Thermal fixing device, electrophotographic image forming apparatus and laminated structure

A laminated structure with a specific silicon-to-carbon ratio in the intermediate layer enhances DLC film adhesion and thermal conductivity, addressing issues of adhesion and slidability in thermal fixing devices, ensuring stable and high-quality image formation.

JP7590911B2Active Publication Date: 2024-11-27CANON KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021072076
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-21
Filing Date
2021-04-21
Publication Date
2024-11-27
Estimated Expiration
2041-04-21

AI Technical Summary

Technical Problem

The adhesion of diamond-like carbon (DLC) films to the base material in thermal fixing devices is compromised by the surface roughness of the base material, leading to decreased thermal conductivity and slidability, which results in abnormal noise and poor fixing performance.

Method used

A laminated structure comprising a base material made of aluminum nitride, silicon nitride, or aluminum oxide, an intermediate layer of silicon carbide, and a DLC film with a specific silicon-to-carbon ratio, enhancing adhesion and thermal conductivity.

Benefits of technology

The laminated structure ensures stable heat fixing performance over time with improved adhesion of the DLC film, preventing peeling and maintaining slidability, thus ensuring high-quality electrophotographic image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590911000003
    Figure 0007590911000003
  • Figure 0007590911000004
    Figure 0007590911000004
  • Figure 0007590911000005
    Figure 0007590911000005
Patent Text Reader

Abstract

To provide a heat fixing device that has a long durable life.SOLUTION: A fixing device has a rotatable first member, a heater that heats the first member, and a rotatable second member. The heater is provided with a surface layer that is formed of a diamond-like carbon film, and a substrate that carries the surface layer with an intermediate layer including silicon carbide therebetween. The substrate includes at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon carbide. The ratio of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number of all elements excluding hydrogen atoms (A) in the intermediate layer [(Si)+(C)] / A is 0.8 or more, and the ratio of the number of the silicon atoms (Si) to the number of the carbon atoms (C) (Si) / (C) is larger than 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] SUMMARY The present disclosure is directed to thermal fusing devices, electrophotographic image forming devices and laminate structures. [Background technology]

[0002] Diamond-like carbon (DLC) is widely used as a surface coating for sliding parts due to its wear resistance, including sliding parts in electrophotographic image forming devices such as copiers and printers.

[0003] Patent Document 1 discloses a fixing device having a rotatable first member heated by a heat source, a rotatable second member that forms a nip portion between the first member and the second member and is capable of clamping a recording material, and a pressure member that is disposed inside the first member, has a contact surface with the inner surface of the first member, and presses the first member against the second member, wherein the surface layer of the pressure member that forms the contact surface with the inner surface of the first member is a specific diamond-like carbon film (hereinafter also referred to as a "DLC film"). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-34080 A Summary of the Invention [Problem to be solved by the invention]

[0005] According to the investigations of the present inventors, when the surface of the substrate constituting the pressure member arranged in contact with the inner circumferential surface of the first member facing the DLC film has large irregularities, when the pressure member is used as a heating member, the thermal contact between the inner circumferential surface of the fixing belt and the surface layer of the heater is poor, and the thermal conductivity of the heat from the heater to the first member may decrease.

[0006] On the other hand, when the surface of the substrate facing the DLC film is smoothed, the contact area between the DLC film and the substrate is reduced, and the adhesion of the DLC film to the substrate is reduced. As a result, during use of the fixing device, the DLC film may peel off from the substrate, and the sliding property between the first member and the pressure member may be reduced. The reduction in the sliding property between the first member and the pressure member may cause abnormal noise and poor fixing. Therefore, the present inventors recognized the need to develop a technology that can improve the adhesion of the DLC film to the substrate, regardless of the roughness of the substrate surface on which the DLC film is formed. [Means for solving the problem]

[0007] One aspect of the present disclosure is directed to providing a thermal fixing device that has excellent thermal transfer to a first member and can exhibit stable thermal fixing performance over a long period of time. Another aspect of the present disclosure is directed to providing an electrophotographic image forming apparatus that can stably form high-quality electrophotographic images. Still another aspect of the present disclosure is directed to providing a laminated structure that has excellent adhesion of a DLC film regardless of the smoothness of a substrate that is the adhesion surface.

[0008] According to one aspect of the present disclosure, a rotatable first member is provided. a heater for heating the first member; a rotatable second member that forms a nip portion capable of holding a recording material between the first member and the second member, The heater is a surface layer that constitutes a surface that slides against the inner circumferential surface of the first member; A substrate supporting the surface layer via an intermediate layer, The substrate comprises at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon nitride; The surface layer is made of a diamond-like carbon film, the intermediate layer comprises silicon carbide; the ratio of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements other than hydrogen atoms in the intermediate layer, [(Si)+(C)] / A, is 0.8 or more; and A thermal fixing apparatus is provided in which the ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) is greater than 1.

[0009] According to another aspect of the present disclosure, there is provided an electrophotographic image forming apparatus including a thermal fixing device that heats a toner image on a recording material to fix the toner image on the recording material, the thermal fixing device being the thermal fixing device described above.

[0010] According to another aspect of the present disclosure, there is provided a laminated structure having a substrate, an intermediate layer, and a diamond-like carbon film in this order, comprising: The substrate comprises at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon nitride; the intermediate layer comprises silicon carbide; The intermediate layer has a ratio of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements other than hydrogen atoms, [(Si)+(C)] / A, which is 0.8 or more, and a ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) greater than 1. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one aspect of a fixing belt-pressure roller type thermal fixing device according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view showing one aspect of a fixing belt-pressure belt type thermal fixing device according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a heater using a laminate structure according to an embodiment of the present disclosure. [Figure 4] 1 is a schematic cross-sectional view illustrating an example of an electrophotographic image forming apparatus according to an embodiment of the present disclosure. [Diagram 5] 1 is a schematic cross-sectional view showing an example of an intermediate layer forming apparatus for forming an intermediate layer in a laminated structure according to an embodiment of the present disclosure. [Figure 6]FIG. 2 is a schematic cross-sectional view showing an example of a diamond-like carbon film forming apparatus in a laminated structure according to an embodiment of the present disclosure. [Figure 7] 3 is a graph showing the bonding state of silicon atoms obtained as a result of analyzing the intermediate layer formed in Example 1 by XPS. [Figure 8] 2 is a graph showing the bonding state of carbon atoms obtained by analyzing the intermediate layer formed in Example 1 by XPS. [Figure 9] 4 is a graph showing the bonding state of silicon atoms obtained as a result of analyzing the intermediate layer formed in Comparative Example 1 by XPS. [Figure 10] 4 is a graph showing the results of a durability test of the thermal fixing device according to the present disclosure. [Figure 11] FIG. 2 is a schematic cross-sectional view of a laminated structure according to another embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Preferred embodiments of the present disclosure will be described in detail below with reference to the schematic drawings. Note that the present disclosure is not limited to the following embodiments, and can be implemented in various applications within the technical scope of the present disclosure.

[0013] A schematic cross-sectional view of an example of a fixing belt-pressure roller type thermal fixing device using a heater having a laminated structure according to an embodiment of the present disclosure is shown in Fig. 1. The thermal fixing device in Fig. 1 has a rotatable first member, a rotatable second member, and a heater that heats the first member.

[0014] The fixing belt 120, which is a first member, is sleeve-shaped and rotatable. The pressure roller 130, which is a second member, forms a nip portion N between the fixing belt 120 and the pressure roller 130, which can hold the recording material 141, and is rotatable. The heater 300, which is a heating member and also functions as a pressure member, is disposed inside the fixing belt 120, contacts the inner circumferential surface of the fixing belt 120, and presses the fixing belt. As the fixing belt 120 rotates, the inner circumferential surface of the fixing belt 120 and the surface layer of the heater 300 form surfaces that slide against each other.

[0015] The fixing belt 120 is composed of a sleeve-shaped stainless steel substrate, a silicone rubber layer coated on the outer circumferential surface thereof, and a fluororesin layer coated on the silicone rubber layer. An example of the fluororesin is a copolymer (hereinafter, also referred to as "PFA") of tetrafluoroethylene (hereinafter, referred to as "TFE") and perfluoroalkylvinylether (hereinafter, referred to as "PAVE"). An example of PAVE is perfluoromethylvinylether (CF 2 =CF-O-CF 3 ), perfluoroethyl vinyl ether (CF 2 =CF-O-CF 2 CF 3 ) and perfluoropropyl vinyl ether (CF 2 =CF-O-CF 2 CF 2 CF 3 Hereinafter, a specific example of the fluororesin constituting the fluororesin layer is similarly PFA.

[0016] The fixing belt 120 may have a resin film that forms the inner circumferential surface. The resin film that forms the inner circumferential surface preferably contains polyimide. The size of the fixing belt 120 is not particularly limited, but for example, the inner diameter is about 55 mm. When the inner diameter of the fixing belt 120 is about 55 mm, the thicknesses of the stainless steel base material, the silicone rubber layer, the fluororesin layer, and the polyimide film are, for example, 600 μm, 300 μm, 20 μm, and 1 to 20 μm, respectively.

[0017] The pressure roller 130 is composed of a stainless steel core 131, a silicone layer 132 coated on the outer circumferential surface thereof, and a fluororesin layer 133. The size of the pressure roller 130 is not particularly limited, but for example, the diameter is about 30 mm. When the diameter of the pressure roller 130 is about 30 mm, the thicknesses of the silicone layer 132 and the fluororesin layer 133 are, for example, 3 mm and 40 μm, respectively.

[0018] The heater 300 includes a laminated structure whose cross-sectional structure is shown in Fig. 3. The laminated structure includes a substrate 311, an intermediate layer 316, and a surface layer 315 made of a diamond-like carbon film (DLC film). The substrate 311 has a flat rectangular shape with its elongated direction being perpendicular to the conveying direction of the recording material 141 (the direction indicated by the arrow in FIG. 1) (the direction perpendicular to the paper surface).

[0019] The surface layer 315 of the heater 300 constitutes a surface that slides against the inner circumferential surface of the fixing belt 120. That is, the surface of the surface layer 315 opposite to the side facing the substrate 311 constitutes a surface that slides against the inner circumferential surface of the fixing belt 120. In addition, it is preferable to interpose a lubricant between the inner circumferential surface of the fixing belt 120 and the surface layer 315, because good sliding properties can be obtained between the inner circumferential surface of the fixing belt and the surface layer. Examples of the lubricant include fluorine-based grease using PFPE (perfluoropolyether) oil and PTFE (polytetrafluoroethylene) as a thickener, and silicone oil.

[0020] The heater 300 is held by a heater holder 111, which is supported by a reinforcing metal plate 112 having an inverted U-shaped cross section. That is, the heater holder 111 to which the heater 300 is fixed is supported by the reinforcing metal plate 112. The heater holder 111 may be made of, for example, a liquid crystal polymer resin having high heat resistance. Hereinafter, the heater 300, the heater holder 111, and the reinforcing metal plate 112 are also referred to as a heater unit 110.

[0021] The pressure roller 130 has both ends of a core metal 131 rotatably supported by a device frame (not shown). The pressure roller 130 is rotated at a predetermined speed by a motor (not shown) in the direction of the arrow in FIG. 1 while being pressed against the outer circumferential surface of the fixing belt 120.

[0022] The heater unit 110 has both ends of a reinforcing metal plate 112 fixed to an apparatus frame (not shown). The fixing belt 120 is fitted onto the heater unit 110, and the heater unit 110 is pressed against the inner circumferential surface of the fixing belt 120.

[0023] As a result, the fixing belt 120 rotates through the recording material 141 that is transported by the rotation of the pressure roller 130, and a nip portion N that sandwiches the recording material 141 is formed by the pressure roller 130, the fixing belt 120, and the heater 300. At this time, electricity is passed through the resistance heating element 312 of the heater 300 that slides against the inner circumferential surface of the fixing belt 120, so that the fixing belt 120 is heated at the sliding surface with the heater 300 and adjusted to a predetermined temperature.

[0024] 1 by the rotation of the pressure roller 130 and the fixing belt 120. At this time, unfixed toner 142 on the recording material 141 is heated by the heated fixing belt 120 as a heat source, and is fixed to the recording material 141.

[0025] The fixing belt-pressure roller type thermal fixing device is not limited to the form shown in Fig. 1. In the form shown in Fig. 1, the heater 300, which is a heating member, constitutes a part of the pressure member that presses the fixing belt 120 against the pressure roller 130, but the pressure member and the heating member may be separate members. In this case, the heater 300 is brought into contact with the inner circumferential surface of the fixing belt 120 at a position different from the position shown in Fig. 1 to heat the fixing belt 120. In this case, the laminated structure 1101 according to another embodiment of the present disclosure, which has a base material 311, an intermediate layer 316, and a diamond-like carbon film in this order, as shown in Fig. 11, can be used as the pressure member.

[0026] As another embodiment of the thermal fixing device of the present disclosure, a schematic cross-sectional view of an example of a fixing belt-pressure belt type thermal fixing device 200 is shown in Fig. 2. The thermal fixing device 200 shown in Fig. 2 is a so-called twin-belt type thermal fixing device in which a fixing belt 211 as a pair of rotatable first members and a pressure belt 212 as a pair of rotatable second members are in pressure contact with each other, and includes a heater 300 that heats the fixing belt 211.

[0027] In the thermal fixing device 200, a fixing belt 211 as a first member and a pressure belt 212 as a second member are stretched around two rollers. The fixing belt 211 and the pressure belt 212 are made of a flexible metal base material, for example, mainly made of nickel, a silicone rubber layer coated on the outer circumferential surface thereof, and a fluororesin layer coated on the silicone rubber layer. The fixing belt 211 may have a resin film that forms the inner circumferential surface. The resin film that forms the inner circumferential surface preferably contains polyimide. The sizes of the fixing belt 211 and the pressure belt 212 are not particularly limited, but for example, the diameter is 55 mm. When the diameter of the fixing belt 211 is 55 mm, the thicknesses of the flexible base material, the silicone rubber layer, the fluororesin layer, and the polyimide film are, for example, 600 μm, 300 μm, 20 μm, and 1 to 20 μm, respectively.

[0028] The heating member of the fixing belt 211 is a heater 300 having a laminated structure according to the present disclosure. As shown in Fig. 2, the heater 300 is disposed inside the fixing belt 211, contacts the inner circumferential surface of the fixing belt 211, and heats the fixing belt.

[0029] The surface temperature of fixing belt 211 is detected by temperature detection element 215 such as a thermistor, and a signal related to the temperature of fixing belt 211 detected by temperature detection element 215 is sent to control circuit section 216. Control circuit section 216 controls the power supplied to resistance heating element 312 so that the temperature information received from temperature detection element 215 is maintained at a predetermined fixing temperature, thereby adjusting the temperature of fixing belt 211 to the predetermined fixing temperature.

[0030] The fixing belt 211 is stretched around a roller 217 and a heating side roller 218, which serve as belt rotating members. The roller 217 and the heating side roller 218 are supported by bearings between left and right side plates (not shown) of the device so as to be freely rotatable.

[0031] Roller 217 is, for example, a hollow iron roller having an outer diameter of 20 mm, an inner diameter of 18 mm, and a thickness of 1 mm, and functions as a tension roller that applies tension to fixing belt 211. Heating side roller 218 is, for example, a highly slidable elastic roller having an outer diameter of 20 mm, an iron alloy core having a diameter of 18 mm, and a silicone rubber layer as an elastic layer provided on the core.

[0032] This heating side roller 218, as a drive roller, receives a driving force from a driving source (motor) D via a driving gear train (not shown), and is driven to rotate in the clockwise direction of the arrow at a predetermined speed. By providing the heating side roller 218 with an elastic layer as described above, the driving force input to the heating side roller 218 can be transmitted well to the fixing belt 211, and a fixing nip can be formed to ensure separation of the recording material 141 from the fixing belt 211. By providing the heating side roller 218 with an elastic layer, heat conduction to the heating side roller is also reduced, which is also effective in shortening the warm-up time.

[0033] When the heating side roller 218 is driven to rotate, the fixing belt 211 rotates together with the roller 217 due to friction between the silicone rubber surface of the heating side roller 218 and the inner surface of the fixing belt 211. The arrangement and size of the roller 217 and the heating side roller 218 are selected according to the size of the fixing belt 211. For example, the dimensions of the roller 217 and the heating side roller 218 are selected so that the fixing belt 211, which has an inner diameter of 55 mm when not attached, can be stretched over them.

[0034] The pressure belt 212 is stretched by a tension roller 219 and a pressure side roller 220, which serve as belt rotation members. The inner diameter of the pressure belt when not attached is, for example, 55 mm. The tension roller 219 and the pressure side roller 220 are supported by bearings that are freely rotatable between left and right side plates (not shown) of the device.

[0035] The tension roller 219 is, for example, an iron alloy core having an outer diameter of 20 mm and an inner diameter of 16 mm, on which a silicone sponge layer is provided to reduce heat conduction from the pressure belt 212. The pressure side roller 220 is, for example, an iron alloy low-sliding rigid roller having an outer diameter of 20 mm, an inner diameter of 16 mm, and a thickness of 2 mm. The dimensions of the tension roller 219 and the pressure side roller 220 are also selected in accordance with the dimensions of the pressure belt 212.

[0036] Here, in order to form a nip portion between the fixing belt 211 and the pressure belt 212, the pressure side roller 220 is pressed toward the heating side roller 218 at a predetermined pressure in the direction of arrow F by a pressure mechanism (not shown) at both left and right ends of the rotating shaft.

[0037] Also, a pressure pad is used to obtain a wide nip portion without increasing the size of the device. The thermal fixing device 200 shown in Fig. 2 uses a heater 300 as a first pressure pad that presses the fixing belt 211 toward the pressure belt 212, and a pressure pad 213 as a second pressure pad that presses the pressure belt 212 toward the fixing belt 211. The heater 300 and the pressure pad 213 are supported between left and right side plates (not shown) of the device. The pressure pad 213 is pressed toward the heater 300 with a predetermined pressure force in the direction of arrow G by a pressure mechanism (not shown).

[0038] The surface layer 315 of the heater 300, which is the first pressure pad, constitutes a surface that slides against the inner circumferential surface of the fixing belt 211. It is preferable to have a lubricant between the inner circumferential surface of the fixing belt 211 and the surface layer 315, since good sliding properties can be obtained. Examples of the lubricant include fluorine-based grease using PFPE (perfluoropolyether) oil and PTFE (polytetrafluoroethylene) as thickeners, silicone oil, etc. In addition, the pressure pad 213, which is the second pressure pad, has a pad base and a sliding sheet 214 that contacts the belt. If the pressure pad 213 directly contacts the inner circumferential surface of the pressure belt 212, the abrasion of the rubbing portion may become large. In that case, the sliding sheet 214 may be interposed between the pressure belt 212 and the pressure pad 213. By using the sliding sheet 214, the abrasion of the pressure pad 213 can be prevented, the sliding resistance can be reduced, and good belt running properties and excellent durability can be obtained. The fixing belt 211 is provided with a non-contact charge removing brush (not shown), and the pressure belt is provided with a contact charge removing brush (not shown).

[0039] The control circuit unit 216 drives the motor D at least when image formation is being performed. This causes the heating side roller 218 to rotate, and the fixing belt 211 to rotate in the same direction as the heating side roller 218. The pressure belt 212 rotates following the fixing belt 211. Here, the most downstream portion of the nip is configured so that the fixing belt 211 and the pressure belt 212 are sandwiched and transported by the roller pair of the heating side roller 218 and the pressure side roller 220, thereby preventing the belts from slipping. The most downstream portion of the nip is the portion where the pressure distribution (recording material transport direction) at the nip is maximum.

[0040] In a state where the fixing belt 211 is heated to a predetermined fixing temperature and maintained (also called temperature control), the recording material 141 having the unfixed toner 142 is conveyed to the nip between the fixing belt 211 and the pressure belt 212. The recording material 141 is introduced with the surface carrying the unfixed toner 142 facing the fixing belt 211 side. Then, the unfixed toner 142 of the recording material 141 is conveyed while being sandwiched and conveyed while being in close contact with the outer peripheral surface of the fixing belt 211, so that heat is applied from the fixing belt 211 and the unfixed toner 142 is fixed to the surface of the recording material 141 by receiving a pressure force. At this time, the heat from the heated base of the fixing belt 211 is efficiently transported to the recording material 141 through an elastic layer having enhanced thermal conductivity in the thickness direction. Thereafter, the recording material 141 is separated from the fixing belt 211 by a separating member 221 and conveyed.

[0041] The fixing belt-pressure belt type thermal fixing device is not limited to the form shown in FIG. 2. For example, in the form shown in FIG. 2, the heater 300, which is a heating member, is also used as the first pressure pad, which is a pressure member. That is, in the form shown in FIG. 2, the pressure member and the heating member are used as the same member, but the heater 300 and the first pressure pad may be separate members. At this time, the heater 300 is brought into contact with the inner circumferential surface of the fixing belt 211 at a position other than the position shown in FIG. 2, and the fixing belt 211 is heated. In this case, as in the fixing belt-pressure roller type thermal fixing device, a laminated structure having a base material 311, an intermediate layer 316, and a surface layer 315 made of a DLC film in this order may be used as the first pressure pad. Also, a pressure pad provided with a sliding sheet may be used as the first pressure pad. Furthermore, a laminated structure having a base material 311, an intermediate layer 316, and a surface layer 315 made of a DLC film in this order may be used as the second pressure pad.

[0042] 3 is a schematic cross-sectional view showing an example of a laminated structure according to an embodiment of the present disclosure. The laminated structure includes a substrate 311, an intermediate layer 316, and a diamond-like carbon film in this order, and the diamond-like carbon (DLC) film constitutes a surface layer 315. When the laminated structure is used as the heater 300, the heater 300 has a resistance heating element 312 and a thermistor as a temperature sensor 313 on the surface of the substrate 311 opposite to the surface on which the intermediate layer 316 is provided. The resistance heating element 312 is insulated by a glass layer 314. The material of the substrate 311 must be an insulating material because the resistance heating element 312 is formed on the substrate. The substrate 311 should have high thermal conductivity so that heat from the resistance heating element 312 can be easily transferred to the fixing belt 120. For this reason, the substrate 311 contains one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon nitride. The substrate 311 is preferably made of one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon nitride. When the substrate 311 is made of aluminum nitride and has a flat rectangular shape of, for example, about 400 mm x 8 mm, the aluminum nitride may be oxidized from its surface to a depth of several hundred nm.

[0043] When DLC contains hydrogen, its hardness decreases. Therefore, except for inevitable components in the manufacturing process and gas adsorbed on the film surface, the DLC film constituting the surface layer 315 is preferably a DLC film that does not substantially contain hydrogen atoms. In other words, it is more preferable that the number of hydrogen atoms in the diamond-like carbon film (H) and the ratio of the number of hydrogen atoms (H) to the number of carbon atoms (C') (H) / [(H)+(C')]) are 0.00 or more and 0.02 or less.

[0044] Between the surface layer 315 and the substrate 311, an intermediate layer 316 containing silicon carbide is formed. The ratio [(Si)+(C)] / A of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements except hydrogen atoms in the intermediate layer is 0.8 or more. Furthermore, the ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) in the intermediate layer 316 is greater than 1. By satisfying these conditions, the intermediate layer 316 exhibits strong adhesion to the substrate 311 and the DLC film, and acts as an excellent adhesion layer for the substrate 311 and the surface layer 315 composed of the DLC film.

[0045] When intermediate layer 316 is analyzed by X-ray photoelectron spectroscopy (XPS), if the position of the peak top of the binding energy of the 2p orbital of silicon atoms in the intermediate layer is above 99.0 eV where the peak top indicating the binding energy of silicon appears and is below 100.4 eV where the peak top indicating the binding energy of silicon carbide appears, this indicates that intermediate layer 316 is a composite of silicon containing elemental silicon or silicon-rich silicon carbide and silicon carbide. Such intermediate layer 316 is preferable because it has the effect of further increasing the adhesion between substrate 311 and surface layer 315.

[0046] Furthermore, when the intermediate layer 316 is analyzed by X-ray photoelectron spectroscopy (XPS), if the ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) in the intermediate layer is 2.0 or more, it indicates that the intermediate layer 316 is a composite of silicon carbide and silicon, or silicon-rich silicon carbide-containing silicon. Such an intermediate layer 316 is preferable because it has an effect of increasing the adhesion between the substrate 311 and the surface layer 315. Furthermore, if the ratio (Si) / (C) is 2.6 or less, the film hardness of the intermediate layer 316 is reduced, and as a result, the adhesion of the DLC film can be more reliably prevented from decreasing. Therefore, it is more preferable that the ratio (Si) / (C) of the intermediate layer is 2.0 or more and 2.6 or less.

[0047] The laminated structure having the above-mentioned configuration can prevent peeling of the surface layer 315 even if the surface of the substrate on which the DLC film is formed is a smooth surface with an arithmetic mean roughness of, for example, 0.13 μm to 0.35 μm. As a result, the life of the thermal fixing device can be increased. In other words, the laminated structure according to the present disclosure contributes to further improving the durability of the thermal fixing device.

[0048] 4 is a schematic cross-sectional view of an electrophotographic full-color printer using a laser exposure method, which is an example of an electrophotographic image forming apparatus using a fixing belt-pressure roller type thermal fixing device 100 according to an embodiment of the present disclosure. The printer 400 includes toner image forming devices 411a-d, a primary transfer device 420, a secondary transfer device 430, a thermal fixing device 100, a paper feed section 441, a paper feed roller 442, a paper output tray 443, an external host device (not shown), and an exposure laser light source (not shown). A full-color image can be formed on a recording material 141 and output in accordance with input image information from the external host device (not shown).

[0049] Based on color separation image signals input from an external host device (not shown), toner images are formed on the surfaces of drum-shaped electrophotographic photoreceptors built into toner image forming devices 411a-d for each color of yellow, magenta, cyan, and black by a laser exposure method using a laser light source for exposure (not shown). The electrophotographic image forming process by the laser exposure method is well known, so its description will be omitted.

[0050] The primary transfer device 420 is made up of an endless flexible primary transfer belt 421 , a primary transfer roller 422 , and a tension roller 423 .

[0051] The four color toner images formed by each toner image forming device 411a to d are superimposed and transferred by each primary transfer roller 422 onto a primary transfer belt 421 which is stretched and rotated by a tension roller 423 and a secondary transfer opposing roller 432, and an unfixed full-color toner image is formed on the primary transfer belt 421.

[0052] Meanwhile, at a predetermined paper feed timing, a recording material (paper) 141 is conveyed by a paper feed roller 442 from a paper feed section 441 to a secondary transfer device 430 consisting of a secondary transfer roller 431 and a secondary transfer opposing roller 432. Here, an unfixed full-color toner image on the primary transfer belt 421 is transferred onto the recording material 141 such as paper.

[0053] Thereafter, the recording material 141 is conveyed to the thermal fixing device 100 and heated. By being heated, the unfixed full-color toner image on the recording material 141 melts and mixes colors, and is fixed on the recording material 141 as a fixed image. Thereafter, the recording material (paper) 141 on which the toner image has been fixed is discharged onto a paper discharge tray 443.

[0054] In addition, the electrophotographic image forming apparatus according to one embodiment of the present disclosure is not limited to the form shown in FIG. 4, and also includes an electrophotographic image forming apparatus in which the fixing belt-pressure roller type thermal fixing device 100 is replaced with a fixing belt-pressure belt type thermal fixing device 200.

[0055] The following will exemplify a method for forming the intermediate layer 316 and the surface layer 315 in the laminated structure according to an embodiment of the present disclosure, although the method is not limited thereto.

[0056] 3 can be formed by physical vapor deposition, such as sputtering or arc evaporation, using a Si or SiC target as a raw material, or chemical vapor deposition, using a hydrocarbon gas and a silane gas as raw materials. Physical vapor deposition is more preferable because it is easy to control the composition ratio and bonding state of impurities, Si, and C.

[0057] As an example, an intermediate layer forming apparatus 500 using a sputtering method, which is one of the physical vapor deposition methods, is shown in Fig. 5. The intermediate layer forming apparatus 500 includes a vacuum chamber 510 in which a film formation process is performed, a vacuum pump (not shown) for evacuating the vacuum chamber 510, a target 521 serving as a film material, a power supply 523 for applying power to the target 521, a magnet 522 disposed on the rear surface of the target, an anode electrode 524 disposed around the target, a gas pipe and a mass flow controller 531 for introducing a process gas into the vacuum chamber 510, a substrate holder 541 on which a substrate 542 to be formed is placed, a drive mechanism (not shown) for moving the substrate holder 541 during film formation, and a mask 551 for controlling the film thickness distribution of the substrate 542 to be formed.

[0058] The intermediate layer 316 is formed using the intermediate layer forming apparatus 500, for example, by the following method: Ar gas is introduced from a gas pipe and a mass flow controller 531 into a vacuum chamber 510 evacuated by a vacuum pump, and the vacuum degree of the vacuum chamber 510 is adjusted to a desired degree.

[0059] When power is applied to the target 521 by the power source 523, an Ar plasma discharge is generated between the target 521 and the anode electrode 524. At this time, the magnetic field lines of the magnet 522 further increase the density of the Ar plasma.

[0060] Ions in the formed Ar plasma sputter material particles from the target 521. The sputtered material particles reach a film-forming substrate 542 placed on a substrate holder 541, and an intermediate layer 316 is formed on the film-forming substrate 542.

[0061] The amount of particles sputtered from the target 521 that reach the deposition substrate 542 varies depending on the position of the deposition substrate 542. Therefore, the substrate holder 541 on which the deposition substrate 542 is placed during deposition is moved in the direction of the arrow in Fig. 5, and in the portion where a large number of sputtered particles reach the deposition substrate 542, the particles are partially blocked by a mask 551 placed between the target 521 and the deposition substrate 542, whereby the thickness of the intermediate layer 316 formed on the deposition substrate 542 is uniformly corrected.

[0062] If the target used is conductive, plasma discharge can be formed by using a DC power supply for the power supply 523 that applies power to the target. If the target is insulating, plasma discharge can be formed by using a radio frequency (RF) power supply for the power supply 523 that applies power to the target.

[0063] Furthermore, the gas introduced into the vacuum chamber 510 is not limited to Ar, and gases such as Xe and He can be used in place of Ar or mixed with Ar.

[0064] As the surface layer 315, a diamond-like carbon (DLC) film can be formed by physical vapor deposition, such as arc evaporation or sputtering, using graphite as a raw material, or chemical vapor deposition, using a hydrocarbon gas as a raw material. A physical vapor deposition method using graphite as a raw material is more preferable because it is easy to reduce the amount of hydrogen in the DLC film.

[0065] As an example, a DLC film forming apparatus 600 using the arc evaporation method is shown in Fig. 6. The DLC film forming apparatus 600 is composed of a film forming chamber 610 where the film forming process is performed, an arc plasma generation chamber 620 where an arc plasma discharge is generated to evaporate the film material, and a duct filter 630 which transports the film material generated in the arc plasma generation chamber 620 to the film forming chamber 610.

[0066] The deposition chamber 610 is maintained in a vacuum state by a vacuum pump (not shown). A substrate 612 to be deposited is placed in the deposition chamber 610 by a substrate holder 611. The substrate holder 611 can be rotated or moved during deposition as necessary, allowing deposition to be performed in a manner suited to the shape of the substrate 612 to be deposited.

[0067] The arc plasma generating chamber 620 is maintained in a vacuum state by a vacuum pump (not shown) in the same manner as the film forming chamber 610. A graphite target 621 is disposed in the arc plasma generating chamber 620. An arc discharge power supply 622 for generating an arc discharge is connected to the graphite target 621. A striker 623 for igniting the arc discharge and an anode 624 for the arc discharge are disposed above the graphite target 621.

[0068] A duct coil 631 for generating a magnetic field for deflecting the film material is disposed in the duct filter 630. A duct coil power supply 632 for energizing the duct coil 631 is connected to the duct coil 631. A scanning coil 633 for generating a magnetic field for scanning the charged particles of the film material is disposed at the tip of the duct filter 630. A scanning coil power supply 634 is connected to the scanning coil 633. The duct filter 630 is insulated from the film forming chamber 610 and the arc plasma generating chamber 620 by an insulating member 635. The duct filter 630 is also connected to a duct filter power supply 636, and the potential thereof can be controlled.

[0069] When a striker 623 connected to earth comes into contact with the graphite target 621 to which power is applied from an arc discharge power supply 622, or when the striker 623 moves away from the graphite target 621, an arc plasma can be generated between the graphite target 621 and the anode 624 by applying power from the arc discharge power supply 622. The film material is evaporated from the graphite target 621 by the arc plasma.

[0070] When the graphite target 621 is evaporated by the arc plasma, fine particles of about several μm in size called droplets are generated. These droplets are not DLC but graphite. Graphite has the disadvantage of reducing the film hardness. For this reason, the number of droplets must be adjusted as necessary.

[0071] The duct filter 630 that transports the film material generated in the arc plasma generating chamber 620 to the film forming chamber 610 is curved. The film material evaporated by the arc plasma is a charged particle, and is transported to the film forming chamber 610 along the axis of the duct filter 630 by the magnetic field formed in the duct filter 630 by the duct coil 631 and the duct coil power supply 632. In contrast, droplets are often neutral, and therefore travel straight without being deflected by the magnetic field formed in the duct filter 630, and collide with the curved portion of the duct filter 630. As a result, the amount of droplets transported to the film forming chamber 610 is reduced and adjusted.

[0072] The film material is generated in the arc plasma generating chamber 620 and transported to the film forming chamber 610 via the duct filter 630, and then collides with the film forming substrate 612 on which the intermediate layer 316 has been formed, and is laminated.

[0073] In addition, by controlling the potential with a duct filter power supply 636 connected to the duct filter 630, the transport amount of the membrane material and the amount of droplets can be adjusted. The hydrogen content of the formed surface layer 315 made of the DLC film by ERDA is usually about 0.5 atomic %.

[0074] Moreover, it is more preferable to form the surface layer 315 and the intermediate layer 316 as the sliding layer successively under a vacuum state. This is because if the substrate 612 on which the intermediate layer 316 is formed is exposed to the atmosphere between the formation of the intermediate layer 316 and the formation of the surface layer 315, the adhesion between the intermediate layer 316 and the surface layer 315 may change due to partial oxidation of the outermost surface of the intermediate layer 316 or adsorption of gas or moisture in the atmosphere to the outermost surface of the intermediate layer 316. For this reason, it is more preferable to use an apparatus having a configuration in which the chambers of the apparatus shown in Figures 5 and 6 are connected.

[0075] According to one aspect of the present disclosure, a thermal fixing device that has excellent heat transfer to the first member and can exhibit stable thermal fixing performance for a long period of time can be obtained. According to another aspect of the present disclosure, an electrophotographic image forming apparatus that can stably form high-quality electrophotographic images can be obtained. Furthermore, according to another aspect of the present disclosure, a laminated structure that has excellent adhesion of the DLC film can be obtained regardless of the smoothness of the substrate that is the adhesion surface. EXAMPLES

[0076] Examples and comparative examples are shown below to specifically describe the thermal fixing device and the like according to one aspect of the present disclosure. Note that the thermal fixing device and the like according to the present disclosure are not limited to the configurations embodied in the examples.

[0077] <Example 1> As Example 1, a laminated structure was produced in which an intermediate layer and a surface layer were formed in this order on one surface of a substrate made of aluminum nitride (hereinafter also referred to as "AlN") using an apparatus having a configuration in which the chambers of the apparatus shown in Figures 5 and 6 are connected. The surface of the substrate was covered with a thin film made of aluminum oxide (hereinafter also referred to as "AlO").

[0078] First, the intermediate layer was formed on a substrate as a substrate 542 to be deposited, the substrate having an arithmetic mean roughness Ra of 0.13 μm, using an apparatus having a similar configuration to the intermediate layer forming apparatus 500 shown in Fig. 5. The deposition conditions were as follows: a composite target of a mixture of silicon and silicon carbide was used as the target 521, the power applied by the power source 523 was 550 W, and the pressure in the vacuum chamber 510 during deposition was 0.9 Pa. The median abundance ratio of silicon to silicon carbide in the composite target was silicon:silicon carbide of 1.4:1.

[0079] Next, using an apparatus having a configuration similar to that of the DLC film forming apparatus 600 shown in FIG. 6, a surface layer 315 composed of a DLC film made from a graphite target 621 was formed on the intermediate layer formed above, thereby producing a laminated structure.

[0080] In a silicon wafer substrate on which a layer corresponding to the intermediate layer was formed under the same film forming conditions as those for the intermediate layer in the manufacture of Example 1, a step was formed between a portion on which the layer corresponding to the intermediate layer was formed and a portion on which the layer was not formed by masking a part. The height of the step was measured using a stylus profiler (product name: P-15, manufactured by KLA-Tenchore Corporation) and found to be 60 nm. This result was taken as the film thickness of the intermediate layer in the laminate structure of Example 1.

[0081] A layer formed under the same conditions as the intermediate layer in the manufacturing of Example 1 was analyzed by X-ray photoelectron spectroscopy (XPS) using an X-ray photoelectron spectrometer (product name: Quantera SXM, manufactured by ULVAC-PHI, light source: AlKα). Only a layer corresponding to the intermediate layer was formed on a silicon wafer substrate, and the outermost surface, a portion etched 13 nm from the outermost surface using Ar ions in a vacuum chamber of the XPS, and a portion etched 25 nm from the outermost surface were analyzed. Elements detected by XPS were silicon, carbon, and oxygen, which is considered to be an unavoidable impurity mixed in during film formation. The oxygen content in the portion etched 13 nm from the outermost surface and the portion etched 25 nm from the outermost surface, i.e., the layer corresponding to the intermediate layer, was 4.9 atomic %, and the layer corresponding to the intermediate layer had a ratio [(Si) + (C)] / A of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements excluding hydrogen, which cannot be detected by XPS, of 0.95, and the layer corresponding to intermediate layer 316 was composed of silicon and carbon. The ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) in the layer corresponding to the intermediate layer was 2.02. In addition, in the film forming method shown in this embodiment using the apparatus with the chambers connected as shown in Figures 5 and 6, there is no active hydrogen source in the DLC film, and the residual moisture in the chamber becomes the hydrogen source. The ratio (H) / [(H)+(C')] of the number of hydrogen atoms (H) to the number of carbon atoms (C') in the DLC film was 0.015. From this, the amount of hydrogen contained in the DLC film according to this embodiment was equal to or less than the amount of oxygen, which is an unavoidable component.

[0082] The bonding state of silicon atoms obtained by XPS is shown in Figure 7. The peak top position of the bonding energy of the 2p orbital of silicon atoms was found to be halfway between 99 e.0 V, where the peak top indicating the bonding energy of silicon appears, and 100.4 eV, where the peak top indicating the bonding energy of silicon carbide appears. A peak indicating the bonding energy of silicon oxide was found on the outermost surface, which was thought to be due to oxidation caused by exposure to the atmosphere between the time of film formation and analysis, and adsorption of moisture from the atmosphere.

[0083] The bonding state of carbon atoms obtained by XPS is shown in Figure 8. The position of the peak top of the bonding energy of the 1s orbital of carbon atoms was found to be at the position where the peak top showing the bonding energy of silicon carbide appeared. Therefore, the results of XPS showed that the intermediate layer was a composite of silicon and silicon carbide.

[0084] The thickness of the surface layer was also measured by a stylus profiler in the same manner as the thickness of the intermediate layer 316, and was found to be 500 μm.

[0085] <Example 2> A laminated structure was manufactured in the same manner as in Example 1, except that the thickness of the intermediate layer was set to 20 nm. Analysis was performed by XPS in the same manner as in Example 1, and the elements detected were silicon, carbon, and oxygen, which is considered to be an inevitable impurity mixed in during film formation. The oxygen content in the layer corresponding to the intermediate layer 316 was 2.8 atomic %, and the ratio [(Si)+(C)] / A of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements except oxygen atoms and hydrogen that cannot be detected by XPS was 0.95, and the layer corresponding to the intermediate layer 316 was composed of silicon and carbon. In addition, the ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) was 2.55.

[0086] <Example 3> Except for setting the thickness of the surface layer to 650 nm, a laminated structure was manufactured in the same manner as in Example 2. Analysis was performed by XPS in the same manner as in Example 1, and the oxygen content and ratio (Si) / (C) in the layer corresponding to intermediate layer 316 were the same as in Example 2.

[0087] <Example 4> A laminated structure was produced in the same manner as in Example 1, except that a substrate having an arithmetic mean surface roughness Ra of 0.35 μm was used.

[0088] <Example 5> A laminated structure was produced in the same manner as in Example 1, except that the ratio (Si) / (C) in the layer corresponding to the intermediate layer was set to 1.55.

[0089] <Comparative Example 1> A laminated structure was produced in the same manner as in Example 1, except that no intermediate layer was formed.

[0090] <Comparative Example 2> A titanium target was used as the target to form an intermediate layer made of Ti with a thickness of 60 nm. Except for this, the laminated structure was manufactured in the same manner as in Example 1.

[0091] <Comparative Example 3> A laminated structure was manufactured in the same manner as in Example 1, except that a silicon carbide target was used as the target to form an intermediate layer made of silicon carbide with a thickness of 60 nm. Here, the bonding state of silicon atoms obtained by XPS of the intermediate layer according to this comparative example is shown in FIG. 9. The position of the peak top of the bonding energy of the 2p orbital of silicon atoms was observed at the position where the peak top indicating the bonding energy of silicon carbide appeared. The ratio [(Si)+(C)] / A of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements except oxygen atoms and hydrogen that cannot be detected by XPS in the intermediate layer was 0.95, and the ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) in the intermediate layer 316 was 0.86.

[0092] Table 1 shows the results of evaluating the adhesion and robustness of the laminated structures of Example 1 and Comparative Examples 1 to 3 by a scratch test in accordance with Japanese Industrial Standards (JIS) R3255 (1997). A stylus with a tip radius of 5 μm was pressed against the film while scanning it, and the pressure load was increased to evaluate the adhesion and robustness of the laminated structure from the load value (critical load value) at which the film was destroyed.

[0093] In the laminate structure according to Comparative Example 1, after the laminate structure was manufactured and before the scratch test was performed, peeling of the surface layer composed of the DLC film occurred. Furthermore, as a result of the scratch test, the laminate structure according to Example 1 exhibited a critical load that was more than twice as high as the critical loads exhibited by the laminate structures according to Comparative Examples 2 and 3.

[0094] The mechanism by which the laminated structure according to Example 1 exhibits such a high critical load is believed to be as follows: The intermediate layer according to Example 1 contains excess silicon in the Si-C bond and elemental silicon, and therefore has particularly high adhesion to aluminum nitride and DLC, and also contains silicon carbide, which is believed to contribute to its robustness.

[0095] In addition, in the laminated structures of Example 1 and Comparative Examples 1 to 3, aluminum nitride was used as the base material, but its outermost surface, including the natural oxide film, was composed of aluminum oxide. Therefore, it is considered that the same results as those of the laminated structures of Example 1 and Comparative Examples 1 to 3 can be obtained even when aluminum oxide is used as the base material.

[0096] A durability test was also carried out on the thermal fixing device shown in FIG. 1 using the laminated structure of Example 1. FIG. 10 shows the change over time in the torque for rotating the fixing belt. As shown in FIG. 10, no increase or abnormality in the torque was observed even after 350 hours of operation. Furthermore, no abnormal noise was generated during the fixing operation, and no damage was observed to the members of the thermal fixing device, including the fixing belt. Devices that did not produce abnormal noise during the fixing operation or damage to the members of the thermal fixing device, including the fixing belt, were rated as "durable."

[0097] A durability test of a thermal fixing device was carried out in the same manner as for the laminated structure of Example 1 for the laminated structures of Examples 2 to 5. As a result, as shown in Table 2, similar to the laminated structure of Example 1, even after 350 hours of operation, there was no increase in torque or damage to the members of the thermal fixing device, and the structure showed high durability and was evaluated as "durable."

[0098] [Table 1]

[0099] [Table 2] [Explanation of symbols]

[0100] 100 Heat fixing device 110 Heater unit 111 Heater holder 112 Reinforced metal plate 120 Fixing belt 141 Recording material 142 Toner 130 Pressure Roller 131 Core 132 Silicone layer 133 Perfluoroalkoxyalkane resin layer 300 Heater 311 Base material 312 Resistance heating element 313 Temperature Sensor

Claims

1. a rotatable first member; a heater for heating the first member; a rotatable second member that forms a nip portion capable of holding a recording material between the first member and the second member, The heater is a surface layer that constitutes a surface that slides against the inner circumferential surface of the first member; A substrate supporting the surface layer via an intermediate layer, The substrate comprises at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon nitride; The surface layer is made of a diamond-like carbon film, the intermediate layer comprises silicon carbide; the ratio of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements other than hydrogen atoms in the intermediate layer, [(Si)+(C)] / A, is 0.8 or more; and a ratio (Si) / (C) of the number of said silicon atoms (Si) to the number of said carbon atoms (C) is greater than 1.

2. 2. The thermal fixing device according to claim 1, wherein the surface of the base material facing the intermediate layer has an arithmetic mean roughness Ra of 0.13 μm to 0.35 μm.

3. 3. The thermal fixing device according to claim 1, wherein the ratio (H) / [(H)+(C')] of the number of hydrogen atoms (H) in the diamond-like carbon film to the sum of the number of hydrogen atoms (H) in the diamond-like carbon film and the number of carbon atoms (C') in the diamond-like carbon film is 0.00 or more and 0.02 or less.

4. The thermal fixing device according to any one of claims 1 to 3, wherein when the intermediate layer is analyzed by X-ray photoelectron spectroscopy using an AlKα light source, the position of the peak top of the binding energy of the 2p orbital of a silicon atom is greater than 99.0 eV and less than 100.4 eV.

5. 5. The thermal fixing device according to claim 1, wherein the ratio (Si) / (C) is 2.0 or more.

6. 6. The thermal fixing device according to claim 1, wherein the ratio (Si) / (C) is 2.0 or more and 2.6 or less.

7. 7. The thermal fixing device according to claim 1, wherein the first member has a resin film that constitutes the inner circumferential surface, and the resin film contains polyimide.

8. 8. The thermal fixing device according to claim 1, wherein a lubricant is present between the inner circumferential surface of the first member and the surface layer.

9. the first member is a fixing belt having an endless shape, 9. The thermal fixing device according to claim 1, wherein the second member is a pressure roller.

10. the first member is a fixing belt having an endless shape, 9. The thermal fixing device according to claim 1, wherein the second member is a pressure belt having an endless shape.

11. 11. An electrophotographic image forming apparatus comprising the thermal fixing device according to claim 1.

12. A laminated structure having a substrate, an intermediate layer, and a diamond-like carbon film in this order, The substrate comprises at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, and silicon nitride; the intermediate layer comprises silicon carbide; A laminate structure characterized in that the ratio [(Si)+(C)] / A of the sum of the number of silicon atoms (Si) and the number of carbon atoms (C) to the total number (A) of all elements excluding hydrogen atoms in the intermediate layer is 0.8 or more, and the ratio (Si) / (C) of the number of silicon atoms (Si) to the number of carbon atoms (C) is greater than 1.

13. The laminated structure according to claim 12, wherein the ratio (H) / [(H)+(C')] of the number of hydrogen atoms (H) in the diamond-like carbon film to the sum of the number of hydrogen atoms (H) in the diamond-like carbon film and the number of carbon atoms (C') in the diamond-like carbon film is 0.00 or more and 0.02 or less.

14. 14. The laminate structure according to claim 12 or 13, wherein when the intermediate layer is analyzed by X-ray photoelectron spectroscopy using an AlKα light source, the position of the peak top of the binding energy of the 2p orbital of a silicon atom is located at more than 99.0 eV and less than 100.4 eV.

15. The laminate structure according to any one of claims 12 to 14, wherein the ratio (Si) / (C) is 2.0 or more.

16. The laminate structure according to any one of claims 12 to 15, wherein the ratio (Si) / (C) is 2.0 or more and 2.6 or less.

Citation Information

Patent Citations

  • Heating / Fixing device and manufacture thereof

    JP1995295409A

  • Rolling slide member and bearing for steel pipe forming roll

    JP2009243619A

  • Sheet feeder and image formation apparatus

    JP2015034080A

  • Fixing apparatus and image forming apparatus

    JP2015034980A

  • Fixing device and image forming apparatus

    JP2019219649A