Soundproofing material and its manufacturing method
A transparent fire-resistant sound-insulating material using recycled rubber and sodium silicate enhances soundproofing and fire resistance, offering flexible application and improved adhesion, addressing the limitations of existing materials.
Patent Information
- Application Number
- JP2022526851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-05
- Filing Date
- 2020-05-26
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-05-26
AI Technical Summary
Existing soundproofing materials suffer from low soundproofing capacity and low fire resistance, with known materials exhibiting poor thermal insulation, high flammability, and low cohesiveness.
A transparent fire-resistant sound-insulating material composed of recycled rubber particles coated with carbon black, mixed with aqueous sodium silicate, water glass stabilizer, water glass hardener, and aluminum hydroxide, forming a flexible and pliable material with enhanced adhesion and flame retardancy.
The material achieves high non-flammability, heat resistance, excellent soundproofing, and antifungal properties, with good adhesion to surfaces and the ability to be applied in both solid and liquid forms, suitable for various applications including floors, ceilings, and hard-to-reach areas.
Abstract
Description
[Technical field]
[0001] The present invention relates to a soundproofing material, in particular a permeable fire-resistant soundproofing material comprising water glass and rubber, and a method for producing the same. [Background technology]
[0002] From the current state of the art it is known that a technical problem is to solve the recycling of used rubber, in particular used pneumatic tires.
[0003] Used tires are usually either disposed of as landfill or incinerated - neither of these methods are ecologically sound.
[0004] The use of recycled tires in the form of rubber granules is also known. These particles of various coarses are used, for example, in the automotive industry, where they are useful for the production of bumpers, seals and tires. They are also used in construction, as an additive to asphalt in road construction. Further applications include the preparation of surfaces for playgrounds and sports fields, at-grade crossings, the creation of safety thresholds in interlocking tiles or covers and grates, which are relatively resistant to chemical gritting and frost.
[0005] Additionally, there are materials which use bonded rubber particles, or particles of other plastic foam substances and organic polymer binders. This bond presents a number of drawbacks, among which are primarily related to flammability and instability.
[0006] From patent application CZ PV2017-127, a soundproofing and thermal insulation material for use in structures is known. 3 It consists of a slurry of an air-hardening mixture containing 5-76% by weight of bulk insulation material with a specific volumetric mass of less than 0.001-1 mm, 9-36% by weight of 0.001-1 mm brick dust fraction, 6-30% by weight of water glass, 7-30% by weight of water and up to 5% by weight of detergent. The disadvantages of this material are poor insulation properties, high flammability and poor cohesion.
[0007] Another patent application, CZ PV1990-2151, discloses a thermal insulation material with fire retardant properties, which contains an aqueous dispersion of a film-forming thermoplastic polymer, hydrosol silica, inert mineral fillers, silica excreted from ferroalloys, expanded volcanic water glass, a loose mixture of cork and rubber particles, and water, where the binder is a polymeric thermoplastic aqueous dispersion. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Czech Republic Patent Application No. CZ PV2017-127 [Patent Document 2] Czech Republic Patent Application No. CZ PV1990-2151 Summary of the Invention [Problem to be solved by the invention]
[0009] The disadvantages are low sound insulation capacity and mainly low fire resistance. From the above current technology, it is clear that the main disadvantages of the current technology are the low sound insulation properties of the known materials and the relatively low fire resistance.
[0010] The object of the present invention is the construction of a soundproofing material using recycled rubber and plastic waste, which has high fire resistance while at the same time being flexible and pliable and resistant to deterioration. [Means for solving the problem]
[0011] The above-mentioned disadvantages are largely eliminated, and the object of the present invention is achieved by a soundproofing material, in particular a permeable fire-resistant soundproofing material containing water glass and rubber, in particular recycled rubber. According to the present invention, the material is characterized in that it is made of a hardening compound containing 47-61% by weight of rubber particles, 30-50% by weight of aqueous sodium silicate, 0.1-0.5% by weight of a water glass stabilizer, 0.4-1.5% by weight of a water glass hardener, and 2-6% by weight of aluminum hydroxide, and the surface of the rubber particles is provided with carbon black constituting 0.1-1% by weight of the total weight. The advantage of the soundproofing material is its high incombustibility and heat resistance.
[0012] Another advantage is the very good permeability and antifungal effect. Thus, a major advantage is the very good adhesion to all surfaces and the excellent bonding and sealing effect. The main advantage is the very good soundproofing ability. The rubber particles can advantageously be replaced by another equivalent particle with the same or similar properties, for example plastic particles, the material of which is then, for example, foamed rubber. The advantage of using aluminum hydroxide is that it significantly improves the flame retardancy. The advantage of providing the surface of the rubber particles with carbon black is that the carbon black thus applied reduces the thermal conductivity and advantageously absorbs to a certain extent into the rubber particles, thereby stabilizing its bond with the rubber particles in the resulting mixture. A further advantage is that the carbon black acts as a flame retardant. Another advantage is that the carbon black acts as a retarder of the decomposition process due to solar irradiation. They capture the common oxygen free radicals and thus slow down the natural decomposition of the polymer. The water glass hardener may be glycerol mono- to triacetate or a mixture of these.
[0013] In an advantageous embodiment, the rubber particles are recycled. Advantageously, the recycled rubber particles can be replaced with other plastic foam materials, such as PUR and PIR foams and foamed rubber.
[0014] The stabilizer for the water glass is also preferably a hydrophilic alkoxyalkyl-ammonium salt.
[0015] Sodium silicate solution is 1370-1400kg / m 3 It is highly advantageous for the water glass to have a density in the range of 0.1 to 0.5, and a molar ratio of SiO2 to Na2O in the range of 3.2 to 3.4. The molar mass ratio of silicon oxide to sodium oxide and the associated solution density and solution concentration have a significant effect on the rheological properties of the water glass as a polymer mixture, its electrical properties in electrolytes, compressibility and adhesive strength, as well as hardness, strength, etc. The advantages of the above mentioned parameters are the sound insulation obtained. The material is partially flexible and pliable after curing.
[0016] The above-mentioned disadvantages are largely eliminated and the object of the present invention is achieved by a method for producing a soundproofing material, in particular a method for producing a permeable fire-resistant soundproofing material containing water glass and rubber. According to the present invention, the method is characterized in that first, rubber particles are mixed with an aqueous carbon black solution so that their entire surface is coated, then aluminum hydroxide is added and the whole is mixed to form a soundproofing mixture, then a water glass stabilizer is added to the aqueous sodium silicate solution, and then a water glass hardener is mixed into the solution. The solution is stirred for 1 to 10 minutes to form a binder solution, after which the soundproofing mixture is poured into the binder solution with constant stirring, and after further mixing, poured into the application site. The advantage is that it is possible to produce both solid products such as soundproofing panels and fittings, and the soundproofing material can be applied in its liquid state.
[0017] It is highly advantageous to preheat the binder solution to a temperature of about 65°C before adding the soundproofing mixture. At this temperature, weak interactions are formed between the water glass and the rubber, resulting in a strong bond with flexibility.
[0018] It is convenient to pour the resulting mixture into a mold, which is the application site, and then extrude a certain amount of binder solution from the resulting mixture by means of a press, so as to produce the desired ratio of soundproofing mixture and binder solution. The advantage of this is that it is possible to easily produce products with precise parameters.
[0019] It is also advantageous to finally leave the mixture obtained until it hardens, the advantage of which is that the obtained soundproofing material can be made precisely with respect to the geometric parameters of the soundproofing space: due to the fact that the hardening length can be regulated, the soundproofing material can be precisely molded to the desired shape.
[0020] The main advantage of the soundproofing material according to the invention and its manufacturing method is that it has significantly better soundproofing properties and higher fire resistance than previously known soundproofing materials using recycled rubber or recycled foamed materials, while it has vapor permeability, resistance to rainwater and moisture, antifungal properties, flexibility, resistance to external influences such as UV radiation, etc. Another advantage is the simple method of application. Both covering plates and fittings can be made from the soundproofing material, which can be easily applied as a liquid mixture by stretching, casting or spraying. The soundproofing material is therefore suitable for floors and ceilings, horizontal and slightly inclined roofs. The advantage is that sodium silicate after curing effectively reflects flames and has a negative heat of combustion, effectively reducing the burning of each mixture in which sodium silicate is present. It completely covers the rubber particles and protects them from fire.
[0021] Unlike soundproofing with mineral wool or polystyrene boards, it is conveniently applied in hard-to-reach places and on uneven edges of the surface. It has good adhesion to various substrates, including trapezoidal and folded sheets, eternit or asphalt, which are usually found on roofs. At the same time, the soundproofing material can be strong enough and even walkable. A great advantage of the soundproofing material according to the invention over existing materials is also the possibility of combining the board with a liquid mixture. One of the problems associated with the fastening of conventional polystyrene boards is the filling of the joints between the board and the holes around the dowels. Thanks to the possibility of filling these gaps and openings with the soundproofing material in liquid form, a uniform surface with no heat escape is created very simply and quickly. A great advantage is also that the semi-finished soundproofing material in the form of a liquid mixture can be applied as a soundproof lining in industry, for example in household appliances, electrical technology, automobiles, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Example 1
[0023] The permeable fire-resistant sound-proofing material is composed of a hardening mixture containing 54% by weight of recycled rubber particles, 40% by weight of aqueous sodium silicate, 0.3% by weight of water glass stabilizer, 4% by weight of aluminum hydroxide, and 1.2% by weight of water glass hardener.
[0024] The surface of the rubber particles is provided with carbon black, which constitutes 0.5% by weight of the total weight.
[0025] The waterglass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt in the form of a 98% aqueous solution of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine.
[0026] The density of sodium silicate solution is 1380 kg / m 3 and the molar ratio of SiO2 to Na2O is in the range of 3.3.
[0027] The waterglass hardener is a mixture of pure glycerol diacetate / triacetate in a ratio of 7:3 parts by volume, with a concentration of 3% by weight relative to pure waterglass.
[0028] According to the manufacturing method of the breathable flame-retardant soundproofing material, firstly, the rubber particles are mixed with an aqueous solution of carbon black with a concentration of 25% by weight, and the entire surface is coated with carbon black, then aluminum hydroxide is added, and the whole is mixed to form a soundproofing mixture, and the water glass stabilizer is added to the sodium silicate solution, and then the water glass hardener is mixed into this solution, and then the solution is stirred for 3 minutes to form a binder solution, which is preheated to 65°C, and the soundproofing mixture is further mixed into the binder solution, and the resulting mixture is poured into a silicone mold, and the resulting mixture is further extruded by pressing such an amount of binder solution that the desired ratio of the soundproofing mixture to the binder solution is obtained.
[0029] The resulting product is a soundproof board or fitting.
[0030] Example 2
[0031] The permeable fire-resistant soundproofing material is composed of a hardening mixture containing 61% by weight of recycled rubber particles, 30% by weight of aqueous sodium silicate, 0.1% by weight of water glass stabilizer, 6% by weight of aluminum hydroxide, and 1.5% by weight of water glass hardener.
[0032] The surface of the rubber particles is provided with carbon black, which constitutes 1% by weight of the total weight.
[0033] The waterglass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt in the form of a 98% aqueous solution of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine.
[0034] The density of sodium silicate solution is 1400 kg / m 3 and the molar ratio of SiO2 to Na20 is in the range of 3.4.
[0035] The waterglass hardener is a mixture of pure glycerol diacetate / triacetate in a ratio of 7:3 parts by volume, with a concentration of 5% by weight relative to pure waterglass.
[0036] According to the manufacturing method of the breathable flame-retardant soundproofing material, firstly, the rubber particles are mixed with an aqueous solution of carbon black with a concentration of 25% by weight, the entire surface is covered with carbon black, aluminum hydroxide is added, the whole is mixed to form a soundproofing mixture, water glass stabilizer is added to the sodium silicate solution, then water glass hardener is mixed into the solution, then the solution is stirred for 10 minutes to form a binder solution, which is preheated to 65°C, the soundproofing mixture is further mixed into the binder solution, and the resulting mixture is poured into a silicone mold, and the resulting mixture is further extruded by pressing such an amount of binder solution that the desired ratio of the soundproofing mixture to the binder solution is obtained.
[0037] Finally, the resulting mixture is left to set.
[0038] The resulting product is a soundproofing fixture.
[0039] Example 3
[0040] The permeable fire-resistant soundproofing material is composed of a hardening mixture containing 47% by weight of recycled rubber particles, 50% by weight of aqueous sodium silicate, 0.5% by weight of water glass stabilizer, 2% by weight of aluminum hydroxide, and 0.4% by weight of water glass hardener.
[0041] The surface of the rubber particles is provided with carbon black, which constitutes 0.1% by weight of the total weight.
[0042] The waterglass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt in the form of a 98% aqueous solution of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine.
[0043] The density of sodium silicate solution is 1370 kg / m3 and the molar ratio of SiO2 to Na2O is in the range of 3.2.
[0044] The waterglass hardener is a mixture of pure glycerol diacetate / triacetate in a ratio of 7:3 parts by volume, with a concentration of 0.8% by weight relative to pure waterglass.
[0045] According to the manufacturing method of the breathable flame-retardant soundproofing material, firstly, rubber particles are mixed with an aqueous solution of carbon black with a concentration of 25% by weight, the entire surface is coated with carbon black, aluminum hydroxide is added, and the whole is mixed to form a soundproofing mixture, water glass stabilizer is added to the sodium silicate solution, then water glass hardener is mixed into the solution, then the solution is stirred for 1 minute to form a binder solution, which is preheated to 65°C, the soundproofing mixture is further mixed into the binder solution, and then the resulting mixture is poured into the application site, which is a flat divided attic space, spread, surface-treated, and left to harden. [Industrial Applicability]
[0046] The soundproofing material according to the invention can in particular be used in the building industry to create transparent, fire-resistant soundproofing systems.
Claims
1. A soundproofing material comprising a curable mixture containing 47-61% by weight of rubber particles, 30-50% by weight of aqueous sodium silicate, 0.1-0.5% by weight of a water glass stabilizer, 0.4-1.5% by weight of a water glass hardener, and 2-6% by weight of aluminum hydroxide, the surface of the rubber particles being provided with carbon black constituting 0.1-1% by weight of the total weight.
2. 2. The soundproofing material according to claim 1, wherein the rubber particles are recycled.
3. 3. The soundproofing material according to claim 1, wherein the water glass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt.
4. The water glass stabilizer is added to the sodium silicate aqueous solution, The density of the sodium silicate aqueous solution is 1370 to 1400 kg / m 3 4. The soundproofing material according to claim 1, wherein the thickness of said soundproofing material is within the range of 0.1 to 0.5 mm.
5. The ratio of SiO to Na2O in the sodium silicate aqueous solution 2 The soundproofing material according to claim 4, characterized in that the molar ratio of is in the range of 3.2 to 3.
4.
6. The method for producing a soundproofing material according to any one of claims 1 to 5, characterized in that first, rubber particles are mixed with an aqueous carbon black solution to coat the entire surface thereof, then aluminum hydroxide is added to the aqueous carbon black solution, and the whole is mixed to form a soundproofing mixture, then a water glass stabilizer is added to an aqueous sodium silicate solution, then a water glass hardener is mixed into the solution, and the solution is stirred for another 1 to 10 minutes to form a binder solution, and the soundproofing mixture is added to the binder solution while constantly stirring, the whole is mixed, and the resulting mixture is then poured onto the application site.
7. 7. The method of claim 6, further comprising preheating the binder solution to a temperature of 65° C. before adding the soundproofing mixture.
8. 8. A method for producing a soundproofing material according to claim 6 or 7, characterized in that the mixture obtained is poured into the application site, which is a mould, and then from the mixture obtained, such an amount of binder solution is extruded by a pressing means so as to obtain a desired ratio of soundproofing mixture and binder solution.
9. 8. The method for producing a soundproofing material according to claim 6 or 7, further comprising the step of finally allowing the mixture to stand and harden.
Citation Information
Patent Citations
Modified rubber powder doped thermal-insulation wall building block and preparation method thereof
CN106242616A
CZPV1990-2151
CZPV2017-127
Rubber composition for tread, and tire
JP2007291178A
Curable composition and repair material
JP2018177595A