to surround the central outlet, and stretching the polymeric material from the spinning nozzle with an airflow from the high-speed blowing outlet while vaporizing the solvent. How to produce the body The laminate is washed with water, methanol or isopropyl alcohol for a predetermined time, and the laminate is supported by a nonwoven fabric, a cloth, a mesh made of plain woven monofilaments, or the like to form a nanofiber filter laminate. How to produce and a mask using the same. The polymeric material as the spinning solution is preferably a polymeric material selected from polyvinylidene fluoride (PVDF), polyvinyl butyral (PVB), polyvinyl alcohol (PVA), polyurethane (PU), polyamide (registered trademark; nylon), etc., and the nanofiber laminate produced in Example 1 can be used as building materials such as screen doors, ventilation fans, ventilation windows for agricultural greenhouses, etc. by disposing a separate nonwoven fabric on the edge. When used as a mask, nonwoven fabric is disposed on both sides of the front and back ends of the nanofiber laminate, and the thickness of the nonwoven fabric is selected from polyethylene nonwoven fabric, polypropylene nonwoven fabric, and nylon nonwoven fabric, and the thickness of the nonwoven fabric is 0.1 to 0.7 mm and the basis weight is 10 g to 60 g / m. 2 The nanofiber filter laminate is excellent and is ideal for use as a mask for general daily life, a medical mask, and an industrial dust mask. Furthermore, by using a plain-woven monofilament mesh as the surface substrate as in Example 2 and spraying nanofibers onto it, it is possible to easily produce a mask that can maintain its three-dimensional shape without the need for reinforcing nonwoven fabric as in Example 1.

[0009] In addition, the nanofiber filter laminate is manufactured using a spinning method using high-speed jetting, not an electrospinning method, and therefore, in Example 1, an endless circulating collection substrate is formed by plain weaving monofilaments without knots of polymer material to form a coarse mesh, a polymer material having a long molecular arrangement is dissolved in a solvent and pressurized to be spun from a spinning nozzle toward the collection substrate, a ring-shaped high-speed blowing outlet is provided coaxially with the central outlet of the spinning nozzle so as to surround the central outlet of the spinning nozzle, the polymer material from the spinning nozzle is stretched by the airflow from the high-speed blowing outlet, and the solvent is vaporized to stack and collect the nanofiber-like fibers on the collection substrate, and the nanofiber layer attached to the collection substrate is simply peeled off and wound up. Furthermore, in the manufacturing process of the nanofiber laminate of Examples 1 and 2, it is preferable to wash off excess carbon black fine particles and the like with water, methanol, or isopropyl alcohol. Effect of the Invention

[0010] Nanofiber filter laminate of the present invention A method for producing A mask using the laminate, particularly when used as a mask filter substrate, has the characteristic of having low air loss and no breathlessness despite its high collection efficiency. In particular, if a monofilament mesh material is used as the surface substrate to reinforce the nanofiber filter, for example, if a polypropylene monofilament material of about 20 mesh is used to support the nanofiber filter laminate of the mask, the spatial shape of the three-dimensional mask can be firmly maintained. In addition, in the manufacturing process, the nanofiber layer of Examples 1 and 2 can be easily made thicker as needed. By making the nanofiber layer thicker and particularly increasing the collection efficiency, droplets of fine particulate matter PM2.5, viruses, and the like can be collected, and the nanofiber layer can be used as an industrial filter for window screens, ventilation fans, and the like. Furthermore, since the spinning solution is sprayed from a nozzle of a nanofiber spray in the manufacturing process, carbon black fine particles can be mixed into the spinning solution, and if the nozzle is made of stainless steel or ceramic, the central outlet is heat-resistant and durable with little deformation, and even if the polymer fiber heated to a high temperature is spun for a long time, the nanofiber does not deform and a uniform nanofiber diameter can be maintained. Furthermore, the nanofiber layer has sufficient breathability and strength, and can be mass-produced at low cost. Furthermore, the nanofiber filter laminate for masks produced by the present invention can be safely produced as a nanofiber laminate made of polymeric materials with long molecular arrangements, such as polyvinylidene fluoride (PVDF), polyvinyl butyral (PVB), polyvinyl alcohol (PVA), polyurethane (PU), and polyamide (registered trademark; nylon). In particular, when the nanofiber material is polyvinylidene fluoride (PVDF), it is a resin that has excellent weather resistance and is resistant to radiation, and is therefore suitable as a filter for screen doors and ventilation fans that come into contact with the outdoors, as well as for agricultural greenhouses, and is easy to clean. Furthermore, by attaching a deodorant to a mask, etc., a deodorizing effect can be obtained and a sterilizing effect against bacteria, etc. can also be expected. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is an explanatory diagram showing an entire apparatus for producing a nanofiber laminate according to Example 1; [Diagram 2] FIG. 2 is an explanatory diagram showing an entire apparatus for forming the nanofiber laminate in FIG. 1 into a nanofiber filter; [Diagram 3] FIG. 2 is an enlarged front view of a pair of heat-pressure fusing rollers; [Figure 4] FIG. 2 is a schematic diagram of the nanofiber production section in FIG. [Diagram 5] FIG. 5 is an enlarged view of the nozzle of FIG. 4 and the air jet nozzle at its tip; [Figure 6] FIG. 6(a) is a side view of the polymer supply pipe of FIG. 2, FIG. 6(b) is a cross-sectional view thereof, [Figure 7] A plan view of the mask for Example 1, which was created by processing the final product. [Figure 8] A diagram of an example of inserting a filter into the mask of Example 2, which was created by processing the final product. [Figure 9] FIG. 1 is a perspective view of a first example of wearing a mask; [Figure 10] FIG. 10(a) is an electron microscope photograph at 200x magnification of the polyvinylidene fluoride (PVDF) of Example 1 mixed with carbon black particles having a diameter of 24 nm, and FIG. 10(b) is an electron microscope photograph at 1000x magnification of the same. [Figure 11] Figure 11(a) is an electron microscope photograph at 200x magnification of the carbon black-containing polyvinylidene fluoride (PVDF) nanofibers shown in Figure 10 after washing in a methanol washing bath for 5 minutes, and Figure 11(b) is an electron microscope photograph at 1000x magnification. [Figure 12] FIG. 1 is an explanatory diagram showing an entire apparatus for producing a nanofiber laminate according to Example 2; [Figure 13] FIG. 13 is an explanatory diagram showing the whole of an apparatus for forming the nanofiber laminate in FIG. 12 into a nanofiber filter; [Figure 14] FIG. 13 is a schematic explanatory diagram of the spraying portion of the first and second polymer adhesives in FIG. 12; [Figure 15] FIG. 15 is an enlarged cross-sectional view of the nozzle of FIG. 14 and the jet air blowing nozzle at its tip; [Figure 16] 13 is an enlarged cross-sectional view of the first polymer adhesive spraying section and the cooling device in FIG. 12; [Figure 17] FIG. 16 is an explanatory diagram of the Peltier device; [Figure 18] 1 is a cross-sectional view of the nanofiber filter laminate of Example 2; [Figure 19] FIG. 3 is a perspective view of a mask according to Example 3, which is produced by processing the final product according to Example 2; [Figure 20] 1 is an electron microscope photograph at 200x magnification showing a state in which the first and second polymer adhesives are entangled in a fibrous form on a surface substrate J1 of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Example 1 The overall configuration of Example 1 of the present invention is roughly as shown in Figure 1. First, from the left of the drawing, there is a nanofiber production process A in which nanofibers are produced. This nanofiber production process A is composed of a material liquid supply section 1, a spinning section 2, and a spraying section 3. Nanofiber spinning liquid N1 is stored in the material liquid supply section 1, and nanofiber fibers N2 are produced in the spinning section 2 and spraying section 3. Next, there is a capture layer formation process B which receives the sprayed nanofiber fibers N2 and laminates them as a nanofiber laminate N3, and this capture layer formation process B is composed of a collection section 3. Next, in a laminate removal process C, the collected nanofiber laminate N3 is peeled off from the collection zone 31 of the collection section 3. This laminate removal process C consists of an upper air blowing device 381 and a lower air suction device 382 of the laminate removal section 38, and the nanofiber laminate N3 adsorbed to the collection zone 31 is removed from the collection zone 31 by air blown from the blowing nozzle 3811 of the upper air blowing device 381 and the suction nozzle 3821 of the lower air suction device 382. The detached nanofiber laminate N3 is compressed at one end by a pair of pinch rollers 41 to form a nanofiber laminate N4, which is then washed in methanol (Example 1) (or isopropyl alcohol) in a cleaning device 4 and washed for a predetermined period of time by a group of rollers 44 (Example 1) (or a group of rollers that reciprocate up and down) moving back and forth from side to side.Then, the nanofiber laminate N5 is passed through a guide roller 45 and a pinch roller 46 and wound up by a winding device 5 as the intermediate product nanofiber laminate N5.

[0013] The lot 5A of the laminate N5 wound up as the intermediate product nanofiber laminate N5 illustrates the manufacturing apparatus for the nanofiber filter laminate N6 shown in Figs. In Fig. 2, the nanofiber laminate N5 lot 5A, which is an intermediate product of the winding device 5 in Fig. 1, is set in the supply device 61 in Fig. 2, and a thin net or a thin microfiber nonwoven fabric is supplied to the upper and lower surfaces of the nanofiber laminate N5 of the lot 51 (5A) set in this supply device 61 by supply devices 71, 72, and the upper and lower surfaces of the nanofiber laminate N5 are sandwiched by a pair of feed rollers 73, and then, a predetermined portion of the nanofiber laminate N5 is heat-welded by a pair of heating and pressing rollers 74 shown in Fig. 3 to form a semi-finished nanofiber filter laminate N6, and the resulting nanofiber filter laminate N6 is wound on the winding device 8 to form a lot 81 (8A). Thereafter, the semi-finished nanofiber filter laminate N6 is cut as necessary and processed into a mask or the like.

[0014] [Material liquid supply section 1] Next, each of the above-mentioned processing steps will be described in detail. First, the raw material used in Example 1 was polyvinylidene fluoride (PVDF), In addition to polyvinylidene fluoride (PVDF), polymer materials such as polyvinyl alcohol (PVA) and polyvinyl butyral (PVB) may also be used.

[0015] [Nanofiber production process A] Each of the above steps will be described in detail below. First, the nanofiber production process A is composed of a material liquid supply section 1, a spinning section 2, and a spraying section 3. The following will explain the details in this order. [Material liquid supply section 1] In Fig. 1, on the left side are the material liquid supply section 1 and the spinning section 2, and Fig. 4 is an enlarged view of these, and as shown in the figure, a plurality of spinning nozzles 22 are provided, and in Example 1, polyvinylidene fluoride (PVDF) spinning solution N1 is charged into the material liquid tank 11. The composition of the polyvinylidene fluoride (PVDF) spinning solution N1 used in Example 1 is as follows. Example 1 [Table 1] Composition of polyvinylidene fluoride (PVDF) spinning solution N1 Polyvinylidene fluoride (PVDF) 13.00% by weight N-Methyl-2-pyrrolidone (NMP) 85.15% by weight Toluene: 1.00% by weight. Carbon black particles: 0.85% by weight Total...100.00% by weight

[0016] In this embodiment, PVDF is first dissolved in N-methyl-2-pyrrolidone (NMP) in order to stretch it. As described above, 85.15% by weight of N-methyl-2-pyrrolidone (NMP) is mixed with 13.00% by weight of PVDF pellets to create a solution, but if there is too much N-methyl-2-pyrrolidone (NMP) than this value, nanofibers are not formed, and if the concentration of polyvinylidene fluoride (PVDF) is too high, thick fibers are not formed, or the nozzle is clogged, which are problems that occur. In addition, in order to improve the performance of capturing suspended fine particles, carbon black fine particles (manufactured by Mitsubishi Chemical Corporation) having a diameter of 30 nm or less (24 nm in this Example 1) are mixed into the solution and nanofibers are spun. The diameter must be smaller than the inner diameter of the smallest central axial hole 2211 of the blowout port 2212 of the nozzle part 2 in FIG. 5, which is 0.13 mm, and in this Example, carbon black fine particles having a particle diameter of 20 nm, MA110, manufactured by Mitsubishi Chemical Corporation, were used. As will be described later, the completed polyvinylidene fluoride (PVDF) nanofiber laminate is washed in isopropyl alcohol for a predetermined time of 40 to 70 minutes to be finished as a nanofiber filter for capturing fine particles. Note that N,N-dimethylformamide (DMF), dimethylacetamide (DMAC), and dimethylsulfoxide (DMSO) may be used as a solvent instead of N-methyl-2-pyrrolidone (NMP). It is also possible to manufacture nanofibers using a melting method instead of a dissolution method. In this case, polypropylene (PP) can be used as the base material, and nanofibers that melt at high heat are also used. Although details are not mentioned in this specification, a nanofiber manufacturing device developed by the present inventors that melts polypropylene (PP) at high heat can be used.

[0017] Such polyvinylidene fluoride (PVDF) is dissolved in N-methyl-2-pyrrolidone (NMP) and carbon black particles are mixed into the spinning solution N1, which is supplied from the material solution tank 11 to the spinning section 2 via the feed pump 12 and the transfer pipe 13 in this order. Hot water from the hot water insulation section 14 is supplied to this transfer pipe 13 through a hot water distributor 141 provided on each transfer pipe 13, and this hot water distributor 141 is configured to maintain the spinning solution N1, in which the nanofiber material (polyvinylidene fluoride (PVDF)) in the nozzle section 22 is dissolved in N-methyl-2-pyrrolidone (NMP), at 40°C to 60°C, so that each nozzle section 22 also maintains a predetermined temperature. This arrangement is as shown in Figure 4, and the water is circulated so as to return to the hot water return port 146 by connecting in series with piping 145 from the hot water outlet 144. The reason why the nanofiber spinning solution N1 in each transfer pipe 13 is heated to about 40° C. to 60° C. by this distributor 141 is that room temperature of 40° C. to 60° C. is the appropriate temperature for stretching polyvinylidene fluoride (PVDF). In this embodiment, the hot water insulation unit 14 stores the hot water required for each distributor 141 at about 40°C to 60°C from the water heater 142, and supplies and circulates the hot water to each distributor 141 by the pump 143, so that the nanofiber spinning solution N1 to be supplied to each spinning unit 2 is also heated to a predetermined temperature of about 40°C to 60°C. The reason why hot water is used to maintain the temperature is that, unlike a heater, the temperature can be relatively easily controlled and the spatial environment does not become dry.

[0018] [Spinning section 2, spraying section 3] Next, the spinning section 2 and the spraying section 3 to which the nanofiber spinning solution N1 is sent from the transfer pipe 13 will be described. The spinning section 2 is as shown in Figures 4 to 6. The spinning section 2 dissolves polyvinylidene fluoride (PVDF) in N-methyl-2-pyrrolidone (NMP), mixes carbon black particles, and blows and stretches the solution from the nozzle section 22 of the nanofiber spraying section 21 to the outside. As shown in the partially enlarged view of Figure 4, the transfer pipe 13 of the material liquid supply section 1 is first connected to the polymer supply pipe 241 of the polymer supply section 24 of the nozzle section 22. As shown in Figure 4, the through hole 234 provided at the center of the polymer supply pipe 241 communicates with the nozzle body 221 of the nozzle section 22, and the nanofiber fiber N2 is sprayed from its tip. The nozzle section 22 is made of ceramic, and in particular, the nozzle body 221 made of ruby ​​has a central axial hole 2211 at its center that continues to the discharge port 2212 at the tip. 1, six rows of nozzle section 22 groups are provided in the vertical direction, and six rows of nozzle section 22 groups (per row) are provided in the horizontal direction, for a total of 36 nozzle sections 22. The six nozzle sections 22 in the horizontal direction of each row are fixed to a horizontal bar or the like at 15 cm intervals, and the nozzle sections 22 and the material liquid supply section 1 operate as a single unit to move horizontally left and right by about 15 cm in the width direction. Therefore, the completed nanofiber fibers N2 are distributed left and right with a width of 90 cm to form a nanofiber laminate N3. In each group of nozzles 22 arranged in the vertical direction, the positions of adjacent nozzle sections 22 in the vertical direction are staggered so that the seams of the nanofiber laminate N2 do not overlap, thereby ensuring that the thickness of the nanofiber laminate N is uniform.

[0019] In addition, the distance from the nozzle portion 22 to the collection zone 31 of the laminate collection section 3 is set to approximately 165 cm, which is a distance that allows the polymer material polyvinylidene fluoride (PVDF) to be sufficiently stretched and the solvent to be sufficiently vaporized so that the solvent is scattered from the nozzle portion 22 toward the laminate collection section 3. In addition, the inner diameter of the discharge port 2212 is set to 0.1 mm to 0.2 mm, and in this embodiment it is set to 0.15 mm. If it is more than 0.2 mm, it is difficult to obtain nano-order thinness even when stretched, and although it is better to make it thinner, if it is less than 0.1 mm, it will become clogged and the spinning speed will slow down.

[0020] [High-speed wind outlet 26] As shown in FIG. 5, the high-speed air blowing nozzle section 261 of the high-speed air blowing section 26 has a nozzle body 221 in which a ring-shaped high-speed air blowing passage 262 is formed coaxially around the central axial hole 2211 so as to surround the central axial hole 2211, and a ring-shaped high-speed air blowing outlet 263 having a predetermined blowing angle is provided at the tip of the high-speed air blowing passage 262, and this high-speed air blowing outlet 263 protrudes slightly from the blowing outlet 263 by about X=5 mm (5 to 7 mm) to generate straightening of the air flow and to promote evaporation of the contained moisture, and the aperture of the high-speed air blowing outlet 263 is somewhat wider than conventional. An air supply section 28 communicating with the other end of the high-speed air outlet passage 262 is provided in the middle of the nanofiber blowing section 21, and air (airflow) at room temperature of 20°C or slightly warmer temperature of about 20-40°C is supplied to this air supply section 28 by an air pump 281, and the polyvinylidene fluoride (PVDF) nanofiber fibers spun from the discharge port 2212 are wrapped in the high-speed airflow from the high-speed air outlet 263 and stretched by pulling them downstream. This high-speed air outlet 263 having a predetermined blowing angle constitutes the stretching airflow means.

[0021] 3, the nozzle section 22 of the stretching airflow means is mainly composed of a nozzle body 221 and a nozzle support 222, and as shown in the enlarged view of the vicinity of the discharge port 2212 in FIG. 3, the nozzle body 221 is provided with a central axial hole 2211 from which PVDF, a dissolved polymer, is ejected in the longitudinal direction, and a discharge port 2212 is provided at the tip part on the downstream side of this central axial hole 2211. The material of the nozzle body 221 in the nozzle section 22 of the present invention is optimally stainless steel, ceramic, ruby, etc., and in Example 1, it is ruby. The inner diameter of the nozzle, which is the discharge port 2212, was set to 0.10 mm to 0.18 mm, but if it was 0.18 mm or more, it was difficult to generate nano-fibers in nano-unit fibrous form, and if it was 0.10 mm or less, the dissolved polymer would clog the inner diameter of the nozzle, so in this embodiment it was set to about 0.15 mm. In addition, the nozzle inner diameter was previously set to 0.15 mm, but it was found that the material was stainless steel metal, which quickly changed into thick fibers. It was found that this was due to the stainless steel nozzle inner diameter expanding due to repeated weight and pressure. For this reason, by using ruby ​​(ceramic), which has excellent heat resistance and abrasion resistance and does not deform even at high temperatures, a high-quality polymer nanofiber laminate N3 could be produced even when operated continuously for a long time.

[0022] However, ceramics and ruby ​​are difficult to process, and it is difficult to fix the nozzle outlet 2212 to the metal nozzle support 222 with screws or the like. Therefore, as shown in Fig. 3, a thick flange 2213 protruding outward is provided at the upstream end of the nozzle body 221, and a locking part 2222 protruding inward is provided at the downstream end of the corresponding inner hole 2221 of the nozzle support 222, and the nozzle body 221 is inserted from the upstream opening 2223 of the inner hole 2221 of the nozzle support 222, and the flange 2213 is tightly fitted into the locking part 2222 to be fixed. With this structure, the nozzle body 221 will not come off the nozzle support 222 even if a dissolved polymer is inserted at a high pressure on the downstream side. In this case, the inner diameter of the inner hole 2221 must be larger than the outer diameter of the nozzle body 221 and the outer diameter of the flange portion 2213, and the inner diameter of the tip engagement portion 2222 of the nozzle support body 222 must be smaller than the outer diameter of the nozzle body 221 and the outer diameter of the flange portion 2213. Spacer portions that maintain the passage gap are provided in appropriate positions between the outer periphery 231 of the central axial hole 2211 and the outer periphery 2224 on the discharge port 2212 side and the inner periphery wall of the high-speed air blowing passage 262, thereby maintaining the gap and forming the high-speed air blowing passage 262. The polymer introduction pipe 23 is as shown in Figure 4, and the high-speed air blowing passage 262 has an injection air introduction groove 232 formed in the gap between the air introduction section frame 272 and the outer periphery 231 of the polymer introduction pipe 23, and the high-speed air passes through this groove.

[0023] To further explain this stretching airflow means, since the polyvinylidene fluoride (PVDF) fibers are further stretched by the high-speed airflow, the blowing angle of the ring-shaped high-speed air outlet 263 (the combined angle on the left and right sides around the axis of the central axis hole 2211) is important, and as a result of experiments, an angle of about 30° to 60°, that is, the blowing direction of the high-speed airflow from the high-speed air outlet 263 is preferably in the range of an angle of 15° to 30° with respect to the central axis line of the central axis of the discharge port 2212, and if the angle is 30° or less (angle 15° from the central axis), the contact force with the polyvinylidene fluoride (PVDF) is small and the stretching action is small, and if the angle is 60° or more (angle 30° from the central axis), negative pressure is not generated by contact, so the stretching action is also small, and in this Example 1, the angle was 38° (angle 19° from the central axis) to ensure efficient stretching action.

[0024] In this way, if the airflow from the high-speed air outlet 263 does not hit the appropriately spun polyvinylidene fluoride (PVDF) fibers, they will end up as ultrafine fibers on the order of μ, and will not become nanofibers. Furthermore, in order to efficiently stretch polyvinylidene fluoride (PVDF) fibers to nano-units, it is important to dissolve them in a solvent and make them low-viscosity, but the stretching airflow means needs to stretch them with high-speed injected air even after they are spun from the discharge port 2212, and more importantly, it is necessary to vaporize and remove the solvent N-methyl-2-pyrrolidone (NMP) contained in the polyvinylidene fluoride (PVDF) fibers while stretching them. For this reason, the high-speed air outlet 263 is configured to protrude slightly by about X1 = 5 mm (5 to 7 mm) from the discharge port 2212 of the spinning nozzle section 22, in order to promote the evaporation of the solvent of the polyvinylidene fluoride (PVDF) fibers spun from the discharge port 2212. It has been found through experiments that when the specified distance X1 in the flow direction between this high-speed air outlet 263 and the discharge outlet 2212 is set to a protrusion of about 5 to 7 mm, the stretching action of the polyvinylidene fluoride (PVDF) fibers by the high-speed air acts appropriately, making it possible to achieve both the stretching of the polyvinylidene fluoride (PVDF) fibers and the rapid removal of the solvent.

[0025] [Spraying section 3] Then, the nanofiber spinning solution N1 is sprayed from the nozzle portion 2 and flies in the spatial environment to the collection zone 31 of the laminate collection portion 3. In this case, the spatial distance from the nozzle portion 22 to the collection zone 31 of the nanofiber layered collection section 3 was set to approximately 165 cm, which is considered to be a distance at which the polymer material polyvinylidene fluoride (PVDF) is sufficiently stretched, causing the solvent to disperse and promoting evaporation.The nanofiber fiber N2 will not reach the layered collection section 3 with just the spray force of the nozzle portion 2, but a powerful suction mechanism is provided in the next collection layer formation process B to generate a strong airflow downstream, allowing the nanofiber fiber N2 to reach the layered collection section 3. In addition, in order to promote the evaporation of the solvent contained in the polyvinylidene fluoride (PVDF) fibers, for example, infrared heating devices 29 are installed on both sides of the space in which the nanofibers generated fly from the nozzle section 2 to the capture layer formation process B, and infrared light is irradiated to excite the polyvinylidene fluoride (PVDF) molecules, thereby raising the temperature of the molecules themselves rather than raising the temperature of the environment, thereby promoting the evaporation of the solvent in the polyvinylidene fluoride (PVDF) N1 material liquid. Here, in the manufacturing process of the nanofiber filter laminate, the spatial environment in which the polymer material is stretched needs to have a temperature of 30° C. to 40° C. and a humidity of 80% or less. In addition, the spatial environment in which the water-soluble polymer material is stretched is provided with an infrared heater 29 and an infrared reflector to promote evaporation of the solvent of the polymer material to be spun.

[0026] [Nanofiber capture layer formation process B] Next, the laminate collection unit 3 in the [nanofiber accumulation layer formation process B] in which the nanofibers generated in the nanofiber generation process A are laminated downstream will be described with reference to FIG. The laminate collection section 3 of the nanofiber laminate N is an endlessly moving mesh-like collection zone 31, as shown in Figure 1, made of a non-conductive synthetic resin and shaped like a net or mesh, and can be any material that allows a large amount of air to pass through. In this embodiment 1, the laminate collection section 3 is a monofilament mesh of polypropylene (PP), a synthetic resin, with a fiber diameter of 0.24 mm and an opening size of 1.03 mm. The mesh (hereinafter referred to as mesh) is a plain weave mesh with no knots made of a polymer material and has free intersections, but the intersections may also be fixed by welding. Since this laminate collection part 3 has the above-mentioned configuration (density 15-20 fibers / inch), the air resistance of the air passing through is sufficiently small, and the collection zone 31 only lightly holds the nanofiber laminate N3, and since there are no bundling parts, the nanofiber laminate N3 does not become entangled in the collection zone 31, and it can be quickly detached in a later process. In some cases, the front surface may be treated in advance with a fluorine-based resin or silicone-based resin as a release agent. The material of the collection zone 31 may be polyethylene resin other than polypropylene (PP) resin, or a metal conveyor net without bundling parts, as long as the nanofiber laminate N3 can be extremely easily removed from the conveyor net.

[0027] In addition, the mesh sizes that can be used are as shown in Table 2 below. [Table 2] (1) 18 mesh: fiber diameter 0.26 mm, opening size 1.15 mm (2) 20 mesh: fiber diameter 0.24 mm, opening size 1.03 mm (3) 24 mesh: fiber diameter 0.22 mm, opening size 0.84 mm (4) 26 mesh: fiber diameter 0.19 mm, opening size 0.78 mm (5) 30 mesh: fiber diameter 0.18 mm, opening size 0.67 mm 1 by driving roller 32, and is supported at predetermined positions by driven support rollers 33a-c and moves counterclockwise. The mesh in Example 1 is 20 mesh (2) in [Table 2] above.

[0028] The drive of the drive roller 32 adjusts the thickness of the finished nanofiber laminate N3, and is controlled so that the thickness of the nanofibers is 5 to 100 μm. In Figure 1, at a position opposite the nozzle portion 22 of the nanofiber production process A, a collection surface 34 having an approximately vertical plane is formed by driven support rollers 33b, 33c. This collection surface 34 continuously collects the nanofiber laminate N3, which then moves to the laminate removal process C described below, where the nanofiber laminate N3 is separated from the collection zone 31 and redirected upward by the drive roller 32, then further redirected by the driven support roller 33a, and guided by the driven support roller 33e for circulation.

[0029] On the back side of the collection surface 34, there are provided a suction chamber 361 and multiple suction ducts 362 (three in this embodiment 1, an upper, middle and lower ducts) arranged in the vertical direction, and an air suction mechanism 36 connected to these, and each suction duct 362 is provided with an air volume adjustment shutter 363 for adjusting the air volume, and the nanofiber fibers N2 and nanofiber laminate N3 generated in the nanofiber production process A are sucked into the collection zone 31. In order to keep the collection zone 31 flat, flatness-maintaining members 341 made of synthetic resin or the like are provided at intervals on the back surface of the collection zone 31. Note that a trumpet-shaped guide member 291 is provided on the front side of the collection surface 34 so as to converge on the collection surface 34 in order to efficiently guide the nanofiber fibers N2 to the collection surface 34.

[0030] The suction ducts 362 are each provided with an air volume adjustment shutter 363 for adjusting the air volume, and the amount of the nanofiber laminate N adhering to the collection surface 34 is adjusted by the opening area of ​​the suction duct 362. If the amount of adsorption is large, it will be difficult for the nanofiber laminate N3 to separate from the collection zone 31 in the detachment process C, so the amount of adsorption is adjusted so that it will separate easily. In this way, the nanofiber laminate N3 formed vertically and continuously on the collection zone 31 moves horizontally to the right as the collection zone 31 moves downward, and the nanofiber laminate N3 is detached at the laminate detachment section 38 and guided in circulation from the drive roller 32.

[0031] [Removal process C of nanofiber laminate N3] In this way, the nanofiber laminate N3 laminated in the collection zone 31 is detached by the laminate detachment section 38 arranged between the driven support roller 33c of the collection zone 31 and the drive roller 42, and the laminate detachment section 38 detaches from the collection zone 31 on a mesh-like end-S belt 383 stretched around a drive roller 384 and a guide roller 385, and moves onto the belt 383 in the detaching step C. This laminate detachment section 38 comprises an upper air blowing device 381 and a lower air suction device 382, ​​and detaches the nanofiber laminate N3 adsorbed to the collection zone 31 from the collection zone 31 by air blown from the blowing nozzle 3811 of the upper air blowing device 381 and the suction nozzle 3821 of the lower air suction device 382. To explain this in more detail, the laminated nanofiber laminate N3 is detached by jetting air from the blowing nozzle 3811 of the air blowing device 381 from above (detachment process C), and the suction force of the suction nozzle 3821 is used to suck and remove solvents such as N-methyl-2-pyrrolidone (NMP) and toluene adhering in small amounts to the nanofiber laminate N4, as well as dust adhering to the collection surface 34. In this case, if the laminated collection section 3 is a monofilament net made of polypropylene (PP), a synthetic resin, the nanofiber laminate N3 can be easily detached by air from the blowing nozzle 3811 above and the suction force of the suction nozzle 3821 below. In this way, the suction nozzle 3821 also serves to remove dust, removing nanofiber pieces and dust remaining in the collection zone 31 and sending out a clean collection zone 31. If necessary, a release agent applicator or the like may be provided to make it easier for the nanofibers to separate. At this time, the nanofiber laminate N3 has a basis weight of 3 to 20 g / m 2 It was.

[0032] [Cleaning process D] The nanofiber laminate N4 detached from the collection zone 31 is transferred to the cleaning device 4 for the next cleaning step D, where the nanofiber laminate N4 is first compressed by pinch rollers 41 and then sent to the cleaning tank 43 by guide rollers 42. In the first embodiment, the cleaning tank 43 of the cleaning device 4 is a tank filled with methanol liquid (or isopropyl alcohol). The purpose of cleaning with this methanol liquid is to remove excess carbon black fine particles. Although the carbon black fine particles adsorb and remove the fine particles suspended in the air, clogging can occur, so the purpose of cleaning with this methanol liquid is to improve air permeability. A predetermined time for washing in methanol is required to remove excess carbon black fine particles, but in reality, about 3 to 30 minutes is required, and it is 5 minutes in Example 1. The carbon black is immersed (or washed) in the methanol liquid (Example 1) (or isopropyl alcohol) in the washing tank 43 of the washing device 4, guided into the washing tank 43 and washed in the methanol liquid by a roller group 44 (Example 1) that reciprocates left and right, and the number of reciprocations is adjusted to wash for a predetermined time, and the nanofiber laminate N5 is sent from the guide roller 45 to the pinch roller 46 as the nanofiber laminate, and the methanol of the washing liquid is removed by a drying device 47 or the like as necessary, and the nanofiber laminate N5 is wound up as the intermediate product in the winding process E.

[0033] [Intermediate product winding process E] In the winding process E of the intermediate product, which is the nanofiber laminate N5, the nanofiber laminate N5 is transported by pinch rollers 46, through a drying device 47 such as a blower, and then by feed rollers 48, and is wound up in the product winding section 5 as a lot 5A. The rotating shaft 52 of the product winding roll 51 in the product winding section 5 is wound by a winding drive motor 54 via a powder clutch 53. This intermediate product winding section 5 is equipped with an ultrasonic sensor 55 for detecting winding diameter, and since the winding tension changes with changes in the winding diameter, a powder clutch 53 is provided between the drive source, winding drive motor 54, and the rotating shaft 52 to keep this tension constant; therefore, by controlling the slippage of the powder clutch 53, the product nanofiber laminate N5 can be wound with a constant tension.

[0034] [Nanofiber filter laminate formation process F] In Fig. 2, a lot 5A of nanofiber laminate N5, which is an intermediate product of the winding device 5 in Fig. 1, is set in the supply device 6 in Fig. 2, and the lot 5A set in this supply device 6 is transferred by a drive device 61 with a powder clutch and a feed roller 62, and then in a nonwoven fabric attachment device 7, a thin net or a thin microfiber nonwoven fabric or the like is driven and supplied to the upper and lower surfaces of the nanofiber laminate N5 by the drive devices 711, 721 of the supply devices 71, 72. The upper and lower surfaces of the nanofiber laminate N5 are sandwiched by a pair of feed rollers 73, and then predetermined parts of the nanofiber laminate N5 are heat-welded by a pair of heating and pressure rollers 74 shown in Fig. 3 to form a nanofiber filter laminate N6. The heating and pressurizing rollers 74 shown in FIG. 3 press the nanofiber laminate N5 with heating parts 741 of the upper and lower rollers 74, and at the same time, heat predetermined parts to pressure-weld them. Here, when nonwoven fabrics (Example 1) are used on both sides of the nanofiber filter laminate N5, the thickness of the nonwoven fabric is selected from polyethylene nonwoven fabric, polypropylene nonwoven fabric, and nylon nonwoven fabric, and the thickness of the nonwoven fabric is 0.1 to 0.7 mm and the basis weight is 10 g to 60 g / m 2 Furthermore, the nanofiber laminate mask is ideal as a filter for regular masks, medical masks, or industrial dust masks. [Winding process G of the final product (nanofiber filter laminate)] In the winding process G for the final product, the nanofiber filter laminate N6 is wound by the winding device 8 using a driving device 82 to become the final product, a winding lot 81 (8A). The winding device 8 has almost the same configuration as the winding section 6 in the winding process E for the intermediate product, the nanofiber laminate N5. Thus, the final product, lot 8A of the nanofiber filter laminate N6, is rewound and cut as necessary to be processed into masks or the like.

[0035] [Examples of use in mask products] These semi-finished products can be used for applications such as screen doors and agricultural greenhouses, as well as for processing the nanofiber filter laminate (final product) N6 into the base material of a mask or a filter to be attached to the pocket of a mask. For example, as shown in Example 1 of FIG. 7, the final product N6 is cut from the welded portion 87a by applying pressure and heat to the rectangular end to match the state of use of the mask, to form the mask substrate 85, and rubber strings or elastic bodies 87 are pressure welded to both sides of this to form the mask N8 of Example 1 of Use. As shown in Figure 8 of another usage example 2, the final product N6 may be cut into a slightly smaller rectangular end portion under pressure and heat to fit the mask in use, to form a mask filter substrate 85b, which may then be inserted into a pocket portion 88 of the mask to form a pocket-type mask. 7 and 8, when worn by fitting it to the shape of the nose with a nose fit wire 86 as shown in FIG. 9, the gap between the face and the mask becomes smaller, reducing the amount of droplets leaking out. In this embodiment, since fine carbon black particles are used, the entire surface is black or gray, but if the entire surface is covered with a thin film-like mesh, the surface can be colored any desired color, and printing can be applied thereto.

[0036] Here, Figure 10(a) shows an electron microscope photograph at 200x magnification of the nanofiber laminate N3 produced in Figure 1 of Example 1, containing carbon black microparticles, and Figure 10(b) shows an electron microscope photograph at 1000x magnification. Next, Figure 11(a) shows an electron microscope photograph at 200x magnification of the nanofiber filter laminate N4 after the nanofiber laminate N3 had been washed to remove excess carbon black particles using cleaning device 53, and Figure 11(b) shows an electron microscope photograph at 1000x magnification. As can be seen from these photographs, FIG. 10 shows that the carbon black is firmly attached to the nanofibers, and FIG. 11 shows that the excess carbon black has been removed by washing.

[0037] [Test Results] First, the experimental results regarding the collection efficiency will be described. (1) [Table 3] [Particle collection rate] (1-1) Here, the effects of the fine particle collection efficiency and capture rate will be shown by comparing the nanofiber filter laminate N6 in FIG. 2 with a conventional nanofiber filter laminate that does not contain carbon black fine particles. Test Method ASTM F2299, but does not neutralize particles (static removal). Test conditions Test area: 49.0cm 2 Test flow rate: 28.9L / min Particle size: 0.1μm(0.100±0.0003μm) Particle type: JSR SIZE STANDARD PARITECLES SC-0100-D (JSR Life Sciences Co., Ltd.) Spherical polystyrene standard particles Test Subjects: A: Conventional nanofiber filter laminate without carbon black particulates A1: Collection rate of a conventional nanofiber filter laminate with a thickness of 10 μm: 90.7% (average collection efficiency) A2: Collection efficiency of a conventional nanofiber filter laminate with a thickness of 50 μm: 93.7% (average collection efficiency) B: Nanofiber filter laminate containing carbon black particles from Example 1 B1: Collection rate of the nanofiber filter laminate of Example 1 with a thickness of 10 μm: 98.0% (average collection efficiency) B2: Collection rate of the nanofiber filter laminate of Example 1 with a thickness of 50 μm: 99.5% (average collection efficiency) The above collection efficiency test results show that the collection efficiency of the nanofiber filter laminate containing carbon black fine particles is improved. Also, the suspended fine particles collection efficiency of the nanofiber filter laminate (N6) of Example 1 depending on the thickness is shown in [Table 3]. The suspended fine particle collection efficiency of the nanofiber filter laminate of Example 1B1 having a thickness of 10 μm is about 98.0%, but the nanofiber filter laminate of Example 1B2 having a thickness of 50 μm has a fine particle collection efficiency of 99.5%, which shows that the nanofiber filter laminate can sufficiently collect fine particles.

[0038] Next, an experiment on pressure loss related to breathlessness when breathing through the mouth using a mask or the like will be described. (2) [Pressure loss] This experiment examines the pressure loss related to breathlessness when breathing through the mouth. Pressure drop measurement test results for nanofiber filter laminate N6 Test method 1 The pressure loss (unit: Pa Pascal) at standard airflow was measured for the nanofiber filter laminate N6 of Example 1 having a thickness of 50 μm when used as (1) a ventilation fan, (2) a mask, and (3) an air conditioning filter, as well as for a commercially available mask from Company A. [Table 4] 1. Measurement object: Nanofiber filter laminate N6 of Example 1 Filter under test Air flow conditions Pressure loss measurement results Ventilator 350CMH=264.6L / min 87Pa Mask 85L / min=170.5L / min 55Pa Filter 5.33 / min=65.675L / min 22Pa 2. Measurement subject: A commercially available mask made with nanofiber from company A Mask 85L / min=150a From the pressure loss test results in Table 4 above, it can be seen that the pressure loss (unit: Pa·pascal) of the fiber filter laminate containing carbon black particles in each object is smaller than that of the commercially available mask made by Company A. In addition, at an appropriate point in the manufacturing process after the nanofibers of Example 1 are completed, a deodorant attachment process as used in the following Example 2 may be added.

[0039] As described above in detail, according to Example 1 of the present invention, the nanofiber filter laminate of the present invention and the mask using the same are prepared by dissolving a polymeric material having a long molecular arrangement, pressurizing a spinning solution in which carbon black fine powder is mixed into the polymeric material, spinning the polymeric material from a spinning nozzle, providing a ring-shaped high-speed outlet coaxially with the central outlet of the spinning nozzle so as to surround the central outlet of the spinning nozzle, and stretching the polymeric material from the spinning nozzle and vaporizing the solvent by an airflow from the high-speed outlet. The nanofiber filter laminate is further washed for a predetermined time with water, methanol or isopropyl alcohol, and the nanofiber laminate has a thickness of 5 to 100 μm and a basis weight of 3 to 20 g / m. 2 The nanofiber filter laminate is made by sandwiching both sides of the nanofiber laminate between nonwoven fabrics and welding them at predetermined locations, and the mask using the same is made, so the carbon black fine powder is firmly mixed in and does not come off even when washed. The polymeric material to be spun is preferably a polymeric material selected from polyvinylidene fluoride (PVDF), polyvinyl butyral (PVB), polyvinyl alcohol (PVA), polyurethane (PU), polyamide (registered trademark; nylon), etc., and the nonwoven fabric on both sides of the manufactured nanofiber laminate is selected from polyethylene nonwoven fabric, polypropylene nonwoven fabric, and nylon nonwoven fabric, and the thickness of the nonwoven fabric is 0.1 to 0.7 mm and the basis weight is 10 to 60 g / m. 2 The nanofiber filter laminate is a nanofiber filter laminate having a thickness of 100 nm and a thickness of 150 nm. Furthermore, a mask using this nanofiber filter laminate is ideal as a mask for general use, a medical mask, and an industrial dust mask.

[0040] The nanofiber filter laminate of the present invention How to produce The method employs a spinning method using high-speed jets rather than an electrospinning method, in which a collecting substrate is formed by plain weaving unbonded monofilaments of a polymer material in an endless circulating manner to form a coarse mesh, a polymer material having a long molecular arrangement is dissolved in a solvent and pressurized to be spun from a spinning nozzle toward the collecting substrate, a ring-shaped high-speed blowing outlet is provided coaxially with the central outlet of the spinning nozzle so as to surround the central outlet, the polymer material from the spinning nozzle is stretched by the airflow from the high-speed blowing outlet and the solvent is vaporized to layer and collect nanofiber-like fibers on the collecting substrate, and the nanofiber layer attached to the collecting substrate is easily peeled off and wound up, so that the nanofiber layer can be easily washed in methanol or isopropyl alcohol for a predetermined period of time. In addition, the nanofiber filter laminate can use a polymer material selected from polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyurethane (PU), and polyamide (registered trademark; nylon) as the polymer material to be spun, and since the mask uses this laminate, it can be mass-produced at low cost.

[0041] When these nanofiber filter laminates are used as filters for general-use masks, medical masks, and industrial dust masks, they can capture pollen, fine particulate matter PM2.5, and other dust and viruses, and are optimal for this purpose with little air pressure loss and little breathability. In addition, when used as filters for ventilation fan filters, screen doors, and agricultural greenhouses in places exposed to the outside air, if the nanofiber material is polyvinylidene fluoride (PVDF), it is a resin that has excellent weather resistance and is resistant to radiation, making it suitable as a building material for outdoor screen doors, agricultural greenhouses, and the like, and is easy to clean. Furthermore, the nanofiber layer has sufficient breathability and strength, and can be mass-produced at low cost. Furthermore, according to the manufacturing process for the filter laminate of Example 1, the nanofiber layer can be easily made thick, and since an endless, circulating collection substrate is used in which unbonded polymeric monofilaments are plain woven to form coarse meshes, the nanofiber layer can be easily made thick, and since the nanofiber layer is thick, the collection efficiency is increased, making it possible to capture droplets of fine particulate matter PM2.5, viruses, and the like.

[0042] [Example 2] Next, Example 2 will be described with reference to Figures 12 to 19. The difference from Example 1 is that first, a plain woven monofilament mesh is used as the surface substrate J1, and then polyvinylidene fluoride (PVDF) nanofibers are sprayed onto it to adhere it. The integrated mesh and nanofiber are then wound up, and two of the nanofiber laminates J5 of Lot 95A are exposed with the mesh side facing outward to complete the nanofiber filter laminate J6.

[0043] The second embodiment will be described in detail below. Figures 12 and 13 are conceptual explanatory diagrams showing an outline of the overall manufacturing method of Example 2. As shown in Figure 12, the outline of the manufacturing equipment for laminating nanofibers into an air filter or mask filter substrate is as follows: The first step is a step of paying out the surface base material J1, which is a 20-mesh net made of plain woven polypropylene, a polymer material [surface base material paying out step H], and the next step is a mesh-like reinforcing fiber formation step, which is roughly made up of three steps. First, the first polymer adhesive J2 is sprayed onto the paid-out surface base material J1 to form a spider web-like or zigzag-like mesh with adhesive fibers [first polymer adhesive spraying step I], the second step is [cooling and fixing K] to harden the fiber-like first polymer adhesive, and the third step is [second polymer adhesive spraying step L]. The first polymer adhesive has good adhesion to the surface substrate J1, and the second polymer adhesive has good adhesion to the first polymer adhesive J2 and the polyvinylidene fluoride (PVDF) of the nanofiber J4. As a result, adhesion between the surface substrate J1 and the nanofiber J4 is good, and then, in the [nanofiber production process M], the polyvinylidene fluoride (PVDF) nanofiber J4 is sprayed onto the surface substrate J1. A nanofiber laminate J4 is formed, titanium oxide is attached in the [deodorant attachment process N], and the intermediate product is temporarily wound up in the [winding process O]. As shown in Figure 13, in [nanofiber filter laminate formation process P], two pieces of intermediate product lot 971 (95A) are set in upper and lower payout devices, combined by combining rollers that combine so that the surface substrate J1 is exposed to the outside, and laminated by overlapping with the nanofiber surfaces facing each other to complete the air filter or mask filter, which is then wound up in [winding process R] as the product nanofiber filter laminate J6.

[0044] The manufacturing process of Example 2 is roughly as described above, but will be described in more detail below. [Surface base material feeding process H] The surface substrate J1 of Example 2 was a monofilament having a rectangular space, and was a typical 20 mesh PP (polypropylene) having a diameter of 0.24 mm, a thickness of 125 μm, and a basis weight of 30 g / m 2 and has sufficient breathability, and the surface base material J1 is strong enough to be used as a building material for window screens, an air filter for a fan, a filter for a mask, etc. Note that, other than the above-mentioned PP (polypropylene), for example, polyethylene (PE), polyester (PET), polyphenylene sulfide (PPS), etc. may be used as the surface base material J1. As shown in FIG. 12 , this surface base material J1 is provided with a winding diameter detection ultrasonic sensor 916 at a payout section 91 for the surface base material J1, and since the winding tension changes with changes in the winding diameter, a powder clutch 954 is provided between a winding drive motor 953, which is the drive source, and the rotation shaft to keep this tension constant. By controlling slippage of the powder clutch 954, a constant tension is applied to the surface base material J1 to prevent slack, and the surface base material J1 is sent to the next process, the [net-like reinforcing fiber forming process], via a plurality of guide rollers 913 and a delivery mechanism 914.

[0045] [Net reinforcing fiber formation process] As described above, the reticulated reinforcing fiber forming process is composed of the [first polymer adhesive spraying step I], the [cooling step K] for hardening the first polymer adhesive, and the [second polymer adhesive spraying step L]. [First polymer adhesive spraying process I] In the [first polymer adhesive spraying process I], a first initial intermediate product (J2) is formed in a state in which a first polymer adhesive J2 is sprayed onto the delivered surface base material J1 by a first polymer adhesive (resin) spraying unit 921, and this forms a mesh by bridging with spider web-like or zigzag fibers, preventing the woven mesh of the surface base material J1 from shifting, and further forming an even finer mesh in the spaces between the mesh of the surface base material J1, thereby reinforcing the strength of the thin nanofiber layer to be laminated in a later process and preventing the nanofiber layer from breaking. A first nanofiber-like polymer adhesive is used to fill the spaces in this surface substrate J1, with fibers that are thicker than the nanofibers J4 and have an average thickness of 10 to 100 μm. The fibers are cross-linked and woven in a spider web or zigzag pattern to form a finer mesh (J2). A nanofiber layer J4 is then bonded to this finer mesh in a later process using a nanofiber-like second polymer adhesive J3, thereby improving the strength of the nanofiber laminate J4.

[0046] The first polymer adhesive J2 used to form this fiber is a cross-linking and reinforcing adhesive (Kleiberit PUR reactive hot melt (product number: No. 703.5) manufactured by KLEIBERIT Co., Ltd.), which has the property of stretching like threads in a spider web shape, making it ideal for forming a fine cross-linked network. In addition, this first polymer adhesive does not require heating and gradually hardens (within a few seconds) at room temperature, so it does not deteriorate the surface substrate J1 or the nanofiber J4 (N4). However, even if the first polymer adhesive J2 dries quickly, if it does not harden completely, that is, if the adhesion between the surface substrate J1 and the second polymer adhesive J3 or the nanofibers J4 in the subsequent process is insufficient, the surface substrate J1 often peels off. For this reason, even though the first polymer adhesive N2 is quick-drying, it is necessary for it to completely solidify (harden) before moving on to the next process, and for this reason a cooling process K for the fiber-shaped first polymer adhesive is provided in which the fiber-shaped first polymer adhesive J2, which will be described in detail in the next process, is sprayed and then cooled. The reason why the first polymer adhesive J2 is used to form a spider web-like or zigzag-like mesh in the spaces of the square mesh (20 mesh) in the surface base material J1 is to reduce blocking of the spaces formed by the nanofibers J4. If the spaces of the mesh were reduced by the monofilaments of the surface base material J1 themselves, not only would the weight of the shielding member increase, but the light blocking rate would also increase, which is an inconvenience.

[0047] The mesh-like reinforcing fiber forming section 92 in which the fibers are laid out in a spider web or zigzag pattern will be described with reference to Figs. As shown in FIG. 12, the reticulated reinforcing fiber forming unit 92 is located between the [surface substrate feeding process H] and the [nanofiber generating process M], and sprays a first polymer adhesive J2 onto the mesh surface of a polypropylene (or polyethylene) surface substrate J1 to form a fine mesh in the square spaces of the surface substrate J1. Therefore, just before the nanofibers J4 and the second polymer adhesive J3 are sprayed onto the surface substrate J1, as shown in FIGS. 14 and 15, the nanofibers J4 and the second polymer adhesive J3 are sprayed onto the surface substrate J1 from a nozzle unit 922 in the form of fibers that are slightly thicker and stronger than the nanofibers J4.

[0048] The fiber-like first polymer adhesive J2 is a polyurethane hot melt adhesive (moisture curing type) (PUR reactive hot melt (product number) No. 703.5) manufactured by KLEIBERIT Japan Co., Ltd., and its physical properties are as shown in the following [Table 5]. [Table 5] (A) Main component of the first polymer adhesive: polyurethane viscosity 120℃: 11,000 mPas 140℃: 6,000 mPas Open time (time required to evaporate the solvent (hardening)) φ3mm bead: 30sec Open time 90μm: 30sec Features: Heat resistance, water resistance, cold resistance, low temperature coating, elastic type, stringiness

[0049] When spraying the first polymer adhesive J2 to form this fiber, if the gaps between the nanofibers J4 are filled, the excellent breathability of the nanofibers J4 will be hindered, so it is important that the first polymer adhesive J2 is as thin as possible and is formed in a spider web or zigzag net so as not to fill the gaps between the nanofibers J4. In addition, the first polymer adhesive J2 was a PUR reactive hot melt (product number No. 703.5), and the selection criteria were as follows: (1) It is necessary to reinforce the mesh spaces (between the meshes) of the surface substrate J1 and to enlarge the adhesive application surface (enlargement of the adhesive area) of the second polymer adhesive J3 described later, (2) it is fibrous and has strong threading properties and excellent crosslinking properties, and (3) since the distance from the spraying process of the first polymer adhesive to the spraying process of the second polymer adhesive J3 is short, the surface is hardened immediately after the adhesive is applied. Note that similar results were obtained with another first polymer adhesive J2, a polyurethane hot melt adhesive (moisture curing type) with product number VP9484 / 10, which is a non-yellowing discoloration type (transparent or white) manufactured by KLEIBERIT JAPAN CO., LTD.

[0050] 12, the spraying section 21 of the first polymer adhesive J2 of the network reinforcing fiber forming section 92 is disposed above the surface base material J1 moving from an upper guide roller 913a to a lower guide roller 913b, and moves back and forth a distance of 110 cm (nanofiber generation width) parallel to the surface of the surface base material J1 with which the nozzle section 922 moves together. This is because the first polymer adhesive J2 does not need to be laminated like the nanofiber laminate J4, and it is sufficient if the strength of the nanofibers J4 is reinforced, and in fact the less the better. The viscosity of the above-mentioned first polymer adhesive J2 decreases at higher temperatures, with the viscosity at 140°C being 6000 (mPa s), so that it can be used in this state, a heater 9264 is provided in the nozzle portion 922 as shown in Fig. 14. Note that the first fibrous polymer adhesive J2 needs to be quick-drying (in a few seconds) so that it does not melt and fuse entirely with the fibrous second polymer adhesive J3 described below.

[0051] 12, 14 and 15, the first polymer adhesive J2 is heated to about 140° C. and supplied from a supply unit 924 to a central nozzle 9221 having a tip nozzle diameter of 0.15 mm through a supply pipe 9241 of the first polymer adhesive J2 by ​​a supply pump 9242. A cylindrical hot air blowing unit 926 is provided to surround the outer periphery 9231 of the outer cylinder at the tip of the central nozzle 9221, and high-velocity heated air H is sprayed from a hot air blowing nozzle portion 9261 of the hot air blowing unit 926 to pull out the molten adhesive from the central nozzle 9221, turning it into the second polymer adhesive J2 and spraying it toward the surface substrate J1. At this time, the air pump 928 blows high-speed heated air H to the hot air blowing nozzle portion 9261 at 50 liters / minute, and the air is introduced into the high-speed air blowing passage formed between the heated air path forming cap 927 and the molten resin introduction pipe 923 via the heated air generator 9281, heated air supply pipe 9282, and heated air introduction portion frame 9272, and the high-speed heated air H is sprayed out from the hot air blowing nozzle portion 9261 at the tip of the heated high-speed air outlet 9263 which is connected to the high-temperature, high-velocity blowing passage. The air outlet nozzle 9261 has an outlet area of ​​1 mm 2The entire nozzle portion 922 is adjusted to a high temperature of about 140° C. using a heater 9264, and the ejected air is also heated to about 140° C. before being ejected, so that the adhesive is maintained at 140° C. even at the tip of the nozzle portion 922.

[0052] As described above, the molten resin introduction pipe 923 has a molten resin introduction passage 9234 at its center which is connected to the nozzle portion 922 of the adhesive, and on its downstream outer periphery 9231 is provided a hot air introduction groove 9232 which is connected to the nozzle portion 922, and the other end of this hot air introduction groove 9232 is connected to a hot air generator 9281. This hot air introduction groove 9232 has the same structure as the molten resin introduction pipe 234 in FIG. 6 of the first embodiment, so a description thereof will be omitted. With this configuration, it was found that, without using the ESD method in particular, the adhesive can be produced in large quantities in the form of fibers with fiber diameters of 500 nm to 500 μm, although the fibers are somewhat thicker than with this method. Of these, the first polymer adhesive J2 is melted into fibers with diameters of 10 μm to 100 μm and sprayed onto the polypropylene surface base material J1 in a spider web or zigzag pattern so that the fibers adhere to the surface, and are evenly applied over the entire surface.

[0053] As shown in FIG. 15, the nozzle body 9221 has a ring-shaped high-velocity hot air blowing passage 9262 coaxially arranged around a central axial hole 92211 so as to surround the central axial hole 92211, and a ring-shaped high-velocity air outlet 9263 having a predetermined blowing angle is provided at the tip of the high-velocity hot air blowing passage 9262, and the outlet 92212 of the nozzle body 9221 protrudes slightly by approximately X=3 mm (2 to 4 mm) from the high-velocity air outlet 9263 to generate a straightened flow. 14, since the high-speed hot air blowing passage 9262 of the heated air path forming cap 927 is inclined and the outer periphery of the central nozzle main body 9221 is also inclined, the protrusion amount X of this discharge port 92212 from the high-speed air blowing outlet 9263 can be adjusted by interposing a fine adjustment washer 9273 of the hot air blowing outlet between the heated air path forming cap 927 and the heated air introduction part frame 9272 and selecting a fine adjustment washer 9273 with a different thickness or by adjusting the number of washers. This makes it possible to adjust the protrusion amount X and at the same time finely adjust the gap between the inner wall of the hot air blowing passage of the high-speed hot air blowing passage 9262 and the outer periphery of the nozzle main body 9221, i.e., the opening area of ​​the hot air blowing nozzle part 9261. In this way, the amount of hot air blown out from the hot air blowing nozzle portion 9261 can be finely adjusted, so that the amount of hot air blown out from the multiple nozzle portions 922 can be made the same, as shown in Figure 12, and a more uniform laminate of adhesive and nanofibers of molecular material can be produced.

[0054] 15, the nozzle body 9221 is provided with a central axial hole 92211 through which the molten polymer is ejected in the longitudinal direction, and the nozzle body 92212 is provided at the downstream tip of the central axial hole 92211. The important thing here is the material of the nozzle body 9221, and the material of the nozzle body 9221 in the spinning nozzle part 922 of the present invention is preferably stainless steel, ceramic, or ruby. Since the surface base material J1 has a large grain and is strong, the first polymer adhesive J2 (and the second polymer adhesive J3) passes through the surface base material J1, and dust and the like are collected by an adhesive collector 925 at the rear.

[0055] 15, a thick flange 92213 protruding outward is provided at the upstream end of the nozzle body 9221, and a locking portion 92222 protruding inward is provided at the downstream end of the corresponding inner hole 92221 of the nozzle support 9222, and the nozzle body 9221 is inserted from the upstream opening 92223 of the inner hole 92221 of the nozzle support 9222, and the flange 92213 is tightly fitted into the locking portion 92222 to be fixed. With this structure, the nozzle body 9221 will not come off the nozzle support 9222 even if molten polymer is injected downstream at high pressure. In this case, the inner diameter of the inner hole 92221 must be larger than the outer diameter of the nozzle body 9221 and the outer diameter of the flange 92213, and the inner diameter of the tip engagement portion 92222 of the nozzle support 9222 must be smaller than the outer diameter of the nozzle body 9221 and the outer diameter of the flange 92213. Further, molten resin is supplied to a molten resin introduction pipe 923 communicating with the nozzle portion 922 by an appropriate means, for example, as shown in Fig. 14, the molten resin is supplied from an adhesive supply portion 924 via a supply pump 9242 and an adhesive supply pipe 9241. If the nozzle main body 9221 is made to move at the same distance in the horizontal direction relative to the surface base material J1 as necessary, it is possible to reduce the number of nozzle main bodies 9221. Next, the process proceeds to a cooling step K in which the fiber-like first polymer adhesive J2 is cooled.

[0056] [Cooling process K] In this embodiment, the cooling device 93 in the [cooling step K] of the first polymer adhesive uses a Peltier element. As shown in FIG. 16, the aluminum cooling plate 931 is cooled to a surface temperature of -10°C to -20°C, and an insulating plate 932 is placed opposite the cooling plate 931 with a gap of 5 mm or less. It is also preferable that the gap between the mesh-like reinforcing fiber to which the first polymer adhesive J2 has been applied in the previous process and the cooling plate 931 be 1.5 mm or less, from the viewpoints of promoting the hardening of the first polymer adhesive J2 and saving energy. A Peltier element cooling mechanism 933 is built in behind the cooling plate 931, and the principle of the Peltier element is as shown in Fig. 17, where a Peltier device 934 is composed of, for example, multiple Peltier elements, and multiple N-type thermoelectric semiconductors (n) 9341 and P-type thermoelectric semiconductors (p) 9342 are alternately arranged, and they are connected in a staggered manner by metal electrodes 9343, and current is supplied to both ends from a DC power source 9345. In this connected state, as shown by the right-facing arrow in Fig. 17, electrons and holes in the semiconductor carry heat downward, so that the metal electrode 9343u on the left side is cooled and the metal electrode 9343d on the right side is heated. The multiple upper surfaces of the left metal electrode 9343u are connected and covered with a thin plate-like insulating material 9344, and are stacked in close contact with each other so that heat is efficiently conducted to the cooling plate 931 that cools or heats via the insulating material 9344. Similarly, the multiple upper surfaces of the right metal electrode 9343d are connected and covered with a thin insulating material 9344, and are stacked in close contact with each other so that heat is efficiently conducted to the cooling plate 931 that cools (absorbs heat) (generates heat) via the insulating material 9344. The cooling process K of this first polymer adhesive is very important. When the first polymer adhesive is passed through this cooling process K, the second polymer adhesive J3 is reinforced with a neat spider web-like mesh of fibers, whereas the second polymer adhesive J3 is shriveled and does not have a spider web-like structure, and therefore does not provide strong reinforcement. The solidification (curing) of the adhesive of the mesh-reinforced surface base material J1 is promoted, and the next step is the [second polymer adhesive spraying step L], in which the second polymer adhesive J3 that adheres in a fibrous form is sprayed.

[0057] [Second polymer adhesive spraying process L] Next, in the [Reticulated Reinforcing Fiber Formation Process], the initial intermediate product (J3) will be described for the [Second Polymer Adhesive Spraying Process L] in which the second polymer adhesive J3, which will mainly adhere nanofibers J4 in the next process, is sprayed onto the surface substrate reinforced with the first fibrous polymer adhesive J2 at the second polymer adhesive spraying section 921b in Figure 12. This state is as shown in the micrograph of Fig. 20 (surface substrate J1 + first polymer adhesive J2 + second polymer adhesive J3), where the fibrous second polymer adhesive J3, with a fiber diameter of 500 nm to 10 μm (preferably 100 nm to 10 μm in Example 2), which is even thinner than the fibrous first polymer adhesive J2, is sprayed thinly onto the net and allowed to shrink in a spider web shape so as not to block the gaps. In this way, the second polymer adhesive J3 adheres and shrinks while the polymer adhesive J2 clings to the surface substrate N1. Therefore, compared to the state of the first polymer adhesive J2 (surface base material N1 + first polymer adhesive J2), the micrograph in Fig. 20 shows that the second polymer adhesive J3 is sprayed thinly so as not to block the gaps in the mesh. Note that the spider web-like second polymer adhesive J3 itself has a filter function that captures relatively large-diameter pollen and P2.5. As shown in Figure 12, the equipment configuration for the [second polymer adhesive spraying process L] is located between the [cooling process K] and the [nanofiber generation process M] of the first polymer adhesive, and the nozzle is basically the same as that for the [mesh reinforcing fiber formation process], and the second polymer adhesive J3 is sprayed onto the mesh surface of the polypropylene (or polyethylene) surface base material J1 and the first polymer adhesive J2.

[0058] This second fibrous polymer adhesive J3 is a polyurethane hot melt adhesive (moisture curing type) (PUR reactive hot melt (product number) No. 701.1 or 701.2) manufactured by KLEIBERIT JAPAN CO., LTD., and its physical properties are as shown in the following [Table 6]. In this example, UR reactive hot melt (product number) No. 701.2 was used. Similar results were also obtained with another second polymer adhesive J3, a polyurethane hot melt adhesive (moisture curing type) manufactured by Henkel Corporation, product number LA7575UV, which is a non-yellowing discoloration type (transparent or white). [Table 6] (B) PUR reactive hot melt (product number) No. 701.1 Main component: Polyurethane viscosity 80℃: 12,000 mPas 100℃: 4,000 mPas 120℃: 2,000 mPas Open time:>1hour Green Intensity: Strong Features: Low-temperature coating, no stringiness, hydrolysis resistance (C) PUR reactive hot melt (product number) No. 701.2 Main component: Polyurethane Viscosity (at the time of manufacture) brookfield HBTD 10rpm 100℃ approx. 5,000±1,500mPas 120℃: Approx. 3,000±1,000mPas

[0059] The second polymer adhesive N3 was a PUR reactive hot melt (product number: No. 701.1 or 701.2). The selection criteria were: (1) Good adhesion is required between the nonwoven fabric surface of the surface substrate J1 and the reinforcing mesh surface substrate J1 formed by crosslinking the first polymer adhesive J2; (2) the ventilation space of the nonwoven fabric is not blocked and deformation such as stringiness is minimal; (3) it takes a long time for the surface to harden after the second polymer adhesive N3 is applied, and the nanofibers are applied using this relatively long time (3 minutes to 1 hour) until the surface hardens, thereby maintaining a long time for the surface substrate J1 and the nanofibers J4 to bond and harden; and (4) it is highly adhesive before hardening, so that the titanium oxide of the deodorant can easily adhere to the sprayed nanofibers J4 and the surface substrate J1. Therefore, any other polymer adhesive may be used as long as it satisfies these conditions and is capable of forming fibers with a fiber diameter of 500 nm to 10 μm. The nozzle device used is the same as that in the [net-like reinforcing fiber forming process], and only the polymer adhesive that is supplied is different. This second polymer adhesive J3 is an adhesive (second polymer adhesive J3) that bonds and fixes the first polymer adhesive J2 and the nanofibers J4 to the surface substrate J1, and has stronger adhesive properties, making it suitable for bonding the nanofiber laminate J4 to the surface substrate J1. Furthermore, this second polymer adhesive J3 does not need to be heated and hardens gradually at room temperature, so it does not alter the nanofiber laminate J4. The reason why the fiber-like second polymer adhesive J3 forms a spider web-like or zigzag-like mesh in the spaces of the mesh of the surface substrate J1, etc., is to reduce blockage of the spaces formed by the nanofiber laminate J4. This is different from reducing the spaces on the surface of the nonwoven fabric of the surface substrate J1, because it would not only increase the weight of the shielding member but would also result in the disadvantage of a higher light-blocking rate.

[0060] In this way, when forming the adhesive of the second fibrous polymer adhesive J3, it is important to make the fibers thin enough so as not to block the space formed by the nanofibers J4, and it is preferable to use fibers as thin as possible, since using an adhesive that spreads into a film would defeat the purpose of using the nanofibers J4. In Example 2, it is important that the second polymer adhesive J3 is made of fibers with a fiber diameter of 500 nm to 10 μm, and is sprayed thinly onto the reinforced surface base material so as not to block the gaps, and to make it easy to shrink. In short, it is an absolute requirement that the first polymer adhesive J2 and the second polymer adhesive J3 form thin fibers, but in particular, it is desirable for the first polymer adhesive J2 to fill the spaces in the mesh and harden instantly while retaining its adhesive function and maintaining its fibrous shape, while conversely, it is desirable for the second polymer adhesive J3 to enhance the function of adhering the surface substrate J1 or the first polymer adhesive J2 to the nanofiber laminate J4, maintain a sufficient adhesive time, and harden relatively slowly. Example 2 is also configured to travel a sufficiently long distance before being wound up, as shown in Figure 12. That is, in Example 2, the distance from the reticulate reinforcing fiber forming section 92 to the nanofiber laminate take-up section 95 was 10 to 20 m, and the moving speed of the surface base material J1 was 90 mm / 120 sec to 90 mm / 60 sec, whereas in Example 2, the distance from the adhesive supply section 24 to the nanofiber laminate take-up section 7 was 15 m, and the moving speed of the surface base material J1 was 90 mm / 90 sec, allowing enough time for the second fibrous polymer adhesive J3 to slowly harden. The above numerical value of 90 mm / 90 sec means that the surface base material J1 moves a vertical distance of 90 mm over 90 seconds, and the nozzle tip also traverses a width of 1 m.

[0061] As described above, the first polymer adhesive J2 supplied is changed to the second polymer adhesive J3, and the structure of the nozzle itself and the setting conditions for the first polymer adhesive J2 are as shown in Figure 15. However, since the structure itself is the same as the nozzle portion 922 and air blowing nozzle portion 9261 in Figures 14 and 15, and the spraying portion 921 for the first polymer adhesive, a description thereof will be omitted. Regarding the thickness of the fibers of the first polymer adhesive J2 and the second polymer adhesive J3, the first polymer adhesive J1 is quick-drying and quickly solidifies, so the thickness can be measured. In Example 2, the thickness of the first polymer adhesive J2 + the second polymer adhesive J3 is 80 μm, and the basis weight is 47 g / m 2 The second polymer adhesive J3 has low viscosity, and the combined thickness of the first polymer adhesive J2 and the second polymer adhesive J3 is difficult to measure accurately because they have seeped into each other, but as a whole it is an extremely thin layer, as shown in Figure 20. Note that Figure 20 is a micrograph at 50x magnification of the state in which the first and second polymer adhesives (J2+J3) have been sprayed onto the surface substrate J1.

[0062] [Nanofiber production process M] The nanofiber production process M mainly comprises a nanofiber generation process M1 and a nanofiber collection process M2. [Nanofiber generation process M1] FIG. 20 is a micrograph showing the state of surface base material J1+first polymer adhesive J2+second polymer adhesive J3 after the [second polymer adhesive spraying step L] is completed. In the nanofiber production section M1, the produced polyvinylidene fluoride (PVDF) nanofibers J4 are sprayed and laminated. This process is the same as the configuration of the material liquid supply section 1, spinning section 2, and spray section 3 in the nanofiber production process A in FIG. 1 of Example 1, so The explanation of the material liquid supply section 1, the spinning section 2 and the spraying section 3 will be omitted. The composition of the spinning solution in Example 2 is as shown in [Table 7] below, and is the same as that in [Table 1] in Example 1. [Table 7] Composition of polyvinylidene fluoride (PVDF) spinning solution N1 Polyvinylidene fluoride (PVDF) 13.00% by weight N-Methyl-2-pyrrolidone (NMP) 85.15% by weight Toluene: 1.00% by weight. Carbon black particles: 0.85% by weight Total 100.00% by weight Here too, the carbon black particles used had a diameter of 20 nm. [Nanofiber collection process M2] In addition, the nanofiber collection process M2 corresponds to the laminate collection section 3 of [Nanofiber generation process A] in Figure 1 of Example 1, but in Example 2, the nanofiber laminate J4 is reinforced with a surface substrate J1, so as shown in Figure 12, it is basically sufficient to provide a flatness maintaining grid (or wire mesh) 37 and a suction duct 362 on the back side where the nanofibers J4 are sprayed, and the function is the same as in Example 1.

[0063] [Deodorant attachment process N] In the nanofiber collecting process M2, before the second fiber-shaped polymer adhesive J3 of the nanofiber laminate produced is completely cured, titanium oxide is attached to the nanofiber laminate. Conventionally, zinc oxide was kneaded into polyvinylidene fluoride (PVDF), but since it is attached near the surface of the fiber, it also has a deodorizing effect. In addition, when light is irradiated to titanium oxide near the nanofiber surface, active oxygen such as OH radicals is generated, and this OH radical has a much stronger oxidizing power than chlorine, hypochlorous acid, hydrogen peroxide, ozone, etc., and it can be understood that it can safely decompose chemical substances that are difficult to decompose by its oxidizing power, and it is expected to have a deodorizing effect better than conventional zinc oxide, and since titanium oxide is attached and fixed to the front and back surfaces of the laminate J4, the deodorizing effect is further enhanced. This deodorant attachment unit 96 will be explained with reference to Figure 12. Compressed air 965 is sent into a pressurized tank 963 storing a deodorant liquid in which 1 to 5% titanium oxide is dissolved in water, and the titanium oxide solution is sprayed from the pressurized tank 963 through a spray supply pipe 964 from a deodorant spray 961 onto the nanofiber laminate J4. The specific composition of this deodorant liquid is as follows: Deodorizer (odor absorbing agent): Titanium oxide 4.4 wt / % (% of total weight: w / w%) Pure water: 95.6wt / % This deodorant spray 961 uses a spray drive device 962 to evenly spray the titanium oxide solution onto the front and back surfaces of the nanofiber laminate J4, and then transports it to the next nanofiber winding process O.

[0064] Here, the deodorizing performance of the nanofiber laminate J5 after the deodorant attachment step N was measured and the results are shown in the following [Table 8]. First, the ammonia gas removal performance evaluation test was conducted by the Kaken Test Center, a general incorporated foundation, following the method stipulated in the SEK Mark Textile Product Certification Standards (Japan Textile Evaluation Technology Council). However, the amount of samples was "90 sheets of 10cm x 10cm + 10 sheets of 10cm x 3cm", the type of bag used was Smart Bag PA (manufactured by GL Sciences), and the test conditions for the ammonia gas removal performance evaluation test were as follows: In an atmosphere of a given volume (200ml) with the same initial concentration of ammonia gas of 100ppm, the amount of sample in this example was left for 2 hours, and the gas concentrations were compared as shown in [Table 8] below, with the same amount of sample as in the present example, and with the same amount of sample as in the conventional example and comparative example (blank test) left for 2 hours. [Table 8] Ammonia gas removal performance evaluation test Test sample Initial concentration (ppm) Gas concentration after 2 hours (ppm) Decrease rate (%) Example 1 100 1.0 ≧99 Conventional example (zinc oxide mixed in) 100 15 81 Comparative Example (Blank) 100 80 --- As described above, the ammonia gas concentration was reduced by 99% compared to an empty environment, which is a significant effect compared to the 81% reduction achieved with the conventional nanofiber laminate mixed with zinc oxide.

[0065] Next, a hydrogen sulfide gas removal performance evaluation test was conducted, which was carried out by applying the method stipulated in the SEK Mark Textile Product Certification Standard (Japan Textile Evaluation Technology Council, Inc.) and was requested to be carried out by the Kaken Test Center, a general incorporated foundation. However, the amount of samples was "90 pieces of 10cm x 10cm + 10 pieces of 10cm x 3cm", the type of bag used was Smart Bag PA (manufactured by GL Sciences, Inc.), and the test conditions for the hydrogen sulfide gas removal performance evaluation test were as follows: In an atmosphere of a specified volume (200 ml) with the same hydrogen sulfide gas initial concentration of 4.0 ppm, the amount of sample in this example was left in the atmosphere, and in a comparative example (blank test) with no sample, and the gas concentrations were compared for two hours, as shown in Table 9 below. [Table 9] Ammonia gas removal performance evaluation test Test sample Initial concentration (ppm) Gas concentration after 2 hours (ppm) Decrease rate (%) Example 1 4.0 ≦ 0.05 ≧ 99 Comparative Example (Blank) 4.0 4.0 --- As can be seen from the above, the concentration of hydrogen sulfide gas is reduced by 99% compared to an empty sky, demonstrating a remarkable effect. [Intermediate product winding process O] The intermediate product of the nanofiber laminate J5 that has passed through the deodorant attachment process N is transported by a feed roller or the like, if necessary, via a drying device such as a blower, and is then wound up as a lot 951 (95A) in the intermediate product winding section 95. At this time, the rotating shaft of the product winding roll 951 in the intermediate product winding section 5 is temporarily wound up as an intermediate product by a winding drive motor 953 at a constant tension via a powder clutch or the like.

[0066] [Process for forming the final product, nanofiber filter laminate] As shown in Figure 13, the process of forming a nanofiber filter laminate consists of an intermediate product unwinding process P, a two-ply combining process Q, a cleaning process R, and a final product winding process. [Intermediate product delivery process P] In FIG. 13, two lots 971 (95A) of the nanofiber laminate J5, which is an intermediate product of the winding device 5 in FIG. 12, are set in the supply device 971 of the upper and lower payout processes P in FIG. 13, and the lot 95A set in the supply device 971 is transported by a drive device 972 with a powder clutch and a feed roller 983, during which the lots are combined by a pressure roller 984 so that the surface on which the surface base material J1 is exposed faces outward, and are sent to the next combining process Q in which two sheets are superimposed. [Combining process Q] In this combining step Q, the surface substrate J1 is combined with a heating and pressurizing roller 984 so that the 20-mesh monofilament net of the surface substrate J1 is exposed on the outer surface to increase its strength, and is then transferred to the next washing step R. [Cleaning process R] In Example 2, the combined nanofiber filaments are sent to a cleaning process, in which excess carbon black particles and dust are washed away and removed with water from a cleaning solution. The cleaning device 4 in this [cleaning step] specific step is almost the same as that in the first embodiment, so a detailed description thereof will be omitted. After passing through this [washing process], the washed nanofibers J7 are dried using a drying device or the like to remove the washing liquid as necessary, and the final product is sent to the [final product winding process S] to be wound up. [Final product winding process S] The nanofiber filter laminate, which is the final product, is wound up in a final product winding process S, and the nanofiber filter laminate J7 is wound up by a winding device 98 using a driving device 982 to form a winding lot 981 (98A). A cross section of this J7 is shown in Figure 18. The front and back surface substrates J1 are monofilament plain woven meshes, and nanofiber laminates J5 are bonded to both surfaces via a first polymer adhesive J2 and a second polymer adhesive J3. The winding device 98 has substantially the same configuration as the winding section 5 in the winding process E of the intermediate product, which is the nanofiber laminate N5 in Example 1, and the winding process O of the intermediate product in Example 2, so a detailed description will be omitted. Thus, the final product, lot 981 (98A) of nanofiber filter laminate J7, is rewound and cut as necessary to be processed into masks or the like.

[0067] [Examples of use in mask products] The nanofiber filter laminate J5 of Example 2 can also be used for building materials such as window screens, but in terms of its use as a mask, in addition to the use example in Example 1, Use Example 3 is possible, as shown in Figure 18. This is based on the fact that the 20 mesh of Example 2 has excellent shape retention and can be used to make a three-dimensional mask. It is used as a mesh surface base material J7 (98A) for a mask, cut to fit the bridge of the nose and welded, and rubber strings or elastic bodies 87 are pressure welded to both sides. Since gaps are created on both sides of the nose, soft cloth is attached to fill these gaps and provide gap closing members 89.

[0068] FIG. 20 shows an electron microscope photograph at 50x magnification of the nanofiber laminate J3 produced in FIG. 12 of Example 2, which shows that the first polymer adhesive J2 and the second polymer adhesive J3 have become fibrous and are entangled with the mesh surface base material J1. Next, the performance will be explained based on tests, showing the test results of the fine particle capture rate and pressure loss of a nanofiber filter laminate made by stacking one 20-mesh filter used in a mask and two 20-mesh filters from Example 2 with the mesh sides facing outwards. [Test Results] (1) [Particle collection rate] (1-1) Here, the effects of fine particle collection efficiency and capture rate are shown by comparing the nanofiber filter laminate J7 in FIG. 18 of Example 2, in which carbon black fine particles are kneaded, with a conventional commercially available nanofiber filter laminate. [Table 10] Specifications of nanofiber filter laminate J7 of Example 2 Mask area: 13cm x 20cm Thickness 0.5mm Minimum collection particle 0.3μm Particle collection efficiency: 99.9% or more Pressure loss (85L / min) 4Pa Comparative Example 1 A mask made of nanofiber filter laminate from company A Pressure loss (85L / min) 150Pa As shown above, at the particle collection efficiency required for a mask, the pressure loss is orders of magnitude lower and breathability is very minimal.

[0069] Example 3 In Example 3, manganese oxide was used as the adsorbent in the spinning dope instead of the carbon black fine particles used in Example 2. This was done to obtain a white nanofiber laminate and nanofiber filter laminate with an increased collection rate, since the finished nanofiber laminate would inevitably turn black or gray if carbon black fine particles were mixed in. Next, the composition of the spinning solution in Example 3 is shown in Table 11. [Table 11] Composition of polyvinylidene fluoride (PVDF) spinning solution N1 Polyvinylidene fluoride (PVDF) 13.00% by weight N-Methyl-2-pyrrolidone (NMP) 85.30% by weight Toluene: 1.00% by weight. Manganese tetroxide fine particles: 0.70% by weight Total 100.00% by weight Here, the manganese tetroxide fine particles used were BLOWNOX X (manganese tetroxide, Mn3O4) manufactured by Tosoh Corporation and had a particle size of 0.5 μm to 10 μm. The apparatus was almost the same as that of Example 2, but when air was passed through the nanofiber laminate containing the carbon black fine particles of Example 2 and the nanofiber laminate containing the manganese compound of Example 3 and the static electricity was measured under the same conditions, the charge of the nanofiber laminate of Example 2 was 8.4 KV, whereas the charge of the nanofiber laminate of Example 3 was 9.3 to 9.5 KV. Therefore, the charged voltage of Example 3 was also high, and high dust collection capacity can be expected.

[0070] As described above in detail, Example 1 of the present invention has the characteristics that, despite its high collection efficiency, the air loss pressure is small and there is no stuffiness. The nanofiber layer can be easily made thicker as needed. By making the nanofiber layer thicker and particularly increasing the collection efficiency, it is possible to collect droplets of fine particulate matter PM2.5, viruses, and the like, and the nanofiber layer can be used as an industrial filter for window screens, ventilation fans, and the like. In addition, since the spinning method involves spraying nanofibers from a nozzle in the manufacturing process, carbon black particles or manganese oxide particles can be mixed into the spinning solution, and if the nozzle is made of stainless steel or ceramic, the central outlet is heat-resistant and durable with little deformation, so that even if the polymer fiber heated to a high temperature is spun for a long time, the nanofibers will not deform and a uniform nanofiber diameter can be maintained. Furthermore, the nanofiber layer has sufficient breathability and strength, and can be mass-produced at low cost. Furthermore, the nanofiber filter laminate for masks produced by the present invention can be safely produced as a nanofiber laminate made of polymeric materials with long molecular arrangements, such as polyvinylidene fluoride (PVDF), polyvinyl butyral (PVB), polyvinyl alcohol (PVA), polyurethane (PU), and polyamide polyamide (registered trademark; nylon). In particular, when the nanofiber material is polyvinylidene fluoride (PVDF), it is a resin that has excellent weather resistance and is resistant to radiation, and is therefore suitable as a filter for screen doors and ventilation fans that come into contact with the outdoors, as well as for agricultural greenhouses, and is easy to clean. Furthermore, if you attach a deodorant to a mask, it will have a deodorizing effect and can also be expected to have a sterilizing effect against bacteria, etc. In particular, according to Examples 2 and 3, the nanofiber filter laminate using a monofilament mesh as the surface substrate and the mask using the same do not come off even when washed because the carbon black fine powder or manganese compound is firmly mixed in the nanofiber spinning solution. Moreover, according to Example 3, a white nanofiber filter laminate with high dust collection efficiency can be produced. Furthermore, in Examples 2 and 3, a monofilament mesh was used for the surface substrate, and the monofilament was meshed, providing shape retention, and the nanofiber filter laminate had enough shape retention to stand on its own. In Example 2, two sheets were combined, making it easier to mold into a three-dimensional mask, and the mask was easy to cut and process, resulting in a higher collection efficiency and the ability to capture droplets of fine particulate matter PM2.5, viruses, etc. When these nanofiber filter laminates are used as filters for general-use masks, medical masks, and industrial dust masks, they can capture pollen, fine particulate matter PM2.5, and other dust and viruses, and are optimal for this purpose with little air pressure loss and little breathability. In addition, when used as filters for ventilation fan filters, screen doors, and agricultural greenhouses in places exposed to the outside air, if the nanofiber material is polyvinylidene fluoride (PVDF), it is a resin that has excellent weather resistance and is resistant to radiation, making it suitable as a building material for outdoor screen doors, agricultural greenhouses, and the like, and is easy to clean. Furthermore, the nanofiber layer has sufficient breathability and strength, and can be mass-produced at low cost. It goes without saying that the present invention is not limited to the above-mentioned embodiments as long as the characteristics of the present invention are not impaired. [Explanation of symbols]

[0071] A: Nanofiber production process, B: Capture layer formation process, C: Laminated body removal process, D: Cleaning process, E: Winding process of intermediate products, F: Forming process of the filter laminate, G: Winding process of the final product, H1...Upper non-woven fabric, H2...Lower non-woven fabric, H3: Upper mesh surface board, H4: Lower mesh surface board, N1: Nanofiber material liquid, N2: Nanofiber fiber, N3: Nanofiber laminate, N4: Detached nanofiber laminate N5: Nanofiber filter laminate after cleaning. N6: Nanofiber filter laminate with nonwoven fabric (net) on the top and bottom N8·· Mask product example 1, N8b·· Mask product example 2, H: Surface substrate feeding process, I: First polymer adhesive spraying process, K: Cooling process, L: Second polymer adhesive spraying process, M: Nanofiber production process, M1: Nanofiber generation process, M2: Nanofiber collection process, N: Deodorant attachment process, O: Rolling up the intermediate product, Q: The nanofiber filter laminate forming process. S: The final product winding process. J1...surface substrate, J2...first polymer adhesive, J3...second polymer adhesive, J4: Nanofiber laminate, J5: Nanofiber laminate, J6: The final product is a nanofiber laminate made by combining two sheets. J8·· Mask product example 3 1... Material liquid supply unit, 11... Material liquid tank, 12... Feed pump, 13...Transfer pipe, 14...Hot water insulation section, 141...Hot water distributor, 142 water heater, 143 pump, 144 hot water outlet, 145··Pipe, 146··Connecting hot water return port, 2... spinning section, 21... nanofiber spraying section, 22 nozzle portion, 221 nozzle body, 2211 central axial hole, 2212··Discharge port, 2213··Brim part, 222 nozzle support, 2221 inner hole, 2222 tip engaging portion, 2223: opening; 2224: outer periphery; 23... Polymer introduction pipe, supply port, 231... Outer periphery, 232... Injection air introduction groove, 234...Through hole, 24...Polymer supply section, 241...Polymer supply pipe, 26...High-speed air blowing section, 261...High-speed air blowing nozzle section, 262...High-speed wind outlet, 263...High-speed wind outlet, 27: Air injection passage forming cap; 272: Air introduction portion frame; 28... air supply unit, 281... air pump, 29··Infrared heating device, 291··Hood 3 laminate collection section, 31 collection zone, 32 drive roller, 33a,b,c··Driven support rollers; 34··Collection surface; 36··Suction mechanism, 361··Suction chamber, 362, 362a, b, c··Suction duct, 363a,b,c··Air volume adjustment shutter, 37. Grid (or wire mesh) for maintaining flatness 38: stacked body detachment portion, 381: blowing device, 3811: blowing nozzle, 382··Suction device; 3821··Suction nozzle; 383: endless belt; 384: drive roller; 385: guide roller; 4 cleaning device, 41 pinch roller 41, 42 guide roller, 43 cleaning tank, 44 roller group, 45 guide roller, 46 pinch roller, 47 drying device, 48 feed roller, 5··Product winding section, 51(5A)··Winding roll 5, 52 rotating shaft, 53 powder clutch, 54 winding drive motor, 55··Ultrasonic sensor for detecting winding diameter 6... feeding device, 61... driving device, 62... feed roller, 7...Nonwoven fabric attachment device, 71, 72...Nonwoven fabric supply device, 73 feed roller, 74 heating and pressure roller, 741 heating unit, 8 ·· Winding device, 81 (8A) ·· Winding rod, 82 ·· Drive device, 85 Mask base material, 86 Nose wire, 87 Rubber string (elastic body), 87b, 87c ·· Welded portion, 87 ·· Rubber string (elastic body), 88 ·· Pocket portion, 89... Gap sealing member, 91... Surface substrate supply unit, 911... Winding rod, 912... Feed roller, 913: guide roller; 914: tension adjustment mechanism; 92: Net-like reinforcing fiber forming section; 921: First polymer adhesive spraying section; 922: Nozzle part; 9221: Nozzle body (center nozzle); 92211...Central shaft hole, 92212...Discharge port, 92213...Brim part, 9222: Nozzle support; 92221: Inner hole; 92222: Tip locking portion; 92224...Outer periphery, 923: Molten resin introduction pipe, 9231: Outer periphery, 9232: Hot air introduction groove, 924: Supply unit; 9241: Supply pipe; 9242: Supply pump; 926: hot air blowing section, 9261: hot air blowing nozzle section, 9262: blowing passage, 9263··High-speed air outlet, 9264··Heater, 927··Heated air passage forming cap, 9272··Heated air introduction part frame, 9273··Fine adjustment washer, 928··Air pump, 9281 Heated air generator, 9282 Heated air supply pipe, 93... cooling device, 931... cooling plate, 932... heat insulating plate, 933... cooling mechanism, 934··Peltier device, 9341··N-type thermoelectric semiconductor, 9342 P-type thermoelectric semiconductor, 9343 Metal electrode, 9344 Insulating material, 9345...DC power supply, 95··Intermediate product winding section, 951(95A)··Rot, 953··Drive motor, 96··Deodorant attachment part, 961··Deodorant spray, 962··Spray drive device, 963 Pressurized tank, 964 Spray agent supply pipe, 965 Compressed air, 971(95A)··Feeding device, 983··Feed roller, 984 ·· Combining roller, 981 ·· Final product lot, 982 ·· Driving device,

Claims

1. A method for producing a nanofiber filter laminate, comprising: dissolving a polymeric material having a long molecular arrangement in a solvent; mixing carbon black fine particles having a diameter of 24 nm or less into the solvent to prepare a nanofiber spinning solution; pressurizing the spinning solution to spin fibers from a spinning nozzle; providing a ring-shaped high-speed blowing outlet coaxially with a central outlet of the spinning nozzle so as to surround the central outlet of the spinning nozzle; forming a nanofiber laminate in which the polymeric material from the spinning nozzle is stretched by an airflow from the high-speed blowing outlet and the solvent is vaporized; and washing the nanofiber laminate with water, methanol, or isopropyl alcohol to wash away excess carbon black fine particles.

2. The method for producing a nanofiber filter laminate according to claim 1, characterized in that the polymer material having a long molecular sequence is polyvinylidene fluoride (PVDF) and the solvent is selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), dimethylacetamide (DMAC), and dimethylsulfoxide (DMSO).

3. A method for producing a nanofiber filter laminate as described in claim 1 or 2, characterized in that a deodorizer attachment process is performed in which titanium oxide is attached before the polymer adhesive is completely hardened after forming the nanofiber laminate.

4. The method for producing a nanofiber filter laminate selected from those described in claims 1 to 3, characterized in that the method is used in producing masks for daily use, medical masks, and industrial dust masks, and both the front and back sides of the nanofiber laminate are supported by a nonwoven fabric, a cloth, or a plain weave mesh net.

Citation Information

Patent Citations

  • JP1975010788A

  • Anticharging textile and filter cloth

    JP1978053074A

  • Method for producing nanofiber

    JP2011127234A

  • Nanofiber laminated thin film shield member for building material, and manufacturing apparatus for the same

    JP2014047474A

  • Method for manufacturing nonwoven fabric substrate for air filter or mask

    JP2014114521A