Layered catalytic reactor system and method for hydroprocessing of hydrocarbon feedstocks - Patents.com

A layered catalytic reactor system with alternating supported and free-standing catalysts addresses the issue of runaway temperatures in hydroprocessing, enhancing efficiency and activity.

JP7591178B2Active Publication Date: 2024-11-27CHEVRON USA INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024508715
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-13
Filing Date
2022-06-28
Publication Date
2024-11-27
Estimated Expiration
2042-06-28

AI Technical Summary

Technical Problem

Free-standing catalysts in hydroprocessing are susceptible to runaway temperature increases due to excessive heat generation, leading to irreversible coke formation and reduced efficiency.

Method used

A layered catalytic reactor system with alternating layers of supported and free-standing catalysts, including demetalization, hydrotreating, hydrocracking, and hydroprocessing catalysts, to manage temperature and enhance activity.

Benefits of technology

The system effectively minimizes runaway temperature increases while increasing hydroprocessing efficiency and activity without increasing catalyst volume.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591178000014
    Figure 0007591178000014
  • Figure 0007591178000015
    Figure 0007591178000015
  • Figure 0007591178000016
    Figure 0007591178000016
Patent Text Reader

Abstract

A layered catalyst reactor system and method for hydrotreating a hydrocarbon feedstock. The layered catalyst system reactor comprises a vertical bed structure including a demetallization catalyst layer, multiple layers of a supported hydrotreating catalyst layer, and multiple alternating layers of supported hydrocracking catalyst and free-standing hydrotreating catalyst. The arrangement of the catalyst layers reduces the risk of temperature runaway while improving hydrotreating performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Applications

[0001] This application claims priority to U.S. patent application Ser. No. 17 / 401,757, filed Aug. 13, 2021, the entire contents of which are incorporated herein by reference.

[0002] This disclosure relates to layered catalytic reactor systems and methods for use in hydrocarbon reforming. [Background technology]

[0003]

[0003] Catalytic hydroprocessing refers to a petroleum refining process in which a carbonaceous feedstock is contacted with hydrogen and a catalyst at higher temperatures and pressures to remove undesirable impurities and / or convert the feedstock into improved products. Examples of hydroprocessing processes include hydrotreating, hydrodemetallization, hydrocracking, and hydroisomerization processes.

[0004]

[0004] Hydrotreating processes are used to remove impurities such as sulfur, nitrogen and oxygen to control end product specifications or prepare the feed for further processing. Supported mixed metal catalysts used in hydrotreating carbonaceous feedstocks include a porous alumina matrix impregnated with a combination of nickel, molybdenum, tungsten and / or cobalt. Free-standing mixed metal sulfide catalysts that are not diluted with a support pack more metal sulfides, and therefore more hydrogenation powder, into a smaller reactor volume compared to supported mixed metal sulfide catalysts.

[0005]

[0005] However, free-standing catalysts are more susceptible to localized "runaway" temperature increases than supported catalysts. Such runaway temperature increases occur when the hydrogenation catalyst generates more heat than can be absorbed by its surroundings and becomes hotter than the bed or reactor temperature. The resulting temperature increase accelerates hydrogen consumption, which in turn increases the catalyst temperature until the hydrogenation (hydrogen consumption) rate exceeds the hydrogen feed rate. At that stage, the catalyst begins to dehydrogenate the feed, generating coke and hydrogen. This process results in irreversible coke deactivation.

[0006]

[0006] Supported hydroprocessing catalysts typically comprise one or more metals deposited on a support or carrier consisting of an amorphous oxide and / or a crystalline microporous material (e.g., zeolite). A suitably sized top layer of supported hydroprocessing catalyst may be used to protect the bottom layer of the free-standing catalyst from excessive hydroprocessing activity. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above, there remains a need to provide an improved hydrotreating catalyst system that increases the activity and efficiency of the hydrotreating process while minimizing the risk of runaway temperature increases. [Means for solving the problem]

[0008]

[0008] This Summary is provided to introduce various concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify required or essential features of the claimed subject matter, nor is the Summary intended to limit the scope of the claimed subject matter.

[0009] Aspects of the present disclosure relate to a layered catalytic reactor system and method for hydroprocessing of a hydrocarbon feedstock.

[0010] In one embodiment, the layered catalytic reactor system comprises, from top to bottom:

[0011] (i) a layer containing one or more demetallization catalysts that is about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0012] (ii) a layer of one or more supported hydrotreating catalysts that is about 17 to about 27% of the total volume of the catalyst in a vertical bed;

[0013] (iii) a layer of one or more supported hydrocracking catalysts that is about 5 to about 15% of the total volume of the catalyst in a vertical bed;

[0014] (iv) a layer of one or more self-supported hydrotreating catalysts, the layer being about 5 to about 25% of the total volume of the catalyst in a vertical bed;

[0015] (v) a layer of one or more supported hydrocracking catalysts that is about 5 to about 15% of the total volume of the catalyst in a vertical bed;

[0016] (vi) a layer of one or more free-standing hydroprocessing catalysts that is about 5 to about 25% of the total volume of the catalyst in a vertical bed;

[0017] (vii) comprising a vertical bed or stack of catalyst layers arranged in a sequence of layers of one or more supported hydrotreating catalysts that are about 2 to about 9% of the total volume of catalyst in the vertical bed.

[0010]

[0018] In another aspect, the layered catalytic reactor system comprises, from top to bottom:

[0019] (i) a layer containing one or more demetallization catalysts that is about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0020] (ii) a layer of one or more supported hydroprocessing catalysts that is about 17 to about 27% of the total volume of the catalyst in a vertical bed;

[0021] (iii) a layer of one or more supported hydrocracking catalysts that is about 5 to about 10% of the total volume of the catalyst in a vertical bed;

[0022] (iv) a layer of one or more free-standing hydroprocessing catalysts that is about 3 to about 15% of the total volume of the catalyst in a vertical bed;

[0023] (v) a layer of one or more supported hydrocracking catalysts that is about 5 to about 10% of the total volume of the catalyst in a vertical bed;

[0024] (vi) a layer of one or more free-standing hydroprocessing catalysts that is about 3 to about 15% of the total volume of the catalyst in a vertical bed;

[0025] (vii) a layer of one or more supported hydrocracking catalysts that is about 5 to about 10% of the total volume of the catalyst in a vertical bed;

[0026] (vii) a layer of one or more free-standing hydroprocessing catalysts that is about 3 to about 15% of the total volume of the catalyst in a vertical bed;

[0027] (viii) comprising a vertical bed or stack of catalyst layers arranged in a sequence of layers of one or more supported hydrotreating catalysts that are about 2 to about 9% of the total volume of catalyst in the vertical bed.

[0011]

[0028] In another aspect, the layered catalytic reactor system comprises, from top to bottom:

[0029] (i) a layer comprising one or more demetallization catalysts;

[0030] (ii) a layer of one or more supported hydroprocessing catalysts;

[0031] (iii) a layer of one or more supported hydrocracking catalysts;

[0032] (iv) one or more layers of free-standing hydroprocessing catalyst;

[0033] (v) a layer of one or more supported hydrocracking catalysts;

[0034] (vi) one or more layers of free-standing hydroprocessing catalyst;

[0035] (vii) a layer of one or more supported hydroprocessing catalysts.

[0036] wherein the total volume of the two layers containing one or more free-standing hydroprocessing catalysts is about 10% to about 50% of the total volume of the catalyst in the vertical bed;

[0037] The total volume of the two layers containing the one or more supported hydrocracking catalysts is about 10 to about 30% of the total volume of catalyst in the vertical bed.

[0012]

[0038] In another aspect, the layered catalytic reactor system comprises, from top to bottom:

[0039] (i) a layer comprising one or more demetallization catalysts;

[0040] (ii) a layer of one or more supported hydroprocessing catalysts;

[0041] (iii) a layer of one or more supported hydrocracking catalysts;

[0042] (iv) one or more layers of free-standing hydroprocessing catalyst;

[0043] (v) a layer of one or more supported hydrocracking catalysts;

[0044] (vi) one or more layers of free-standing hydroprocessing catalyst;

[0045] (vii) a layer of one or more supported hydrocracking catalysts;

[0046] (viii) one or more layers of free-standing hydroprocessing catalyst;

[0047] (ix) a layer of one or more supported hydrotreating catalysts.

[0048] wherein the total volume of the three layers containing one or more free-standing hydroprocessing catalysts is about 9 to about 45% of the total volume of catalyst in the vertical bed;

[0049] The total volume of the three layers containing the one or more supported hydrocracking catalysts is about 15 to about 30% of the total volume of catalyst in the vertical bed.

[0013]

[0050] In another aspect, the present invention relates to a process for hydrotreating a hydrocarbon feedstock, the process comprising: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen, and olefins with the layered catalytic reactor system described herein in the presence of hydrogen to produce a hydrocarbon product having lower contents of metals, sulfur, nitrogen, and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically from top to bottom sequentially through layers of the layered catalytic reactor system; and (iii) recovering the hydrocarbon product from the bottom of the layered catalytic reactor system.

[0014]

[0051] This summary and the following detailed description provide examples and are merely illustrative of the present disclosure. Thus, the above summary and the following detailed description should not be considered limiting. In addition to those described herein, additional features or variations thereof, such as combinations and subcombinations of various features of those described in the detailed description, may be provided. [Brief description of the drawings]

[0015] [Figure 1]

[0052] 1 is a graph showing the normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (no hydrocracking or freestanding hydrotreating catalyst layer; BSU607-56). [Diagram 2]

[0053] 1 is a graph showing normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (one hydrocracking catalyst layer and one freestanding hydrotreating catalyst layer; BSU607-57). [Diagram 3]

[0054] 1 is a graph showing normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (one hydrocracking catalyst layer and one freestanding hydrotreating catalyst layer; BSU911-160). [Figure 4]

[0055] 1 is a graph showing normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (one hydrocracking catalyst layer and one freestanding hydrotreating catalyst layer; BSU607-59). [Diagram 5]

[0056] 1 is a graph showing the normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (no hydrocracking or freestanding hydrotreating catalyst layer; BSU612-37). [Figure 6]

[0057] 1 is a graph showing the normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (no hydrocracking or freestanding hydrotreating catalyst layer; BSU 612-38). [Figure 7]

[0058] 1 is a graph showing normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (one hydrocracking catalyst layer and one freestanding hydrotreating catalyst layer; BSU607-60). [Figure 8]

[0059] 1 is a graph showing normalized temperature of a hydrotreating process through an exemplary layered catalytic reactor system (two hydrocracking catalyst layers and two free-standing hydrotreating catalyst layers; BSU612-40). [Figure 9]

[0060] 1 is a graph showing the normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (no hydrocracking or freestanding hydrotreating catalyst layer; BSU612-39). [Figure 10]

[0061] 1 is a graph showing normalized temperature of a hydrotreating process through a comparative layered catalytic reactor system (one hydrocracking catalyst layer and one freestanding hydrotreating catalyst layer; BSU607-61). [Figure 11]

[0062] 1 is a graph showing normalized temperature of a hydrotreating process through an exemplary layered catalytic reactor system (two hydrocracking catalyst layers and two free-standing hydrotreating catalyst layers; BSU612-41). [Figure 12]

[0063] 1 is a graph showing normalized temperature of a hydrotreating process through an exemplary layered catalytic reactor system (two hydrocracking catalyst layers and two free-standing hydrotreating catalyst layers; BSU911-61). [Figure 13]

[0064] 1 is a graph showing diesel yield versus hydrocracking conversion for various feeds. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] definition

[0065] In order to more clearly define the terms used herein, the following definitions are provided. Unless otherwise specified, the following definitions may be applied to this disclosure. If a term is used in this disclosure but is not specifically defined herein, the definition from the IUPAC Compendium of Chemical Terminology may be applied, unless that definition contradicts any other disclosure or definition applied herein, or obscures or invalidates any claim to which that definition applies. If any definition or usage provided by any document incorporated herein by reference contradicts the definition or usage described herein, the definition or usage described herein shall prevail.

[0017]

[0066] Although compositions and methods are described in terms of "comprising" various components or steps, the compositions and methods can also "consist essentially of" or "consist of" the various components or steps, unless otherwise specified.

[0018]

[0067] The terms "a," "an," and "the" are intended to include multiple possibilities, e.g., at least one. "Including," "with," and "having," as used herein, unless otherwise specified, are defined as comprising (i.e., open language).

[0019]

[0068] Various numerical ranges are disclosed herein.When applicant discloses or claims any kind of range, applicant intends to disclose or claim each possible number that such range can reasonably encompass, including the end point of the range, and any subrange and combination of subranges encompassed therein, unless otherwise specified.For example, all numerical end points of the ranges disclosed herein are approximate unless excluded by condition.

[0020]

[0069] Values ​​or ranges may be expressed herein as "about," "from about" one specific value, and / or "to about" another specific value. When such values ​​or ranges are expressed, other disclosed embodiments include the recited specific value, from one specific value, and / or to the other specific value. Similarly, when values ​​are expressed as approximations by use of the preceding word "about," it will be understood that the specific value forms another embodiment. Furthermore, it will be understood that several values ​​have been disclosed, and that each value is also disclosed herein as "about" that specific value in addition to the value itself. In another aspect, use of the term "about" means ±20% of the stated value, ±15% of the stated value, ±10% of the stated value, ±5% of the stated value, ±3% of the stated value, or ±1% of the stated value.

[0021]

[0070] "Periodic Table" refers to the IUPAC Periodic Table of the Elements, version dated June 22, 2007, where the numbering scheme for the Periodic Table Groups is as set forth in Chemical and Engineering News, 63(5), 27 (1985).

[0022]

[0071] "Hydrocarbonaceous" and "hydrocarbon" refer to compounds containing only carbon and hydrogen atoms. Other identifiers, if any, may be used to indicate the presence of specific groups in the hydrocarbon (e.g., a halogenated hydrocarbon indicates the presence of one or more halogen atoms replacing an equal number of hydrogen atoms in the hydrocarbon).

[0023]

[0072] "Hydrotreating" or "hydroconversion" refers to a process in which a carbonaceous feedstock is contacted with hydrogen and a catalyst at higher temperatures and pressures to remove undesirable impurities and / or convert the feedstock into desired products. Such processes include, but are not limited to, methanation, water-gas shift reaction, hydrogenation, hydrotreating, hydrodesulfurization, hydrodenitrogenation, hydrodemetallization, hydrodearomatization, hydroisomerization, hydrodewaxing, and hydrocracking, including selective hydrocracking. Depending on the type of hydrotreating and reaction conditions, the products of hydrotreating may exhibit improved physical properties, such as improved viscosity, viscosity index, saturates content, low temperature properties, volatility, and depolarization.

[0024]

[0073] "Hydrotreating" refers to a hydrogenation process used to remove contaminants such as nitrogen, sulfur, oxygen, and metals from liquid petroleum fractions. In certain embodiments, the hydrotreating process removes at least about 90% of the nitrogen-, sulfur-, oxygen-, and / or metal-containing contaminants. In certain embodiments, the hydrotreating process converts olefins and aromatics to saturates.

[0025]

[0074] "Hydrocracking" refers to a process in which hydrogenation and dehydrogenation are accompanied by the thermal cracking / fragmentation of hydrocarbons, e.g., the conversion of heavier hydrocarbons to lighter hydrocarbons.

[0075] The term "supported" with respect to a catalyst (e.g., an active phase material) refers to a catalyst attached to a conventional material, which is typically a solid having a high surface area. The support material may be inert or may participate in the catalytic reaction. The support material may be porous or non-porous. Typical catalyst supports include various types of carbon, alumina, silica, and silica-alumina, such as amorphous silica aluminates, zeolites, alumina-boria, silica-alumina-magnesia, silica-alumina-titania, and materials obtained by adding other zeolites and other complex oxides thereto.

[0026]

[0076] The term "free-standing" with respect to a catalyst refers to an unsupported catalyst or a catalyst that is not attached to any other material.

[0077] The terms "catalyst particle," "catalyst composition," "catalyst mixture," "catalyst system," and the like, encompass the initial starting components of the composition and any product or products that may result from the contact of these initial starting components, including both heterogeneous and homogeneous catalyst systems or compositions.

[0027]

[0078] If for any reason Applicant chooses to claim less than the entire range of the present disclosure, for example to account for references of which Applicant may not be aware as of the filing date, Applicant reserves the right to qualify or exclude any individual members of any such groups of values ​​or ranges, including any subranges or combinations of subranges within a group, that may be claimed according to ranges or in any similar manner. Additionally, Applicant reserves the right to qualify or exclude any members of a claimed group.

[0028]

[0079] Although any processes and materials similar or equivalent to those described herein can be used in the practice or testing of the invention, exemplary processes and materials are described herein.

[0029]

[0080] All publications and patents mentioned herein are incorporated herein by reference for the purpose of describing and disclosing, for example, compositions and methodologies described in the publications that may be used in connection with the presently described invention. Publications discussed throughout the document are provided solely for their disclosure prior to the filing date of this application. Nothing herein is to be construed as an admission that the inventors are not entitled to antedate such disclosure by virtue of prior invention.

[0030] Detailed Description

[0081] It is to be understood that the disclosure is not limited in its application to the details of construction and the arrangement of components set forth in the following description or illustrated in the drawings.

[0031]

[0082] The present disclosure generally relates to a layered catalytic reactor system and method for hydroconversion of hydrocarbon feedstocks. The layered catalytic reactor system disclosed herein comprises an arrangement of alternating separate layers of supported and free-standing catalysts, which increases hydroprocessing activity and effectiveness without increasing catalyst volume. In particular, the layered catalytic reactor system and method achieves non-monotonous hydroprocessing activity by layering supported hydroprocessing and hydrocracking catalysts between layers of highly active free-standing hydroprocessing catalyst. In certain embodiments, the free-standing hydroprocessing catalyst is a mixed metal sulfide catalyst. The configuration of catalyst layers in the reactor disclosed herein can be used to mitigate risk.

[0032]

[0083] An exemplary layered catalytic reactor system in which two or more free-standing (or unsupported) hydrotreating catalyst layers are sandwiched between supported catalyst layers is superior to a comparable system with the same total volume of supported and free-standing catalyst in which a supported catalyst layer rests on a single free-standing catalyst layer.

[0033]

[0084] The layered catalytic reactor system is useful for hydroconversion of hydrocarbon feedstocks or processes for upgrading petroleum feedstocks. The methods disclosed herein can be used to react a hydrocarbon feedstock at high temperature and pressure conditions in the presence of hydrogen and the layered catalytic reactor system to convert the feedstock into lower molecular weight products with reduced contaminant levels. Hydroconversion processes are those used for hydrotreating or hydrocracking of hydrocarbon feedstocks and can include, for example, hydrogenation, desulfurization, denitrogenation, and removal of metals. In one embodiment, the hydroconversion process includes hydrocracking and / or hydrotreating of the hydrocarbon feedstock.

[0034]

[0085] Layered Catalytic Reactor System

[0086] In one aspect, the present invention relates to a layered catalytic reactor system for hydrotreating a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen and olefins. The layered catalytic reactor system can be used to remove impurities such as metals, sulfur and nitrogen, as well as to saturate olefins and aromatics.

[0035]

[0087] According to an embodiment, the layered catalytic reactor system comprises, from top to bottom:

[0088] (i) a layer containing one or more demetallization catalysts that is about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0089] (ii) a layer of one or more supported hydroprocessing catalysts that is about 17 to about 27% of the total volume of the catalyst in a vertical bed;

[0090] (iii) a layer of one or more supported hydrocracking catalysts that is about 5 to about 15% of the total volume of the catalyst in a vertical bed;

[0091] (iv) a layer of one or more free-standing hydroprocessing catalysts that is about 5 to about 25% of the total volume of the catalyst in a vertical bed;

[0092] (v) a layer of one or more supported hydrocracking catalysts that is about 5 to about 15% of the total volume of the catalyst in a vertical bed;

[0093] (vi) a layer of one or more free-standing hydroprocessing catalysts that is about 5 to about 25% of the total volume of the catalyst in a vertical bed;

[0094] (vii) comprising a vertical bed or stack of catalyst layers arranged in a sequence of layers of one or more supported hydrotreating catalysts that are about 2 to about 9% of the total volume of catalyst in the vertical bed.

[0036]

[0095] As referred to herein, "total volume of catalyst in a vertical bed" means the total volume of material forming the layers of free-standing and supported catalyst in the vertical bed.

[0096] In certain embodiments, one or more of the layers of the one or more freestanding hydrotreating catalysts is about 9 to about 19%, or about 15 to about 25% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (iv) is about 9 to about 19% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (vi) is about 15 to about 25% of the total volume of the catalyst in the vertical bed.

[0037]

[0097] In certain embodiments, the layered catalytic reactor system comprises, from top to bottom:

[0098] (i) a layer containing one or more demetallization catalysts that is about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0099] (ii) a layer of one or more supported hydroprocessing catalysts that is about 17 to about 27% of the total volume of the catalyst in a vertical bed;

[0100] (iii) a layer of one or more supported hydrocracking catalysts that is about 5 to about 10% of the total volume of the catalyst in a vertical bed;

[0101] (iv) a layer of one or more free-standing hydroprocessing catalysts that is about 3 to about 15% of the total volume of the catalyst in a vertical bed;

[0102] (v) a layer of one or more supported hydrocracking catalysts that is about 5 to about 10% of the total volume of the catalyst in a vertical bed;

[0103] (vi) a layer of one or more free-standing hydroprocessing catalysts that is about 3 to about 15% of the total volume of the catalyst in a vertical bed;

[0104] (vii) a layer of one or more supported hydrocracking catalysts that is about 5 to about 10% of the total volume of the catalyst in a vertical bed;

[0105] (vii) a layer of one or more free-standing hydroprocessing catalysts that is about 3 to about 15% of the total volume of the catalyst in a vertical bed;

[0106] (viii) comprising a vertical bed or stack of catalyst layers arranged in a sequence of layers of one or more supported hydrotreating catalysts that are about 2 to about 9% of the total volume of catalyst in the vertical bed.

[0038]

[0107] In certain embodiments, one or more layers of the one or more freestanding hydrotreating catalysts are about 4 to about 10%, or about 10 to about 15% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (iv) is about 4 to about 10% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (vi) is about 10 to about 15% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (viii) is about 10 to about 15% of the total volume of the catalyst in the vertical bed.

[0039]

[0108] In certain embodiments, the layered catalytic reactor system comprises, from top to bottom:

[0109] (i) a layer comprising one or more demetallization catalysts;

[0110] (ii) a layer of one or more supported hydroprocessing catalysts;

[0111] (iii) a layer of one or more supported hydrocracking catalysts;

[0112] (iv) one or more layers of free-standing hydroprocessing catalyst;

[0113] (v) a layer of one or more supported hydrocracking catalysts;

[0114] (vi) one or more layers of free-standing hydroprocessing catalyst;

[0115] (vii) a layer of one or more supported hydroprocessing catalysts.

[0116] wherein the total volume of the two layers containing one or more free-standing hydroprocessing catalysts is about 10% to about 50% of the total volume of the catalyst in the vertical bed;

[0117] The total volume of the two layers containing the one or more supported hydrocracking catalysts is about 10 to about 30% of the total volume of catalyst in the vertical bed.

[0040]

[0118] In certain embodiments, the layered catalytic reactor system comprises, from top to bottom:

[0119] (i) a layer comprising one or more demetallization catalysts;

[0120] (ii) a layer of one or more supported hydroprocessing catalysts;

[0121] (iii) a layer of one or more supported hydrocracking catalysts;

[0122] (iv) one or more layers of free-standing hydroprocessing catalyst;

[0123] (v) a layer of one or more supported hydrocracking catalysts;

[0124] (vi) one or more layers of free-standing hydroprocessing catalyst;

[0125] (vii) a layer of one or more supported hydrocracking catalysts;

[0126] (viii) one or more layers of free-standing hydroprocessing catalyst;

[0127] (ix) a layer of one or more supported hydrotreating catalysts.

[0128] wherein the total volume of the three layers containing one or more free-standing hydroprocessing catalysts is about 9 to about 45% of the total volume of catalyst in the vertical bed;

[0129] The total volume of the three layers containing the one or more supported hydrocracking catalysts is about 15 to about 30% of the total volume of catalyst in the vertical bed.

[0041]

[0130] In certain embodiments, the total volume of the layers containing one or more demetallization catalysts is about 5 to about 25% of the total volume of catalyst in the vertical bed, hi certain embodiments, the top layer comprises or consists of one or more demetallization catalysts.

[0042]

[0131] In certain embodiments, the total volume of the layers containing one or more supported hydrotreating catalysts is about 19 to about 36% of the total volume of catalyst in the vertical bed. In certain embodiments, the bottom layer comprises or consists of one or more supported hydrotreating catalysts. In certain embodiments, the layer below and in contact with the top layer comprises or consists of one or more supported hydrotreating catalysts.

[0043]

[0132] In one particular embodiment, the total volume of the catalyst in the vertical bed is about 1,416 m 3 (50,000ft 3 ) ~ approx. 8,495m 3 (300,000ft 3 In one particular embodiment, the vertical floor is in the range of about 1,416 m 3 (50,000ft 3 ) ~ approx. 8,495m 3 (300,000ft 3 )

[0044]

[0133] An exemplary layered catalytic reactor system comprises multiple zones. The first zone at the top of the vertical bed is the demetallization zone, where demetallization occurs within a layer containing one or more demetallization catalysts. The demetallization zone is generally responsible for removing contaminating metals from the hydrocarbon feedstock.

[0045]

[0134] The second zone below the first zone is the hydrotreating zone, where hydrotreating occurs within a bed containing one or more supported hydrotreating catalysts. This hydrotreating zone is designed to selectively minimize inhibitors such as organic-N, organic-S, and aromatics by hydrogenation or saturation. This zone serves to protect subsequent hydrocracking and hydrotreating (e.g., self-supporting catalytic hydrotreating) zones that may be sensitive to inhibitors.

[0046]

[0135] The third, fourth, fifth and sixth zones are alternating layers of hydrotreating zones following the hydrocracking zone, and hydrotreating occurs in the layers containing one or more self-supporting hydrotreating catalysts. In certain embodiments, the one or more self-supporting hydrotreating catalysts are mixed metal sulfide (MMS) catalysts. The MMS catalyst can be any mixed metal sulfide catalyst that is a self-supporting or unsupported catalyst. These catalysts have a high level of activity. In one embodiment, the MMS catalyst is a self-supporting multimetallic catalyst prepared from precursors in oxide or hydroxide form. In a preferred embodiment, the precursor is in hydroxide form.

[0047]

[0136] The third and fifth zones below the second and fourth zones, respectively, are hydrocracking zones. Each hydrocracking zone is responsible for hydrocracking a feed to reduce the boiling point of the feed.

[0048]

[0137] The fourth and sixth zones below the third and fifth zones, respectively, are hydrotreating zones, in which hydrotreating is carried out over one or more free-standing hydrotreating catalysts.

[0049]

[0138] In certain embodiments, the layered catalytic reactor system comprises additional self-supporting catalytic hydrotreating zones (sixth and seventh zones) followed by an additional hydrocracking zone.

[0139] The final zone (either the seventh or ninth) is a post-treatment zone or additional hydrotreating zone, where hydrotreating occurs in a bed containing one or more free-standing hydrotreating catalysts.

[0050]

[0140] Generally, the hydrocarbon feedstock is introduced into a first zone (i.e., the top layer) of the layered catalytic reactor system to produce a treated effluent. Hydrogen is also introduced into the layered catalytic reactor system to facilitate the hydrogenation reaction. The treated effluent from each layer travels in a downward path to the next layer of the layered catalytic reactor system. In this manner, the initial hydrocarbon feedstock and the resulting treated effluent from each layer pass through the layered catalytic reactor system.

[0051]

[0141] In certain embodiments, the operating temperature of the layered catalytic reactor system is within the range of about 379°C to about 404°C (about 715°F to about 760°F), or about 371°C to about 412°C (about 700°F to about 775°F).

[0052]

[0142] Weight hourly space velocity (WHSV) is defined as the weight of flowing feed per unit weight of catalyst per hour at the operating conditions of the reactor. In certain embodiments, the WHSV is in the range of about 0.41 to about 1.1, or about 0.4 to about 1.1 / h.

[0053]

[0143] Liquid hourly space velocity (LHSV) is the ratio of the liquid volumetric flow rate per hour to the catalyst volume. In certain embodiments, the LHSV is in the range of about 0.39 to about 0.81, or about 0.3 to about 0.9 / h.

[0054]

[0144] In one particular embodiment, the total pressure within the layered catalytic reactor system during operation is about 1598×10 4 ~Approx. 1620×10 4 Pa (approximately 2318 to 2350 psig), or approximately 1593 x 10 4 ~Approx. 1627×10 4 Pa (approximately 2310 to approximately 2360 psig).

[0055]

[0145] In one particular embodiment, the inlet hydrogen pressure in an operating layered catalytic reactor system is about 1547×10 4 ~Approx. 1593×10 4 Pa (approximately 2244 to 2310 psia), or approximately 1544 x 10 4 ~Approx. 1600×10 4 Pa (approximately 2240 to 2320 psia).

[0056]

[0146] In certain embodiments, the gas velocity in an operating layered catalytic reactor system is between about 1337 and about 1431 S m 3 / m 3 (approximately 7512 to 8040 scfb), or approximately 1335 to 1442 S m 3 / m 3 (approximately 7,500 to 8,100 scfb).

[0057]

[0147] In certain embodiments, the normalized temperature of the layered catalytic reactor system is maintained below about 410° C. (770° F.), or below about 407° C. (765° F.) during the hydrotreating reaction.

[0058]

[0148] Demetalization catalyst

[0149] Metal contaminants, such as vanadium and nickel contaminants, are removed from the hydrocarbon feedstock by contact with one or more demetallization catalysts. In general, the demetallization catalyst according to the embodiment may be a conventional demetallization catalyst known in the art. Examples of demetallization catalysts (i.e., hydrodemetallization catalysts) include, but are not limited to, synthetic aluminum oxides or natural aluminum silicates enriched with oxides of molybdenum, cobalt, and nickel, such as nickel oxide-molybdenum oxide, cobalt oxide, molybdenum oxide, nickel oxide-tungsten oxide, all supported on alumina; and those prepared from bauxite promoted with iron, cobalt, molybdenum, nickel, zinc, and manganese.

[0059]

[0150] In certain embodiments, the demetallization catalyst is a catalyst comprising, for example, ICR132 (available from Advanced Refining Technologies LLC).

[0060]

[0151] In certain embodiments, the supported hydrotreating catalyst layer comprises or consists of one type of supported hydrotreating catalyst. In certain embodiments, the supported hydrotreating catalyst layer comprises or consists of two types of supported hydrotreating catalyst.

[0061]

[0152] Supported Hydrotreating Catalysts

[0153] In general, the supported hydrotreating catalyst according to the embodiment may be a conventional hydrotreating (e.g., hydrodesulfurization) catalyst known in the art. Examples of supported hydrotreating catalysts include, but are not limited to, catalysts comprising at least one Group VIII metal, such as iron, cobalt, or nickel, and at least one Group VIB metal, such as molybdenum or tungsten, on a relatively high surface area support material, such as alumina. Other suitable catalyst supports include zeolites, amorphous silica-alumina, and titania-alumina. In certain embodiments, the supported hydrotreating catalyst comprises a noble metal, such as Pd and Pt. Two or more hydrotreating catalysts may be used in the same or different beds of a layered catalytic reactor system. In certain embodiments, the Group VIII metal is typically present in an amount ranging from about 2 to about 20 wt.%, or from about 4 to about 12 wt.%. The Group VIB metal is typically present in an amount ranging from about 5 to about 50 wt.%, from about 10 to about 40 wt.%, or from about 20 to about 30 wt.%. All metal weight percentages are on the support (percentages are based on the weight of the support).

[0062]

[0154] In certain embodiments, the supported hydrotreating catalyst comprises one or more Group VIII metals selected from iron, cobalt, or nickel. In certain embodiments, the supported hydrotreating catalyst comprises one or more Group VIII metals selected from cobalt and nickel. In certain embodiments, the supported hydrotreating catalyst comprises cobalt.

[0063]

[0155] In certain embodiments, the supported hydrotreating catalyst comprises a support material selected from alumina, zeolite, amorphous silica-alumina, and titania-alumina.

[0156] In certain embodiments, the supported hydrotreating catalyst is a catalyst comprising nickel and molybdenum. In certain embodiments, the supported hydrotreating catalyst is a catalyst comprising nickel oxide and molybdenum trioxide, such as ICR513 (available from Advanced Refining Technologies LLC).

[0064]

[0157] In certain embodiments, the supported hydrotreating catalyst layer comprises or consists of one type of supported hydrotreating catalyst. In certain embodiments, the supported hydrotreating catalyst layer comprises or consists of two types of supported hydrotreating catalyst.

[0065]

[0158] Hydrocracking Catalyst

[0159] Suitable hydrocracking catalysts for use in the systems and methods described herein include, but are not limited to, catalysts containing pyrolysis activity, such as catalysts containing crystalline aluminosilicates. In general, hydrocracking catalysts according to embodiments may be conventional hydrocracking catalysts known in the art. Examples of hydrocracking catalysts include, but are not limited to, nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and nickel-tungsten and / or nickel-molybdenum containing catalysts, of which the latter two are preferred. Non-limiting examples of noble metal catalysts include those based on platinum and / or palladium. Porous support materials that may be used for both noble and non-noble metal catalysts include refractory oxide materials such as alumina, silica, alumina-silica, Kieselguhr, diatomaceous earth, magnesia, or zirconia, with alumina, silica, and alumina-silica being preferred and most common. Zeolite supports may also be used, particularly large pore faujasites, such as ultrastable Y (USY).

[0066]

[0160] Numerous hydrocracking catalysts are available from different commercial suppliers and may be used according to the feedstock and product requirements, and their functionality may be determined experimentally. Any catalyst, including conventional hydrocracking catalysts, that has the desired hydroconversion functionality under the selected operating conditions may be used.

[0067]

[0161] In certain embodiments, the hydrocracking catalyst is not the same as the catalyst used in the demetallization, supported hydrotreating, or unsupported hydrotreating catalyst layer.

[0162] In certain embodiments, the hydrocracking catalyst comprises nickel, cobalt, molybdenum and / or tungsten. In certain embodiments, the hydrocracking catalyst comprises nickel. In certain embodiments, the hydrocracking catalyst comprises nickel-cobalt-molybdenum. In certain embodiments, the hydrocracking catalyst comprises cobalt-molybdenum. In certain embodiments, the hydrocracking catalyst comprises nickel-tungsten. In certain embodiments, the hydrocracking catalyst comprises nickel-molybdenum.

[0068]

[0163] In certain embodiments, the hydrocracking catalyst comprises a support material selected from refractory oxide materials such as alumina, silica, alumina-silica, Kieselguhr, diatomaceous earth, magnesia, or zirconia, and alumina, silica, or alumina-silica, and zeolite supports, e.g., large pore faujasites such as USY.

[0069]

[0164] In certain embodiments, the hydrocracking catalyst is a catalyst containing nickel and molybdenum or nickel and tungsten, such as ICR250 (available from Advanced Refining Technologies LLC).

[0070]

[0165] In certain embodiments, the hydrocracking catalyst is a supported hydrocracking catalyst. In certain embodiments, the hydrocracking catalyst layer comprises or consists of one type of hydrocracking catalyst. In certain embodiments, the hydrocracking catalyst layer comprises or consists of two types of hydrocracking catalysts.

[0071]

[0166] Free-standing hydrotreating catalyst

[0167] In certain embodiments, the free-standing hydroprocessing catalyst is an unsupported hydroprocessing catalyst, i.e., not supported or attached to another material. Generally, free-standing hydroprocessing catalysts have a higher level of activity by volume than supported hydroprocessing catalysts.

[0072]

[0168] Examples of free-standing (or unsupported) hydrotreating catalysts include, but are not limited to, unsupported multimetallic catalysts prepared by sulfiding a precursor catalyst of the formula:

[0169] A v [(M P )OH) x (L) n y ] z (M VIB O4) where A is one monovalent cationic species; M P is a promoter metal having an oxidation state of +2 or +4 selected from one or more of Group IIA, IIB, IVA, and VIII metals (particularly Group VIII, e.g., Ni); L is an organic oxygen-containing ligand (e.g., maleate); M VIB is a Group VIB metal (e.g., one or more of Mo, W).

[0073]

[0170] An important aspect of the catalyst precursor (before sulfiding) is that it is in the hydroxide form.

[0171] In one embodiment, L is selected from carboxylates, carboxylic acids, aldehydes, ketones, the enolate form of an aldehyde, the enolate form of a ketone, and a hemiacetal, and combinations thereof.

[0074]

[0172] In one embodiment, A is a monovalent cation, such as NH + , other quaternary ammonium ions, organic phosphonium cations, alkali metal cations, and combinations thereof.

[0075]

[0173] In one embodiment where both molybdenum and tungsten are used as the Group VIB metals, the atomic ratio of molybdenum to tungsten (Mo:W) is within the range of about 10:1 to 1:10. In another embodiment, the ratio of Mo:W is between about 1:1 to 1:5. In an embodiment where molybdenum and tungsten are used as the Group VIB metals, the charge neutral catalyst precursor is represented by the formula A v [(M P )(OH) x (L) n y ] z (Mo t W t’ In yet another embodiment where molybdenum and tungsten are used as the Group VIB metals, some or all of the tungsten may be replaced with chromium, and the ratio of (Cr+W):Mo is in the range of about 10:1 to 1:10. In another embodiment, the ratio of (Cr+W):Mo is 1:1 to 1:5. In one embodiment where molybdenum, tungsten and chromium are the Group VIB metals, the charge neutral catalyst precursor is represented by the formula A v [(M P )(OH) x (L) n y ] z (Mo t W t’ Cr t” O4) precursor.

[0076]

[0174] In one embodiment, the promoter metal M P is at least a Group VIII metal, M P has an oxidation state of +2, and the catalyst precursor has the formula A v [(M P )(OH) x (L) n y ] z (M VIB O4), where (v-2+2z-x*z+n*y*z)=0.

[0077]

[0175] In one embodiment, the promoter metal M Pis a mixture of two Group VIII metals, for example Ni and Co. In yet another embodiment, M P is a combination of three metals, for example Ni, Co and Fe.

[0078]

[0176] M P In one embodiment where is a mixture of two Group IIB metals, e.g., Zn and Cd, the charge neutral catalyst precursor is represented by the formula A v [(Zn a CD a’ )(OH) x (L) y ] z (M VIB O4) precursor. M P In yet another embodiment where is a combination of three metals, such as Zn, Cd and Hg, the charge neutral catalyst precursor has the formula A v [(Zn a CD a’ Hg a” )(OH) x (L) n y ] z (M VIB O4) precursor.

[0079]

[0177] M P In one embodiment where is a mixture of two Group IVA metals, e.g., Ge and Sn, the charge neutral catalyst precursor has the formula A v [(Ge b ,Sn b’ )(OH) x (L) n y ] z (M VIB O4) precursor. M P In another embodiment where is a combination of three Group IVA metals, e.g., Ge, Sn and Pb, the charge neutral catalyst precursor has the formula A v [(Ge b Sn b’ Pba b” )(OH) x (L) n y ] z (M VIB O4) precursor.

[0080]

[0178] Promoter Metal Component M P In one embodiment, the promoter metal (M P The source of the promoter metal is in solution, with the entire amount of the promoter metal compound dissolved in the liquid to form a homogeneous solution. In another embodiment, the source of the promoter metal is partially present as a solid and partially dissolved in the liquid. In a third embodiment, the source of the promoter metal is entirely in a solid state.

[0081]

[0179] Promoter Metal Compound M P may be a metal salt or mixture of metal salts selected from nitrates, hydrated nitrates, chlorides, hydrated chlorides, sulfates, hydrated sulfates, carbonates, formates, acetates, oxalates, citrates, maleates, fumarates, phosphates, hypophosphites, and mixtures thereof.

[0082]

[0180] In one embodiment, the promoter metal M P is a nickel compound at least partially in a solid state, e.g., a water insoluble nickel compound such as nickel carbonate, nickel hydroxide, nickel phosphate, nickel phosphite, nickel formate, nickel fumarate, nickel sulfide, nickel molybdate, nickel tungstate, nickel oxide, a nickel alloy such as nickel-molybdenum alloy, Raney nickel, or mixtures thereof.

[0083]

[0181] In one embodiment, the promoter metal M P is selected from the group of IIB and VIA metals in their elemental, compound, or ionic form, such as zinc, cadmium, mercury, germanium, tin, or lead, and combinations thereof. In yet another embodiment, the promoter metal M P further comprises at least one of Ni, Co, Fe and combinations thereof in their elemental, compound, or ionic form.

[0084]

[0182] In one embodiment, the promoter metal compound is a zinc compound at least partially in the solid state, e.g., a zinc compound that is sparingly soluble in water, such as zinc carbonate, zinc hydroxide, zinc phosphate, zinc phosphite, zinc formate, zinc fumarate, zinc sulfide, zinc molybdate, zinc tungstate, zinc oxide, a zinc alloy, e.g., a zinc-molybdenum alloy.

[0085]

[0183] In one embodiment, the promoter metal is a Group IIA metal compound selected from the group of magnesium, calcium, strontium and barium compounds, at least a portion of which is in the solid state, e.g., a water-insoluble compound such as a carbonate, hydroxide, fumarate, phosphate, phosphite, sulfide, molybdate, tungstate, oxide, or mixtures thereof.

[0086]

[0184] In one embodiment, the promoter metal compound is a tin compound at least partially in the solid state, e.g., a tin compound that is sparingly soluble in water, such as tannic acid, tin phosphate, tin formate, tin acetate, tin molybdate, tin tungstate, tin oxide, or a tin alloy, e.g., a tin-molybdenum alloy.

[0087]

[0185] VIB group metal component: VIB group metal (M VIBThe compound may be added in a solid state, a partially dissolved state, or in a solution state. In one embodiment, the Group VIB metal compound is selected from molybdenum, chromium, tungsten compounds, and combinations thereof. Examples of such compounds include, but are not limited to, alkali metal, alkaline earth metal, or ammonium metallates of molybdenum, tungsten, or chromium (e.g., ammonium tungstate, ammonium meta-, para-, hexa-, or polytungstate, ammonium chromate, ammonium molybdate, ammonium iso-, peroxo-, di-, tri-, tetra-, hepta-, octa-, or tetradecamolybdate, alkali metal heptamolybdate, alkali metal orthomolybdate, or alkali metal isomolybdate), ammonium salts of phosphomolybdic acid, ammonium salts of phosphotungstic acid, ammonium salts of phosphochromate, molybdenum (di- and tri)oxide, tungsten (di- and tri)oxide, chromium or chromium oxide, molybdenum carbide, molybdenum nitride, aluminum molybdate, molybdic acid, chromate, tungstic acid, Mo-P heteropolyanion compounds, Wo-Si heteropolyanion compounds, WP heteropolyanion compounds. A W-Si heteropolyanion compound, a Ni-Mo-W heteropolyanion compound, a Co-Mo-W heteropolyanion compound, or a mixture thereof, added in the solid, partially dissolved, or solute state.

[0088]

[0186] Chelating agent (ligand) L: In one embodiment, the catalyst precursor composition comprises at least one non-toxic organic oxygen-containing ligand having an LD50 (as a single oral dose to rats) of more than 500 mg / kg. In a second embodiment, the organic oxygen-containing ligand L has an LD50 of more than 700 mg / kg. In a third embodiment, the organic oxygen-containing chelating agent has an LD50 of more than 1000 mg / kg. As used herein, the term "non-toxic" means that the ligand has an LD50 (as a single oral dose to rats) of more than 500 mg / kg. As used herein, the term "at least one organic oxygen-containing ligand" means that the composition may have two or more organic oxygen-containing ligands in some embodiments, and some of the organic oxygen-containing ligands may have an LD50 of less than 500 mg / kg, but at least one of the organic oxygen-containing ligands has an LD50 of more than 500 mg / kg.

[0089]

[0187] In one embodiment, the oxygen-containing chelating agent L is selected from the group of non-toxic organic acid addition salts such as formic acid, acetic acid, propionic acid, maleic acid, fumaric acid, succinic acid, tartaric acid, citric acid, oxalic acid, glyoxylic acid, aspartic acid, alkanesulfonic acids such as methanesulfonic acid and ethanesulfonic acid, arylsulfonic acids such as benzenesulfonic acid and p-toluenesulfonic acid, and arylcarboxylic acids such as benzoic acid. In one embodiment, the oxygen-containing chelating agent L is maleic acid (LD50 of 708 mg / kg).

[0090]

[0188] In another embodiment, the non-toxic chelating agent L is selected from the group consisting of glycolic acid (having an LD50 of 1950 mg / kg), lactic acid (LD50 of 3543 mg / kg), tartaric acid (LD50 of 7500 mg / kg), malic acid (LD50 of 1600 mg / kg), citric acid (LD50 of 5040 mg / kg), gluconic acid (LD50 of 10380 mg / kg), methoxy-acetic acid (LD50 of 3200 mg / kg), ethoxy-acetic acid (LD50 of 1292 mg / kg), malonic acid (LD50 of 1310 mg / kg), succinic acid (LD50 of 500 mg / kg), fumaric acid (LD50 of 10700 mg / kg), and glyoxylic acid (LD50 of 3000 mg / kg). In yet another embodiment, the non-toxic chelating agent is selected from the group of organosulfur compounds including, but not limited to, mercapto-succinic acid (LD50 of 800 mg / kg) and thio-diglycolic acid (LD50 of 500 mg / kg).

[0091]

[0189] In yet another embodiment, the oxygen-containing ligand L is a carboxylate-containing compound. In one embodiment, the carboxylate compound contains one or more carboxylate functional groups. In yet another embodiment, the carboxylate compound includes monocarboxylates, including but not limited to formates, acetates, propionates, butyrates, pentanoates, and hexanoates, and dicarboxylates, including but not limited to oxalates, malonates, succinates, glutarates, adipates, malates, maleates, fumarates, and combinations thereof. In a fourth embodiment, the carboxylate compound includes maleates.

[0092]

[0190] The organic oxygen-containing ligand may be mixed with a promoter metal-containing solution or mixture, a Group VIB metal-containing solution or mixture, or a combination of promoter metal and Group VIB metal-containing precipitates, solutions, or mixtures. The organic oxygen-containing ligand may be in solution with the entire amount of the organic oxygen-containing ligand dissolved in a liquid such as water. The organic oxygen-containing ligand may be partially dissolved and partially solid during mixing with the promoter metal(s), Group VIB metal(s), and combinations thereof.

[0093]

[0191] Diluent Component: The term diluent may be used interchangeably with binder. The use of a diluent is optional in the preparation of the catalyst precursor.

[0192] In one embodiment, a diluent is included in the process for making the catalyst precursor composition. In general, the diluent material added has lower catalytic activity than the catalyst prepared from the catalyst precursor composition (without the diluent) or has no catalytic activity at all. In one embodiment, the activity of the catalyst can be reduced by adding a diluent. Thus, the amount of diluent added in the process generally depends on the desired activity of the final catalyst composition. Depending on the envisioned catalyst application, a diluent amount of 0-95 wt% of the total composition can be suitable.

[0094]

[0193] The diluent may be added simultaneously or sequentially to the promoter metal component(s), promoter metal-containing mixture, Group VIB metal(s), or metal-containing mixture. Alternatively, the promoter metal and Group VIB metal mixture may be combined together and then the diluent may be added to the combined metal mixture. It is also possible to combine a portion of the metal mixture simultaneously or sequentially, then add the diluent, and finally add the remainder of the metal mixture simultaneously or sequentially. It is also possible to combine the diluent with the metal mixture in the solute state, and then add at least a portion of the metal compound in the solid state. An organic oxygen-containing ligand is present in at least one of the metal-containing mixtures.

[0095]

[0194] In one embodiment, the diluent is complexed with a Group VIB metal and / or a promoter metal prior to being complexed with the bulk catalyst precursor composition and / or added during its preparation. In one embodiment, complexing the diluent with any of these metals is carried out by impregnating the solid diluent with these metals.

[0096]

[0195] The diluent material includes any material conveniently applied as a diluent or binder in hydroprocessing catalyst precursors. Examples include silica, silica-alumina, such as conventional silica-alumina, silica-coated alumina and alumina-coated silica, alumina such as (pseudo)boehmite or gibbsite, titania, zirconia, cationic or anionic clays such as saponite, bentonite, kaolin, sepiolite or hydrotalcite, or mixtures thereof. In one embodiment, the binder material is selected from silica, aluminum-doped colloidal silica, silica-alumina, alumina, titania, zirconia, or mixtures thereof.

[0097]

[0196] These diluents can be applied as they are or after peptization. It is also possible to apply precursors of these diluents that are converted into any of the above-mentioned diluents during the process. Suitable precursors are, for example, alkali metal or ammonium aluminates (to obtain alumina diluents), water glass or ammonium- or acid-stabilized silica sol (to obtain silica diluents), mixtures of aluminates and silicates (to obtain silica-alumina diluents), mixtures of sources of divalent, trivalent and / or tetravalent metals, such as mixtures of water-soluble salts of magnesium, aluminum and / or silicon (to prepare cationic and / or anionic clays), chlorohydrol, aluminum sulfate, or mixtures thereof.

[0098]

[0197] Other optional components: If desired, in addition to the components mentioned above, other materials, including other metals, may be added. These materials include any metals that are added during conventional hydroprocessing catalyst precursor preparation. Suitable examples are phosphorus compounds, boron compounds, additional transition metals, rare earth metals, fillers, or mixtures thereof. Suitable phosphorus compounds include ammonium phosphate, phosphoric acid, or organic phosphorus compounds. The phosphorus compounds may be added at any stage of the process steps. Suitable additional transition metals that may be added to the process steps include, for example, rhenium, ruthenium, rhodium, iridium, chromium, vanadium, iron, cobalt, nickel, zinc, platinum, palladium, cobalt, and the like. In one embodiment, the additional metals are applied in the form of a water-insoluble compound. In another embodiment, the additional metals are added in the form of a water-soluble compound. Apart from adding these metals during the process, it is also possible to composite the final catalyst precursor composition with optional materials. For example, it is possible to impregnate the final catalyst precursor composition with an impregnation solution that includes any of these additional materials.

[0099]

[0198] Methods for making hydroprocessing catalyst precursors: The preparation methods allow for systematic variation of the composition and structure of the catalyst precursor by controlling the relative amounts of elements, the types of reagents, and the length and extent of the various reactions and reaction steps.

[0100]

[0199] The order of addition of the reagents used to form the catalyst precursor is not important. For example, the organic oxygen-containing ligand may be combined with a mixture of the promoter metal(s) and Group VIB metal(s) prior to precipitation or cogelation. The organic oxygen-containing ligand may be mixed with a solution of the promoter metal and then added to a solution of the Group VIB metal(s). The organic oxygen-containing ligand may be mixed with a solution of the Group VIB metal(s) and then added to a solution of the promoter metal(s).

[0101]

[0200] Formation of a precipitate or cogel with Group VIB / promoter metal: In one embodiment of the process, the first step is a precipitation or cogelation step, which involves reacting in a mixture a promoter metal component(s) in solution and a Group VIB metal component in solution to obtain a precipitate or cogel. The precipitation or cogelation is carried out at a temperature and pH at which the promoter metal compound and the Group VIB metal compound form a precipitate or cogel. An organic oxygen-containing ligand in solution or at least partially in solution is then combined with the precipitate or cogel to form one embodiment of the catalyst precursor.

[0102]

[0201] In one embodiment, the temperature at which the catalyst precursor is formed is between 50 and 150° C. If the temperature is below the boiling point of the protic liquid, e.g., below 100° C. for water, the process is generally carried out under atmospheric pressure. Above this temperature, the reaction is generally carried out under increased pressure, e.g., in an autoclave. In one embodiment, the catalyst precursor is formed at a temperature between 0 and 2068×10 4 In a second embodiment, the pressure is 69×10 4 ~689×10 4 Pa (100 to 1000 psig).

[0103]

[0202] The pH of the mixture may be altered to increase or decrease the rate of precipitation or cogelation depending on the desired properties of the product. In one embodiment, the mixture is maintained at its natural pH during the reaction step(s). In another embodiment, the pH is maintained within the range of 0-12. In another embodiment, the pH is 4-10. In a further embodiment, the pH is in the range of 7-10. The pH can be altered by adding a base or acid to the reaction mixture, or by adding hydroxide ions or H, which increase or decrease the pH, respectively, as the temperature increases. +This can be accomplished by adding compounds that break down into ions, examples of which include urea, nitrite, ammonium hydroxide, inorganic acids, organic acids, inorganic bases, and organic bases.

[0104]

[0203] In one embodiment, the reaction of the promoter metal compound(s) is carried out with water-soluble metal salts, such as zinc, molybdenum and tungsten metal salts. The solution may further include other promoter metal component(s), such as Group VIII metal compounds including cadmium or mercury compounds, such as Cd(NO3)2 or (CH3CO2)2Cd, cobalt or iron compounds, such as Co(NO3)2 or (CH3CO2)2Co, and Group VIB metal component(s), such as chromium.

[0105]

[0204] In one embodiment, the reaction of the promoter metal compound(s) is carried out with water-soluble tin, molybdenum and tungsten metal salts. The solution may further include other Group IVA metal component(s), for example lead compounds such as Pb(NO3)4 or (CH3CO2)2Pb, and other Group VIB metal compounds such as chromium compounds.

[0106]

[0205] The reaction is carried out with appropriate metal salts resulting in the precipitation or cogel combination of zinc / molybdenum / tungsten, tin / molybdenum / tungsten, zinc / molybdenum, zinc / tungsten, tin / molybdenum, tin / tungsten, or zinc / tin / molybdenum / tungsten, or nickel / molybdenum / tungsten, cobalt / molybdenum / tungsten, nickel / molybdenum, nickel / tungsten, cobalt / molybdenum, cobalt / tungsten, or nickel / cobalt / molybdenum / tungsten. The organic oxygen-containing ligand may be added before or after the precipitation or cogelation of the promoter metal compound and / or Group VIB metal compound.

[0107]

[0206] The metal precursors may be added to the reaction mixture as a solution, a suspension, or a combination thereof. If a soluble salt is so added, it dissolves in the reaction mixture and then precipitates or co-gels. The solution may be heated, optionally under vacuum, to achieve precipitation and evaporation of water.

[0108]

[0207] After precipitation or cogelation, the catalyst precursor may be dried to remove water. Drying may be performed under atmospheric conditions or under an inert atmosphere such as nitrogen, argon or vacuum. Drying may be accomplished at a temperature sufficient to remove water without removing organic compounds. Preferably, drying is performed at about 120° C. until the weight of the catalyst precursor reaches a constant value.

[0109]

[0208] Formation of a precipitate with optional binder component(s): In one embodiment using a binder, the binder component may be added to a reaction mixture containing the metal precursor in solution, suspension, or a combination thereof to form a precipitate or cogelation. The precipitate is then dried to remove water.

[0110]

[0209] In one embodiment using magnesium aluminosilicate clay as a binder, a first reaction mixture is formed that includes a silicon component, an aluminum component, a magnesium component, a promoter metal compound, and / or a Group VIB metal compound. In one embodiment, the first reaction mixture is formed under ambient pressure and temperature conditions. In one embodiment, the reaction is carried out at a pressure in the range of 0.9 bar to 1.2 bar, and at a temperature of about 0° C. to 100° C.

[0111]

[0210] Examples of silicon components include, but are not limited to, sodium silicate, potassium silicate, silica gel, silica sol, hydronium-stabilized or ammonium-stabilized silica sol, and combinations thereof. Examples of aluminum of the aluminum component useful in the process of the present invention include, but are not limited to, sodium aluminate, potassium aluminate, aluminum sulfate, aluminum nitrate, and combinations thereof. Examples of magnesium components useful in the process of the present invention include, but are not limited to, magnesium metal, magnesium hydroxide, magnesium halides, magnesium sulfate, and magnesium nitrate. In one embodiment, an acid is added to the mixture containing the metal precursor and binder component in an amount sufficient to adjust the pH of the mixture to about 1 to about 6 to form a first reaction mixture.

[0112]

[0211] After formation of the first reaction mixture, an alkali base is added to form a second reaction mixture. Examples of alkali bases include, but are not limited to, ammonium hydroxide, sodium hydroxide, and potassium hydroxide. Sufficient alkali base is added to the first reaction mixture such that the resulting second reaction mixture has a pH of about 7 to about 12. The second reaction mixture is then reacted for a sufficient time and at a sufficient temperature to form a catalyst precursor incorporating at least clay as a binder. In an embodiment, the time is at least 1 second. In a second embodiment, the time is 15 minutes. In a third embodiment, the time is at least 30 minutes. The temperature of the second reaction mixture may range from about 0° C. to about 100° C. The reaction may be carried out at ambient pressure, although higher or lower pressures are not excluded.

[0113]

[0212] In one embodiment using magnesium aluminosilicate clay as the binder, the ratio of silicon to aluminum to magnesium can be expressed in terms of elemental molar ratios of aSi:bAl:cMg, where "a" has a value from 3 to 8, "b" has a value from 0.6 to 1.6, and "c" has a value from 3 to 6.

[0114]

[0213] Characterization of the catalyst precursor: Characterization of the charge neutral catalyst precursor can be performed using techniques known in the art, including, but not limited to, powder X-ray diffraction (PXRD), elemental analysis, surface area measurements, average pore size distribution, average pore volume. Porosity and surface area measurements can be performed using BJH analysis under BET nitrogen adsorption conditions.

[0115]

[0214] Properties of the catalyst precursor: In one embodiment, the catalyst precursor has an average pore volume of 0.05-5 mL / g as determined by nitrogen adsorption. In another embodiment, the average pore volume is 0.1-4 mL / g. In a third embodiment, the average pore volume is 0.1-3 mL / g.

[0116]

[0215] In one embodiment, the catalyst precursor is at least 10 2 In a second embodiment, the catalyst precursor has a surface area of ​​at least 50 m 2 In a third embodiment, the catalyst precursor has a surface area of ​​at least 150 m 2 / g surface area.

[0117]

[0216] In one embodiment, the catalyst precursor has an average pore size, as defined by nitrogen adsorption, of 2 to 50 nanometers. In a second embodiment, the catalyst precursor has an average pore size of 3 to 30 nanometers. In a third embodiment, the catalyst precursor has an average pore size of 4 to 15 nanometers.

[0118]

[0217] In one embodiment containing magnesium aluminosilicate clay as a binder, the catalyst precursor is a layered material composed of stacks of elementary clay platelets.

[0218] Forming process: In one embodiment, the catalyst precursor composition can be directly formed into various shapes, generally depending on the intended commercial application. These shapes can be made by any suitable technique, such as extrusion, pelletizing, beading, or spray drying. If the amount of liquid in the bulk catalyst precursor composition is too large to be directly subjected to the forming step, a solid-liquid separation can be performed before forming.

[0119]

[0219] Addition of pore formers: The catalyst precursor may be mixed with a pore former, including, but not limited to, stearic acid, polyethylene glycol polymers, carbohydrate polymers, methacrylates, and cellulose polymers. For example, the dried catalyst precursor may be mixed with a cellulose-containing material, such as methylcellulose, hydroxypropylcellulose, or other cellulose ethers, in a ratio of 100:1 to 10:1 (wt.% catalyst precursor to wt.% cellulose), and water may be added until an extrudable mixture is obtained. Examples of commercially available cellulose-based pore formers include, but are not limited to, METHOCEL™ (available from DuPont), Avicel® (available from DuPont), and Porocel (available from Evonik). The extrudable mixture may be extruded and then optionally dried. In one embodiment, drying may be performed under an inert atmosphere, such as nitrogen, argon, or vacuum. In another embodiment, drying may be performed at elevated temperatures, between 70 and 200°C. In yet another embodiment, drying is performed at 120°C.

[0120]

[0220] Sulfiding Agent Component: The charge-neutral catalyst precursor may be sulfided to form an active catalyst. In one embodiment, the sulfiding agent is elemental sulfur itself. In another embodiment, the sulfiding agent is a sulfur-containing compound capable of decomposing into hydrogen sulfide under prevailing conditions. In yet a third embodiment, the sulfiding agent is H2S itself or H2S in H2.

[0121]

[0221] In one embodiment, the sulfiding agent is ammonium sulfide, ammonium polysulfide ((NH4)2S x), ammonium thiosulfate ((NH4)2S2O3), sodium thiosulfate (Na2S2O3), thiourea (NH2CSNH2), carbon disulfide, dimethyl disulfide (DMDS), dimethyl sulfide (DMS), mercaptans, di-tert-butyl polysulfide (TBPS), tert-nonyl polysulfide (TNPS), and the like. In another embodiment, the sulfiding agent is selected from alkali and / or alkaline earth metal sulfides, alkali and / or alkaline earth metal hydrogen sulfides, and mixtures thereof. The use of sulfiding agents containing alkali and / or alkaline earth metals may require an additional separation process step to remove the alkali and / or alkaline earth metals from the spent catalyst.

[0122]

[0222] In one embodiment, the sulfiding agent is ammonium sulfide in an aqueous solution, which can be synthesized from hydrogen sulfide and ammonia refinery off-gas. The synthetic ammonium sulfide is readily soluble in water and can be easily stored as an aqueous solution in a tank prior to use. In one embodiment, the sulfiding is with an aqueous ammonium sulfide solution and is carried out in the presence of at least one sulfur additive selected from the group of thiadiazoles, thioacids, thioamides, thiocyanates, thioesters, thiophenols, thiosemicarbazides, thioureas, mercaptoalcohols, and mixtures thereof.

[0123]

[0223] In one embodiment, a hydrocarbon feedstock is used as a sulfur source to sulfurize the catalyst precursor. The sulfurization of the catalyst precursor with the hydrocarbon feedstock can be carried out in one or more hydroprocessing reactors during hydroprocessing.

[0124]

[0224] In one embodiment, the sulfiding agent is present in an amount greater than the stoichiometric amount required to form the sulfided catalyst from the catalyst precursor. In another embodiment, the amount of sulfiding agent corresponds to a molar ratio of sulfur to Group VIB metal of at least 3 to 1 to produce the sulfided catalyst from the catalyst precursor. In a third embodiment, the total amount of sulfur-containing compound is generally selected to correspond to any of about 50-300%, 70-200%, and 80-150% of the stoichiometric amount of sulfur required to convert the metal to, for example, Co9S8, MoS2, WS2, Ni3S2, and the like.

[0125]

[0225] Sulfiding step: Sulfiding of the catalyst precursor to form the catalyst (sometimes referred to as "pre-sulfiding") may be carried out prior to introducing the catalyst into the hydroprocessing reactor (hence ex-situ sulfiding). In another embodiment, the sulfiding is in-situ. In one embodiment, where the sulfiding process is carried out ex-situ, the formation of undesirable compounds within the hydroprocessing unit is prevented. In one embodiment, the catalyst precursor is converted to an active catalyst upon contact with a sulfiding agent at a temperature in the range of 70°C to 500°C, for a period of 10 minutes to 15 days, and under H2-containing gas pressure. When the sulfiding temperature is below the boiling point of the sulfiding agent, e.g., below 60-70°C for ammonium sulfide solution, the process is generally carried out under atmospheric pressure. Above the boiling point of the sulfiding agent / optional components, the reaction is generally carried out under increased pressure.

[0126]

[0226] In one embodiment, sulfurization can be carried out in a gas phase containing hydrogen and a sulfur-containing compound decomposable to H2S. Examples include mercaptans, CS2, thiophenes, DMS, DMDS, and suitable S-containing refinery tailings. The use of H2S alone is sufficient. Contacting the catalyst precursor in the gas phase with hydrogen and a sulfur-containing compound can be carried out in one step at a temperature of 125°C to 450°C (257°F to 842°F) in one embodiment, and 225°C to 400°C (437°F to 752°F) in another embodiment. In one embodiment, sulfurization is carried out while gradually increasing the temperature for a period of time, for example, 0.5 to 4°C (0.9 to 7.2°F) per minute, and held for a period of time until completion, for example, 1 to 12 hours.

[0127]

[0227] As used herein, completion of the sulfurization process means that at least 95% of the stoichiometric amount of sulfur required to convert the metal to, for example, Co9S8, MoS2, WS2, Ni3S2, etc. has been consumed.

[0128]

[0228] In another embodiment of sulfurization in the gas phase, the sulfurization is carried out in two or more steps, the first step being carried out at a lower temperature than the subsequent step(s). For example, the first step is carried out at about 100-250°C (212°F-482°F), preferably about 125-225°C (257°F-437°F). After a short period of time, for example 30 minutes to 2 hours (temperature is kept constant), the second step can be carried out at about 225-450°C (437°F-842°F), preferably about 250-400°C (482°F-752°F). The total pressure during the sulfurization step may be from atmospheric pressure to about 10 bar (1 MPa). The gas mixture of H2 and sulfur-containing compounds may be the same or different in the steps. Sulfidation in the gas phase can be carried out in any suitable manner, including fixed bed processes and moving bed processes in which the catalyst moves relative to the reactor, such as ebullated bed processes and rotary furnaces.

[0129]

[0229] In one embodiment, sulfidation is carried out in the liquid phase. First, the catalyst precursor is contacted with an organic liquid in an amount ranging from 20 to 500% of the catalyst precursor pore volume. Contact with the organic liquid may be carried out at a temperature ranging from ambient temperature to 250° C. (482° F.). After introduction of the organic liquid, the catalyst precursor is contacted with hydrogen and a sulfur-containing compound.

[0130]

[0230] In one embodiment, the organic liquid has a boiling range of about 100-550° C. (212-1022° F.). In another embodiment, the organic liquid is a petroleum fraction, such as heavy oil, a lubricating oil fraction, such as mineral lubricating oil, atmospheric gas oil, vacuum gas oil, straight run gas oil, white spirits, middle distillates, such as diesel, jet fuel and kerosene, naphtha, and gasoline. In one embodiment, the organic liquid contains less than 10 wt.% sulfur, preferably less than 5 wt.% sulfur.

[0131]

[0231] In one embodiment, sulfidation in the liquid phase (or "start-up") is carried out as a "fast" process, where the sulfidation is carried out over a period of less than 72 hours with a temperature increase in the range of 0.5-4°C (0.9-7.2°F) per minute. In a second embodiment, the fast start-up takes less than 48 hours. In a third embodiment, the fast start-up takes less than 24 hours.

[0132]

[0232] In fast sulfurization, contacting the catalyst precursor in an organic liquid with hydrogen and a sulfur-containing compound can be carried out in one step at a temperature of 150-450°C in one embodiment, and 225°C-400°C in another embodiment. In yet another embodiment of fast sulfurization, the sulfurization is carried out in two or more steps, the first step being carried out at a lower temperature than the subsequent step(s). For example, the first step is carried out at about 100-250°C (212°F-482°F), or 125-225°C (257°F-437°F). After a short period of time, for example 0.5-2 hours (temperature is held constant), the temperature is raised in a second step, for example to 250-450°C (482°F-842°F), preferably 225°C-400°C (437°F-752°F). The temperature is maintained for 1-36 hours, after which time the sulfurization is complete.

[0133]

[0233] In yet another embodiment, sulfurization in the liquid phase is carried out as a "slow" process, where the sulfurization is carried out for a period of 4 days to 3 weeks, i.e., for at least 96 hours. In this slow process, contacting the catalyst precursor in the organic liquid with hydrogen and a sulfur-containing compound is carried out in two or more steps, where the first step is carried out at a lower temperature than the subsequent step(s) and the temperature is slowly ramped up, e.g., every hour instead of every minute as in the case of a fast start-up. The gas mixture of H2 and sulfur-containing compound may be the same or different in the steps. In one embodiment, the first step is carried out at about 100-375°C (212°F-707°F), preferably about 125-350°C (257°F-662°F), with a temperature ramp rate of 0.25-4°C (0.45-7.2°F) per hour. After the first step, the temperature is held constant for a period of 2 to 24 hours and then increased at a rate of 5 to 20°C (9 to 36°F) per hour in the second step. In one embodiment, the second step is carried out at about 200 to 450°C (392°F to 842°F), preferably about 225 to 400°C (437°F to 752°F).

[0134]

[0234] In one embodiment, sulfurization is carried out with elemental sulfur, which is incorporated into the pores of the catalyst precursor. In this process, elemental sulfur is mixed with the catalyst precursor at a temperature below the melting point of sulfur in an amount of 2-15 wt.% of the catalyst precursor weight. In one embodiment, mixing is carried out at 180-210°F (82-99°C). Continuously or simultaneously with mixing of the precursor and elemental sulfur, the mixture is contacted with a high boiling organic liquid. The mixture is then heated to a temperature within the range of 250-390°F (121-199°C) in the presence of nitrogen to produce H2S and metal sulfides. In one embodiment, the organic liquid is selected from the group consisting of olefins, gasoline, white spirits, diesel, gas oil, mineral oil lubricants, and white oil.

[0135]

[0235] In one embodiment, catalysts sulfided from catalyst precursor embodiments are surprisingly found to provide approximately the same 700°F (371°C)+ conversion whether sulfided via the gas phase or in the liquid phase as a "fast" process. In one embodiment, the 700°F (371°C)+ conversion is found to increase by at least 25% using catalysts sulfided via a "slow" process in the liquid phase. In yet another embodiment, the 700°F+ (371°C) conversion is doubled with catalysts sulfided via the slow process.

[0136]

[0236] In certain embodiments, the self-supporting hydrotreating catalyst comprises nickel, molybdenum, and tungsten. In certain embodiments, the self-supporting hydrotreating catalyst comprises nickel, molybdenum, tungsten, and titanium. In certain embodiments, the self-supporting hydrotreating catalyst comprises nickel, molybdenum, tungsten, and niobium. In certain embodiments, the self-supporting hydrotreating catalyst comprises nickel, molybdenum, tungsten, niobium, and titanium. In certain embodiments, the self-supporting hydrotreating catalyst comprises nickel, molybdenum, tungsten, niobium, and copper. In certain embodiments, the self-supporting hydrotreating catalyst comprises nickel, molybdenum, tungsten, niobium, and copper.

[0137]

[0237] In certain embodiments, the freestanding hydrotreating catalyst comprises about 5 to about 9 wt% molybdenum, about 21 to 31 wt% nickel, and about 33 to about 42 wt% tungsten. In certain embodiments, the freestanding hydrotreating catalyst comprises about 5.9 to about 8.1 wt% molybdenum, about 21.8 to 30.7 wt% nickel, and about 34.4 to about 41.3 wt% tungsten.

[0138]

[0238] A preferred catalyst precursor is a maleated Ni-Mo-W catalyst precursor. The catalyst is preferably sulfided with dimethyl sulfide (DMDS).

[0239] In certain embodiments, the free-standing hydrotreating catalyst is a catalyst containing nickel, molybdenum and tungsten, such as ICR1000, ICR1001, ICR1003 and ICR4000 (all available from Advanced Refining Technologies LLC).

[0139]

[0240] In certain embodiments, the free-standing hydroprocessing catalyst layer comprises or consists of one free-standing hydroprocessing catalyst. In certain embodiments, the free-standing hydroprocessing catalyst layer comprises or consists of two hydrocracking catalysts.

[0140]

[0241] Hydrocarbon Feedstock

[0242] A wide range of petroleum and chemical feedstocks can be hydrotreated (or hydrotreated) by the layered catalytic reactor system and method. Suitable feedstocks include whole crude oil and atmospheric resids, atmospheric and vacuum residues, propane deasphalted residues, such as bright stocks, cycle oils, FCC bottoms, gas oils including atmospheric and vacuum gas oils and coker gas oils, light to heavy distillates including raw distillates, hydrocrackates, hydrotreated oils, dewaxed oils, slack wax, Fischer-Tropsch wax, raffinates, naphtha, and mixtures of these materials. Typical lighter feeds include distillate fractions that generally boil between about 175°C (about 350°F) and about 375°C (about 750°F). This type of feed produces significant amounts of hydrocracked naphtha, which can be used as a low sulfur gasoline blendstock. Typical heavier feeds include, for example, vacuum gas oil boiling up to about 593°C (about 1100°F), usually in the range of about 350°C to about 500°C (about 660°F to about 935°F), in which case the percentage of diesel fuel produced is correspondingly higher.

[0141]

[0243] Processes for hydrotreating hydrocarbon feedstocks

[0244] In one aspect, the present invention relates to a process for hydrotreating a hydrocarbon feedstock, the process comprising: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen and olefins with a layered catalytic reactor system as described herein in the presence of hydrogen to produce a hydrocarbon product having a lower content of metals, sulfur, nitrogen and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically from top to bottom through the layers of the layered catalytic reactor system in sequence; and (iii) recovering a hydrocarbon product from the bottom of the layered catalytic reactor system. The process can be used to remove impurities or contaminants such as metals, sulfur and nitrogen, as well as to saturate olefins and aromatics from the hydrocarbon feedstock. The method is carried out under conditions that promote hydrodemetallization, hydrodesulfurization, and hydrodenitrogenation.

[0142]

[0245] In one embodiment, the process operates by introducing a feed containing high levels of sulfur and nitrogen into a first treatment reaction stage, converting a substantial amount of the sulfur and nitrogen in the feed to inorganic forms, the primary objective of this step being the reduction of the feed nitrogen content. The hydrotreating step is carried out in an exemplary layered catalytic reactor system in the presence of hydrogen. The conditions used are appropriate for hydrodesulfurization and / or denitrification, depending on the characteristics of the feed. The product stream is then passed directly (without separation) or with separation and water washing to a hydrocracking zone, where conversion in the boiling range is achieved. The product streams from the first and second layers in the exemplary system may be passed to a separator along with hydrotreating gas and other hydrotreating / hydrocracking reaction products, including hydrogen sulfide and ammonia, where hydrogen, light ends and inorganic nitrogen and hydrogen sulfide are removed from the hydrocracked liquid product stream. The recycle gas may be washed for ammonia removal and may be subjected to an amine scrub for hydrogen sulfide removal, with the aim of improving the purity of the recycle hydrogen and thus reducing the product sulfur level.

[0143]

[0246] The product stream then proceeds to hydrocracking and a free-standing catalyst bed for treatment. In certain embodiments, removal of "hard sulfur" species, i.e., sulfur species having atmospheric boiling points within the range of about 93°C to about 593°C (200°F to about 1100°F), particularly within the range of about 350°C to about 500°C (660°F to about 935°F). EXAMPLES

[0144]

[0247] The disclosed embodiments are further illustrated by the following examples, which should not be construed as limiting the scope of the disclosure in any way. Various other aspects, embodiments, modifications, and equivalents thereof, which do not depart from the scope of the disclosure, may become apparent to those skilled in the art upon reading the description herein.

[0145]

[0248] Example 1 This study explores the hydroprocessing of products obtained from the LC Fining process. Tests were conducted using LC Finate material based on Arab medium oil and Ural based feed.

[0146] Bench Scale Unit (BSU), Catalyst System, and Feeds

[0245] Several bench-scale units were used in this study (BSU607, 612, and 911). Several catalyst systems were tested in separate runs in BSU607 (Runs 56-62), BSU612 (Runs 37-41), and BSU911 (Runs 160-161).

[0147] The layered catalyst reactor system used is described in Table 1. A total extrudate was shortened to an L / D of 1-2 and packed with about 100 mesh alundum to prevent bypass and channeling. One of the main goals of this study was the evaluation of ICR1000 / 1001 performance in the upgrading of the load feed proposition. Catalyst systems containing about 10% to about 20% ICR1000 and / or about 14% to about 44% ICR1001 were explored. Comparative examples included catalyst systems with ICR183 and ICR191 as hydrocracking catalysts. ICR250 was used in conjunction with ICR1000 and was typically positioned before (above) ICR1000 or ICR1001. One comparative example included a catalyst system containing only ICR250 (no ICR1000 or ICR1001).

[0148]

[0247]

[0149] [Table 1-1]

[0150] [Table 1-2]

[0151]

[0248]

[0249] The feeds used in most units were heavy vacuum gas oil (HVGO) from the LC Fining unit (ABQ1560) and 900°F (482°C) VGO (ABQ1967) derived from this feed. ABQ1560 consists of 75% LC finate HVGO and 25% straight run (SR) HVGO. A blend of ABQ1560 with SRC HVGO to achieve a 50% blend of LC finer product with HVGO was used to evaluate the dilution effect on activity / stability (TGQ9588). Additional feeds used were based on Urals derived feeds from RAM (Milazzo Refinery LC Finer HVGO, TGQ9989) diluted with SRC HVGO to a 50 / 50 blend (CGQ0003) and Neste (Neste LC Finer Heavier VGO, ABQ1956) diluted with SRC HVGO to a 50 / 50 blend (CGQ0107). The properties of the feeds used are shown in Table 2. Descriptions of the feed samples are set forth in Table 2 below.

[0152]

[0250]

[0153] [Table 2-1]

[0154] [Table 2-2]

[0155]

[0251]

[0252]

[0253]

[0254]

[0255]

[0256]

[0257]

[0258]

[0259]

[0156]

[0260] Catalyst sulfidation

[0261] The catalytic system was sulfided prior to use with DMDS-infused VGO.

[0157]

[0262] - The reactor was heated to 250°F (121°C) and held under nitrogen flow (no feed flow, 200 mL / min nitrogen flow) at ambient pressure for 1 hour.

[0263] - Change to hydrogen with a flow rate of 321 mL / min and a pressure of 552 x 10 4 The pressure was increased to 800 psig (800 psig).

[0158]

[0264] - Changed to sulfurization feed (2.5 wt% DMDS in diesel) at 13.45 / h (LHSV=1.3 / h) and hydrogen rate to 255 mL / min (5500 SCF / bbl hydrogen) and held for 10 hours.

[0159]

[0265] - The reactor temperature was increased at 17°C (30°F) / h to 250°C (482°F) and held for 5 hours.

[0266] - The reactor temperature was increased at 17°C (30°F) / h to 300°C (572°F) and held for 5 hours.

[0160]

[0267] - Reactor temperature was increased at 17°C (30°F) / h to 343°C (650°F) and held for 6 hours.

[0268] - Change to diesel ABQ0920 with speed of 5.17g / h (LHSV=0.5 / h) and pressure of 1620×10 4 The pressure was increased to 2350 psig (200 psi) and the hydrogen flow rate was reduced to 5000 scf / bbl (89.07 ml / min) and continued for 3 days to de-edge the catalyst.

[0161]

[0269] Test conditions

[0270] The process conditions for the run were as follows:

[0271] 0.40 / h LHSV (0.50 / h LHSV without demetallization catalyst ICR132) and 0.8 / h LHSV (1.0 / h LHSV without demetallization catalyst ICR132)

[0272] 1620×10 4 Total pressure (1551 x 10 4 Inlet H2 partial pressure of 2250 psi (Pa)

[0273] 1.424×m 3 / l(8000SCFB) 1 time by H2

[0274] - Reactor temperatures ranged from 377°C (710°F) to 407°C (765°F) to achieve targets with different feeds.

[0162]

[0275] - Two strippers were used in unit 607 / 612 with target cut points of 149°C (300°F) and 371°C (700°F).

[0276] - One stripper was used for unit 911 with a target cut point of 371°C (700°F).

[0163]

[0277] - S was targeted to be less than 100 ppm in the total liquid product (WLP) and less than 30 ppm in the diesel fraction (V3O sample) for the two stripper units.

[0278] - N was targeted to be less than 40 ppm in the WLP.

[0164]

[0279] All products (gas, STO, STB or V3O / V3B) were analyzed by SimDist for yield structure calculations.

[0280] The STB or V3O / V3B products were further analyzed for sulfur and nitrogen. Additional analyses were performed for selected yield periods.

[0165]

[0281] These above conditions were chosen as the initial test method with ABQ1560 which is considered a very difficult feed. A recent LC Max hydrotreater / hydrocracker design information (see EDP CLG Hydrocracking / Hydrotreating Technology Shandong Sincier Petrochemical Co Ltd, Vol. 1, September 2014) shows different conditions, namely:

[0282] - 1517×10 4 Reactor inlet pressure of 2200 psi (1379 x 10 4 Average hydrogen partial pressure in Pa (2000 psi).

[0166]

[0283] - The inlet gas to oil ratio is less than 89.07ml / min (5000SCF / bbl) compared to 142.51ml / min (8000SCF / bbl) in our first test case.

[0167]

[0284] - LHSV is 0.7 / h compared to 0.4 / 0.8 / h.

[0285] - The feed is a blend of 45 vol% LC finer product and 55 vol% SR HVGO.

[0168]

[0286] - LC finer HVGO has a distillate EP of 952°F (511°C) with about 22% boiling above 482°F (900°F).

[0287] The additional feeds described in Table 2 and used later in this study addressed this issue, resulting in feed / reaction conditions that more closely resembled the Sincier design.

[0169]

[0288] Feed conversion was generally performed under two different conditions to estimate the activation energies of HCR / HDN / HDS and calculate normalized temperatures. Temperature normalization was generally targeted at 40 ppm nitrogen, 100 ppm sulfur, and 30% hydrocracking to a 371°C (700°F) fraction.

[0170]

[0289] Results and Discussion

[0290] The run conditions and completed run test results for BSU607-56-61, BSU911-160 and 161, and 612-37-40 are shown in Tables 3, 4, 5, and 6 (values ​​shown are averages over multiple 24 hour yield periods).

[0171]

[0291]

[0172] [Table 3-1]

[0173] [Table 3-2]

[0174] [Table 3-3]

[0175]

[0292]

[0176] [Table 4-1]

[0177] [Table 4-2]

[0178]

[0293]

[0179] [Table 5-1]

[0180] [Table 5-2]

[0181]

[0294]

[0182] [Table 6-1]

[0183] [Table 6-2]

[0184]

[0295] Normalized temperatures for hydrocracking to fractions below 371°C (700°F), (HCR<371°C (700°F), 30%), hydrodenitrogenation (HDN, 40 ppm) and hydrodesulfurization (HDS, 100 ppm) are shown in Figures 1-10 along with the actual reactor temperatures and calculated activation energies.

[0185]

[0296] For the large amount of the heaviest feed ABQ1560 boiling above 482°C (900°F), stable operation could not be achieved with either catalyst system. The base case (no ICR1000) and 10%ICR250 / 10%ICR1000 showed high deactivation within the range of 6°C (10°F) / 1000 hours (Figures 1 and 2), while the 10%ICR250 / 20%ICR1000 catalyst system showed increased stability (about 2°C (4°F) / 1000 hours, Figure 3), which was lost when the ICR1000 content was increased to 44% (Figure 4). Compared to the base case, the activity advantage of using ICR1000 can be as high as 11°C (20°F). In Figure 3, the spike in normalized temperature with time for about 400 h of stream is due to the previous feed loss of more than 36 hours, which resulted in an activity penalty after restart.

[0186]

[0297] Diluting ABQ1560 (a 75 / 25 blend of full range LC Finate VGO and SR HVGO) to a 50 / 50 blend of LC Finate and SR HVGO (TGQ9588) gave stable operation in the base case with ICR191 (which is considered to have the same activity as ICR183) for both HDN and HDS. At the low LHSV of 0.4 / h, the temperature required for 40 ppm N and 100 ppm S was 382°C-387°C (720°F-730°F), but increased by over 17°C (30°F) at the higher LHSV of 0.8 (Figure 5), which is closer to the space velocity required for conversion of this feed.

[0187]

[0298] Testing of a 50 / 50 blend of RAM LC Finate and SR HVGO, i.e., CGQ0003, at an LHSV of 0.8 / h showed stable performance with improved activity above 8°C (15°F) (Figure 6), likely due to less 482+°C (900+°F) material (about 25 wt.% in the RAM vs. about 50 wt.% in the GSC feed). Dilution of the LC Finate product is one approach to achieve the required performance.

[0188]

[0299] ABQ1967 was prepared from ABQ1560 by distillation to a lower cut point, which contained about 15 wt.% 482°C (900°F)+ material with an end point of about 499°C (930°F). This feed was tested with the base catalyst system (containing ICR191) and compared to systems containing 34% and 44% ICR1000. Comparison of the base system with diluted ABQ1560 (612-37, Figure 5) and undiluted ABQ1967 (612-39, Figure 9) showed similar activity and stable performance at LHSVs of 0.4 / h and 0.8 / h, suggesting that reducing the 482+°C (900+°F) content of the feed has a similar effect on catalyst system stability / activity as dilution. Comparison of the base case with the 44% ICR1000 case (Figure 10) showed a decrease in stability for the 44% ICR1000 case, with an activity advantage in the range of 6°C (10°F). We started a run with ABQ1967 for a catalyst system containing 34% ICR1000 to check whether there were heat management issues with the 44% ICR1000, as observed with the ABQ1560 feed (see above).

[0189]

[0300] The feed closest to the Sincier design conditions was CGQ0107 / CGQ0520, made from Neste LC Finate and SRC HVGO in a 50 / 50 blend. This feed has been tested so far with 34% ICR1000 and 44% ICR1000, and is currently being tested with a 55% ICR250 system without ICR1000. The difference between these two cases is small, with the 44% ICR1000 system having slightly lower activity in HDN. This may also be due to the fact that the 44% ICR1000 system was first used for ABQ1560 conversion and showed a high deactivation rate. In both cases, the total sulfur and nitrogen contents can be maintained below 40 ppm S and 30 ppm N within the 386-391°C (726-736°F) temperature range, with values ​​as low as 7 ppm N and 15 ppm S (see Table 3).

[0190]

[0301] The diesel yield in all cases varied between 13% and 32% depending on the conversion. Figure 11 shows that the diesel yield depended more on the feed composition than on the catalyst system, with the RAM-based feed giving the highest yield at the same conversion.

[0191]

[0302] Observations

[0303] 1. Catalyst system stability depends on LC Finate cut point and dilution. Dilution to at least a 50 / 50 blend, as well as decreasing end points and overall 482+°C (900+°F) material improves system activity / stability.

[0192]

[0304] 2. The addition of ICR1000 significantly improves hydrodenitrogenation (HDN) and hydrodesulfurization (HDS) activity, but higher ICR1000 contents do not seem to show any improvement compared to those shown by the 34% and 44% ICR1000 cases.

[0193]

[0305] 3. Without ICR1000, low levels of nitrogen / sulfur (<10 ppm / 30 ppm) cannot be achieved at the required start-up temperature of approximately 388°C (730°F).

[0306] 4. Diesel yields at the same conversion (177-371°C (350-700°F) range) depend more on the feed composition than on the catalyst system for the feeds and catalyst systems tested. Specific embodiments of the present invention are as follows. [Aspect 1] From the top to the bottom, (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) one or more layers of free-standing hydroprocessing catalyst; (vii) a layer of one or more supported hydroprocessing catalysts. wherein the total volume of the two layers containing the one or more self-supporting hydroprocessing catalysts is about 10% to about 50% of the total volume of catalyst in the vertical bed; A layered catalytic reactor system, wherein the total volume of the two layers containing the one or more supported hydrocracking catalysts is about 10 to about 30% of the total volume of catalyst in the vertical bed. [Aspect 2] 2. The layered catalyst reactor system of embodiment 1, wherein the one or more free-standing hydroprocessing catalysts comprise about 5 to about 9 wt. % molybdenum, about 21 to 31 wt. % nickel, and about 33 to about 42 wt. % tungsten. [Aspect 3] 2. The layered catalytic reactor system of embodiment 1, wherein the one or more demetallization catalysts are selected from the group consisting of synthetic aluminum oxides or natural aluminum silicates enriched with oxides of molybdenum, cobalt, and nickel. [Aspect 4] 2. The layered catalytic reactor system of embodiment 1, wherein the one or more free-standing hydroprocessing catalysts are selected from the group consisting of catalysts comprising at least one Group VIII metal and at least one Group VIB metal on a support material selected from the group consisting of alumina, zeolite, amorphous silica-alumina, and titania-alumina. [Aspect 5] 2. The layered catalytic reactor system of embodiment 1, wherein the one or more supported hydroprocessing catalysts are selected from the group consisting of Pd or Pt containing catalysts. [Aspect 6] 2. The layered catalytic reactor system of embodiment 1, wherein the one or more hydrocracking catalysts are selected from the group consisting of nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and catalysts comprising nickel-tungsten and / or nickel-molybdenum. [Aspect 7] 2. The layered catalytic reactor system of embodiment 1, wherein the one or more hydrocracking catalysts comprise a porous support material comprising a refractory oxide material. [Aspect 8] 2. The layered catalytic reactor system of embodiment 1, wherein the one or more hydrocracking catalysts comprise nickel, cobalt, molybdenum, and / or tungsten. [Aspect 9] From the top to the bottom, (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) one or more layers of free-standing hydroprocessing catalyst; (vii) a layer of one or more supported hydrocracking catalysts; (viii) one or more layers of free-standing hydroprocessing catalysts; (ix) a layer of one or more supported hydrotreating catalysts. wherein the total volume of the three layers containing the one or more self-supporting hydroprocessing catalysts is about 9 to about 45% of the total volume of catalyst in the vertical bed; A layered catalytic reactor system, wherein the total volume of the three layers containing the one or more supported hydrocracking catalysts is about 15 to about 30% of the total volume of catalyst in the vertical bed. [Aspect 10] 10. The layered catalyst reactor system of embodiment 9, wherein the one or more free-standing hydroprocessing catalysts comprise about 5 to about 9 wt. % molybdenum, about 21 to 31 wt. % nickel, and about 33 to about 42 wt. % tungsten. [Aspect 11] 10. The layered catalytic reactor system of embodiment 9, wherein the one or more free-standing hydroprocessing catalysts are selected from the group consisting of catalysts comprising at least one Group VIII metal and at least one Group VIB metal on a support material selected from the group consisting of alumina, zeolite, amorphous silica-alumina, and titania-alumina. [Aspect 12] 10. The layered catalytic reactor system of embodiment 9, wherein the one or more supported hydroprocessing catalysts are selected from the group consisting of Pd or Pt containing catalysts. [Aspect 13] 10. The layered catalytic reactor system of embodiment 9, wherein the one or more hydrocracking catalysts are selected from the group consisting of nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and catalysts comprising nickel-tungsten and / or nickel-molybdenum. [Aspect 14] 10. The layered catalytic reactor system of embodiment 9, wherein the one or more hydrocracking catalysts comprise a porous support material comprising a refractory oxide material. [Aspect 15] 10. The layered catalytic reactor system of embodiment 9, wherein the one or more hydrocracking catalysts comprise nickel, cobalt, molybdenum, and / or tungsten. [Aspect 16] A method for hydrotreating a hydrocarbon feedstock, comprising: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen, and olefins with a layered catalytic reactor system in the presence of hydrogen to produce a hydrocarbon product having a lower content of metals, sulfur, nitrogen, and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically from top to bottom through successive layers of the layered catalytic reactor system; and (iii) recovering the hydrocarbon product from the bottom of the layered catalytic reactor system, The layered catalyst system comprises, from top to bottom: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) one or more layers of free-standing hydroprocessing catalyst; (vii) a layer of one or more supported hydrotreating catalysts. wherein the total volume of the two layers containing the one or more self-supporting hydroprocessing catalysts is about 10% to about 50% of the total volume of catalyst in the vertical bed; the total volume of the two layers containing the one or more supported hydrocracking catalysts is about 10% to about 30% of the total volume of catalyst in the vertical bed; or The layered catalytic reactor system comprises, from top to bottom: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) one or more layers of free-standing hydroprocessing catalyst; (vii) a layer of one or more supported hydrocracking catalysts; (viii) one or more layers of free-standing hydroprocessing catalysts; (ix) a layer of one or more supported hydrotreating catalysts. wherein the total volume of the three layers containing the one or more self-supporting hydroprocessing catalysts is about 9 to about 45% of the total volume of catalyst in the vertical bed; the total volume of the three layers containing the one or more supported hydrocracking catalysts is about 15 to about 30% of the total volume of catalyst in the vertical bed. [Aspect 17] 17. The method of embodiment 16, wherein the operating temperature of the layered catalytic reactor system is in the range of about 371 to 413 °C (about 700 to about 775 °F). [Aspect 18] 17. The method of embodiment 16, wherein the weight hourly space velocity (WHSV) of the method is in the range of about 0.4 to about 1.1 / hr. [Aspect 19] 17. The method of embodiment 16, wherein the liquid hourly space velocity (LHSV) of said method is in the range of about 0.3 to about 0.9 / hr. [Aspect 20] 17. The method of embodiment 16, wherein the normalized temperature of the layered catalytic reactor system is maintained below about 410° C. (770° F.) during the method.

Claims

1. From the top to the bottom, (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) one or more layers of supported hydrocracking catalyst; (vi) one or more layers of free-standing hydroprocessing catalysts; (vii) a layer of one or more supported hydroprocessing catalysts. wherein the total volume of the two layers containing the one or more self-supporting hydroprocessing catalysts is 10-50% of the total volume of catalyst in the vertical bed; A layered catalytic reactor system, wherein the total volume of the two layers containing said one or more supported hydrocracking catalysts is 10-30% of the total volume of catalyst in said vertical bed.

2. 10. The layered catalytic reactor system of claim 1, wherein the one or more free-standing hydroprocessing catalysts comprise 5-9 wt % molybdenum, 21-31 wt % nickel, and 33-42 wt % tungsten.

3. 2. The layered catalytic reactor system of claim 1, wherein the one or more demetallization catalysts are selected from the group consisting of synthetic aluminum oxides or natural aluminum silicates enriched with oxides of molybdenum, cobalt and nickel.

4. 2. The layered catalytic reactor system of claim 1, wherein the one or more supported hydrotreating catalysts are selected from the group consisting of catalysts comprising at least one Group VIII metal and at least one Group VIB metal on a support material selected from the group consisting of alumina, zeolite, amorphous silica-alumina, and titania-alumina.

5. 10. The layered catalytic reactor system of claim 1, wherein the one or more supported hydrotreating catalysts are selected from the group consisting of Pd or Pt containing catalysts.

6. 2. The layered catalytic reactor system of claim 1, wherein the one or more hydrocracking catalysts are selected from the group consisting of nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and nickel-tungsten and / or nickel-molybdenum containing catalysts.

7. 10. The layered catalytic reactor system of claim 1, wherein the one or more hydrocracking catalysts comprise a porous support material comprising a refractory oxide material.

8. 10. The layered catalytic reactor system of claim 1, wherein the one or more hydrocracking catalysts comprise nickel, cobalt, molybdenum and / or tungsten.

9. From the top to the bottom, (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) one or more layers of supported hydrocracking catalyst; (vi) one or more layers of free-standing hydroprocessing catalysts; (vii) one or more layers of supported hydrocracking catalyst; (viii) one or more layers of free-standing hydroprocessing catalysts; (ix) a layer of one or more supported hydrotreating catalysts. wherein the total volume of the three layers containing the one or more self-supporting hydroprocessing catalysts is between 9 and 45% of the total volume of catalyst in the vertical bed; A layered catalytic reactor system, wherein the total volume of the three layers containing said one or more supported hydrocracking catalysts is 15-30% of the total volume of catalyst in said vertical bed.

10. 10. The layered catalytic reactor system of claim 9, wherein the one or more free-standing hydroprocessing catalysts comprise 5-9 wt % molybdenum, 21-31 wt % nickel, and 33-42 wt % tungsten.

11. 10. The layered catalytic reactor system of claim 9, wherein the one or more demetallization catalysts are selected from the group consisting of synthetic aluminum oxides or natural aluminum silicates enriched with oxides of molybdenum, cobalt and nickel.

12. 10. The layered catalytic reactor system of claim 9, wherein the one or more supported hydrotreating catalysts are selected from the group consisting of catalysts comprising at least one Group VIII metal and at least one Group VIB metal on a support material selected from the group consisting of alumina, zeolite, amorphous silica-alumina, and titania-alumina.

13. 10. The layered catalytic reactor system of claim 9, wherein the one or more supported hydrotreating catalysts are selected from the group consisting of Pd or Pt containing catalysts.

14. 10. The layered catalytic reactor system of claim 9, wherein the one or more hydrocracking catalysts are selected from the group consisting of nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and nickel-tungsten and / or nickel-molybdenum containing catalysts.

15. 10. The layered catalytic reactor system of claim 9, wherein the one or more hydrocracking catalysts comprise a porous support material comprising a refractory oxide material.

16. 10. The layered catalytic reactor system of claim 9, wherein the one or more hydrocracking catalysts comprise nickel, cobalt, molybdenum and / or tungsten.

17. A method for hydrotreating a hydrocarbon feedstock, comprising: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen, and olefins with a layered catalytic reactor system in the presence of hydrogen to produce a hydrocarbon product having a lower content of metals, sulfur, nitrogen, and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically from top to bottom through successive layers of the layered catalytic reactor system; and (iii) recovering the hydrocarbon product from the bottom of the layered catalytic reactor system. The layered catalyst system comprises, from top to bottom: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) one or more layers of supported hydrocracking catalyst; (vi) one or more layers of free-standing hydroprocessing catalysts; (vii) a layer of one or more supported hydroprocessing catalysts. wherein the total volume of the two layers containing the one or more free-standing hydroprocessing catalysts is between 10 and 50% of the total volume of catalyst in the vertical bed, the total volume of the two layers containing the one or more supported hydrocracking catalysts is 10-30% of the total volume of catalyst in the vertical bed; or The layered catalytic reactor system comprises, from top to bottom: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) one or more layers of free-standing hydroprocessing catalysts; (v) one or more layers of supported hydrocracking catalyst; (vi) one or more layers of free-standing hydroprocessing catalysts; (vii) one or more layers of supported hydrocracking catalyst; (viii) one or more layers of free-standing hydroprocessing catalysts; (ix) a layer of one or more supported hydrotreating catalysts. wherein the total volume of the three layers containing the one or more free-standing hydroprocessing catalysts is between 9 and 45% of the total volume of catalyst in the vertical bed; The process wherein the total volume of the three layers containing the one or more supported hydrocracking catalysts is 15-30% of the total volume of catalyst in the vertical bed.

18. 18. The method of claim 17, wherein the operating temperature of the layered catalytic reactor system is within the range of 371 to 413°C (700 to 775°F).

19. 18. The process of claim 17, wherein the weight hourly space velocity (WHSV) of the process is in the range of 0.4 to 1.1 / hr.

20. 18. The process of claim 17, wherein the liquid hourly space velocity (LHSV) of the process is in the range of 0.3 to 0.9 / hr.

21. 20. The method of claim 17, wherein the normalized temperature of the layered catalytic reactor system is maintained below 410°C (770°F) during the method.

Citation Information

Patent Citations

  • Hydroprocessing reactor and method using liquid quench

    JP2002503750A

  • Hydrogen treatment catalysts and their manufacturing

    JP2013528489A

  • Heavy oil upgrading system and method

    JP2019522076A

  • Naphthene ring opening over self-supported multimetallic catalysts.