Thermal insulation composition, thermal insulation article, and method for producing thermal insulation material

A low-density powder and water-soluble polymer solution mixture, freeze-dried to form a porous structure, addresses the bulkiness of conventional insulators, providing efficient and safe heat insulation for various applications.

JP7590773B2Active Publication Date: 2024-11-27OZONESAVE
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021207162
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-21
Publication Date
2024-11-27
Estimated Expiration
2041-12-21

AI Technical Summary

Technical Problem

Conventional heat-insulating materials are bulky, limiting transportation efficiency and storage efficiency, and are not suitable for fine structures due to their thickness and structural fragility.

Method used

A heat-insulating composition comprising a mixture of a low-density powder material and a water-soluble polymer solution in a specific ratio, which is freeze-dried to form a porous structure with excellent insulation properties.

Benefits of technology

The composition achieves reduced bulk with superior heat-insulating performance, suitable for fine structures and safe for applications requiring low solvent resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590773000001
    Figure 0007590773000001
  • Figure 0007590773000002
    Figure 0007590773000002
  • Figure 0007590773000003
    Figure 0007590773000003
Patent Text Reader

Abstract

To provide a heat insulator that has low bulk and high workability and is applicable even to microstructures.SOLUTION: A composition for heat insulation contains a low-density powder material containing at least one of porous powder and hollow powder, and a water-soluble polymer solution. A blending ratio of the low-density powder material and the water-soluble polymer solution is expressed by Va:Vb=1:2-1:5, where Va is volume of the water-soluble polymer solution and Vb is volume of the low-density powder material. There is also provided a heat insulator containing a lyophilizate of the heat insulator composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat insulating composition, a heat insulating article, and a method for producing a heat insulating material using the heat insulating composition. [Background technology]

[0002] In order to prevent deterioration of quality during transportation, refrigerated and frozen products such as medicines and food are usually transported in insulated containers, such as polystyrene foam containers or cardboard boxes with insulating materials such as urethane foam, when not in refrigerated or frozen conditions (e.g., Patent Document 1).

[0003] Such insulated containers are bulky compared to the products they contain, which increases the cost of transporting the products. In addition, it is necessary to prepare an insulated container separate from the product itself to store and pack the product, which makes the transport process complicated.

[0004] On the other hand, there are many situations where a container that can keep a product at a high temperature for a relatively long time is required. Usually, such a container is required not to have a high temperature outside during use, and at the same time, in many cases, it is required that the user can touch it with bare hands. As such a container, containers made of bulky materials such as polystyrene foam, and paper containers having a laminated structure on the side wall are used to provide heat retention. As a paper container having a laminated structure on the side wall, for example, one having an air layer inside the laminated structure of the side wall is known, as in Patent Document 2. In any case, the overall volume is large compared to the internal volume, and the container itself requires a large space when transporting and storing.

[0005] In other fields, in the field of facilities (architecture, plants, vehicle bodies, etc.), a technique is known in which an insulating layer of a thermally foamable polymer or the like is provided on the back side of the substrate constituting the inner wall to improve the thermal insulation inside the substrate (e.g., Patent Document 3). However, conventional insulating layers need to have a certain thickness or more to provide a higher insulating effect, which causes problems such as limited internal volume and increased costs for transporting the substrate.

[0006] As mentioned above, most of the conventional insulation materials in various fields are bulky, which reduces the efficiency of transportation and storage. In addition, the materials used are limited to glass wool, insulation boards, urethane foam, polystyrene foam, etc., and due to their thickness and structural fragility, they are difficult to process and mold finely, so their applications are limited to box-shaped insulation containers and relatively large substrates.

[0007] In response to these problems, the inventors have provided an insulating paint containing a low-density powder material and a water-soluble polymer solution in a specified ratio as an insulating material that is less bulky than conventional materials, has excellent processability, and can be applied to fine structures, as well as an insulating method and insulating sheet material that use the insulating paint (see, for example, Patent Document 4). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 11-147577 [Patent Document 2] JP 2000-247377 A [Patent Document 3] Japanese Patent Application Publication No. 7-48881 [Patent Document 4] JP 2013-100406 A Summary of the Invention [Problem to be solved by the invention]

[0009] As described above, various excellent heat insulating materials are known, but if there were heat insulating materials formed from materials different from the above-mentioned known materials and having good heat insulating performance, this would be preferable as it would allow for a wide variety of products to be available.

[0010] Therefore, an object of the present invention is to provide a thermal insulation material which is excellent in processability, applicable to a microstructure, and has good thermal insulation performance. [Means for solving the problem]

[0011] As a result of extensive research, the inventors discovered that an insulating material with good insulating properties can be obtained by using a composition obtained by mixing a water-soluble polymer solution, which is mainly used as a water-soluble adhesive, with a low-density powder material in a specified ratio, and thus completed the present invention.

[0012] That is, the heat insulating composition of the present invention comprises a low-density powder material including at least one of a porous powder and a hollow powder, and a water-soluble polymer solution, and the mixing ratio of the low-density powder material to the water-soluble polymer solution is Va:Vb=1:2 to 1:5, where Va is the volume of the water-soluble polymer solution and Vb is the volume of the low-density powder material. The thermal insulation article of the present invention comprises a freeze-dried product of the above-mentioned thermal insulation composition.

[0013] The method for producing a thermal insulation material of the present invention includes a molding step of applying the above-mentioned thermal insulation composition to the surface of a base or pouring it into a mold, a freezing step of freezing the thermal insulation composition obtained by the molding step, and a vacuum drying step of vacuum drying the frozen thermal insulation composition obtained by the freezing step. Effect of the Invention

[0014] According to the heat insulating composition and the method for producing a heat insulating material of the present embodiment, a heat insulating material having excellent processability and good heat insulating performance can be provided. In addition, a heat insulating material having a reduced thickness can be provided, in which case a heat insulating material having a low bulk but good heat insulating properties can be provided.

[0015] According to the thermal insulation article of the present embodiment, since it contains the thermal insulation material of the present embodiment, it is possible to exhibit good thermal insulation performance. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a side cross-sectional view showing a schematic configuration of a heat-insulating container used in the examples. [Diagram 2] FIG. 2A is a side cross-sectional view and FIG. 2B is a plan view showing a schematic configuration of another heat-insulating container used in the examples. [Diagram 3] This is a diagram showing the thermal insulation container in FIG. 1 housing a temperature measuring device for high-temperature testing. [Figure 4] 1 is a graph showing changes in measurement temperature in Example 2 and Comparative Example 1. [Diagram 5] FIG. 3 is a diagram showing a temperature measuring device for low-temperature testing housed in the insulated container of FIG. 2. [Figure 6] 1 is a graph showing changes in measurement temperature in Example 2 and Comparative Example 2. [Figure 7] 1 is a graph showing changes in measurement temperature in Example 1 and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the heat insulating composition, the heat insulating article, and the method for producing a heat insulating material using the heat insulating composition of the present invention will be described in detail with reference to one embodiment each.

[0018] <Thermal insulation composition> The heat insulating composition of the present embodiment is a heat insulating composition comprising a low-density powder material containing at least one of a porous powder and a hollow powder, and a water-soluble polymer solution. Each component will be described below.

[0019] (Water-soluble polymer solution) In the present embodiment, the water-soluble polymer solution used is a solution in which purified water or the like is used as a solvent and a water-soluble polymer is dissolved in the solvent as a solute, which is different from the solution in which a polymer compound is dissolved in an organic solvent that has been used in the past for this type of solvent-based paint.

[0020] When silica, such as methyl silicate or critical drying gel, is added to purified water or an aqueous solution of polyvinyl alcohol (PVA) dissolved in purified water, the silica is held above the liquid surface and this state is maintained for more than one week. Therefore, the low-density powder material is unlikely to dissolve or be suspended in the water-soluble polymer solution. Therefore, by using the water-soluble polymer, the reduction in the heat insulating effect due to the collapse of the three-dimensional structure of the low-density powder material is suppressed.

[0021] In contrast, the present inventors have already confirmed that when a porous or hollow low-density powder material described below is mixed with an organic solvent, depending on the type of low-density powder material, the presence of silica such as methyl silicate or critical drying gel cannot be visually confirmed in the solvent (it becomes in a dissolved state (transparent)), and a paint produced by suspending the low-density powder material in an organic solvent does not exhibit a sufficient insulating effect (see Patent Document 4 above).

[0022] It has also been confirmed that when zeolite or calcium carbonate is used as a low-density powder and mixed with an organic solvent, the solvent is likely to penetrate into the powder, and the powder content must be reduced in order to prepare a heat insulating composition. The reason for this is unclear, but it is presumed that the solvent is likely to penetrate into the pores of the powder due to factors such as low surface tension. If the amount of low-density particles in the heat insulating composition is reduced, it becomes difficult to fully exert the heat insulating effect.

[0023] On the other hand, such a phenomenon is not observed in an aqueous PVA solution (5 to 20 mass %), and it is possible to mix with a sufficient amount of zeolite or calcium carbonate, making it possible to achieve a sufficient heat insulating effect.

[0024] In view of the above, it has already been found that in order to fully utilize the performance of an insulating composition containing a low-density powder, it is particularly suitable to use an aqueous solution (particularly the water-soluble polymer solution described below) rather than an organic solvent. In this embodiment, however, an insulating composition that can form a good insulating material in other forms has been found.

[0025] Examples of water-soluble polymers used in this embodiment include polyvinyl alcohol (PVA), polyvinyl acetate, starch, and aqueous urethane. In particular, polyvinyl alcohol is suitable for use because it has a wide range of high affinity for sheet materials such as paper, cloth, and nonwoven fabric, which will be described later, is easy to apply, and has a relatively short drying time after application.

[0026] When polyvinyl alcohol is used as the water-soluble polymer, it is preferable to use one having a molecular weight of 10,000 to 200,000, particularly 50,000 to 150,000. If the molecular weight is too low, it is difficult to form a stable coating film, and if the molecular weight is too high, it is difficult to prepare a desired aqueous solution.

[0027] The concentration of the water-soluble polymer in the water-soluble polymer solution is preferably from 0.5 to 50% by mass, more preferably from 0.5 to 10% by mass, and even more preferably from 0.5 to 5% by mass.

[0028] (Low density powder material) The low-density powder material used in this embodiment contains at least one of a porous powder and a hollow powder, and this low-density powder material is a main material for exerting the heat insulating effect of the heat insulating material. In this specification, the term "low-density powder" refers to a powder having a density of 0.5 g / cm under conditions of 25°C and 1 atmospheric pressure. 3 Less than 0.15g / cm 3 It refers to something that is less than.

[0029] The low-density powder material used in this embodiment may be, for example, a porous or hollow powder made of a known material such as silica, methyl silicate, alumina, silica-alumina, ceramic, zeolite, calcium carbonate, or zirconia.

[0030] In particular, aerogels obtained by drying methyl silicate monomer at normal pressure or critical drying can be preferably used because they can be easily produced at low density, can be relatively easily formed into porous or hollow structures at the nano level, and are not easily disintegrated in aqueous solutions.

[0031] It is preferable to use this low-density powder material having a thermal conductivity of 0.15 W / (m K) or less, particularly 0.1 W / (m K) or less, and even more particularly 0.06 to 0.018 W / (m K), regardless of the degree of porosity.

[0032] When a porous low-density powder is used as the low-density powder material, the porosity is preferably 50.0 to 99.8%, particularly preferably 70 to 99.8%, and further preferably 86 to 99.8%.

[0033] Regardless of the structure of the low-density powder material, the average particle size is preferably 2 to 25 μm, particularly 5 to 23 μm, and further preferably 8 to 17 μm. If the particle size of the low-density powder material contained in the composition is 25 μm or more, the dispersion state of the low-density powder material may not be maintained well when forming the heat insulating material, and if it is 2 μm or more, the amount of air contained in the heat insulating material may be reduced, and sufficient heat insulating effect may not be obtained.

[0034] Low density powder materials have a specific surface area of ​​400m 2 / g or more, especially 500-1000m 2 / g, and 600-1000m 2 It is preferable to use a material with a specific surface area of ​​0.1 mm or less and a specific density of 0.1 mm or less. By increasing the specific surface area, it is possible to increase the porosity when using porous powders, and to increase the amount of air contained within the particles when using hollow particles. In addition, by using a low-density powder material with a large specific surface area, it is possible to reduce the mass of the entire insulation material.

[0035] The heat insulating composition of this embodiment can be produced by mixing the water-soluble polymer solution and the low-density powder material in a volume ratio of 1:2 to 1:5, preferably 1:3 to 1:4. If the amount of low-density powder is too large, the fluidity is poor, making it difficult to form a heat insulating material by coating or pouring, and if the amount is too small, the heat insulating effect, which is the object of this embodiment, cannot be obtained sufficiently.

[0036] (Textile materials) In this embodiment, a fiber material may also be used. This fiber material is an optional component.

[0037] The fiber material is not particularly limited as long as it functions as a structural reinforcement material for the resulting heat insulating material, and both inorganic and organic fibers can be used. Examples of inorganic fibers include glass fibers, alumina fibers, ceramic fibers, and carbon fibers. Examples of organic fibers include resin fibers such as polyimide fibers and polyamide fibers. By including such fiber materials, the strength of the resulting heat insulating material can be improved.

[0038] The fiber material used here has, for example, a fiber diameter of preferably 1 to 5 μm, more preferably 3 to 5 μm, and a fiber length of preferably 1 to 5 mm, more preferably 3 to 5 mm. Note that the fiber diameter and length here are the arithmetic average values ​​of the fibers contained in the fiber material.

[0039] If the fiber diameter is too small, the fibers will be prone to aggregation, which may lead to an increase in the viscosity of the heat insulating composition and a decrease in film-formability. If the diameter is too large, the reinforcing effect will be reduced, and film-formability and heat resistance may be reduced, or a heat transfer path may be formed, increasing thermal conductivity and decreasing insulation properties.

[0040] Furthermore, if the fibers are too short, the reinforcing effect will be small, and there is a risk that the film-forming properties and heat resistance will be reduced. If the fibers are too long, they will be more likely to aggregate, which may increase the viscosity of the heat insulating composition and reduce the film-forming properties. In addition, a heat transfer path may be formed, which may increase the thermal conductivity and reduce the insulation properties.

[0041] The content of this fiber material is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, per 100 parts by mass of the low-density powder. If it exceeds 10 parts by mass, it becomes easy to aggregate, which may cause an increase in viscosity of the heat insulating composition and a decrease in film-forming ability, or a heat transfer path is formed, which increases thermal conductivity and decreases heat insulating ability, while if it is less than 1 part by mass, the reinforcing effect may not be fully exhibited.

[0042] As described above, the heat insulating composition in this embodiment can be obtained by mixing the above-mentioned low-density powder material and the water-soluble polymer solution in a predetermined ratio, and blending a fiber component as necessary. This heat insulating composition is used to form a heat insulating material by the method described below, and is usually prepared as a liquid composition.

[0043] The heat insulating composition obtained as a liquid composition can be formed into a heat insulating material, for example, by coating on a substrate or pouring into a mold, as described below.

[0044] The viscosity of the heat insulating composition is not particularly limited as long as it can form the heat insulating material into a desired shape. For example, when the heat insulating composition is used as a coating material, the viscosity is preferably 500 to 100,000 mPa·s, and the drying time when the coating film has a thickness of 10 μm and is naturally dried at room temperature is preferably 2 hours or less. By adopting such a constitution, the coating material can also be used as an adhesive. In this specification, "viscosity" refers to the viscosity at 25°C.

[0045] When the heat insulating composition of the present embodiment is used as a paint, it is preferable to apply the paint to the target article so that the paint layer has a thickness of 2 to 200 μm. Since this paint is a liquid aqueous solution, it can be easily applied even when the target article has a fine structure, and can impart a heat insulating effect. In this case, when the paint is applied to a sheet material so that the paint layer has a thickness of 2 to 200 μm, a heat insulating sheet material can be formed. This heat insulating sheet material can be used as a packaging material or attached to the target article, and can impart a heat insulating effect to the target article.

[0046] The heat insulating composition of the present embodiment contains at least one of a porous powder and a hollow powder as the low-density powder material. By containing such a powder in the heat insulating composition, air can be contained in the formed heat insulating material, and the internal air can provide a heat insulating effect.

[0047] In addition, the heat insulating composition of the present embodiment can reduce the overall mass of the paint by using such a low density powder. From this viewpoint, when using a porous powder, it is preferable to use particles with higher porosity and particles with a higher specific surface area.

[0048] In addition to the performance aspects described above, the heat insulating composition of the present embodiment can be obtained without using organic solvents, so there is no concern about its effects on the human body, and it can be applied to applications such as packaging for food and medicine, and building materials for housing. Furthermore, even if the coating material of the present embodiment is applied to a resin product or the like, it does not corrode the product and can provide good heat insulating effects. In other words, the heat insulating composition of the present embodiment is a composition that is advantageous in terms of safety and the environment.

[0049] <Insulation material manufacturing method> Next, a method for producing a thermal insulating material using the above-mentioned heat insulating composition will be described.

[0050] First, the heat insulating composition is applied to the surface of a substrate to which heat insulating properties are to be imparted, or poured into a mold for molding a heat insulating material, thereby forming the heat insulating composition into a heat insulating material shape (molding process).

[0051] In this molding step, when the coating is applied to the substrate, the thickness of the coating is not particularly limited, but is, for example, preferably from 2 to 200 μm, more preferably from 5 to 50 μm, and even more preferably from 5 to 25 μm.

[0052] Specifically, the viscosity of the heat insulating composition is preferably 500 to 100,000 mPa·s, and particularly preferably 10,000 to 30,000 mPa·s, because if the viscosity is too high or too low, it becomes difficult to form a coating layer of the above thickness.

[0053] In addition, when pouring into a mold, the mold to be used is not particularly limited as long as it can be molded into a desired shape. In this case, the viscosity of the heat insulating composition may be such that the composition can be sufficiently filled into the mold.

[0054] The above-mentioned base and mold are directly subjected to the freeze-drying step described below, and therefore, it is preferable that they are made of a material that will not cause problems during freezing. For example, a base and mold made of metal, resin, wood, etc. can be used.

[0055] Next, the heat insulating composition formed into a heat insulating material shape by coating or pouring is frozen by cooling (freezing step). This freezing is performed by cooling to a temperature at which the solvent of the water-soluble polymer solution freezes. The solvent is usually water, and it is preferable to cool to, for example, -5 to -80°C. At this time, it is preferable to cool rapidly, and for example, it is preferable to freeze so that the temperature passes through the maximum ice crystal formation zone (-5°C to -1°C) within 30 minutes. By freezing rapidly in this way, the low-density powder material can be maintained in a dispersed state, and the production efficiency of the heat insulating material can be improved.

[0056] The cooling causes ice crystals to form in the solvent. The ice crystals are obtained by first forming crystal nuclei and then growing these nuclei. At this time, it is preferable that the low-density powder material is frozen in a uniformly dispersed state.

[0057] Next, the frozen heat insulating composition is dried (vacuum dried) under reduced pressure (drying process). In this drying process, the frozen solvent (moisture) in the heat insulating composition is sublimated and removed from the heat insulating composition, and the low-density powder materials are bonded and bonded together by the water-soluble polymer. Then, the areas where the removed solvent (moisture) was present remain as spaces, resulting in a heat insulating material (freeze-dried body) with porous spaces between the low-density powder materials.

[0058] The drying step can be carried out under known conditions, and the frozen heat insulating composition is usually dried under reduced pressure at room temperature or with heating. For example, the temperature is set to room temperature to 60° C. under reduced pressure conditions of 4 to 100 Pa. The drying time can be appropriately adjusted depending on the surface area of ​​the heat insulating composition and the size of the structure, and may be set so as to achieve a desired dry state, and is preferably 1 minute to 48 hours, more preferably 4 hours to 36 hours, and even more preferably 18 hours to 30 hours.

[0059] The insulating material obtained in this manner has extremely good insulating performance because both the low-density powder material itself and the porous spaces corresponding to the removed moisture described above contribute to the insulating properties.

[0060] The heat insulating composition and the method for producing a heat insulating material of the present embodiment can be applied to articles having a fine structure or articles with low solvent resistance, and can impart a heat insulating effect to these articles as well.

[0061] <Thermal insulation items> The heat insulating article of the present embodiment includes a heat insulating material (freeze-dried body) obtained by freeze-drying the heat insulating composition described above as described above.

[0062] The insulating material obtained in this manner has, as described above, low-density powder material bound by water-soluble polymers, and has a porous structure that corresponds to the removed moisture, and has good insulating performance.

[0063] The insulating article may be entirely or partially composed of the insulating material. In general, the insulating material (lyophilized material) is included in a part of the insulating article by packaging or attaching the insulating material to a target article.

[0064] Examples of such insulating articles include an insulating container having an insulating material formed on the inner or outer periphery of the container, an insulating container having an inner container and an outer container with the insulating material between the inner container and the outer container, an insulating sheet having a laminated structure in which an insulating material of a predetermined thickness is formed on a sheet material, etc. The insulating material is preferably provided so as not to come into contact with the outside atmosphere.

[0065] For example, this insulating article can provide insulation to refrigerated or frozen products that have conventionally been stored in separate insulated containers for transport. Even when refrigerated or frozen products are stored in an insulated container, the bulk of the container can be reduced, improving transport efficiency.

[0066] It is also possible to manufacture a heat-retaining packaging container that is smaller in bulk than conventional containers relative to the volume of the contents.

[0067] Furthermore, for example, by applying the heat insulating composition of the present embodiment to the back surface of wallpaper for a house, a low-bulk heat insulating material can be provided on the back surface, thereby imparting heat insulation to the wall. EXAMPLES

[0068] The heat insulating composition of the present embodiment will be described in detail below with reference to examples. It is needless to say that the present invention is not limited to the description of these examples.

[0069] Example 1 A heat insulating composition 1 was prepared by uniformly mixing 100 mL of a 1% by mass polyvinyl alcohol (PVA) aqueous solution and 22.5 g (300 mL) of aerogel as a low-density powder using a mixer (mixing ratio (volume ratio) of water-soluble polymer solution: low-density powder = 1:3). Here, the low-density powder was silica powder (manufactured by Yingde City Elite Asia-Pacific Electronics Co., Ltd., product name: aerogel, density 0.0125 to 0.018 g / cm). 3 , average particle size 5μm, specific surface area 650m 2 The viscosity of the heat insulating composition 1 thus prepared was 10,000 mPa·s.

[0070] This insulating composition 1 was poured into the inner wall and inner bottom of a cylindrical container with a diameter of 5 cm, and into the inside of the lid of the cylindrical container, with a mold placed so that the thickness was 1 cm, to form a cylindrical container equipped with the insulating composition.

[0071] The composition was frozen in a freezer at -15°C for 2 days. The composition was then vacuum dried for 1 week at -0.1 MPa (gauge pressure) and room temperature to produce a thermal insulation container 1A having a thermal insulation material. Figure 1 shows a cross-sectional side view of the schematic configuration of this thermal insulation container.

[0072] Here, the insulated container 1A consists of a cylindrical container 3 formed with a thermal insulation material 2 and its lid 3a. When the lid is closed, the inside of the insulated container 1A becomes a space surrounded by the thermal insulation material 2.

[0073] Furthermore, the heat insulating composition 1 was placed in a mold having an inner dimension of 100 mm×100 mm×100 mm, and a cylinder having a diameter of 65 mm was placed in the center so as to be inserted from above to a depth of 75 mm.

[0074] This was cooled in a freezer at -15°C for 2 days to freeze the heat insulating composition. Thereafter, it was vacuum dried for 1 week under conditions of -0.1 MPa (gauge pressure) and room temperature, and the freeze-dried body obtained was taken out of the mold, and the cylindrical body was removed to produce a heat insulating container 1B consisting of only the heat insulating material having a cylindrical container part.

[0075] Here, as shown in FIG. 2, the heat-insulating container 1B is formed only from a heat-insulating material 2, and has a container portion that is open at the center of the upper portion.

[0076] Example 2 As in Example 1, 100 mL of a 1% by mass aqueous solution of polyvinyl alcohol (PVA) and 22.5 g (300 mL) of aerogel as a low-density powder were mixed, and 1 g of polyimide fiber was added and mixed uniformly using a mixer to prepare heat insulating composition 2 (the mixing ratio (volume ratio) was water-soluble polymer solution:low-density powder = 1:3). The polyimide fibers used herein had an average fiber length of 1 cm and an average fiber diameter of 12 μm.

[0077] This insulating composition 2 was poured into the inner wall and inner bottom of a cylindrical container with a diameter of 5 cm, and into the inside of the lid of the cylindrical container, with a mold placed so that the thickness was 2 cm, to form a cylindrical container of the same shape as Example 1 and equipped with the insulating composition.

[0078] The composition was frozen in a freezer at -15°C for 2 days. The composition was then vacuum dried for 1 week at -0.1 MPa (gauge pressure) and room temperature to produce an insulated container 2A having a heat insulating material. Figure 1 shows a cross-sectional side view of the schematic configuration of this insulated container.

[0079] Furthermore, the heat insulating composition 2 was placed in a container with inner dimensions of 100 mm×100 mm×100 mm, and a cylinder with a diameter of 65 mm was placed at the center from above to a depth of 75 mm.

[0080] This was cooled in a freezer at -15°C for 2 days to freeze the heat insulating composition. Thereafter, it was vacuum dried for 1 week under conditions of -0.1 MPa (gauge pressure) and room temperature, and the resulting freeze-dried material was taken out of the container, and the cylindrical body was removed to produce a heat insulating container 2B consisting only of a heat insulating material having a cylindrical container part.

[0081] Here, as shown in FIG. 2, the heat-insulating container 2B is formed only from the heat-insulating material 2, and has an opening in the center of the upper part thereof.

[0082] Comparative Example 1 As Comparative Example 1, a container C1 was prepared which was not provided with the insulating material of the above-mentioned insulated container 2A.

[0083] Comparative Example 2 As a comparative example 2, a heat insulating container C2B made of style foam (expanded polysteel) having the same shape as the heat insulating container 2B was prepared as a heat insulating material.

[0084] Comparative Example 3 As Comparative Example 3, a heat insulating composition C3 was prepared by the same procedure as in Example 1 above, except that the compounding ratio (volume ratio) of the polyvinyl alcohol (PVA) aqueous solution to the low-density powder was water-soluble polymer solution:low-density powder = 1:1.

[0085] Furthermore, a thermally insulated container C3B consisting only of a thermal insulating material having a cylindrical container portion was produced by the same procedure as in the production of the thermally insulated container 2B, except that the thermal insulating composition C3 was used.

[0086] <Test Example> [High temperature side test] A thermometer 51 was placed inside the insulated container 2A produced in Example 2, and the inside was sealed with a lid. The thermometer 51 was fixed to a base 52 so that the temperature of the internal atmosphere of the insulated container 2B could be measured (see FIG. 3).

[0087] This was heated from room temperature (23°C) to 136°C over 20 minutes using an autoclave (manufactured by Toho Giken Co., Ltd., product name: SUN-1500), and the heated state at 136°C was maintained for 20 minutes. Thereafter, the heated state was changed to just over 100°C, which was maintained for 20 minutes, and then the sample was cooled to room temperature and the temperature change was measured.

[0088] The results of the temperature change of the thermometer in the above test are shown in Fig. 4. In Fig. 4, the dashed line indicates Comparative Example 1 and the solid line indicates Example 2.

[0089] As can be seen from the results in Fig. 4, in Comparative Example 1, the temperature fluctuated in accordance with the heating temperature of the autoclave, whereas in the case of using the insulating material of Example 2, the temperature fluctuated more slowly in response to the heating temperature of the autoclave, and in particular, even when the material was returned to room temperature after being heated once, the heated state was maintained. From these results, it was found that the insulating material obtained using the insulating material composition of the present embodiment had good insulating performance.

[0090] [Low temperature test 1] A test frozen body with the periphery of a thermometer frozen was placed inside the insulated container 2B produced in Example 2 (see FIG. 5), which was then placed in a cooler box and the inside was sealed with a lid. FIG. 5 is a schematic diagram showing the state in which the test frozen body is placed inside the insulated container 2B. Here, a can container was used as the test frozen body, and water was poured into the can container, and frozen with a thermometer 51 placed in the center, forming ice 53 around the thermometer 51. This test frozen body was cylindrical with a diameter of 65 mm and a height of 75 mm. This was left at room temperature (23°C) and the temperature change was measured.

[0091] The results of the temperature change of the thermometer in the above test are shown in Fig. 6. In Fig. 6, the dashed line indicates Comparative Example 2 and the solid line indicates Example 2.

[0092] As can be seen from the results in Fig. 6, in Comparative Example 2, it took about 22:29 for the ice to melt and about 46 hours and 22 minutes for the temperature to change to room temperature, whereas in Example 2, it took about 31 hours and 22 minutes for the ice to melt and about 50 hours and 22 minutes for the temperature to change to room temperature. Between Example 2 and Comparative Example 2, the difference in time until the ice melted was about 8 hours and 53 minutes, and the difference in time until the temperature changed to room temperature was about 4 hours, and it was found that the heat insulating material of this example has better heat insulating performance than the conventionally known heat insulating materials.

[0093] [Low temperature test 2] As in the above-mentioned low-temperature side test 1, a test frozen body was placed in the center of the insulated container C3B obtained in Comparative Example 3 and the above-mentioned insulated container 1B, and these were then placed in a cooler box and a lid was placed on it to seal the inside.

[0094] This was left at room temperature (23° C.) and the temperature change was measured. The results are shown in Fig. 7. In Fig. 7, the dashed line shows Comparative Example 3 and the solid line shows Example 1.

[0095] As can be seen from the results in Fig. 7, it took about 29 hours and 20 minutes for the ice to melt in Comparative Example 3, whereas it took about 30 hours and 48 minutes for the ice to melt in Example 1. The difference in time it took for the ice to melt between Example 1 and Comparative Example 3 was about 1 hour and 28 minutes, which shows that the insulating material of this example has better insulating performance than the insulating material of the comparative example.

[0096] In Comparative Example 3, since the proportion of PVA was relatively high, the fluidity of the resin composition was good, but the processability of the freeze-dried product was inferior to that of Example 1. On the other hand, the heat-insulating container of Example 1 had good processability and high heat-insulating performance.

[0097] From the above, it was found that the insulating article using the insulating composition shown in this embodiment has extremely good insulating performance, is easy to manufacture, and is an excellent product.

[0098] The invention made by the inventor has been specifically described above based on the embodiment and examples. However, the present invention is not limited to the above embodiment or examples, and it goes without saying that various modifications can be made without departing from the gist of the invention. [Industrial Applicability]

[0099] The heat insulating composition, heat insulating article, and heat insulating material manufacturing method according to the present embodiment can be applied in a wide range of fields, such as temperature control in fields requiring consideration of safety and the environment, such as pharmaceuticals (including vaccines), food, and construction, and heat countermeasures for electrical components, such as electronic circuit boards, infrared sensors, and magnetic sensors. [Explanation of symbols]

[0100] 1A, 1B...insulating container, 2...insulating material, 3...container, 3a...lid, 51...thermometer, 52...base, 53...ice

Claims

1. A low-density powder material including at least one of a porous powder and a hollow powder, and a water-soluble polymer solution, a mixing ratio of the low-density powder material to the water-soluble polymer solution is Va:Vb=1:2 to 1:5, where Va is the volume of the water-soluble polymer solution and Vb is the volume of the low-density powder material; The low-density powder material has an average particle size of 2 to 25 μm and a specific surface area of ​​400 m 2 / g or more; Here, the low density powder is a powder having a density of less than 0.5 g / cm 3 under conditions of 25° C. and 1 atmospheric pressure.

2. The heat insulating composition according to claim 1, wherein the water-soluble polymer solution contains at least one water-soluble polymer selected from the group consisting of polyvinyl alcohol, polyvinyl acetate, starch, and aqueous urethane, and the concentration of the water-soluble polymer is 0.5 to 50 mass%.

3. The heat insulating composition described in claim 1 or 2, having a viscosity of 500 to 100,000 mPa·s at 25°C.

4. The heat insulating composition according to any one of claims 1 to 3, further comprising a fibrous material.

5. The insulating composition described in claim 4, wherein the fibrous material is at least one of glass fiber, alumina fiber, ceramic fiber, carbon fiber, polyimide fiber, and polyamide fiber.

6. 6. The heat insulating composition according to claim 4, wherein the fiber material is contained in an amount of 1 to 10 parts by mass per 100 parts by mass of the low-density powder material.

7. A heat insulating article comprising a freeze-dried product of the heat insulating composition according to any one of claims 1 to 6.

8. A molding step of applying the heat insulating composition according to any one of claims 1 to 6 onto a surface of a substrate or pouring the composition into a mold; a freezing step of freezing the heat insulating composition obtained by the molding step; a vacuum drying step of vacuum drying the frozen heat insulating composition obtained by the freezing step; A method for producing a heat insulating material having the above structure.

Citation Information

Patent Citations

  • Heat insulation execution method for building and heat insulation material used threfor

    JP1995048881A

  • Thermal transfer image receiving body and thermal transfer recording method

    JP1998129128A

  • Carrying container for fresh food

    JP1999147577A

  • Heat-retentive and heat-insulating container

    JP2000247377A

  • Thermosensitive transfer image receiving sheet

    JP2008030311A